An additive composition for modified asphalt, a method for preparing the same and a modified asphalt composition comprising the same
A copolymer of conjugated diene and aromatic vinyl monomers, coupled with a non-aromatic agent, addresses the viscosity issue in asphalt modifiers, enhancing temperature resistance and processability.
Patent Information
- Application Number
- KR1020230131546
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-10-04
AI Technical Summary
Existing asphalt modifiers, such as styrene block copolymers, improve temperature resistance but increase viscosity, making processing difficult, and there is a need for an additive that enhances temperature resistance while maintaining low viscosity for improved processability.
A copolymer composition comprising a block of conjugated diene and aromatic vinyl monomers, coupled with a non-aromatic coupling agent, is added to asphalt, allowing for improved temperature resistance and low viscosity, facilitating easier processing.
The additive composition improves asphalt's resistance to high and low temperatures, maintains low viscosity, and enhances processability, resulting in a modified asphalt with excellent stability and workability.
Abstract
Description
Technology Field
[0001] This specification relates to an additive composition for modified asphalt, a method for manufacturing the same, and a modified asphalt composition containing the same. Background Technology
[0002] Asphalt, used in applications such as road paving and the manufacture of waterproofing sheets, is significantly affected by temperature due to its inherent properties. It easily softens and deforms at high temperatures, while conversely, it cracks and is prone to damage at low temperatures. These issues frequently occur when asphalt is paved on roads. Over time, continuous exposure to high and low temperatures, along with constant impact from heavy objects such as passing vehicles, exacerbates the cracking and failure of the asphalt pavement.
[0003] As part of countermeasures for these problems, a method of adding asphalt modifiers to asphalt is known, and polymers such as polybutadiene, ethylene propylene rubber (EPDM, EPR), and styrene block copolymer (SBS, SIS) are used as asphalt modifiers. When asphalt modifiers are mixed into asphalt, the resistance of the asphalt to high and low temperatures is improved, thereby suppressing cracking and failure phenomena in asphalt pavements. Due to this effect, the use of modified asphalt with added modifiers in road pavements is increasing in industrial sites.
[0004] Meanwhile, styrene block copolymers used as asphalt modifiers can show improved effects as the input amount increases, but there is a problem in that increasing the input amount causes the viscosity of the asphalt to rise rapidly, making processing difficult. Therefore, there is a need to develop an additive for modified asphalt that can improve the resistance of asphalt at high and low temperatures, while simultaneously exhibiting low viscosity when mixed with asphalt so that a large amount can be input and the processability of the asphalt composition can be improved. The problem to be solved
[0005] The provisions of this specification are intended to solve the problems of the aforementioned prior art. One objective of this specification is to provide an additive composition for modified asphalt and a method for manufacturing the same, which improves the resistance of asphalt at high and low temperatures, exhibits low viscosity when mixed with asphalt so that a large amount can be added, and improves the processability of the asphalt composition.
[0006] Another objective of this specification is to provide a modified asphalt composition that has excellent high and low temperature characteristics and storage stability, while having excellent processability due to its low viscosity. means of solving the problem
[0007] According to one aspect, an additive composition for modified asphalt is provided, comprising a copolymer represented by the following chemical formula 1.
[0008] <Chemical Formula 1>
[0009] (AB) n -X
[0010] In the above chemical formula 1, A is a block composed of a conjugated diene monomer and an aromatic vinyl monomer, B is a block composed of a conjugated diene monomer, X is a coupling agent, and n is an integer from 2 to 4.
[0011] In one embodiment, the block composed of the conjugated diene monomer and the aromatic vinyl monomer may have a diblock, random, or tapered structure.
[0012] In one embodiment, based on the total weight of the conjugated diene monomer included in the copolymer, the content of the conjugated diene monomer included in the block composed of the conjugated diene monomer and the aromatic vinyl monomer may be 1 to 10 weight percent.
[0013] In one embodiment, the conjugated diene monomer may be one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more of these.
[0014] In one embodiment, the aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene, diphenylethylene including tertiary amines, primary, secondary, or It may be one selected from the group consisting of styrene containing a tertiary amine and combinations of two or more of these.
