Multicyclic dianhydride and acid anhydride compounds with sulfone group and polyimide resin and film prepared therefrom

Polycyclic dianhydrides and acid anhydrides with sulfonate groups are integrated into polyimide-based resins to create films with high heat resistance, low thermal expansion, and transparency, addressing the challenges of flexible display devices in high-temperature processes.

KR103045083B1Active Publication Date: 2026-11-06KOREA ADVANCED INST OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250050851
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2025-02-10
Filing Date
2025-04-18
Publication Date
2026-11-06
Estimated Expiration
2045-04-18

AI Technical Summary

Technical Problem

Existing polyimide-based films struggle to achieve high heat resistance, low thermal expansion, and transparency simultaneously, making them unsuitable for high-temperature processes in flexible display devices like LTPO and OLEDs.

Method used

Development of polycyclic dianhydrides and acid anhydrides with sulfonate groups, incorporated into polyimide-based resins, which are prepared through specific oxidation and reaction processes to form films with repeating units that enhance heat resistance, flexibility, and transparency.

Benefits of technology

The resulting polyimide-based films exhibit a glass transition temperature of 400°C or higher, a coefficient of thermal expansion of 20 ppm/°C or less, and a transmittance of 85% or higher, suitable for flexible display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025044219977-PAT00147_ABST
    Figure 112025044219977-PAT00147_ABST
Patent Text Reader

Abstract

The present invention relates to polycyclic dianhydride and acid anhydride compounds having sulfonate groups, a method for preparing dianhydride and acid anhydride compounds, and a polyimide-based resin and film having excellent heat resistance, flexibility, and transparency comprising repeating units of dianhydride and acid anhydride compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to polycyclic dianhydrides and acid anhydrides having sulfonate groups, and polyimide-based resins and films having excellent heat resistance, flexibility, and transparency prepared therefrom. Background Technology

[0002] As display devices have recently evolved into various forms, lightweighting, thinning, and variability—such as the ability to fold or roll—have become increasingly important. Consequently, there are ongoing attempts to replace conventional glass substrates with polyimide-based films that are lightweight, flexible, and possess excellent chemical resistance. Flexible displays are lightweight, unbreakable, and free from shape limitations, allowing for diverse designs. Furthermore, they are not constrained by portability or size limitations, making it possible to manufacture display devices of various shapes. Polymer materials intended to replace glass substrates must possess physical, thermal, and optical properties comparable to those of glass. While polyimide resins exhibit excellent physical properties such as heat resistance, applying polyimide-based films to display devices requires improving inherent yellowness characteristics and imparting colorless, transparent optical properties without compromising heat resistance or dimensional stability.

[0003] In particular, low-temperature polycrystalline oxide (LTPO) and organic light-emitting diode (OLED) display devices, for which demand has recently been increasing, involve high-temperature processes such as the deposition and annealing of thin film transistors (TFTs) and organic materials, so deformation must not occur even during high-temperature processes. For example, thermal properties such as a low coefficient of thermal expansion similar to that of inorganic materials and metals used in TFTs, and a high glass transition temperature of 400°C or higher are required.

[0004] However, attempting to impart transparency to polyimide-based films generally results in reduced heat resistance and an increased coefficient of thermal expansion. Although research is ongoing to develop colorless, transparent polyimide-based films with high heat resistance and a low coefficient of thermal expansion, this is considered a very difficult technical challenge. Prior art literature

[0005] Republic of Korea Published Patent Application No. 10-2024-0117279 (2024.08.01) The problem to be solved

[0006] The present invention provides polycyclic dianhydric and acid anhydric compounds having sulfonate groups, and a method for preparing the same.

[0007] The present invention also provides a novel polyimide-based resin and film having excellent heat resistance, flexibility, and transparency, comprising repeating units of the above-mentioned dianhydride and acid anhydride compounds.

[0008] Another aspect of the present invention provides a flexible display device comprising the polyimide-based film. means of solving the problem

[0009] One embodiment of the present invention provides a dianhydric compound of the following formula 1 and an acid anhydric compound of the following formula 2.

[0010] [Chemical Formula 1] [Dianhydride Compound]

[0011]

[0012] [Chemical Formula 2] [Acid Anhydride Compound]

[0013]

[0014] According to one embodiment, the method for preparing Formula 1 may include the step of oxidizing a precursor of Formula 25 in the presence of an oxidizing agent. Additionally, the method for preparing Formula 2 may include the step of oxidizing a precursor of Formula 26 in the presence of an oxidizing agent.

[0015] [Chemical Formula 25]

[0016]

[0017] [Chemical Formula 26]

[0018]

[0019] One embodiment of the present invention provides a polyimide-based resin comprising repeating units represented by the following chemical formula 3 or chemical formula 4.

[0020] [Chemical Formula 3]

[0021]

[0022] [Chemical Formula 4]

[0023]

[0024] Ar1 each independently, or And,

[0025] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2.

[0026] The polyimide-based resin of the present invention may include repeating units selected from the following chemical formulas 5 to 8.

[0027] [Chemical Formula 5]

[0028]

[0029] [Chemical Formula 6]

[0030]

[0031] [Chemical Formula 7]

[0032]

[0033] [Chemical Formula 8]

[0034]

[0035] X can be a single bond, -CH2-, -O-, -S-, -SO2-, -CO-, isopropylidene, hexafluoroisopropylidene, or a combination thereof, and

[0036] Ar1 and Ar2 are each independently or And,

[0037] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2.

