Magnetically tunable plasmon coupling of nanoshells made possible by space-free localized growth

A space-free growth process using a deformable polymer shell on magnetic cores addresses the challenges of Au nanoshell fabrication, enabling tunable plasmon coupling and resonance scattering for advanced optical applications.

KR103045418B1Active Publication Date: 2026-11-10RGT UNIV OF CALIFORNIA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020237015123
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-09
Filing Date
2021-10-11
Publication Date
2026-11-10
Estimated Expiration
2041-10-11

AI Technical Summary

Technical Problem

Existing methods for fabricating Au nanoshells face challenges in achieving large-scale production of high-quality, tunable resonant scattering due to issues with seed distribution and growth kinetics, particularly on small cores, leading to low scattering efficiency and uneven shell thickness, which hampers their application in biomedical and optical technologies.

Method used

A space-free localized growth process using a deformable polymer shell confines Au growth on a magnetic Fe3O4 core, enabling controlled seed-mediated growth and magnetic assembly into plasmonic chains, allowing for tunable plasmon coupling and resonance scattering.

Benefits of technology

The method produces high-quality Au nanoshells with enhanced scattering efficiency and tunability, suitable for applications in transparent displays and anti-counterfeiting devices, offering rapid, reversible, and chemical-free control over plasmon coupling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023049312514-PCT00001_ABST
    Figure 112023049312514-PCT00001_ABST
Patent Text Reader

Abstract

A method for forming a magnetic / plasmon hybrid structure is disclosed. The method comprises the steps of: synthesizing colloidal magnetic nanoparticles; modifying the magnetic nanoparticles in a solution of polymeric ligands; attaching metal seed nanoparticles to the surface of the magnetic nanoparticles; and forming a magnetic / plasmon hybrid structure by performing seed-mediated growth on the metal seed nanoparticles by reducing a metal salt in the solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This invention was made with government support under CHE-1808788 awarded by the National Science Foundation (NSF). The government holds specific rights to this invention.

[0002] The present disclosure generally relates to magnetically tunable plasmon coupling of nanoshells made possible by space-free localized growth, more particularly, for example, a method for forming magnetic / plasmon hybrid structures. Background Technology

[0003] Resonant scattering of plasmonic nanoparticles is garnering increasing attention due to new applications in flexible transparent displays, optical metasurfaces, smart windows, wearable electronics, and color holograms. These applications rely on strong localized surface plasmon resonance (LSPR), which can efficiently scatter light of specific wavelengths while remaining "transparent" at off-resonant wavelengths. Significant research efforts have been made to develop plasmonic structures with large scattering cross-sections and tunable resonant wavelengths by controlling the size, shape, and chemical characteristics of the plasmonic structures. In previous studies, it was recognized that large plasmonic nanospheres, particularly those of Au and Ag, possess scattering-dominant LSPR, and that their resonant wavelengths can be tuned from the visible region to the near-infrared (NIR) region simply by increasing the particle size. Since LSPR attenuates along depth from the surface, scattering efficiency decreases significantly as particle size increases. In the case of Au nanoparticles, their active skin depth was estimated to be only tens of nanometers, and due to a higher percentage of inert internal atoms, this leads to relatively low scattering efficiency in large solid particles.

[0004] Plasmon nanoshells with noble metal coatings on dielectric cores exhibit significantly higher scattering efficiency and wavelength tunability in LSPR than their solid counterparts. However, their practical implementation has been hampered by the lack of a robust method for the large-scale fabrication of high-quality nanoshells with tunable resonant scattering and significantly low off-resonant absorption. The conventional approach for Au nanoshells is to grow them directly from pre-immobilized seeds on organic or inorganic cores. Careful control of seed binding and growth kinetics may be required to avoid self-nucleation, which makes scaling up the process difficult. A more critical issue may lie in the fabrication of uniform and thin nanoshells, as the free growth of multiple seeds generates only thick Au shells through the fusion of large grains, which induces low plasmon activity and significantly broadened quenching due to the presence of high-density grain boundaries. Such growth is particularly problematic when the core size is less than approximately 100 nm due to the uneven distribution of metal seeds, e.g., gold (Au) seeds, and increased difficulty in controlling growth kinetics on highly curved surfaces. This poses an additional challenge to fully utilize the potential of Au nanoshells, particularly in biomedical applications, as small, thin shells allow for efficient extravasation into tissues or tumors and enable more convenient localization of LSPR in the most biomedically relevant visible and NIR regions.

[0005] Considering the above problem, a space-free localized growth process would be desirable to enable the production of high-quality, e.g., gold (Au), silver (Ag), or copper (Cu) nanoshells on a relatively small magnetic Fe3O4 core (e.g., 10 nm to 150 nm) having excellent plasmonic properties. According to an exemplary embodiment, the resulting core-shell nanoparticles can be magnetically assembled into a plasmonic chain, which can exhibit dynamically tunable coupled resonance scattering.

[0006] According to an exemplary embodiment, a soft, deformable, and highly transparent polymer shell is used to mediate and confine the seeded growth of metallic metals, e.g., Au, Ag, or Cu. The deformable polymer shell confines the seeded growth to the interface with the magnetic core, enabling the control of Au, Ag, or Cu growth without the need to create additional confining spaces or gaps in the templated synthesis. Its high deformability provides space for the formation of a complete metallic shell, while the elastomeric shell inhibits the deposition of metal (e.g., Au, Ag, or Cu) atoms and thus limits their growth along the radial direction. Additionally, the high magnetic susceptibility of the core enables the development of a new method for actively and reversibly tuning the plasmon coupling and resonant scattering of Au, Ag, or Cu nanoshells through the magnetic assembly of hybrid nanoparticles into plasmonic chains, making it a promising material for creating novel transparent displays and anti-counterfeiting devices.

[0007] According to one aspect, a method for forming a magnetic / plasmon hybrid structure is provided, comprising the steps of: synthesizing colloidal magnetic nanoparticles; modifying the magnetic nanoparticles in a solution of polymeric ligands; bonding metal seed nanoparticles to the surface of the magnetic nanoparticles; and performing seed-mediated growth on the metal seed nanoparticles by reducing a metal salt in the solution to form a magnetic / plasmon hybrid structure.

[0008] According to another aspect, a method of using a magnetic / plasmon structure in an anti-counterfeiting device is provided, comprising the steps of: fixing a one-dimensional plasmon chain in a pre-designed orientation to a solid polymer using a magnetic field; applying polarization from a first direction to the one-dimensional plasmon chain to produce a first color spectrum; and applying polarization from a second direction to the one-dimensional plasmon chain to produce a second color spectrum, wherein the first color spectrum is different from the second color spectrum.

