A PET Waste-Derived Acoustic Absorption Material And A Manufacturing Method Thereof

By manufacturing sound-absorbing materials from waste PET using electrospinning and crosslinked nanofibers, the method addresses environmental pollution and enhances sound absorption across a wide frequency range, achieving effective noise reduction.

KR103045394B1Active Publication Date: 2026-11-06MYONGJI UNIV IND & ACAD COOPERATION FOUND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020230002354
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-01-06
Publication Date
2026-11-06
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

Existing sound-absorbing materials derived from waste PET struggle to effectively absorb sound waves across a wide frequency range, particularly in the low-frequency range, and contribute to environmental pollution due to non-biodegradability.

Method used

A method is developed to create sound-absorbing materials from waste PET using electrospinning technology to produce polyethylene terephthalate nanofibers, which are then processed into aerogels with perforations and crosslinked with glutaraldehyde, enhancing sound absorption and permeability.

Benefits of technology

The method improves sound absorption and transparency while reducing environmental impact by recycling PET waste, offering effective sound absorption across a broad frequency range and maintaining lightweight, flexible, and cost-effective properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023002420647-PAT00001_ABST
    Figure 112023002420647-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a sound-absorbing material derived from waste PET and a method for manufacturing the same. Specifically, it relates to a sound-absorbing material derived from waste PET and a method for manufacturing the same, which can improve sound absorption and sound permeability while recycling waste PET by manufacturing a sound-absorbing material containing polyethylene terephthalate nanofiber aerogel from waste PET through electrospinning.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a sound-absorbing material derived from waste PET and a method for manufacturing the same. Specifically, it relates to a sound-absorbing material derived from waste PET and a method for manufacturing the same, which can improve sound absorption and sound permeability while recycling waste PET by manufacturing a sound-absorbing material containing polyethylene terephthalate nanofiber aerogel from waste PET through electrospinning. Background Technology

[0002] It is undeniable that plastic is already a part of our daily lives. A world without plastic seems unimaginable today. With large-scale production and use dating back to around 1950, the rapid growth of plastic production is remarkable. Particularly in the packaging industry, where plastic is primarily used, the global shift from reusable to single-use containers has led to a dramatic increase in the proportion of plastic in urban solid waste (by mass), rising from less than 1% in 1960 to over 10% by 2005. Since most of these plastics originate from fossil hydrocarbons such as ethylene and propylene, they are generally non-biodegradable. Consequently, rather than decomposing, they accumulate and pile up in landfills or the natural environment. Only 9% of all plastic waste generated globally is recycled. Therefore, the majority of this total plastic waste pollutes our land and water. If these waste management trends continue, it is projected that 12 million tons of waste plastic will be dumped into landfills or our oceans by 2050. Poly(ethylene terephthalate) (PET) is considered the most widely used plastic for beverage packaging, such as water, soft drinks, and juices, due to its low weight, durability, excellent abrasion resistance, chemical resistance, and low market price. In 1987, over 350,000 tons of PET were consumed, and this figure has rapidly increased explosively. Among the classifications of PET recycling, (a) primary or mechanical recycling, (b) secondary or chemical recycling, and (c) tertiary recycling or the recovery of stored energy through incineration, mechanical recycling, and chemical upcycling are considered the most promising strategies. This is because incineration and landfill deposition are more polluting; in the latter case, PET waste completely loses its value. While mechanical processes such as crushing, extrusion, and melting may require low-cost operation, recycled materials generally have low value.Meanwhile, chemical recycling—dissolution (hydrolysis, methanol decomposition, and glycolysis) and other chemical recycling technologies (catalytic depolymerization and enzymatic depolymerization)—holds significant potential in the circular economy of plastics. This is because they can break the cycle by producing monomers, petroleum liquids, and gases that can be reprocessed to produce high-value chemicals. Similarly, tertiary recycling, including pyrolysis (pyrolysis, gasification, hydrocracking), photolysis, ultrasonic degradation, and microwave degradation, produces high-value products. While significant advancements have been made in chemical processing over the past few years, mechanical recycling remains a more mature and superior-performing technology. To date, PET accounts for 12% of global waste. Therefore, the current scenario demands a simple, ecological, and cost-effective pathway for recycling PET waste, which can disrupt the balance of our environment due to its non-biodegradability.

[0003] Here, we present an alternative method for recycling plastic waste by producing nanofibers from waste PET bottles using electrospinning technology, which are then used to manufacture aerogels that serve as sound absorbers and insulators for potential noise reduction. Due to rapid industrial development and the growth of urban areas, unpleasant noise generated from vehicles, machinery, aircraft, and subways has become a major issue today, negatively impacting human physiological and psychological well-being. This includes hearing loss, hypertension, and increased physiological stress. Indeed, noise pollution was identified by the World Health Organization (WHO) in 2011 as one of the critical factors directly adversely affecting public health. In particular, prolonged exposure to high levels of noise can induce neurocognitive dysfunction, mood disorders, and neurodegenerative diseases. Therefore, reducing noise levels is essential. To address these potential risks, the use of acoustic materials has been one of the strategies proposed to effectively reduce noise. This approach provides a sustainable ecological means to mitigate plastic accumulation while simultaneously resolving noise pollution. A wide range of materials is used for noise reduction, ranging from natural fibers (including cotton and wool) to synthetic materials such as melamine foam, polyurethane, and polyester. While these materials have been proven to effectively absorb sound, they are efficient in systems operating only in the high-frequency range. Such porous sound-absorbing materials act as dissipation media that convert sound into heat. On the other hand, low-frequency sound-absorbing materials operate using resonance, which limits them to a narrow range of absorption frequencies.

[0004] Conventional porous media based on foams and fibers possess efficient sound absorption capabilities, exhibiting a wide range of sound absorption frequencies and structural flexibility. However, due to their large pore structures, sound absorption performance in the low-frequency range is suppressed, requiring greater thickness to achieve satisfactory performance. Strategies to improve the sound absorption of these porous materials include reducing fiber diameter, increasing porosity, increasing bulk density, and increasing curvature. One approach receiving attention is the use of nanotechnology to enhance broadband acoustic absorption by creating nanoscale fibers. Thin fiber diameters provide a high surface-to-volume ratio, which is an ideal characteristic for manufacturing very lightweight porous materials. It has been proposed that when exposed to incident sound waves, the nanofiber layer promotes air friction within the nanopores and scatters sound from the fibers, thereby reducing the sound. Furthermore, the layer acts as an acoustic resonance membrane. Specific frequencies allow the nanofibers to vibrate, converting sound energy into thermal energy and efficiently attenuating the sound. Reinforced nanofibrous aerogel randomly deposited on nonwoven PET microfibers exhibiting a hierarchical porous structure enhanced sound absorption by inducing complexity in the sound transmission path. Significant broadband sound absorption was observed as a result of employing a gradient-structured micro / nanofiber approach based on polyvinylidene fluoride (PVDF) and polysulfone (PSU) to exhibit multiple dense, mixed, and fluffy layers of sound-absorbing materials. While recently reported approaches to improve low-frequency sound absorption in nanofiber materials have utilized perforations in poly(vinyl alcohol) (PVA) nanofiber membranes, the use of perforations for sound absorption dates back to the 1940s. Bolt demonstrated a perforated panel resonance structure to effectively reduce noise.However, Maa established a theoretical basis for predicting the sound absorption performance of microperforated materials based on electroacoustic equivalent circuits under simplified conditions. Such perforated plates are generally made of high-density and rigid materials. In this invention, a microperforated nanofiber aerogel is proposed as an attempt to achieve enhanced broadband sound absorption based on ultralightweight, flexibility, cost-effectiveness, sustainability, and eco-friendly materials. The problem to be solved

[0005] The technical problem to be solved by the present invention is to provide a sound-absorbing material derived from waste PET and a method for manufacturing the same, which is environmentally friendly and capable of improving sound absorption and sound permeability by including nanofibers with a thin diameter to complicate the path of pores through which sound waves pass and perforating the sound-absorbing material to absorb sound waves, and by manufacturing the sound-absorbing material from waste PET.

