Method for manufacturing printed wiring board
A resin composition with controlled inorganic filler content and plasma treatment addresses hollowing and irregularities in printed circuit boards, ensuring uniform conductive layer thickness and thermal stability.
Patent Information
- Application Number
- KR1020210137452
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-19
- Filing Date
- 2021-10-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-10-15
AI Technical Summary
The formation of via holes or trenches in printed circuit boards using laser irradiation leads to hollowing phenomena and irregularities on the insulating layer surfaces, causing non-uniform conductive layer thickness due to heat-induced delamination and erosion of the resin and inorganic filler.
A resin composition with a specific inorganic filler content (50-70% by mass) and particle diameter (0.1-0.7 μm) is used, combined with plasma treatment to form via holes or trenches, suppressing hollowing and irregularities, and a conductive layer is formed by sputtering.
The method effectively suppresses hollowing and irregularities on via hole and trench surfaces, ensuring uniform conductive layer thickness and improved thermal expansion properties.
Smart Images

Figure 112021118270017-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing a printed circuit board and a resin composition for forming via holes or trenches by plasma treatment. Background Technology
[0002] Recently, in printed circuit boards, there is a demand for multilayered build-up layers and for finer and higher-density wiring. The build-up layer is formed by a build-up method in which insulating layers and conductive layers are alternately stacked. In the manufacturing method using the build-up method, the insulating layer is generally formed by heat-curing a resin composition.
[0003] Proposals for resin compositions suitable for forming an insulating layer of an inner layer circuit board have been made numerously, including, for example, the resin composition described in Patent Document 1. Prior art literature
[0004] Japanese Patent Publication No. JP 2017-59779 The problem to be solved
[0005] However, in manufacturing printed circuit boards, via holes or trenches may be formed in the insulating layer. A "via hole" typically refers to a hole that penetrates the insulating layer. Also, a "trench" typically refers to a groove that does not penetrate the insulating layer. As a method for forming via holes or trenches, a method using a laser can be considered.
[0006] The inventors have discovered that when a laser is irradiated, heat is generated, and this heat is transmitted to the insulating layer and the underlying metal of the inner layer circuit board, thereby causing a hollowing phenomenon. A hollowing phenomenon refers to the delamination that occurs between the insulating layer and the inner layer circuit board around a via hole. This hollowing phenomenon typically occurs when the resin around the via hole deteriorates due to heat, and the deteriorated portion is eroded by a chemical solution such as a charring solution. Furthermore, the deteriorated portion is typically observed as a discolored area.
[0007] In addition, the inventors discovered that when a via hole is formed using a laser, the cured resin component and inorganic filler are excavated from the side and bottom surfaces of the via hole, causing irregularities and resulting in a non-uniform surface. Consequently, they discovered that when a conductive layer is formed by sputtering within such a via hole, the thickness of the conductive layer becomes non-uniform.
[0008] The objective of the present invention is to provide a method for manufacturing a printed circuit board that can suppress hollowing phenomena and suppress the occurrence of irregularities on the side and bottom surfaces of via holes and trenches, and a resin composition for forming via holes or trenches by plasma treatment. means of solving the problem
[0009] The inventors, after carefully examining the above problem, discovered that the problem could be solved by forming via holes or trenches in an insulating layer formed using a resin composition with adjusted inorganic filler content and average particle diameter, and thus completed the present invention.
[0010] That is, the present invention includes the following contents.
[0011] [1] (A) A process of forming an insulating layer comprising a cured resin composition on an inner layer circuit board and
[0012] (B) A process comprising forming via holes or trenches by performing plasma treatment on the surface of an insulating layer, and
[0013] The resin composition includes an inorganic filler, and
[0014] When the content of the inorganic filler is 50 mass% or more and 70 mass% or less, based on 100 mass% of the non-volatile component in the resin composition, the average particle diameter of the inorganic filler is 0.1 μm or less, and
[0015] A method for manufacturing a printed circuit board in which the content of the inorganic filler is 20 mass% or more and less than 50 mass%, and the average particle diameter of the inorganic filler is 0.7 μm or less.
[0016] [2] (D) A method for manufacturing a printed circuit board as described in [1], further comprising a process for forming a conductor layer.
[0017] [3] A method for manufacturing a printed circuit board as described in [2], wherein process (D) forms a conductive layer by sputtering.
[0018] [4] A method for manufacturing a printed circuit board as described in any one of [1] to [3], wherein the reactive gas used in the plasma treatment includes O2.
[0019] [5] A method for manufacturing a printed circuit board as described in any one of [1] to [4], wherein the reactive gas used for plasma treatment comprises a mixed gas of O2 and CF4.
[0020] [6] A method for manufacturing a printed circuit board as described in any one of [1] to [5], wherein the linear thermal expansion coefficient of the cured resin composition is 10 ppm / ℃ or higher and 50 ppm / ℃ or lower.
[0021] [7] A method for manufacturing a printed circuit board as described in any one of [1] to [6], wherein the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass%.
[0022] [8] A method for manufacturing a printed circuit board as described in any one of [1] to [7], wherein the inorganic filler is silica.
[0023] [9] A resin composition (a) comprises a curable resin, and
[0024] (a) A method for manufacturing a printed circuit board as described in any one of [1] to [8], wherein the curable resin comprises an epoxy resin and a curing agent.
[0025]
[10] A resin composition for forming an insulating layer of a printed circuit board,
[0026] A resin composition for forming via holes or trenches by plasma treatment in an insulating layer of a printed circuit board, comprising an inorganic filler having an average particle diameter of 0.1 μm or less, wherein the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass%.
[0027]
[11] A resin composition for forming an insulating layer of a printed circuit board,
[0028] A resin composition for forming via holes or trenches by plasma treatment in an insulating layer of a printed circuit board, comprising an inorganic filler having an average particle diameter of 0.7 μm or less, wherein the content of the inorganic filler is 20 mass% or more and less than 50 mass% when the non-volatile component in the resin composition is 100 mass%.
[0029]
[12] A resin composition comprises (a) a curable resin, and
[0030] (a) A resin composition described in
[10] or
[11] , wherein the curable resin comprises an epoxy resin and a curing agent.
[0031]
[13] A resin composition described in any one of
[10] to
[12] , wherein the linear thermal expansion coefficient of the cured resin composition is 20 ppm / ℃ or higher and 40 ppm / ℃ or lower. Effects of the invention
[0032] According to the present invention, a method for manufacturing a printed circuit board capable of suppressing hollowing phenomena and suppressing the occurrence of irregularities on the side and bottom surfaces of via holes and trenches, and a resin composition for forming via holes or trenches by plasma treatment can be provided. Brief explanation of the drawing
[0033] [Fig. 1] Fig. 1 is a schematic cross-sectional view showing an example of forming a via hole in process (C). [Fig. 2] Fig. 2 is a schematic plan view showing an insulating layer immediately before forming a conductor layer of a printed circuit board in which via holes are formed by conventional laser processing. [Fig. 3] Fig. 3 is a cross-sectional view schematically showing an insulating layer immediately before forming a conductor layer of a printed circuit board in which via holes are formed by conventional laser processing. Specific details for implementing the invention
[0034] The present invention will be described in detail below by presenting embodiments and examples. However, the present invention is not limited to the embodiments and examples given below, and may be implemented with arbitrary modifications within the scope of the claims of the present invention and their equivalents without departing from the scope of the claims and equivalents thereof.
[0035] Before describing in detail the method for manufacturing a printed circuit board according to the present invention, the "resin composition" and "resin sheet" used in the method for manufacturing a printed circuit board according to the present invention will be described. The resin composition is suitable for forming via holes or trenches in the insulating layer of a printed circuit board by plasma treatment. By using such a resin composition, when forming via holes or trenches by plasma treatment, the hollowing phenomenon can be suppressed, and the sidewalls of via holes and the sidewalls and bottom surfaces of trenches can be suppressed from becoming uneven surfaces. In addition, by using such a resin composition, it is also possible to lower the coefficient of thermal expansion (CTE).
[0036] [Resin Composition]
[0037] The resin composition used for forming the cured body may be one that can be used in a process for forming via holes or trenches by performing plasma treatment on the surface of an insulating layer, which is a cured product of the resin composition. In one embodiment, the resin composition comprises (a) an inorganic filler. In addition to component (a), the resin composition may additionally comprise, if necessary, (b) a curable resin, (c) a curing accelerator, (d) a thermoplastic resin, and (e) other additives. Each component included in the resin composition will be described in detail below.
[0038] <(a) Weapon Filler>
[0039] The resin composition contains (a) an inorganic filler, and (a) the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass%, and the average particle diameter of the inorganic filler is 0.1 μm or less (1st embodiment). In addition, when the content of (a) the inorganic filler is 20 mass% or more and less than 50 mass%, the average particle diameter of the inorganic filler is 0.7 μm or less (2nd embodiment). By using such (a) inorganic filler, it is possible to suppress the hollowing phenomenon and suppress the occurrence of irregularities on the side and bottom surfaces of via holes and trenches.
[0040] (a) When the inorganic filler is in the first embodiment, the cured product of the resin component is etched by plasma irradiation, and even if component (a) is excavated, the average particle diameter of component (a) is small, so it is possible to reduce the irregularity (depth and length) of the sidewall of the via hole and suppress the sidewall from becoming an uneven surface. As a result, it is possible to make the thickness of the conductor layer uniform. "Resin component" refers to a component other than the inorganic filler among the non-volatile components included in the resin composition, unless otherwise mentioned.
[0041] In the first embodiment, the content of component (a) is 50 mass% or more, preferably 55 mass% or more, more preferably 60 mass% or more, with respect to reducing the coefficient of linear thermal expansion when the non-volatile component in the resin composition is 100 mass%, and the upper limit is 70 mass% or less, preferably 69 mass% or less, more preferably 68 mass% or less. In addition, in the present invention, unless otherwise noted, the content of each component in the resin composition is a value when the non-volatile component in the resin composition is 100 mass%.
[0042] In the first embodiment, (a) the average particle diameter of the component is 0.1 μm or less, preferably 0.09 μm or less, more preferably 0.08 μm or less, with respect to reducing the irregularities of the sidewall of the via hole or the bottom surface and sidewall of the trench, preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more.
[0043] (a) When the inorganic filler is of the second embodiment, the cured product of the resin component is etched by plasma irradiation, and even if component (a) is removed, the content of component (a) is low, so it is possible to reduce the irregularity (depth and length) of the sidewall of the via hole and suppress the sidewall from becoming an uneven surface. As a result, it is possible to make the thickness of the conductor layer uniform.
[0044] In the second embodiment, the content of component (a) is less than 50 mass%, preferably 49 mass% or less, more preferably 48 mass% or less, with respect to reducing the irregularities on the sidewalls of the via hole when the non-volatile component in the resin composition is 100 mass%, and the lower limit is 20 mass% or more, preferably 30 mass% or more, more preferably 40 mass% or more.
[0045] In the second embodiment, (a) the average particle diameter of the component is 0.7 μm or less, more preferably 0.5 μm or less, even more preferably 0.1 μm or less, preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more, in order to reduce the irregularities of the sidewall of the via hole or the bottom surface and sidewall of the trench.