[0009] According to an additional aspect, a magnetic / plasmon hybrid structure is provided comprising: a magnetic nanoparticle core; a deformable and permeable polymeric ligand shell; and a metal seed attached to the magnetic nanoparticle core, wherein the metal seed is configured to have limited growth as a result of the deformable and permeable polymeric ligand shell on the magnetic core inhibiting the deposition of metal atoms and limiting the growth of metal atoms along the radial direction. Brief explanation of the drawing

[0010] Figures 1a-1f, where Figure 1a is a schematic diagram of the seed-mediated growth of Au nanoshells on iron oxide nanospheres. TEM images of Fe3O4 nanospheres (Figure 1b), Fe3O4 / Au@RF (Figure 1c), and Fe3O4@Au@RF nanospheres (Figure 1d). Occurrence of plasmon peaks during the seeded growth of Au nanoshells on 125-nm (Figure 1e) and 20-nm (Figure 1f) Fe3O4 nanospheres. Figures 2a–2f are examples of customized resonance scattering of Au nanoshells. TEM images of Fe3O4@Au@RF nanospheres synthesized using Fe3O4 nanospheres with core diameters of 20 nm (Fig. 2a), 70 nm (Fig. 2b), 125 nm (Fig. 2c), and 150 nm (Fig. 2d). Figure 2e is an example of the UV-Vis spectra of Fe3O4@Au@RF nanospheres with different core diameters. Figure 2f is a digital photograph of a colloidal dispersion of Fe3O4@Au@RF nanospheres with core diameters of (i) 20 nm, (ii) 70 nm, (iii) 125 nm, and (iv) 150 nm. Figure 2g shows the UV-Vis spectra of the synthesized Au nanoshells as is after RF etching. The inset of Fig. 2g is from left to right: Fe3O4@Au@RF, Fe3O4@Au, and Fe3O4@Au solutions exposed to a magnetic field directed horizontally from left to right. The diameter of the Fe3O4 core is 20 nm. Figures 3a–3h illustrate the resonance scattering of Au nanoshells for transparent displays. Figure 3a shows the optical properties of Au nanoshells fabricated using 70-nm Fe3O4 nanospheres as cores. Figure 3b is an example of the light incidence direction during plasmonic excitation of Au nanoshells (70-nm core and 25-nm shell, left panel) and the color-coded surface (right panel) of the far-field radiation pattern of Au nanoshells excited by 710 nm light. Figure 3c shows the corresponding surface pointing vectors (surface arrows) and electric field distribution (color map) of the Au nanoshells. Figure 3d illustrates the fabrication of a PVA / Au composite film for transparent displays. The inner diameter of the gold nanoshells is 70 nm. Figure 3e is a photograph of the composite film under natural lighting. Figures 3f and 3g are photographs showing PVA / Au composite films containing hybrid nanoparticles with 70-nm (Fig. 3f) and 20-nm (Fig. 3g) Fe3O4 cores. Characters were generated by a projector, and then the films were illuminated with white light from the top column and monochromatic light from the bottom column. Figure 3h is a photograph of a pure PVA film under the same light illumination. Scale bar: 1 cm. Figures 4a–4c illustrate the plasmon coupling of Au nanoshells enabled by the self-assembly of Fe3O4@Au@RF nanospheres into plasmon chains. Figure 4a shows the extinction spectra of the plasmon chains measured under different electric field strengths. Figure 4b shows the measured extinction spectra of the plasmon chains under different orientations. Figure 4c is a polarized optical macroscopic (POM) image of Fe3O4@Au@RF nanoparticles under different magnetic fields. White arrows indicate the direction of the magnetic field. The polarization of the incident light is horizontal. Figures 5a–5d illustrate the coupled resonance scattering of Au nanoshells enabled by the self-assembly of Fe3O4@Au@RF nanospheres into plasmonic chains. Figure 5a is a schematic diagram of the lithography process for fabricating thin films with different chain orientations. Figure 5b is a normal and polarized optical microscope image of the boundary region with horizontal (left region) and vertical (right region) plasmonic nanochains. White arrows indicate the polarization of the incident light. The panel on the bottom right is under normal photoexcitation. Figure 5c is a digital photograph of the pattern under horizontal (top) and vertical polarization (bottom). Figure 5d is a digital image of the pattern under horizontal (top), vertical (middle), and 45° polarization (bottom). Scale bar: 10 μm (Figure 5b); Figures 5c and 500 μm (Figures 5c and 5d). Figures 6a–6h show the conceptual design. Simulated absorption (Fig. 6a), scattering (Fig. 6b), and extinction (Fig. 6c) cross-sections of an Au nanoshell. The thickness of the Au nanoshell is 25 nm. The core size increases from 20 nm to 150 nm. Figures 6d and 6e show simulated atomic scattering cross-sections of Au nanoshells (Fig. 6d) and solid Au nanoparticles (Fig. 6e) with different diameters. An Au nanoshell with a thickness of 25 nm was used for the simulation. Figure 6f shows the simulated atomic absorption cross-section of the Au nanoshell. Figure 6g shows the scattering performance index of the Au nanoshell. Figure 6h shows the near-field electric field distribution (right) and Poynting vector (left) of the Au nanoshell excited at the resonance wavelength as indicated. Figures 7a-7d are TEM images of Fe3O4 nanoparticles at 20 nm (Fig. 7a), 70 nm (Fig. 7b), 125 nm (Fig. 7c), and 150 nm (Fig. 7d). Figures 8a-8c show the chemical structures of PAA (Figure 8a) and branched PEI (Figure 8b). Figure 8c shows the zeta potential of magnetic nanoparticles before and after PEI modification. Figure 9 is an example of a TEM image of an Au seed. Figures 10a–10d show backscatter scanning electron microscopy of Fe3O4@Au@RF nanospheres with a 125-nm core in Figure 10a, corresponding elemental mapping of Au (Figure 10b) and Fe (Figure 10c), and the merged image in Figure 10d. Figures 11a and 11b show a typical TEM image of an Fe3O4@Au@RF nanosphere using 125-nm colloidal nanoparticles as a core and a high-magnification TEM image of the same. The selected area for the high-resolution image is indicated by a dashed box in Figure 11a. FIGS. 12a–12e show mock quenching cross-sections of Au nanoshells with different core sizes, as shown in FIG. 12a. Mock optical cross-sections of Au nanoshells with core diameters of 20 nm (Fig. 12b), 70 nm (Fig. 12c), 125 nm (Fig. 12d), and 150 nm (Fig. 12e). Figures 13a–13g show TEM images of Fe3O4@Au nanoparticles prepared by etching RF shells in NaOH solution. Core sizes: 20 nm (Fig. 13a), 70 nm (Fig. 13b), and 125 nm (Fig. 13c). Fig. 13d shows the quenching spectrum of Fe3O4@Au nanoparticles. Fig. 13e shows the mock quenching spectrum of Fe3O4@Au nanoparticles. UV-Vis spectra of synthesized and unsynthesized Au nanoshells before and after RF etching: Fig. 13f is the 20-nm core, and Fig. 13g is the 70-nm core. Inset of Fig. 13g: Solutions of Fe3O4@Au@RF and Fe3O4@Au with 70-nm cores under brightfield and darkfield conditions. Photographs highlighted by black and red frames represent the solutions before and after etching the RF shells, respectively. Figures 14a–14c show the "characters" projected onto a transparent screen by a commercial projector in Figure 14a. Specifically, "UCR" in the top column is white. The characters "UCR" in the bottom column are red, green, and blue, respectively, from left to right. Figures 14b and 14c are photographs showing projected images of a PVA / Au composite film as a transparent display fabricated with 20 nm (Fig. 14b) and 70 nm (Fig. 14c) Fe3O4 nanospheres as cores. Scale bar: 1 cm. Figure 15 is a schematic diagram of the active tuning of the plasmon coupling of the Au shell made possible by the self-assembly of Fe3O4@Au@RF nanoparticles. Specifically, a change in chain orientation with respect to optical polarization will change the plasmon excitation of the 1D nanochain, which further leads to a change in the scattering characteristics of the chain. Figures 16a–16d show the simulated extinction spectra of a plasmon chain under different particle separation, as shown in Figure 16a. Figure 16b is an example of the localized electric field distribution at intervals of 5 nm, 20 nm, and 40 nm. The excitation wavelengths from left to right are 750, 710, and 690 nm, respectively. Figure 16c is the simulated extinction spectrum of a plasmon chain under different orientations. The interparticle separation was set to 30 nm. Figure 16d is an example of the localized electric field distribution of a plasmon chain under orientations of 0°, 45°, and 90°. Figure 17 is a POM image of Fe3O4 / Au@RF dispersion under different magnetic fields. White arrows indicate the direction of the applied magnetic field. Fig. 18a shows the optical properties of an Au shell fabricated using 70 nm Fe3O4 nanoparticles as a core. Fig. 18b is a polarity plot showing the angular distribution of scattered light from the Au shell at 738 nm under p- and s-mode excitation. Fig. 18c shows the corresponding surface Poynting vector and electric field distribution of the Au shell. Fig. 18d shows the fabrication of a PVA / Au composite film for a transparent display. Fig. 18e is a photograph of the fabricated film under natural light. Photographs showing a transparent display fabricated with the PVA / Au composite film of Fig. 18f and the pure PVA film of Fig. 18g. Specific details for implementing the invention