[0006] However, the problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem

[0007] One embodiment of the present invention provides a method for manufacturing a sound-absorbing material comprising the steps of: preparing a polyethylene terephthalate-based solution; electrospinning the polyethylene terephthalate-based solution to produce an electrospun polyethylene terephthalate nanofiber; pre-treating and freeze-drying the polyethylene terephthalate nanofiber to produce a polyethylene terephthalate nanofiber aerogel; and crosslinking the polyethylene terephthalate nanofiber aerogel.

[0008] According to one embodiment of the present invention, the step of preparing a polyethylene terephthalate nanofiber aerogel by pre-treating and freeze-drying the polyethylene terephthalate nanofiber further includes the step of adding a PVA solution after pre-treating the polyethylene terephthalate nanofiber, and the step of crosslinking the polyethylene terephthalate nanofiber aerogel may be crosslinked with a crosslinking agent containing glutaraldehyde.

[0009] According to one embodiment of the present invention, the PVA solution may be included in an amount of 3% or more and 10% by weight with respect to the polyethylene terephthalate nanofiber aerogel.

[0010] According to one embodiment of the present invention, the step of crosslinking the polyethylene terephthalate nanofiber aerogel may be to crosslink with a crosslinking agent comprising glutaraldehyde.

[0011] According to one embodiment of the present invention, the step of pretreating the polyethylene terephthalate nanofiber may include: a step of treating an alcohol-based mixture; a step of washing the polyethylene terephthalate nanofiber treated with the alcohol-based mixture; and a step of treating the washed polyethylene terephthalate nanofiber with an alkaline solution.

[0012] According to one embodiment of the present invention, the alkaline solution may be a 0.5 M or greater and 2 M or less M NaOH solution.

[0013] According to one embodiment of the present invention, the method may further include the step of manufacturing the polyethylene terephthalate nanofiber aerogel into a predetermined shape; and the step of processing a hole in the surface of the manufactured shape.

[0014] According to one embodiment of the present invention, a sound-absorbing material manufactured by the above manufacturing method is provided, wherein the sound-absorbing material comprises a plurality of holes.

[0015] According to one embodiment of the present invention, the thickness of the sound-absorbing material may be 10 cm or more and 45 cm or less, and the diameter of the sound-absorbing material may be 30 mm or more and 100 mm or less.

[0016] According to one embodiment of the present invention, the density of the sound-absorbing material is 0.0243 g / cm³ 3 Up to 0.0314 g / cm³ 3 It could be.

[0017] According to one embodiment of the present invention, the depth of the hole may be 25% or more and 75% or less of the thickness of the sound-absorbing material.

[0018] According to one embodiment of the present invention, the diameter of the hole may be 1 mm or more and 3 mm or less. Effects of the invention

[0019] A method for manufacturing a sound-absorbing material according to one embodiment of the present invention can prevent environmental pollution and improve the sound absorption performance of the sound-absorbing material by manufacturing a sound-absorbing material by preparing a solution from waste PET.

[0020] A sound-absorbing material according to one embodiment of the present invention can improve sound absorption and sound transparency. Brief explanation of the drawing

[0021] FIG. 1 is a schematic diagram illustrating the general manufacturing process for producing PET nanofiber (PETNF) aerogel according to one embodiment of the present invention, including the preparation of a PET solution, electrospinning, PETNF pretreatment, and the production of a PETNF aerogel. Figure 2(a) is an SEM image of electrospun PET nanofibers. Figure 2(b) is a photograph of PETNF aerogel. Figure 2(c) is an enlarged photograph of PETNF aerogel showing the crosslinking structure and actual morphology of PETNF. Figure 2(d) is a schematic diagram showing the structure of aerogel crosslinking using PVA and GA. Figure 2(e) is a graph showing the fiber diameter distribution of PETNF. Figure 2(f) is a graph showing the FTIR (Fourier Transform infrared) spectrum of PETNF according to the concentration of the crosslinking agent added to PETNF. Figure 2(g) is a graph showing the thermal decomposition profile (mass change with temperature) according to the concentration of the crosslinking agent added to PETNF. Fig. 3(a) is an actual photograph of PETNF aerogel and PU foam. Fig. 3(b) is an SEM image of PETNF aerogel (PETNF) with a PVA concentration of 0 wt%. Fig. 3(c) is an SEM image of PETNF aerogel (PETNF-0.1) with a PVA concentration of 3 wt%. Fig. 3(d) is an SEM image of PETNF aerogel (PETNF-0.3) with a PVA concentration of 7 wt%. Fig. 3(e) is an SEM image of PETNF aerogel (PETNF-0.5) with a PVA concentration of 10 wt%. Fig. 3(f) is an SEM image of a polyurethane (PU)-based commercial acoustic foam (CF). Figure 4(a) is a graph of the compressive stress-strain curve of PETNF aerogel (PETNF-0.1) with a PVA concentration of 3 wt%. Figure 4(b) is a graph of the compressive stress-strain curve of PETNF aerogel (PETNF-0.3) with a PVA concentration of 7 wt%. Figure 4(c) is a graph of the compressive stress-strain curve of PETNF aerogel (PETNF-0.5) with a PVA concentration of 10 wt%. Figure 4(d) is a photograph of PETNF aerogel during the axial and release cycles. Figure 4(e) is a graph showing the Young's modulus of PETNF aerogels prepared at various PVA concentrations. Fig. 5(a) is a photograph of a laser-cut PETNF aerogel sample with a thickness of 15 mm. Fig. 5(b) is a photograph of a laser-cut PETNF aerogel sample with a diameter of 100 mm for low-frequency and medium-frequency impedance measurements. Fig. 5(c) is a photograph of a laser-cut PETNF aerogel sample with a diameter of 30 mm for high-frequency impedance measurements. Fig. 5(d) is a diagram showing the impedance tube setup for sound absorption testing. Fig. 5(e) is a diagram showing the impedance tube setup for acoustic transmission testing. FIG. 6(a) is the sound absorption profile of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, and PETNF aerogels with a thickness of 15 mm and a PVA concentration of 3 wt% (PETNF-0.1-15), 7 wt% (PETNF-0.3-15), and 10 wt% (PETNF-0.5-15). FIG. 6(b) is the sound absorption profile of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, a commercial sound-absorbing material (CF-15) with a thickness of 30 mm, a PETNF aerogel with a thickness of 15 mm and a PVA concentration of 7 wt% (PETNF-0.3-15), and a PETNF aerogel with a thickness of 30 mm and a PVA concentration of 7 wt% (PETNF-0.3-30). FIG. 6(c) is the transmission loss profile of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, and PETNF aerogels with a thickness of 15 mm and PVA concentrations of 3 wt% (PETNF-0.1-15), 7 wt% (PETNF-0.3-15), and 10 wt% (PETNF-0.5-15). FIG. 6(b) is the transmission loss profile of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, a commercial sound-absorbing material (CF-15) with a thickness of 30 mm, a PETNF aerogel with a thickness of 15 mm and PVA concentration of 7 wt% (PETNF-0.3-15), and a PETNF aerogel with a thickness of 30 mm and PVA concentration of 7 wt% (PETNF-0.3-30). Figure 7(a) is a graph showing the effect of density on the noise reduction coefficient (NRC) of PETNF aerogel compared to a commercial polyurethane foam sound absorber. Figure 7(b) is a graph showing the noise reduction coefficient (NRC) of PETNF aerogel and a conventional fibrous sound absorber. Figure 7(c) is a graph showing the effect of Young's modulus on the sound transmission coefficient (STC). Figure 7(d) is a graph showing the effect of perforation diameter on the noise reduction coefficient and sound transmission coefficient of the PETNF aerogel sound absorber. Fig. 8(a) is a schematic diagram showing the manufacturing process of perforated PETNF aerogel. Fig. 8(b) is a photograph of a sample prepared for sound absorption and acoustic transmission tests. Fig. 8(c) is a schematic diagram showing sound propagation in a porous medium with perforations. Fig. 8(d) is a diagram showing the sound absorption profile of PETNF aerogel (PETNF-0.3-30) containing 7 wt% PVA concentration with a thickness of 30 mm according to perforation diameter (1D = 1 mm, 2D = 2 mm, 3D = 3 m). Fig. 8(e) is a diagram showing the transmission loss profile of PETNF aerogel (PETNF-0.3-30) containing 7 wt% PVA concentration with a thickness of 30 mm according to perforation diameter (1D = 1 mm, 2D = 2 mm, 3D = 3 m). FIG. 9 is a flowchart of a method for manufacturing a sound-absorbing material according to one embodiment of the present invention. Specific details for implementing the invention

[0022] In this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0023] In this specification, "A and / or B" means "A and B, or A or B".

