Thin-layer asphalt pavement repair method using polymer cement concrete
The use of polymer cement concrete with precise component ratios and joint formation enhances asphalt pavement durability, addressing deformation and cracking issues, ensuring long-term performance and adhesion.
Patent Information
- Application Number
- KR1020250086952
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-06-30
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2045-06-30
AI Technical Summary
Asphalt pavements suffer from deformation, cracking, and durability issues due to high temperatures and de-icing agents, leading to frequent repairs and reduced lifespan, with existing concrete precasting methods being challenging and prone to unevenness, especially in areas with heavy vehicle traffic.
A method involving the use of polymer cement concrete (PCC) is applied to asphalt pavements, comprising specific ratios of cement, polymer solids, coarse and fine aggregates, and chemical admixtures, followed by cutting and coating the surface and forming joints at regular intervals to enhance adhesion and durability.
The method significantly improves durability by preventing cracks and deformation, extending the pavement's lifespan by at least three times, while maintaining adhesion to the underlying asphalt layer and resisting vehicle impacts.
Smart Images

Figure 112025073385030-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention is a construction method that uses polymer cement concrete to repair existing asphalt pavement surfaces, enabling long-term use. Background Technology
[0003] Asphalt pavements experience deformation due to high temperatures in the summer and damage to labeling caused by the deterioration of the bituminous material due to the use of de-icing agents.
[0004] As asphalt utilizes thermoplastic bituminous material, plastic deformation occurs, particularly in areas such as bus stops and intersections where heavy vehicles wait for relatively long periods during the summer when high temperatures begin. Following this plastic deformation, the bituminous material is lost from the asphalt concrete, leading to labeling or fading where aggregates detach. As asphalt pavements used for extended periods develop potholes along with cracks, requiring periodic repairs.
[0005] The periodic maintenance of asphalt pavements is generally 5 to 7 years, and while the lifespan is significantly shorter compared to concrete pavements, there are advantages such as reduced fatigue and noise during driving.
[0006] When such asphalt reaches the end of its life, it is usually recycled into an overlay pavement, typically by cutting away a thickness of 4 to 8 cm and repaving that section with asphalt concrete (refer to Registered Patent No. 10-2123329 (hereinafter Prior Art 1)).
[0007] In this case, if the asphalt pavement is in a section vulnerable to plastic deformation, it is necessary to propose an alternative, and recently, a method using concrete precast has been proposed (see Registered Patent No. 10-2731407 (hereinafter Prior Art 2)).
[0008] However, such concrete precasting is difficult to construct, and in the case of wide roadways, not only is construction significantly challenging, but there may also be issues such as unevenness in the precasting after construction.
[0009] Overseas, asphalt pavement repair using polymer cement concrete (PCC) has been carried out since around 1910. Although issues such as adhesion problems with the asphalt were raised in the early stages, subsequent research and development have resulted in excellent durability and weather resistance, leading to its development and use as a paving method.
[0010] However, the conventional method for improving the asphalt pavement surface of PCC can lead to deterioration in durability due to the occurrence of cracks during construction, so improvement is necessary. Prior art literature
[0012] Registered Patent Publication No. 10-1922227 The problem to be solved
[0013] The present invention aims to solve the above-mentioned problems and to repair asphalt pavement surfaces, with the objective of improving durability by suppressing the occurrence of cracks. means of solving the problem
[0015] To achieve the above objective, the present invention comprises the steps of: manufacturing polymer cement concrete by mixing 8.2 to 90 parts by weight of cement, 0.5 to 28 parts by weight of polymer solids, 14.2 to 180 parts by weight of coarse aggregate, and 17.1 to 200 parts by weight of fine aggregate, based on 4 parts by weight of water (S10); cutting the upper surface of an asphalt paved road and applying the polymer cement concrete to the cut upper surface of the asphalt paved road (S20); and forming a plurality of joints at intervals of 1.2m to 1.8m on the upper surface of the polymer cement concrete (S30).
[0016] In addition, each of the above coarse aggregate and the above fine aggregate has a density of 2.5 g / cm³ and an absorption rate of 3% or less, and the above coarse aggregate may have a size of less than 25 mm and may be smaller than 1 / 3 of the construction surface. Effects of the invention
[0018] The present invention, as described above, is intended for repairing asphalt pavement surfaces and has the effect of improving durability by suppressing the occurrence of cracks. Brief explanation of the drawing
[0020] FIG. 1 is a schematic flowchart illustrating an asphalt pavement repair method according to one embodiment of the present invention. Specific details for implementing the invention
[0021] The advantages and features of the present invention and the methods for achieving them will become clear by referring to the embodiments described below in detail together with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below but may be implemented in various different forms. These embodiments are provided merely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims.