[0015] In one embodiment, the coupling agent may be one selected from the group consisting of dialkyl carbonate, dialkyl malonate, dialkyl phthalate, dialkyl succinate, dialkyl glutarate, dialkyl adipate, dialkyl pimella, dialkyl suberate, dialkyl sebacate, dialkyl azelate, dialkyl brasylate, dialkyl tetracandioate, dicarboxylate, tricarboxylate, diester compound, tryster compound, tetrachlorosilane, dichlorodimethylsilane, divinyl naphthalene, divinylbenzene, 2,5-divinylthiophene, trivinylbenzene, 1,4-divinyloxybenzene, methoxy-substituted divinylbenzene, diisopropenbenzene, 4-(4-(2-isopropenphenoxy)butyl)styrene, and combinations of two or more of these.
[0016] In one embodiment, the coupling agent may be a non-aromatic compound having two or more epoxy groups.
[0017] In one embodiment, the content of the aromatic vinyl monomer in the copolymer may be 10 to 60 weight percent.
[0018] In one embodiment, the vinyl content of the block composed of the conjugated diene monomer may be 10 to 80 mol%.
[0019] In one embodiment, the weight-average molecular weight (Mw) of the copolymer may be 20,000 to 1,000,000 g / mol.
[0020] According to another aspect, a method for preparing an additive composition for modified asphalt is provided, comprising: (a) polymerizing a conjugated diene monomer and an aromatic vinyl monomer simultaneously or sequentially in the presence of an initiator; (b) polymerizing the product of step (a) by introducing a conjugated diene monomer; and (c) reacting the product of step (b) by introducing a coupling agent.
[0021] In one embodiment, based on the total weight of the conjugated diene monomer polymerized in step (a) and step (b), the weight ratio of the conjugated diene monomer polymerized in step (a) may be 1 to 10 weight percent.
[0022] In one embodiment, the coupling efficiency of the additive composition for modified asphalt may be 15 to 96%.
[0023] According to another aspect, a modified asphalt composition is provided, comprising asphalt; and an additive composition for the modified asphalt.
[0024] In one embodiment, based on 100 parts by weight of the asphalt, the content of the additive composition for the modified asphalt may be 0.5 to 40 parts by weight. Effects of the invention
[0025] An additive composition for modified asphalt according to one aspect of the present specification can improve the resistance of asphalt at high and low temperatures, while exhibiting low viscosity when mixed with asphalt, allowing a large amount to be added, and can improve the processability of the modified asphalt composition.
[0026] In addition, a modified asphalt composition according to another aspect of the present specification can exhibit excellent high and low temperature characteristics and storage stability, while having low viscosity and excellent processability.
[0027] The effects of one aspect of this specification are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configurations described in the detailed description or claims of this specification. Specific details for implementing the invention
[0028] Hereinafter, one aspect of this specification will be described based on specific examples. However, the details described in this specification may be implemented in various different forms and are therefore not limited to the embodiments described herein.
[0029] Throughout the specification, when it is stated that a part is "connected" to another part, this includes not only cases where they are "directly connected," but also cases where they are "indirectly connected" with other members interposed between them. Furthermore, when it is stated that a part "includes" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.
[0030] When a range of numerical values is described in this specification, unless a specific range is otherwise described, the value has the precision of significant figures provided according to the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.
[0031] Additive composition for modified asphalt
[0032] An additive composition for modified asphalt according to one aspect of the present specification comprises a copolymer represented by the following chemical formula 1.
[0033] <Chemical Formula 1>
[0034] (AB) n -X
[0035] In the above chemical formula 1, A is a block composed of a conjugated diene monomer and an aromatic vinyl monomer, B is a block composed of a conjugated diene monomer, X is a coupling agent, and n is an integer from 2 to 4.
[0036] The above additive composition for modified asphalt includes a copolymer comprising a block composed of a conjugated diene monomer and an aromatic vinyl monomer, thereby exhibiting lower viscosity when mixed with asphalt compared to conventional additive compositions for modified asphalt, allowing a large amount to be added to the asphalt, and improving the processability of the asphalt composition to exhibit enhanced stability.