[0025] The present invention will be described in more detail below.

[0027] One embodiment of the present invention provides a method for manufacturing a sound-absorbing material comprising the steps of: preparing a polyethylene terephthalate-based solution (S10); electrospinning the polyethylene terephthalate-based solution to produce an electrospun polyethylene terephthalate nanofiber (S20); pre-treating and freeze-drying the polyethylene terephthalate nanofiber to produce a polyethylene terephthalate nanofiber aerogel (S30); and crosslinking the polyethylene terephthalate nanofiber aerogel (S40).

[0028] A method for manufacturing a sound-absorbing material according to one embodiment of the present invention can prevent environmental pollution and improve the sound absorption performance of the sound-absorbing material by manufacturing a sound-absorbing material by preparing a solution from waste PET.

[0030] FIG. 9 is a flowchart of a method for manufacturing a sound-absorbing material according to one embodiment of the present invention. The method for manufacturing a sound-absorbing material according to the present invention will be described in detail with reference to FIG. 9.

[0031] According to one embodiment of the present invention, the method includes the step (S10) of preparing a polyethylene terephthalate-based solution. By including the step of preparing a polyethylene terephthalate-based solution as described above, the polyethylene terephthalate-based solution can be electrospun. In this specification, “polyethylene terephthalate-based solution” may mean the same as a PET solution.

[0032] According to one embodiment of the present invention, the polyethylene terephthalate-based solution may comprise polyethylene terephthalate, trifluoroacetic acid, and dichloromethane. As described above, by using the polyethylene terephthalate-based solution comprising polyethylene terephthalate, trifluoroacetic acid, and dichloromethane, the polyethylene terephthalate can be easily dissolved.

[0033] According to one embodiment of the present invention, the polyethylene terephthalate contained in the polyethylene terephthalate-based solution may be derived from waste PET. By using polyethylene terephthalate derived from waste PET as described above, the recycling rate of waste PET can be increased.

[0034] According to one embodiment of the present invention, the step of preparing the polyethylene terephthalate-based solution (S10) may include the step of cutting waste PET into a predetermined size (S11); and the step of dissolving the cut waste PET in a solvent (S15). By including the step of cutting waste PET into a predetermined size (S11) as described above; and the step of dissolving the cut waste PET in a solvent (S15), the waste PET can be easily dissolved in the solvent.

[0035] According to one embodiment of the present invention, the solvent may comprise trifluoroacetic acid and dichloromethane. By using a solvent comprising trifluoroacetic acid and dichloromethane as described above, a PET solution can be easily prepared.

[0036] According to one embodiment of the present invention, the weight ratio of trifluoroacetic acid and dichloromethane in the solvent may be 1:0.5 or higher and 1:2 or lower. By adjusting the weight ratio of trifluoroacetic acid and dichloromethane in the solvent within the above-described range, a PET solution can be easily prepared.

[0037] According to one embodiment of the present invention, after the step (S11) of cutting waste PET into a predetermined size, the method may include the step (S12) of washing the cut waste PET and the step (S13) of drying the washed waste PET. Specifically, the step (S13) of drying the waste PET may be performed prior to the step (S15) of dissolving the cut waste PET in a solvent. By including the step (S12) of washing the cut waste PET and the step (S13) of drying the washed waste PET after the step (S11) of cutting waste PET into a predetermined size as described above, the inclusion of foreign substances in the polyethylene terephthalate-based solution can be minimized, and the polyethylene terephthalate-based solution can be prevented from being contaminated by the liquid remaining after washing.

[0038] According to one embodiment of the present invention, the method may further include the step of preparing the polyethylene terephthalate-based solution (S10); and the step of removing gas generated from the polyethylene terephthalate-based solution (S17). By further including the step of preparing the polyethylene terephthalate-based solution (S10) as described above; and the step of removing gas generated from the polyethylene terephthalate-based solution (S17), the uniformity of the polyethylene terephthalate nanofibers can be improved.

[0039] According to one embodiment of the present invention, the step (S17) of removing gas generated in the polyethylene terephthalate-based solution may be performed for 4 hours or more and 24 hours or less. By controlling the step (S17) of removing gas generated in the polyethylene terephthalate-based solution within the above-described range, the uniformity of the polyethylene terephthalate nanofibers can be improved.

[0040] According to one embodiment of the present invention, the polyethylene terephthalate in the polyethylene terephthalate-based solution may contain at least 5% by weight and at least 20% by weight of polyethylene terephthalate. By controlling the concentration of polyethylene terephthalate in the polyethylene terephthalate-based solution within the above-described range, electrospinning can be easily performed.

[0041] According to one embodiment of the present invention, the method comprises the step (S20) of producing an electrospun polyethylene terephthalate nanofiber by electrospinning the polyethylene terephthalate-based solution. By including the step (S20) of producing an electrospun polyethylene terephthalate nanofiber by electrospinning the polyethylene terephthalate-based solution as described above, the polyethylene terephthalate nanofiber can be easily produced and the diameter of the nanofiber can be controlled. In this specification, “PET nanofiber” or “PETNF’” may refer to a polyethylene terephthalate nanofiber.

[0042] According to one embodiment of the present invention, the electrospinning may be performed by applying a voltage of 10 kV or more and 20 kV or less. By controlling the voltage of the electrospinning within the above-described range, polyethylene terephthalate nanofibers can be easily manufactured and the diameter of the nanofibers can be controlled.

[0043] According to one embodiment of the present invention, the injection rate of the polyethylene terephthalate-based solution in the electrospinning may be 0.5 mL / hr or more and 2.0 mL / hr or less. By controlling the injection rate in the electrospinning within the above-described range, polyethylene terephthalate nanofibers can be easily manufactured and the diameter of the nanofibers can be controlled.

[0044] According to one embodiment of the present invention, the polyethylene terephthalate-based solution may be extruded by a nozzle in the electrospinning. By implementing the electrospinning in such a way that the polyethylene terephthalate-based solution is extruded by a nozzle as described above, the diameter of the nanofiber can be controlled.

[0045] According to one embodiment of the present invention, the diameter of the nozzle may be 20 G or more and 30 G or less. By adjusting the diameter of the nozzle within the above-described range, the diameter of the nanofiber can be adjusted.

[0046] According to one embodiment of the present invention, the distance between the tip of the nozzle and the object to be spun in the electrospinning may be 10 cm or more and 20 cm or less. By adjusting the distance between the tip of the nozzle and the object to be spun in the electrospinning within the above-described range, the thickness of the polyethylene terephthalate nanofiber mat can be controlled.

[0047] According to one embodiment of the present invention, the spinneret may be a rolling drum covered with aluminum foil, and the electrospun polyethylene terephthalate nanofibers may be collected in a mat shape. As described above, the spinneret may be a rolling drum covered with aluminum foil, and by collecting the electrospun polyethylene terephthalate nanofibers in a mat shape, it is possible to prevent the polyethylene terephthalate nanofibers from being contaminated with foreign substances, etc.

[0048] According to one embodiment of the present invention, the method may further include the step (S20) of producing an electrospun polyethylene terephthalate nanofiber, which is an electrospun product, by electrospinning the polyethylene terephthalate-based solution; and the step (S25) of vacuum drying the polyethylene terephthalate nanofiber thereafter. As described above, by further including the step (S20) of producing an electrospun polyethylene terephthalate nanofiber, which is an electrospun product, by electrospinning the polyethylene terephthalate-based solution; and the step (S25) of vacuum drying the polyethylene terephthalate nanofiber thereafter, residual solvent can be removed.

