Dispersant, conductive slurry, and preparation method thereof and use thereof

A dispersant with polyester and polyaniline chain segments addresses aggregation issues in carbon nanomaterials, achieving low viscosity and high solid content in conductive slurry for improved lithium-ion battery performance.

KR103045174B1Active Publication Date: 2026-11-06안후이 하오페이 뉴 머티리얼 컴퍼니 리미티드 +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020267004261
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-08-30
Filing Date
2023-12-26
Publication Date
2026-11-06
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

One-dimensional and two-dimensional carbon nanomaterials in conductive slurry are prone to aggregation and poor dispersion during the grinding and dispersion process in organic solvents, leading to high viscosity and limited conductive performance.

Method used

A dispersant comprising compounds with a structure represented by Formula I, containing polyester and polyaniline chain segments, is used to adsorb conductive agents, preventing aggregation and improving dispersibility, resulting in a conductive slurry with low viscosity and high solid content.

Benefits of technology

The dispersant effectively prevents aggregation and enhances dispersibility, allowing for a conductive slurry with high electrical conductivity and suitable for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112026017325729-PCT00001
    Figure 112026017325729-PCT00001
  • Figure 112026017325729-PCT00002
    Figure 112026017325729-PCT00002
  • Figure 112026017325729-PCT00003
    Figure 112026017325729-PCT00003
Patent Text Reader

Abstract

The present invention provides a dispersant, a conductive slurry, a method for manufacturing the same, and applications thereof. The dispersant comprises one or at least a combination of two compounds having a structure represented by Formula I. The compound having a structure represented by Formula I described above includes both polyester chain segments and polyaniline chain segments. Since it not only acts as a strong adsorbent for the conductive agent but also has excellent affinity for organic solvents, it can effectively prevent the aggregation of the conductive agent in organic solvents and improve the dispersibility of the conductive agent in organic solvents, thereby enabling the resulting conductive slurry to have high electrical conductivity, low viscosity, and high solid content simultaneously, making it suitable for applications in lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention belongs to the field of conductive slurry technology, and specifically relates to a dispersant, a conductive slurry, and a method for manufacturing the same and its application.

[0002] This application claims priority to the Chinese patent application No. 202311106920.7, filed with the Chinese Intellectual Property Office on August 30, 2023, titled "Dispersant, conductive slurry and method of manufacturing and application thereof," all of which are incorporated by reference into this application. Background Technology

[0003] As people's awareness of environmental protection continues to deepen, new energy batteries are becoming increasingly widely used in automobiles, energy storage, and electronic devices. Conductive agents are a critical component of new energy batteries, and their performance directly affects the battery's electrical performance.

[0004] Currently, general conductive agents can be classified into zero-dimensional carbon nanomaterials, one-dimensional carbon nanomaterials, and two-dimensional carbon nanomaterials depending on their form; here, one-dimensional and two-dimensional carbon nanomaterials are increasingly becoming major research subjects for researchers because they possess excellent conductive performance. CN113327700A disclosed a low-viscosity, high-conductivity carbon nanotube conductive slurry, a method for manufacturing the same, and applications, wherein the carbon nanotube conductive slurry comprises a composition of 10 to 30 parts by weight of carbon nanotubes, 2 to 10 parts by weight of a dispersant, and 400 to 750 parts by weight of an organic solvent; and the dispersant comprises a combination of polyvinylpyrrolidone and a hydroxyalkylammonium salt polymer. The manufacturing method comprises: (1) a step of mixing carbon nanotubes, a dispersant, and an organic solvent to obtain a mixture; and (2) a step of continuously mixing the mixture obtained in step (1) to obtain the array carbon nanotube conductive slurry; The carbon nanotube conductive slurry provided in the invention has excellent conductivity, low viscosity, and excellent storage stability, and is applied in the field of lithium-ion batteries.