[0046] (a) The average particle diameter of the component can be measured by a laser diffraction scattering method based on the Mie scattering theory. Specifically, the average particle diameter can be measured by creating a volume-based particle diameter distribution of the inorganic filler using a laser diffraction scattering particle diameter distribution measuring device and taking the median diameter as the average particle diameter. For the measurement sample, 100 mg of inorganic filler and 10 g of methyl ethyl ketone can be weighed into a vial and dispersed by ultrasound for 10 minutes. Using a laser diffraction particle diameter distribution measuring device, the wavelength of the light source used is set to blue and red, and the volume-based particle diameter distribution of the component (a) is measured using a flow cell method. From the obtained particle diameter distribution, the average particle diameter can be calculated as the median diameter. Examples of laser diffraction particle diameter distribution measuring devices include the “LA-960” manufactured by Horiba Sesakusho Co., Ltd.
[0047] (a) Inorganic compounds are used as materials for inorganic fillers. Examples of materials for inorganic fillers include silica, alumina, aluminosilicate, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, calcium carbonate and silica are suitable, and silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. In addition, spherical silica is preferred as silica. (a) The inorganic filler may be used as a single type or in combination of two or more types.
[0048] (a) Examples of commercially available products of the ingredient include “UFP-30” manufactured by Denka; “SP60-05”, “SP507-05”, “SPH516-05” manufactured by Nittetsu Chemical & Material; “YC100C”, “YA050C”, “YA050C-MJE”, “YA010C” manufactured by Adomatex; “Silfil NSS-3N”, “Silfil NSS-4N”, “Silfil NSS-5N” manufactured by Tokuyama Corporation; and “SC2500SQ” manufactured by Adomatex.
[0049] (a) The specific surface area of the component is preferably 1 m² / g or more, more preferably 2 m² / g or more, and particularly preferably 3 m² / g or more. There is no specific limit on the upper limit, but it is preferably 60 m² / g or less, 50 m² / g or less, or 40 m² / g or less. The specific surface area can be obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mounttec) according to the BET method, and calculating the specific surface area using the BET multi-point method.
[0050] (a) It is preferable that the component be treated with a surface treatment agent to improve moisture resistance and dispersibility. Examples of surface treatment agents include vinylsilane-based coupling agents, (meth)acrylic-based coupling agents, fluorine-containing silane coupling agents, aminosilane-based coupling agents, epoxysilane-based coupling agents, mercaptosilane-based coupling agents, silane-based coupling agents, alkoxysilanes, organosilazanes, titanate-based coupling agents, etc. Among these, vinylsilane-based coupling agents, (meth)acrylic-based coupling agents, and aminosilane-based coupling agents are preferred to obtain the effects of the present invention, and aminosilane-based coupling agents are more preferred. In addition, the surface treatment agent may be used as a single type or may be used in combination of two or more types.
[0051] As commercially available surface treatment agents, for example, "KBM1003" (vinyltriethoxysilane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., "KBM503" (3-methacryloxypropyltriethoxysilane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., "KBM403" (3-glycidoxypropyltrimethoxysilane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., "KBM803" (3-mercaptopropyltrimethoxysilane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., "KBE903" (3-aminopropyltriethoxysilane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., "SZ-31" (hexamethyldisilazane) manufactured by Shinetsu Kagaku Kogyo Co., Ltd., and others manufactured by Shinetsu Kagaku Kogyo Co., Ltd. Examples include “KBM103” (phenyltrimethoxysilane), “KBM-4803” (long-chain epoxy-type silane coupling agent) manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd., and “KBM-7103” (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd.
[0052] The degree of surface treatment by the surface treatment agent is preferably within a predetermined range from the perspective of improving the dispersibility of the inorganic filler. Specifically, 100 parts by mass of the inorganic filler is preferably surface-treated with 0.2 to 5 parts by mass of the surface treatment agent, preferably surface-treated with 0.2 to 3 parts by mass, and preferably surface-treated with 0.3 to 2 parts by mass.
[0053] The degree of surface treatment by a surface treatment agent can be evaluated by the carbon content per unit surface area of the inorganic filler. From the perspective of improving the dispersibility of the inorganic filler, the carbon content per unit surface area of the inorganic filler is preferably 0.02 mg / m² or more, more preferably 0.1 mg / m² or more, and even more preferably 0.2 mg / m² or more. In addition, from the perspective of suppressing the increase in melt viscosity of the resin varnish and melt viscosity in sheet form, it is preferably 1 mg / m² or less, more preferably 0.8 mg / m² or less, and even more preferably 0.5 mg / m² or less.
[0054] The carbon content per unit surface area of an inorganic filler can be measured after the inorganic filler is cleaned with a solvent (e.g., methyl ethyl ketone (MEK)) following surface treatment. Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler surface-treated with a surface treatment agent, and ultrasonically cleaned at 25°C for 5 minutes. After removing the supernatant and drying the solids, the carbon content per unit surface area of the inorganic filler can be measured using a carbon analyzer. As a carbon analyzer, the "EMIA-320V" manufactured by Horiba Sesakusho Co., Ltd. can be used.
[0055] <(b) Curable Resin>
[0056] The resin composition may contain (b) a curable resin. (b) Examples of curable resins include thermosetting resins and photocurable resins, but a thermosetting resin that can be used to form an insulating layer of a printed circuit board is preferred.
[0057] Examples of thermosetting resins include epoxy resin, phenolic resin, naphthol resin, benzoxazine resin, active ester resin, cyanate ester resin, carbodiimide resin, amine resin, acid anhydride resin, etc. (b) The component may be used as a single type or two or more types may be used in combination in any ratio. Hereinafter, resins capable of reacting with epoxy resin to cure the resin composition, such as phenolic resin, naphthol resin, benzoxazine resin, active ester resin, cyanate ester resin, carbodiimide resin, amine resin, and acid anhydride resin, are collectively referred to as "curing agents." As for the resin composition, from the perspective of forming an insulating layer, it is preferable to include an epoxy resin and a curing agent as component (b), it is more preferable to include any one of an epoxy resin, an active ester resin, a cyanate ester resin, and a phenolic resin, and it is even more preferable to include an epoxy resin and an active ester resin.
[0058] (b) Examples of epoxy resins as components include, for instance, bixylenol-type epoxy resin, bisphenol A-type epoxy resin, bisphenol F-type epoxy resin, bisphenol S-type epoxy resin, bisphenol AF-type epoxy resin, dicyclopentadiene-type epoxy resin, trisphenol-type epoxy resin, naphthol novolak-type epoxy resin, phenol novolak-type epoxy resin, tert-butyl-catechol-type epoxy resin, naphthalene-type epoxy resin, naphthol-type epoxy resin, anthracene-type epoxy resin, glycidylamine-type epoxy resin, glycidyl ester-type epoxy resin, cresol novolak-type epoxy resin, biphenyl-type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro-ring containing epoxy resin, cyclohexane-type epoxy resin, cyclohexanedimethanol-type epoxy resin, naphthylene ether-type epoxy resin, trimethylol-type epoxy resin, tetraphenylethane-type epoxy resin, etc. There is. Epoxy resin may be used as a single type or in combination of two or more types.
[0059] The resin composition preferably comprises, as component (b), an epoxy resin having two or more epoxy groups in one molecule. In order to significantly obtain the desired effect of the present invention, the ratio of the epoxy resin having two or more epoxy groups in one molecule to 100 mass% of the non-volatile component of component (b) is preferably 50 mass% or more, more preferably 60 mass% or more, and particularly preferably 70 mass% or more.
[0060] Epoxy resins include an epoxy resin that is in a liquid state at a temperature of 20°C (hereinafter referred to as "liquid epoxy resin") and an epoxy resin that is in a solid state at a temperature of 20°C (hereinafter referred to as "solid epoxy resin"). The resin composition may include only liquid epoxy resin or only solid epoxy resin as component (b), but it is preferable to include a combination of liquid epoxy resin and solid epoxy resin to significantly obtain the effects of the present invention.
[0061] As for the liquid epoxy resin, a liquid epoxy resin having two or more epoxy groups in one molecule is preferred.
[0062] As for the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin; glycidyl ester type epoxy resin, glycidylamine type epoxy resin, phenol novolak type epoxy resin, alicyclic epoxy resin having an ester backbone, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, glycidylamine type epoxy resin, and epoxy resin having a butadiene structure are preferred, and bisphenol A type epoxy resin and bisphenol F type epoxy resin are more preferred.
[0063] Specific examples of liquid epoxy resins include “HP4032”, “HP4032D”, and “HP4032SS” (naphthalene-type epoxy resins) manufactured by DIC; “828US”, “jER828EL”, “825”, and “Epicote 828EL” (bisphenol A-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; “jER807” and “1750” (bisphenol F-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; “jER152” (phenol novolak-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; “630” and “630LSD” (glycidylamine-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; and “ZX1059” (a mixture of bisphenol A-type epoxy resin and bisphenol F-type epoxy resin) manufactured by Nittetsu Chemical & Materials. Examples include “EX-721” (glycidyl ester type epoxy resin) manufactured by Nagase Chemtex; “Celoxide 2021P” (alicyclic epoxy resin having an ester backbone) manufactured by Daicel; “PB-3600” (epoxy resin having a butadiene structure) manufactured by Daicel; and “ZX1658” and “ZX1658GS” (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nittetsu Chemical & Materials. These may be used individually or in combination of two or more types.
[0064] As for the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferred, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferred.
[0065] As for solid epoxy resins, bixylenol-type epoxy resin, naphthalene-type epoxy resin, naphthalene-type tetrafunctional epoxy resin, cresol novolak-type epoxy resin, dicyclopentadiene-type epoxy resin, trisphenol-type epoxy resin, naphthol-type epoxy resin, biphenyl-type epoxy resin, naphtylene ether-type epoxy resin, anthracene-type epoxy resin, bisphenol A-type epoxy resin, bisphenol AF-type epoxy resin, and tetraphenylethane-type epoxy resin are preferred, and naphthalene-type epoxy resin is more preferred.
[0066] As for solid epoxy resins, naphthalene-type tetrafunctional epoxy resin, cresol novolak-type epoxy resin, dicyclopentadiene-type epoxy resin, trisphenol-type epoxy resin, naphthol-type epoxy resin, biphenyl-type epoxy resin, naphtylene ether-type epoxy resin, anthracene-type epoxy resin, bisphenol A-type epoxy resin, and tetraphenylethane-type epoxy resin are preferred, and naphthalene-type tetrafunctional epoxy resin, naphthol-type epoxy resin, and biphenyl-type epoxy resin are more preferred. Specific examples of solid-length epoxy resins include “HP4032H” (naphthalene-type epoxy resin), “HP-4700”, “HP-4710” (naphthalene-type tetrafunctional epoxy resin), “N-690” (cresol novolak-type epoxy resin), “N-695” (cresol novolak-type epoxy resin), “HP-7200”, “HP-7200HH”, “HP-7200H” (dicyclopentadiene-type epoxy resin), “EXA-7311”, “EXA-7311-G3”, “EXA-7311-G4”, “EXA-7311-G4S”, and “HP6000” (naphtylene ether-type epoxy resin) manufactured by DIC. "EPPN-502H" (trisphenol-type epoxy resin), "NC7000L" (naphthol novolak-type epoxy resin), "NC3000H", "NC3000", "NC3000L", "NC3100" (biphenyl-type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "ESN475V" (naphthalene-type epoxy resin), "ESN485" (naphthol novolak-type epoxy resin) manufactured by Nittetsu Chemical & Materials Co., Ltd.; "YX4000H", "YL6121" (biphenyl-type epoxy resin), "YX4000HK" (bicylenol-type epoxy resin), "YX8800" (anthracene-type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; Examples include "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd., and "YL7760" (bisphenol AF type epoxy resin), "YL7800" (fluorene type epoxy resin), "jER1010" (solid bisphenol A type epoxy resin), and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.These may be used as a single type, or two or more types may be used in combination.