[0049] According to one embodiment of the present invention, the method comprises the step (S30) of pre-treating and freeze-drying the polyethylene terephthalate nanofibers to produce a polyethylene terephthalate nanofiber aerogel. Specifically, the method comprises the step (S30A) of pre-treating the polyethylene terephthalate nanofibers and the step (S30B) of freeze-drying the pre-treated polyethylene terephthalate nanofibers to produce a polyethylene terephthalate nanofiber aerogel.

[0050] As described above, by including the step (S30) of pre-treating and freeze-drying the polyethylene terephthalate nanofibers to produce a polyethylene terephthalate nanofiber aerogel, the mechanical properties of the polyethylene terephthalate nanofiber aerogel can be improved.

[0051] According to one embodiment of the present invention, the step of pretreating the polyethylene terephthalate nanofiber (S30A) may include the step of treating an alcohol-based mixture (S31); the step of washing the polyethylene terephthalate nanofiber treated with the alcohol-based mixture (S33); and the step of treating the washed polyethylene terephthalate nanofiber with an alkaline solution (S35). As described above, by including the step of pretreating the polyethylene terephthalate nanofiber (S30A) in the step of treating the polyethylene terephthalate nanofiber (S31); the step of washing the polyethylene terephthalate nanofiber treated with the alcohol-based mixture (S33); and the step of treating the washed polyethylene terephthalate nanofiber with an alkaline solution (S35), the modification efficiency of the polyethylene terephthalate nanofiber by PVA can be improved.

[0052] According to one embodiment of the present invention, the alcohol-based mixture may be a water / t-BuOH mixture. By using the alcohol-based mixture as a water / t-BuOH mixture as described above, foreign substances can be easily removed from the surface of the polyethylene terephthalate nanofiber.

[0053] According to one embodiment of the present invention, the alcohol-based mixture may be a mixture of water and t-BuOH in a weight ratio of 5:1 to 20:1. By adjusting the weight ratio of the water and t-BuOH mixture within the above-described range, foreign substances on the surface of the polyethylene terephthalate nanofiber can be easily removed.

[0054] According to one embodiment of the present invention, in the step (S30) of pre-treating the polyethylene terephthalate nanofiber, the step (S1) of treating the alcohol-based mixture may be performed for 12 hours or more and 48 hours or less. As described above, by controlling the execution time of the step (S1) of treating the alcohol-based mixture in the step (S30) of pre-treating the polyethylene terephthalate nanofiber, foreign substances on the surface of the polyethylene terephthalate nanofiber can be easily removed.

[0055] According to one embodiment of the present invention, the step (S33) of washing the polyethylene terephthalate nanofibers treated with the alcohol-based mixture may be to wash with deionized water. As described above, by implementing the step (S33) of washing the polyethylene terephthalate nanofibers treated with the alcohol-based mixture as to washing with deionized water, foreign substances on the surface of the polyethylene terephthalate nanofibers can be easily removed.

[0056] According to one embodiment of the present invention, the step (S35) of treating the washed polyethylene terephthalate nanofibers with an alkaline solution may be to be stirred at a temperature of 50°C or higher and 80°C or lower for 1 minute or more and 10 minutes or less. By controlling the time and temperature of the step (S35) of treating the washed polyethylene terephthalate nanofibers with an alkaline solution within the above-described range, the polyethylene terephthalate nanofibers can be easily bonded with the PVA.

[0057] According to one embodiment of the present invention, the alkaline solution may be a 0.5 M or higher and 2 M or lower M NaOH solution. By controlling the concentration of the alkaline solution within the range described above, the polyethylene terephthalate nanofiber can be easily bonded with the PVA.

[0058] According to one embodiment of the present invention, the step (S30) of pre-treating and freeze-drying the polyethylene terephthalate nanofibers to produce a polyethylene terephthalate nanofiber aerogel may further include the step (S36) of adding a PVA solution after pre-treating the polyethylene terephthalate nanofibers. Specifically, it may be the step (S35) of treating the washed polyethylene terephthalate nanofibers with an alkaline solution followed by the addition of the PVA solution (S36). As described above, by further including the step (S36) of pre-treating and freeze-drying the polyethylene terephthalate nanofibers to produce a polyethylene terephthalate nanofiber aerogel, the step (S30) of pre-treating the polyethylene terephthalate nanofibers and adding a PVA solution, reaction sites to be combined with the crosslinking agent to be described later can be formed to enhance the degree of crosslinking while simultaneously increasing the density of the sound-absorbing material.

[0059] According to one embodiment of the present invention, the PVA solution may be in an amount of 3% by weight or more and 10% by weight with respect to the polyethylene terephthalate nanofiber aerogel. By controlling the content of the PVA solution within the above-described range, reaction sites to be combined with the crosslinking agent described later can be formed to increase the degree of crosslinking and at the same time increase the density of the sound-absorbing material.

[0060] According to one embodiment of the present invention, the polyethylene terephthalate nanofiber may be frozen (S37) prior to freeze-drying (S38). Specifically, the invention may further include a freezing step of freezing (S37) prior to freeze-drying (S38) the polyethylene terephthalate nanofiber. As described above, by freezing (S37) the polyethylene terephthalate nanofiber prior to freeze-drying (S38), it can be effectively dried.

[0061] According to one embodiment of the present invention, the freezing (S37) may be performed at -100°C or higher and -60°C or lower for 1 day or more and 7 days or less. By controlling the freezing temperature within the above-described range, the polyethylene terephthalate nanofiber can be easily freeze-dried.

[0062] According to one embodiment of the present invention, the method includes a step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel. By including the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel as described above, the density of the sound-absorbing material can be increased.

[0063] According to one embodiment of the present invention, the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel may be to crosslink using a crosslinking agent containing glutaraldehyde. As described above, by crosslinking the polyethylene terephthalate nanofiber aerogel using a crosslinking agent containing glutaraldehyde in the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel, the polyethylene terephthalate nanofiber aerogel can be easily crosslinked and the density of the sound-absorbing material can be increased.

[0064] According to one embodiment of the present invention, the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel may be performed in a sealed space. As described above, by performing the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel in a sealed space, the crosslinking efficiency can be improved.

[0065] According to one embodiment of the present invention, the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel may be to crosslink using steam in which the crosslinking agent has been evaporated. As described above, by implementing the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel by crosslinking using steam in which the crosslinking agent has been evaporated, the uniformity of the crosslinking can be improved.

[0066] According to one embodiment of the present invention, the crosslinking agent may be a mixture of glutaraldehyde and hydrochloric acid in a weight ratio of 2:1 or more and 4:1 or less. By controlling the weight ratio of glutaraldehyde and hydrochloric acid contained in the crosslinking agent as described above, the polyethylene terephthalate nanofiber aerogel can be easily crosslinked, and the density of the sound-absorbing material can be increased.

[0067] According to one embodiment of the present invention, after the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel, the crosslinked polyethylene terephthalate nanofiber aerogel may be vacuum dried (S45). Specifically, the method may further include the step (S45) of vacuum drying the crosslinked polyethylene terephthalate nanofiber aerogel after the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel. As described above, by vacuum drying the crosslinked polyethylene terephthalate nanofiber aerogel after the step (S40) of crosslinking the polyethylene terephthalate nanofiber aerogel, the crosslinking agent remaining after crosslinking can be removed.

[0068] According to one embodiment of the present invention, the vacuum drying (S45) may be performed at a temperature of 25°C or higher and 75°C or lower for 12 hours or more and 48 hours or less. By controlling the conditions of the vacuum drying (S45) as described above, the efficiency of removing the crosslinking agent remaining after crosslinking can be improved.

[0069] According to one embodiment of the present invention, the method may further include the step (S50) of manufacturing the polyethylene terephthalate nanofiber aerogel into a predetermined shape. By further including the step (S50) of manufacturing the polyethylene terephthalate nanofiber aerogel into a predetermined shape as described above, sound-absorbing materials can be manufactured in various shapes.

[0070] According to one embodiment of the present invention, the step (S60) of machining a hole in the surface of the manufactured shape may be further included. By further including the step (S60) of machining a hole in the surface of the manufactured shape as described above, the sound absorption efficiency of the sound-absorbing material can be improved.