[0005] However, 1D carbon nanomaterials and 2D carbon nanomaterials are prone to problems such as aggregation and poor dispersion during the grinding and dispersion process in organic solvents, which affects the conductivity of the conductive slurry. Generally, a dispersant must be added to disperse them. Commonly used dispersants include polyvinylpyrrolidone (PVP) and polyvinylidene fluoride (PVDF). Although these types of dispersants have improved the dispersion performance of 1D carbon nanomaterials and 2D carbon nanomaterials in organic solvents, the viscosity of the resulting conductive slurry is high, making it impossible to produce a conductive slurry with a high content of conductive agent, thereby limiting the improvement of the conductive performance of the conductive slurry.

[0006] Therefore, in order to solve the aforementioned technical problems, it is urgent to develop a dispersant that can effectively improve the dispersion performance of the conductive slurry. The problem to be solved

[0007] Taking into account the disadvantages of the prior art, the objective of the present invention is to provide a dispersant, a conductive slurry, and a method for manufacturing the same and an application thereof. The dispersant comprises a compound having a structure represented by Formula I, and the structural formula of the compound described above includes polyester chain segments and polyaniline chain segments, which act as a strong adsorption agent for the conductive agent and have excellent affinity for organic solvents, thereby effectively preventing the aggregation of the conductive agent in the organic solvent and improving the dispersibility of the conductive agent in the organic solvent, so that the resulting conductive slurry has low viscosity and high solid content simultaneously. means of solving the problem

[0008] To achieve this objective, the present invention uses the following technical method.

[0009] In a first aspect, the present invention provides a dispersant, said dispersant comprising any one or at least a combination of two compounds having a structure represented by the chemical formula I;

[0010] [Equation 1]

[0011]

[0012] Here, R is selected from alkyl groups, m is selected from integers between 1 and 500, and n is selected from integers between 1 and 10.

[0013] Here, the above m may be 20, 30, 40, 50, 60, 70, 80, 90, 100, 150, 200, 250, 300, 350, 400, or 450, etc.

[0014] The above n can be 2, 4, 6, 8, or 10, etc.

[0015] The dispersant provided in the present invention comprises one or at least a combination of two compounds having a structure represented by Formula I, wherein the compound having a structure represented by Formula I described above comprises a polyester structure unit and a polyaniline structure unit, wherein the polyaniline structure unit acts as a strong surface adsorption for the conductive agent, thereby adsorbing the conductive agent onto the surface of a material, and the polyester structure unit belongs to a solvation long chain and has a strong dispersion function and excellent affinity for organic solvents, so that the conductive agent adsorbed on the surface of the material effectively prevents aggregation, thereby effectively improving the dispersibility of the conductive agent in the organic solvent, so that the resulting conductive slurry can simultaneously have a high solid content and low viscosity.

[0016] It should be noted that the present invention does not specifically limit the method for manufacturing a compound having a structure represented by the provided formula I, and may, by way of example, be manufactured as follows, and said method specifically comprises the following steps.

[0017] (1) Terephthalic acid and ethylene glycol are reacted under conditions in the presence of a catalyst, and R-OH is added dropwise to end-capping to obtain a polyester; wherein R is selected from alkyl groups;

[0018] N-phenyl-1,4-p-phenylenediamine produces aniline oligomers under the oxidation of trivalent iron ions;

[0019] (2) The polyester obtained in step (1) is reacted with the aniline oligomer to obtain a compound having the structure represented by the above formula I.

[0020] Preferably, the molar ratio of terephthalic acid to ethylene glycol in step (1) is 1:(1.002 to 1.05), for example 1:1.005, 1:1.007, 1:1.01, 1:1.02, 1:1.03 or 1:1.04, etc.

[0021] Preferably, the catalyst in step (1) contains paramethylbenzenesulfonic acid.

[0022] Preferably, based on 100% of the amount of terephthalic acid used in step (1), the amount of catalyst used in step (1) is 0.1 to 2%, for example 0.2%, 0.4%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, or 1.8%, etc.

[0023] Preferably, the amount of R-OH used in step (1) is the difference in the number of moles of terephthalic acid more than ethylene glycol.