[0038] y:z is 100:0 to 10:90.

[0039] In one embodiment, the polyimide-based resin of the present invention may include repeating units represented by the following chemical formulas 9 to 11.

[0040] [Chemical Formula 9]

[0041]

[0042] [Chemical Formula 10]

[0043]

[0044] [Chemical Formula 11]

[0045]

[0046] A polyimide-based resin according to one embodiment of the present invention may include repeating units represented by the following chemical formula 12.

[0047] [Chemical Formula 12]

[0048]

[0049] Ar1 and Ar2 are each independently or And,

[0050] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0051] y:z is 100:0 to 10:90.

[0052] In one embodiment, the number average molecular weight of the polyimide-based resin may be 10,000 to 200,000 g / mol.

[0053] A polyimide-based resin according to one embodiment of the present invention can be prepared by reacting a dianhydride compound represented by the following chemical formula 1 with an aromatic diamine represented by chemical formula 21; sequentially reacting a dianhydride compound represented by chemical formula 23 with an aromatic diamine represented by chemical formula 22; and imidizing to include a repeating unit represented by chemical formula 5.

[0054] [Chemical Formula 1]

[0055]

[0056] [Chemical Formula 21]

[0057]

[0058] [Chemical Formula 22]

[0059]

[0060] [Chemical Formula 23]

[0061]

[0062] [Chemical Formula 5]

[0063]

[0064] X can be a single bond, -CH2-, -O-, -S-, -SO2-, -CO-, isopropylidene, hexafluoroisopropylidene, or a combination thereof, and

[0065] Ar1 and Ar2 are each independently or And,

[0066] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0067] y:z is 100:0 to 10:90.

[0068] A polyimide-based resin according to one embodiment of the present invention can be prepared by reacting an acid anhydride compound represented by the following formula 2 with an aromatic diamine represented by formula 21; sequentially reacting the acid anhydride compound represented by formula 2 with an aromatic diamine represented by formula 22; and imidizing to include a repeating unit represented by formula 12.

[0069] [Chemical Formula 2]

[0070]

[0071] [Chemical Formula 21]

[0072]

[0073] [Chemical Formula 22]

[0074]

[0075] [Chemical Formula 12]

[0076]

[0077] Ar1 and Ar2 are each independently or And,

[0078] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0079] y:z is 100:0 to 10:90.

[0080] A polyimide-based resin according to one embodiment of the present invention can be prepared by reacting a dianhydride compound represented by the following formula 1 with an aromatic diamine represented by formula 21; sequentially reacting an aromatic acyl chloride represented by formula 24 with an aromatic diamine represented by formula 22; and imidizing to include a repeating unit represented by formula 6.

[0081] [Chemical Formula 1]

[0082]

[0083] [Chemical Formula 21]

[0084]

[0085] [Chemical Formula 22]

[0086]

[0087] [Chemical Formula 24]

[0088]

[0089] [Chemical Formula 6]

[0090]

[0091] Ar1 and Ar2 are each independently or And,

[0092] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0093] y:z is 100:0 to 10:90.

[0094] A composition for forming a polyimide-based film according to one embodiment of the present invention may include the polyimide-based resin described above.

[0095] In one embodiment, the composition for forming a polyimide-based film may further include an organic solvent.

[0096] In one embodiment, the composition for forming a polyimide-based film may contain 5 to 50 weight percent of a polyimide-based resin based on the total weight of the composition.

[0097] A polyimide-based film according to one embodiment of the present invention can be formed from the above-described film-forming composition.

[0098] In one embodiment, the polyimide-based film may have a glass transition temperature (Tg) of 400°C or higher.

[0099] In one embodiment, the polyimide-based film may have a coefficient of thermal expansion of 20 ppm / ℃ or less.

[0100] In one embodiment, the polyimide-based film may have a transmittance of 85% or more at a wavelength of 550 nm.

[0101] A flexible display device according to one embodiment of the present invention may include the above-mentioned polyimide-based film. Effects of the invention

[0102] A novel polyimide-based resin and film comprising an acid anhydride compound and a dianhydride compound according to one embodiment of the present invention exhibit excellent heat resistance, flexibility, and transparency. Specifically, a polyimide-based film according to one embodiment has a glass transition temperature of 400°C or higher, a coefficient of thermal expansion of 20 ppm / °C or lower, and is transparent with a transmittance of 85% or higher at a wavelength of 550 nm. The polyimide-based film may also minimize the difference in expansion and contraction between heterogeneous materials caused by heat generated during processing and operation. A polyimide-based film according to one embodiment can be utilized as a flexible display device. Brief explanation of the drawing

