Hot-rolled steel sheet
A hot-rolled steel sheet with a specific chemical composition and metal structure addresses the need for high strength, limit fracture plate thickness reduction, and improved formability, enhancing its suitability for automotive and structural applications.
Patent Information
- Application Number
- KR1020247008763
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-11
- Filing Date
- 2022-09-14
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-09-14
AI Technical Summary
Existing hot-rolled steel sheets lack high strength, adequate limit fracture plate thickness reduction rate, and excellent hole expandability and shear workability, which are crucial for automotive components requiring precise formability and crash resistance.
A hot-rolled steel sheet with a specific chemical composition and metal structure, including a high percentage of martensite and tempered martensite, controlled Mn segregation, and a defined entropy value, ensuring high strength, improved hole expandability, and shear workability.
The steel sheet achieves high strength, excellent hole expandability, and shear workability, with suppressed cracking during bending, making it suitable for automotive, machine structural, and building components.
Smart Images

Figure 112024029160581-PCT00030_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a hot-rolled steel sheet. Specifically, it relates to a hot-rolled steel sheet that is formed into various shapes by press processing or the like and used, particularly a hot-rolled steel sheet having high strength and a limit fracture plate thickness reduction rate, and also having excellent hole expandability and shear workability.
[0002] The present application claims priority based on Japanese Patent Application No. 2021-166960 filed in Japan on October 11, 2021, and incorporates the contents thereof herein by reference. Background Technology
[0003] In recent years, many sectors have been working to reduce carbon dioxide emissions from the perspective of protecting the global environment. Automobile manufacturers are also actively developing technologies for vehicle body lightweighting aimed at improving fuel efficiency. However, since emphasis is also placed on improving crash resistance characteristics to ensure passenger safety, vehicle body lightweighting is not an easy task.
[0004] To achieve both vehicle body weight reduction and crash resistance, the use of high-strength steel sheets to thin components is being considered. Consequently, there is a strong demand for steel sheets that combine high strength with excellent formability, and several technologies have been proposed to meet these requirements. Since automotive components undergo various processing methods, the required formability varies depending on the component; however, among these, the reduction rate of plate thickness at the limit of fracture and hole expansion are positioned as important indicators of formability. The reduction rate of plate thickness at the limit of fracture is a value calculated from the minimum difference between the plate thickness of the tensile test specimen before fracture and the plate thickness after fracture. A low reduction rate is undesirable because it makes the material prone to premature fracture when tensile deformation is applied during press forming.
[0005] Automotive components are formed by press forming, but the blanks produced are often manufactured by shearing, which offers high productivity. For blanks manufactured by shearing, excellent precision of the end faces after the shearing process is required.
[0006] For example, if the linearity of the boundary between the fracture plane and the shear plane at the shear end plane is low, the precision of the shear end plane deteriorates significantly.
[0007] For example, Patent Document 1 discloses a hot-rolled steel sheet that serves as a material for a cold-rolled steel sheet with excellent surface properties after press processing, in which the degree of Mn segregation and the degree of P segregation in the central part of the sheet thickness are controlled.
[0008] However, in Patent Document 1, the limiting plate thickness reduction rate and shear workability of hot-rolled steel sheets are not considered. Prior art literature
[0009] International Publication No. 2020 / 044445
[0010] J. Webel, J. Gola, D. Britz, F. Mucklich, Materials Characterization 144 (2018) 584-596D. L. Naik, H. U. Sajid, R. Kiran, Metals 2019, 9, 546K. Zuiderveld, Contrast Limited Adaptive Histogram Equalization, Chapter VIII.5, Graphics Gems IV. P.S. Heckbert (Eds.), Cambridge, MA, Academic Press, 1994, pp.474-485 The problem to be solved
[0011] The present invention is made in consideration of the above-described circumstances and aims to provide a hot-rolled steel sheet having high strength and a reduction rate in plate thickness at the limit of fracture, as well as excellent hole expandability and shear workability. means of solving the problem
[0012] The gist of the present invention is as follows.
[0013] (1) A hot-rolled steel sheet according to one embodiment of the present invention has a chemical composition in mass%,
[0014] C: 0.040 to 0.250%,
[0015] Si: 0.05 to 3.00%,
[0016] Mn: 1.00 to 4.00%,
[0017] sol.Al: 0.001 to 0.500%,
[0018] P: 0.100% or less,
[0019] S: 0.0300% or less,
[0020] N: 0.1000% or less,
[0021] O: 0.0100% or less,
[0022] Ti: 0 to 0.300%,
[0023] Nb: 0 to 0.100%,
[0024] V: 0 to 0.500%,
[0025] Cu: 0 to 2.00%,
[0026] Cr: 0 to 2.00%,
[0027] Mo: 0 to 1.00%,
[0028] Ni: 0 to 2.00%,
[0029] B: 0 to 0.0100%,
[0030] Ca: 0 to 0.0200%,
[0031] Mg: 0 to 0.0200%,
[0032] REM: 0 to 0.1000%,
[0033] Bi: 0 to 0.0200%,
[0034] As: 0 to 0.100%,
[0035] Zr: 0 to 1.00%,
[0036] Co: 0 to 1.00%,
[0037] Zn: 0 to 1.00%,
[0038] W: 0 to 1.00%,
[0039] Sn: 0 to 0.05%, and
[0040] Remainder: Fe and impurities,
[0041] Satisfying the following equation (A),
[0042] Metal structure, in area %,
[0043] The total of martensite and tempered martensite is greater than 92.0% and less than or equal to 100.0%, and
[0044] The retained austenite is less than 3.0%, and
[0045] Ferrite is less than 5.0%, and
[0046] The entropy value represented by the following equation (1), obtained by analyzing the SEM image of the metal structure by the gray level co-generation matrix method, is 11.0 or higher, and
[0047] The inverse difference normalized value represented by the following equation (2) is less than 1.020, and
[0048] The Cluster Shade value represented by the following equation (3) is -8.0×10 5 Up to 8.0×10 5 And,
[0049] The standard deviation of the Mn concentration is 0.60 mass% or less, and
[0050] The tensile strength is 980 MPa or higher.
[0051]
[0052] However, each element symbol in the above formula (A) represents the content based on the mass % of the element, and if the element is not contained, 0% is substituted.
[0053] Here, P(i, j) in the following equations (1) to (5) is a gray level co-generation matrix, L in the following equation (2) is the number of gray scale levels that the SEM image can take, i and j in the following equations (2) and (3) are natural numbers from 1 to L, and μ in the following equation (3) x and μ y These are represented by the following equations (4) and (5), respectively.
[0054]
[0055]
[0056]
[0057]
[0058]
[0059] (2) The hot-rolled steel sheet described in (1) above may have an average crystal grain size of less than 3.0 μm on the surface layer.
[0060] (3) The hot-rolled steel sheet described in (1) or (2) above has the chemical composition in mass%,
[0061] Ti: 0.001 to 0.300%,
[0062] Nb: 0.001 to 0.100%,
[0063] V: 0.001 to 0.500%,
[0064] Cu: 0.01 to 2.00%,
[0065] Cr: 0.01 to 2.00%,
[0066] Mo: 0.01 to 1.00%,
[0067] Ni: 0.01 to 2.00%,
[0068] B: 0.0001 to 0.0100%,
[0069] Ca: 0.0001 to 0.0200%,
[0070] Mg: 0.0001 to 0.0200%,
[0071] REM: 0.0001 to 0.1000%,
[0072] Bi: 0.0001 to 0.0200%,
[0073] As: 0.001 to 0.100%,
[0074] Zr: 0.01 to 1.00%,
[0075] Co: 0.01 to 1.00%,
[0076] Zn: 0.01 to 1.00%,
[0077] W: 0.01 to 1.00%, and
[0078] Sn: 0.01 to 0.05%
[0079] It may contain one or more types selected from the group consisting of Effects of the invention
[0080] According to the above embodiment of the present invention, a hot-rolled steel sheet having high strength and a reduction rate of plate thickness at the limit of fracture, along with excellent hole expandability and shear workability, can be obtained. Furthermore, according to the above preferred embodiment of the present invention, a hot-rolled steel sheet having the above various characteristics and also having excellent crack resistance during bending, that is, in which the occurrence of cracks during bending is suppressed, can be obtained.
[0081] The hot-rolled steel sheet according to the above embodiment of the present invention is suitable as an industrial material used for automobile components, machine structural components, and furthermore, building components. Brief explanation of the drawing
[0082] Figure 1 is a drawing for explaining a method for measuring the linearity of the boundary between the fracture surface and the shear surface in the end surface after shear processing. Specific details for implementing the invention
[0083] The chemical composition and metal structure of the hot-rolled steel sheet according to the present embodiment are described in more detail below. However, the present invention is not limited to the configuration disclosed in the present embodiment, and various modifications are possible within the scope of the spirit of the present invention.
[0084] In the numerical limit ranges listed below separated by "to," lower and upper limits are included. In numerical values indicated as "less than" or "greater than," those values are not included in the numerical range. In the following description, % regarding chemical composition is mass % unless specifically designated.