[0067] (b) When a combination of liquid epoxy resin and solid epoxy resin is used as components, the ratio of liquid epoxy resin to solid epoxy resin is, in terms of mass ratio, preferably 1:0.1 to 1:20, more preferably 1:0.3 to 1:15, and particularly preferably 1:0.5 to 1:10. By having the ratio of liquid epoxy resin to solid epoxy resin within this range, the desired effects of the present invention can be significantly obtained. In addition, when used in the form of a resin sheet, suitable tackiness is formed. In addition, when used in the form of a resin sheet, sufficient flexibility can be obtained and handling properties are improved. In addition, a cured product having sufficient breaking strength can be obtained.
[0068] (b) The epoxy equivalent of the epoxy resin as a component is preferably 50 g / eq. to 5,000 g / eq., more preferably 50 g / eq. to 3,000 g / eq., even more preferably 80 g / eq. to 2,000 g / eq., and even more preferably 110 g / eq. to 1,000 g / eq. By being within this range, the cured product of the resin composition can form a cured body with a sufficient crosslinking density. The epoxy equivalent is the mass of the resin containing 1 equivalent of epoxy groups. This epoxy equivalent can be measured according to JIS K7236.
[0069] (b) The weight average molecular weight (Mw) of the epoxy resin as a component is preferably 100 to 5,000, more preferably 250 to 3,000, and even more preferably 400 to 1,500, in order to significantly obtain the desired effect of the present invention. The weight average molecular weight of the epoxy resin is the weight average molecular weight in polystyrene equivalent measured by gel permeation chromatography (GPC).
[0070] (b) The content of epoxy resin as a component is preferably 10 mass% or more, more preferably 15 mass% or more, and even more preferably 20 mass% or more, when the non-volatile component in the resin composition is 100 mass%, in order to obtain a cured product exhibiting good mechanical strength and insulation reliability. The upper limit of the content of epoxy resin is preferably 90 mass% or less, more preferably 85 mass% or less, particularly preferably 45 mass% or less, 40 mass% or less, and 35 mass% or less, in order to significantly obtain the desired effects of the present invention.
[0071] (b) As for the content of epoxy resin as a component, in order to significantly obtain the effects of the present invention, when the resin component in the resin composition is 100 mass%, it is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, preferably 95 mass% or less, more preferably 90 mass% or less, and even more preferably 88 mass% or less. The resin component refers to a component among the non-volatile components in the resin composition, excluding (a) inorganic filler.
[0072] (b) As an active ester resin as a component, a resin having one or more active ester groups per molecule may be used. Among these, as the active ester resin, a resin having two or more highly reactive ester groups per molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferred. The active ester resin is preferably obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester resin obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester resin obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred.
[0073] Examples of carboxylic acid compounds include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc.
[0074] Examples of phenol compounds or naphthol compounds include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucine, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing two molecules of phenol with one molecule of dicyclopentadiene.
[0075] Preferred specific examples of active ester resins include active ester resins comprising a dicyclopentadiene-type diphenol structure, active ester resins comprising a naphthalene structure, active ester resins comprising an acetylated compound of phenol novolac, and active ester resins comprising a benzoylated compound of phenol novolac. Among these, active ester resins comprising a naphthalene structure and active ester resins comprising a dicyclopentadiene-type diphenol structure are more preferred. "Dicyclopentadiene-type diphenol structure" refers to a divalent structural unit composed of phenylene, dicyclopentylene, and phenylene.
[0076] As commercially available active ester resins, active ester resins containing a dicyclopentadiene-type diphenol structure include “EXB9451”, “EXB9460”, “EXB9460S”, “HPC-8000-65T”, “HPC-8000H-65TM”, and “EXB-8000L-65TM” (manufactured by DIC); and naphthalene-type active ester resins containing a naphthalene structure include “EXB9416-70BK”, “EXB-8100L-65T”, “EXB-8150L-65T”, “EXB-8150-65T”, “HPC-8150-60T”, “HPC-8150-62T”, and “HPB-8151-62T” (manufactured by DIC); Examples include “PC1300-02-65T” (manufactured by Air Water Co.); “DC808” (manufactured by Mitsubishi Chemical Co.) as an active ester resin containing an acetylated compound of phenol novolak; “YLH1026” (manufactured by Mitsubishi Chemical Co.) as an active ester resin containing a benzoylated compound of phenol novolak; “DC808” (manufactured by Mitsubishi Chemical Co.) as an active ester resin containing an acetylated compound of phenol novolak; “YLH1026” (manufactured by Mitsubishi Chemical Co.), “YLH1030” (manufactured by Mitsubishi Chemical Co.), “YLH1048” (manufactured by Mitsubishi Chemical Co.) as active ester resins containing a benzoylated compound of phenol novolak; and “EXB-8500-65T” (manufactured by DIC Co.).
[0077] (b) The content of the active ester resin as a component is, in order to significantly obtain the effect of the present invention, preferably 1 mass% or more, more preferably 2 mass% or more, even more preferably 4 mass% or more, with respect to 100 mass% of the non-volatile component in the resin composition, preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.
[0078] (b) The content of the active ester resin as a component is preferably 3 mass% or more, more preferably 5 mass% or more, even more preferably 8 mass% or more, when the resin component in the resin composition is 100 mass%, in order to significantly obtain the effect of the present invention. It is preferably 25 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less.
[0079] (b) As for the phenolic resin and naphthol resin as components, it is preferable that they have a novolak structure in terms of heat resistance and water resistance. In addition, nitrogen-containing phenolic resin is preferred in terms of adhesion to the conductor layer, and triazine-frame-containing phenolic resin is more preferred.
[0080] Specific examples of phenolic resins and naphthol resins include, for example, “MEH-7700”, “MEH-7810”, “MEH-7851” manufactured by Meiwa Kasei Co., Ltd., “NHN”, “CBN”, “GPH” manufactured by Nippon Kayaku Co., Ltd., “SN-170”, “SN-180”, “SN-190”, “SN-475”, “SN-485”, “SN-495”, “SN-495V”, “SN-375”, “SN-395” manufactured by Nittetsu Chemical & Material Co., Ltd., and “TD-2090”, “LA-7052”, “LA-7054”, “LA-1356”, “LA-3018-50P”, “EXB-9500” manufactured by DIC Co., Ltd.
[0081] (b) Specific examples of benzoxazine-based resins as components include “JBZ-OD100” (benzoxazine ring equivalent 218 g / eq.), “JBZ-OP100D” (benzoxazine ring equivalent 218 g / eq.), and “ODA-BOZ” (benzoxazine ring equivalent 218 g / eq.) manufactured by JFE Chemical Co., Ltd.; “Pd” (benzoxazine ring equivalent 217 g / eq.), and “Fa” (benzoxazine ring equivalent 217 g / eq.) manufactured by Shikoku Kasei Kogyo Co., Ltd.; and “HFB2006M” (benzoxazine ring equivalent 432 g / eq.) manufactured by Showa Kobunshi Co., Ltd.
[0082] (b) Examples of cyanate ester resins as components include, for instance, bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylidene))benzene, bis(4-cyanatephenyl)thioether and bis(4-cyanatephenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially triazinated. Specific examples of cyanate ester resins include “PT30,” “PT30S,” and “PT60” (phenol novolak type polyfunctional cyanate ester resins) manufactured by Lonza Japan, “ULL-950S” (polyfunctional cyanate ester resin), “BA230,” and “BA230S75” (prepolymers in which part or all of bisphenol A dicyanate is triazinated to form a trimer).
[0083] (b) Specific examples of carbodiimide resins as components include Carbodilite (registered trademark) V-03 (carbodiimide group equivalent: 216 g / eq.), V-05 (carbodiimide group equivalent: 216 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.) manufactured by Nisshinbo Chemical Co., Ltd.; V-09 (carbodiimide group equivalent: 200 g / eq.); and Stavacuzol (registered trademark) P (carbodiimide group equivalent: 302 g / eq.) manufactured by Rhein Chem.
[0084] (b) As for the amine-based resin as a component, a resin having one or more amino groups in one molecule may be used. Examples include aliphatic amines, polyetheramines, alicyclic amines, aromatic amines, etc. Among these, aromatic amines are preferred from the perspective of exhibiting the desired effect of the present invention. The amine-based resin is preferably a primary amine or a secondary amine, and a primary amine is more preferred. Specific examples of amine-based resins include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenyl ether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, Examples include 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. For the amine-based resin, commercially available products may be used, for example, "KAYABOND C-200S", "KAYABOND C-100", "Kayahad AA", "Kayahad AB", "Kayahad AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Co., Ltd.
[0085] (b) As an acid anhydride resin as a component, a resin having one or more acid anhydride groups in one molecule may be cited. Specific examples of acid anhydride resins include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl anhydride succinic acid, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic acid dihydride, biphenyltetracarboxylic acid dihydride, naphthalenetetracarboxylic acid dihydride, oxydiphthalic acid dihydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic acid dihydride, Examples include 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycolbis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin copolymerized with styrene and maleic acid.
[0086] (b) When the composition contains epoxy resin and a curing agent, the ratio of the epoxy resin to all curing agents is [total number of epoxy groups of the epoxy resin]:[total number of reactive groups of the curing agent], preferably in the range of 1:0.01 to 1:5, more preferably in the range of 1:0.05 to 1:3, and even more preferably in the range of 1:0.1 to 1:2. Here, "number of epoxy groups of the epoxy resin" is the sum of the values obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition by the epoxy equivalent. Also, "number of active groups of the curing agent" is the sum of the values obtained by dividing the mass of the non-volatile components of the curing agent present in the resin composition by the active group equivalent. By setting the ratio of the epoxy resin and the curing agent as (b) components within this range, a cured body with excellent flexibility can be obtained.
[0087] (b) The content of the curing agent as a component is, in order to significantly obtain the effect of the present invention, preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, with respect to 100 mass% of the non-volatile component in the resin composition, preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less.
[0088] (b) The content of the curing agent as a component is preferably 5 mass% or more, more preferably 10 mass% or more, even more preferably 15 mass% or more, and preferably 40 mass% or less, more preferably 30 mass% or less, and even more preferably 25 mass% or less, when the resin component in the resin composition is 100 mass% in order to obtain the effect of the present invention.
[0089] <(c) Curing Accelerator>
[0090] The resin composition may contain (c) a curing accelerator. Examples of curing accelerators include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, etc., and amine-based curing accelerators and imidazole-based curing accelerators are preferred, and amine-based curing accelerators are more preferred. The curing accelerator may be used alone or in combination of two or more types.
[0091] Examples of phosphorus-based curing accelerators include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, etc., and triphenylphosphine and tetrabutylphosphonium decanate are preferred.
[0092] Examples of amine-based curing accelerators include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, and 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene are preferred.
[0093] As imidazole-based curing accelerators, for example, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-Cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, Examples include imidazole compounds such as 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, and adducts of imidazole compounds and epoxy resins, and 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.
[0094] As an imidazole-based curing accelerator, commercially available products may be used, for example, “P200-H50” manufactured by Mitsubishi Chemical Co., Ltd.
[0095] As guanidine-based curing accelerators, for example, dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]deca-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]deca-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, Examples include 1-phenylbiguanide, 1-(o-tolyl)biguanide, etc., and dicyandiamide and 1,5,7-triazabicyclo[4.4.0]deca-5-ene are preferred.