[0022] When we say that a part is "connected," this includes not only cases where it is "directly connected," but also cases where it is "indirectly connected" with other components in between.
[0024] FIG. 1 is a schematic flowchart illustrating an asphalt pavement repair method according to one embodiment of the present invention.
[0025] The asphalt pavement repair method according to one embodiment of the present invention is a thin-layer asphalt pavement repair method using polymer cement concrete, and for convenience of explanation, it will be referred to as the ‘this method’ below.
[0026] This method is designed to solve the aforementioned problems and manufactures the PCC described below using conventional inorganic materials composed of cement, aggregates, and gravel, as well as organic materials composed of latex as a polymer, chemical admixtures for concrete to improve workability, crack reducers to prevent cracking, and fibers. The PCC applied to asphalt pavement repair is also known as white topping; conventional white topping (WT) refers to a thickness of 20 cm or more, thin white topping (TWT) refers to a thickness of 10 to 20 cm, and ultra-thin white topping (UTWT) refers to a thickness of 10 cm or less. During the design phase, WT is constructed without considering the adhesion between the underlying asphalt layer and the upper concrete layer, and in the case of TWT, adhesion with the underlying layer may not be considered in some cases. On the other hand, in the case of UTWT, adhesion to the lower layer must be achieved, because if the upper concrete and the lower asphalt pavement layer are not adhered, the upper concrete plate may detach and collapse due to repeated impacts.
[0027] Referring to FIG. 1, the present method (asphalt pavement repair method) may include a PCC manufacturing step (S10), a cutting and coating step (S20), and a joint construction step (S30).
[0028] The PCC manufacturing step (S10) is a step of manufacturing polymer cement concrete (PCC) by mixing 8.2 to 90 parts by weight of cement, 0.5 to 28 parts by weight of polymer solids, 14.2 to 180 parts by weight of coarse aggregate and 17.1 to 200 parts by weight of fine aggregate, based on 4 parts by weight of water.
[0029] In this method, each component constituting the PCC was described based on 4 parts by weight of water.
[0030] First, the cement must be based on ordinary Portland cement (OPC), but either Type 3 rapid-hardening cement (rapid-hardening type) or ultra-rapid-hardening cement must be used. Otherwise, it will be difficult to secure the required strength for repair, and there is a risk of cracking or detachment.
[0031] It is preferable to use 8.2 to 90 parts by weight of the above cement based on 4 parts by weight of water. If the cement is less than 8.2 parts by weight, it is difficult to obtain the required strength, and if it exceeds 90 parts by weight, it may result in economic losses due to overmixing.
[0032] Polymers such as acrylic, styrene, EVA (Ethylene Vinyl-Acetate), polyvinyl alcohol, acryl latex, SB (Styrene-Butadiene) rubber latex, etc., can be used.
[0033] Polymer solids refer to the actual active solid components of a polymer in liquid form, excluding water and solvents.
[0034] The above polymer preferably has a solid content of 35 to 60 weight%. If the solid content is less than 35 weight%, the amount used increases, which may lead to significant changes in workability during manufacturing. If it is 60 weight% or more, manufacturing is difficult and the price is high, making it uneconomical.
[0035] The polymer solid content can be used in an amount of 0.5 to 28 parts by weight based on 4 parts by weight of water.
[0036] If less than 0.5 parts by weight of the above polymer solid content is used, impact resistance may be poor and adhesion to the underlying asphalt concrete layer may be reduced.
[0037] In addition, if the polymer solid content exceeds 28 parts by weight, the curing time increases, which slows down traffic development, and the PCC deforms too easily, which can cause problems such as the repaired road being easily damaged.
[0038] Coarse aggregate and fine aggregate are used as aggregates; coarse aggregate is aggregate that passes through a 4.75mm sieve, and fine aggregate is aggregate that passes through a 4.75mm sieve.
[0039] Coarse aggregate can be used in an amount of 14.2 to 180 parts by weight based on 4 parts by weight of water.
[0040] If less than 14.2 parts by weight of coarse aggregate is used, crack development in the PCC produced during the PCC manufacturing step (S10) may increase, and if more than 180 parts by weight of coarse aggregate is used, there is a problem of reduced workability.
[0041] Fine aggregate can be used in an amount of 17.1 to 200 parts by weight based on 4 parts by weight of water. If the amount of fine aggregate is less than 17.1 parts by weight, the repaired part will have a rough surface, making the work difficult, and if it exceeds 200 parts by weight, a decrease in durability may occur due to an increase in s / a (Sand / Aggregate).