[0085] Chemical composition
[0086] Hereinafter, the chemical composition of the hot-rolled steel sheet according to the present embodiment will be described in detail.
[0087] C: 0.040 to 0.250%
[0088] C increases the area ratio of the hard phase. In addition, C increases the strength of the martensite by combining with precipitation strengthening elements such as Ti, Nb, and V. If the C content is less than 0.040%, it becomes difficult to obtain the desired strength. Furthermore, if the C content is less than 0.040%, the ferrite fraction increases, and the I value also increases due to the influence of the flat ferrite structure. Therefore, the C content is set to 0.040% or more. The C content is preferably 0.060% or more, more preferably 0.070% or more, or 0.080% or more.
[0089] Meanwhile, if the C content exceeds 0.250%, the formation of low-strength pearlite is promoted, and the area ratio of martensite and tempered martensite decreases, thereby lowering the strength of the hot-rolled steel sheet. Additionally, if the C content exceeds 0.250%, the E value decreases due to the influence of increased flat cementite structure and the formation of carbide regions with small brightness differences. Therefore, the C content is set to 0.250% or less or 0.220% or less. The C content is preferably 0.200% or less, 0.170% or less, 0.150% or less, or 0.120% or less.
[0090] Si: 0.05 to 3.00%
[0091] Si has the effect of delaying the precipitation of cementite. Through this effect, the area ratio of martensite and tempered martensite can be increased, and the strength of hot-rolled steel sheets can also be increased through solid solution strengthening. In addition, Si has the effect of soundening the steel through deoxidation (suppressing the occurrence of defects such as blowholes in the steel). If the Si content is less than 0.05%, the effect due to the above action cannot be obtained. Furthermore, if the Si content is less than 0.05%, the flat cementite structure increases, and the I value also increases due to the influence of the formation of carbide regions with small luminance differences. Therefore, the Si content is 0.05% or more. The Si content is preferably 0.50% or more, 0.80% or more, or 1.00% or more.
[0092] Meanwhile, if the Si content exceeds 3.00%, the surface properties, chemical treatment properties, and weldability of the steel sheet deteriorate significantly, and the A3 transformation point rises significantly. As a result, it becomes difficult to perform hot rolling stably. In addition, if the Si content exceeds 3.00%, the area ratio of ferrite increases, and the E value decreases due to the influence of the flat ferrite structure. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.70% or less, more preferably 2.50% or less, 2.20% or less, 2.00% or less, 1.80% or less, or 1.50% or less.
[0093] Mn: 1.00 to 4.00%
[0094] Mn has the effect of increasing the strength of hot-rolled steel sheets by suppressing ferrite transformation. If the Mn content is less than 1.00%, the desired strength cannot be obtained. Therefore, the Mn content is 1.00% or more. The Mn content is preferably 1.50% or more, 2.00% or more, or 2.30% or more.
[0095] On the other hand, if the Mn content exceeds 4.00%, the difference in crystal orientation of the grains in the hard phase becomes non-uniform due to Mn segregation, and the linearity of the boundary between the fracture plane and the shear plane at the end plane after shear processing is reduced. In addition, if the Mn content exceeds 4.00%, the area ratio of retained austenite increases, and the I value also increases due to the influence of the flat retained austenite structure. Therefore, the Mn content is set to 4.00% or less. The Mn content is preferably 3.70% or less, 3.50% or less, 3.20% or less, or 2.90% or less.
[0096] sol.Al: 0.001 to 0.500%
[0097] Al, like Si, has the effect of soundening the steel through deoxidation and, by suppressing the precipitation of cementite from austenite, has the effect of increasing the area ratio of martensite and tempered martensite. If the sol.Al content is less than 0.001%, the effect of the above action cannot be obtained. Therefore, the sol.Al content is 0.001% or more. The sol.Al content is preferably 0.010% or more, 0.030% or more, or 0.050% or more, and more preferably 0.080% or more, 0.100% or more, or 0.150% or more.
[0098] Meanwhile, if the sol.Al content exceeds 0.500%, the above effect becomes saturated and is not economically desirable, so the sol.Al content is set to 0.500% or less. The sol.Al content is preferably 0.400% or less, or more preferably 0.300% or less or 0.250% or less.
[0099] In addition, in this embodiment, sol.Al means acid-soluble Al and represents solid solution Al present in the steel in a solid solution state.
[0100] P: 0.100% or less
[0101] P is an element that is generally contained as an impurity, but it is also an element that has the effect of increasing strength through solid solution strengthening. Therefore, it is acceptable to actively include P; however, P is an element prone to segregation, and if the P content exceeds 0.100%, the reduction rate of plate thickness at the limit fracture caused by grain boundary segregation becomes significant. Therefore, the P content is set to 0.100% or less. The P content is preferably 0.050% or less, 0.030% or less, 0.020% or less, or 0.015% or less. Although there is no need to specifically specify a lower limit for the P content, the lower limit for the P content is 0%. From the perspective of refining costs, it may be set to 0.001%, 0.003%, or 0.005%.
[0102] S: 0.0300% or less
[0103] S is an element contained as an impurity and forms sulfide inclusions in the steel, thereby reducing the hole expandability and the limit fracture plate thickness reduction rate of hot-rolled steel sheets. If the S content exceeds 0.0300%, the hole expandability and the limit fracture plate thickness reduction rate of hot-rolled steel sheets are significantly reduced. Therefore, the S content is set to 0.0300% or less. The S content is preferably 0.0100% or less, 0.0070% or less, or 0.0050% or less. Although there is no need to specifically specify a lower limit for the S content, the lower limit for the S content is 0%. From the perspective of refining costs, the lower limit for the S content may be set to 0.0001%, 0.0005%, 0.0010%, or 0.0020%.
[0104] N: 0.1000% or less
[0105] N is an element contained in steel as an impurity and has the effect of reducing the hole expandability and the limit fracture plate thickness reduction rate of hot-rolled steel sheets. If the N content exceeds 0.1000%, the hole expandability and the limit fracture plate thickness reduction rate of hot-rolled steel sheets are significantly reduced. Therefore, the N content is set to 0.1000% or less. The N content is preferably 0.0800% or less, and more preferably 0.0700% or less or 0.0500% or less.
[0106] There is no need to specifically specify a lower limit for the N content, but the lower limit for the N content is 0%. The lower limit for the N content may be 0.0001%. As described below, when refining the metal structure by including one or more of Ti, Nb, and V, it is preferable to have an N content of 0.0010% or more to promote the precipitation of carbonitrides, and it is more preferable to have an N content of 0.0020% or more, 0.0080% or more, or 0.0150% or more.
[0107] O: 0.0100% or less
[0108] O, when present in large quantities in steel, forms coarse oxides that serve as the starting point for fracture, causing brittle fracture or hydrogen-induced cracking. Therefore, the O content is to be 0.0100% or less. It is preferable to keep the O content 0.0080% or less, 0.0050% or less, or 0.0030% or less. Although the lower limit of the O content is 0%, the O content may be 0.0005% or more and 0.0010% or more in order to disperse a large number of fine oxides during the deoxidation of molten steel.
[0109] The hot-rolled steel sheet according to the present embodiment may contain the following elements as optional elements in addition to the above elements. The lower limit of the content when optional elements are not included is 0%. The optional elements will be described in detail below.
[0110] Ti: 0.001 to 0.300%
[0111] Nb: 0.001 to 0.100%
[0112] V: 0.001 to 0.500%
[0113] Since Ti, Nb, and V all precipitate as carbides or nitrides in steel and have the effect of refining the metal structure through the peening effect, one or more of these elements may be included. In order to obtain the effect resulting from the above action more reliably, it is desirable to have a Ti content of 0.001% or more, a Nb content of 0.001% or more, or a V content of 0.001% or more. That is, it is desirable to have a content of 0.001% or more of at least one of Ti, Nb, and V.
[0114] However, even if these elements are contained in excess, the effect of the above action becomes saturated and is not economically desirable. Therefore, the Ti content is set to 0.300% or less, the Nb content to 0.100% or less, and the V content to 0.500% or less.
[0115] Cu: 0.01 to 2.00%
[0116] Cr: 0.01 to 2.00%
[0117] Mo: 0.01 to 1.00%
[0118] Ni: 0.01 to 2.00%
[0119] B: 0.0001 to 0.0100%
[0120] Cu, Cr, Mo, Ni, and B all have the effect of increasing the quenchability of hot-rolled steel sheets. In addition, Cu and Mo precipitate as carbides in the steel at low temperatures and have the effect of increasing strength. Furthermore, when Cu is included, Ni has the effect of effectively suppressing grain boundary cracks in the slab caused by Cu. Therefore, one or more of these elements may be included.
[0121] As described above, Cu has the effect of increasing the quenchability of hot-rolled steel sheets and precipitating as carbides in the steel at low temperatures to increase the strength of the hot-rolled steel sheets. In order to obtain the effects of the above actions more reliably, it is preferable that the Cu content be 0.01% or more, and more preferable that it be 0.05% or more. However, if the Cu content exceeds 2.00%, grain boundary cracks may occur in the slab. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably 1.50% or less, more preferably 1.00% or less, 0.70% or less, or 0.50% or less.