[0011] Now, preferred embodiments of the present disclosure will be described in detail, and examples thereof are illustrated in the accompanying drawings.

[0012] According to exemplary embodiments, the active tuning of the plasmon coupling of metal nanoshells having well-confined plasmonic properties, e.g., Au, Ag, or Cu nanoshells, by unconventional space-free confined growth and nanoscale self-assembly is disclosed. Seeded growth of Au occurred exclusively at the hard-soft interface between the Fe3O4 core and the phenolic resin without the need to create confined space, which represents a general and clear approach for various core-shell nanostructures. The deformability of the permeable phenolic layer plays an essential role in controlling the interfacial growth of Au, Ag, or Cu nanoshells. While polymer elasticity inhibits the radial deposition of atoms, e.g., Au, Ag, and Cu atoms, its high deformability can provide sufficient space for the formation of conformal metallic shells. The coupled magnetic-plasmon properties enable active tuning of plasmon coupling and resonance scattering of Au, Ag, or Cu nanoshells by self-assembly of hybrid nanoparticles into plasmon chains, and their potential in application can be used to design transparent displays and anti-counterfeiting devices.

[0013] According to an exemplary embodiment, active tuning of the scattering of Au nanoshells is designed based on the fact that Au nanoshells are nearly "transparent" at off-resonant wavelengths and can selectively scatter light at specific wavelengths due to LSPR. According to an exemplary embodiment, simulations show that the resonant scattering of a 25-nm thick Au nanoshell redshifts from 590 nm to 980 nm as its core size increases from 20 nm to 70 nm, 125 nm, and eventually to 150 nm (Figs. 6a-6d). Compared to solid nanoparticles of the same diameter (Fig. 6e), Au nanoshells exhibit higher scattering efficiency due to enhancement at multiple interfaces and a wider tuning range due to their hybridized plasmon modes. First-order resonant scattering is located far from the strongest resonant absorption in the Au nanoshell (Fig. 6f), which facilitates scattering-based applications and induces reduced optical loss at the resonant frequency. In addition, the ratio between scattering efficiency and maximum absorption efficiency increases progressively with core size, and its value is greater than 1 over a broad spectrum (Fig. 6g). The surface scattering profile of the Au nanoshell (left panel of Fig. 6h) shows strong scattering around the entire surface. The electric field in the Au nanoshell with a larger core (right panel of Fig. 6h) has a much lower magnitude, which further confirms its lower absorption at the on-resonance wavelength.

[0014] According to an exemplary embodiment, a unique localized synthesis of Au nanoshells on magnetic nanoparticles is illustrated in Fig. 1a. For example, magnetite (Fe3O4) nanoparticles of different sizes ranging from 20 nm to 150 nm were synthesized using polyacrylic acid (PAA) as a capping ligand (Figs. 7a-7b). Fig. 1b shows a typical TEM image of 125-nm iron oxide nanoparticles with uniform size and excellent dispersibility. These exhibited superparamagnetism because each nanoparticle consisted of multiple sub-10-nm particles. Branched polyethyleneimine (PEI) was introduced onto the surface of the PAA-capped nanoparticles via electrostatic interactions, which was confirmed by a significant change in zeta potential from -70 mV to +90 mV (Fig. 8a). Subsequently, negatively charged Au seeds (approximately 2 nm, Fig. 9) capped with tetrakis(hydroxymethyl)phosphonium chloride were immobilized on the iron oxide surface via electrostatic adsorption to form Fe3O4 / Au nanoparticles for further seeded growth. Afterward, the composite particles were overcoated with a layer of water-permeable and soft phenolic resin via base-catalyst-growth polymerization of resorcinol and formaldehyde (RF). The thickness of the RF shell was 35 nm (Fig. 1c).

[0015] According to exemplary embodiments, one of the key aspects for the synthesis of uniform Au nanoshells is to ensure the homogeneous deposition of Au atoms on multiple seeds and to minimize the self-nucleation of free Au nanoparticles, which can be achieved by maintaining a low reduction rate. For example, H2O2 can be used as a mild reducing agent to support the seeded growth of Au nanoshells, as H2O2 has a pH-dependent standard reduction potential: 1.763 V in acidic solutions and 0.867 V in alkaline solutions. Under alkaline conditions, the role of H2O2 as a reducing agent is due to the anionic HO2 -This is made possible by the formation of. Therefore, to avoid etching the Au seed by H2O2, H2O2 is AuCl4 - (+0.93 V) and AuCl2 - The pH of the growth solution was adjusted to a slightly basic level by adding sodium oleate to have a reduction potential lower than (+1.15 V). Thus, H2O2 can sustain the continuous and exclusive deposition of Au atoms on multiple seeds to form an conformal coating, while its reducing power is carefully mitigated to minimize self-nucleation during seeded growth. Under alkaline conditions, the seeded growth of Au nanoshells occurs through the following process:

[0016] H2O2+ OH - = HO2 - + H2O (1)

[0017] 3HO2 - + AuCl4 - = Au + 3HO2· + 4Cl - (2)

[0018] Figure 1d shows the morphology of the particles after seeding and growth, where the complete Au nanoshell has a thickness of ~25 nm. The back-scattered scanning electron microscope (SEM) image in Figure 10a confirms the core / shell structure of the nanoparticles. Since Au has a much higher atomic number than Fe and O, the Au nanoshell can scatter electrons more efficiently and thus appears much "brighter" than the Fe3O4 core. Conversely, the RF shell cannot be observed in back-scatter mode due to the small atomic number of C, H, and O atoms and low electron scattering efficiency. Elemental mapping is shown in Figures 10b–10d, which also helps explain the core / shell structure of the final product. High-magnification TEM images are presented in Figures 11a and 11b, and the results clearly demonstrate the conformal coating of Au nanoshells rather than the presence of colloidal clusters at the Fe3O4-RF interface. In particular, the thickness of the RF shell decreased from an initial 35 nm to 18 nm during seeded growth, which suggests its expansion induced by the continuous deposition of Au atoms.