[0103] Figure 1 shows the results of the proton nuclear magnetic resonance (1H NMR) analysis of intermediate D-2. Figure 2 shows the carbon nuclear magnetic resonance (13C NMR) analysis results of intermediate D-2. Figure 3 shows the results of the proton nuclear magnetic resonance (13C NMR) analysis of intermediate D-3. Figure 4 shows the carbon nuclear magnetic resonance (13C NMR) analysis results of intermediate D-3. Figure 5 is the result of (1) proton nuclear magnetic resonance (13C NMR) analysis of the dianhydride compound. Figure 6 is the result of (1) carbon nuclear magnetic resonance (13C NMR) analysis of the dianhydride compound. Figure 7 shows the results of the proton nuclear magnetic resonance (1H NMR) analysis of the polyamic acid of Example 1. Figure 8 shows the Fourier transform infrared spectroscopy (FT-IR) analysis results of the polyimide (PI-1) of Example 1. Figure 9 is a graph of the thermogravimetric analysis of the polyimide (PI-1) of Example 1 in nitrogen and air environments. Figure 10 is a differential scanning calorimetry analysis graph of the polyimide (PI-1) of Example 1. Figure 11 is a photograph of the polyimide film of Examples 1 and 3. Specific details for implementing the invention

[0104] To fully understand the structure and effects of the present invention, preferred embodiments of the present invention are described with reference to the attached drawings. However, the present invention is not limited to the embodiments disclosed below, but can be implemented in various forms and various modifications can be made. The description of these embodiments is provided merely to ensure that the disclosure of the present invention is complete and to fully inform those skilled in the art of the scope of the invention. Those skilled in the art will understand that the concept of the present invention can be carried out in any suitable environment.

[0105] The terms used herein are for describing the embodiments and are not intended to limit the invention. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text. As used herein, 'comprises' and / or 'comprising' do not exclude the presence or addition of one or more other components, steps, actions, and / or elements to the mentioned components, steps, actions, and / or elements.

[0106] In this specification, the alkyl group may be a linear alkyl group, a branched alkyl group, or a cyclic alkyl group. The number of carbon atoms in the alkyl group is not particularly limited, but may be an alkyl group having 1 to 5 carbon atoms. Examples of alkyl groups include, but are not limited to, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an i-butyl group, a 2-ethylbutyl group, a 3,3-dimethylbutyl group, an n-pentyl group, an i-pentyl group, a neopentyl group, a t-pentyl group, and a cyclopentyl group.

[0107] In this specification, the number of carbon atoms in the alkoxy group is not particularly limited, but may be 1 or more and 5 or less. The alkoxy group may include alkyl alkoxy groups and aryl alkoxy groups.

[0108] In this specification, examples of halogens include fluorine (F), chlorine (Cl), bromine (Br), and iodine (I), but are not limited thereto.

[0109] In this specification, "substituted or unsubstituted" may mean substituted or unsubstituted with one or more substituents selected from the group consisting of hydrogen atoms, halogen atoms, hydroxyl groups, alkoxy groups, alkyl halides, alkoxy halides, alkyl groups, alkenyl groups, aryl groups, and heterocyclic groups. Additionally, each of the substituents exemplified above may be substituted or unsubstituted. For example, an alkoxy halide may be interpreted as an alkoxy group.

[0110] Unless otherwise defined in the chemical formulas of this specification, if a chemical bond is not drawn at a position where a chemical bond should be drawn, it may mean that a hydrogen atom is bonded at said position.

[0111] In this specification, the same reference numeral throughout the text may refer to the same component.

[0112] In this specification, "polyimide-based" may refer to all polymers in which imide bonds (-CO-N-CO-) are included in repeating units.

[0113] The present invention will be described in detail below.

[0114] The present invention provides polycyclic dianhydrides and acid anhydrides having sulfonate groups that can be used to manufacture polyimide-based films with excellent heat resistance, flexibility, and transparency.

[0115] Specifically, the above dianhydride and acid anhydride compounds can be represented by the following chemical formulas 1 and 2.

[0116] [Chemical Formula 1] [Dianhydride Compound]

[0117]

[0118] [Chemical Formula 2] [Acid Anhydride Compound]

[0119]

[0120] The method for preparing Chemical Formula 1 above may include a step of oxidizing a precursor of Chemical Formula 25 below in the presence of an oxidizing agent. After the oxidation reaction of the precursor, the method may include a step of reacting with acetic anhydride to finally obtain a dianhydride from the precursor. A more detailed explanation of the method for preparation is provided in Preparation Example 1 described below.

[0121] [Chemical Formula 25]

[0122]

[0123] The method for preparing Formula 2 above may include a step of oxidizing a precursor of Formula 26 below in the presence of an oxidizing agent. After the oxidation reaction of the precursor, the acid anhydride may be finally obtained by vacuum sublimation. A more detailed explanation of the above method is provided in Preparation Example 2 described below.

[0124] [Chemical Formula 26]

[0125]

[0126] The above oxidizing agent is not particularly limited, but any one selected from potassium permanganate (KMnO4), hydrogen peroxide (H2O2), chromic acid (H2CrO4), calcium sulfate (K2S2O8) and potassium dichromate (K2Cr2O7) may be used.

[0127] The polyimide-based resin of the present invention may include repeating units represented by the following chemical formula 3 or chemical formula 4.

[0128] [Chemical Formula 3]

[0129]

[0130] [Chemical Formula 4]

[0131]

[0132] Ar1 each independently, or And,

[0133] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2.

[0134] The polyimide-based resin of the present invention may include repeating units selected from the following chemical formulas 5 to 8.