[0122] As described above, Cr has the effect of increasing the quenchability of hot-rolled steel sheets and precipitating as carbides in the steel at low temperatures to increase strength. To obtain the effects of the above actions more reliably, it is desirable to have a Cr content of 0.01% or more, and more desirable to have a Cr content of 0.05% or more. However, if the Cr content exceeds 2.00%, the chemical treatment properties of the hot-rolled steel sheets are significantly reduced. Therefore, the Cr content is set to 2.00% or less. The Cr content is preferably 1.50% or less, more preferably 1.00% or less, 0.70% or less, or 0.50% or less.
[0123] As described above, Mo has the effect of increasing the quenchability of hot-rolled steel sheets and precipitating as carbides in the steel to increase the strength of the hot-rolled steel sheets. In order to obtain the effect of the above action more reliably, it is desirable to have a Mo content of 0.01% or more, and more desirable to have a Mo content of 0.02% or more. However, even if the Mo content exceeds 1.00%, the effect of the above action becomes saturated and is not economically desirable. Therefore, the Mo content is set to 1.00% or less. The Mo content is preferably 0.50% or less, more preferably 0.20% or less, or 0.10% or less.
[0124] As described above, Ni has the effect of increasing the quenchability of hot-rolled steel sheets. In addition, when Cu is included, Ni has the effect of effectively suppressing intergranular cracking of the slab caused by Cu. To obtain the effect resulting from the above action more reliably, it is desirable to have a Ni content of 0.01% or more. Since Ni is an expensive element, it is not economically desirable to include it in large amounts. Therefore, the Ni content is set to 2.00% or less. The Ni content is preferably 1.50% or less, more preferably 1.00% or less, 0.70% or less, or 0.50% or less.
[0125] As described above, B has the effect of increasing the quenchability of hot-rolled steel sheets. In order to obtain the effect of this action more reliably, it is preferable to have a B content of 0.0001% or more, and more preferable to have a B content of 0.0002% or more. However, since the hole expansion ability of the hot-rolled steel sheet is significantly reduced if the B content exceeds 0.0100%, the B content is set to 0.0100% or less. It is preferable to have a B content of 0.0050% or less or 0.0025% or less.
[0126] Ca: 0.0001 to 0.0200%
[0127] Mg: 0.0001 to 0.0200%
[0128] REM: 0.0001 to 0.1000%
[0129] Bi: 0.0001 to 0.0200%
[0130] As: 0.001 to 0.100%
[0131] Ca, Mg, and REM all have the effect of increasing the hole expandability of hot-rolled steel sheets by adjusting the shape of inclusions to a desirable shape. Additionally, Bi has the effect of increasing the formability of hot-rolled steel sheets by refining the solidification structure. Therefore, one or more of these elements may be included. To obtain the effects of the above actions more reliably, it is desirable to have a content of at least one of Ca, Mg, REM, and Bi of 0.0001% or more. However, if the Ca content or Mg content exceeds 0.0200%, or the REM content exceeds 0.1000%, excessive inclusions are generated in the steel, which may actually reduce the hole expandability of the hot-rolled steel sheets. Furthermore, even if the Bi content exceeds 0.0200%, the effects of the above actions become saturated, which is not economically desirable. Accordingly, the Ca and Mg content is set to 0.0200% or less, the REM content to 0.1000% or less, and the Bi content to 0.0200% or less. The Ca, Mg, and Bi content are preferably 0.0100% or less, and more preferably 0.0070% or less or 0.0040% or less. The REM content is preferably 0.0070% or less or 0.0040% or less. As contributes to the improvement of ductility in hot-rolled steel sheets by lowering the austenite single-phase temperature, thereby refining the old austenite grains. To reliably obtain this effect, it is desirable to set the As content to 0.001% or more. On the other hand, since the above effect becomes saturated even if a large amount of As is included, the As content is set to 0.100% or less.
[0132] Here, REM refers to a total of 17 elements consisting of Sc, Y, and lanthanides, and the content of REM refers to the total content of these elements. In the case of lanthanides, they are added industrially in the form of misch metals.
[0133] Zr: 0.01 to 1.00%, Co: 0.01 to 1.00%, Zn: 0.01 to 1.00%, W: 0.01 to 1.00%
[0134]
[0135] However, each element symbol in the above formula (A) represents the content based on the mass % of the element, and if the element is not contained, 0% is substituted.
[0136] Sn: 0 to 0.05%
[0137] With respect to Zr, Co, Zn, and W, the inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if these elements are contained in a total of 1.00% or less. Therefore, one or more of Zr, Co, Zn, and W may be contained in a total of 1.00% or less. That is, the value of the left side of the above formula (A) may be 1.00% or less, 0.50% or less, 0.10% or less, or 0.05% or less. The content of each of Zr, Co, Zn, W, and Sn may be 0.50% or less, 0.10% or less, or 0.05% or less, respectively. Since Zr, Co, Zn, and W do not need to be contained, their respective contents may be 0%. In order to strengthen the steel sheet by solid solution strengthening to improve strength, the content of Zr, Co, Zn, and W may each be 0.01% or more.
[0138] In addition, the inventors have confirmed that the effect of the hot-rolled steel sheet according to the present embodiment is not impaired even if a small amount of Sn is included. However, since scratches may occur during hot rolling if a large amount of Sn is included, the Sn content is set to 0.05% or less. Since Sn does not need to be included, the Sn content may be 0%. To increase the corrosion resistance of the hot-rolled steel sheet, the Sn content may be 0.01% or more.
[0139] The remainder of the chemical composition of the hot-rolled steel sheet according to the present embodiment may consist of Fe and impurities. In the present embodiment, impurities refer to those incorporated from raw materials such as ore, scrap, or the manufacturing environment, and are permitted within a range that does not adversely affect the hot-rolled steel sheet according to the present embodiment.
[0140] The chemical composition of the hot-rolled steel sheet described above can be measured by general analytical methods. For example, it can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). In addition, sol.Al can be measured by ICP-AES using the filtrate obtained after heating and decomposing the sample with acid. C and S can be measured using the combustion-infrared absorption method, N using the inert gas melting-thermal conductivity method, and O using the inert gas melting-non-dispersive infrared absorption method.
[0141] If the hot-rolled steel sheet has a plating layer on its surface, the plating layer may be removed by mechanical grinding or the like, if necessary, and then the chemical composition may be analyzed.
[0142] Metal structure of hot-rolled steel sheets
[0143] Next, the metal structure of the hot-rolled steel sheet according to the present embodiment will be described.
[0144] The hot-rolled steel sheet according to the present embodiment has a metal structure in which, in area %, the total of martensite and tempered martensite is greater than 92.0% and less than or equal to 100.0%, the retained austenite is less than 3.0%, and the ferrite is less than 5.0%, wherein the entropy value represented by the following equation (1), obtained by analyzing the SEM image of the metal structure by the gray level co-generation matrix method, is 11.0 or greater, the inverse difference normalized value represented by the following equation (2) is less than 1.020, and the cluster shade value represented by the following equation (3) is -8.0×10 5 Up to 8.0×10 5 And, the standard deviation of Mn concentration is 0.60 mass% or less.
[0145] Accordingly, the hot-rolled steel sheet according to the present embodiment can obtain excellent hole expandability and shear workability while having high strength and a reduction rate in plate thickness at the limit fracture. In addition, in the present embodiment, the metal structure is defined at a position 1 / 4 of the plate thickness from the surface (an area from 1 / 8 of the plate thickness from the surface to 3 / 8 of the plate thickness from the surface) and at the center of the plate width direction in a cross-section parallel to the rolling direction. The reason is that the metal structure at this position represents the typical metal structure of the steel sheet.
[0146] In addition, the term "surface" as used herein refers to the interface between the plating layer and the steel sheet in cases where the hot-rolled steel sheet is provided with a plating layer.
[0147] Area percentage of retained austenite: less than 3.0%
[0148] Retained austenite is a metallic structure that exists as a face-centered cubic lattice even at room temperature. Retained austenite acts to increase the hole expansion of hot-rolled steel sheets through transformation-induced plasticity (TRIP). On the other hand, since retained austenite transforms into high-carbon martensite during shearing, it hinders stable crack formation and causes a decrease in the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing. If the area percentage of retained austenite is 3.0% or more, the above effects become apparent, and the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing is reduced. Therefore, the area percentage of retained austenite is kept below 3.0%. The area percentage of retained austenite is preferably 1.5% or less, and more preferably less than 1.0%. Since it is desirable to have less retained austenite, the area percentage of retained austenite may be 0%. However, it is not easy to make the area percentage of retained austenite 0%, and the lower limit may be 0.5% or 1.0%.
[0149] Ferrite area percentage: Less than 5.0%
[0150] Ferrite is a generally soft metallic structure. If a material contains more than a predetermined amount of ferrite, it may not be possible to obtain the desired strength, or the area of the shear plane at the end surface after shearing may increase. An increase in the area of the shear plane at the end surface after shearing is undesirable because it reduces the linearity of the boundary between the fracture surface and the shear plane at the end surface after shearing. If the area percentage of ferrite is 5.0% or more, the above effect becomes apparent. Therefore, the area percentage of ferrite is kept below 5.0%. The area percentage of ferrite is preferably 3.0% or less, more preferably 2.0% or less, and even more preferably less than 1.0%. Since it is desirable to have less ferrite, the area percentage of ferrite may be 0%. However, since it is not easy to make the area percentage of ferrite 0%, the lower limit may be set to 0.5%, 1.0%, or 1.5%.