[0071] According to one embodiment of the present invention, the step of manufacturing the polyethylene terephthalate nanofiber aerogel into a predetermined shape (S50); and the step of processing a hole on the surface of the manufactured shape (S60) may each be performed by cutting or drilling with a laser. As described above, by implementing the step of manufacturing the polyethylene terephthalate nanofiber aerogel into a predetermined shape (S50); and the step of processing a hole on the surface of the manufactured shape (S60) by cutting or drilling with a laser, the accuracy of the shape manufacturing and the size and location of the hole can be accurately formed.

[0073] One embodiment of the present invention provides a sound-absorbing material manufactured by the above manufacturing method, wherein the sound-absorbing material comprises a plurality of holes.

[0074] A sound-absorbing material according to one embodiment of the present invention can improve sound absorption and sound transparency.

[0075] According to one embodiment of the present invention, the thickness of the sound-absorbing material may be 10 cm or more and 45 cm or less. By adjusting the thickness of the sound-absorbing material within the above-described range, the sound-absorbing effect of the sound-absorbing material can be improved.

[0076] According to one embodiment of the present invention, the diameter of the sound-absorbing material may be 30 mm or more and 100 mm or less. By adjusting the diameter of the sound-absorbing material within the above-described range, the sound-absorbing effect of the sound-absorbing material can be improved.

[0077] According to one embodiment of the present invention, the density of the sound-absorbing material is 0.0243 g / cm³ 3 Up to 0.0314 g / cm³ 3 It may be. By adjusting the density of the sound-absorbing material within the aforementioned range, the sound-absorbing effect of the sound-absorbing material can be improved.

[0078] According to one embodiment of the present invention, the depth of the hole may be 25% or more and 75% or less of the thickness of the sound-absorbing material. By adjusting the depth of the hole within the above-described range, the sound-absorbing effect of the sound-absorbing material can be improved.

[0079] According to one embodiment of the present invention, the diameter of the hole may be 1 mm or more and 3 mm or less. By adjusting the diameter of the hole within the above-described range, the sound absorption effect of the sound-absorbing material can be improved.

[0080] According to one embodiment of the present invention, the plurality of holes may be formed at regular intervals on the surface of the sound-absorbing material. By forming the plurality of holes at regular intervals on the surface of the sound-absorbing material as described above, the sound absorption effect of the sound-absorbing material can be improved.

[0081] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention is not to be interpreted as being limited to the embodiments described below. The embodiments of this specification are provided to more completely explain the present invention to those with average knowledge in the art.

[0082] 1. Ingredients

[0083] Polyethylene terephthalate (hereinafter referred to as 'PET') was obtained from a local waste PET bottle generator. Trifluoroacetic acid (hereinafter referred to as 'TFA'), dichloromethane (hereinafter referred to as 'DCM'), poly(vinyl alcohol) (hereinafter referred to as 'PVA'), hydrochloric acid (HCl), glutaraldehyde (hereinafter referred to as 'GA'), and tert-butanol (t-BuOH) were purchased from Alfa Aesar and used without further purification.

[0084] 2. Fabrication of PET nanofibers (PETNF)

[0085] FIG. 1 is a schematic diagram illustrating the general manufacturing process for producing a PET nanofiber (hereinafter referred to as 'PETNF') aerogel according to one embodiment of the present invention, including the preparation of a PET solution, electrospinning, PETNF pretreatment, and the preparation of a PETNF aerogel. Referring to FIG. 1, a PET bottle was cut into small pieces (1 cm × 1 cm), washed thoroughly with water, completely dried, and then dissolved. A 15 wt% PET solution was prepared by dissolving PET in a solvent mixture of TFA and DCM (1:1 weight ratio). The PET solution was left overnight to remove gas. The degassed PET solution was electrospun at a voltage of 13 kV with an injection rate of 1 mL / hr and a spacing of 15 cm between the tips of the nozzles (nozzle diameter: 23G) and collected by a rolling drum covered with aluminum foil to produce a PETNF mat containing PET nanofibers (PETNF). The PETNF mat was dried under vacuum to remove residual solvent. It was kept in a dry state before use.

[0086] 3. Preparation of PETNF Aerogel

[0087] The above PETNF mat was cut into 1 cm x 1 cm pieces. The cut PETNF (5 g) was stirred in 500 mL of a water / t-BuOH mixture (10:1 weight ratio) at ambient temperature for 24 hours. The PETNF was thoroughly washed with deionized water prior to alkali treatment. The PETNF was treated by stirring in 330 mL of a 1 M NaOH solution at 65 °C for 5 minutes. The pre-treated PETNF was washed until all residual NaOH was removed. The PETNF was homogenized in 500 mL of deionized water for 2 minutes using an X-type blade. After adding a certain amount of PVA solution, it was homogenized for an additional 2 minutes. The mixture was immediately transferred to a mold (15 cm x 20 cm x 2.5 cm) and placed in a deep freezer to solidify at -80 °C for 4 days, and then freeze-dried (iLsin Biobase Freeze-dry-dryer) to obtain an ultralight aerogel with a thickness of 15 mm (see Fig. 1).

[0088] 4. Crosslinking of PETNF Aerogel

[0089] A GA / HCl (3:1) solution was prepared as a crosslinking agent. The PETNF aerogel was exposed to vapors generated by a solution (100 mL) containing the crosslinking agent in a sealed chamber at 25 °C for 24 hours. Subsequently, the crosslinked PETNF aerogel was vacuum dried for 24 hours and the residue was removed at 50 °C (see Fig. 1).

[0090] 5. Specialization

[0091] Scanning electron microscope (SEM) images of the sample were acquired using a field emission scanning electron microscope (FE-SEM), LEO Supra 55, Genesis 2000 (Carl Zeiss, EDAX). FTIR spectra of the sample were generated by a Nicole iS5, Thermo Scientific, coupled with an ATR Pike MIRacle. A Belsorp Mini X (Microtrac MRB) was used to determine the surface area of ​​the sample. The thermal properties of the sample were verified using a TGAN-1000 (Scinco). Mechanical properties were analyzed using a universal testing machine (UTM), LF Plus Lloyd Instruments.

[0092] 6. Sound Absorption and Acoustic Transmission Analysis

[0093] PETNF aerogel samples with diameters of 3 cm and 10 cm were prepared using a laser cutter. Similarly, perforations of various diameters (2 and 3 mm) were formed in the samples using a laser cutter. The acoustic characteristics of the sound absorption coefficient (SAC) and transmission loss (TL) values ​​of the PETNF sound-absorbing material samples were analyzed using an impedance tube (BSWA Technology). In cases where a gap existed between the inner wall of the impedance tube and the sample, petroleum gel was partially used.

[0094] 7. Results and Discussion

[0095] In one embodiment of the present invention, nanofibers (NF) were produced by electrospinning a 15 wt% PET solution into TFA / DCM as a result of parameter optimization. Fig. 2(a) is an SEM image of the electrospun PET nanofibers. Fig. 2(b) is a photograph of the PETNF aerogel. Fig. 2(c) is an enlarged photograph of the PETNF aerogel, capturing the crosslinking structure and actual morphology of the PETNF. Fig. 2(d) is a schematic diagram showing the structure of the aerogel crosslinking using PVA and GA. Fig. 2(e) is a graph showing the fiber diameter distribution of PETNF. Fig. 2(f) is a graph showing the Fourier Transform Infrared (FTIR) spectrum of PETNF according to the concentration of the crosslinking agent added to PETNF. Fig. 2(g) is a graph showing the thermal decomposition profile (mass change with temperature) according to the concentration of the crosslinking agent added to PETNF. As indicated in the SEM image of Fig. 2(a), the PETNF is linear, smooth, and bead-free. The PETNF described above has an average fiber diameter of 529 nm (see Fig. 2(e)). Pretreatment of the PETNF with sodium hydroxide is essential to support the overall 3D structure of the aerogel by forming ester and hydrogen bonds with PVA (see Figs. 2(b) and (c)). However, this step reduced the nanofiber diameter to approximately 483 nm. To further reinforce the PETNF aerogel structure, a GA crosslinking agent was introduced to form a scaffold network by creating acetal bridges not only between PVA and PET molecules but also between PVA molecules (Fig. 2(d)). An uncrosslinked control sample was prepared, and it was observed to collapse immediately upon removal from the mold after freeze-drying. To further support the successful crosslinking, the FTIR spectrum of the crosslinked aerogel was obtained. The 2199 cm⁻¹ region is attributed to the CH₄ region of PVA. -1The strong presence of the peak is shown in the IR spectrum in Fig. 2(f). The 1245 cm⁻¹ peak is attributed to the CO region of PET. -1 and 1095 cm -1 The intensity of the peak at 1724 cm⁻¹ increased, indicating the formation of ester bonds between PET and PVA molecules. -1 The CO of PET appearing in is also amplified due to the presence of the GA crosslinking agent. Furthermore, the presence of GA at 2855 cm -1 It is also confirmed that a peak appears at [location], which is attributed to the CH band of GA.