[0024] Preferably, the above-described step (1) specifically comprises adding terephthalic acid and ethylene glycol to a reactor, adding a catalyst, heating to 120 to 140°C (e.g., 122°C, 124°C, 126°C, 128°C, 130°C, 132°C, 134°C, 136°C, or 138°C, etc.) in a steam bath, reacting for 1 to 4 hours (e.g., 1.5 hours, 2 hours, 2.5 hours, 3 hours, or 3.5 hours, etc.), collecting the effluent liquid under nitrogen protection, raising the temperature to 160 to 195°C (e.g., 165°C, 170°C, 175°C, 180°C, 185°C, or 190°C, etc.), slowly adding R-OH dropwise to end cap, and obtaining the polyester.

[0025] Preferably, the above step (2) specifically comprises dissolving N-phenyl-1,4-p-phenylenediamine in ether, then slowly adding it dropwise to hydrochloric acid at a concentration of 0.5 to 3 mol / L (e.g., 1 mol / L, 1.5 mol / L, 2 mol / L, or 2.5 mol / L), and mechanically stirring for 1 to 5 h (e.g., 2 h, 3 h, or 4 h, etc.) to obtain a reaction solution, then adding a hydrochloric acid solution containing iron trichloride dropwise to the above reaction solution, continuing to stir for 1 to 5 h (e.g., 2 h, 3 h, or 4 h, etc.), then washing the precipitated solid three times with hydrochloric acid, then washing it once with ammonia water, finally reducing it to hydrazine hydrate, and then suction filtration to obtain the aniline oligomer.

[0026] Preferably, the above-described step (3) specifically comprises dissolving a polyester in dimethyl sulfoxide (DMSO), adding thionyl chloride and refluxing, reacting at 60 to 80°C (e.g., 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, or 78°C, etc.) for 1 to 3 hours (e.g., 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, or 2.8 hours, etc.), then distilling the thionyl chloride under reduced pressure, finally adding petroleum ether to precipitate the product, and then separating and drying to obtain a treated polyester; The above-described treated polyester and aniline oligomer are dissolved in DMSO, heated to 170–190°C (e.g., 172°C, 174°C, 176°C, 178°C, 180°C, 182°C, 184°C, 186°C, or 188°C, etc.) and reacted for 2–4 hours (e.g., 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours, 3 hours, 3.2 hours, 3.4 hours, 3.6 hours, or 3.8 hours, etc.), after which the product is discharged with distilled water and washed several times to obtain a compound having a structure represented by Formula I.

[0027] Preferably, R is selected from C1 to C20 alkyl groups, such as alkyl groups of C2, C3, C4, C5, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, or C19, and more preferably is a C1 to C5 alkyl group.

[0028] Preferably, the m is selected from an integer between 10 and 100.

[0029] Preferably, the above n is selected from an integer between 4 and 10.

[0030] In a second aspect, the present invention provides a conductive slurry, said conductive slurry comprising a dispersant, a conductive agent, and a solvent according to a first aspect.

[0031] The conductive slurry provided in the present invention can be dispersed by adding a dispersant according to the first aspect, thereby reducing the processing difficulties of the conductive slurry while increasing the solid content of the obtained conductive slurry.

[0032] Preferably, the conductive agent comprises carbon nanotubes and / or graphene.

[0033] Here, the carbon nanotubes can be selected from powder provided by Tiannai Technology, and the graphene can be selected from powder provided by Nanjing Xianfeng Nano.

[0034] Preferably, the mass percentage of the conductive agent in the conductive slurry is 18 to 30%, for example 19%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, or 29%, etc.

[0035] Preferably, the solvent is an organic solvent.

[0036] Preferably, the organic solvent comprises N-methylpyrrolidone (NMP).

[0037] Preferably, the mass percentage of the organic solvent in the conductive slurry is 65 to 80%, for example 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 76%, or 78%, etc.

[0038] Preferably, the mass percentage of the dispersant according to the first aspect in the conductive slurry is 2 to 6%, for example 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or 5.5%, etc.