[0151] Methods for measuring the area percentage of retained austenite include X-ray diffraction, EBSP (Electron Back Scattering Diffraction Pattern) analysis, and magnetic measurement. In this embodiment, the area percentage of retained austenite is measured by X-ray diffraction, which is less susceptible to the effects of polishing (since the retained austenite may change into other phases such as martensite if it is affected by polishing, the true area percentage may not be measured), and accurate measurement results are obtained relatively easily.
[0152] In the measurement of the area percentage of retained austenite by X-ray diffraction in the present embodiment, first, the integrated intensity of a total of six peaks of α (110), α (200), α (211), γ (111), γ (200), and γ (220) is obtained using Co-Kα rays in a cross-section of the plate thickness parallel to the rolling direction at a depth of 1 / 4 of the plate thickness of the hot-rolled steel plate (an area from the surface to a depth of 1 / 8 of the plate thickness and from the surface to a depth of 3 / 8 of the plate thickness) and at a central position in the plate width direction, and the volume percentage of retained austenite is calculated using the intensity average method. The obtained volume percentage of retained austenite is considered as the area percentage of retained austenite.
[0153] The area ratio of ferrite is measured by the following method.
[0154] The cross-section of the plate thickness parallel to the rolling direction is finished to a mirror surface, polished for 8 minutes using colloidal silica that does not contain alkaline solutions at room temperature, and the deformation introduced into the surface layer of the sample is removed. At any position along the longitudinal direction of the sample cross-section, crystal orientation information is obtained by measuring an area with a length of 50 μm and a depth of 1 / 8 to 3 / 8 of the plate thickness from the surface using electron backscatter diffraction at a measurement interval of 0.1 μm. For the measurement, an EBSD analysis device consisting of a thermal field emission scanning electron microscope (JEOL JSM-7001F) and an EBSD detector (TSL DVC5 type detector) is used. At this time, the vacuum level inside the EBSD analysis device is 9.6 × 10⁻⁶ -5 The pressure is set to Pa or less, the acceleration voltage to 15 kV, the irradiation current level to 13, and the electron beam irradiation level to 62. The observation area is 40,000 µm. 2 ...does as.
[0155] Next, a reflected electron image is taken in the same field of view. From the reflected electron image, the crystal grains in which ferrite and cementite are precipitated in layers are identified, and by calculating the area ratio of said crystal grains, the area ratio of pearlite can be obtained.
[0156] After that, among the grains excluding those identified as pearlite, the grains identified as having a body-centered cubic structure are identified using the obtained crystal orientation information and the “Grain Average Misorientation” function installed in the software “OIM Analysis (registered trademark)” attached to the EBSD analysis device, and the region where the Grain Average Misorientation value is 1.0° or less is identified as ferrite. At this time, the Grain Tolerance Angle is set to 15°, and the area ratio of the region identified as ferrite is obtained by calculating the area ratio of the ferrite.
[0157] Next, among the regions excluding the regions identified as pearlite or ferrite, the regions exceeding Iα / 2 when the maximum value of the "Grain Average IQ" of the ferrite region is set to Iα are extracted (determined) as bainite. By calculating the area ratio of the regions extracted (determined) as bainite, the area ratio of bainite is obtained.
[0158] Sum of area percentages of martensite and tempered martensite: greater than 92.0% and less than or equal to 100.0%
[0159] If the total area ratio of martensite and tempered martensite is 92.0% or less, the desired strength cannot be obtained. Therefore, the total area ratio of martensite and tempered martensite is to be greater than 92.0%. Preferably, it is 93.0% or more, 95.0% or more, 97.0% or more, or 99.0% or more. Since a higher total area ratio of martensite and tempered martensite is desirable, it may be 100.0%.
[0160] The method for measuring the area ratio of martensite and tempered martensite is described below.
[0161] First, to observe the same area as the EBSD measurement area where the ferrite area ratio was measured using SEM, a Vickers indentation is made near the observation location. Then, the structure of the observation surface is left intact, surface contaminants are polished away, and Nital etching is performed. Next, the same field of view as the EBSD observation surface is observed using SEM at a magnification of 3000x.
[0162] In EBSD measurement, among the regions identified as having a structure other than ferrite, the region having a substructure within the grain and cementite precipitated in multiple variants is determined to be tempered martensite. The region with high brightness and where the substructure is not revealed by etching is determined to be "martensite and retained austenite." By calculating the respective area percentages, the area percentage of tempered martensite and the area percentage of "martensite and retained austenite" are obtained. By subtracting the area percentage of retained austenite obtained by the above-described X-ray diffraction from the area percentage of "martensite and retained austenite," the area percentage of martensite is obtained. By calculating the sum of the area percentages of martensite and tempered martensite, the sum of the area percentages of martensite and tempered martensite is obtained.
[0163] In addition, for removing contaminants from the surface layer of the observation surface, methods such as buff polishing using alumina particles with a particle size of 0.1 μm or less, or Ar ion sputtering, can be used.
[0164] The hot-rolled steel sheet according to the present embodiment may contain one or two types of bainite and pearlite as the remainder structure, with a total area percentage of 0% or more and less than 8.0%. The upper limit of the area percentage of the remainder structure may be 6.0%, 5.0%, 4.0%, 3.0%, or 2.5%.
[0165] In this embodiment, since the area ratio of each tissue is measured by X-ray diffraction, EBSD analysis, and SEM observation, there may be cases where the sum of the area ratios of each tissue obtained by measurement does not equal 100.0%. If the sum of the area ratios of each tissue obtained by the above-described method does not equal 100.0%, the area ratio of each tissue is converted so that the sum of the area ratios of each tissue equals 100.0%. For example, if the sum of the area ratios of each tissue is 103.0%, the area ratio of each tissue is obtained by multiplying the area ratio of each tissue by "100.0 / 103.0".
[0166] Entropy value: 11.0 or higher, Inverse difference normalized value: less than 1.020
[0167] In order to improve the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing, it is important to reduce the periodicity of the metal structure and also reduce the uniformity of the metal structure. In the present embodiment, the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing is improved by controlling the Entropy value (E value), which represents the periodicity of the metal structure, and the Inverse difference normalized value (I value), which represents the uniformity of the metal structure.
[0168] The E value represents the periodicity of the metal structure. When the luminance is arranged periodically due to influences such as the formation of band-shaped structures, i.e., when the periodicity of the metal structure is high, the E value decreases. In this embodiment, since it is necessary to have a metal structure with low periodicity, it is necessary to increase the E value. If the E value is less than 11.0, the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing tends to deteriorate. In a metal structure with high periodicity, i.e., a low E value, cracks occur along multiple band-shaped structures existing near the starting point, starting from the periodically arranged structure, and a fracture surface is formed. As a result, it is estimated that the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing tends to deteriorate. Therefore, the E value is set to 11.0 or higher. Preferably, it is 11.1 or higher, and more preferably, it is 11.2 or higher. The higher the E value, the more desirable it is, and although the upper limit is not specifically specified, it may be 13.5 or less, 13.0 or less, 12.5 or less, or 12.0 or less.
[0169] The I value indicates the uniformity of the metal structure and increases as the area of the region having a constant brightness increases. A high I value signifies high uniformity of the metal structure. In the hot-rolled steel sheet having a metal structure in which the sum of the area ratios of martensite and tempered martensite in the present embodiment is 92.0% or less, it is necessary to have a metal structure mainly composed of martensite, which has low uniformity of brightness. For this reason, in the present embodiment, it is necessary to reduce the I value. If the uniformity of the metal structure is high, that is, if the I value is high, cracks are prone to occur from the tip of the shearing tool due to the influence of differences in precipitates and elemental concentration within the crystal grains, and differences in hardness caused by the soft ferrite phase. As a result, the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing is prone to deterioration. In other words, if the I value is 1.020 or higher, it is estimated that the linearity of the boundary between the fracture surface and the shear surface at the end surface after shearing cannot be improved. Accordingly, the I value is less than 1.020. Preferably, it is 1.015 or less, and more preferably 1.010 or less. Although the lower limit of the I value is not specifically specified, it may be 0.900 or more, 0.950 or more, or 1.000 or more.
[0170] Cluster Shade Value: -8.0×10 5 Up to 8.0×10 5
[0171] The Cluster Shade (CS) value represents the degree of deformation of the metal structure. The CS value is positive if there are many points with luminance exceeding the average value of the image obtained by photographing the metal structure, and negative if there are many points with luminance below the average value.
[0172] In the secondary electron image of a scanning electron microscope, the brightness increases in areas where the surface roughness of the object being observed is large, and decreases in areas where the roughness is small. The surface roughness of the object being observed is greatly influenced by the grain size or intensity distribution within the metal structure. In this embodiment, the CS value increases when the variation in the intensity of the metal structure is large or the structure unit is small, and decreases when the variation in intensity is small or the structure unit is large.