[0096] The effect of PVA on the overall mechanical stability of PETNF aerogels was analyzed by varying the concentration (3 wt%, 7 wt%, 10 wt%). Since PVA pellets do not dissolve easily in water, a 20 wt% PVA solution was prepared using deionized water before adding it to the PET-PVA mixture. Figure 3 shows SEM images of PETNF aerogels at different PVA concentrations, including a control sample which is a polyurethane (PU)-based commercial acoustic foam (CF). Figure 3(a) is an actual photograph of PETNF aerogels and PU foam. Figure 3(b) is an SEM image of PETNF aerogels (PETNF) with a PVA concentration of 0 wt%. Figure 3(c) is an SEM image of PETNF aerogels (PETNF-0.1) with a PVA concentration of 3 wt%. Figure 3(d) is an SEM image of PETNF aerogels (PETNF-0.3) with a PVA concentration of 7 wt%. Figure 3(e) is an SEM image of PETNF aerogel (PETNF-0.5) with a PVA concentration of 10 wt%. Figure 3(f) is an SEM image of a polyurethane (PU)-based commercial acoustic foam (CF). As can be seen in the pieces of PVA with multiple strands of PET nanofibers attached, crosslinking is evident in all samples (PETNF-0.5, PETNF-0.3, and PETNF-0.1, which contain 10 wt%, 7 wt%, and 3 wt% PVA, respectively). Similarly, the thermal decomposition profiles of the other PETNF samples were obtained using thermogravimetric analysis and are shown in Figure 2(g). Two major mass loss regions were observed. The first region is at approximately 250 °C and is due to the decomposition of PVA, and the second region is at approximately 450 °C and is due to the decomposition of PET. As PET crosslinked with PVA, the thermal stability of the PETNF aerogel was slightly improved. This also confirms the successful reinforcement of the aerogel with GA-crosslinked PVA. To further explain the successful crosslinking of PVA and PETNF, the mechanical properties of the PETNF aerogel were evaluated by Young's modulus.Figure 4(a) is a graph of the compressive stress-strain curve of PETNF aerogel (PETNF-0.1) with a PVA concentration of 3 wt%. Figure 4(b) is a graph of the compressive stress-strain curve of PETNF aerogel (PETNF-0.3) with a PVA concentration of 7 wt%. Figure 4(c) is a graph of the compressive stress-strain curve of PETNF aerogel (PETNF-0.5) with a PVA concentration of 10 wt%. Figure 4(d) is a photograph of PETNF aerogel during the axial and release cycles. Figure 4(e) is a graph showing the Young's modulus of PETNF aerogels prepared at various PVA concentrations. The compressive stress-strain profiles of each sample (see Figures 4 (a) to (c)) were measured using a universal testing machine. Furthermore, samples placed between the plates of a general-purpose testing machine were compressed at a strain of 1 mm / min and various maximum strains (40%, 60%, 80%) (see Fig. 4(d)). Even at a large strain of 80%, no plastic deformation was observed, and the PETNF aerogel could recover from shape deformation after the stress was removed. However, PETNF without PVA was not tested because it does not form a stable 3D structure; it collapses immediately upon removal from the mold. As the amount of PVA increases, an increasing trend in Young's modulus is observed, which may be due to more fibers being cross-linked (see Fig. 4(e)). Thus, the successful fabrication of flexible PETNF aerogel is achieved.

[0097] Nanofiber aerogels are ideal candidates for lightweight and efficient sound absorption because they exhibit a hierarchical structure, highly interconnected pores, and mechanical stability. Fig. 5(a) is a photograph of a laser-cut PETNF aerogel sample with a thickness of 15 mm. Fig. 5(b) is a photograph of a laser-cut PETNF aerogel sample with a diameter of 100 mm for low-frequency and mid-frequency impedance measurements. Fig. 5(c) is a photograph of a laser-cut PETNF aerogel sample with a diameter of 30 mm for high-frequency impedance measurements. Fig. 5(d) is a diagram showing the impedance tube setup for sound absorption testing. Fig. 5(e) is a diagram showing the impedance tube setup for acoustic transmission testing. To evaluate the acoustic characteristics of the above sound-absorbing material, PETNF aerogel with a thickness of 15 mm was laser-cut to obtain circular samples with diameters of 100 mm and 30 mm (see Figs. 5 (a) to (c)) and evaluated using an impedance tube. The absorption coefficient (SAC) and transmission loss (TL) were calculated using the method set in Figs. 5(d) and 5(e), respectively, and the data were measured within a frequency range of 63 Hz to 6300 Hz. For comparison, commercial polyurethane foam (CF), which is used as a porous sound-absorbing material similar to a sponge, was also tested at the same thickness as these PETNF aerogels (see Fig. 3). FIG. 6(a) is the sound absorption profile of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, and PETNF aerogels with a thickness of 15 mm and a PVA concentration of 3 wt% (PETNF-0.1-15), 7 wt% (PETNF-0.3-15), and 10 wt% (PETNF-0.5-15). FIG. 6(b) is the sound absorption profile of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, a commercial sound-absorbing material (CF-15) with a thickness of 30 mm, a PETNF aerogel with a thickness of 15 mm and a PVA concentration of 7 wt% (PETNF-0.3-15), and a PETNF aerogel with a thickness of 30 mm and a PVA concentration of 7 wt% (PETNF-0.3-30).Figure 6(c) shows the transmission loss profiles of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, and PETNF aerogels with a thickness of 15 mm containing 3 wt% (PETNF-0.1-15), 7 wt% (PETNF-0.3-15), and 10 wt% (PETNF-0.5-15) of PVA. Figure 6(b) shows the transmission loss profiles of a commercial sound-absorbing material (CF-15) with a thickness of 15 mm, a commercial sound-absorbing material (CF-15) with a thickness of 30 mm, a PETNF aerogel with a thickness of 15 mm containing 7 wt% (PETNF-0.3-15) of PVA, and a PETNF aerogel with a thickness of 30 mm containing 7 wt% (PETNF-0.3-30) of PVA. As in Figure 6(a), CF showed relatively poor sound absorption, particularly in the low-frequency and mid-frequency regions. The optimal SAC indicated by CF is observed at 0.33 in the range of 5000 Hz to 5600 Hz. However, as shown in Fig. 6 (a), the PETNF aerogel shows a major improvement in the SAC profile mainly in the mid-to-high frequency range. This significant increase in the sound absorption coefficient is basically attributed to the high density of the PETNF aerogel. Fig. 7(a) is a graph showing the effect of density on the noise reduction coefficient (NRC) of PETNF aerogel compared to a commercial polyurethane foam sound absorber. Fig. 7(b) is a graph showing the noise reduction coefficient (NRC) of PETNF aerogel and a conventional fibrous sound absorber. Fig. 7(c) is a graph showing the effect of Young's modulus on the sound transmission coefficient (STC). Fig. 7(d) is a graph showing the effect of perforation diameter on the noise reduction coefficient and sound transmission coefficient of the PETNF aerogel sound absorber. Specifically, Fig. 7(a) is 0.0243 g / cm. 3 Up to 0.0314 g / cm³ 3 It shows the density of the sound-absorbing material in the range of 0.0196 g / cm³. 3It is relatively higher than that of CF. Although CF has very high porosity, its relatively low density reduces the resistance between incident sound waves and the pore walls of CF. As shown in Figure 3, due to the large pore size of CF, sound propagates more easily compared to PETNF. Conversely, due to their supermicroscopic size, nanofibers tend to fill more space at the nanoscale. Therefore, this increases the density of the material. In this case, the collision frequency increases. Furthermore, as space is filled more, the pore distribution narrows, and as density increases, the maximum distribution of pore sizes decreases. Similarly, airflow resistivity increases with increasing density, which is because the distortion of the sound wave transmission path increases. The acoustic characteristics of the SAC of PETNF aerogel follow the Johnson-Champoux-Allard (JCA) model. Cao et al. reported an initial study on aerogels using nanofibers, in which the sound-absorbing material becomes a composite of microfibers and nanofibers. As a result of incorporating PAN / PVB nanofibers into the gaps of PET staple fibers, the noise reduction factor was significantly improved compared to known forms and approaches. However, as in the present invention, sound absorption performance was greatly enhanced by composing the entire sound-absorbing material with nanofibers, which can be observed in the SAC within the mid-frequency range. Sound-absorbing materials of the same thickness (15 mm) were compared. This improvement is primarily due to the increased density of the sound-absorbing material. Similar results can be detected in the remaining PETNF aerogel (see Fig. 6 (a)). When the PVA concentration is 3 wt%, PETNF-0.1 is 0.0299 g / cm³ 3 It exhibits a density, which provides the PETNF aerogel with an SAC of 0.26 to 0.7 in the mid-frequency range. When the PVA concentration is 7 wt%, the density of PETNF-0.3 is 0.0314 g / cm³. 3 It increased to. On the other hand, the density of PETNF-0.5 was 0.0243 g cm / 3And the SAC ranged from 0.24 to 0.76. Among the above PETNF aerogels, PETNF-0.3 exhibits superior sound absorption compared to the others. SAC depends not only on density but also on many other factors (in the case of the JCA model), such as porosity, distortion coefficient, airflow resistivity, viscous characteristic length, and thermal characteristic length. The effect of thickness on SAC is shown in Fig. 6(b). Considering the aerogel with the best sound absorption performance, the thickness of PETNF-0.3 was doubled to 30 mm, and an expansion of the sound absorption width at mid-range frequencies (175 Hz to 2000 Hz) was observed. Similar results were observed in CF, where mid-to-high frequency ranges were significantly improved. The thickness effect is not new, as it is an established characteristic in acoustics. This improvement is simply explained by the deviation in surface impedance, where the reflection of sound energy weakens as thickness increases. This indicates that more sound waves are absorbed by the sound-absorbing material. Therefore, the above PETNF aerogel can provide absorption performance similar to that of a commercial sound-absorbing material that is already twice as thick.

