Method for preparing positive electrode active material and lithium secondary battery applying positive active material prepared thereby

The additional calcination process for lithium nickel cobalt manganese oxide-based cathode materials addresses thermal stability and efficiency imbalances, enhancing the performance of lithium secondary batteries by maintaining high charge capacity and reducing discharge capacity, suitable for use with silicon-based anode materials.

KR1020260162014APending Publication Date: 2026-11-10LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020250058127
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-02
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing lithium nickel oxide-based cathode materials in lithium secondary batteries suffer from poor thermal stability and efficiency imbalances due to the decomposition of the positive active material during charging, while silicon-based anode materials have low initial charge/discharge efficiency, leading to performance degradation.

Method used

A manufacturing method involving additional calcination steps to produce a low-efficiency positive electrode active material, including mixing transition metal compounds with lithium raw materials, followed by controlled calcination at specific temperatures and times, and optionally adding additional lithium and coating with specific elements to enhance electrochemical performance.

Benefits of technology

The method results in a positive electrode active material with larger primary particles, maintaining high initial charge capacity while reducing discharge capacity, balancing efficiency with the silicon-based anode, thereby improving the overall stability and performance of lithium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PAT00002_ABST
    Figure PAT00002_ABST
Patent Text Reader

Abstract

A method for manufacturing a positive electrode active material is provided. The manufacturing method comprises the steps of (1) mixing a transition metal compound with a lithium raw material and calcining to produce a first positive electrode active material, and (2) further calcining the first positive electrode active material to produce a second positive electrode active material. The calcination temperature of step (1) is 860°C to 1,100°C, and the additional calcination temperature of step (2) is 90% to 100% of the calcination temperature of step (1). Through the manufacturing method, a low-efficiency positive electrode active material suitable for a lithium secondary battery using a silicon-based negative electrode active material, etc., can be manufactured.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a method for manufacturing a positive electrode active material and a secondary battery using the positive electrode active material manufactured thereby. Specifically, the present invention relates to a method for manufacturing a low-efficiency positive electrode active material through additional calcination and a lithium secondary battery using the low-efficiency positive electrode active material manufactured thereby. Background Technology

[0002] With the increasing technological development and demand for mobile devices, the demand for rechargeable batteries as an energy source is rapidly rising. Among these rechargeable batteries, lithium-ion batteries, which possess high energy density and voltage, long cycle life, and low self-discharge rates, have been commercialized and are widely used.

[0003] Lithium transition metal oxides are used as cathode active materials for lithium secondary batteries; among these, lithium cobalt oxide (LiCoO2) has been primarily used due to its high operating voltage and excellent capacity characteristics. However, LiCoO2 exhibits very poor thermal properties due to the descaling of its crystal structure following lithium delithiation, and its high cost limits its mass use as a power source in fields such as electric vehicles.

[0004] As materials to replace LiCoO2, lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compounds (LiFePO4, etc.), or lithium nickel oxide (LiNiO2, etc.) have been developed. Among these, research and development on lithium nickel oxide is being conducted more actively because it has a high reversible capacity of about 200 mAh / g, making it easy to implement large-capacity batteries. However, LiNiO2 has poor thermal stability compared to LiCoO2, and there is a problem in that if an internal short circuit occurs due to external pressure or other factors while charged, the positive active material itself decomposes, causing the battery to rupture and ignite.

[0005] Accordingly, as a method to improve the low thermal stability of LiNiO2 while maintaining its excellent reversible capacity, LiNi in which a portion of the nickel is substituted with cobalt 1-α Co α A nickel-cobalt-manganese-based lithium composite metal oxide (hereinafter simply referred to as 'NCM-based lithium oxide') in which O2 (α=0.1~0.3) or a portion of nickel is substituted with Mn and Co has been developed. In addition, a lithium transition metal oxide having a concentration gradient of metal composition has been proposed to solve stability issues, such as the leaching of metal elements, while maintaining excellent power characteristics.

[0006] Meanwhile, the development of silicon-based anode active materials is steadily progressing to increase the energy density of batteries. However, compared to graphite, which is a conventional anode active material, the initial charge / discharge efficiency is low. Consequently, due to the imbalance in charge / discharge efficiency between the anode active material and the anode active material, the excess lithium ions generated during the charge / discharge process of the anode active material can become a substance that impairs the overall stability of the anode active material. Therefore, it is necessary to maintain the overall performance of the battery by developing an anode active material that balances efficiency with that of the anode active material.

[0007] Low-efficiency cathode material technology is being researched to balance the efficiency of the anode active material. In low-efficiency cathode material technology, it is crucial to maintain a high charge capacity while reducing only the discharge capacity. Conventionally, low-efficiency cathode active materials were manufactured using methods that compromised material quality, such as introducing structural instability or mixing low-capacity products, in order to artificially lower efficiency. Furthermore, when manufacturing low-efficiency cathode active materials during the coating process that determines electrochemical properties, there is a problem where the charge capacity decreases along with the material quality, even though the material quality is maintained.

[0008] Accordingly, the inventors completed the present invention after researching a method to manufacture a low-efficiency cathode active material having superior performance. Prior art literature

[0009] Republic of Korea Published Patent Application No. 10-2014-0081467 The problem to be solved

[0010] The present invention aims to provide a method for manufacturing a low-efficiency positive electrode active material suitable for a lithium secondary battery using a silicon-based negative electrode active material, etc., by additionally calcining the positive electrode active material after manufacturing, and a lithium secondary battery applying the low-efficiency positive electrode active material manufactured thereby. means of solving the problem

[0011] According to the first aspect of the present invention,

[0012] The present invention provides a method for manufacturing a positive electrode active material.