[0173] In this embodiment, it is important to maintain the CS value within a desired range close to 0. The CS value is -8.0 × 10 5 If it is less than this, the reduction rate of plate thickness at the limit fracture of hot-rolled steel sheets decreases. This is presumed to be because large-sized crystal grains exist in the metal structure, and these grains fracture preferentially during extreme deformation. Therefore, the CS value is -8.0×10⁻⁶. 5 It should be above. Preferably -7.5×10 5 That is all, and more preferably -7.0×10 5 That is all.
[0174] Meanwhile, the CS value is 8.0×10 5 If it exceeds this value, the reduction rate of plate thickness at the limit fracture of hot-rolled steel sheets decreases. This is presumed to be because the fluctuation in microscopic strength within the metal structure is large, and deformation during ultimate deformation becomes localized, making fracture more likely. Therefore, the CS value is 8.0 × 10⁻⁶ 5 It shall be less than or equal to 7.5 × 10⁻⁶. Preferably, 7.5 5 Less than, and more preferably 7.0×10 5 It is as follows.
[0175] The E, I, and CS values can be obtained by the following method.
[0176] In this embodiment, the imaging area of the SEM image (secondary electron image of a scanning electron microscope) taken to calculate the E value, I value, and CS value is set to a position at a depth of 1 / 4 of the plate thickness from the surface (an area from a depth of 1 / 8 of the plate thickness from the surface to a depth of 3 / 8 of the plate thickness from the surface) and also to a central position in the plate width direction. For capturing the SEM image, a SU-6600 Schottky electron gun manufactured by Hitachi High Technologies Co., Ltd. is used, the emitter is made of tungsten, and the acceleration voltage is set to 1.5 kV. Under the above settings, an SEM image is output in a 256-gradation grayscale at a magnification of 1000x.
[0177] Next, the obtained SEM image is cropped into an area of 880×880 pixels (the observation area is 160㎛×160㎛ in actual dimensions), and a smoothing process is performed on the image with a tile grid size of 8×8 and a contrast enhancement limiting magnification of 2.0 as described in Non-Patent Literature 3. The SEM image after the smoothing process is rotated counterclockwise for every degree from 0 to 179 degrees, excluding 90 degrees, and an image is created for each degree, thereby obtaining a total of 179 images. Next, for each of these 179 images, the frequency values of luminance between adjacent pixels are collected in the form of a matrix using the GLCM method described in Non-Patent Literature 1.
[0178] The matrix of 179 frequency values collected by the above method, with k as the rotation angle from the original image, p k It is expressed as (k=0 … 89, 91, … 179). For each image, the generated p k After summing for all k (k=0 … 89, 91 … 179), a 256×256 matrix P is produced that is normalized so that the sum of each component is 1. In addition, the values of E, I, and CS are each calculated using the following equations (1) to (5) described in Non-Patent Literature 2.
[0179] In the following equations (1) to (5), P(i, j) is a gray level co-generation matrix, and the value in the i-th row and j-th column of matrix P is denoted as P(i, j). Additionally, as previously mentioned, since it is calculated using a 256×256 matrix P, if you wish to emphasize this point, the following equations (1) to (5) can be modified to the following equations (1') to (5').
[0180] Here, L in the following equation (2) is the number of quantization levels of grayscale that the SEM image can take, and since the SEM image is output with 256 grayscale levels as described above in this embodiment, L is 256. i and j in the following equations (2) and (3) are natural numbers from 1 to L, and μ in the following equation (3) x and μ y These are represented by the following equations (4) and (5), respectively.
[0181] In the following equations (1') to (5'), the value at the i-th row and j-th column of matrix P is P ij It is written as .
[0182]
[0183]
[0184]
[0185]
[0186]
[0187]
[0188]
[0189]
[0190]
[0191]
[0192] Standard deviation of Mn concentration: 0.60 mass% or less
[0193] The standard deviation of Mn concentration at a position 1 / 4 of the plate thickness from the surface of the hot-rolled steel sheet according to the present embodiment (an area from 1 / 8 of the plate thickness from the surface to 3 / 8 of the plate thickness from the surface) and at a position in the center of the plate width direction is 0.60 mass% or less. By doing so, the hard phase can be uniformly dispersed, and the deterioration of the linearity of the boundary between the fracture surface and the shear surface at the end surface after shear processing can be prevented. The standard deviation of Mn concentration is preferably 0.55 mass% or less or 0.50 mass% or less, and more preferably 0.47 mass% or less. From the perspective of suppressing excessive burrs, the lower limit of the standard deviation of Mn concentration is preferably as small as possible, but due to constraints of the manufacturing process, the practical lower limit is 0.10 mass%. If necessary, the lower limit may be 0.20 mass% or 0.28 mass%.
[0194] After mirror-polishing the cross-section of the plate thickness parallel to the rolling direction of the hot-rolled steel sheet, the standard deviation of Mn concentration is measured using an electron probe micro analyzer (EPMA) at a depth of 1 / 4 of the plate thickness from the surface (an area from 1 / 8 of the plate thickness to 3 / 8 of the plate thickness from the surface) and at the center of the plate width direction. The measurement conditions are set with an acceleration voltage of 15 kV and a magnification of 5000x to measure the distribution pattern in a range of 20 µm in the rolling direction of the sample and 20 µm in the thickness direction of the sample plate. More specifically, the measurement interval is set to 0.1 µm, and Mn concentrations are measured at more than 40,000 locations. Subsequently, the standard deviation of Mn concentration is obtained by calculating the standard deviation based on the Mn concentrations obtained from all measurement points.
[0195] Average crystal grain size of the surface layer: Less than 3.0㎛
[0196] By making the crystal grain size of the surface layer finer, cracks within the bend of hot-rolled steel sheets can be suppressed. As the strength of the hot-rolled steel sheet increases, cracks are more likely to occur from the inner side of the bend during bending processing (hereinafter referred to as cracks within the bend). The mechanism of cracks within the bend is estimated as follows. During bending processing, compressive stress is generated on the inner side of the bend. Initially, processing proceeds with the entire inner side of the bend deforming uniformly, but as the amount of processing increases, uniform deformation alone cannot handle the deformation, and deformation proceeds as deformation becomes concentrated in a local area (occurrence of a shear deformation zone). As this shear deformation zone grows further, cracks along the shear zone occur and grow from the inner surface of the bend. It is presumed that the reason cracks within bending become more likely to occur with increasing strength is that the decrease in work hardening ability accompanying the increase in strength makes it difficult for uniform deformation to proceed, thereby making deformation uneven and causing a shear deformation zone to occur early in the processing (or under gentle processing conditions).
[0197] Through the research of the inventors, it was found that cracking during bending becomes pronounced in steel sheets with a tensile strength of 980 MPa or higher. Furthermore, the inventors discovered that the finer the crystal grain size of the surface layer of a hot-rolled steel sheet, the more localized deformation concentration is suppressed, making it difficult for cracking during bending to occur. To achieve the above effect, it is preferable that the average crystal grain size of the surface layer of the hot-rolled steel sheet be less than 3.0 μm. More preferably, it is 2.7 μm or less or 2.5 μm or less. Although the lower limit of the average crystal grain size of the surface layer region is not specifically defined, it may be 0.5 μm or 1.0 μm.
[0198] In addition, in this embodiment, the surface layer is a region from the surface of the hot-rolled steel sheet to a depth of 50 μm from the surface. As described above, the surface referred to herein refers to the interface between the plating layer and the steel sheet in cases where the hot-rolled steel sheet is provided with a plating layer.
[0199] The crystal grain size of the surface layer is measured using the EBSP-OIM (Electron Back Scatter Diffraction Pattern-Orientation Image Microscopy) method. The EBSP-OIM method is performed using a device combining a scanning electron microscope and an EBSP analysis unit, and OIM Analysis (registered trademark) manufactured by AMETEK. The analyzable area of the EBSP-OIM method is the area observable by the SEM. Although it varies depending on the resolution of the SEM, the EBSP-OIM method allows for analysis with a resolution of at least 20 nm.
[0200] Analysis is performed in at least 5 fields of view in an area of 40㎛ × 30㎛ at a magnification of 1200x in a cross-section parallel to the rolling direction of the hot-rolled steel sheet, from the surface of the hot-rolled steel sheet to a depth of 50㎛ from the surface and also at the center of the sheet width direction. A location where the angle difference between adjacent measurement points is 5° or more is defined as a grain boundary, and the area average grain size is calculated. The obtained area average grain size is taken as the average grain size of the surface layer.
[0201] In addition, since the retained austenite is not a structure formed by a phase transformation at 600°C or lower and does not have the effect of dislocation accumulation, the retained austenite is not subject to analysis in this measurement method (method for measuring the average crystal grain size of the surface layer). In cases where the area ratio of the retained austenite is 0%, it is not necessary to exclude it from the subject of analysis, but in cases where it may affect the measurement of the average crystal grain size of the surface layer, the retained austenite with an fcc crystal structure is excluded from the subject of analysis in the EBSP-OIM method.