[0135] [Chemical Formula 5]

[0136]

[0137] [Chemical Formula 6]

[0138]

[0139] [Chemical Formula 7]

[0140]

[0141] [Chemical Formula 8]

[0142]

[0143] X can be a single bond, -CH2-, -O-, -S-, -SO2-, -CO-, isopropylidene, hexafluoroisopropylidene, or a combination thereof, and

[0144] Ar1 and Ar2 are each independently or And,

[0145] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2.

[0146] y:z is 100:0 to 10:90. Also, y:z can be 90:10, or 80:20, or 70:30, or 60:40, or 50:50, or 40:60, or 30:70, or 20:80.

[0147] In one embodiment, Ar1 and Ar2 can each be independently selected from the following structure.

[0148]

[0149]

[0150]

[0151]

[0152]

[0153] In one embodiment, the polyimide-based resin of the present invention may include repeating units represented by the following chemical formulas 9 to 11, but is not limited thereto.

[0154] [Chemical Formula 9]

[0155]

[0156] [Chemical Formula 10]

[0157]

[0158] [Chemical Formula 11]

[0159]

[0160] A polyimide-based resin according to one embodiment of the present invention may include repeating units represented by the following chemical formula 12.

[0161] [Chemical Formula 12]

[0162]

[0163] Ar1 and Ar2 are each independently or And,

[0164] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0165] y:z is 100:0 to 10:90. Also, y:z can be 90:10, or 80:20, or 70:30, or 60:40, or 50:50, or 40:60, or 30:70, or 20:80.

[0166] In one embodiment, the number average molecular weight of the polyimide-based resin may be 10,000 to 200,000 g / mol. The lower limit may be 10,000 g / mol or more, or 20,000 g / mol or more, or 30,000 g / mol or more, or 50,000 g / mol or more, or 100,000 g / mol, or 150,000 g / mol or more. The upper limit may be 200,000 g / mol or less, or 180,000 g / mol or less, or 160,000 g / mol or less, or 130,000 g / mol or less, or 110,000 g / mol or less, or 900,000 g / mol or less. Or, it may be 10,000 to 200,000 g / mol, or 50,000 to 200,000 g / mol, or 80,000 to 200,000 g / mol.

[0167] A polyimide resin according to one embodiment of the present invention can be prepared by reacting a dianhydride compound represented by the following formula 1 with an aromatic diamine represented by formula 21; sequentially reacting a dianhydride compound represented by formula 23 with an aromatic diamine represented by formula 22; and imidizing to include a repeating unit represented by formula 5.

[0168] [Chemical Formula 1]

[0169]

[0170] [Chemical Formula 21]

[0171]

[0172] [Chemical Formula 22]

[0173]

[0174] [Chemical Formula 23]

[0175]

[0176] [Chemical Formula 5]

[0177]

[0178] X can be a single bond, -CH2-, -O-, -S-, -SO2-, -CO-, isopropylidene, hexafluoroisopropylidene, or a combination thereof, and

[0179] Ar1 and Ar2 are each independently or And,

[0180] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0181] y:z is 100:0 to 10:90. Also, y:z can be 90:10, or 80:20, or 70:30, or 60:40, or 50:50, or 40:60, or 30:70, or 20:80.

[0182] A polyimide-based resin according to one embodiment of the present invention can be prepared by reacting an acid anhydride compound represented by the following formula 2 with an aromatic diamine represented by formula 21; sequentially reacting the acid anhydride compound represented by formula 2 with an aromatic diamine represented by formula 22; and imidizing to include a repeating unit represented by formula 12.

[0183] [Chemical Formula 2]

[0184]

[0185] [Chemical Formula 21]

[0186]

[0187] [Chemical Formula 22]

[0188]

[0189] [Chemical Formula 12]

[0190]

[0191] Ar1 and Ar2 are each independently or And,

[0192] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0193] y:z is 100:0 to 10:90. Also, y:z can be 90:10, or 80:20, or 70:30, or 60:40, or 50:50, or 40:60, or 30:70, or 20:80.

[0194] A polyimide-based resin according to one embodiment of the present invention can be prepared by reacting a dianhydride compound represented by the following formula 1 with an aromatic diamine represented by formula 21; sequentially reacting an aromatic acyl chloride represented by formula 24 with an aromatic diamine represented by formula 22; and imidizing to include a repeating unit represented by formula 6.

[0195] [Chemical Formula 1]

[0196]

[0197] [Chemical Formula 21]

[0198]

[0199] [Chemical Formula 22]

[0200]

[0201] [Chemical Formula 24]

[0202]

[0203] [Chemical Formula 6]

[0204]

[0205] Ar1 and Ar2 are each independently or And,

[0206] L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, and c are each independently integers from 0 to 2;

[0207] y:z is 100:0 to 10:90. Also, y:z can be 90:10, or 80:20, or 70:30, or 60:40, or 50:50, or 40:60, or 30:70, or 20:80.

[0208] A composition for forming a polyimide-based film according to one embodiment of the present invention may include the polyimide-based resin described above.