[0042] Meanwhile, the above coarse aggregate and fine aggregate may each have a density of 2.5 g / cm³ or more and an absorption rate of 3% or less.
[0043] If the above coarse aggregate and fine aggregate each have a density of less than 2.55 g / cm³ and an absorption rate exceeding 3%, there may be changes in workability before hardening of the concrete, loss of compressive strength after hardening, and occurrence of cracks.
[0044] In addition, the above coarse aggregate may have a size of less than 25 mm and may be smaller than 1 / 3 of the construction surface.
[0045] If the size of the coarse aggregate is larger than 25 mm, it is advantageous for crack suppression, but workability is poor, which increases the amount of water used and can have a negative effect on the quality of the concrete.
[0046] Considering workability, it is preferable that the size of the above coarse aggregate be 19 mm or less.
[0047] If the size of the coarse aggregate is larger than 1 / 3 of the construction surface, there is a problem of reduced adhesion.
[0048] The above PCC manufacturing step (S10) may be a step of mixing, based on 4 parts by weight of water, 8.2 to 90 parts by weight of cement, 0.5 to 28 parts by weight of polymer solids, 14.2 to 180 parts by weight of coarse aggregate, 17.1 to 200 parts by weight of fine aggregate, and 0.0057 to 4 parts by weight of chemical admixture solids. The chemical admixture is viscous class It is desirable to use polycarboxylic acid-based chemical admixtures to improve workability and thereby minimize water usage, which are used for the purpose of increasing strength or to produce homogeneous concrete. If other admixtures are used, the ability to maintain workability must be verified, and in particular, those that pose a risk of delayed strength development due to maintenance must be excluded.
[0049] delete
[0050] As mentioned above, chemical admixtures are used in an amount of 0.0057 to 4 parts by weight based on 4 parts by weight of water. If less than 0.0057 parts by weight is used, there is a risk of reduced strength due to increased water usage resulting from reduced workability, and if more than 4 parts by weight is used, the cement reacts with water to slow down the hardening speed, which may result in a decrease in early strength.
[0051] Referring to FIG. 1, the cutting and coating step (S20) is a step of cutting the upper part of the asphalt pavement to be constructed and applying the polymer cement concrete (PCC) to the upper part of the cut asphalt pavement.
[0052] Cutting of paved roads (asphalt paved roads) can be performed using cutting equipment such as cold milling machines and small cold planers.
[0053] After the above cutting and coating step (S20), the PCC can be cured by attaching a polymer solid to the cut portion of the paved road (asphalt paved road).
[0055] Below, we will describe a PCC manufactured in the PCC manufacturing step (S10) and a comparative example.
[0056] The physical properties of the PCC (Example) and the Comparative Example manufactured in the above PCC manufacturing step (S10) were evaluated by comparison according to the Korea Expressway Corporation's LMC (latex Modified Concrete) specifications.
[0057] The example satisfies the composition ratio of the PCC component, and the comparative example has the same amount of other components as the example, but the amount of polymer solids is 0, and the amount of water is increased by the amount of the reduced amount of polymer solids.
[0058] S Company's polycarboxylic acid series was used as the chemical admixture, Kumho Corporation's SBR latex was used as the polymer, and Union Corporation's micro-cement was used as the cement.
[0059] Table 1 below is a table for comparing the physical properties of the examples and comparative examples.
[0061] [Table 1]
[0062]
[0064] Referring to Table 1 above, both the example and the comparative example showed similar resistance to compressive force. However, regarding adhesion strength with the underlying asphalt concrete layer, the example obtained 0.8 MPa, while the comparative example obtained 0.6 MPa, raising concerns about damage during long-term use. In particular, after 100 freeze-thaw cycles, the adhesion strength in the comparative example dropped significantly to 0.2 MPa, raising concerns about partial damage, whereas in the example, it decreased only slightly to 0.7 MPa. Therefore, it was determined that detachment or partial damage would not occur even with long-term use. Thus, when applied to asphalt concrete roads such as bus stop intersections, it was found to have a significant advantage in compensating for disadvantages such as plastic deformation and asphalt detachment compared to conventional asphalt overlays.
[0066] Referring to FIG. 1, the joint construction step (S30) is a step of forming a plurality of joints at intervals of 1.2m to 1.8m on the upper surface of the polymer cement concrete.