[0013] In one embodiment of the present invention, the manufacturing method comprises: (1) a step of mixing a transition metal compound with a lithium raw material and calcining it to produce a first positive electrode active material; and (2) a step of further calcining the first positive electrode active material to produce a second positive electrode active material.

[0014] In one embodiment of the present invention, the firing temperature of step (1) is 860°C to 1,100°C, and the additional firing temperature of step (2) is 90% to 100% based on the firing temperature of step (1).

[0015] In one embodiment of the present invention, the firing of step (1) is performed for 5 to 15 hours.

[0016] In one embodiment of the present invention, step (2) involves mixing additional lithium raw materials with the first positive electrode active material before additional calcination.

[0017] In one embodiment of the present invention, the amount of additional lithium raw material in step (2) is 0.1% to 10% by weight based on the amount of lithium raw material in step (1).

[0018] In one embodiment of the present invention, the first positive electrode active material and the second positive electrode active material are in the form of single particles.

[0019] In one embodiment of the present invention, the primary particle size of the first positive electrode active material is 60% to 80% based on the primary particle size of the second positive electrode active material.

[0020] In one embodiment of the present invention, the additional firing of step (2) is performed for 5 to 15 hours.

[0021] In one embodiment of the present invention, the additional firing time of step (2) is 60% to 120% based on the firing time of step (1).

[0022] In one embodiment of the present invention, the transition metal compound of step (1) comprises one or more of the compounds represented by the following chemical formula 1 and the compounds represented by the following chemical formula 2.

[0023] [Chemical Formula 1]

[0024] [Ni x Co y M 1 z M 2 w ](OH)2

[0025] [Chemical Formula 2]

[0026] [Ni x Co y M 1 z M 2 w ]OOH

[0027] In the above chemical formulas 1 and 2, 0.5≤x<1, 0 <y≤0.5, 0<z≤0.5, 0≤w≤0.2이고,

[0028] M 1 is at least one selected from the group consisting of Mn and Al, and

[0029] M 2 is selected from the group consisting of Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y and combinations thereof.

[0030] In one embodiment of the present invention, the mixing weight ratio of the transition metal compound and the lithium raw material in step (1) is 6:4 to 8:2.

[0031] In one embodiment of the present invention, the manufacturing method further includes the step of grinding one or more of the first positive active material manufactured in step (1) and the second positive active material manufactured in step (2) so that the average particle size is 1 μm to 10 μm.

[0032] In one embodiment of the present invention, the manufacturing method further comprises the step of (3) mixing a second positive active material with a coating raw material and calcining it to produce a third positive active material, wherein the coating raw material comprises an element selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y and combinations thereof.

[0033] In one embodiment of the present invention, the firing temperature of step (3) is 400°C to 600°C.

[0034] According to a second aspect of the present invention,

[0035] The present invention provides a lithium secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte.

[0036] In one embodiment of the present invention, the anode comprises an anode active material manufactured by the manufacturing method described above.

[0037] In one embodiment of the present invention, the cathode comprises a silicon-based cathode active material. Effects of the invention

[0038] A method for manufacturing a positive electrode active material according to one embodiment of the present invention is characterized by manufacturing a first positive electrode active material in the form of lithium nickel cobalt manganese oxide that can be utilized as a final product, and then manufacturing a second positive electrode active material with low efficiency through additional calcination. Compared to the first positive electrode active material, the second positive electrode active material according to one embodiment of the present invention has a significantly larger primary particle within a single particle, and when applied to a battery, it can maintain a high initial charge capacity while significantly lowering only the initial discharge capacity. Such a positive electrode active material can resolve the problem of efficiency imbalance with the anode active material of a general lithium nickel cobalt manganese oxide positive electrode active material in a lithium secondary battery using silicon-based anode active materials, and thus can be suitablely used in the said lithium secondary battery. Brief explanation of the drawing

[0039] Figure 1 is a scanning electron microscope (SEM) image of the first positive electrode active material prepared according to Example 1. Figure 2 is a scanning electron microscope (SEM) image of the second positive electrode active material prepared according to Example 1. Figure 3 is a scanning electron microscope (SEM) image of the first positive electrode active material prepared according to Comparative Example 1. Figure 4 is a scanning electron microscope (SEM) image of the second positive electrode active material prepared according to Comparative Example 1. Specific details for implementing the invention

[0040] All embodiments provided according to the present invention can be achieved by the following description. It should be understood that the following description describes preferred embodiments of the present invention and that the present invention is not necessarily limited thereto.

[0041] Where measurement conditions and methods are not specifically described for the physical properties described in this specification, said physical properties are measured according to measurement conditions and methods generally used by a person skilled in the art in the relevant technical field.

[0043] Method for manufacturing positive electrode active material

[0045] The present invention provides a method for manufacturing a low-efficiency cathode active material. The low-efficiency cathode active material can be utilized in general lithium secondary batteries, and specifically, in lithium secondary batteries using silicon-based anode active materials. Silicon-based anode active materials have lower initial charge / discharge efficiency compared to graphite, which is a conventional anode active material, and consequently, there may be an imbalance between the charge / discharge efficiency of the cathode active material and the silicon-based material. This imbalance can generate an excess amount of lithium ions, thereby degrading the performance of the battery; however, the low-efficiency cathode active material manufactured according to the manufacturing method of one embodiment of the present invention can resolve this problem. The present invention possesses excellent processability in that the objective can be achieved through a relatively simple method of additional calcination when manufacturing a low-efficiency cathode active material that maintains a high charge capacity while lowering only the discharge capacity.