[0209] In one embodiment, the composition for forming a polyimide-based film may further include an organic solvent. The organic solvent is a ketone such as gamma-butyrolactone, 1,3-dimethyl-2-imidazolidinone, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone; an aromatic hydrocarbon such as toluene, xylene, tetramethylbenzene; a glycol ether (cellosolve) such as ethylene glycol monoethyl ether, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; Acetates such as ethyl acetate, butyl acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol monomethyl ether acetate; alcohols such as methanol, ethanol, propanol, ethylene glycol, propylene glycol, carbitol; amides such as N,N-dimethylpropionamide (DMPA), N,N-diethylpropionamide (DEPA), N,N-dimethylacetamide (DMAc), N,N-diethylacetamide (DEAc), N,N-dimethylformamide (DMF), N,N-diethylformamide (DEF), N-methylpyrrolidone (NMP), N-ethylpyrrolidone (NEP), N,N-dimethylmethoxyacetamide; and one or more mixtures selected from the above, but are not limited thereto.

[0210] In one embodiment, the composition for forming a polyimide-based film may contain 5 to 50 weight% of a polyimide-based resin based on the total weight of the composition. Specifically, it may contain 10 to 50 weight%, or 10 to 40 weight%, or 20 to 50 weight%, or 20 to 40 weight%.

[0211] A polyimide-based film according to one embodiment of the present invention can be formed from the above-described film-forming composition.

[0212] The above polyimide-based film may have a thickness of 1 to 500 μm, or 1 to 100 μm, or 1 to 50 μm, or 1 to 20 μm.

[0213] In one embodiment, the polyimide-based film may have a glass transition temperature (Tg) of 400°C or higher. That is, the polyimide-based film of the present invention has excellent thermal stability, so that deformation does not occur even in high-temperature processes required for flexible devices, thereby minimizing the difference in expansion and contraction between heterogeneous materials. Specifically, the glass transition temperature (Tg) may be 400 to 480°C. In addition, the thermal decomposition temperature (Td) may be 480°C or higher.

[0214] In one embodiment, the polyimide-based film may have a coefficient of thermal expansion of 20 ppm / °C or less. Specifically, the coefficient of thermal expansion may be 15 ppm / °C or less, or 11 ppm / °C or less, more preferably 3 ppm / °C or less. Or it may be 1 to 15 ppm / °C, or 1 to 11 ppm / °C.

[0215] In one embodiment, the polyimide-based film may have a transmittance of 85% or more for a wavelength of 550 nm. The transmittance may be 85% to 99%, and specifically, it may be 85% or more, or 88% or more, or 89% or more, or 90% or more.

[0216] The polyimide-based film of the present invention is transparent and can have high heat resistance and a low coefficient of thermal expansion, so it is expected to be applicable as a flexible display device involved in high-temperature processes.

[0217] The above-described embodiment will be explained in more detail below through examples. However, the following examples are for illustrative purposes only and are not intended to limit the scope of the rights.

[0218] [Methods for Measuring Physical Properties]

[0219] (1) Number average molecular weight

[0220] Measurements were performed using gel permeation chromatography (GPC). A PLgel MIXED-B 10 µm column, polystyrene as the standard sample, and tetrahydrofuran (THF) as the solvent were used. Under conditions of a temperature of 30 ℃ and a flow rate of 1.0 mL / min, samples were prepared at a concentration of 5 mg / 10 mL and supplied in a volume of 200 µl for measurement.

[0221] (2) Yellowness

[0222] It was measured according to ASTM D1925 standards.

[0223] (3) Cut-off wavelength

[0224] Transmittance was measured according to ASTM D1003 standards, and the wavelength at which transmittance begins to appear was set as the cutoff wavelength (λ0) of each film.

[0225] (4) Transmittance

[0226] Transmittance (T550nm) at a wavelength of 550 nm was measured according to ASTM D1003 standards.

[0227] (5) Thermal decomposition temperature (Td, 5%)

[0228] Thermogravimetric analysis (TA instruments, TGA Q50) was used. Measurement conditions were set at a temperature range from room temperature to 800°C, a heating rate of 5°C / min, and a pressure of 1.5 bar / min under nitrogen gas injection, and the temperature at which a 5% mass loss occurs was defined as the thermal decomposition temperature (Td, 5%).

[0229] (6) Glass transition temperature (Tg)

[0230] Using Isothermal Differential Scanning Calorimetry (TA instruments, DSC Q20), the second value was measured by heating and cooling from 0℃ to 400℃ at a rate of 10℃ / min.

[0231] (7) Coefficient of Thermal Expansion (CTE)

[0232] It was measured using a thermomechanical analyzer (TA instruments, TMA-Q400). The expansion rate was measured by averaging under conditions of a temperature range from room temperature to 450℃ with a load of 0.01N and a heating rate of 5℃ / min.

[0233] [Preparation Example 1] Preparation of a dianhydride compound

[0234] <Reaction Equation 1>

[0235]

[0236] 4-bromo-1,2-xylene (6.00 g, 32.4 mmol), 3,4-dimethylphenol (4.99 g, 40.8 mmol), iron(III) acetylacetonate (Fe(acac)3) (2.22 g, 6.29 mmol), potassium carbonate (11.30 g, 81.8 mmol), copper(I) iodide (1.20 g, 6.30 mmol), and dimethylformamide (DMF, 60.0 ml) were added to a three-necked round-bottom flask to obtain a reaction solution, which was stirred at 135°C for 12 hours. The reaction mixture was filtered through filter paper, washed with brine, extracted with hexane, and dried with anhydrous magnesium sulfate. The mixture was purified by silica gel column chromatography using dichloromethane (MC) / hexane (v / v=1 / 5) as the developing agent and dried under reduced pressure to obtain the final product D-1, a white solid powder (4.80 g, 66%).

