Protection processing method of device on wafer
A coating film applied to wafers during processing protects devices from contamination and damage, ensuring clean surfaces and reliable performance by preventing debris and oxide film issues.
Patent Information
- Application Number
- KR1020220038628
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-29
- Filing Date
- 2022-03-29
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2042-03-29
AI Technical Summary
Existing wafer processing methods fail to adequately protect devices from contamination by grinding and dicing debris, adhesive fragments, and oxide film damage during back grinding and dicing processes, leading to performance degradation, especially in imaging elements.
Applying a coating film to the wafer surface before processing, which covers the devices throughout grinding and dicing, using a combination of resins and additives that can be easily removed, to prevent contamination and damage.
The coating film effectively prevents contamination and damage, ensuring a clean, functional device surface throughout processing, allowing for reliable device performance and easy removal post-processing.
Smart Images

Figure 112022033649946-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an improvement in a processing method for a wafer having a plurality of devices formed on its surface. Background Technology
[0002] In a wafer having an LSI, CMOS, power device, or other pattern formed on a substrate such as silicon or sapphire, each device (device chip) is formed in multiple units by being partitioned by streets extending vertically and horizontally.
[0003] A wafer having multiple devices formed on such a surface needs to be made as thin as possible so that the thickness of the wafer containing the devices is reduced. To achieve this, the surface on the device side is covered and protected with an adhesive protective tape (back grind (BG) tape), and after fixing the BG tape side, a thinning (back grind) process is performed to reduce the thickness of the wafer by grinding the back side of the wafer.
[0004] After the wafer thinning treatment is finished, the back side is attached to a dicing tape installed on a wafer frame, and after peeling off the BG tape on the surface, the device is reorganized by dicing along the street with a high-speed rotating blade. After that, ultraviolet (UV) light is irradiated onto the dicing tape to weaken its adhesive action, the reorganized device is transferred to a shipping sheet, a pure cleaning is performed, the device is inspected, and then shipped to the next process.
[0005] In the above-mentioned conventional processes, during the back grinding and dicing processes on the back side of the wafer, it was often observed that fine particles, such as grinding chips, adhered to the device formed on the surface of the wafer and contaminated it.
[0006] In other words, during the grinding process on the back side of the wafer, it is difficult for the BG tape to sufficiently cover the surface of the device due to the height difference between the wafer surface and the device formed on the surface. As a result, grinding debris may enter between the wafer surface and the device and contaminate the device. In addition, the adhesive of the BG tape also causes contamination.
[0007] In addition, during the device refining process, a processing fluid is flowed between the wafer and the rotating dicing blade to cool the cutting area and reduce frictional resistance during cutting, thereby facilitating smooth dicing. Furthermore, cutting debris generated by dicing is removed by washing it away with water (pure water). However, it is difficult to sufficiently remove this cutting debris, and there are cases where it contaminates the device.
[0008] When dicing the above wafer, the wafer is attached to the back side with an adhesive dicing tape, and the dicing process is performed by fixing the dicing tape to the wafer frame.
[0009] When performing this dicing process, the dicing blade cuts each device along the street of the wafer. At this time, the cutting is performed by allowing the cutting tip of the dicing blade to enter the adhesive layer of the dicing tape attached to the wafer.
[0010] At this time, the dicing blade generates dicing debris from the wafer, and the blade's cutting edge rolls up the adhesive layer of the dicing tape, scattering it into fine fragments. Since these fine adhesive fragments are adhesive, they adhere to the surface of the device and cannot be washed away, thus becoming a cause of contamination.
[0011] In addition, the surface of the device formed on the wafer is covered by an oxide film. When this oxide film is cut into each device by the dicing blade, it is partially cracked and peeled off by the blade. It can be seen that the peeled oxide film scatters and scratches the surface of the device.
[0012] In particular, regarding imaging elements (image sensors) used in cameras, even the slightest attachment of dicing debris or fine pieces of adhesive to the lens (sensor pixel portion) on the surface of the device (chip), or scratching of the pixel portion, degrades the performance of the element and is a major cause of increased defect rates. Therefore, further improvements are required to avoid such phenomena.
[0013] In addition, the device, after the dicing process is finished and the device is reassembled, is transferred from the dicing tape to a sheet for shipment, cleaned with pure water, and then inspected for shipment to the next process. However, even during these processes, dust that is difficult to remove due to the manufacturing environment and the presence of workers adheres to the surface of the device, such as the imaging element, and the resulting performance degradation cannot be ignored. Prior art literature
[0014] Japanese Patent Publication No. 2003-94295 The problem to be solved
[0015] The present invention consistently and reliably protects the device from contamination caused by grinding debris or dicing debris generated from the wafer from the beginning of the back grinding process, in which the back surface of the wafer formed on the surface of the device is ground, until the end of the dicing process. Furthermore, it effectively prevents contamination of the device by fine adhesive fragments generated from the adhesive layer of the dicing tape, which are considered to have a more adverse effect than the grinding debris or dicing debris. Additionally, it reliably prevents damage to the device caused by the scattering of the oxide film fragments. means of solving the problem
[0016] From before entering the back grinding process, which grinds the back side of the wafer on which the device has been formed, through the back grinding process, until the device reorganization process is completed, the device on the wafer surface is consistently protected with a coating film, and the device on the wafer is processed while being protected.