[0098] The Noise Reduction Coefficient (NRC) is used to evaluate the general acoustic characteristics of sound-absorbing materials such as wall panels, ceiling tiles, baffles, and banners. It describes the average sound absorption performance of the material, which is technically the average value of the absorption coefficient at octave band center frequencies of 250 Hz, 500 Hz, 1000 Hz, and 2000 Hz. An NRC of 0.0 indicates that the object reflects acoustic energy without attenuating mid-frequency sounds. An NRC value of 0.09 indicates that the CF sound-absorbing material actually has poor sound absorption performance (see Fig. 7(a)). Using PETNF aerogel as the sound-absorbing material can improve the NRC to >0.30. Increasing the thickness of the PETNF aerogel to 30 mm increases the NRC value to 0.58. Compared to some NRC values ​​reported for other sound-absorbing materials (see Fig. 7(b)), the PETNF aerogel prepared in the present invention generally outperforms most of these sound-absorbing materials. Most exhibit very high areal densities. However, their NRC values ​​are relatively low. This implies that thicker materials are required to achieve the desired performance. In the case of the PAN / PVB+PET aerogel, it can be seen that while its areal density is relatively lower than that of all materials shown in the figure, it has a higher NRC than most materials. On the other hand, the PETNF aerogel exhibits a higher areal density than the PAN / PVB+PET aerogel but shows the highest NRC among all materials. In fact, the sound-absorbing performance of the nanofiber aerogel can be controlled by adjusting the density of the material.

[0099] Another parameter to consider when designing sound-absorbing materials is the acoustic transmission class (STC). STC represents the ability of a material to provide sound insulation or noise control from one space to another. The transmission loss (TL) of PETNF aerogel was obtained using the method of Fig. 5(e), and the results are shown in Fig. 6(c). The STC was calculated based on the average of the transmission loss (TL) values ​​recorded at 34 different frequencies. It can be clearly observed that, compared to CF's 0.63 dB at the same thickness (15 mm), PETNF aerogel has a much higher STC of 5.3 dB (PETNF-0.1), 6.1 dB (PETNF-0.3), and 6.1 dB (PETNF-0.5) (see Fig. 7(c)). This implies that the use of nanofibers is better than simply using microfibers in terms of sound blocking. Transmission loss depends primarily on physical factors such as mass and stiffness. Since mass is related to density, we generally attribute the favorable permeability loss characteristics of PETNF aerogel to its relatively high density compared to sponge-type foams such as polyurethane CF. As in the case of PETNF-0.3, the STC increased from 5.3 dB to 6.1 dB as density increased. However, we observed that although the density of PETNF-0.5 was relatively lower, the STC remained equivalent to that of PETNF-0.3. To explain this, we examine the stiffness modulus. Stiffness is actually proportional to the Young's modulus of the material (see Fig. 7(c)). Therefore, when the modulus of PETNF-0.5 is 0.024 MPa, the TL remains equivalent to, if not slightly better than, that of PETNF-0.3. This is attributed to the formation of a more rigid network due to the additional amount of PVA. This made the aforementioned PETNF aerogel stiffer compared to those with a smaller amount of PVA. The dependence of STC on material thickness is also shown in Fig. 6(d).By doubling the material thickness, the STC improved significantly from 6.1 dB to 9.93 dB (PETNF-0.3 at a thickness of 30 mm), nearly two-thirds of the previous level (see Fig. 7(d)). On the other hand, the STC for the CF sound absorber improved only slightly from 0.63 dB to 1.1 dB, even though the thickness was doubled. However, this value for PETNF aerogel is still significantly lower than the minimum acceptable value (>25 dB) for useful sound insulation. This value is still not practical for commercial sound insulation. Nevertheless, this significant improvement could be practical in many other applications and could enhance overall acoustic performance when used in combination with other sound absorbers. Further modifications could promote higher STCs, thereby meeting the requirements for better sound insulation.