[0046] According to one embodiment of the present invention, a method for manufacturing a positive electrode active material comprises: (1) a step of manufacturing a first positive electrode active material by mixing a transition metal compound with a lithium raw material and calcining it; and (2) a step of manufacturing a second positive electrode active material by further calcining the first positive electrode active material. Both the first positive electrode active material and the second positive electrode active material can be utilized as positive electrode active materials in a lithium secondary battery in the form of lithium transition metal oxides. However, the second positive electrode active material corresponds to a low-efficiency positive electrode active material manufactured by further calcining the first positive electrode active material.

[0047] In step (1) above, the transition metal compound is mixed with the lithium raw material. The transition metal compound is a precursor for a positive electrode active material in the form of a transition metal oxide, and is a material containing a hydroxy group or a hydroperoxy group before being completely oxidized. The transition metal compound is not particularly limited as long as it is a material commonly used in the relevant art. According to one embodiment of the present invention, the transition metal compound comprises one or more of the compounds represented by the following chemical formula 1 and the compounds represented by the following chemical formula 2.

[0048] [Chemical Formula 1]

[0049] [Ni x Co y M 1 z M 2 w ](OH)2

[0050] [Chemical Formula 2]

[0051] [Ni x Co y M 1 z M 2 w ]OOH

[0052] In the above chemical formulas 1 and 2, 0.5≤x<1, 0 <y≤0.5, 0<z≤0.5, 0≤w≤0.2이고, M 1 is at least one selected from the group consisting of Mn and Al, and M 2 is selected from the group consisting of Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y, and combinations thereof. M 1 If α contains 2 or more elements, the sum of the mole ratios of each element can be z. M 2If the compound contains two or more elements, the sum of the molar ratios of each element may be w. Specifically, the transition metal compound may include a compound represented by Chemical Formula 2.

[0053] The above lithium raw material is a material that provides lithium elements to the cathode active material, and is not particularly limited as long as it is a material commonly used in the relevant technical field. The above lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a mixture thereof may be used. Specifically, Li2CO3 may be used as the above lithium raw material.

[0054] The transition metal compound and the lithium raw material may be mixed such that the molar ratio of the transition metal to lithium is close to 1. According to one embodiment of the present invention, the mixing weight ratio of the transition metal compound and the lithium raw material is 6:4 to 8:2. Specifically, the mixing weight ratio of the transition metal compound and the lithium raw material may be 6:4 to 8:2, 6:4 to 7.5:2.5, or 6.5:3.5 to 7.5:2.5.

[0055] In step (1) above, the mixing of raw materials is not particularly limited as long as it is a method commonly used in the relevant technical field. The mixing is intended to uniformly disperse various raw materials, and a milling device (e.g., a ball mill) may be utilized.

[0056] A first positive active material is prepared by calcining a mixture of the above transition metal compound and a lithium raw material. The first positive active material is calcined sufficiently so that it can also be utilized as a positive active material in a lithium secondary battery in the form of a lithium transition metal oxide. According to one embodiment of the present invention, the calcination temperature of step (1) is 860°C to 1,100°C. Specifically, the above firing temperature is 860°C or higher, 870°C or higher, 880°C or higher, 890°C or higher, 900°C or higher, 910°C or higher, 920°C or higher, 930°C or higher, 1,100°C or lower, 1,090°C or lower, 1,080°C or lower, 1,070°C or lower, 1,060°C or lower, 1,050°C or lower, 1,040°C or lower, 1,030°C or lower, 1,020°C or lower, 1,010°C or lower, 1,000°C or lower, and may be 860°C to 1,100°C, 880°C to 1,050°C, and 900°C to 1,000°C.

[0057] According to one embodiment of the present invention, the firing of step (1) is performed for 5 to 15 hours. Specifically, the firing time may be 5 hours or more, 6 hours or more, 7 hours or more, 8 hours or more, 15 hours or less, 14 hours or less, 13 hours or less, 12 hours or less, 5 to 15 hours, 7 to 14 hours, 8 to 12 hours.

[0058] In step (2) above, a second positive active material is prepared by further calcining the first positive active material. The second positive active material, like the first positive active material, can also be utilized as a positive active material in a lithium secondary battery in the form of a lithium transition metal oxide, but has low efficiency characteristics compared to the first positive active material due to the additional calcination. According to one embodiment of the present invention, the additional calcination temperature in step (2) is 90% to 100% based on the calcination temperature in step (1). The additional calcination temperature in step (2) may be 90% to 100%, 91% to 100%, 92% to 100%, or 93% to 100%.

[0059] According to one embodiment of the present invention, the firing of step (2) is performed for 5 to 15 hours. Specifically, the firing time may be 5 hours or more, 6 hours or more, 7 hours or more, 15 hours or less, 14 hours or less, 13 hours or less, 12 hours or less, 11 hours or less, 10 hours or less, 5 to 15 hours, 6 to 13 hours, 7 to 11 hours. According to one embodiment of the present invention, the additional firing time of step (2) is 60% to 120% based on the firing time of step (1). Specifically, the above ratio may be 60% or more, 65% or more, 70% or more, 120% or less, 115% or less, 110% or less, 105% or less, and may be 60% to 120%, 65% to 115%, or 70% to 110%.