[0039] As a preferred technical solution of the present invention, by additionally limiting the mass percentage of the dispersant in the conductive slurry to 2 to 6%, the obtained conductive slurry can be made to have an excellent dispersion effect, and when subsequently applied to a lithium-ion battery, the battery can be made to have a high capacity. If the mass percentage of the dispersant in the conductive slurry is less than 2%, the dispersibility of the conductive slurry is reduced, the viscosity is increased, and the processing performance is poor. If the mass percentage of the dispersant in the conductive slurry exceeds 6%, on the one hand, the role of enhancing the dispersion effect of the conductive slurry is not significant, and on the other hand, when the conductive slurry is applied to a battery, it results in a reduction of the battery's capacity.

[0040] Preferably, the mass ratio of the dispersant to the conductive agent is 1:(4 to 10), for example 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:85, 1:9, or 1:1.95, and more preferably 1:(4 to 6).

[0041] Preferably, the conductive slurry further comprises another dispersant, and the other dispersant comprises polyvinylpyrrolidone and / or polyvinylidene fluoride.

[0042] As a preferred technical solution of the present invention, the conductive slurry provided in the present invention may be used for dispersion together with the dispersant according to the first aspect by adding another dispersant.

[0043] In a third aspect, the present invention provides a method for preparing a conductive slurry according to a second aspect, comprising the step of mixing a dispersant according to a first aspect, a conductive agent, a solvent, and any other dispersant to obtain the conductive slurry.

[0044] In a fourth aspect, the present invention provides an anode slurry comprising a conductive slurry according to the second aspect.

[0045] In a fifth aspect, the present invention provides an application of a conductive slurry according to the second aspect in a lithium-ion battery. Effects of the invention

[0046] The present invention has the following advantageous effects compared to the prior art.

[0047] The dispersant provided in the present invention comprises one or at least a combination of two compounds having a structure represented by Formula I. The compound having a structure represented by Formula I described above includes both polyester chain segments and polyaniline chain segments, and not only performs a strong adsorption role for conductive agents but also has excellent affinity for organic solvents. Therefore, it can effectively prevent aggregation of conductive agents in organic solvents and improve the dispersibility of conductive agents in organic solvents, so that the resulting conductive slurry has high electrical conductivity and can simultaneously have low viscosity and high solid content, making it suitable for application in lithium-ion batteries. Specific details for implementing the invention

[0048] The technical solution of the present invention is further explained below through specific embodiments. Those skilled in the art will understand that the described embodiments are merely for the purpose of assisting in understanding the present invention and should not be construed as specific limitations on the present invention.

[0049] Example 1

[0050] In the case of dispersant M1, the specific structural formula is as follows, and

[0051]

[0052] The method for manufacturing dispersant M1 provided in this embodiment includes the following steps.

[0053] (1) 6.207 g of ethylene glycol and 17.444 g of terephthalic acid were added to a reactor, followed by the addition of 0.1744 g of paramethylbenzenesulfonic acid, heated to 130°C in a steam bath, and reacted for 90 minutes. After collecting the effluent under nitrogen protection, the temperature was raised to 180°C, and 0.16 g of methanol was slowly added dropwise and end-capped to obtain a polyester;

[0054] 9.2 g of N-phenyl-1,4-p-phenylenediamine monomer is dissolved in 100 mL of anhydrous ether, slowly added dropwise to 1000 mL of hydrochloric acid at a concentration of 1 mol / L, and mechanically stirred for 4 hours to obtain a reaction solution; 14 g of iron chloride hexahydrate is dissolved in 150 mL of hydrochloric acid at a concentration of 1 mol / L, the obtained hydrochloric acid solution containing iron trichloride is slowly added dropwise to the above-described reaction solution, stirred continuously for 4 hours, and obtained a solid by suction filtration; the obtained solid is washed three times with hydrochloric acid at a concentration of 1 mol / L, then washed once with ammonia water at a concentration of 1 mol / L, finally reduced with hydrazine hydrate, and obtained a crude product by suction filtration; the crude product is vacuum dried for 72 hours to obtain an aniline oligomer;