[0019] The optical properties of the Au nanoshells gradually changed during seeded growth (Fig. 1e). At 1 min, a single plasmon band appeared at 810 nm, indicating successful growth of Au within the RF shell. As the reaction progressed, the band shifted red first and then blue to 880 nm, consistent with the gradual thickening following the formation of a thin shell. Notably, another plasmon peak appeared at 675 nm in addition to the initial peak at 545 nm. Furthermore, as shown in Figs. 6a–6h, calculations indicate that the plasmon band at 880 nm originates from strong scattering by the Au nanoshells, whereas the two bands at shorter wavelengths exhibit absorption-dominant resonance. When using a 20-nm Fe3O4 core, a continuous red shift of a single plasmon band from 525 nm to 600 nm was observed (Fig. 1f). The absence of a plasmon band at 530 nm in the final product suggests that there were no self-nucleation events during seeded growth.

[0020] According to exemplary embodiments, the present method can be easily used to fabricate Au nanoshells having different core sizes. FIGS. 2a-2d present some Fe3O4@Au@RF nanoparticles synthesized using Fe3O4 cores of 20, 70, 125, and 150 nm, and 25 nm Au nanoshells. In their quenching spectra (Fig. 2d), a red shift of the plasmon band from 585 nm to 730, 875, and 960 nm, and a corresponding change in solution color from blue to green and brown were observed (Fig. 2f). The measured quenching spectra of the Au nanoshells match the mock spectra in FIGS. 12a-12e, indicating their high quality and well-defined plasmon characteristics. Considering the need for accessible metal surfaces in many plasmonic applications, particularly in biosensing, imaging, and SERS, a reliable etching process was further developed that can be used to remove the RF layer in an NaOH solution at 80°C while maintaining the excellent plasmonic properties of the hybrid particles. For Au nanoshells containing a 20-nm core, a blue shift from 600 nm to 540 nm was observed, accompanied by a color change from blue to red and a reduced peripheral refractive index from approximately 1.5 to 1.33 (Fig. 2g). Sharper peaks confirm the removal of RF and the excellent dispersibility of the Au nanoshells (Figs. 13a–13g). Fe3O4@Au nanoparticles could be magnetically detached from the solution when a magnet was placed near the solution (Inset in Fig. 2g).

[0021] This robust and flexible synthesis process allows for the convenient tuning of the optical scattering of Au nanoshells, providing significant opportunities for the fabrication of scattering-based applications. Simulations demonstrate that Fe3O4@Au nanoparticles with a 70-nm core and a 25-nm shell exhibit resonant scattering much stronger than absorption (Fig. 3a). At the resonant wavelength, the scattering field of the Au nanoshells resembles the radiation pattern of a typical dipole antenna (Fig. 3b). In Fig. 3c, the Poynting vector and localized electric field distribution further confirm the wide-angle scattering of the Au nanoshells. To utilize these interesting optical properties, Au nanoshells were incorporated into a transparent polymer matrix at a final Fe3O4@Au concentration of approximately 0.005 mg / mL, and the mixture was subsequently spin-cast onto a PDMS substrate (Fig. 3d). Upon drying, the film appeared highly transparent under ambient illumination (Fig. 3e). Interestingly, when strong white light was shone on the film, it appeared red (Fig. 3f, top column) when hybrid nanoparticles containing a 70-nm core were used and green (Fig. 3g, top column) when they had a 20-nm core, demonstrating selective scattering depending on the resonance frequency of the Au nanoshells. In both cases, a commercial image projector was used to illuminate the film, which had three white characters in the top column and three primary color (blue, green, and red) characters in the bottom column, as shown in Figs. 14a-14c. In Fig. 3f, because the Au nanoshell with a 70-nm core has a resonance wavelength at 685 nm and preferentially scatters red light, the film can display red characters (on the top column) when illuminated by character-containing white light. In FIG. 3g, the composite film displays green characters because the resonance wavelength (approximately 540 nm) of the embedded Au nanoshell is in the green color gamut (500 nm to 565 nm). More importantly, under monochromatic light illumination, the film can display a corresponding pattern only when the wavelength of the projected light and the plasmon band match.As shown in the bottom column of FIGS. 3f and 3g, films prepared from Au nanoshells having 20-nm and 70-nm cores can selectively display green and red characters, respectively, whereas characters are not easily recognizable in the case of mismatch. In contrast, due to the lack of strong scattering, images could hardly be observed on a pure polymer film without Au nanoshells under the same projected light (Fig. 3h). According to exemplary embodiments, such transparent films can find interesting applications such as anti-counterfeiting devices or information displays.

[0022] The integration of magnetic and plasmonic properties in the core-shell structure enables the active tuning of the plasmonic coupling of Au nanoshells by their self-assembly into 1D nanochains (Fig. 15). Optical cross-sections of the assembled chains under different interparticle separation and orientations were first calculated. For plasmonic chains containing Au nanoshells with a 50-nm core, the redshift of the coupling band could be observed from, for example, 40 nm to 5 nm as the interparticle separation decreased, and the enhancement of the localized electric field within the gap also increased significantly (Figs. 16a and 16b). Meanwhile, for nanochains with an interparticle separation of 30 nm, the intensity of the peak at approximately 695 nm decreased as the angle between the chain orientation and polarization changed from 0° to 90° (Figs. 16c and 16d). To confirm the plasmon coupling of Au nanoshells, the extinction spectra of Fe3O4@Au@RF were measured under different magnetic fields. The peak position of the coupling band was slightly red-shifted due to reduced inter-particle separation as the electric field strength increased (Fig. 4a). In Fig. 4b, the coupling peak reached a maximum value when a magnetic field parallel (0°) to the polarization of the incident light was applied. A gradual increase in the angle weakened the coupling strength, and accordingly, the peak intensity of the coupling band at approximately 725 nm decreased.

[0023] Self-assembly and orientation control represent a reliable method for actively controlling the coupled resonant scattering of Au nanoshells. As shown in the optical microscope image in Fig. 4c, only bright spots resulting from scattering by individual nanoparticles were observed in the absence of any magnetic field. When a magnetic field parallel to optical polarization was applied, 1D chains with a bright red color were immediately formed. This extremely rapid response is attributed to the high saturation magnetization of the Fe3O4 core. When the magnetic field was removed, the chains disintegrated due to surface electrostatic repulsion of the RF shell, which enabled reversible and dynamic tuning of the plasmon coupling of the Au nanoshells. Interestingly, the apparent color of the 1D chains depended on their orientation under linear polarization. When the orientation of the chains was parallel to optical polarization, a bright red color was observed. Under the other two vertical orientations, the red color disappeared. To further confirm the plasmon origin of the color, control experiments were performed using nanoparticles as building blocks prior to seeded growth. As shown in Fig. 17, no distinct color was observed under three typical orientations. Therefore, it is reasonable to conclude that the perceived red color of the 1D chain originates from the coupled resonance scattering of the Au nanoshells.

[0024] Compared to previous methods for actively tuning the coupling of plasmonic nanostructures, such as altering surrounding dielectrics or interparticle separation through chemical and electronic doping, the self-assembly approach offers the advantages of rapid response, complete reversibility, and chemical-free control. The magnetic anisotropy of the 1D plasmonic chain also facilitates control over the assembly orientation. Thus, a color-changing anti-counterfeiting device can be fabricated by immobilizing the plasmonic chain in a pre-designed orientation onto a photocurable polymer (Fig. 5a). As shown in the optical microscope image in Fig. 5b, under vertical polarization, the right region appeared red due to coupled resonant scattering of the Au nanoshells, while the left region was brown. When the polarizer was rotated to a horizontal position, the colors of these two regions were switched. Furthermore, the color contrast between the two regions disappeared at a relative angle of 45° or in the absence of the polarizer, as the plasmonic excitation of the 1D chain was the same in both cases. Figures 5c and 5d show two patterns generated by a multi-step lithography method. The color contrast of the perceived pattern can be simply changed by switching the polarization of the incident light, which can potentially be used for anti-counterfeiting or information encryption.