[0202] Tensile properties
[0203] The hot-rolled steel sheet according to the present embodiment has a tensile strength (TS) of 980 MPa or more. If the tensile strength is less than 980 MPa, the applicable parts are limited, and the contribution to vehicle body weight reduction is small. Although there is no need to specifically limit the upper limit, it may be 1780 MPa from the perspective of suppressing mold wear.
[0204] Tensile strength is measured in accordance with JIS Z 2241:2011 using a No. 5 test specimen of JIS Z 2241:2011. The sampling location for the tensile test specimen should be set to the 1 / 4 portion from the end in the plate width direction, and the direction perpendicular to the rolling direction should be the length direction.
[0205] Hole expansion characteristics
[0206] The hot-rolled steel sheet according to the present embodiment preferably has a hole expansion rate (λ) of 55% or more. If the hole expansion rate (λ) is 55% or more, the applicable parts are not limited, and a hot-rolled steel sheet that contributes significantly to vehicle body weight reduction can be obtained. There is no need to specifically limit the upper limit. Although there is no need to set an upper limit for the hole expansion rate λ, it may be 85% or 80%.
[0207] The hole expansion rate (λ) is measured in accordance with JIS Z 2256:2010 using a No. 5 test specimen of JIS Z 2241:2011. The sampling location for the hole expansion test specimen should be set to 1 / 4 of the length from the end in the width direction of the hot-rolled steel sheet.
[0208] Plate thickness
[0209] The thickness of the hot-rolled steel sheet according to the present embodiment is not particularly limited, but may be 0.5 to 8.0 mm. By making the thickness of the hot-rolled steel sheet 0.5 mm or more, it becomes easier to secure the rolling completion temperature and reduce the rolling load, and hot rolling can be performed easily. Therefore, the thickness of the hot-rolled steel sheet according to the present embodiment may be 0.5 mm or more. Preferably, it is 1.2 mm or more, 1.4 mm or more, or 1.8 mm or more. In addition, by making the thickness 8.0 mm or less, it becomes easier to refine the metal structure and easily secure the metal structure described above. Therefore, the thickness may be 8.0 mm or less. Preferably, it is 6.0 mm or less, 5.0 mm or less, or 4.0 mm or less.
[0210] plating layer
[0211] The hot-rolled steel sheet according to the present embodiment having the chemical composition and metal structure described above may be provided with a plating layer on its surface for the purpose of improving corrosion resistance, etc., and thus become a surface-treated steel sheet. The plating layer may be an electroplated layer or a hot-dip plating layer. Examples of the electroplated layer include electro-galvanizing and electro-Zn-Ni alloy plating. Examples of the hot-dip plating layer include hot-dip galvanizing, alloyed hot-dip galvanizing, hot-dip aluminum plating, hot-dip Zn-Al alloy plating, hot-dip Zn-Al-Mg alloy plating, and hot-dip Zn-Al-Mg-Si alloy plating. The amount of plating applied is not particularly limited and may be performed in the same manner as in the past. Furthermore, it is possible to further increase corrosion resistance by performing a suitable chemical treatment (e.g., application and drying of a silicate-based chromium-free chemical treatment solution) after plating.
[0212] Manufacturing conditions
[0213] A suitable method for manufacturing a hot-rolled steel sheet according to the present embodiment having the chemical composition and metal structure described above is as follows.
[0214] In a suitable manufacturing method for a hot-rolled steel sheet according to the present embodiment, the following processes (1) to (9) are performed sequentially. In addition, the temperature of the slab and the temperature of the steel sheet in the present embodiment refer to the surface temperature of the slab and the surface temperature of the steel sheet. In addition, stress refers to the tension applied in the rolling direction of the steel sheet.
[0215] (1) After maintaining the slab in a temperature range of 700 to 850°C for 900 seconds or more, it is heated and maintained in a temperature range of 1100°C or higher for 6000 seconds or more.
[0216] (2) Hot rolling is performed in a temperature range of 850 to 1100°C, resulting in a total plate thickness reduction of 90% or more.
[0217] (3) After rolling one stage before the final stage of hot rolling, and also before rolling the final stage, a stress of 170 kPa or more is applied to the steel plate.
[0218] (4) The reduction rate at the final stage of hot rolling is 8% or more, and the hot rolling is completed such that the rolling completion temperature Tf is 900°C or higher and less than 960°C.
[0219] (5) After the final stage of hot rolling, and until the steel plate is cooled to 800°C, the stress applied to the steel plate is less than 200 kPa.
[0220] (6) Within 1 second after the completion of hot rolling, the temperature is cooled to a temperature range of Tf-50°C or lower, and then accelerated cooling is performed so that the average cooling rate to 600°C is 50°C / s or higher. However, cooling to a temperature range of Tf-50°C or lower within 1 second after the completion of hot rolling is a more desirable cooling condition.
[0221] (7) Cooling is performed such that the average cooling rate in the temperature range of 450 to 600°C is 30°C / s or more and less than 50°C / s.
[0222] (8) Cool the temperature range from the coil temperature to 450℃ so that the average cooling rate is 50℃ / s or more.
[0223] (9) It is wound in a temperature range of 350℃ or lower.
[0224] By employing the above manufacturing method, it is possible to stably produce hot-rolled steel sheets having high strength and a reduction rate in plate thickness at the limit of fracture, as well as excellent hole expandability and shear workability. That is, by appropriately controlling the slab heating conditions and hot rolling conditions, the reduction of Mn segregation and the equiaxing of austenite before transformation are promoted, and in combination with the cooling conditions after hot rolling described later, it is possible to stably produce hot-rolled steel sheets having a desired metal structure.
[0225] (1) Slab, slab temperature and holding time when providing to hot rolling
[0226] The slabs provided for hot rolling may be slabs obtained by continuous casting or slabs obtained by casting and ingots. Additionally, if necessary, slabs that have undergone additional hot or cold working may be used.
[0227] It is preferable that the slab provided for hot rolling be maintained at a temperature range of 700°C to 850°C for at least 900 seconds when heated, and then further heated to a temperature range of 1100°C or higher for at least 6000 seconds. In addition, when maintaining at a temperature range of 700°C to 850°C, the steel plate temperature may be varied within this temperature range or kept constant. In addition, when maintaining at a temperature range of 1100°C or higher, the steel plate temperature may be varied within the temperature range of 1100°C or higher or kept constant.
[0228] In the austenite transformation at 700°C to 850°C, Mn is distributed between the ferrite and austenite, and by extending the transformation time, Mn can diffuse within the ferrite region. This eliminates Mn micro-segregation localized in the slab and significantly reduces the standard deviation of Mn concentration. By reducing the standard deviation of Mn concentration, the linearity of the fracture surface and the shear surface at the end surface after shear processing can be improved. In addition, the I value can be set to a desired value.
[0229] In addition, to reduce the standard deviation of Mn concentration and to obtain a desired I value, it is desirable to maintain the holding time in the temperature range of 1100°C or higher for 6000 seconds or more. To obtain a desired amount of martensite and tempered martensite, it is desirable to maintain the temperature for 6000 seconds or more at 1100°C or higher.
[0230] Hot rolling is preferably performed using a reverse mill or a tandem mill as a multi-pass rolling process. Particularly from the perspective of industrial productivity, it is more preferable to perform hot rolling using a tandem mill at least as the final step.
[0231] (2) Hot rolling reduction rate: A total plate thickness reduction of 90% or more in the temperature range of 850 to 1100°C
[0232] By performing hot rolling in a temperature range of 850 to 1100°C that results in a total plate thickness reduction of 90% or more, the refinement of recrystallized austenite grains is primarily promoted, and the accumulation of deformation energy into unrecrystallized austenite grains is promoted. Additionally, as the recrystallization of austenite is promoted, the atomic diffusion of Mn is promoted, thereby reducing the standard deviation of the Mn concentration. Furthermore, the I value can be set to a desired value. Therefore, it is desirable to perform hot rolling in a temperature range of 850 to 1100°C that results in a total plate thickness reduction of 90% or more.
[0233] In addition, the reduction in plate thickness in the temperature range of 850 to 1100°C can be expressed as (t0-t1) / t0×100(%), where t0 is the inlet plate thickness before the first pass in rolling in this temperature range and t1 is the outlet plate thickness after the final pass in rolling in this temperature range.
[0234] (3) Stress after rolling one step prior to the final stage of hot rolling, and also before rolling at the final stage: 170 kPa or more
[0235] It is desirable to set the stress applied to the steel plate after rolling one step prior to the final stage of hot rolling, and also prior to rolling at the final stage, to 170 kPa or more. Accordingly, among the recrystallized austenite after rolling one step prior to the final stage, {110} <001> The number of crystal grains having the crystal orientation of can be reduced. {110} <001> Since this is a crystal orientation that is difficult to recrystallize, suppressing the formation of this crystal orientation can effectively promote recrystallization by the final stage of reduction. As a result, the band-shaped structure of the hot-rolled steel sheet is improved, the periodicity of the metal structure is reduced, and the E value increases. If the stress applied to the steel sheet is less than 170 kPa, the E value may not be set to the desired value. More preferably, the stress applied to the steel sheet is 190 kPa or more. The stress applied to the steel sheet can be controlled by adjusting the roll rotation speed during tandem rolling, and can be calculated by dividing the load in the rolling direction measured at the rolling stand by the cross-sectional area of the sheet being passed through.