[0055] (2) Dissolve the polyester obtained in step (1) of 22g in 120mL of DMSO, add 6mL of thionyl chloride, heat to 70℃ and react for 2h, then distill the thionyl chloride under reduced pressure, then put the solution into petroleum ether, filter and dry the precipitate to obtain the treated polyester;

[0056] (3) The treated polyester obtained in step (2) of 9.558 g and the aniline oligomer obtained in step (1) of 1.458 g are dissolved in 40 mL of DMSO, heated to 180°C and reacted for 3 hours, then the product is discharged with distilled water and washed five times to obtain the dispersant M1.

[0057] Characterized data:

[0058] The dispersant M1 provided in this embodiment was tested using a nuclear magnetic resonance spectrometer (Varian-300), and the H-NMR nuclear magnetic spectrum obtained from the test showed a single peak at 8.4 ppm, proving that an amide bond was formed; the dispersant M1 provided in this embodiment was tested using a Fourier infrared spectrometer, and the infrared spectrum obtained from the test showed at 1400 cm⁻¹ -1 A new peak appeared at [location], which is the carbon-nitrogen stretching peak of the amide bond. All of the above results prove that dispersant M1 having the specific structure described in Example 1 was successfully synthesized.

[0059] Example 2

[0060] In the case of dispersant M2, the specific structural formula is as follows, and

[0061]

[0062] The method for manufacturing dispersant M2 provided in this embodiment includes the following steps.

[0063] (1) 6.207 g of ethylene glycol and 18.274 g of terephthalic acid were added to a reactor, followed by the addition of 0.1827 g of paramethylbenzenesulfonic acid, heated to 130°C in a steam bath, and reacted for 90 minutes. After collecting the effluent under nitrogen protection, the temperature was raised to 180°C, and 0.32 g of methanol was slowly added dropwise and end-capped to obtain a polyester;

[0064] 9.2 g of N-phenyl-1,4-p-phenylenediamine monomer is dissolved in 100 mL of anhydrous ether, slowly added dropwise to 1000 mL of hydrochloric acid at a concentration of 1 mol / L, and mechanically stirred for 4 hours to obtain a reaction solution; 14 g of iron chloride hexahydrate is dissolved in 150 mL of hydrochloric acid at a concentration of 1 mol / L, the obtained hydrochloric acid solution containing iron trichloride is slowly added dropwise to the above-described reaction solution, stirred continuously for 4 hours, and obtained a solid by suction filtration; the obtained solid is washed three times with hydrochloric acid at a concentration of 1 mol / L, then washed once with ammonia water at a concentration of 1 mol / L, finally reduced with hydrazine hydrate, and obtained a crude product by suction filtration; the crude product is vacuum dried for 72 hours to obtain an aniline oligomer;

[0065] (2) Dissolve the polyester obtained in step (1) of 22g in 120mL of DMSO, add 6mL of thionyl chloride, heat to 70℃ and react for 2h, then distill the thionyl chloride under reduced pressure, then put the solution into petroleum ether, filter and dry the precipitate to obtain the treated polyester;

[0066] (3) The treated polyester obtained in step (2) of 5.806 g and the aniline oligomer obtained in step (1) of 3.6416 g are dissolved in 32 mL of DMSO, heated to 180°C and reacted for 3 hours, then the product is discharged with distilled water and washed five times to obtain the dispersant M2.

[0067] Characterized data :

[0068] The dispersant M2 provided in this embodiment was tested using a nuclear magnetic resonance spectrometer (Varian-300), and the H-NMR nuclear magnetic spectrum obtained from the test showed a single peak at 8.4 ppm, proving that an amide bond was formed; the dispersant M2 provided in this embodiment was tested using a Fourier infrared spectrometer, and the infrared spectrum obtained from the test showed at 1400 cm⁻¹-1 A new peak appeared at [location], which is the carbon-nitrogen stretching peak of the amide bond. All of the above results prove that dispersant M2 having the specific structure described in Example 2 was successfully synthesized.