[0067] The joint construction step (S30) can be performed using joint construction equipment such as a concrete cutter, water jet cutter, grinder, hand roll, and spacer, and since the joint construction equipment is known, a more detailed description is omitted.
[0068] In the above joint construction step (S30), the joints can be installed in a square shape, and if the spacing of the joints is less than 1.2m, the cost is high, and if it is greater than 1.8m, there is a problem of cracking.
[0069] The width of the joint can be 4 to 6 mm. If it is smaller than 4 mm, it is difficult to accommodate changes in length due to temperature, and if it is larger than 6 mm, the cost of cutting is high, which is not economical.
[0071] This method is used for overlaying after cutting down aged asphalt pavement surfaces. Unlike conventional asphalt overlays, it does not cause potholes or plastic deformation and is a highly durable repair method with an expected lifespan of at least three times longer. In particular, it can fundamentally prevent deformation caused by temperature changes in the asphalt pavement surface due to global warming. It also has the advantage of preventing temperature increases on the road pavement surface caused by solar heat in the summer, as it absorbs less infrared radiation than the asphalt pavement surface.
[0072] More specifically, the PCC manufactured in the PCC manufacturing step (S10) of the present method is a composition used for repairing asphalt pavement surfaces in intersections with high vehicle density or severe traffic congestion, such as underpasses, and by bonding to the underlying asphalt pavement layer to resist vehicle loads and impacts, plastic deformation of the existing asphalt pavement does not occur, thereby extending the lifespan of the road pavement surface.
[0073] In other words, this method is a repair method that is considered to contribute to asphalt pavement repair suitable for city roads, etc., because when repairing aged asphalt concrete pavement surfaces, deformation or cracking of the asphalt pavement surface caused by heavy vehicles does not occur, and when applied to bus stops, underpasses, intersections, etc., the asphalt pavement surface can be used for a long time without cracking, detachment, or deformation even when overlaying is performed.
[0075] As described above, the present invention has been explained by specific details such as specific components, limited embodiments, and drawings; however, this is provided merely to aid in a more comprehensive understanding of the invention, and the invention is not limited to the above embodiments. A person skilled in the art can make various modifications and variations from this description.
[0076] Accordingly, the scope of the present invention should not be limited to the described embodiments, and all things equivalent to or having equivalent variations to the claims set forth below, as well as the claims set forth below, shall be considered to fall within the scope of the concept of the present invention.
Claims
Claim 1 A step of manufacturing polymer cement concrete by mixing 8.2 to 90 parts by weight of cement, 0.5 to 28 parts by weight of polymer solids, 14.2 to 180 parts by weight of coarse aggregate, 17.1 to 200 parts by weight of fine aggregate, and 0.0057 to 4 parts by weight of polycarboxylic acid-based chemical admixture solids, based on 4 parts by weight of water (S10); a step of cutting the upper surface of an asphalt paved road using cutting equipment and applying the polymer cement concrete to the cut upper surface of the asphalt paved road (S20); The method includes the step (S30) of forming a plurality of joints at intervals of 1.2m to 1.8m on the upper surface of the polymer cement concrete using joint construction equipment, wherein the coarse aggregate and the fine aggregate each have a density of 2.5g / cm3 and an absorption rate of 3% or less, the coarse aggregate has a size of less than 19mm and is smaller than 1 / 3 of the construction surface, the joint has a width of 4 to 6mm, the polycarboxylic acid-based chemical admixture is used to induce improvement in the viscosity and workability of the polymer cement concrete, for the purpose of increasing strength and creating homogeneous concrete, the polymer solid content is used to improve adhesion (adhesion strength) with asphalt concrete, suppress the decrease in adhesive strength under freeze-thaw conditions, suppress detachment and partial damage during long-term use, and reduce plastic deformation and asphalt detachment compared to asphalt overlay, the joints formed in the step (S30) are square, and the coarse aggregate The aggregate is sieveable by a 4.75mm sieve, the fine aggregate is aggregate that passes through a 4.75mm sieve, and the cement is based on ordinary cement and uses Type 3 rapid hardening cement or ultra-rapid hardening cement. The above-described polymer cement concrete is an asphalt pavement repair method characterized by the polymer solid component adhering to and hardening in the cut portion of the pavement after the cutting and coating step (S20). Claim 2 delete Claim 3 delete Claim 4 delete
Citation Information
Patent Citations
Mortar composition of polymer cement and paving method using the same
KR100953212B1
Concrete overlay methode using foam shotcrete after cutting out asphalt pavement
KR1020150092843A
A high functionality of high early strength cement concrete composition for road pavement and a repairing method of road pavement using the same
KR102085621B1