[0236] (4) Reduction rate at the final stage of hot rolling: 8% or more, hot rolling completion temperature Tf: 900℃ or more, less than 960℃
[0237] It is desirable to set the reduction rate at the final stage of hot rolling to 8% or more and the hot rolling completion temperature Tf to 900°C or more. By setting the reduction rate at the final stage of hot rolling to 8% or more, recrystallization caused by the reduction at the final stage can be promoted. As a result, the band-shaped structure of the hot-rolled steel sheet is improved, the periodicity of the metal structure is reduced, and the E value increases. By setting the hot rolling completion temperature Tf to 900°C or more, the excessive increase in the number of ferrite nucleation sites in the austenite can be suppressed. Consequently, the formation of ferrite in the final structure (the metal structure of the hot-rolled steel sheet after manufacturing) can be suppressed, thereby obtaining a high-strength hot-rolled steel sheet. Furthermore, by setting the hot rolling completion temperature Tf to less than 960°C, the coarsening of the austenite grain size can be suppressed, thereby reducing the periodicity of the metal structure and allowing the E value to be set to a desired value.
[0238] (5) Stress after rolling the final stage of hot rolling and until the steel sheet cools to 800°C: less than 200 kPa
[0239] It is desirable that the stress applied to the steel plate after the final stage of hot rolling and until the steel plate is cooled to 800°C be less than 200 kPa. By keeping the stress (tension) applied in the rolling direction of the steel plate less than 200 kPa, the recrystallization of austenite proceeds preferentially in the rolling direction, and the increase in periodicity of the metal structure can be suppressed. As a result, the E value can be set to a desired value. More preferably, the stress applied to the steel plate is 180 MPa or less. In addition, the stress applied in the rolling direction of the steel plate can be controlled by adjusting the rotational speeds of the rolling stand and the winding device, and can be obtained by dividing the measured load in the rolling direction by the cross-sectional area of the plate being passed through.
[0240] (6) Accelerated cooling from the completion of hot rolling to 600℃ at an average cooling rate of 50℃ / s or more
[0241] By accelerating cooling from the completion of hot rolling to 600°C at an average cooling rate of 50°C / s or more, ferrite transformation, bainite transformation, and / or pearlite transformation within the steel sheet can be suppressed, thereby obtaining the desired strength. Additionally, the I value can be set to a desired value. If air cooling or the like is performed during the accelerated cooling to 600°C after the completion of hot rolling, the amount of ferrite may increase and the I value may not be set to a desired value, which is undesirable.
[0242] Although there is no specific upper limit for the average cooling rate, increasing the cooling rate results in larger cooling equipment and higher equipment costs. Therefore, considering equipment costs, it is desirable for the average cooling rate of accelerated cooling to be 300℃ / s or less.
[0243] In addition, the average cooling rate referred to here means the value obtained by dividing the range of temperature drop of the steel plate from the start of accelerated cooling (when the steel plate is introduced into the cooling facility) to 600°C by the time required for the steel plate temperature to reach 600°C from the start of accelerated cooling.
[0244] In cooling after the completion of hot rolling, it is more desirable to cool to a temperature range of the hot rolling completion temperature Tf-50°C within 1 second after the completion of hot rolling. That is, it is more desirable to cool to 50°C or higher within 1 second after the completion of hot rolling. This is because it can suppress the growth of austenite grains that have been refined by hot rolling. To cool to a temperature range of the hot rolling completion temperature Tf-50°C or lower within 1.0 second after the completion of hot rolling, cooling with a high average cooling rate can be performed immediately after the completion of hot rolling, for example, by spraying cooling water onto the surface of the steel sheet. By cooling to a temperature range of Tf-50°C or lower within 1 second after the completion of hot rolling, the crystal grain size of the surface layer can be refined, thereby increasing the crack resistance during bending of the hot-rolled steel sheet.
[0245] Within 1 second after the completion of hot rolling, after cooling to the temperature range of the hot rolling completion temperature Tf-50℃, accelerated cooling can be performed so that the average cooling rate up to 600℃ is 50℃ / s or more, as described above.
[0246] (7) Cooling such that the average cooling rate in the temperature range of 450 to 600℃ is 30℃ / s or more and less than 50℃ / s.
[0247] After the above accelerated cooling is completed, it is preferable to cool such that the average cooling rate in the temperature range of 450 to 600°C is 30°C / s or more and less than 50°C / s. By setting the average cooling rate in the above temperature range to 30°C / s or more and less than 50°C / s, the CS value can be set to a desired value. If the average cooling rate exceeds 50°C / s, coarse grains are prone to forming in the metal structure, and the CS value becomes -8.0×10⁻⁶ 5 It becomes less than. When the average cooling rate is less than 30℃ / s, the strength of the hard tissue increases and the strength difference with the soft tissue widens, so the CS value is 8.0×10 5 It exceeds.
[0248] In addition, the average cooling rate referred to here means the value obtained by dividing the range of temperature drop of the steel plate from the cooling stop temperature of accelerated cooling with an average cooling rate of 50℃ / s or more to the cooling stop temperature of cooling with an average cooling rate of 30℃ / s or more and less than 50℃ / s by the time required from the time of cessation of accelerated cooling with an average cooling rate of 50℃ / s or more to the time of cessation of cooling with an average cooling rate of 30℃ / s or more and less than 50℃ / s.
[0249] (8) Average cooling rate in the temperature range from the coiling temperature to 450℃: 50℃ / s or higher
[0250] In order to suppress the area ratio of pearlite and obtain the desired strength, it is desirable to set the average cooling rate in the temperature range from the coiling temperature to 450°C to 50°C / s or higher. By doing so, the matrix structure can be made hard.
[0251] In addition, the average cooling rate referred to here means the value obtained by dividing the range of temperature drop of the steel sheet from the cooling stop temperature to the coiling temperature at an average cooling rate of 30℃ / s or more and less than 50℃ / s by the time required from the cooling stop to the coiling at an average cooling rate of 30℃ / s or more and less than 50℃ / s.
[0252] (9) Winding temperature: 350℃ or lower
[0253] It is desirable to set the coiling temperature to 350°C or lower. By setting the coiling temperature to 350°C or lower, the driving force for the transformation from austenite to bcc can be increased, and the deformation strength of the austenite can also be increased. Consequently, when the hard phase transforms from austenite to martensite, the hard phase is uniformly distributed, thereby improving the variation. As a result, the I value can be reduced, and the linearity of the boundary between the fracture plane and the shear plane at the end surface after shear processing can be improved. Therefore, it is desirable to set the coiling temperature to 350°C or lower.
[0254] Examples
[0255] Next, the effects of one embodiment of the present invention will be explained in more detail by way of examples. However, the conditions in the examples are examples of conditions adopted to verify the feasibility and effects of the present invention, and the present invention is not limited to these examples of conditions. The present invention may adopt various conditions as long as the objectives of the present invention are achieved without departing from the gist of the present invention.
[0256] Steel having the chemical compositions shown in Tables 1 and 2 was melted, and slabs with a thickness of 240 to 300 mm were manufactured by continuous casting. Using the obtained slabs, hot-rolled steel sheets shown in Tables 5 and 6 were obtained under the manufacturing conditions shown in Tables 3 and 4.
[0257] In addition, Manufacturing No. 11 was cooled to 791°C after the completion of hot rolling, and then air-cooled for 5.0 seconds. The average cooling rate during air cooling was less than 5.0°C / s.
[0258] For the obtained hot-rolled steel sheet, the area ratio of the metal structure, E value, I value, CS value, standard deviation of Mn concentration, average crystal grain size of the surface layer, tensile strength (TS), and hole expansion factor (λ) were obtained by the method described above. The obtained measurement results are shown in Tables 5 and 6.
[0259] In addition, the residual tissue was one or two types of bainite and pearlite.
[0260] Method for evaluating the characteristics of hot-rolled steel sheets
[0261] tensile strength
[0262] If the tensile strength (TS) is 980 MPa or higher, it is judged to have high strength and pass. On the other hand, if the tensile strength (TS) is less than 980 MPa, it is judged to have no high strength and fail.
[0263] Hole expansion rate
[0264] If the hole expansion rate (λ) is 55% or more, it is judged to be excellent and passed. On the other hand, if the hole expansion rate is less than 55%, it is judged to be poor and failed.
[0265] Limit fracture plate thickness reduction rate
[0266] The limiting plate thickness reduction rate of hot-rolled steel sheets was evaluated by tensile testing.
[0267] A tensile test was performed using the same method as when evaluating tensile properties. With the plate thickness before the tensile test set to t1 and the minimum plate thickness at the center of the tensile specimen in the width direction after fracture set to t2, the limit fracture plate thickness reduction rate was obtained by calculating the value of (t1-t2)×100 / t1. The tensile test was performed five times, and the limit fracture plate thickness reduction rate was obtained by calculating the average value of three tests, excluding the maximum and minimum values of the limit fracture plate thickness reduction rate.