[0037] The block composed of the above conjugated diene monomer and aromatic vinyl monomer may have a diblock, random, or tapered structure, but is not limited thereto.
[0038] The above-mentioned diblock structure refers to a structure in which a block composed of a conjugated diene monomer and a block composed of an aromatic vinyl monomer are combined. When the block composed of the conjugated diene monomer and the aromatic vinyl monomer is a diblock structure, the above-mentioned Chemical Formula 1 is (block composed of conjugated diene monomer - block composed of aromatic vinyl monomer - B) n It may be a structure of -X, but is not limited to this.
[0039] The above random structure refers to a structure in which conjugated diene monomers and aromatic vinyl monomers are randomly distributed within the block.
[0040] The above tapered structure refers to a structure in which the proportion of a specific monomer gradually changes as it moves from one end of the block to the other.
[0041] Based on the total weight of the conjugated diene monomer included in the copolymer, the content of the conjugated diene monomer included in the block composed of the conjugated diene monomer and the aromatic vinyl monomer may be 1 to 10 wt%. For example, it may be 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, or a range between two of these values. If the content of the conjugated diene monomer included in the block composed of the conjugated diene monomer and the aromatic vinyl monomer exceeds the above range, the high and low temperature properties of the modified asphalt composition may be degraded.
[0042] The above conjugated diene monomer may be one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more of these, but is not limited thereto.
[0043] The above aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene, diphenylethylene including tertiary amines, primary, secondary, or tertiary amines It may be one selected from the group consisting of styrene containing and combinations of two or more of these, but is not limited thereto.
[0044] The above coupling agent is a dialkyl carbonate, dialkyl malonate, dialkyl phthalate, dialkyl succinate, dialkyl glutarate, dialkyl adipate, dialkyl pimella, dialkyl suberate, dialkyl sebacate, dialkyl azelate, dialkyl brasylate, dialkyl tetracandioate, dicarboxylate, tricarboxylate, diester compound, tryster compound, tetrachlorosilane, dichlorodimethylsilane, divinyl naphthalene (e.g., 1,4-divinyl naphthalene, 1,6-divinyl naphthalene, 1,8-divinyl naphthalene, 2,7-divinyl naphthalene), divinylbenzene (e.g., 1,2-divinylbenzene, 1,3-divinylbenzene, 1,4-divinylbenzene), 2,5-divinylthiophene (e.g., 3-hexyl-2,5-divinylthiophene, 3-methyl-2,5-divinylthiophene), trivinylbenzene (e.g., 1,2,3-trivinylbenzene, 1,2,4-trivinylbenzene, 1,3,5-trivinylbenzene), 1,4-divinyloxybenzene, methoxy-substituted divinylbenzene (e.g., 2-methoxy-1,4-divinylbenzene, 4-methoxy-1,2-divinylbenzene, 4-methoxy-1,3-divinylbenzene, 2-methoxy-1,3-divinylbenzene, 5-methoxy-1,3-divinylbenzene), diisopropenbenzene (e.g., 1,4-diisopropenbenzene, 1,2-diisopropenbenzene, 1,3-diisopropenbenzene), It may be one selected from the group consisting of 4-(4-(2-isopropenphenylphenoxy)butyl)styrene and combinations of two or more of these, but is not limited thereto, and may be a conventional 2- to 4-valent coupling agent.
[0045] The above coupling agent may be a non-aromatic compound having two or more epoxy groups. When the above non-aromatic compound having two or more epoxy groups is used as a coupling agent, the additive composition for modified asphalt may have a higher coupling number compared to a conventional additive composition for modified asphalt, or even if the coupling number is the same, may have a higher solubility in asphalt and exhibit a lower solution viscosity, thereby exhibiting excellent processability, workability, and storage stability.