[0100] Conventional perforated panels and micro-perforated panels (MPPs) have been developed over the years to further regulate noise. The acoustic effects of perforated panels vary depending on the perforation rate, pore size, plate thickness, flow resistance, and installation conditions. Many studies have already reported on the effects of perforation on various materials such as metal plates, substrates, plastics, and foams. Recent studies on perforated nanofiber membranes have reported good sound absorption performance in both low and high frequency ranges. Microfabrication was performed by perforating these PVA nanofiber-based membranes. However, to our knowledge, this invention is the first to study and report perforation on nanofiber aerogels. Fig. 8(a) is a schematic diagram showing the manufacturing process of perforated PETNF aerogel. Fig. 8(b) is a photograph of a sample prepared for sound absorption and acoustic transmission tests. Fig. 8(c) is a schematic diagram showing sound propagation in a porous medium with perforations. Fig. 8(d) shows the sound absorption profile of a PETNF aerogel (PETNF-0.3-30) containing 7 wt% PVA concentration with a thickness of 30 mm according to perforation diameters (1D = 1 mm, 2D = 2 mm, 3D = 3 m). Fig. 8(e) shows the transmission loss profile of a PETNF aerogel (PETNF-0.3-30) containing 7 wt% PVA concentration with a thickness of 30 mm according to perforation diameters (1D = 1 mm, 2D = 2 mm, 3D = 3 m). Perforations of different diameters were created in the PETNF aerogel using a state-of-the-art laser cutter, and each pore is regularly spaced (see Figs. 8(a) and (b)). The spacing between each perforation was kept constant for all samples. To evaluate the final product, a perforated 15 mm thick aerogel was bonded to another standard slab of the same thickness (unperforated). Thus, a PETNF aerogel with a total thickness of 30 mm and a perforation depth of 15 mm was produced.The above sound-absorbing material is also referred to as a "dual-porous material" because it consists of two interconnected networks of pores of different characteristic sizes, namely micropores and mesopores. Micropores are pores formed during the manufacturing process of the nanofiber aerogel, and mesopores are perforations created through laser cutting (see Fig. 8(c)). In particular, in the mid-to-high frequency range (1000 Hz to 6300 Hz), the upper SAC increased when using 2 mm wide perforations (PETNF-0.3-30-2D). Specifically, at 2000 Hz, the sound absorption performance improved from 0.83 to 0.9 when using the SAC. This effect occurs through pressure changes in the micropores at the mesoscopic scale and an increase in the virtual portion of the material's macroscopic bulk modulus. This phenomenon was modeled and discussed in detail by Sgard et al. Figure 8 (c) illustrates the diffusion effect phenomenon occurring within the microporous aerogel for this type of configuration. The contour plot of the internal pressure of the material at the maximum absorption frequency showed the development of a boundary layer in the microporous aerogel around the pores. This essentially leads to increased sound absorption in the PETNF aerogel. When the pore diameter was increased to 3 mm (PETNF-0.3-30-3D), an additional increase in SAC occurred from 0.9 to 0.95. On the other hand, PETNF-0.3-30-1D with a pore diameter of 1 mm showed a significant decrease in SAC, particularly in the low-to-mid frequency range (63-2000 Hz). To obtain a significant increase in the sound absorption coefficient, the pore size, mesopority, and shape factor (depending on the pore shape and mesopority distribution) must be balanced to induce a pressure diffusion effect. This means that both microstructures and mesostructures must have substrate porosity and resistivity as high as possible, while maintaining the lowest possible curvature. Additionally, for certain geometries, the mesostructure must possess low mesoporeity with a large hole radius.If these conditions are not met, the pressure diffusion effect may become negligible or even non-existent. Modification of the PETNF aerogel may reduce the sound absorption properties of the material. This is evident in the case of PETNF-0.3-30-1D with a pore diameter of 1 mm. The low-to-mid frequency range was significantly reduced (see Fig. 8(d)). The opposite phenomenon occurs in the case of transmission loss (see Fig. 8(e)). The STC decreased from 9.93 dB to 8.6 dB with 2 mm wide perforations (PETNF-0.3-30-2D), and further decreased to 8.1 dB as the pore diameter reached 3 mm (PETNF-0.3-30-3D). Increasing the perforation ratio is expected to lead to a decrease in STC, which in turn reduces transmission loss. This phenomenon is already established and is evident at higher frequencies. In the case of PETNF-0.3-30-1D, the reduction in STC was also distinct, decreasing to 9.75 dB. However, the increase in STC values ​​above 2000 Hz is significant compared to PETNF-0.3-30-2D and PETNF-0.3-30-3D based on PETNF-0.330. This activity is similar to micro-perforated panels with holes in a scale of less than 1 mm. Micro-perforation improves the sound insulation properties of the material by creating resistance that restricts the movement of air inside the holes, resulting in a stiffness control regime. By controlling the hole diameter to less than 1 mm, the transmission loss performance of PETNF aerogel can actually be further improved at high frequencies, but conversely, it can limit the sound absorption of PETNF aerogel.

[0101] Accordingly, according to one embodiment of the present invention, the fabrication of a flexible PETNF aerogel proposes a method of utilizing waste plastic bottles as a porous medium for powerful applications, such as sound-absorbing materials for sound absorption and sound insulation. Here, nano-sized fibers were prepared by electrospinning PET, and a 3D pore network was fabricated by processing these fibers through freeze-drying and crosslinking. The highly tortuous pore structure created by the densely packed nanofibers is effective in absorbing sound waves, exhibiting an NRC value of 0.37 (actual density 465 g / m³) that is similar to or greater than that of most fiber-based acoustic materials. 2 It provides ). Similarly, when a porous medium is formed using nanofibers instead of microfibers, the overall transmission is improved. Nanofiber aerogel exhibits an STC of 6.1 dB, which is approximately 10 times that of commercial polyurethane-based acoustic foams. Since density and stiffness are the main factors affecting the acoustic transmission of PETNF aerogel, a material reinforced with glutaraldehyde-crosslinked PVA is used. Additionally, using dual porosity by creating perforations further enhances the sound absorption of the material, so the NRC is 0.54 (actual density 930 g / m³). 2 ...can be obtained. Perforation induces changes in pressure within micropores on a mesoscopic scale. However, this affects the sound insulation performance of PETNF aerogel, causing STC to decrease by 18% when the perforation diameter is 3 mm. However, maintaining it at 1 mm has a slight effect on STC. Explanation of the symbols

[0102] S10: Solution preparation step S20: Nanofiber manufacturing step S30: Nanofiber aerogel manufacturing step S40: Nanofiber aerogel crosslinking step S50: Shape manufacturing step S60: Hole machining step

Claims

Claim 1 A method for manufacturing a sound-absorbing material comprising: a step of preparing a polyethylene terephthalate-based solution; a step of manufacturing polyethylene terephthalate nanofibers, which are electrospun materials, by electrospinning the polyethylene terephthalate-based solution; a step of manufacturing a polyethylene terephthalate nanofiber aerogel by pretreating and freeze-drying the polyethylene terephthalate nanofibers; and a step of crosslinking the polyethylene terephthalate nanofiber aerogel, wherein the step of manufacturing the polyethylene terephthalate nanofiber aerogel by pretreating and freeze-drying the polyethylene terephthalate nanofibers further comprises a step of adding a PVA solution after pretreating the polyethylene terephthalate nanofibers, and the step of crosslinking the polyethylene terephthalate nanofiber aerogel is crosslinking with a crosslinking agent containing glutaraldehyde, and wherein the PVA solution is contained in an amount of more than 3% by weight and less than or equal to 7% by weight with respect to the polyethylene terephthalate nanofiber aerogel. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 A method for manufacturing a sound-absorbing material according to claim 1, wherein the step of pre-treating the polyethylene terephthalate nanofiber comprises: a step of treating with an alcohol-based mixture; a step of washing the polyethylene terephthalate nanofiber treated with the alcohol-based mixture; and a step of treating the washed polyethylene terephthalate nanofiber with an alkaline solution. Claim 6 A method for manufacturing a sound-absorbing material according to claim 5, wherein the alkaline solution is a 0.5 M or more and 2 M or less M NaOH solution. Claim 7 A method for manufacturing a sound-absorbing material according to claim 1, further comprising the steps of: manufacturing the polyethylene terephthalate nanofiber aerogel into a predetermined shape; and processing holes in the surface of the manufactured shape. Claim 8 A sound-absorbing material manufactured by the method of claim 1 comprises a plurality of holes, and the density of the sound-absorbing material is 0.0299 g / cm³ 3 Exceeding 0.0314 g / cm³ 3 Sound-absorbing material that is as follows. Claim 9 A sound-absorbing material according to claim 8, wherein the thickness of the sound-absorbing material is 10 cm or more and 45 cm or less, and the diameter of the sound-absorbing material is 30 mm or more and 100 mm or less. Claim 10 delete Claim 11 A sound-absorbing material according to claim 8, wherein the depth of the hole is 25% or more and 75% or less of the thickness of the sound-absorbing material. Claim 12 A sound-absorbing material according to claim 8, wherein the hole diameter is 1 mm or more and 3 mm or less.

Citation Information

Patent Citations

  • Sound absorption module panel with adjustable sound absorption rate

    KR101859463B1

  • Method for manufacturing non woven fabric

    KR101929160B1

  • Sound absorptive sheet having microresonance structure and method of manufacturing the same and sound absorption type soundproof panel using the same

    KR1020140073276A

  • Acoustic absorber

    JP2016121426A

  • Multilayered sound absorbing material

    WO2021117901A1