[0025] In summary, an unconventional synthesis approach for Au nanoshells was developed by confining the seeded growth of Au within the hard-soft interface between an Fe3O4 core and a deformable RF shell. The growth of Au nanoshells does not require a confining gap or space, but instead relies on the elastic deformation of the cross-linked RF shell. The fabricated Au nanoshells possess excellent plasmonic properties, which can be easily tuned from the visible region to the NIR region simply by increasing the core size. This space-free confined growth can potentially be extended to synthesize other core-shell nanostructures, where growth is preferably parallel rather than perpendicular to the core surface. The well-confined, highly customizable optical properties of Au nanoshells enable the successful development of unique transparent displays and anti-counterfeiting colorimetric devices. Furthermore, nanoscale self-assembly strategies offer many advantages for actively tuning the plasmonic coupling of nanostructures, including instantaneous response, chemical-free remote control, and complete reversibility.

[0026] Synthesis of Au shells

[0027] Chemicals: All chemicals were used directly without further purification. Ethanol was purchased from Decon Labs. Iron(III) chloride hexahydrate, tetraethyl orthosilicate (TEOS), polyacrylic acid (PAA, MW=1800), sodium hydroxide, polyvinylpyrrolidone (PVP, MW=10000), resorcinol (R), formaldehyde f, 2-hydroxy-2-methylpropiophenone, polyvinyl alcohol (PVA), 2-hydroxy-2-methylpropiophenone, and tetrakis(hydroxymethyl)phosphonium chloride (THPC) were purchased from Sigma-Aldrich. Ammonium hydroxide and hydrogen peroxide (H2O2) were purchased from Fisher Scientific. Chlorogenic(III) acid trihydrate (HAuCl4·3H2O) and ethylene glycol (EG) were from Acros Organics. Acrylamide (AM) and N,N'-methylenebisacrylamide (BIS) were purchased from Fluka. Sodium oleate salt (NaOL) was purchased from TCI America. Sylgard 184 silicone elastomer curing agent and Sylgard 184 silicone elastomer base were purchased from Dow Silicon Corporation. Acrylamide (AM) and N,N'-methylenebisacrylamide (BIS) were purchased from Fluka.

[0028] Synthesis of Fe3O4 Nanoparticles: Colloidal particles of Fe3O4 nanoparticles with adjustable sizes were synthesized. The reaction was carried out in solution at elevated temperatures. A stock solution was prepared by dissolving 50 mmol NaOH in 20 mL of DEG and heated at 120°C for 1 hour under nitrogen protection. The solution was maintained at 70°C as the stock solution. In a typical synthesis, PAA (4 mmol) and FeCl3 (0.4 mmol) were dissolved in DEG (17 mL), and the mixture was heated to 22°C for 30 minutes under nitrogen protection. A specific amount of stock solution was rapidly injected. The mixture was heated at 220°C for an additional 1 hour. The volumes of the stock solution were 1.7, 1.75, and 1.8 mL for the synthesis of Fe3O4 nanoparticles with average diameters of 70, 125, and 150 nm, respectively. The obtained Fe3O4 nanoparticles were washed several times with deionized water and dispersed in 20 mL of water.

[0029] PEI Modification: For PEI modification, 5 mL (0.25 batch) of an aqueous solution of Fe3O4 nanoparticles was added to 30 mL of a PEI solution (20 mg / mL, Mw=800) under sonication. The mixed solution was stirred overnight by vortexing. Magnetic stirring was not suggested during PEI modification to eliminate magnetic field-induced aggregation. Subsequently, the Fe3O4 nanoparticles were washed three times with water and then dispersed in 5 mL of water.

[0030] Au seed preparation: THPC (12 μL) and NaOH (250 μL, 2M) were added to 45 mL of water. After stirring for 5 minutes, 2 mL of HAuCl4 was added. The Au seed (Aus) solution was stored in a dark room for further attachment.

[0031] Au Seed Attachment: 5 mL of a PEI-modified Fe3O4 nanoparticle solution was slowly added to 30 mL of an Au seed solution under sonication. The mixed solution was stirred for approximately 1 hour. Excess Au seeds were removed by centrifugation. Au seeds were attached to the surface of Fe3O4 nanoparticles via electrostatic interactions to form Fe3O4 / Aus nanoparticles. These were further washed three times with water and dispersed in 10 mL of water.

[0032] RF Coating: PVP modification was performed prior to RF coating. In a typical process, 10 mL of a Fe3O4 / Aus solution was added to 30 mL of a PVP solution (5 mg / mL) under sonication. The solution was stirred overnight by vortexing. The solution was washed three times with water to remove excess PVP. Finally, these were dispersed in 28 mL of water for RF coating. In the base-catalyst step-growth polymerization, 20 mg R and 28 μL of F were added sequentially. 100 μL of an ammonia solution (2.8%) was added to the solution. The reaction mixture was first sonicated for 1 hour and then transferred to a 50 mL round-bottom flask. The reaction was maintained at 100°C for 3 hours to further condense the RF resin and increase its crosslinking ratio. After cooling to room temperature, the solution was washed three times with water. Subsequently, the obtained Fe3O4 / Aus@RF was finally dispersed in 2 mL of water.

[0033] Seed-mediated growth of Au nanoshells: In a typical process, 500 μL of PVP (50 mg / mL, Mw=40000), 100 μL of NaOL (10 mM), 20 μL of HAuCl4 (0.25 M), and 250 μL of H2O were sequentially added to 7.5 mL of deionized water. Subsequently, 25 μL of Fe3O4 / Aus@RF solution was added. The reaction was carried out at room temperature for 30 minutes. The product was washed three times with deionized water and dispersed in deionized water for characterization.

[0034] RF Shell Etching: A solution of Fe3O4@Au@RF nanoparticles was first dispersed in a 2 M NaOH solution. To improve the dispersibility of the colloidal particles, the reaction was carried out in the presence of 0.5 M PVP. After incubation overnight at 80°C, the Fe3O4@Au nanoparticles were washed three times with deionized water. The removal of RF also led to a blue shift from 730 nm to 685 nm in the plasmon band of the Au shell synthesized with a 70-nm core (Fig. S8g). In contrast to a bright background, the color perceived in the colloidal dispersion was complementary to the plasmon quenching. Thus, the color changed from green to light blue (left two panels in the inset of Fig. 13g). Interestingly, in contrast to the dark background, the two solutions before and after removing the RF shell appeared red (the two right panels in Fig. 13g), which is attributed to strong scattering of red light at 622 to 770 nm.

[0035] Characterization: Extinction spectra were measured using an Ocean Optics HR2000 spectrometer. TEM images were taken at 120 kV on a Tecnai 12 transmission electron microscope. Dark-field optical macroscopic images were taken using a Zeiss AXIO Imager optical microscope. SEM images were taken on a ThermoFisher Scientific (formerly FEI / Philips) NNS450 scanning electron microscope equipped with a backscatter electron detector. Elemental mapping was performed at 50 kV.