[0069] Example 3

[0070] In the case of dispersant M3, the specific structural formula is as follows, and

[0071]

[0072] The method for manufacturing dispersant M3 provided in this embodiment includes the following steps.

[0073] (1) 6.207 g of ethylene glycol and 16.779 g of terephthalic acid were added to a reactor, followed by the addition of 0.1678 g of paramethylbenzenesulfonic acid, heated to 130°C in a steam bath, and reacted for 90 minutes. After collecting the effluent under nitrogen protection, the temperature was raised to 180°C, and 0.32 g of methanol was slowly added dropwise and end-capped to obtain a polyester;

[0074] 9.2 g of N-phenyl-1,4-p-phenylenediamine monomer is dissolved in 100 mL of anhydrous ether, slowly added dropwise to 1000 mL of hydrochloric acid at a concentration of 1 mol / L, and mechanically stirred for 4 hours to obtain a reaction solution; 14 g of iron chloride hexahydrate is dissolved in 150 mL of hydrochloric acid at a concentration of 1 mol / L, the obtained hydrochloric acid solution containing iron trichloride is slowly added dropwise to the above-described reaction solution, stirred continuously for 4 hours, and obtained a solid by suction filtration; the obtained solid is washed three times with hydrochloric acid at a concentration of 1 mol / L, then washed once with ammonia water at a concentration of 1 mol / L, finally reduced with hydrazine hydrate, and obtained a crude product by suction filtration; the crude product is vacuum dried for 72 hours to obtain an aniline oligomer;

[0075] (2) Dissolve the polyester obtained in step (1) of 22g in 120mL of DMSO, add 6mL of thionyl chloride, heat to 70℃ and react for 2h, then distill the thionyl chloride under reduced pressure, then put the solution into petroleum ether, filter and dry the precipitate to obtain the treated polyester;

[0076] (3) 19.204 g of the treated polyester obtained in step (2) and 0.728 g of the aniline oligomer obtained in step (1) are dissolved in 32 mL of DMSO, heated to 180°C and reacted for 2 hours, then the product is discharged with distilled water and washed five times to obtain the dispersant M3.

[0077] Characterized data :

[0078] The dispersant M3 provided in this embodiment was tested using a nuclear magnetic resonance spectrometer (Varian-300), and the H-NMR nuclear magnetic spectrum obtained from the test showed a single peak at 8.4 ppm, proving that an amide bond was formed; the dispersant M3 provided in this embodiment was tested using a Fourier infrared spectrometer, and the infrared spectrum obtained from the test showed at 1400 cm⁻¹ -1 A new peak appeared at [location], which is the carbon-nitrogen stretching peak of the amide bond. All of the above results prove that the dispersant M3 having the specific structure described in Example 3 was successfully synthesized.

[0079] Comparative Example 1

[0080] In polyvinylpyrrolidone (PVP), the number average molecular weight is 40,000.

[0081] Comparative Example 2

[0082] In polyvinylidene fluoride (PVDF), the number average molecular weight is 1200,000.

[0083] Application Example 1

[0084] A conductive slurry composed of NMP with mass percentages of 70%, 5%, and 25% in sequence, dispersant M1 provided in Example 1, and carbon nanotubes;

[0085] The method for manufacturing a conductive slurry provided in Application Example 1 includes the following steps.

[0086] (1) A dispersant M1 and NMP provided in Example 1 are uniformly mixed to obtain an adhesive solution;

[0087] (2) Carbon nanotubes are added to the adhesive obtained in step (1) and ground uniformly to obtain the conductive slurry.

[0088] Application Example 2

[0089] A conductive slurry composed of NMP with mass percentages of 65%, 6%, and 29% in sequence, dispersant M2 provided in Example 2, and graphene;

[0090] The method for manufacturing a conductive slurry provided in Application Example 2 comprises the following steps.

[0091] (1) Obtain an adhesive solution by uniformly mixing the dispersant M2 provided in Example 2 and NMP;

[0092] (2) Graphene is added to the adhesive obtained in step (1) and ground uniformly to obtain the conductive slurry.