[0060] In step (2) above, an additional lithium raw material may be mixed with the first cathode active material before additional calcination. The additional lithium raw material may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and for example, Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, Li3C6H5O7, or a mixture thereof. Specifically, Li2CO3 may be used as the lithium raw material. The additional lithium raw material in step (2) above may be the same material as the lithium raw material in step (1), but is not necessarily limited thereto.

[0061] The above additional lithium raw material can improve the electrochemical performance of the second cathode active material by adding a small amount. According to one embodiment of the present invention, the amount of the additional lithium raw material in step (2) is 0.1 wt% to 10 wt% based on the amount of the lithium raw material in step (1). Specifically, the amount of the additional lithium raw material is 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.4 wt% or more, 0.5 wt% or more, 0.6 wt% or more, 0.7 wt% or more, 0.8 wt% or more, 0.9 wt% or more, 1 wt% or more, 10 wt% or less, 9 wt% or less, 8 wt% or less, 7 wt% or less, 6 wt% or less, 5 wt% or less, 4 wt% or less, 3 wt% or less, and may be 0.1 wt% to 10 wt%, 0.5 wt% to 5 wt%, and 1 wt% to 3 wt%.

[0062] The above manufacturing method may further include a step of grinding one or more of the first positive active material manufactured in step (1) and the second positive active material manufactured in step (2). Grinding the first positive active material can increase efficiency during subsequent calcination. Additionally, grinding the second positive active material can improve the performance of the battery when applied to the battery, and can increase calcination efficiency if additional calcination is performed. The grinding method is not particularly limited as long as it is a method generally used in the relevant technical field. The grinding can be performed by a milling device and may undergo a process of coarse grinding followed by fine grinding. Coarse grinding refers to a process of grinding into relatively large particles, and, for example, a roll mill may be utilized. Fine grinding refers to a process of grinding into relatively small particles, and, for example, a jet mill may be utilized. According to one embodiment of the present invention, grinding can be performed so that the average particle size is 1 μm to 10 μm, 2 μm to 9 μm, or 3 μm to 7 μm. The above average particle size may be a particle size corresponding to 50% of the volume accumulation and may be measured by a method commonly used in the relevant technical field. The above average particle size may be measured, for example, through a laser diffraction particle size measuring device (e.g., Microtrac MT 3000), a particle size measuring device utilizing SEM images (e.g., LG Chem DX program), etc.

[0063] According to one embodiment of the present invention, the first positive active material and the second positive active material are in the form of single particles. Since the first positive active material and the second positive active material are particles in the form of single particles, they have high mechanical strength and can provide excellent battery performance when applied to a battery. Since sufficient calcination is carried out at a high temperature even in step (1), the first positive active material can also be obtained as a particle in the form of a single particle. In this specification, the single particle form is a concept contrasted with the spherical secondary particle form formed by the aggregation of tens to hundreds of primary particles manufactured by conventional methods. It is a form in which particles are separated and / or dispersed from each other to form independent and / or distinct phases, but may include a form in which 2 to 10 particles are attached to each other. That is, the single particle form may be a form consisting of only one particle or a form consisting of 2 to 10 primary particles. In this specification, primary particles refer to the smallest unit particles observed during scanning electron microscope (SEM) measurements. Secondary particles refer to aggregates formed by primary particles aggregating together through physical or chemical bonding between primary particles without any intentional aggregation or assembly process of the primary particles constituting the secondary particles, i.e., secondary structures.

[0064] The additional calcination in step (2) above can grow primary particles in a single-particle form of the positive active material. According to one embodiment of the present invention, the primary particle size of the first positive active material is 60% to 80% based on the primary particle size of the second positive active material. At this time, the primary particle size refers to the average size and can be measured using a scanning electron microscope and an image processing program. Specifically, the primary particle size of the first positive active material is 60% or more, 61% or more, 62% or more, 63% or more, 64% or more, 65% or more, 80% or less, 79% or less, 78% or less, 77% or less, 76% or less, 75% or less, and may be 60% to 80%, 65% to 80%, or 65% to 75% relative to the primary particle size of the second positive active material. When manufacturing the first cathode active material, by appropriately controlling the growth level of the primary particles, the manufacturing efficiency of the low-efficiency cathode active material through additional calcination can be increased.

[0065] According to one embodiment of the present invention, the primary particle size of the second positive active material is 1 μm to 4 μm. At this time, the primary particle size refers to the average size and can be measured using a scanning electron microscope and an image processing program. Specifically, the primary particle size of the second positive active material is 1 μm or more, 1.5 μm or more, 2 μm or more, 4 μm or less, 3.5 μm or less, 3 μm or less, 2.5 μm or less, and may be 1 μm to 4 μm, 1.5 μm to 3.5 μm, or 2 μm to 3 μm.

[0066] A method for manufacturing a positive electrode active material according to one embodiment of the present invention further includes the step (3) of mixing a second positive electrode active material with a coating raw material and calcining it to produce a third positive electrode active material. When the manufacturing method includes step (3), the final positive electrode active material may be the third positive electrode active material, but the positive electrode active material may already have low efficiency characteristics through additional calcination in step (2). Therefore, in step (3), the lacking characteristics can be supplemented through coating in addition to the above characteristics. According to one embodiment of the present invention, the coating raw material includes an element selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y, and combinations thereof. The elements may be included in the doping raw material in a suitable form such as sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide. The elements added by the above coating raw material are mainly located on the surface of the positive electrode active material, but some may be incorporated into the interior of the positive electrode active material.