[0046] The coupling agent may be a non-aromatic compound having two or more epoxy groups and one or more alkyl halide groups. That is, the coupling agent may be a non-aromatic compound having two or more epoxy groups and not including an alkyl halide group, or a non-aromatic compound having both two or more epoxy groups and one or more alkyl halide groups. For example, the second coupling agent may be a non-aromatic compound having two epoxy groups and not including an alkyl halide group, a non-aromatic compound having two epoxy groups and one alkyl halide group, or a non-aromatic compound having two epoxy groups and two alkyl halide groups, but is not limited thereto.
[0047] The above alkyl halide group may be one selected from the group consisting of alkyl chloride, alkyl fluoride, alkyl bromide, alkyl iodide, and combinations of two or more of these.
[0048] When a non-aromatic compound having two or more epoxy groups and one or more alkyl halides is used as a coupling agent, the additive composition for modified asphalt can exhibit a higher coupling number compared to the additive composition for modified asphalt prepared using a divalent coupling agent, and accordingly, exhibits low viscosity when mixed with asphalt, allowing a larger amount of the additive composition to be added to the asphalt compared to conventional methods.
[0049] The content of the aromatic vinyl monomer in the copolymer may be 10 to 60 wt%, preferably 15 to 40 wt%, but is not limited thereto. For example, it may be 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, or a range between two of these values. If the content of the aromatic vinyl monomer is less than the above range, the softening point of the modified asphalt composition may be lowered, and if it exceeds the above range, the low-temperature properties may be lowered.
[0050] The vinyl content of the block composed of the above conjugated diene monomer may be 10 to 80 mol%, preferably 50 to 70 mol%, but is not limited thereto. For example, it may be 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, or a range between two of these values. If the vinyl content of the block composed of the conjugated diene monomer satisfies the above range, it may exhibit excellent solubility with respect to asphalt. If the vinyl content is below the above range, the high-temperature properties of the modified asphalt composition may be degraded, and if it exceeds the above range, storage stability may be reduced or viscosity may increase.
[0051] The weight-average molecular weight (Mw) of the copolymer may be 20,000 to 1,000,000 g / mol, preferably 20,000 to 300,000 g / mol, and more preferably 20,000 to 150,000 g / mol, but is not limited thereto. For example, 20,000 g / mol, 40,000 g / mol, 60,000 g / mol, 80,000 g / mol, 100,000 g / mol, 110,000 g / mol, 120,000 g / mol, 130,000 g / mol, 140,000 g / mol, 150,000 g / mol, 160,000 g / mol, 170,000 g / mol, 180,000 g / mol, 190,000 g / mol, 200,000 g / mol, 300,000 g / mol, 400,000 g / mol, 500,000 g / mol, 600,000 g / mol, 700,000 g / mol, It may be 800,000 g / mol, 900,000 g / mol, 1,000,000 g / mol, or a range between two of these values. If the weight-average molecular weight of the copolymer is below the above range, high-temperature properties such as the softening point of the modified asphalt composition may be reduced, or the expression of mechanical application properties may not be easy, and if it exceeds the above range, storage stability may be reduced, or processability may be reduced due to increased viscosity.
[0052] In addition to the copolymer represented by Chemical Formula 1, the above additive composition for modified asphalt may further include a block copolymer in which only a block composed of a conjugated diene monomer and an aromatic vinyl monomer and a block composed of a conjugated diene monomer are combined, a copolymer in which the block copolymer is combined without a coupling agent, etc., but is not limited thereto.
[0053] Method for preparing an additive composition for modified asphalt
[0054] A method for preparing an additive composition for modified asphalt according to another aspect of the present specification comprises: (a) polymerizing a conjugated diene monomer and an aromatic vinyl monomer simultaneously or sequentially in the presence of an initiator; (b) polymerizing the product of step (a) by introducing a conjugated diene monomer; and (c) reacting the product of step (b) by introducing a coupling agent.
[0055] The type of monomer used in the above manufacturing method is the same as that described above.
[0056] Step (a) above is a step of polymerizing a conjugated diene monomer and an aromatic vinyl monomer simultaneously or sequentially in the presence of an initiator to form a block composed of the conjugated diene monomer and the aromatic vinyl monomer. In Step (a), the polymerization reaction of the conjugated diene monomer and the aromatic vinyl monomer is initiated to produce a living polymer.