[0237] A three-necked round-bottom flask containing aluminum chloride (2.82 g, 21.2 mmol), thionyl chloride (3.03 g, 25.5 mmol), and anhydrous dichloromethane (MC, 105 ml) was placed in an ice water bath and cooled. Compound D-1 (4.80 g, 21.2 mmol) was dissolved in MC and slowly poured into the flask containing the mixture under a nitrogen flow. The reaction mixture was stirred under a nitrogen flow at 0°C for 1 hour, after which the reaction mixture was washed with ice water and the organic layer was dried with anhydrous magnesium sulfate. The mixture was purified by silica gel column chromatography using dichloromethane (MC) / hexane (v / v=1:20) as the developing agent and dried under reduced pressure to obtain product D-2, a white solid powder (1.18 g, 20.5%). 1 1H NMR (400 MHz, acetone-d 6 , 25℃, ppm): δ 6.90 (s, 1H), 6.81 (s, 1H), 2.19 (s, 3H), 2.16 (s, 3H). (Refer to Figs. 1 and 2).

[0238] A solution of potassium permanganate (42.5 g, 268.8 mmol) dissolved in distilled water (48 ml) was added to a three-necked round-bottom flask containing compound D-2 (6.60 g, 24.3 mmol) and pyridine (260 ml) in six equal portions at 30-minute intervals, while the temperature was raised each time until it finally reached 90°C. The reaction mixture was stirred at 90°C for 15 hours. After filtering the reaction mixture through filter paper, it was washed with hot water / pyridine (v / v=3:1), and the filtrate was concentrated under reduced pressure. The resulting product was placed in the same round-bottom flask, sodium hydroxide (4.88 g, 122.0 mmol), potassium permanganate (42.5 g, 268.8 mmol), and distilled water (170 ml) were added, and the reaction mixture was refluxed for 3 hours. Methanol was added to the reaction mixture to terminate the reaction, and the mixture was filtered through filter paper. The solid product obtained by acidifying the filtrate with sulfuric acid was then filtered. The final product was dried under reduced pressure to obtain a white solid powder product D-3 (4.30 g, 43.1%). 1 ¹H NMR (400 MHz, DMSO- d 6 , 25℃, ppm): δ 8.40 (s, 1H), 7.87 (s, 1H). (Refer to Figs. 3 and 4).

[0239] Compound D-3 (2.45 g, 6.0 mmol) and acetic anhydride (25.0 ml) were placed in a round-bottom flask and stirred at 85°C for 6 hours. After filtering the reaction mixture, it was washed with acetic anhydride and toluene and dried under reduced pressure to obtain dianhydride compound 1, a white solid powder (2.0 g, 89.6%). 1 1H NMR (400 MHz, acetone-d 6 , 25℃, ppm): δ 8.86 (s, 1H), 8.39 (s, 1H). (Refer to Figs. 5 and 6)

[0240] [Preparation Example 2] Preparation of an acid anhydride compound

[0241] <Reaction Equation 2>

[0242]

[0243] 4-bromo-1,2-xylene (6.00 g, 32.4 mmol), 3-ethylphenol (4.98 g, 40.8 mmol), iron(III) acetylacetonate (Fe(acac)3) (2.22 g, 6.29 mmol), potassium carbonate (11.30 g, 81.8 mmol), copper(I) iodide (1.20 g, 6.30 mmol), and dimethylformamide (DMF, 60.0 ml) were added to a three-necked round-bottom flask to obtain a reaction solution, which was stirred at 135°C for 12 hours. The reaction mixture was filtered through filter paper, washed with brine, extracted with hexane, and dried with anhydrous magnesium sulfate. The mixture was purified by silica gel column chromatography using dichloromethane (MC) / hexane (v / v=1 / 5) as the developing agent and dried under reduced pressure to obtain the final product E-1, a white solid powder (4.60 g, 63%).

[0244] A three-necked round-bottom flask containing aluminum chloride (2.82 g, 21.2 mmol), thionyl chloride (3.03 g, 25.5 mmol), and anhydrous dichloromethane (MC, 105 ml) was placed in an ice water bath and cooled. Compound E-1 (4.60 g, 20.3 mmol) was dissolved in MC and slowly poured into the flask containing the mixture under a nitrogen flow. The reaction mixture was stirred at 0°C for 1 hour, after which the reaction mixture was washed with ice water and the organic layer was dried with anhydrous magnesium sulfate. The mixture was purified by silica gel column chromatography using dichloromethane (MC) / hexane (v / v=1:20) as the developing agent and dried under reduced pressure to obtain product E-2, a white solid powder (1.35 g, 24.4%).

[0245] A solution of potassium permanganate (32.0 g, 202.8 mmol) dissolved in distilled water (48 ml) was added to a three-necked round-bottom flask containing compound E-2 (4.6 g, 16.9 mmol) and pyridine (240 ml) in six equal portions at 30-minute intervals, while the temperature was raised each time until it finally reached 90°C. The reaction mixture was stirred at 90°C for 12 hours. After filtering the reaction mixture through filter paper, it was washed with hot water / pyridine (v / v=3:1), and the filtrate was concentrated under reduced pressure. The resulting product was placed in the same round-bottom flask, sodium hydroxide (4.0 g, 100 mmol), potassium permanganate (32.0 g, 202.8 mmol), and distilled water (150 ml) were added, and the reaction mixture was refluxed for 3 hours. Methanol was added to the reaction mixture to terminate the reaction, filtered through filter paper, and the solid product obtained by acidifying the filtrate with sulfuric acid was filtered. The final product was dried under reduced pressure to obtain a white solid powder product E-3 (3.30 g, 53.6%). Compound E-3 was vacuum sublimated at 200°C to obtain acid anhydride compound 2.