[0096] Examples of metal-based hardening accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organic cobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organic copper complexes such as copper(II) acetylacetonate, organic zinc complexes such as zinc(II) acetylacetonate, organic iron complexes such as iron(III) acetylacetonate, organic nickel complexes such as nickel(II) acetylacetonate, and organic manganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0097] (c) The content of the curing accelerator is preferably 0.01 mass% or more, more preferably 0.02 mass% or more, particularly preferably 0.03 mass% or more, when the non-volatile component in the resin composition is 100 mass%, in order to significantly obtain the effect of the present invention, and is preferably 3 mass% or less, more preferably 1 mass% or less, and particularly preferably 0.5 mass% or less.
[0098] (c) The content of the curing accelerator is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and preferably 3 mass% or less, more preferably 2 mass% or less, and even more preferably 1 mass% or less, when the resin component in the resin composition is 100 mass% in order to significantly obtain the effect of the present invention.
[0099] <(d) Thermoplastic resin>
[0100] The resin composition may contain (d) a thermoplastic resin. Examples of thermoplastic resins include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polyetheretherketone resin, polyester resin, etc., and phenoxy resin is preferred. The thermoplastic resin may be used as a single type or in combination of two or more types.
[0101] (d) The weight-average molecular weight of the thermoplastic resin in terms of polystyrene is preferably 38,000 or more, more preferably 40,000 or more, and even more preferably 42,000 or more. The upper limit is preferably 100,000 or less, more preferably 70,000 or less, and even more preferably 60,000 or less. (d) The weight-average molecular weight of the thermoplastic resin in terms of polystyrene is measured by gel permeation chromatography (GPC). Specifically, (d) the weight-average molecular weight of the thermoplastic resin in terms of polystyrene can be calculated by using an LC-9A / RID-6A manufactured by Shimadzu Sesakusho as the measuring device, a Shodex K-800P / K-804L / K-804L manufactured by Showa Denko as the column, chloroform or the like as the mobile phase, measuring at a column temperature of 40°C, and using a calibration curve of standard polystyrene.
[0102] Examples of phenoxy resins include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminals of the phenoxy resin may be functional groups such as phenolic hydroxyl groups and epoxy groups. The phenoxy resin may be used as a single type or in combination of two or more types. Specific examples of phenoxy resins include “1256” and “4250” (both bisphenol A backbone-containing phenoxy resins), “YX8100” (bisphenol S backbone-containing phenoxy resin), and “YX6954” (bisphenol acetophenone backbone-containing phenoxy resin) manufactured by Mitsubishi Chemical Corporation, and additionally, “FX280” and “FX293” manufactured by Nittetsu Chemical & Materials Corporation, and “YL7800BH40”, “YL7500BH30”, “YX6954BH30”, “YX7553”, “YX7553BH30”, “YL7769BH30”, “YL6794”, “YL7213”, “YL7290”, and “YL7482” manufactured by Mitsubishi Chemical Corporation. You can lift the back.
[0103] Examples of polyvinyl acetal resins include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred. Specific examples of polyvinyl acetal resins include, for example, "Denka Butyral 4000-2," "Denka Butyral 5000-A," "Denka Butyral 6000-C," and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and the S-Rec BH series, BX series (e.g., BX-5Z), KS series (e.g., KS-1), BL series, BM series, etc. manufactured by Sekisui Kagaku Kogyo Co., Ltd.
[0104] Specific examples of polyimide resins include "Ricacoat SN20" and "Ricacoat PN20" manufactured by Shin Nippon Rica Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimide obtained by reacting a difunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimide described in Japanese Patent Publication No. JP 2006-37083), and polyimide containing a polysiloxane backbone (polyimide described in Japanese Patent Publication No. JP 2002-12667 and JP 2000-319386, etc.).
[0105] Specific examples of polyamideimide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Corporation. Specific examples of polyamideimide resins also include modified polyamideimides such as "KS9100" and "KS9300" (polyamideimide containing a polysiloxane backbone) manufactured by Hitachi Kasei Kogyo Corporation.
[0106] Specific examples of polyethersulfone resins include "PES5003P" manufactured by Sumitomo Chemicals. Specific examples of polyphenylene ether resins include "OPE-2St 1200" oligophenylene ether styrene resin manufactured by Mitsubishi Gas Chemicals. Specific examples of polyetheretherketone resins include "Sumiproi K" manufactured by Sumitomo Chemicals. Specific examples of polyetherimide resins include "Ultem" manufactured by GE.
[0107] Specific examples of polysulfone resins include the polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0108] Examples of polyolefin resins include, for instance, ethylene-based copolymer resins such as low-density polyethylene, ultra-low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin-based elastomers such as polypropylene and ethylene-propylene block copolymer.
[0109] Examples of polyester resins include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, polycyclohexanedimethyl terephthalate resin, etc.
[0110] Among these, (d) as the thermoplastic resin, phenoxy resin and polyvinyl acetal resin are preferred. Accordingly, in a suitable embodiment, the thermoplastic resin comprises one or more selected from the group consisting of phenoxy resin and polyvinyl acetal resin. Among these, as the thermoplastic resin, phenoxy resin is preferred, and a phenoxy resin having a weight average molecular weight of 40,000 or more is particularly preferred.
[0111] (d) The content of the thermoplastic resin is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and even more preferably 0.5 mass% or more, when the non-volatile component in the resin composition is 100 mass%, in order to significantly obtain the effects of the present invention. The upper limit is preferably 5 mass% or less, more preferably 4 mass% or less, and even more preferably 3 mass% or less.
[0112] (d) The content of the thermoplastic resin is preferably 0.5 mass% or more, more preferably 1 mass% or more, even more preferably 1.5 mass% or more, and preferably 10 mass% or less, more preferably 8 mass% or less, even more preferably 5 mass% or less, when the resin component in the resin composition is 100 mass% in order to obtain the effect of the present invention.
[0113] <(e) Other Additives>
[0114] In addition to the above components, the resin composition may additionally include other additives as optional components. Examples of such additives include, for instance, flame retardants; organic fillers; organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; resin additives such as thickeners; defoaming agents; leveling agents; adhesion promoters; and coloring agents. These additives may be used individually or in combination of two or more types in any proportion. The content of each can be appropriately set by a person skilled in the art.
[0115] The method of preparing the resin composition is not particularly limited, and examples include a method of mixing and dispersing the formulation components together with a solvent, etc., using a rotary mixer, etc., as needed.
[0116] In the case where the inorganic filler is of the first embodiment, that is, when the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass% and the average particle diameter is 0.1 μm or less, the resin composition can be suitably used for forming via holes or trenches by plasma treatment in the insulating layer of a printed circuit board. In addition, in the case where the inorganic filler is of the second embodiment, that is, when the content of the inorganic filler is 20 mass% or more and less than 50 mass% when the non-volatile component in the resin composition is 100 mass% and the average particle diameter is 0.7 μm or less, the resin composition can be suitably used for forming via holes or trenches by plasma treatment in the insulating layer of a printed circuit board.
[0117] [Resin Sheet]
[0118] The resin sheet comprises a support and a layer of resin composition formed from a resin composition provided on the support. The resin composition is as described in the [Resin Composition] column.
[0119] The thickness of the resin composition layer is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less, 30 μm or less, or 20 μm or less, from the perspective of thinning the printed circuit board and providing a cured product with excellent insulation properties even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can typically be 1 μm or more, 5 μm or more, etc.
[0120] Examples of supports include films made of plastic materials, metal foils, and release papers, and films made of plastic materials and metal foils are preferred.
[0121] When a film made of a plastic material is used as a support, examples of plastic materials include polyesters such as polyethylene terephthalate (hereinafter abbreviated as "PET") and polyethylene naphthalate (hereinafter abbreviated as "PEN"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetylcellulose (TAC), polyether sulfide (PES), polyether ketone, and polyimide. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0122] When using a metal foil as a support, examples of metal foils include copper foil and aluminum foil, and copper foil is preferred. As for the copper foil, a foil made of copper may be used, or a foil made of an alloy of copper and other metals (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0123] The support may have a matte treatment, corona treatment, or antistatic treatment applied to the surface bonded to the resin composition layer.
[0124] In addition, as a support, a release layer-attached support having a release layer on the surface bonded to the resin composition layer may be used. As for the release agent used in the release layer of the release layer-attached support, for example, one or more release agents selected from the group consisting of alkyd resin, polyolefin resin, urethane resin, and silicone resin may be used. As for the release layer-attached support, commercially available products may be used, and examples include PET films having a release layer mainly composed of alkyd resin-based release agents such as “SK-1”, “AL-5”, “AL-7” manufactured by Lintec, “Lumira T60” manufactured by Tore, “Purex” manufactured by Teijin, and “Unifil” manufactured by Unichika; “U2-NR1” manufactured by DuPont Films, etc.
[0125] The thickness of the support is not particularly limited, but a range of 5㎛ to 75㎛ is preferred, and a range of 10㎛ to 60㎛ is more preferred. In addition, when using a support with a release layer attached, it is preferable that the total thickness of the support with the release layer attached is within the above range.
[0126] In one embodiment, the resin sheet may additionally include other layers as needed. Examples of such other layers include a protective film similar to a support provided on the side that is not bonded to the support of the resin composition layer (i.e., the side opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, the adhesion of dust or the like to the surface of the resin composition layer and scratches can be suppressed.
[0127] A resin sheet can be manufactured, for example, by preparing a resin varnish by dissolving a resin composition in an organic solvent, applying the resin varnish onto a support using a die coater or the like, and further drying it to form a layer of the resin composition.
[0128] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; acetic acid esters such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvent may be used alone or in combination of two or more types.
[0129] Drying may be carried out by known methods such as heating or hot air spraying. Although the drying conditions are not particularly limited, drying is performed so that the content of the organic solvent in the resin composition layer is 10 mass% or less, preferably 5 mass% or less. Depending on the boiling point of the organic solvent in the resin varnish, for example, when using a resin varnish containing 30 mass% to 60 mass% of an organic solvent, a resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0130] The resin sheet can be stored by winding it into a roll shape. If the resin sheet has a protective film, it becomes usable by removing the protective film.
[0131] [Method for manufacturing a printed circuit board]
[0132] The method for manufacturing a printed circuit board of the present invention is,
[0133] (A) A process of forming an insulating layer comprising a cured resin composition on an inner layer circuit board and
[0134] (B) A process of forming via holes or trenches by performing plasma treatment on the surface of the insulating layer.
[0135] In the present invention, via holes or trenches are formed in the insulating layer by plasma treatment rather than laser treatment. Accordingly, the occurrence of hollowing phenomena can be suppressed, and the occurrence of irregularities on the sides of via holes and the sides and bottom surfaces of trenches can be suppressed.
[0136] In addition, the method for manufacturing a printed circuit board of the present invention, in addition to process (A) and process (B), may, as needed,
[0137] (C) Process of harmonizing the surface of the insulating layer,
[0138] (D) It may include a process of forming a conductive layer on the surface of the insulating layer.
[0139] Processes (A) and (B) are preferably performed in this order, and are more preferably performed in the order of process (A), process (B), process (C), and process (D). Below, each process of the method for manufacturing a printed circuit board will be described.
[0140] <Process (A)>
[0141] Process (A) is a process of forming an insulating layer comprising a cured resin composition on an inner layer circuit board. In process (A), an insulating layer is typically formed on the main surface of the inner layer circuit board. The main surface of the inner layer circuit board refers to the surface of the inner layer circuit board on which the insulating layer is provided.
[0142] In performing process (A), the process (A-1) may include a step of preparing an inner layer circuit board. The inner layer circuit board typically comprises a support substrate and a metal layer provided on the surface of the support substrate. The metal layer is exposed on the main surface of the inner layer circuit board.