[0057] The above initiator may use an organic lithium compound such as n-butyllithium, but is not limited thereto, and a conventional anionic initiator may be used.
[0058] The above step (a) may include the step of introducing a conjugated diene monomer and an aromatic vinyl monomer into a reactor simultaneously or sequentially.
[0059] The above step (a) may further include the step of introducing a polar modifier into the reactor. When the polar modifier is introduced, the vinyl content of the block composed of conjugated diene monomers can be controlled.
[0060] The above polar modifier may be one selected from the group consisting of ditetrahydrofurylpropane (DTHFP), tetramethylethylenediamine (TMEDA), tetrahydrofuran (THF), and combinations of two or more of these, but is not limited thereto.
[0061] Based on the total weight of the conjugated diene monomer polymerized in steps (a) and (b) above, the weight ratio of the conjugated diene monomer polymerized in step (a) above may be 1 to 10 wt%. For example, it may be 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, or a range between two of these values. If the weight ratio of the conjugated diene monomer polymerized in step (a) above exceeds the above range, the high and low temperature properties of the modified asphalt composition may be degraded.
[0062] Step (b) above is a step of polymerizing conjugated diene monomers to form a block composed of conjugated diene monomers. In step (b), the living polymer may react with the polymer of conjugated diene monomers to form a block copolymer represented by the following chemical formula 2.
[0063] <Chemical Formula 2>
[0064] AB
[0065] In the above chemical formula 2, A is a block composed of a conjugated diene monomer and an aromatic vinyl monomer, and B is a block composed of a conjugated diene monomer.
[0066] In step (a) above, when the conjugated diene monomer and the aromatic vinyl monomer are polymerized simultaneously, A of Formula 2 may have a random or tapered structure. The random structure refers to a structure in which the conjugated diene monomer and the aromatic vinyl monomer are randomly distributed within the block. The tapered structure refers to a structure in which the proportion of a specific monomer gradually changes from one end of the block to the other.
[0067] In step (a) above, when the conjugated diene monomer and the aromatic vinyl monomer are polymerized sequentially, A of Formula 2 may be a diblock structure in which a block composed of the conjugated diene monomer and a block composed of the aromatic vinyl monomer are combined.
[0068] The weight-average molecular weight (Mw) of the block copolymer represented by the above chemical formula 2 may be 5,000 to 500,000 g / mol. For example, 5,000 g / mol, 10,000 g / mol, 15,000 g / mol, 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, 35,000 g / mol, 40,000 g / mol, 45,000 g / mol, 50,000 g / mol, 55,000 g / mol, 60,000 g / mol, 65,000 g / mol, 70,000 g / mol, 75,000 g / mol, 80,000 g / mol, 85,000 g / mol, 90,000 g / mol, 95,000 g / mol, 100,000 g / mol, 150,000 g / mol, 200,000 It may be g / mol, 250,000 g / mol, 300,000 g / mol, 350,000 g / mol, 400,000 g / mol, 450,000 g / mol, 500,000 g / mol, or a range between two of these values. If the weight-average molecular weight of the block copolymer represented by Chemical Formula 2 is less than the above range, the high-temperature properties of the modified asphalt composition may be reduced, and if it exceeds the above range, the viscosity may increase, thereby reducing processability or storage stability.
[0069] In step (c) above, some of the block copolymer represented by Chemical Formula 2 may be coupled with the residue of the coupling agent.