[0036] Production of Plasmon Films

[0037] Preparation of PVA-Au Composite Film: A PDMS film served as a transparent substrate for the PVA-plasmonic composite film. A silicon elastomer curing agent and a silicon elastomer base were thoroughly mixed in a mass ratio of 1 to 10. The mixture was left under ambient conditions for 2 hours to remove air bubbles from the viscous solution. Subsequently, it was cured at 60°C for 2 hours. First, a 10% PVA solution was prepared by dissolving PVA in deionized water under sonication. Then, a specific amount of the PVA solution was added to the Au shell solution to a final concentration of approximately 0.005 mg / mL. The obtained mixture solution was spin-cast onto a PDMS substrate. To form a uniform thin PVA film, the PDMS substrate was first treated with plasma for 20 minutes. The cast film was dried under vacuum at room temperature.

[0038] Preparation of anti-counterfeiting film: 2-hydroxy-2-methylpropiophenone acts as a photoinitiator. AM is the monomer, and BIS is the crosslinking agent. In a typical process, 250 mg of AM, 14 mg of BIS, and 3 μL of 2-hydroxy-2-methylpropiophenone were added to 1 mL of DEG. The Au shell was first precipitated by centrifugation and then dispersed in the DEG solution. The mixture solution was sandwiched between glass slides and then exposed to UV light (254 nm) for 1 minute. A photomask having a pre-designed pattern was placed over the sample, and a magnetic field was applied (B1). After the first UV exposure, 1D plasmon chains aligned parallel to the external field were fixed to the uncovered area. Subsequently, the photomask was removed, and a second UV exposure was applied to polymerize the remainder of the film under a horizontal magnetic field (B2). Magnetic alignment was achieved by placing the mixture at the center of two identical permanent magnets. The electric field strength was measured to be 25 mT (250 G).

[0039] Analysis of optical properties of Au nanoshells by the finite element method

[0040] Calculation of the optical cross-section of a single Au nanoshell: The calculation of the optical cross-section and efficiency is achieved based on the finite element method (Comsol Multiphysics). Spheres with a core-shell-shell geometry are modeled to mimic the Fe3O4@Au@RF nanostructure. The refractive index of RF is confirmed to be 1.5. The Au domain is defined by the embedded "Au" material. Its physical properties, such as the wavelength-dependent complex refractive index, are fully described in the Comsol Multiphysics materials library. In the case of the Fe3O4 domain, its refractive index is also wavelength-dependent and has a complex value where the real part determines the scattering properties and the imaginary part determines the absorption of the Fe3O4 material. To analyze the size-dependent chance of the Au shell (Figs. 1a-1f), the thicknesses of the Au and RF shells are 25 nm and 20 nm, respectively. Instead, the diameter of the magnetic core increases from 20 nm to 30 nm, 50 nm, 70 nm, 80 nm, 90 nm, 100 nm, 125 nm, and 150 nm. Its scattering (σ sca ), absorption (σ abs ) and extinction (σ ext The cross-section is calculated by solving Maxwell's equations in Comsol Multiphysics. The optical coefficients (Q) of the Au shell, such as scattering and absorption coefficients, were calculated by dividing the corresponding optical cross-section by the physical cross-section of the Au shell. The correlation between them is σ = Qπr 2 It can be expressed as, where r is the radius of the Au shell.

[0041] Analysis of coupling between Au nanoshells within the plasmonic chain: The optical cross-section of the plasmonic chain was also calculated by the finite element method. In terms of geometry, 1D chains containing Au shells with well-controlled interparticle separation and orientation were first generated in Comsol Multiphysics. Subsequently, σ ext Calculated and normalized with respect to the number of Au shells in the 1D chain.

[0042] Synthesis of Au shells

[0043] Chemicals: All chemicals were used directly without further purification. Ethanol was purchased from Decon Labs. Iron(III) chloride hexahydrate, tetraethyl orthosilicate (TEOS), polyacrylic acid (PAA, MW=1800), sodium hydroxide, polyvinylpyrrolidone (PVP, MW=10000), resorcinol(R), formaldehyde f, 2-hydroxy-2-methylpropiophenone, polyvinyl alcohol (PVA), 2-hydroxy-2-methylpropiophenone, and tetrakis(hydroxymethyl)phosphonium chloride (THPC) were purchased from Sigma-Aldrich. Ammonium hydroxide and hydrogen peroxide (H2O2) were purchased from Fisher Scientific. Chlorogenic(III) acid trihydrate (HAuCl4·3H2O) and ethylene glycol (EG) were from Acros Organics. Acrylamide (AM) and N,N'-methylenebisacrylamide (BIS) were purchased from Fluka. Sodium oleate salt (NaOL) was purchased from TCI America. Sylgard 184 silicone elastomer curing agent and Sylgard 184 silicone elastomer base were purchased from Dow Silicon Corporation. Acrylamide (AM) and N,N'-methylenebisacrylamide (BIS) were purchased from Fluka.

[0044] Synthesis of Fe3O4 Nanoparticles: Colloidal particles of Fe3O4 nanoparticles with adjustable sizes were synthesized. The reaction was carried out in solution at elevated temperatures. A stock solution was prepared by dissolving 50 mmol NaOH in 20 mL of DEG and heated at 120°C for 1 hour under nitrogen protection. The solution was maintained at 70°C as the stock solution. In a typical synthesis, PAA (4 mmol) and FeCl3 (0.4 mmol) were dissolved in DEG (17 mL), and the mixture was heated to 22°C for 30 minutes under nitrogen protection. A specific amount of stock solution was rapidly injected. The mixture was heated at 220°C for an additional 1 hour. The volumes of the stock solution were 1.7, 1.75, and 1.8 mL for the synthesis of Fe3O4 nanoparticles with average diameters of 70, 125, and 150 nm, respectively. The obtained Fe3O4 nanoparticles were washed several times with deionized water and dispersed in 20 mL of water.

[0045] PEI Modification: For PEI modification, 5 mL (0.25 batch) of an aqueous solution of Fe3O4 nanoparticles was added to 30 mL of a PEI solution (20 mg / mL, Mw=800) under sonication. The mixed solution was stirred overnight by vortexing. Magnetic stirring was not suggested during PEI modification to eliminate magnetic field-induced aggregation. Subsequently, the Fe3O4 nanoparticles were washed three times with water and then dispersed in 5 mL of water.

[0046] Au seed preparation: THPC (12 μL) and NaOH (250 μL, 2M) were added to 45 mL of water. After stirring for 5 minutes, 2 mL of HAuCl4 was added. The Au seed (Aus) solution was stored in a dark room for further attachment.

[0047] Au Seed Attachment: 5 mL of a PEI-modified Fe3O4 nanoparticle solution was slowly added to 30 mL of an Au seed solution under sonication. The mixed solution was stirred for approximately 1 hour. Excess Au seeds were removed by centrifugation. Au seeds were attached to the surface of Fe3O4 nanoparticles via electrostatic interactions to form Fe3O4 / Aus nanoparticles. These were further washed three times with water and dispersed in 10 mL of water.

[0048] RF Coating: PVP modification was performed prior to RF coating. In a typical process, 10 mL of a Fe3O4 / Aus solution was added to 30 mL of a PVP solution (5 mg / mL) under sonication. The solution was stirred overnight by vortexing. The solution was washed three times with water to remove excess PVP. Finally, these were dispersed in 28 mL of water for RF coating. In the base-catalyst step-growth polymerization, 20 mg R and 28 μL of F were added sequentially. 100 μL of an ammonia solution (2.8%) was added to the solution. The reaction mixture was first sonicated for 1 hour and then transferred to a 50 mL round-bottom flask. The reaction was maintained at 100°C for 3 hours to further condense the RF resin and increase its crosslinking ratio. After cooling to room temperature, the solution was washed three times with water. Subsequently, the obtained Fe3O4 / Aus@RF was finally dispersed in 2 mL of water.