[0093] Application Example 3

[0094] A conductive slurry composed of NMP with mass percentages of 75%, 4%, and 21% in sequence, dispersant M3 provided in Example 3, and carbon nanotubes;

[0095] The method for manufacturing a conductive slurry provided in Application Example 3 includes the following steps.

[0096] (1) Obtain an adhesive solution by uniformly mixing the dispersant M3 and NMP provided in Example 3;

[0097] (2) Carbon nanotubes are added to the adhesive obtained in step (1) and ground uniformly to obtain the conductive slurry.

[0098] Application Example 4

[0099] The conductive slurry is different from Application Example 1 only in that the mass percentages of NMP, dispersant M1 provided in Example 1, and carbon nanotubes are 80%, 2%, and 18%, respectively, and the manufacturing method refers to Application Example 1.

[0100] Application Example 5

[0101] The conductive slurry is different from Application Example 1 only in that the mass percentages of NMP, dispersant M1 provided in Example 1, and carbon nanotubes are 70%, 6%, and 24%, respectively, and the manufacturing method refers to Application Example 1.

[0102] Application Example 6

[0103] The conductive slurry is different from Application Example 1 only in that the mass percentages of NMP, dispersant M1 provided in Example 1, and carbon nanotubes are 70%, 1%, and 29%, respectively, and the manufacturing method refers to Application Example 1.

[0104] Application Example 7

[0105] The conductive slurry is different from Application Example 1 only in that the mass percentages of NMP, the dispersant M1 provided in Example 1, and the carbon nanotube are 70%, 8%, and 22%, respectively, and the manufacturing method refers to Application Example 1.

[0106] Application Example 8

[0107] A conductive slurry composed of NMP with mass percentages of 70%, 3%, 2%, and 25% in sequence, dispersant M1 provided in Example 1, PVP (number average molecular weight 40,000), and carbon nanotubes;

[0108] The method for manufacturing a conductive slurry provided in Application Example 8 comprises the following steps.

[0109] (1) Obtain an adhesive solution by uniformly mixing the dispersant M1, PVP, and NMP provided in Example 1;

[0110] (2) Carbon nanotubes are added to the adhesive obtained in step (1) and ground uniformly to obtain the conductive slurry.

[0111] Comparative Application Example 1

[0112] In the conductive slurry, it differs from Application Example 1 only in that the dispersant M1 provided in Example 1 is replaced with the PVP dispersant provided in Comparative Example 1, and all other materials, amounts, and manufacturing methods are the same as Application Example 1.

[0113] Comparative Application Example 2

[0114] In the conductive slurry, it differs from Application Example 1 only in that the dispersant M1 provided in Example 1 is replaced with the PVDP dispersant provided in Comparative Example 2, and all other materials, amounts, and manufacturing methods are the same as Application Example 1.

[0115] Performance Test:

[0116] (1) Conductive agent content: Calculate the mass percentage of the conductive agent in the conductive slurry;

[0117] (2) Viscosity: Tests are performed according to the test method provided in 'GB / T10247-2008', using a Brookfield rotational viscometer, with the temperature at 25℃, using rotor No. 4, and the rotational speed at 6 to 60 rpm.

[0118] Conductive slurries provided in Application Examples 1 to 8 and Comparative Application Examples 1 to 2 were tested according to the test method described above, and the test results are shown in Table 1.