[0268] If the limit fracture plate thickness reduction rate is 75.0% or higher, it was determined to be a hot-rolled steel sheet with a high limit fracture plate thickness reduction rate and was judged to be acceptable. On the other hand, if the limit fracture plate thickness reduction rate is less than 75.0%, it was judged to be an unacceptable steel sheet that is not a hot-rolled steel sheet with a high limit fracture plate thickness reduction rate.
[0269] Shear workability (evaluation of the linearity of the boundary between the fracture plane and the shear plane)
[0270] Among the shear workability of hot-rolled steel sheets, the linearity of the boundary between the fracture surface and the shear surface was evaluated by performing a punching test and determining the degree of linearity at the boundary between the fracture surface and the shear surface.
[0271] Five punching holes were produced at the center of the width of a hot-rolled steel sheet with a hole diameter of 10 mm, a clearance of 15%, and a punching speed of 3 m / s. Next, for the five punching holes, the end surfaces parallel to the rolling direction at 10 locations (two end surfaces per punching hole) were photographed using an optical microscope. In the obtained observation photographs, the end surfaces as shown in FIG. 1 (a) can be observed. As shown in FIG. 1 (a) and (b), deflection, shear surface, fracture surface, and burr are observed on the end surfaces after punching. In addition, FIG. 1 (a) is a schematic diagram of the end surface parallel to the rolling direction of the punching hole, and FIG. 1 (b) is a schematic diagram of the side view of the punching hole. Deflection is a smooth surface of the R shape, shear plane is a punched end surface separated by shear deformation, fracture plane is a punched end surface separated by a crack that occurs near the cutting edge after the shear deformation ends, and burr is a surface having a protrusion protruding from the lower surface of a hot-rolled steel sheet.
[0272] In the observation photos of 10 end faces obtained from 5 end faces, the straightness at the boundary between the fracture face and the shear was measured by the method described below, and the maximum value of the obtained straightness was calculated.
[0273] In addition, the straightness at the boundary between the fracture surface and the shear was obtained by the following method.
[0274] As shown in FIG. 1(b), the boundary points between the shear plane and the fracture plane (points A and B in FIG. 1(b)) were determined with respect to the end plane. The length x of the straight line connecting these points A and B was measured. Next, the length y of the curve along the fracture plane-shear plane boundary was measured. The value obtained by dividing the obtained y by x was defined as the straightness at the boundary between the fracture plane and the shear plane.
[0275] In the punching test, if the maximum value of the straightness obtained is less than 1.045, it is judged to be a hot-rolled steel sheet with excellent shear workability and is deemed acceptable.
[0276] Meanwhile, if the maximum value of the obtained straightness is 1.045 or higher, it is judged to be unsatisfactory as a hot-rolled steel sheet that does not have excellent shear workability.
[0277] Crack resistance in bending
[0278] For the bending test specimen, a rectangular specimen of 100 mm × 30 mm was cut from the halfway point in the width direction of the hot-rolled steel sheet, and the crack resistance during bending was evaluated by the following bending test.
[0279] For both bending where the bending ridge is parallel to the rolling direction (L direction) (L-axis bending) and bending where the bending ridge is parallel to the direction perpendicular to the rolling direction (C direction) (C-axis bending), tests were conducted in accordance with the V-block method of JIS Z 2248:2006 (bending angle θ is 90°). By doing so, the minimum bending radius at which no crack occurs was determined. Crack resistance during bending was investigated. The value obtained by dividing the average of the minimum bending radii of the L-axis and C-axis by the plate thickness was set as the limiting bending R / t and used as an indicator value for crack resistance during bending. If R / t was 3.0 or less, it was determined to be a hot-rolled steel sheet with excellent crack resistance during bending.
[0280] However, the presence or absence of cracks was determined by mirror polishing the cross-section of the test specimen cut in a plane parallel to the bending direction and perpendicular to the plate surface after the test, observing the cracks with an optical microscope, and judging that cracks were present if the crack length observed on the inner side of the bend of the test specimen exceeded 30 μm.
[0281]
[0282]
[0283]
[0284]
[0285]
[0286]
[0287] Looking at Tables 5 and 6, it can be seen that the hot-rolled steel sheet according to the examples of the present invention has high strength and a limit fracture plate thickness reduction rate, as well as excellent hole expandability and shear workability. In addition, among the examples of the present invention, the hot-rolled steel sheet having an average crystal grain size of less than 3.0 μm in the surface layer has the above various characteristics and also has excellent crack resistance during bending.
[0288] Meanwhile, it can be seen that the hot-rolled steel sheet according to the comparative example has deteriorated one or more of the strength, limit fracture plate thickness reduction rate, hole expandability, and shear workability. Industrial applicability
[0289] According to the above embodiment of the present invention, a hot-rolled steel sheet having high strength and a reduction rate of plate thickness at the limit of fracture, along with excellent hole expandability and shear workability, can be provided. Furthermore, according to the above preferred embodiment of the present invention, a hot-rolled steel sheet having the above various characteristics and also having excellent crack resistance during bending, that is, in which the occurrence of cracks during bending is suppressed, can be obtained.
[0290] The hot-rolled steel sheet according to the present invention is suitable as an industrial material used for automobile components, machine structural components, and even building components.
Claims
Claim 1 The chemical composition, in mass%, is C: 0.040 to 0.250%, Si: 0.05 to 3.00%, Mn: 1.00 to 4.00%, sol.Al: 0.001 to 0.500%, P: 0.001 to 0.100% or less, S: 0 to 0.0300% or less, N: 0 to 0.1000% or less, O: 0 to 0.0100% or less, Ti: 0 to 0.300%, Nb: 0 to 0.100%, V: 0 to 0.500%, Cu: 0 to 2.00%, Cr: 0 to 2.00%, Mo: 0 to 1.00%, Ni: 0 to 2.00%, B: 0 to 0.0100%, Ca: 0 to 0.0200%, Mg: 0 to 0.0200%, REM: 0 to 0.1000%, Bi: 0 to 0.0200%, As: 0 to 0.100%, Zr: 0 to 1.00%, Co: 0 to 1.00%, Zn: 0 to 1.00%, W: 0 to 1.00%, Sn: 0 to 0.05%, and the remainder: Fe and impurities, satisfying the following formula (A), wherein the metal structure, in area %, has a total of martensite and tempered martensite exceeding 92.0% and not exceeding 100.0%, retained austenite less than 3.0%, ferrite less than 5.0%, and the remainder being bainite and pearlite with a total area percentage of 0% or more and less than 8.0%. One or two types are included, and the entropy value represented by the following equation (1), obtained by analyzing the SEM image of the metal structure by the gray level co-generation matrix method, is 11.0 or higher, the inverse difference normalized value represented by the following equation (2) is less than 1.020, and the cluster shade value represented by the following equation (3) is -8.0×10 5 Up to 8.0×10 5 A hot-rolled steel sheet characterized by having a standard deviation of Mn concentration of 0.60 mass% or less, wherein the standard deviation of Mn concentration is measured in an area from 1 / 8 depth of the plate thickness from the surface of the hot-rolled steel sheet to 3 / 8 depth of the plate thickness from the surface, and having a tensile strength of 980 MPa or more. However, each element symbol in the above formula (A) represents the content based on the mass % of the corresponding element, and if the corresponding element is not contained, 0% is substituted. Here, P(i, j) in the following formulas (1) to (5) is a gray level co-generation matrix, L in the following formula (2) is the number of gray scale levels that the above SEM image can take, i and j in the following formulas (2) and (3) are natural numbers from 1 to L, and μ in the following formula (3) x and μ y These are represented by the following equations (4) and (5), respectively. Claim 2 A hot-rolled steel sheet according to claim 1, characterized in that the average crystal grain size of the surface layer is less than 3.0 μm, and the surface layer is a region from the surface of the hot-rolled steel sheet to a depth of 50 μm from the surface. Claim 3 In claim 1 or 2, the chemical composition is, in mass%, Ti: 0.001 to 0.300%, Nb: 0.001 to 0.100%, V: 0.001 to 0.500%, Cu: 0.01 to 2.00%, Cr: 0.01 to 2.00%, Mo: 0.01 to 1.00%, Ni: 0.01 to 2.00%, B: 0.0001 to 0.0100%, Ca: 0.0001 to 0.0200%, Mg: 0.0001 to 0.0200%, REM: 0.0001 to 0.1000%, Bi: 0.0001 to 0.0200%, As: 0.001 to A hot-rolled steel sheet characterized by containing one or more types selected from the group consisting of 0.100%, Zr: 0.01 to 1.00%, Co: 0.01 to 1.00%, Zn: 0.01 to 1.00%, W: 0.01 to 1.00%, and Sn: 0.01 to 0.05%.
Citation Information
Patent Citations
Hot rolled steel sheet
JP2015098629A
Hot rolled steel sheet and production method therefor
JP2015214718A
700mpa high strength hot rolling q&p steel and manufacturing method thereof
WO2014166323A1
Hot-rolled steel sheet
WO2020184372A1