[0049] Seed-mediated growth of Au nanoshells: In a typical process, 500 μL of PVP (50 mg / mL, Mw=40000), 100 μL of NaOL (10 mM), 20 μL of HAuCl4 (0.25 M), and 250 μL of H2O were sequentially added to 7.5 mL of deionized water. Subsequently, 25 μL of Fe3O4 / Aus@RF solution was added. The reaction was carried out at room temperature for 30 minutes. The product was washed three times with deionized water and dispersed in deionized water for characterization.

[0050] RF Shell Etching: A solution of Fe3O4@Au@RF nanoparticles was first dispersed in a 2 M NaOH solution. To improve the dispersibility of the colloidal particles, the reaction was carried out in the presence of 0.5 M PVP. After incubation overnight at 80°C, the Fe3O4@Au nanoparticles were washed three times with deionized water. The removal of RF also led to a blue shift from 730 nm to 685 nm in the plasmon band of the Au shell synthesized with a 70-nm core (Fig. 13g). In contrast to a bright background, the color perceived in the colloidal dispersion was complementary to the plasmon quenching. Thus, the color changed from green to light blue (the two left panels in the inset of Fig. 13g). Interestingly, in contrast to the dark background, the two solutions before and after removing the RF shell appeared red (the two right panels in Fig. 13g), which is attributed to strong scattering of red light at 622 to 770 nm.

[0051] Characterization: Extinction spectra were measured using an Ocean Optics HR2000 spectrometer. TEM images were taken at 120 kV on a Technai 12 transmission electron microscope. Dark-field optical macroscopic images were taken using a Zeiss Axio Imager optical microscope. SEM images were taken on a Thermo Fisher Scientific (formerly FEI / Philips) NNS450 scanning electron microscope equipped with a backscatter electron detector. Elemental mapping was performed at 50 kV.

[0052] Production of Plasmon Films

[0053] Preparation of PVA-Au Composite Film: A PDMS film served as a transparent substrate for the PVA-plasmonic composite film. A silicon elastomer curing agent and a silicon elastomer base were thoroughly mixed in a mass ratio of 1 to 10. The mixture was left under ambient conditions for 2 hours to remove air bubbles from the viscous solution. Subsequently, it was cured at 60°C for 2 hours. First, a 10% PVA solution was prepared by dissolving PVA in deionized water under sonication. Then, a specific amount of the PVA solution was added to the Au shell solution to a final concentration of approximately 0.005 mg / mL. The obtained mixture solution was spin-cast onto a PDMS substrate. To form a uniform thin PVA film, the PDMS substrate was first treated with plasma for 20 minutes. The cast film was dried under vacuum at room temperature.

[0054] Preparation of anti-counterfeiting film: 2-hydroxy-2-methylpropiophenone acts as a photoinitiator. AM is the monomer, and BIS is the crosslinking agent. In a typical process, 250 mg of AM, 14 mg of BIS, and 3 μL of 2-hydroxy-2-methylpropiophenone were added to 1 mL of DEG. The Au shell was first precipitated by centrifugation and then dispersed in the DEG solution. The mixture solution was sandwiched between glass slides and then exposed to UV light (254 nm) for 1 minute. A photomask having a pre-designed pattern was placed over the sample, and a magnetic field was applied (B1). After the first UV exposure, 1D plasmon chains aligned parallel to the external field were fixed to the uncovered area. Subsequently, the photomask was removed, and a second UV exposure was applied to polymerize the remainder of the film under a horizontal magnetic field (B2). Magnetic alignment was achieved by placing the mixture at the center of two identical permanent magnets. The electric field strength was measured to be 25 mT (250 G).

[0055] Analysis of optical properties of Au nanoshells by the finite element method

[0056] Calculation of the optical cross-section of a single Au nanoshell: The calculation of the optical cross-section and efficiency is achieved based on the finite element method (Comsol Multiphysics). Spheres with a core-shell-shell geometry are modeled to mimic the Fe3O4@Au@RF nanostructure. The refractive index of RF is confirmed to be 1.5. The Au domain is defined by the embedded "Au" material. Its physical properties, such as the wavelength-dependent complex refractive index, are fully described in the Comsol Multiphysics materials library. In the case of the Fe3O4 domain, its refractive index is also wavelength-dependent and has a complex value where the real part determines the scattering properties and the imaginary part determines the absorption of the Fe3O4 material. To analyze the size-dependent chance of the Au shell (Figs. 1a-1f), the thicknesses of the Au and RF shells are 25 nm and 20 nm, respectively. Instead, the diameter of the magnetic core increases from 20 to 30, 50, 70, 80, 90, 100, 125, and 150 nm. Its scattering (σ sca ), absorption (σ abs ) and extinction (σ ext The cross-section is calculated by solving Maxwell's equations in Comsol Multiphysics. The optical coefficients (Q) of the Au shell, such as scattering and absorption coefficients, were calculated by dividing the corresponding optical cross-section by the physical cross-section of the Au shell. The correlation between them is σ = Qπr 2 It can be expressed as, where r is the radius of the Au shell.

[0057] Analysis of coupling between Au nanoshells within the plasmonic chain: The optical cross-section of the plasmonic chain was also calculated by the finite element method. In terms of geometry, 1D chains containing Au shells with well-controlled interparticle separation and orientation were first generated in Comsol Multiphysics. Subsequently, σ ext Calculated and normalized with respect to the number of Au shells in the 1D chain.

[0058] Manufacturing of transparent displays

[0059] According to an exemplary embodiment, a transparent display was fabricated by incorporating an Au shell into a PVA film to utilize the strong scattering of the Au shell. Its scattering characteristics were first investigated by finite element analysis. As shown in Fig. 18a, the peak positions of the measured spectrum of Fe3O4@Au with a 70 nm core match well with the calculated cross-section. The slight discrepancy at the off-resonance wavelength is likely due to the broadband absorption of iron oxide. The calculated cross-section confirms that the resonance scattering of the Au shell is much stronger than the absorption, and thus confirms that the Au shell is ideal for transparent displays because it scatters light only at specific wavelengths while remaining "transparent" elsewhere. Under p-mode (Fig. 18b), a similar scattering pattern was observed as a Lambertian distribution of an ideal diffuse reflective surface. However, in the case of s-mode, scattering occurred over a wider range, indicating that the scattering of the Au shell can be seen from a wide angle. The Poynting vector and localized electric field distribution are illustrated in Fig. 18c, which further confirm the wide-angle scattering of the Au shell. To incorporate the Au shell into the transparent polymer matrix, a 10 wt% aqueous PVA solution was added to the Au shell dispersion to a final concentration of approximately 0.005 mg / mL. The mixture was spin-cast onto a PDMS film, placed under ambient conditions to remove bubbles, and dried (Fig. 18d). The digital photograph of the film shown in Fig. 18e demonstrates the high transparency of the fabricated film, as details behind the landscape could be observed with only slight changes in their appearance color and brightness. In Fig. 18f, the transparent film was observed during operation using red text projected onto a screen. The projected image was clearly visible and could be viewed from all directions. Conversely, the pure polymer film without the Au shell appeared dark, and the image was barely observable under the same laser projector due to a lack of scattering (Fig. 18g).