[0246] [Example 1] Preparation of Polyimide Resin (PI-1)

[0247] <Reaction Equation 3>

[0248]

[0249] A 10 wt% solution was prepared by adding dianhydride compound 1 (2.40 g, 6.45 mmol), diamine monomer 2,2'-bis(trifluoromethyl)benzidine (TFMB) (2.06 g, 6.44 mmol), and 45 mL of N-methyl-2-pyrrolidone (NMP) to a three-necked round-bottom flask. A nitrogen inlet, an outlet, and a mechanical stirrer were connected to the round-bottom flask, and the prepared solution was reacted by stirring at room temperature for 24 hours to produce polyamic acid. After applying 1 mL of the prepared polyamic acid solution onto a glass substrate, an imidization reaction was carried out in a vacuum oven at 60°C for 4 hours, 110°C for 24 hours, and 350°C for 2 hours, respectively, to prepare a polyimide film (PI-1). Fig. 7 is the NMR spectrum of the polyamic acid prepared according to Example 1. Fig. 8 is the FT-IR spectrum of the polyimide film prepared according to Example 1. Fig. 9 is a thermogravimetric analysis graph of the polyamide film (PI-1) prepared in Example 1 in a nitrogen environment (N2) and an air environment. Fig. 10 is a differential scanning calorimetry analysis graph of the polyimide film (PI-1) prepared in Example 1. The prepared polyimide film was measured using the physical property measurement method described above and is shown in Table 1 below.

[0250] [Example 2] Preparation of Polyimide Resin (PI-2)

[0251] <Reaction Equation 4>

[0252]

[0253] A 10 wt% solution was prepared by adding dianhydride compound 1 (2.223 g, 5.80 mmol), 2,2-bis(4-aminophenyl)hexafluoropropane (6FDA) (0.286 g, 0.644 mmol), the diamine monomer 2,2'-bis(trifluoromethyl)benzidine (TFMB) (2.06 g, 6.44 mmol), and 45 mL of N-methyl-2-pyrrolidone (NMP) to a three-necked round-bottom flask. A nitrogen inlet, an outlet, and a mechanical stirrer were connected to the round-bottom flask, and the prepared solution was reacted by stirring at room temperature for 24 hours to produce a polyamic acid (a:b = 9:1). After applying 1 mL of the prepared polyamic acid solution onto a glass substrate, an imidization reaction was carried out in a vacuum oven at 60°C for 4 hours, 110°C for 24 hours, and 350°C for 2 hours, respectively, to prepare a polyimide film (PI-2). The properties of the prepared polyimide film were measured using the method described above and are shown in Table 1 below.

[0254] [Example 3] Preparation of Polyimide Resin (PI-3)

[0255] A 10 wt% solution was prepared by adding dianhydride compound 1 (1.917 g, 5.152 mmol), 2,2-bis(4-aminophenyl)hexafluoropropane (6FDA) (0.572 g, 1.288 mmol), diamine monomer 2,2'-bis(trifluoromethyl)benzidine (TFMB) (2.06 g, 6.44 mmol), and 45 mL of N-methyl-2-pyrrolidone (NMP) to a three-necked round-bottom flask (a:b = 8:2). A polyimide film was prepared in the same manner as in Example 2 (PI-3). Figure 11 is an image of the polyimide film prepared in Example 3. The manufactured polyimide film was measured using the physical property measurement method described above and is shown in Table 1 below.

[0256] [Table 1]

[0257]

[0258] λ 0 Cutoff wavelength, the wavelength at which the film begins to exhibit transmittance.

[0259] T550nm: Transmittance of the film at 550nm

[0260] Td5: Temperature at which the film weight decreased by 5% according to thermogravimetric analysis results

[0261] Tg: Glass transition temperature, not observed in differential scanning calorimetry

[0262] CTE: Coefficient of Thermal Expansion

[0263] As shown in Table 1 above, it was confirmed that the polyimide-based film of the present invention has high transmittance and low yellowness for wavelengths in the visible light region and transmits light over a wide wavelength range. In addition, it was found that it has a high thermal decomposition temperature under both nitrogen and air conditions, exhibiting excellent heat resistance without being affected by high-temperature environments, and has a low coefficient of thermal expansion of 20 ppm / ℃ or less.

[0264] Referring to FIGS. 9 and 10, the glass transition temperature (Tg) of Example 1 is 400°C or higher, and no decomposition occurs even at high temperatures exceeding 400°C. Additionally, referring to FIG. 11, the polyimide-based film of the present invention is transparent, so it can be seen that the logo at the bottom of the film is clearly visible.

[0265] That is, the polyimide-based film of the present invention is not only colorless and transparent, but also does not undergo deformation even during high-temperature processes, thereby minimizing the difference in expansion and contraction between heterogeneous materials. Therefore, the polyimide-based film of the present invention is expected to be usefully applied as a flexible display device.