[0067] In step (3) above, the firing for coating may be performed at a lower temperature than the firing in step (1) and the additional firing in step (2). At such temperatures, the growth of primary particles is not significantly affected. According to one embodiment of the present invention, the firing temperature in step (3) above is 400°C to 600°C, 450°C to 600°C, or 450°C to 550°C.

[0069] <Polar>

[0071] The present invention provides a positive electrode comprising a positive electrode active material manufactured by the manufacturing method described above.

[0072] According to one embodiment of the present invention, the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer comprises the positive electrode active material described above.

[0073] According to one embodiment of the present invention, the positive current collector may include a highly conductive metal, and is not particularly limited as long as it allows the positive active material layer to adhere easily and is non-reactive within the voltage range of the battery. The positive current collector may be, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum, and may be used as a stainless steel surface treated with carbon, nickel, titanium, silver, etc. Additionally, the positive current collector may typically have a thickness of 3 μm to 500 μm, and may form fine irregularities on the surface of the current collector to increase the adhesion of the positive active material. The positive current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0074] According to one embodiment of the present invention, the positive active material layer may include, together with the positive active material, a conductive material and a binder optionally as needed. In this case, the positive active material may be included in the positive active material layer in an amount of 80% to 99% by weight, more specifically 85% to 98.5% by weight, based on the total weight of the positive active material layer, and may exhibit excellent capacity characteristics within this range.

[0075] According to one embodiment of the present invention, the conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it has electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The conductive material may be included in the positive electrode active material layer in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.

[0076] According to one embodiment of the present invention, the binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which hydrogens thereof are substituted with Li, Na, or Ca, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The above binder may be included in the positive active material layer in an amount of 0.1% to 15% by weight relative to the total weight of the positive active material layer.

[0077] According to one embodiment of the present invention, the anode may be manufactured according to a conventional anode manufacturing method, except for using the anode active material described above. Specifically, the anode may be manufactured by applying a composition for forming an anode active material layer, prepared by dissolving or dispersing the anode active material described above and optionally a binder, a conductive material, and a dispersant in a solvent, onto an anode current collector, followed by drying and rolling, or by casting the composition for forming an anode active material layer onto a separate support and then laminating the film obtained by peeling from the support onto an anode current collector.

[0078] According to one embodiment of the present invention, the solvent may be a solvent generally used in the relevant technical field, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the solvent used is sufficient to dissolve or disperse the cathode active material, conductive material, binder, and dispersant, taking into account the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that can exhibit excellent thickness uniformity when coated for cathode manufacturing thereafter.

[0080] Lithium secondary battery

[0082] The present invention provides a lithium secondary battery comprising the anode described above.

[0083] According to one embodiment of the present invention, the lithium secondary battery comprises the anode described above; a cathode; a separator interposed between the anode and the cathode; and an electrolyte. Additionally, the lithium secondary battery may optionally further comprise a battery container housing an electrode assembly of the anode, cathode, and separator described above, and a sealing member sealing the battery container.

[0084] According to one embodiment of the present invention, the cathode may comprise a cathode current collector and a cathode active material layer located on the cathode current collector.

[0085] According to one embodiment of the present invention, the negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. The negative current collector may be, for example, copper, stainless steel, aluminum, nickel, titanium, or calcined carbon, and may be a copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy. In addition, the negative current collector may typically have a thickness of 3 μm to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to increase the adhesion of the negative active material. The negative current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0086] According to one embodiment of the present invention, the negative electrode active material layer may optionally include a binder and a conductive material together with the negative electrode active material.

[0087] According to one embodiment of the present invention, the negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. General embodiments include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO₂ β Examples include metal oxides capable of doping and dedoping lithium, such as (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites comprising the metal compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material. Furthermore, the carbon material may include low-crystallinity carbon and high-crystallinity carbon. Representative examples of the above low-crystallinity carbon include soft carbon and hard carbon, and representative examples of the above high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes. The above negative electrode active material may be included in the negative electrode active material layer in an amount of 80% to 99% by weight based on the total weight of the negative electrode active material layer.

[0088] The positive electrode active material prepared according to the manufacturing method of one embodiment of the present invention is a low-efficiency positive electrode active material and can be used together with a silicon (Si)-based negative electrode active material. Compared to graphite, which is a conventional negative electrode active material, the silicon-based negative electrode active material has a high capacity, which can improve the energy density of the battery. However, the silicon-based negative electrode active material has a low initial charge / discharge efficiency, which may cause a problem of imbalance in charge / discharge efficiency with the positive electrode active material; the low-efficiency positive electrode active material can resolve this problem. The silicon-based negative electrode active material may be used without special restrictions as long as it is generally used in the relevant technical field. Examples of the silicon-based negative electrode active material include metallic silicon (Si) and silicon oxide (SiO₂). x , here 0 <x<2) 실리콘 탄화물(SiC) 및 Si-Y 합금(상기 Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 및 이들의 조합으로 이루어진 군에서 선택되는 원소이며, Si은 아님)로 이루어진 군으로부터 선택된 1종 이상을 포함할 수 있다. 상기 원소 Y로는 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db (dubnium), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, 및 이들의 조합으로 이루어진 군에서 선택될 수 있다. 또한, 상기 실리콘계 음극 활물질은 필요에 따라 탄소계 음극 활물질 등과 함께 사용될 수 있다.