[0143] Examples of materials for the support substrate include glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, thermosetting polyphenylene ether substrates, etc. Examples of materials for the metal layer include copper foil, carrier-attached copper foil, and the materials for the conductor layer described later, and copper foil is preferred.
[0144] In addition, when performing process (A), the process (A-2) may include a step of preparing a resin sheet. The resin sheet is as described above.
[0145] In process (A), for example, a layer of resin composition of a resin sheet is laminated on the main surface of an inner layer circuit board, and an insulating layer is formed by heat-curing the layer of resin composition.
[0146] Lamination of the inner layer circuit board and the resin sheet can be performed, for example, by heat-pressing the resin sheet onto the inner layer circuit board from the support side. As for the member that heat-presses the resin sheet onto the inner layer circuit board (hereinafter also referred to as the "heat-pressing member"), examples include a heated metal plate (such as a SUS hard plate) or a metal roll (such as a SUS roll). Furthermore, rather than pressing the heat-pressing member directly onto the resin sheet, it is preferable to press by interposing an elastic material, such as heat-resistant rubber, so that the resin sheet sufficiently follows the surface irregularities of the inner layer circuit board.
[0147] Lamination of the inner layer circuit board and the resin sheet may be carried out by a vacuum lamination method. In the vacuum lamination method, the heat pressing temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heat pressing pressure is preferably in the range of 0.098 MPa to 1.77 MPa, more preferably in the range of 0.29 MPa to 1.47 MPa, and the heat pressing time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. Lamination is preferably carried out under reduced pressure conditions of 26.7 hPa or less.
[0148] Lamination can be performed using a commercially available vacuum laminator. Examples of commercially available vacuum laminators include the vacuum pressure laminator manufactured by Meiki Sesakusho Co., Ltd., the vacuum applicator manufactured by Nikko Materials Co., Ltd., and the batch vacuum pressure laminator.
[0149] After lamination, the laminated resin sheets may be smoothed by pressing a heat-pressing member from the support side under atmospheric pressure. The pressing conditions for the smoothing treatment may be the same as the heat-pressing conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. Additionally, lamination and the smoothing treatment may be performed continuously using the commercially available vacuum laminator.
[0150] The support may be removed before heat curing the resin sheets after lamination, or after process (A).
[0151] After laminating the resin sheet onto the inner layer circuit board, the resin composition layer is heat-cured to form an insulating layer. The heat-curing conditions of the resin composition layer are not particularly limited, and conditions commonly used when forming an insulating layer of a printed circuit board may be used.
[0152] For example, the thermal curing conditions of the resin composition layer vary depending on the type of resin composition, but the curing temperature is preferably 120°C to 240°C, more preferably 150°C to 220°C, and even more preferably 170°C to 210°C. The curing time can preferably be 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.
[0153] Before heat-curing the resin composition layer, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to heat-curing the resin composition layer, the resin composition layer may be preheated for at least 5 minutes (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, even more preferably 15 minutes to 100 minutes) at a temperature of 50°C or higher and less than 120°C (preferably 60°C or higher and 115°C or lower, more preferably 70°C or higher and 110°C or lower).
[0154] The thickness of the insulating layer is preferably 100 μm or less, more preferably 50 μm or less, even more preferably 40 μm or less, 30 μm or less, 20 μm or less, preferably 1 μm or more, more preferably 5 μm or more.
[0155] In addition, instead of forming an insulating layer using a resin sheet, an insulating layer may be formed by directly applying a resin composition onto the main surface of the inner layer circuit board. The conditions for forming the insulating layer in this case are the same as those for forming an insulating layer using a resin sheet. Furthermore, the resin composition to be applied is as described above.
[0156] Before performing process (B) after process (A) is completed, in order to effectively form via holes or trenches in the insulating layer, the process may include (A-3) a process of laminating a dry film on the insulating layer or on a support, and (A-4) a process of obtaining a patterned dry film by exposing and developing the dry film using a photomask.
[0157] In process (A-3), a dry film is laminated onto an insulating layer or a support formed on the main surface of an inner layer circuit board. The lamination conditions of the insulating layer and the dry film may be the same as the lamination conditions of the inner layer circuit board and the resin sheet.
[0158] As for the dry film used in process (A-3), it is preferable that a patterned dry film be obtained by exposure and development, and it is even better if the film is resistant to plasma treatment in process (B). Additionally, as the dry film, a photosensitive dry film made of a photoresist composition may be used. As such a dry film, for example, a dry film formed from a resin such as novolak resin or acrylic resin may be used.
[0159] As for the thickness of the dry film, from the perspective of improving the processability of the via hole, it is preferably 10 μm or more, more preferably 15 μm or more, even more preferably 20 μm or more, preferably 100 μm or less, more preferably 70 μm or less, and even more preferably 50 μm or less.
[0160] In process (A-4), exposure is performed by irradiating an active energy line through a photomask having a predetermined pattern. The details of the exposure are typically such that an active energy line is irradiated onto the surface of a dry film through a photomask to photocur the exposed portion of the dry film. Examples of active energy lines include ultraviolet rays, visible light, electron beams, X-rays, etc., and ultraviolet rays are preferred. The amount and duration of ultraviolet irradiation can be appropriately set according to the dry film. Examples of exposure methods include a contact exposure method in which a mask pattern is in close contact with the dry film for exposure, and a non-contact exposure method in which parallel light rays are used for exposure without the mask pattern being in close contact with the dry film.
[0161] After exposure, by developing, one of the exposed and unexposed portions of the dry film (usually the unexposed portion) is removed to form a patterned dry film. The development may be performed using either wet development or dry development. Examples of development methods include dip method, paddle method, spray method, brushing method, scraping method, etc.
[0162] In the process (B) described below, plasma treatment is performed using a pattern dry film as a mask to form via holes or trenches.
[0163] Process (B)
[0164] Process (B) is a process of forming via holes or trenches on the surface of an insulating layer by performing plasma treatment on the surface of the insulating layer. As shown in the example of Process (B) in FIG. 1, a via hole (110) is formed by removing the cured resin composition contained in the insulating layer (100) using plasma with a predetermined gas. Normally, only the cured resin component (1020) is etched by the plasma. When an inorganic filler (1010) is contained in the insulating layer (100), the inorganic filler (1010) is not normally etched, but is excavated by etching the surrounding cured resin component (1020). The excavated inorganic filler (1010) can be detached from the cured resin and blown away. In the case where the inorganic filler (1010) is of the first embodiment, its average particle diameter is 0.1 μm or less, so the depth and diameter of the location (1030) where the inorganic filler (1010) on the side wall of the via hole (110) is excavated are small. That is, the difference in unevenness of the side wall is reduced, and the formation of an uneven surface is suppressed. In addition, in the case where the inorganic filler (1010) is of the second embodiment, its content is small, so the depth and diameter of the location (1030) where the inorganic filler (1010) on the side wall of the via hole (110) is excavated are small. As a result, it becomes possible to make the thickness of the conductor layer formed within the via hole (110) uniform in the process (D) described later.
[0165] Plasma treatment forms via holes or trenches on the surface of an insulating layer by treating the surface of the insulating layer with plasma generated by introducing gas into a plasma generator. There are no particular limitations on the method of generating plasma, and examples include microwave plasma generated by microwaves, high-frequency plasma using high frequency, atmospheric pressure plasma generated under atmospheric pressure, and atmospheric pressure plasma generated under vacuum, and atmospheric pressure plasma generated under vacuum is preferred.
[0166] In addition, the plasma used in process (C) is preferably an RF plasma excited by high frequency.
[0167] As the reactive gas for plasmafication, a gas that etches only the cured resin components within the insulating layer and removes inorganic fillers can be used in terms of processing speed. In this regard, it is preferable for the reactive gas to include O2. The reactive gas may also include inert gases such as Ar and N2. Additionally, the reactive gas may include fluorocarbon-based fluorine compounds such as CF4, C4F6, C4F8, CH2F2, and CHF3. As the reactive gas, a mixed gas containing O2 and CF4 is particularly preferred.
[0168] When using a mixed gas containing O2, the mixing ratio of the mixed gas (gas other than O2 / O2: unit is sccm) is preferably 0.1 / 10 to 1 / 1, more preferably 0.5 / 10 to 1 / 2, and more preferably 1 / 10 to 1 / 2, in terms of making the thickness of the conductor layer formed inside the via hole or trench uniform. When using a mixed gas of CF4 and O2, the mixing ratio of the mixed gas of CF4 and O2 (CF4 / O2: unit is sccm) is preferably 0.1 / 10 to 1 / 1, more preferably 0.5 / 10 to 1 / 2, and more preferably 1 / 10 to 1 / 2, in terms of making the thickness of the conductor layer formed inside the via hole or trench uniform.
[0169] In order to significantly obtain the effects of the present invention, the pressure inside the chamber vessel in plasma treatment is preferably 50 Pa or more, more preferably 75 Pa or more, even more preferably 100 Pa or more, preferably 300 Pa or less, more preferably 250 Pa or less, and even more preferably 200 Pa or less.
[0170] The irradiation time in plasma treatment is not particularly limited, but 1 minute or more is preferred, 2 minutes or more is more preferred, and 3 minutes or more is even more preferred. The upper limit is not particularly limited, but 20 minutes or less is preferred, 15 minutes or less is even more preferred, and 10 minutes or less is even more preferred.
[0171] The present invention forms via holes or trenches by plasma treatment, thereby allowing the opening diameter of the via holes or trenches to be reduced. The opening diameter is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, or 20 μm or less. The lower limit is not particularly limited, but can be 1 μm or more.
[0172] Process (C)
[0173] Process (C) is a process for treating the surface of the insulating layer, and in detail, it is a process for removing foreign substances, such as inorganic fillers removed by process (B), from via holes or trenches using a treatment solution. Foreign substances may exist on the surface of the insulating layer after process (B). Such foreign substances may include, for example, inorganic fillers removed by plasma treatment. Such foreign substances may cause a decrease in the adhesion strength of the conductor layer. Therefore, process (C) is performed to remove these foreign substances. In detail, process (C) is a process for removing the foreign substances by bringing the surface of the insulating layer into contact with a treatment solution after the completion of process (B). Process (C) may be performed once or multiple times.
[0174] The sequence and conditions of process (C) are not particularly limited, and known sequences and conditions commonly used when forming an insulating layer of a printed circuit board may be adopted. For example, the insulating layer can be harmonized by performing swelling treatment with a swelling solution, harmonization treatment with an oxidizing agent, and neutralization treatment with a neutralizing solution in this order. The swelling solution used for the harmonization treatment is not particularly limited, but may include an alkali solution, a surfactant solution, etc., and preferably an alkali solution, and as the alkali solution, a sodium hydroxide solution or a potassium hydroxide solution is more preferable. Examples of commercially available swelling solutions include "Swelling Deep Securigans P," "Swelling Deep Securigans SBU," and "Swelling Deep Securigans P" manufactured by Atotech Japan. Swelling treatment using a swelling solution is not particularly limited, but can be performed, for example, by immersing the insulating layer in a swelling solution at 30°C to 90°C for 1 minute to 20 minutes. From the perspective of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling solution at 40°C to 80°C for 5 minutes to 15 minutes. As for the oxidizing agent used for the oxidizing treatment, it is not particularly limited, but for example, an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide may be used. It is preferable to perform oxidizing treatment using an oxidizing agent such as an alkaline permanganate solution by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan. In addition, an acidic aqueous solution is preferred as the neutralizing solution used for the harmonization treatment, and examples of commercially available products include "Reduction Solution Securigans P" manufactured by Atotech Japan.Treatment with a neutralizing solution can be performed by immersing a treated surface that has undergone oxidizing agent treatment in a neutralizing solution at 30°C to 80°C for 1 minute to 30 minutes. In terms of workability, a method of immersing an object that has undergone oxidizing agent treatment in a neutralizing solution at 40°C to 70°C for 5 minutes to 20 minutes is preferred.