[0017] In addition, a coating agent is applied to the surface of a wafer on which a device is formed to form a coating film, and a BG tape for back grinding is attached over it. The wafer is then thinned by fixing the surface side and grinding the back side. Next, the back side of the wafer is fixed with a dicing tape installed on a wafer frame, the BG tape is peeled off, and a reorganization process is performed to cut and divide the wafer into individual devices. Until this reorganization process is completed, the coating film consistently covers the surface of each device. After the reorganization process is finished, the coating film is cleaned and removed. Effects of the invention
[0018] According to the present invention, the surface of the device is consistently covered with a coating film from before entering the thinning process on the back side of the wafer on which the device is formed on the surface, until immediately before finishing the device remodeling process and shipping it to the next process. Accordingly, the device on the surface of the wafer is not contaminated at all during each of the above processing processes, and thus its function as a device can be reliably maintained.
[0019] In addition, this coating film prevents cutting debris generated by the dicing blade or adhesive fragments from the dicing tape from adhering to the surface of the device, and prevents damage to the device caused by scattering of partially peeled oxide films, and also prevents the adhesion of dust.
[0020] And since this coating film is cleanly removed by cleaning after the above consistent processing process, a refurbished device with a clean, contamination-free surface can be obtained. Brief explanation of the drawing
[0021] FIG. 1 is an explanatory diagram showing an overview of an embodiment of the protection treatment method of the present invention. Specific details for implementing the invention
[0022] After the process of forming a device on the surface of the wafer (1) is finished, the back side of the wafer is ground to thin the wafer.
[0023] This thinning of the wafer reduces the overall thickness of the device, thereby reducing the thickness of the mounting area. In addition, by reducing the volume occupied by the device, it enables integrated mounting.
[0024] Since a number of devices are formed on the surface of this wafer through streets extending in the longitudinal and transverse directions, the surface of the wafer is covered with a coating agent before entering the thinning process on the back side of the wafer (2).
[0025] As substrates for such coating agents, there are types of rosins such as gum rosin, wood rosin, rosin ester, hydrogenated rosin, hydrogenated rosin ester, polymerized rosin, polymerized rosin ester, maleic acid-modified rosin, and rosin-modified phenolic resin.
[0026] In addition, there are copolymers of (meth)acrylic acid and other copolymerizable monomers, and acrylic resins such as polyacrylic acid, polymethacrylic acid, and polyacrylamide.
[0027] Examples include epoxy resins such as phenol novolak type epoxy resin and cresol novolak type epoxy resin, as well as terpene resin, phenol resin, polyester resin, polypropylene glycol, etc.
[0028] Preferably as a substrate for the above coating agent, there is a mixture of rosin, terpene resin, acrylic resin, epoxy resin, phenolic resin, polyester resin, and polypropylene glycol as needed.
[0029] The average molecular weight of the acrylic resin is 1,000 to 100,000, and preferably about 6,000 to 35,000.
[0030] As described below, the substrate of the coating agent described above is particularly effective as a resin that can be removed by an alkaline cleaning solution such as an alkaline aqueous solution. Among such resins, examples include rosins, alkali-soluble acrylic resins, epoxy resins, etc., and mixtures thereof.
[0031] Polysaccharides, fatty acids, fatty acid esters, surfactants, etc., may be additionally added to the substrate of this coating agent. These may be used individually or in an appropriate mixture. These added components can improve the film-forming properties and washability of the coating agent.
[0032] Examples of the above additive components include polysaccharides such as cellulose, starch, and glycogen. Fatty acids include capronic acid, caprylic acid, palmitic acid, stearic acid, and lauric acid. Fatty acid esters include methyl capronic acid, ethyl capronic acid, methyl caprylic acid, and ethyl caprylic acid. Surfactants include anionic, cationic, nonionic, and amphoteric surfactants.
[0033] The glass transition point (Tg) of the above coating agent is not particularly limited, but it can be about 50 to 80°C.
[0034] The above-mentioned coating agent, additives, etc., can be appropriately mixed with an organic solvent and uniformly dissolved and dispersed by a known method to form a solution of typically about 10 to 40 mass% for use.