[0089] According to one embodiment of the present invention, the binder of the negative electrode active material layer is a component that assists in the bonding between the conductive material, the active material, and the current collector, and can typically be added to the negative electrode active material layer in an amount of 0.1% to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0090] According to one embodiment of the present invention, the conductive material of the negative electrode active material layer may be added to the negative electrode active material layer in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer, as a component for further improving the conductivity of the negative electrode active material. Such a conductive material is not particularly limited as long as it possesses conductivity without causing chemical changes in the battery. For example, the conductive material may be graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; fluorinated carbon; metal powders such as aluminum or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives.

[0091] According to one embodiment of the present invention, the cathode may be manufactured by applying and drying a composition for forming a cathode active material layer, prepared by dissolving or dispersing a cathode active material and optionally a binder and a conductive material in a solvent, on a cathode current collector, or by casting the composition for forming a cathode active material layer onto a separate support and then laminating the film obtained by peeling from the support onto a cathode current collector.

[0092] According to one embodiment of the present invention, the separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions. It can be used without special limitations as long as it is typically used as a separator in a lithium secondary battery, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity. Specifically, a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, a coated separator containing a ceramic component or a polymer material may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.

[0093] According to one embodiment of the present invention, the electrolyte may be an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, a molten inorganic electrolyte, etc., which are usable in the manufacture of a lithium secondary battery, but is not limited thereto. As a specific example, the electrolyte may include an organic solvent and a lithium salt.

[0094] According to one embodiment of the present invention, the organic solvent may be used without particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; and aromatic hydrocarbon-based solvents such as benzene and fluorobenzene. Carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a straight-chain, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms and may include a double bond, a directional ring, or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, a carbonate-based solvent is preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound (e.g., ethylmethyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) is more preferred.

[0095] According to one embodiment of the present invention, the lithium salt may be used without special limitations as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, as the anion of the lithium salt, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be at least one selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, etc. It is preferable to use the lithium salt within the range of 0.1 M to 2.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0096] According to one embodiment of the present invention, in addition to the electrolyte components, the electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the additive may be included in the electrolyte in an amount of 0.1% to 5% by weight relative to the total weight of the electrolyte.

[0097] A lithium secondary battery comprising a positive electrode active material according to one embodiment of the present invention stably exhibits excellent capacity characteristics, output characteristics, and lifespan characteristics, and is therefore useful in fields such as portable devices like mobile phones, laptop computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs) and electric vehicles (EVs).

[0098] There are no specific restrictions on the external shape of the above lithium secondary battery, but it may be a cylindrical type using a can, a prismatic type, a pouch type, or a coin type.

[0099] A lithium secondary battery according to one embodiment of the present invention can be used not only as a battery cell used as a power source for a small device, but can also preferably be used as a unit cell in a medium-to-large battery module comprising a plurality of battery cells.

[0100] Accordingly, according to one embodiment of the present invention, a battery module comprising the lithium secondary battery as a unit cell and a battery pack comprising the same are provided.

[0101] According to one embodiment of the present invention, the battery module or battery pack may be used as a power source for one or more medium-to-large devices, including a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0103] Hereinafter, preferred embodiments are presented to aid in understanding the present invention, but the following embodiments are provided only to facilitate a better understanding of the present invention and do not limit the present invention thereto.

[0105] Example (Preparation of positive electrode active material)

[0107] Example 1

[0108] Ni, a transition metal compound 0.6 Co 0.1 Mn 0.370 wt% of OOH and 30 wt% of the lithium raw material Li2CO3 were uniformly mixed, the mixture was placed in a ceramic container, and then introduced into a Roller Hearth Kiln (RHK) furnace. The mixture was calcined for 10 hours in a furnace heated to 950°C to produce a first positive active material in the form of lithium nickel cobalt manganese oxide. The produced first positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce first positive active material particles with an average particle size of 4.0 μm by volume. An additional 0.4 wt% of the lithium raw material was uniformly mixed with the ground first positive active material particles, the mixture was placed in a ceramic container, and then introduced into a Roller Hearth Kiln furnace. The mixture was further calcined for 10 hours in a furnace heated to 900°C to produce a second positive active material in the form of lithium nickel cobalt manganese oxide. The manufactured second positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce second positive active material particles with an average particle size of 3.8 μm based on volume.

[0110] Example 2

[0111] Ni, a transition metal compound 0.6 Co 0.1 Mn 0.370 wt% of OOH and 30 wt% of the lithium raw material Li2CO3 were uniformly mixed, the mixture was placed in a ceramic container, and then introduced into a Roller Hearth Kiln (RHK) furnace. The mixture was calcined for 10 hours in a furnace heated to 950°C to produce a first positive active material in the form of lithium nickel cobalt manganese oxide. The produced first positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce first positive active material particles with an average particle size of 4.0 μm by volume. An additional 0.4 wt% of the lithium raw material was uniformly mixed with the ground first positive active material particles, the mixture was placed in a ceramic container, and then introduced into a Roller Hearth Kiln furnace. The mixture was further calcined for 7 hours in a furnace heated to 950°C to produce a second positive active material in the form of lithium nickel cobalt manganese oxide. The manufactured second positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce second positive active material particles with an average particle size of 3.8 μm based on volume.