[0175] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after harmonization treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but is preferably 30 nm or more, more preferably 40 nm or more, and even more preferably 50 nm or more. The arithmetic mean roughness (Ra) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0176] Process (D)
[0177] Process (D) is a process of forming a conductor layer on the surface of an insulating layer. The conductor material used for the conductor layer is not particularly limited. In a suitable embodiment, the conductor layer comprises one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. The conductor layer may be a single metal layer or an alloy layer, and as an alloy layer, for example, a layer formed of an alloy of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy) may be used. Among these, from the perspective of universality of forming a conductor layer, cost, and ease of patterning, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0178] The conductor layer may be a single-layer structure, or a multilayer structure in which two or more single-metal layers or alloy layers made of different types of metals or alloys are stacked. In the case where the conductor layer is a multilayer structure, the layer in contact with the hardened body is preferably a single-metal layer of chromium, zinc, or titanium, or an alloy layer of a nickel-chromium alloy.
[0179] The thickness of the conductor layer depends on the design of the desired printed circuit board, but is generally 3㎛ to 35㎛, preferably 5㎛ to 30㎛.
[0180] As a suitable embodiment of process (D), the conductor layer is formed by sputtering. In the present invention, since the resin composition includes an inorganic filler having a predetermined amount and a predetermined average particle diameter, the difference in unevenness at the location where the inorganic filler on the sidewall of the via hole is excavated is reduced. As a result, it is possible to make the thickness of the conductor layer formed in the via hole or trench uniform.
[0181] When forming a conductor layer by sputtering, typically, a conductor seed layer is first formed on the surface of an insulating layer by sputtering, and then a conductor sputtered layer is formed on the conductor seed layer by sputtering. Before forming the conductor seed layer by sputtering, the surface of the insulating layer may be cleaned by reverse sputtering. Various gases may be used as the gas for the reverse sputtering, but among them, Ar, O2, and N2 are preferred. If the seed layer is Cu and a Cu alloy, Ar or O2 or a mixed gas of Ar and O2 is preferred; if the seed layer is Ti, Ar or N2 or a mixed gas of Ar and N2 is preferred; and if the seed layer is Cr and a Cr alloy (such as nichrome), Ar or O2 or a mixed gas of Ar and O2 is preferred. Sputtering can be performed using various sputtering devices such as magnetron sputtering or mirrortron sputtering. Examples of metals forming the conductor seed layer include Cr, Ni, Ti, and nichrome. Cr and Ti are particularly preferred. The thickness of the conductor seed layer is typically formed to be 5 nm or more, more preferably 10 nm or more, preferably 1,000 nm or less, and more preferably 500 nm or less. Examples of metals forming the conductor sputter layer include Cu, Pt, Au, Pd, etc. Cu is particularly preferred. The thickness of the conductor sputter layer is typically formed to be 50 nm or more, more preferably 100 nm or more, preferably 3,000 nm or less, and more preferably 1,000 nm or less.
[0182] After forming a conductor layer by sputtering, a copper plating layer may be additionally formed on the conductor layer by electrolytic copper plating. The thickness of the copper plating layer is typically, preferably 5 μm or more, more preferably 8 μm or more, preferably 75 μm or less, more preferably 35 μm or less. Known methods such as the subtractive method and the semi-additive method may be used for circuit formation.
[0183] The method for manufacturing a printed circuit board according to the present invention exhibits the characteristic that the hollowing phenomenon is suppressed. Hereinafter, the hollowing phenomenon will be explained with reference to the drawings.
[0184] FIG. 2 is a schematic plan view showing the side (100U) opposite to the metal layer (210) (not shown in FIG. 2) of the insulating layer (100) immediately before the conductor layer is formed, of a conventional printed circuit board in which a via hole is formed by a laser. FIG. 3 is a schematic cross-sectional view showing the insulating layer (100) immediately before the conductor layer is formed, of a conventional printed circuit board in which a via hole is formed by a laser, together with the metal layer (210) of the inner layer circuit board (200). FIG. 3 shows a cross-section of the insulating layer (100) cut in a plane passing through the center (120C) of the via bottom (120) of the via hole (110) and also parallel to the thickness direction of the insulating layer (100).
[0185] As shown in FIG. 2, when a via hole is formed with a laser, a discolored portion (140) may occur due to the degradation of the resin caused by the heat of the laser. In this discolored portion (140), erosion by the agent during the shaping process may occur, causing the insulating layer (100) to peel off from the metal layer (210) and a gap portion (160) continuous from the edge (150) of the via bottom (120) to be formed (hollowing phenomenon).
[0186] In the present invention, via holes or trenches are formed by plasma treatment, which is difficult to generate heat, so the deterioration of the resin can be suppressed. Therefore, peeling of the insulating layer (100) from the metal layer (210) can be suppressed, the size of the gap portion (160) can be reduced, and ideally, the discolored portion (140) and the gap portion (160) can be eliminated.
[0187] The size of the discolored portion (140) can be evaluated by the hollowing distance (Wt) from the edge (180) of the via top (130) of the via hole (110).
[0188] The edge (180) of the via top (130) corresponds to the inner circumferential edge portion of the discolored portion (140). The hollowing distance (Wt) from the edge (180) of the via top (130) represents the distance from the edge (180) of the via top (130) to the outer circumferential edge portion (190) of the discolored portion (140). The smaller the hollowing distance (Wt) from the edge (180) of the via top (130), the more effectively the formation of the discolored portion (140) can be suppressed.
[0189] For example, plasma is irradiated onto an insulating layer (100) obtained by curing a resin sheet formed on a copper foil by heating it at 100°C for 30 minutes and then at 180°C for 30 minutes, thereby forming a via hole (110) with a tower diameter (Lt) of about 15 μm. The hollowing distance (Wt) from the edge (180) of the via tower (130) of the insulating layer (100) obtained in this way can be preferably 15 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The lower limit is not particularly limited, but can be 0 μm or more, 0.01 μm or more, etc.
[0190] The hollowing distance (Wt) from the edge (180) of the via top (130) can be measured by observation with an optical microscope.
[0191] In addition, according to the inventor's review, it has been found that, generally, the larger the diameter of the via hole (110), the greater the tendency for the size of the discolored portion (140) to increase. Therefore, the degree of inhibition of the formation of the discolored portion (140) can be evaluated by the ratio of the size of the discolored portion (140) to the diameter of the via hole (110). For example, it can be evaluated by the hollowing ratio (Ht) relative to the top radius (Lt / 2) of the via hole (110). Here, the top radius (Lt / 2) of the via hole (110) refers to the radius of the via top (130) of the via hole (110). Additionally, the hollowing ratio (Ht) to the top radius (Lt / 2) of the via hole (110) is a ratio obtained by dividing the hollowing distance (Wt) from the edge (180) of the via top (130) by the top radius (Lt / 2) of the via hole (110). The smaller the hollowing ratio (Ht) to the top radius (Lt / 2) of the via hole (110), the more effectively the formation of the discolored portion (140) can be suppressed.
[0192] For example, plasma is irradiated onto an insulating layer (100) obtained by curing a resin sheet formed on a copper foil by heating it at 100°C for 30 minutes and then at 180°C for 30 minutes, thereby forming a via hole (110) with a top diameter (Lt) of about 15 μm. The hollowing ratio (Ht) relative to the top radius (Lt / 2) of the via hole (110) formed in the insulating layer (100) obtained in this way can be preferably 35% or less, more preferably 25% or less, even more preferably 10% or less, or 5% or less. The lower limit is not particularly limited, but can be 0% or more, 0.01% or more, etc.
[0193] The hollowing ratio (Ht) for the top radius (Lt / 2) of the via hole (110) can be calculated from the top diameter (Lt) of the via hole (110) and the hollowing distance (Wt) from the edge (180) of the via top (130) of the via hole (110).
[0194] The edge (150) of the via bottom (120) corresponds to the inner circumferential edge of the gap portion (160). Accordingly, the distance (Wb) from the edge (150) of the via bottom (120) to the outer circumferential end of the gap portion (160) (i.e., the end farther from the center (120C) of the via bottom (120)) (170) corresponds to the size in the in-plane direction of the gap portion (160). Here, the in-plane direction refers to a direction perpendicular to the thickness direction of the insulating layer (100). In addition, in the following description, the distance (Wb) may be referred to as the hollowing distance (Wb) from the edge (150) of the via bottom (120) of the via hole (110).
[0195] The size of the discolored portion (140) may be evaluated for the degree of suppression of the hollowing phenomenon by the hollowing distance (Wb) from the edge (150) of the via bottom (120). Specifically, the smaller the hollowing distance (Wb) from the edge (150) of the via bottom (120), the more effectively the hollowing phenomenon can be suppressed.
[0196] The hollowing distance (Wb) from the edge (150) of the via bottom (120) of the via hole (110) of the insulating layer (100) is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 4.5 μm or less, and particularly preferably 4 μm or less. The lower limit is not particularly limited, but can be 0 μm or more, 0.01 μm or more, etc. The hollowing distance (Wb) can be measured by using a FIB (Focused Ion Beam) to cut the insulating layer (100) so that a cross-section parallel to the thickness direction of the insulating layer (100) and passing through the center (120C) of the via bottom (120) appears, and then observing the cross-section with an electron microscope.
[0197] In addition, in the conventional method using a laser, it has been found that the larger the diameter of the via hole, the larger the size of the gap portion (160) tends to be. Therefore, the degree of suppression of the hollowing phenomenon can be evaluated by the ratio of the size of the gap portion (160) to the diameter of the via hole (110). For example, it can be evaluated by the hollowing ratio (Hb) to the bottom radius (Lb / 2) of the via hole (110). Here, the bottom radius (Lb / 2) of the via hole (110) refers to the radius of the via bottom (120) of the via hole (110). Additionally, the hollowing ratio (Hb) to the bottom radius (Lb / 2) of the via hole (110) is a ratio obtained by dividing the hollowing distance (Wb) from the edge (150) of the via bottom (120) by the bottom radius (Lb / 2) of the via hole (110). The smaller the hollowing ratio (Hb) to the bottom radius (Lb / 2) of the via hole (110), the more effectively the hollowing phenomenon can be suppressed.
[0198] The hollowing ratio (Hb) can be preferably 35% or less, more preferably 30% or less, and even more preferably 25% or less. The hollowing ratio (Hb) for the non-bottom radius (Lb / 2) of the via hole (110) can be calculated from the bottom diameter (Lb) of the via hole (110) and the hollowing distance (Wb) from the edge (150) of the via bottom (120) of the via hole (110).
[0199] In the manufacturing process of a printed circuit board, the via hole (110) is typically formed in a state where no other conductor layer (not shown) is provided on the surface (100U) of the insulating layer (100) opposite to the metal layer (210). Therefore, if one knows the manufacturing process of the printed circuit board, one can clearly recognize a structure in which a via bottom (120) is located on the metal layer (210) side and a via top (130) is opened on the side opposite to the metal layer (210). However, in the finished printed circuit board, there may be cases where conductor layers are provided on both sides of the insulating layer (100). In this case, it may be difficult to distinguish between the via bottom (120) and the via top (130) due to the positional relationship with the conductor layer. However, typically, the top diameter (Lt) of the via top (130) is larger than the bottom diameter (Lb) of the via bottom (120). Therefore, in the above case, it is possible to distinguish between the via bottom (120) and the via top (130) based on the diameter.