[0060] According to an exemplary embodiment, a method for forming a magnetic / plasmon hybrid structure is provided, comprising the steps of: synthesizing colloidal magnetic nanoparticles; modifying the magnetic nanoparticles in a solution of a polymeric ligand; attaching a metal seed nanoparticle to the surface of the magnetic nanoparticles; and performing seed-mediated growth on the metal seed nanoparticles by reducing a metal salt in the solution to form a magnetic / plasmon hybrid structure. The method may further comprise, prior to performing seed-mediated growth, coating the magnetic nanoparticles containing the surface-attached metal seed nanoparticles with a polymer shell of resorcinol-formaldehyde resin. Additionally, optionally, the resorcinol-formaldehyde coating is removed from the plasmon structure after seed-mediated growth.

[0061] According to an exemplary embodiment, the polymeric ligand is polyethyleneimine (PEI). The magnetic nanoparticles comprise iron oxide, e.g., Fe3O4. The metal seed nanoparticles may comprise gold, silver, or copper. Additionally, the metal salt may comprise a salt of gold, silver, or copper.

[0062] According to an exemplary embodiment, the method may further comprise mediating and localizing the seeded growth of a metal on magnetic nanoparticles by a polymeric ligand, wherein the polymeric ligand forms a deformable and permeable polymer shell on the magnetic nanoparticles that inhibits the deposition of metal atoms and limits the growth of metal atoms along the radial direction. Additionally, the magnetic / plasmon hybrid structure may be a plurality of magnetic / plasmon hybrid structures, which are magnetically assembled into a plasmon chain in an active transparent display or anti-counterfeiting device. According to an exemplary embodiment, the synthesis of the colloidal particles may be controlled to an outer diameter of 10 nm to 150 nm.

[0063] The above detailed description describes the method for forming a magnetic / plasmon hybrid structure, the method for using a magnetic / plasmon hybrid structure, and versions of the magnetic / plasmon hybrid structure, illustrating examples of the magnetic / plasmon hybrid structure disclosed herein. However, the present invention is not limited to the exact embodiments and variations described. Various variations, modifications, and equivalents may be made by those skilled in the art without departing from the spirit and scope of the invention as defined in the appended claims. All such variations, modifications, and equivalents falling within the scope of the claims are clearly intended to be encompassed by the claims.

Claims

Claim 1 A method for forming a magnetic / plasmon hybrid structure, comprising the steps of: synthesizing colloidal magnetic nanoparticles; modifying the magnetic nanoparticles in a solution of polymeric ligands; attaching metal seed nanoparticles to the surface of the magnetic nanoparticles; performing seed-mediated growth on the metal seed nanoparticles by reducing a metal salt in the solution to form a magnetic / plasmon hybrid structure; and coating the magnetic nanoparticles containing the surface-attached metal seed nanoparticles with a polymer shell of resorcinol-formaldehyde resin, and then performing seed-mediated growth of the metal. Claim 2 A method for forming a magnetic / plasmon hybrid structure according to claim 1, optionally further comprising removing a resorcinol-formaldehyde coating from a plasmon structure after seed-mediated growth. Claim 3 A method for forming a magnetic / plasmon hybrid structure according to claim 1, wherein the polymeric ligand is polyethyleneimine (PEI). Claim 4 A method for forming a magnetic / plasmon hybrid structure according to claim 1, wherein the magnetic nanoparticles contain iron oxide. Claim 5 A method for forming a magnetic / plasmon hybrid structure in which iron oxide is Fe3O4, according to claim 4. Claim 6 A method for forming a magnetic / plasmon hybrid structure according to claim 1, wherein the metal seed nanoparticles comprise gold, silver, or copper. Claim 7 A method for forming a magnetic / plasmon hybrid structure according to claim 1, wherein the metal salt comprises a salt of gold, silver, or copper. Claim 8 A method for forming a magnetic / plasmon hybrid structure according to claim 1, further comprising forming a deformable and permeable polymer shell on magnetic nanoparticles that mediates and localizes the seeded growth of metal on the magnetic nanoparticles with a polymeric ligand, inhibits the deposition of metal atoms, and limits the growth of metal atoms along the radial direction. Claim 9 A method for forming a magnetic / plasmon hybrid structure according to claim 1, wherein the magnetic / plasmon hybrid structure comprises a plurality of magnetic / plasmon hybrid structures, and further comprises magnetically assembling the plurality of magnetic / plasmon hybrid structures into a plasmon chain in an active transparent display or anti-counterfeiting device. Claim 10 A method for forming a magnetic / plasmon hybrid structure according to claim 1, further comprising controlling the synthesis of colloidal particles to an outer diameter of 10 nm to 150 nm. Claim 11 A method for forming a magnetic / plasmon hybrid structure according to claim 1, further comprising using the plasmon structure in a biomedical application. Claim 12 A method of using a magnetic / plasmon structure in an anti-counterfeiting device, comprising the steps of: fixing a one-dimensional plasmon chain in a pre-designed orientation to a solid polymer using a magnetic field; applying polarization from a first direction to the one-dimensional plasmon chain, which represents a first color spectrum; and applying polarization from a second direction to the one-dimensional plasmon chain, which represents a second color spectrum, wherein the first color spectrum is different from the second color spectrum. Claim 13 A method of using a magnetic / plasmon structure in an anti-counterfeiting device, wherein, in paragraph 12, the first color spectrum and the second color spectrum each include a first color region and a second color region, and the first color region and the second color region for each of the first color spectrum and the second color spectrum are switched from a first direction of polarization to a second direction. Claim 14 A method of using a magnetic / plasmon structure in an anti-counterfeiting device, wherein the first direction and the second direction are one of vertical polarization and horizontal polarization, in paragraph 12. Claim 15 A method of using a magnetic / plasmon structure in an anti-counterfeiting device according to claim 12, further comprising synthesizing colloidal magnetic nanoparticles; modifying the magnetic nanoparticles in a solution of a polymeric ligand; bonding a metal seed nanoparticle to the surface of the magnetic nanoparticles; and forming a one-dimensional plasmon chain from the magnetic / plasmon structure by performing seed-mediated growth on the metal seed nanoparticles by reducing a metal salt in the solution to form a magnetic / plasmon hybrid structure. Claim 16 A magnetic / plasmon hybrid structure comprising: a magnetic nanoparticle core; a deformable and permeable polymer, wherein the polymer comprises a resorcinol-formaldehyde resin; and a metal seed attached to the magnetic nanoparticle core, wherein the metal seed is configured to have limited growth as a result of the deformable and permeable polymer on the magnetic core inhibiting the deposition of metal atoms and limiting the growth of metal atoms along the radial direction. Claim 17 In claim 16, a magnetic / plasmon hybrid structure in which the magnetic nanoparticle core contains iron oxide. Claim 18 In claim 17, a magnetic / plasmon hybrid structure in which iron oxide is Fe3O4. Claim 19 In paragraph 16, a magnetic / plasmon hybrid structure in which the metal seed comprises gold, silver, or copper. Claim 20 delete Claim 21 delete

Citation Information

Patent Citations

  • Composite nanoparticles and methods for making the same

    US20120168669A1

  • Iron oxide-gold core-shell nanoparticles and uses thereof

    US20150037818A1