[0035] Examples of such organic solvents that can disperse the entire substance in a homogeneous state include alcohols, ethers, esters, ketones, and aromatics. These may be used individually or in combination of two or more.
[0036] This coating agent is applied to the surface of a wafer on which a device is formed by methods such as immersion, roll coating, spin coating, and spraying (2). Preferably, it is applied by spin coating and dried at about 80°C to 150°C to form a uniform coating film on the wafer surface.
[0037] The thickness of this coating film should be about 1.50 to 7.50 μm, and preferably about 2.00 to 4.50 μm.
[0038] It is desirable that the hardness of the coating film formed as described above be not too hard, but rather be approximately B to 2H in terms of pencil hardness.
[0039] On the surface of the wafer coated with such a coating agent, a known BG tape for a back grinding process, having an adhesive layer formed on one side of a plastic sheet, is further attached (3).
[0040] Then, the BG tape side covering the surface of the wafer is fixed, and the back side of the wafer is ground (back grind) (4) to thin the wafer.
[0041] At this time, even if the ground pieces of the wafer enter through the gap between the BG tape and the wafer surface, the device formed on the wafer surface is covered by a coating film, so the device is not contaminated.
[0042] When the above thinning treatment is finished, the back side is fixed by attaching it with dicing tape (5) and attached to the dicing frame.
[0043] Next, the BG tape is peeled off (6), and the thinned wafer covered by the coating film is sent to the next reorganization process (dicing) (7).
[0044] This reorganization process reorganizes each device by a dicing blade that rotates at high speed along longitudinal and transverse streets that isolate each device formed on the wafer surface for a fixed wafer.
[0045] In this dicing process, cutting fluid is supplied, and the dicing blade moves along the street, separating the blade into individual devices. At this time, cutting debris is ejected from the wafer by the cutting action of the blade. Additionally, during cutting, the tip of the blade penetrates into the adhesive layer of the dicing tape and the underlying dicing tape substrate, breaking them into smaller pieces and rolling them up.
[0046] These cutting debris or fragmented adhesives are removed by cutting water, but some are not sufficiently removed and remain. While the cutting debris of the wafer is relatively easy to remove, the fragments from the adhesive layer retain adhesiveness and have a tendency to adhere to the surface of the wafer. However, as described above, the device on the surface side of the wafer is covered by a coating film, so the device can be protected without contamination.
[0047] In addition, since the oxide film formed on the surface of the device is also covered by the aforementioned coating film, it is possible to effectively suppress the partial peeling (delamination) of the oxide film by the dicing blade and the scattering of the peeled oxide film fragments onto the surface of the device to cause damage.
[0048] After the above dicing is finished, the coating agent covering each device is cleaned and removed (8).
[0049] As a cleaning agent for removing the coating film formed by this coating agent, cleaning with an alkaline cleaning solution, such as an alkaline aqueous solution as described above, is particularly effective.
[0050] As such a cleaning agent, there is an alkaline aqueous solution composed of alkaline agents such as caustic soda, caustic potassium, and ammonia.
[0051] In addition, water-soluble solutions such as organic alkalis like alkanolamines, amyl alcohol, and water-soluble amines, and inorganic alkali salts like silicates or carbonates can be used.
[0052] In this way, when the coating film that consistently covered the surface of the device is removed, ultraviolet (UV) light is irradiated onto the adhesive layer of the dicing tape (9) to weaken the adhesiveness of the adhesive layer.
[0053] The reorganized device placed on the adhesive layer of the dicing tape with weakened adhesiveness is placed side by side on a sheet for shipment to the next process and moved (10).
[0054] After transferring the material onto a sheet for shipment, it is also thoroughly cleaned with pure water (11) to obtain a clean device free from contamination.
[0055] In this way, each device that has been cleaned can be sent to the next process after passing through an inspection process (12) and passing the specifications.
[0056] Depending on the case, the removal of the above-mentioned coating film may be performed after transferring the refurbished device onto a shipping sheet, and may also be performed afterward by thoroughly cleaning it with pure water.
[0057] (Example)
[0058] To produce the examples and comparative examples, a coating agent as described below was prepared.
[0059] Sample 1: A coating agent with an average molecular weight of 6,000, comprising 35% acrylic resin with a molecular weight of 10,000 or more, 25% acrylic resin with a molecular weight of less than 10,000, 32% rosin alcohol, and 8% plasticizer.
[0060] Sample 2: A coating agent with an average molecular weight of 8,000, comprising 47% acrylic resin with a molecular weight of 10,000 or more, 33% acrylic resin with a molecular weight of less than 10,000, 10% rosin alcohol, and 10% plasticizer.