[0200] The method for manufacturing a printed circuit board according to the present invention can reduce the difference in unevenness at the location where the inorganic filler on the side wall of the via hole is excavated. Accordingly, a conductor layer of uniform thickness can be formed within the via hole. When cross-sectional observation of the insulating layer is performed using SEM, it can be confirmed that a copper layer is formed uniformly and without interruption in the trench formed in the insulating layer and on the wall of the via hole.
[0201] Since the manufacturing method of the printed circuit board of the present invention is applied in a lamination process by a build-up method, it is desirable for the mismatch of the coefficient of thermal expansion (CTE) of each component to be low. The coefficient of thermal expansion (CTE) of the insulating layer is preferably 50 ppm / °C or less, more preferably 40 ppm / °C or less, even more preferably 30 ppm / °C or less, and 25 ppm / °C or less. The lower limit is not particularly limited, but can be 10 ppm / °C or more, 20 ppm / °C or more, 25 ppm / °C or more, etc. The coefficient of thermal expansion can be measured according to the embodiments described below.
[0202] [Semiconductor Device]
[0203] The semiconductor device of the present invention includes a printed circuit board. The semiconductor device of the present invention can be manufactured using a printed circuit board obtained by the manufacturing method of the present invention.
[0204] Examples of semiconductor devices include various semiconductor devices provided for electrical products (e.g., computers, mobile phones, digital cameras, and televisions) and vehicles (e.g., motorcycles, automobiles, trams, ships, and aircraft).
[0205] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) at a conductive location on a printed circuit board. A "conductive location" is a "location that transmits an electrical signal on a printed circuit board," and the location may be either a surface location or an embedded location. Furthermore, the semiconductor chip is not particularly limited as long as it is an electrical circuit element made of semiconductor material.
[0206] The mounting method of a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively; however, specifically, examples include wire bonding mounting methods, flip-chip mounting methods, mounting methods using a bump-free build-up layer (BBUL), mounting methods using an anisotropic conductive film (ACF), and mounting methods using a non-conductive film (NCF). Here, "mounting method using a bump-free build-up layer (BBUL)" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess of a printed circuit board and the semiconductor chip is connected to the wiring on the printed circuit board."
[0207] [Example]
[0208] The present invention will be described in detail below by presenting examples. However, the present invention is not limited to the following examples. In the following, "parts" and "%" indicating amounts refer to "parts by mass" and "% by mass," respectively, unless otherwise specified. Furthermore, unless otherwise specified, the operations described below were performed in an environment of room temperature and pressure.
[0209] <Used Weapon Filler>
[0210] Inorganic filler 1: Surface treated with 2 parts of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Kagaku Kogyo Co., Ltd., KBM573) for every 100 parts of spherical silica ("UFP-30" manufactured by Denki Kagaku Kogyo Co., Ltd., average particle diameter 0.078 μm, specific surface area 30.7 m² / g).
[0211] Inorganic filler 2: Surface treated with 1 part N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., KBM573) for every 100 parts of spherical silica ("SC2500SQ" manufactured by Adomatex, Inc., average particle diameter 0.63 μm, specific surface area 11.2 m² / g).
[0212] Inorganic filler 3: Surface treated with 1 part N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Kagaku Kogyo, KBM573) for every 100 parts of spherical silica (Adomatex Co., Ltd. “SC4500SQ”, average particle diameter 1.0 μm, specific surface area 4.5 m² / g).
[0213] <Preparation of Resin Composition 1>
[0214] 6 parts of bixylenol-type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical, epoxy equivalent approx. 185 g / eq.), 5 parts of naphthalene-type epoxy resin ("ESN475V" manufactured by Shin-Nippon Steel Sumikin Kagaku, epoxy equivalent approx. 332 g / eq.), 15 parts of bisphenol AF-type epoxy resin ("YL7760" manufactured by Mitsubishi Chemical, epoxy equivalent approx. 238 g / eq.), 2 parts of naphthylene ether-type epoxy resin ("HP6000L" manufactured by DIC, epoxy equivalent approx. 213 g / eq.), 2 parts of cyclohexane-type epoxy resin ("ZX1658GS" manufactured by Mitsubishi Chemical, epoxy equivalent approx. 135 g / eq.), phenoxy resin (manufactured by Mitsubishi Chemical) Two parts of “YL7500BH30”, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30 mass% (Mw=44,000), were heated and dissolved while stirring in a mixed solvent of 20 parts of solvent naphtha and 10 parts of cyclohexanone. After cooling to room temperature, 4 parts of a triazine-skeleton-containing cresol novolak resin (DIC “LA-3018-50P”, hydroxyl group equivalent of about 151 g / eq., 2-methoxypropanol solution with 50% solid content), 6 parts of an active ester resin (DIC “EXB-8000L-65TM”, active group equivalent of about 220 g / eq., toluene solution with 65 mass% non-volatile component), 60 parts of inorganic filler 1, and 0.05 parts of an amine-based curing accelerator (4-dimethylaminopyridine (DMAP)) were mixed and uniformly dispersed using a high-speed rotary mixer, and then filtered using a cartridge filter (ROKITECHNO “SHP020”) to prepare resin composition 1.
[0215] <Preparation of Resin Composition 2>
[0216] In the preparation of resin composition 1,
[0217] 1) Change Weapon Filler 1 (60 parts) to Weapon Filler 2 (80 parts), and
[0218] 2) Two parts of phenoxy resin ("YL7500BH30" manufactured by Mitsubishi Chemical, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30 mass%, Mw=44,000) were replaced with two parts of phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30 mass%, Mw=35,000).
[0219] Resin composition 2 was prepared in the same manner as resin composition 1, except for the above details.
[0220] <Preparation of Resin Composition 3>
[0221] In the preparation of resin composition 2, 80 parts of inorganic filler 2 were replaced with 80 parts of inorganic filler 3. Except for the above, resin composition 3 was prepared in the same manner as resin composition 2.
[0222] <Preparation of Resin Composition 4>
[0223] In the preparation of resin composition 1,
[0224] 1) Change the amount of Weapon Filler 1 from 60 parts to 30 parts, and
[0225] 2) Replace 6 parts of active ester resin (DIC “EXB-8000L-65TM”, active group equivalent approx. 220 g / eq., toluene solution of 65 mass% non-volatile component) with 6 parts of active ester resin (DIC “HPB-8151-62T”, active group equivalent approx. 238 g / eq., toluene solution of 62 mass% non-volatile component), and
[0226] 3) Two parts of phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical, a 1:1 solution of cyclohexanone:methyl ethyl ketone (MEK) with a solid content of 30 mass%, Mw=35,000) were added.
[0227] Resin composition 4 was prepared in the same manner as resin composition 1, except for the above details.
[0228] <Preparation of Resin Composition 5>
[0229] In the preparation of resin composition 4, 30 parts of inorganic filler 1 were replaced with 30 parts of inorganic filler 2. Except for the above, resin composition 5 was prepared in the same manner as resin composition 4.
[0230] The components used in the preparation of resin compositions 1 to 5 and their blending amounts (mass parts of non-volatile components) are shown in the table below. In addition, the content of the curing agent and the active ester-based resin represents the content when the resin component in the resin composition is 100 mass%, and the content of component (a) represents the content when the non-volatile component in the resin composition is 100 mass%.
[0231]
[0232] Measurement of Coefficient of Thermal Expansion (CTE)
[0233] (Preparation of cured material for evaluation)
[0234] A glass cloth-based epoxy resin double-sided copper laminate (Matsushita Denko Corporation “R5715ES”, thickness 0.7 mm, 255 mm) was stacked on the untreated side of a release agent-treated PET film (Lintek Corporation “501010”, thickness 38 μm, 240 mm square) and the four sides were fixed with polyimide adhesive tape (width 10 mm) (hereinafter, “fixed PET film”).
[0235] Resin compositions 1 to 5 were applied using a die coater onto a PET film (Torre Corporation’s “Lumira R80”, thickness 38 μm, softening point 130°C, hereinafter “Release PET”) that had been treated with an alkyd resin-based release agent (“AL-5”) manufactured by Lintec Co., Ltd., so that the thickness of the resin composition layer after drying was 40 μm, and dried at 80°C to 120°C (average 100°C) for 10 minutes to obtain a resin sheet. Each resin sheet (thickness 40 μm, 200 mm each) was laminated in the center using a batch-type vacuum pressure laminator (2-stage build-up laminator, CVP700 manufactured by Nikko Materials Co., Ltd.) so that the resin composition layer was in contact with the release agent-treated surface of the fixed PET film, thereby obtaining a resin sheet. The lamination treatment was carried out by depressurizing for 30 seconds to lower the atmospheric pressure to 13 hPa or less, and then compressing for 30 seconds at 100°C and a pressure of 0.74 MPa.
[0236] Next, under temperature conditions of 100°C, it was placed in an oven at 100°C and heat-cured for 30 minutes, and then transferred to an oven at 175°C and heat-cured for 30 minutes under temperature conditions of 175°C. After that, the substrate was removed under a room temperature atmosphere, the release PET was peeled off from the resin sheet attached to the support, and then heat-cured under curing conditions of 90 minutes after being placed in an oven at 190°C.
[0237] After heat curing, the polyimide adhesive tape was peeled off, and the cured product was separated from the double-sided copper-clad laminate of epoxy resin on a glass sheet substrate. Additionally, a PET film (Lintec "501010") was also peeled off to obtain a sheet-like cured product. The obtained cured product is referred to as the "cured product for evaluation."
[0238] (Measurement of CTE)
[0239] The hardened material for evaluation was cut into a test specimen with a width of 5 mm and a length of 15 mm, and thermomechanical analysis was performed using the tensile weighting method with a thermomechanical analysis device ("Thermo Plus TMA8310" manufactured by Rigaku Co., Ltd.). Specifically, after mounting the test specimen on the thermomechanical analysis device, two consecutive measurements were taken under measurement conditions of a load of 1 g and a heating rate of 5°C / min. In the two measurements, the linear thermal expansion coefficient (ppm / °C) in the planar direction was calculated in the range from 25°C to 150°C. Furthermore, the calculated linear thermal expansion coefficient was evaluated according to the following criteria.
[0240] ◎: CTE 30 ppm / ℃ or less
[0241] ○: CTE exceeds 30 ppm / ℃ and is 40 ppm / ℃ or less
[0242] ×: CTE 40 ppm / ℃ or higher
[0243] <Production of Resin Sheets A and B>
[0244] As a support, a PET film ("Lumira R80" manufactured by Tore, thickness 38 μm, softening point 130°C, "Release PET") was prepared by releasing it with an alkyd resin-based release agent ("AL-5" manufactured by Lintec). Each resin composition 1 to 5 was uniformly coated onto the release agent of the support using a die coater so that the thickness of the resin composition layer after drying was 35 μm, and a resin composition layer was obtained on the release PET by drying at 70°C to 95°C for 2 minutes. Next, a rough surface of a polypropylene film ("Alpan MA-411" manufactured by Oji F-Tex, thickness 15 μm) was laminated as a protective film on the side of the resin sheet not bonded to the support, so as to bond it to the resin composition layer. Thus, a resin sheet A was obtained, consisting of the release PET (support), the resin composition layer, and the protective film in that order.