[0266] As described above, the present invention has been explained by specific details and limited embodiments; however, this is provided merely to aid in a more comprehensive understanding of the invention, and the invention is not limited to the above embodiments. Those skilled in the art can make various modifications and variations from this description.

[0267] Accordingly, the scope of the present invention is not limited to the described embodiments, and all things equivalent to or having equivalent variations to the claims set forth below, as well as the claims set forth below, shall be considered to fall within the scope of the concept of the present invention.

Claims

Claim 1 A polyimide resin comprising repeating units represented by the following chemical formula 3. [Chemical Formula 3] Ar1 is L is a single bond, R2 and R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy or halo(C1-C7)alkyl, b is 1 to 2, and c is an integer from 0 to 2. Claim 2 The polyimide resin according to claim 1, comprising a repeating unit represented by the above chemical formula 3, is a polyimide resin comprising a repeating unit selected from the following chemical formulas 5 to 8. [Chemical Formula 5] [Chemical Formula 6] [Chemical Formula 7] [Chemical Formula 8] X may be a single bond, -CH2-, -O-, -S-, -SO2-, -CO-, isopropylidene, hexafluoroisopropylidene, or a combination thereof, Ar1 is identical to the definition in Claim 1, and Ar2 are each independently or And, L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, a, b, c are each independently integers from 0 to 2, and y:z is 100:0 to 10:

90. Claim 3 In paragraph 2, the above Ar1 and Ar2 are each independently selected from the following structures, polyimide-based resins. Claim 4 In paragraph 3, the polyimide resin is a polyimide resin comprising a repeating unit represented by the following chemical formula 9. [Chemical Formula 9] Claim 5 delete Claim 6 A polyimide resin according to claim 1, wherein the number average molecular weight of the polyimide resin is 10,000 to 200,000 g / mol. Claim 7 A method for producing a polyimide-based resin comprising a repeating unit represented by Chemical Formula 5, wherein the dianhydride compound represented by Chemical Formula 1 below is reacted with an aromatic diamine represented by Chemical Formula 21; the dianhydride compound represented by Chemical Formula 23 is reacted sequentially with an aromatic diamine represented by Chemical Formula 22; and the mixture is imidized. [Chemical Formula 1] [Chemical Formula 21] [Chemical Formula 22] [Chemical Formula 23] [Chemical Formula 5] X may be a single bond, -CH2-, -O-, -S-, -SO2-, -CO-, isopropylidene, hexafluoroisopropylidene, or a combination thereof, Ar1 is the same as the definition in claim 1, and Ar2 is or And, L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, c are each independently integers from 0 to 2; and y:z is 100:0 to 10:

90. Claim 8 delete Claim 9 A method for preparing a polyimide-based resin comprising a repeating unit represented by Chemical Formula 6, wherein a dianhydride compound represented by Chemical Formula 1 below is reacted with an aromatic diamine represented by Chemical Formula 21; an aromatic acyl chloride represented by Chemical Formula 24 is reacted sequentially with an aromatic diamine represented by Chemical Formula 22; and imidized. [Chemical Formula 1] [Chemical Formula 21] [Chemical Formula 22] [Chemical Formula 24] [Chemical Formula 6] Ar1 and Ar2 are each independently or And, L may be a single bond, -O-, -S-, -SO2-, (C1-C7)alkylene, (C6-C12)arylene, or a combination thereof, and the arylene and alkylene of L may be further substituted with one or more selected from (C1-C7)alkyl and halo(C1-C7)alkyl; R1, R2, R3 are each independently (C1-C7)alkyl, (C1-C7)alkoxy, or halo(C1-C7)alkyl, and a, b, c are each independently integers from 0 to 2; and y:z is 100:0 to 10:

90. Claim 10 A polyimide-based film-forming composition comprising: a polyimide-based resin selected from any one of claims 1 to 4 and 6; or a polyimide-based resin produced by a method for producing a polyimide-based resin selected from any one of claims 7 and 9. Claim 11 In claim 10, the polyimide-based film-forming composition further comprises an organic solvent. Claim 12 In claim 10, the polyimide-based film-forming composition comprises 5 to 50 weight% of a polyimide-based resin based on the total weight of the composition. Claim 13 A polyimide film formed from a polyimide film-forming composition according to claim 10. Claim 14 In claim 13, the polyimide-based film is a polyimide-based film having a glass transition temperature (Tg) of 400°C or higher. Claim 15 In Clause 13, the polyimide-based film is a polyimide-based film having a coefficient of thermal expansion of 20 ppm / ℃ or less. Claim 16 In claim 13, the polyimide-based film is a polyimide-based film having a transmittance of 85% or more for a wavelength of 550 nm. Claim 17 A flexible display device comprising the polyimide-based film of claim 13. Claim 18 delete Claim 19 A method for manufacturing a polyimide resin according to claim 7, wherein the dianhydride compound represented by Chemical Formula 1 is prepared by oxidizing a precursor represented by Chemical Formula 25 in the presence of an oxidizing agent. [Chemical Formula 25] Claim 20 delete

Citation Information

Patent Citations

  • Photosensitive Resin Composition, Patterning Method,and Electronic Components

    KR1020010030466A

  • Acid anhydride compound, polyamideimide resin and film using the same

    KR1020240117279A