[0113] Comparative Example 1

[0114] Ni, a transition metal compound 0.6 Co 0.1 Mn 0.370 wt% of OOH and 30 wt% of the lithium raw material Li2CO3 were uniformly mixed, the mixture was placed in a ceramic container, and then introduced into a roller haul kiln. The mixture was calcined for 10 hours in a kiln heated to 960°C to produce a first positive active material in the form of lithium nickel cobalt manganese oxide. The produced first positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce first positive active material particles with an average particle size of 4.0 μm by volume. An additional 0.4 wt% of the lithium raw material was uniformly mixed with the ground first positive active material particles, the mixture was placed in a ceramic container, and then introduced into a roller haul kiln. The mixture was further calcined for 10 hours in a kiln heated to 800°C to produce a second positive active material in the form of lithium nickel cobalt manganese oxide. The manufactured second positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce second positive active material particles with an average particle size of 3.8 μm based on volume.

[0116] Comparative Example 2

[0117] Ni, a transition metal compound 0.6 Co 0.1 Mn 0.3 70 wt% of OOH and 30.3 wt% of the lithium raw material Li2CO3 were uniformly mixed and placed in a ceramic container, and then introduced into a Roller Hearth Kiln (RHK) furnace. The mixture was calcined for 16 hours in a furnace heated to 950°C to produce a first positive active material in the form of lithium nickel cobalt manganese oxide. The produced first positive active material was coarsely ground using a roll mill and then finely ground using a jet mill to produce first positive active material particles with an average particle size of 3.8 μm by volume. No additional process was performed to produce the second positive active material.

[0119] Experimental Example (Evaluation of Anode Active Material)

[0121] Experimental Example 1: Images of the first and second positive electrode active materials

[0123] SEM images of the first and second cathode active materials in Example 1 and the first and second cathode active materials in Comparative Example 1 are shown in FIGS. 1 to 4. The SEM images were obtained using a scanning electron microscope (SEM, manufacturer: FEI, product name: Inspect F, magnification: ×2,000).

[0124] As in Example 1, particles homogenized by grinding after an appropriate level of calcination (Fig. 1) may have a reduced particle size variation between particles as the particles grow through additional calcination (Fig. 2). On the other hand, as in Comparative Example 1, particles homogenized by grinding after an excessive level of calcination (Fig. 3) may maintain a particle size variation between particles even after additional calcination (Fig. 4). When the positive electrode active material has a large particle size variation between particles and contains a large number of relatively small particles, characteristics such as initial discharge capacity may appear high. To verify the appropriate level of calcination and the performance of the battery accordingly, the following additional experiments were conducted.

[0126] Experimental Example 2: Primary particle growth rate within a single particle

[0128] The primary particle growth rate within a single particle of the first and second cathode active materials in Examples 1 and 2 and the first and second cathode active materials in Comparative Example 1 was measured and is shown in Table 1 below. The primary particle growth rate within a single particle is a value calculated through the average size of the primary particles, and the primary particle growth rate of the first cathode active material was calculated by setting the average size of the primary particles of the second cathode active material to 100%. The primary particle size was measured by obtaining SEM images (×2,000 magnification) using a scanning electron microscope (SEM, Manufacturer: FEI, Product Name: Inspect F) and using an image processing program (Manufacturer: LG Chem, Product Name: DX Program). Specifically, the boundaries of the primary particles were divided using the SEM image captured at ×2,000 magnification and displayed in random colors. Subsequently, the area of ​​each primary particle was calculated using the number of pixels corresponding to each, and the average particle size of the primary particles was calculated by dividing the total sum of the diameters by the number of particles using the diameter of a circle having the same area as each particle. At this time, the average particle size is calculated using at least 7 SEM images and after removing outliers based on the particle size distribution. For reference, the average primary particle size of the second cathode active material according to Example 1 measured by the method described above is 2.36 μm, and the second cathode active material according to Example 2 and Comparative Example 1 and the first cathode active material according to Comparative Example 2 were manufactured at a level that is not significantly different from this.

[0130] Primary particle growth rate (%) Example 1 First positive active material 72.5 Second positive active material 100 Example 2 First positive active material 73.7 Second positive active material 100 Comparative Example 1 First positive active material 88.3 Second positive active material 100 Comparative Example 2 First positive active material 100 - - * Comparative Example 2 grows the primary particles to 100% when manufacturing the first positive active material without additional calcination to manufacture the second positive active material.

[0132] According to Examples 1 and 2 and Comparative Examples 1 and 2, additional growth of primary particles may occur when the first positive electrode active material is further calcined, and this affects the performance of the battery when applied to the battery. According to Table 1 above, additional growth of primary particles upon further calcination was confirmed in Examples 1 and 2 and Comparative Example 1, but the primary particle growth rate in Examples 1 and 2 was found to be much greater than that in Comparative Example 1.

[0134] Experimental Example 3: Battery Capacity Characteristics

[0136] The second positive active material particles prepared in Examples 1 and 2 and Comparative Examples 1 and 2 (wherein in Comparative Example 2, the first positive active material was used) were uniformly mixed with a coating raw material containing Al and W elements, and the mixture was placed in a ceramic container and then introduced into a roller haul kiln. At this time, the coating raw material was introduced such that the Al and W elements contained in the coating raw material were 1,500 ppm (Al) and 3,000 ppm (W), respectively, based on the total weight of the second positive active material particles. The mixture was calcined for 10 hours in a kiln heated to 500°C to produce a third positive active material in the form of lithium nickel cobalt manganese oxide coated with Al and W elements.

[0137] An anode slurry was prepared by mixing 95 wt% of a third anode active material based on Examples 1 and 2 and Comparative Examples 1 and 2, 2 wt% of Super P as a conductive material, and 3 wt% of polyvinylidene fluoride (PVDF) as a binder in an N-methylpyrrolidone (NMP) solvent. The prepared anode slurry was applied to one side of an aluminum current collector, dried at 130°C, and then rolled to produce an anode.