[0061] Sample 3: A coating agent with an average molecular weight of 20,000, comprising 89% acrylic resin with a molecular weight of 10,000 or more, 11% acrylic resin with a molecular weight of less than 10,000, 0% rosin alcohol, and 0% plasticizer.
[0062] Sample 4: A coating agent with an average molecular weight of 25,000, comprising 74% acrylic resin with a molecular weight of 10,000 or more, 9% acrylic resin with a molecular weight of less than 10,000, 9% rosin alcohol, and 8% plasticizer.
[0063] Sample 5: A coating agent with an average molecular weight of 35,000, comprising 89% acrylic resin with a molecular weight of 10,000 or more, 11% acrylic resin with a molecular weight of less than 10,000, 0% rosin alcohol, and 0% plasticizer.
[0064] Examples 1 to 9 were prepared using the above sample.
[0065] (Example 1)
[0066] A coating agent was prepared by adding twice the amount (volume) of the solvent alcohol to Sample 1, and this coating agent was applied by spin coating to the surface of an 8-inch wafer having a CMOS image sensor formed as a device on a Si substrate to form a coating film with a thickness of 4.08 μm.
[0067] (Examples 2–9)
[0068] As shown in Table 1, samples 2 to 5 were used to form a coating film with the thickness shown in Table 1 in accordance with Example 1.
[0069] (Comparative Example 1)
[0070] Comparative Example 1 is one in which a coating agent is not used and a coating film is not formed, and otherwise it is the same as Example 1.
[0071] (test)
[0072] In Examples 1 to 9 and Comparative Example 1, the following tests were performed to observe the performance when a coating film was formed using a coating agent.
[0073] (Test of delamination occurrence rate)
[0074] After forming a coating film and performing the aforementioned series of wafer thinning and dicing treatments, and removing the coating film using a cleaning agent, the state of peeling (delamination) occurring on the oxide film on the device surface was observed using an external inspection device.
[0075] The delamination state of Comparative Example 1, which does not form a coating film, was set to 100%, and the state of the Example was similarly quantified and displayed as a percentage.
[0076] (metewand)
[0077] The smaller the value (%), the lower the rate of delamination occurring.
[0078] (test)
[0079] The results of the test are as shown in Table 1.
[0080] In addition, Table 1 also lists the glass transition points (Tg) (°C) of coating agent samples 1 to 5 and the pencil hardness of the formed coating film.
[0081] (Consideration)
[0082] In Examples 1 to 9, the occurrence rate of delamination of the oxide film on the device surface is 44 to 96%, which is lower than 100% in Comparative Example 1, and it can be seen that the formation of the coating film by the coating agent is effectively working to protect the device.
[0083] Explanation of the symbols
[0084] 1 Wafer forming the device 2. Application of coating agent 3 BG Tape Attachment 4 back grind 6 BG tape peeled off 7 Dicing 8. Remove coating agent
Claims
Claim 1 A method for protecting a device on a wafer by consistently protecting the device on the wafer surface with a coating film from before entering a thinning process (back grind) for grinding the back surface of a wafer on which a device is formed on the surface, through the back grind process, until the dicing process of the device is completed, wherein the coating film is formed with an acrylic resin-based surface coating agent, the acrylic resin-based surface coating agent is an acrylic resin-based surface coating agent in which multiple types of acrylic resins with different molecular weights are blended and the average molecular weight is adjusted to 6,000 to 8,000, and the thickness of the coating film is 1.50 to 7.50 μm. Claim 2 A method for protecting a device on a wafer, wherein a coating film is formed on the surface of a wafer on which a device is formed using a coating agent, a surface protection tape (BG tape) for back grinding is attached thereon, the surface side is fixed and the back side is ground (back grinding) to thin the wafer, the back side of the wafer is fixed with a dicing tape installed on a wafer frame, and the coating film that has been consistently covering the surface of the device is cleaned and removed until the reorganization process (dicing) of peeling off the BG tape and cutting and dividing the wafer into individual devices is completed, wherein the coating agent is an acrylic resin-based surface coating agent, the acrylic resin-based surface coating agent is an acrylic resin-based surface coating agent in which multiple types of acrylic resins with different molecular weights are blended and the average molecular weight is adjusted to 6,000 to 8,000, and the film thickness of the coating film is 1.50 to 7.50 μm. Claim 3 A method for protective treatment of a device according to claim 1 or 2, wherein the thickness of the coating film is 2.00 to 4.50 μm. Claim 4 A method for protective treatment of a device according to claim 1 or 2, wherein the pencil hardness of the coating film is B to 2H. Claim 5 In claim 3, a protective treatment method for a device in which the pencil hardness of the coating film is B to 2H. Claim 6 delete Claim 7 delete
Citation Information
Patent Citations
Processing method for wafer
JP2016115800A
Protection film composition and production method of semiconductor package by use thereof