[0119]

[0120] According to the data in Table 1, under conditions where the mass percentage of the conductive agent is the same, it can be confirmed that the viscosity of the conductive slurry prepared with a dispersant having a structure represented by Formula I provided in the present invention is lowered, which indicates that the dispersion effect is superior and the processing performance is superior;

[0121] Specifically, in the conductive slurries obtained in Application Examples 1–3 and Application Example 5, the mass percentage of the conductive agent is high at 21–25%, but the viscosity is only 2999–3877 mPa·s, all lower than 4000 mPa·s, so the processing performance is excellent;

[0122] When comparing the data of Application Example 1 with Comparative Application Examples 1 and 2, it can be confirmed that when the mass percentage of the conductive agent is the same, the viscosity of the conductive slurry prepared with the general dispersant provided in Comparative Examples 1 and 2 is all higher than 30,000 mPa·s, the dispersion of the conductive agent is very non-uniform, and processing is difficult;

[0123] In addition, when comparing the data of Application Example 1, Application Example 4 and Application Examples 6 to 8, the viscosity of the conductive slurry increases when the mass ratio of the dispersant to the carbon nanotube in the conductive slurry is too low, and when the mass ratio of the dispersant to the carbon nanotube in the conductive slurry is too high, the role of the dispersant in increasing the dispersion effect of the conductive slurry is not significant, and when the conductive slurry is applied to a battery, it causes a decrease in the capacity of the battery.

[0124] The applicant clarifies that although the present invention has been described with respect to a dispersant, a conductive slurry, and methods of manufacturing and applications thereof through the embodiments described above, the present invention is not limited to the embodiments described above, that is, it does not mean that the present invention can only be practiced by relying on the embodiments described above. Those skilled in the art should understand that all improvements to the present invention, equivalent substitutions for each raw material of the product of the present invention, addition of auxiliary components, and selection of specific methods are all included within the scope of protection and disclosure of the present invention.

Claims

Claim 1 A dispersant characterized by comprising any one or a combination of at least two compounds having a structure represented by Chemical Formula I: [Formula I] R is selected from alkyl groups, m is selected from integers between 1 and 500, and n is selected from integers between 1 and 10. Claim 2 A dispersant according to claim 1, wherein R is selected from C1 to C20 alkyl groups. Claim 3 A dispersant according to claim 2, wherein R is selected from C1 to C5 alkyl groups. Claim 4 A dispersant according to claim 1, characterized in that m is selected from an integer between 10 and 100. Claim 5 A dispersant according to claim 1, wherein n is selected from an integer between 4 and 10. Claim 6 A conductive slurry characterized by comprising a dispersant, a conductive agent, and a solvent according to claim 1. Claim 7 A conductive slurry according to claim 6, characterized in that the conductive agent comprises carbon nanotubes and / or graphene. Claim 8 A conductive slurry according to claim 6, characterized in that the mass percentage of the conductive agent in the conductive slurry is 18 to 30%. Claim 9 A conductive slurry according to claim 6, characterized in that the solvent is an organic solvent. Claim 10 A conductive slurry according to claim 9, characterized in that the organic solvent is N-methylpyrrolidone. Claim 11 A conductive slurry according to claim 9, characterized in that the mass percentage of the organic solvent in the conductive slurry is 65 to 80%. Claim 12 A conductive slurry according to claim 6, characterized in that the mass percentage of the dispersant in the conductive slurry is 2 to 6%. Claim 13 A conductive slurry according to claim 6, characterized in that the mass ratio of the dispersant to the conductive agent is 1:(4~10). Claim 14 A conductive slurry according to claim 13, characterized in that the mass ratio of the dispersant to the conductive agent is 1:(4~6). Claim 15 A conductive slurry according to claim 6, wherein the conductive slurry further comprises another dispersant, and the other dispersant comprises polyvinylpyrrolidone and / or polyvinylidene fluoride. Claim 16 In any one of claims 6 to 15, the conductive slurry is a conductive slurry used in a lithium-ion battery. Claim 17 A method for manufacturing a conductive slurry according to any one of claims 6 to 15, characterized by comprising the step of mixing a dispersant, a conductive agent, a solvent, and any other dispersant to obtain the conductive slurry. Claim 18 An anode slurry characterized by comprising a conductive slurry according to any one of claims 6 to 15.

Citation Information

Patent Citations

  • Graphene dispersant and applications thereof

    CN105645387A

  • Graphene dispersant and applications thereof

    CN105645388A

  • Graphene conductive coating material, preparation method therefor and application of graphene conductive coating material

    CN105778740A