[0138] An electrode assembly was manufactured by using a lithium metal electrode as the negative electrode and interposing a porous polyethylene separator between the positive and negative electrodes. This was placed inside a battery case, and a coin-type half-cell was manufactured by injecting an electrolyte solution in which 1M LiPF6 was dissolved in an organic solvent mixed with ethylene carbonate (EC):ethyl methyl carbonate (EMC):diethyl carbonate (DEC) in a volume ratio of 3:4:3.

[0139] Each manufactured coin-type half-cell was charged to 4.4 V at 25°C with a constant current of 0.1 C, and then discharged to 2.5 V at 0.1 C to measure the initial charge / discharge capacity and efficiency. The results are shown in Table 2 below.

[0141] Initial charge capacity (mAh / g) Initial discharge capacity (mAh / g) Efficiency (%) Example 1-based third positive electrode active material 216.2 194.9 90.1 Example 2-based third positive electrode active material 215.7 194.2 90.0 Comparative Example 1 based third positive electrode active material 216.2 196.5 90.9 Comparative Example 2 based third positive electrode active material 216.7 196.8 90.8

[0143] According to Table 2 above, the positive active material based on Examples 1 and 2 was found to be able to significantly reduce only the initial discharge capacity while maintaining a similar initial charge capacity compared to the positive active material based on Comparative Examples 1 and 2. These results indicate that the positive active material based on Examples 1 and 2 can resolve the problem of efficiency imbalance with the negative active material, which is a general lithium nickel cobalt manganese oxide positive active material, in lithium secondary batteries using silicon-based negative active materials, etc. Therefore, the positive active material based on Examples 1 and 2 can be used as a low-efficiency positive active material in lithium secondary batteries using silicon-based negative active materials, etc.

[0145] All simple variations or modifications of the present invention fall within the scope of the present invention, and the specific scope of protection of the present invention will be clarified by the appended claims.

Claims

Claim 1 A method for manufacturing a positive electrode active material, wherein the manufacturing method comprises: (1) a step of manufacturing a first positive electrode active material by mixing a transition metal compound with a lithium raw material and calcining it; and (2) a step of manufacturing a second positive electrode active material by further calcining the first positive electrode active material, wherein the calcination temperature of step (1) is 860°C to 1,100°C and the additional calcination temperature of step (2) is 90% to 100% based on the calcination temperature of step (1). Claim 2 A method for manufacturing an anode active material according to claim 1, characterized in that the calcination of step (1) is performed for 5 to 15 hours. Claim 3 A method for manufacturing a positive electrode active material according to claim 1, wherein step (2) involves mixing additional lithium raw materials with the first positive electrode active material before additional calcination. Claim 4 A method for manufacturing a positive electrode active material according to claim 3, wherein the amount of additional lithium raw material in step (2) is 0.1% to 10% by weight based on the amount of lithium raw material in step (1). Claim 5 A method for manufacturing a positive electrode active material according to claim 1, wherein the first positive electrode active material and the second positive electrode active material are in the form of single particles. Claim 6 A method for manufacturing a positive electrode active material according to claim 5, characterized in that the primary particle size of the first positive electrode active material is 60% to 80% based on the primary particle size of the second positive electrode active material. Claim 7 A method for manufacturing an anode active material according to claim 2, characterized in that the additional calcination of step (2) is performed for 5 to 15 hours. Claim 8 A method for manufacturing an anode active material according to claim 7, wherein the additional calcination time of step (2) is 60% to 120% based on the calcination time of step (1). Claim 9 A method for manufacturing an anode active material according to claim 1, wherein the transition metal compound of step (1) comprises one or more of the compounds represented by the following chemical formula 1 and the compounds represented by the following chemical formula 2: [Chemical Formula 1][Ni x Co y M 1 z M 2 w ](OH)2[Chemical Formula 2][Ni x Co y M 1 z M 2 w ]OOH In the above chemical formulas 1 and 2, 0.5≤x<1, 0 <y≤0.5, 0<z≤0.5, 0≤w≤0.2이고,M 1 is at least one selected from the group consisting of Mn and Al, and M 2 is selected from the group consisting of Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y and combinations thereof. Claim 10 A method for manufacturing an anode active material according to claim 1, characterized in that the mixing weight ratio of the transition metal compound and the lithium raw material in step (1) is 6:4 to 8:

2. Claim 11 A method for manufacturing an anode active material according to claim 1, wherein the manufacturing method further comprises the step of grinding one or more of the first anode active material manufactured in step (1) and the second anode active material manufactured in step (2) so that the average particle size is 1 μm to 10 μm. Claim 12 A method for manufacturing a positive electrode active material according to claim 1, wherein the manufacturing method further comprises the step of (3) mixing a second positive electrode active material with a coating raw material and calcining it to produce a third positive electrode active material, and wherein the coating raw material comprises an element selected from the group consisting of Al, Zr, B, W, Mo, Cr, Nb, Mg, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, Y and combinations thereof. Claim 13 A method for manufacturing an anode active material according to claim 1, characterized in that the calcination temperature of step (3) is 400℃ to 600℃. Claim 14 A lithium secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode comprises a positive electrode active material manufactured by the method of claim 1. Claim 15 A lithium secondary battery according to claim 14, wherein the negative electrode comprises a silicon-based negative electrode active material.