[0245] In addition, resin sheet B was obtained in the same manner as resin sheet A, except that each resin composition was uniformly coated with a die coater so that the thickness of the resin composition layer after drying was 15 μm.
[0246] <Measurement of thickness of resin composition layer, etc.>
[0247] The thickness of the resin composition layer was measured using a contact film thickness meter (manufactured by Mitutoyo Corporation, MCD-25MJ).
[0248] - Fabrication of evaluation boards A and B -
[0249] (1) Preparation of copper-clad laminate
[0250] As a copper-clad laminate, a glass-based epoxy resin double-sided copper-clad laminate (copper foil thickness 3 μm, substrate thickness 0.15 mm, manufactured by Mitsubishi Gas Chemical Co., Ltd. “HL832NSF LCA”, 255×340 mm size) with copper foil layers laminated on both sides was prepared, and after being placed in an oven at 130°C, it was dried for 30 minutes.
[0251] (2) Lamination of resin sheets
[0252] The protective film was removed from each prepared resin sheet A, and a batch-type vacuum pressure laminator (manufactured by Nikko Materials, 2-stage build-up laminator, CVP700) was used to laminate the resin composition layer to both sides of the copper-clad laminate so that it came into contact with the copper-clad laminate. The lamination was performed by depressurizing for 30 seconds to reduce the atmospheric pressure to 13 hPa or less, and then pressing at 130°C and a pressure of 0.74 MPa for 45 seconds. Subsequently, a heat press was performed at 120°C and a pressure of 0.5 MPa for 75 seconds.
[0253] (3) Thermosetting of the resin composition layer
[0254] A copper laminate laminate laminated with resin sheet A was placed in an oven at 100°C for 30 minutes, then transferred to an oven at 180°C for 30 minutes to heat-cure, thereby forming an insulating layer, and the support was peeled off. Thus, a copper laminate laminate A with a 35μm insulating layer was obtained.
[0255] In addition, copper laminate B with a 15μm insulating layer was obtained by making it in the same way as copper laminate A, except for using resin sheet B.
[0256] (4) Formation of a pattern on the dry film
[0257] A dry film with a thickness of 20 μm (manufactured by Nikko Materials, “ALPHO 20A263”) was laminated onto the surface of the insulating layer of copper laminate A, on which the insulating layer was formed. Lamination of the dry film was performed using a batch-type vacuum pressure laminator (manufactured by Meiki Sesakusho, “MVLP-500”), by depressurizing for 30 seconds to reduce the atmospheric pressure to 13 hPa or less, and then applying pressure for 20 seconds at a pressure of 0.1 MPa and a temperature of 70°C. Afterward, a glass mask having a trench pattern was placed on a polyethylene terephthalate film, which served as the protective layer of the dry film, and UV irradiation was performed using a UV lamp at an irradiation intensity of 150 mJ / cm². After UV irradiation, a 1% sodium carbonate aqueous solution at 30°C was sprayed for 30 seconds at a spray pressure of 0.15 MPa. After that, washing was performed, and patterning was performed to form a trench pattern with a wiring width of 20 μm, thereby obtaining a trench processed substrate.
[0258] In addition, a via processing substrate was obtained by using a glass mask having a via pattern to form via holes with a tower diameter of 15 μm on copper laminate B in the same way as on copper laminate A.
[0259] (5) Plasma processing
[0260] Examples 1 and 2, Example 4 and Comparative Examples 1 and 2 used a vacuum plasma etching apparatus (M120W manufactured by Nissin Co., Ltd.) and performed treatment for 5 minutes under conditions of a pressure of 120 Pa inside the chamber container with a mixing ratio of 1:7 (sccm) of CF4 / O2 to form a trench structure with a width of about 20 μm on the insulating layer on the trench processing substrate, and then peeled off the dry film to obtain a trench evaluation substrate.
[0261] In addition, a via hole with a top diameter (diameter) of about 15 μm was formed in the insulating layer of a via processing substrate in the same way as the trench evaluation substrate was fabricated, and then a dry film was peeled off to obtain a via evaluation substrate.
[0262] Example 3 was carried out in the same manner as Example 1, except that the CF4 / O2 mixed gas was replaced with O2 gas.
[0263] (6) UV-YAG laser via processing
[0264] Comparative Example 3 used a UV-YAG laser processing machine ("LU-2L212 / M50L" manufactured by Via Mechanics Co., Ltd.) and irradiated a laser light onto the insulating layer of copper-clad laminate B to form multiple via holes with a tower diameter (diameter) of approximately 15 μm. The laser light irradiation conditions were a power of 0.08 W and a number of shots of 25. This substrate was used as a laser evaluation substrate.
[0265] A laser evaluation substrate was immersed in a swelling solution, Swelling Deep Securigant P (aqueous solution of glycol ethers and sodium hydroxide) manufactured by Atotech Japan, at 60°C for 10 minutes, then immersed in a quenching solution, Concentrate Compact P (aqueous solution of KMnO4: 60 g / L and NaOH: 40 g / L) manufactured by Atotech Japan, at 80°C for 20 minutes, and finally immersed in a neutralizing solution, Reduction Solution Securigant P (aqueous solution of sulfuric acid) manufactured by Atotech Japan, at 40°C for 5 minutes, and then dried at 80°C for 30 minutes.
[0266] Observation of trench walls and via walls
[0267] After heating the trench evaluation substrate and via evaluation substrate at 150°C for 30 minutes, a copper layer (thickness 200 nm) was formed on the insulating layer using a sputtering device (E-400S manufactured by Canon Annelvas). Then, cross-sectional observation was performed using a FIB-SEM combined device (SMI3050SE manufactured by SII Nanotechnologies) and evaluated according to the following criteria.
[0268] ○: A copper layer is formed uniformly and without interruption on the wall of a trench or the wall of a via hole formed in the insulating layer.
[0269] ×: The copper layer is not uniformly formed due to irregularities.
[0270] <Via Hole Dimensions, Hollowing Distance Measurement>
[0271] The via evaluation substrate and the laser evaluation substrate after harmonization treatment were observed using an optical microscope (Hyrox "KH8700"). Specifically, the insulating layer around the via hole was observed from the top of the via evaluation substrate using an optical microscope (CCD). The dimensions of the via hole were observed by focusing the optical microscope on the via top. From the observed image, the diameter of the via hole top (Lt) was measured. Further observation revealed that around the via hole, a donut-shaped hollowing portion was visible where the insulating layer had turned white, extending continuously from the edge of the via top of the via hole. Therefore, from the observed image, the radius r1 of the via top of the via hole (equivalent to the inner circumference radius of the hollowing portion) and the outer circumference radius r2 of the hollowing portion were measured, and the difference between these radii r1 and r2, r2 - r1, was calculated as the hollowing distance from the edge of the via top at the measurement point.
[0272] The above measurements were performed at five randomly selected via holes. The average of the measured top diameters of the five via holes was adopted as the top diameter (Lt) of the via hole of the sample. Additionally, the average of the measured hollowing distances of the five via holes was adopted as the hollowing distance (Wt) from the edge of the via top of the sample.
[0273] The hollowing ratio (Ht) represents the ratio “Wt / (Lt / 2)” between the hollowing distance (Wt) from the edge of the via top and the radius (Lt / 2) of the via top of the via hole (the via hole after harmonic treatment in Comparative Example 3). If the hollowing ratio (Ht) is 35% or less, the hollowing evaluation is judged as “○”, and if the hollowing ratio (Ht) is greater than 35%, the hollowing evaluation is judged as “×”.
[0274] Explanation of the symbols
[0275] 100 insulation layers The surface of the insulating layer opposite to the 100U conductor layer 110 Via Hole 120 Via Bottom 120C Via Bottom Center 130 Via Top 140 discolored part 150 edge of the via bottom of the via hole 160 gap 170 End of the outer circumference of the gap 180 Via Top Edge 190 The rim of the outer edge of the discolored part 200 inner layer substrate 210 metal layer 1010 Weapon Filler 1020 Cured resin component 1030 Locations where weapon filler was excavated Bottom diameter of the Lb via hole Top diameter of Lt via hole Hollowing distance from the edge of the Wb via bottom Hollowing distance from the edge of the Wt via top
Claims
Claim 1 (A) a process of forming an insulating layer comprising a cured product of a resin composition on an inner layer circuit board and (B) a process of forming via holes or trenches by performing plasma treatment on the surface of the insulating layer, wherein the resin composition comprises an inorganic filler, and when the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass%, the average particle diameter of the inorganic filler is 0.1 μm or less, and when the content of the inorganic filler is 20 mass% or more and less than 50 mass%, the average particle diameter of the inorganic filler is 0.7 μm or less. Claim 2 A method for manufacturing a printed circuit board according to claim 1, further comprising (D) a process for forming a conductor layer. Claim 3 A method for manufacturing a printed circuit board, wherein, in paragraph 2, process (D) forms a conductive layer by sputtering. Claim 4 A method for manufacturing a printed circuit board according to claim 1, wherein the reactive gas used for plasma treatment includes O2. Claim 5 A method for manufacturing a printed circuit board according to claim 1, wherein the reactive gas used for plasma treatment comprises a mixed gas of O2 and CF4. Claim 6 A method for manufacturing a printed circuit board according to claim 1, wherein the linear thermal expansion coefficient of the cured resin composition is 10 ppm / ℃ or higher and 50 ppm / ℃ or lower. Claim 7 A method for manufacturing a printed circuit board according to claim 1, wherein the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass%. Claim 8 A method for manufacturing a printed circuit board according to claim 1, wherein the inorganic filler is silica. Claim 9 A method for manufacturing a printed circuit board according to claim 1, wherein the resin composition comprises (a) a curable resin, and (a) the curable resin comprises an epoxy resin and a curing agent. Claim 10 A resin composition for forming an insulating layer of a printed circuit board, comprising an inorganic filler having an average particle diameter of 0.1 μm or less, wherein the content of the inorganic filler is 50 mass% or more and 70 mass% or less when the non-volatile component in the resin composition is 100 mass%. A resin composition for forming via holes or trenches by plasma treatment in an insulating layer of a printed circuit board. Claim 11 A resin composition for forming an insulating layer of a printed circuit board, comprising an inorganic filler having an average particle diameter of 0.7 μm or less, wherein the content of the inorganic filler is 20 mass% or more and less than 50 mass% when the non-volatile component in the resin composition is 100 mass%. Claim 12 A resin composition according to claim 10 or 11, wherein the resin composition comprises (a) a curable resin, and (a) the curable resin comprises an epoxy resin and a curing agent. Claim 13 A resin composition according to claim 10 or 11, wherein the linear thermal expansion coefficient of the cured product of the resin composition is 20 ppm / ℃ or higher and 40 ppm / ℃ or lower.
Citation Information
Patent Citations
Apparatus for manufacturing printed circuit board and method for manufacturing printed circuit board using the same
KR1020100053771A
Laminated body, laminated board, multi-layer laminated board, printed wiring board, and production method for laminated board
KR1020140063711A
Circuit board and process for producing same
KR1020160016665A
Resin composition
KR1020170064482A
Use as a thermal expansion adjustment, heat -expanded resin composition, insulation material containing thermosetting resin compositions, insulation materials containing the thermosetting resin composition, a curing of a curing of the thermosetting resin composition, a substrate material having a thermosetting resin composition, and a thermosetting resin composition in the substrate. Prepe legs, the thermosetting resin composition of the prepreg, the method of adjusting the thermal swelling rate, and the member prepared using the adjustment method
KR1020170124537A