[0070] The above coupling agent is a dialkyl carbonate, dialkyl malonate, dialkyl phthalate, dialkyl succinate, dialkyl glutarate, dialkyl adipate, dialkyl pimella, dialkyl suberate, dialkyl sebacate, dialkyl azelate, dialkyl brasylate, dialkyl tetracandioate, dicarboxylate, tricarboxylate, diester compound, tryster compound, tetrachlorosilane, dichlorodimethylsilane, divinyl naphthalene (e.g., 1,4-divinyl naphthalene, 1,6-divinyl naphthalene, 1,8-divinyl naphthalene, 2,7-divinyl naphthalene), divinylbenzene (e.g., 1,2-divinylbenzene, 1,3-divinylbenzene, 1,4-divinylbenzene), 2,5-divinylthiophene (e.g., 3-hexyl-2,5-divinylthiophene, 3-methyl-2,5-divinylthiophene), trivinylbenzene (e.g., 1,2,3-trivinylbenzene, 1,2,4-trivinylbenzene, 1,3,5-trivinylbenzene), 1,4-divinyloxybenzene, methoxy-substituted divinylbenzene (e.g., 2-methoxy-1,4-divinylbenzene, 4-methoxy-1,2-divinylbenzene, 4-methoxy-1,3-divinylbenzene, 2-methoxy-1,3-divinylbenzene, 5-methoxy-1,3-divinylbenzene), diisopropenbenzene (e.g., 1,4-diisopropenbenzene, 1,2-diisopropenbenzene, 1,3-diisopropenbenzene), It may be one selected from the group consisting of 4-(4-(2-isopropenphenylphenoxy)butyl)styrene and combinations of two or more of these, but is not limited thereto, and conventional 2- to 4-valent coupling agents may be used without limitation.
[0071] The above coupling agent may include a non-aromatic compound having two or more epoxy groups. When the above coupling agent includes a non-aromatic compound having two or more epoxy groups, the additive composition for modified asphalt prepared by the above method may exhibit a lower solution viscosity compared to a conventional additive composition for modified asphalt, with a higher number of couplings or, even if the number of couplings is the same, higher solubility in asphalt, and accordingly exhibit excellent processability, workability, and storage stability.
[0072] The coupling agent may include a non-aromatic compound having two or more epoxy groups and one or more alkyl halides. When the coupling agent includes a non-aromatic compound having two or more epoxy groups and one or more alkyl halides, the additive composition for modified asphalt prepared by the above method may exhibit a higher coupling number compared to conventional additive compositions for modified asphalt, and accordingly exhibit low viscosity when mixed with asphalt, allowing a larger amount of the additive composition to be added to the asphalt compared to conventional methods.
[0073] The coupling agent may be a mixture of a non-aromatic compound having two or more epoxy groups and not including an alkyl halide group, and a non-aromatic compound having both two or more epoxy groups and one or more alkyl halide groups. For example, the coupling agent may be a mixture comprising 40 to 60 weight% of a non-aromatic compound having two or more epoxy groups and not including an alkyl halide group, and 40 to 60 weight% of a non-aromatic compound having both two or more epoxy groups and one or more alkyl halide groups, but is not limited thereto.
[0074] The above coupling agent may be a non-aromatic compound having two epoxy groups and not containing an alkyl halide group, a non-aromatic compound having two epoxy groups and one alkyl halide group, and a mixture of a non-aromatic compound having two epoxy groups and two alkyl halide groups, but is not limited thereto.
[0075] The coupling agent may be a hydrogenated bisphenol A type epoxy resin. Compared to a bisphenol A type epoxy resin containing aromatic compounds, the hydrogenated bisphenol A type epoxy resin has less yellowing and excellent weather resistance, and can exhibit excellent workability due to its low viscosity and can reduce the viscosity of the modified asphalt composition.
[0076] The above coupling agent may be the reaction product of hydrogenated bisphenol A and epichlorohydrin (CAS No. 30583-72-3), but is not limited thereto.
[0077] The total weight-average molecular weight (Mw) of the additive composition for modified asphalt prepared by the above method may be 5,000 to 500,000 g / mol. For example, 5,000 g / mol, 10,000 g / mol, 15,000 g / mol, 20,000 g / mol, 25,000 g / mol, 30,000 g / mol, 35,000 g / mol, 40,000 g / mol, 45,000 g / mol, 50,000 g / mol, 55,000 g / mol, 60,000 g / mol, 65,000 g / mol, 70,000 g / mol, 75,000 g / mol, 80,000 g / mol, 85,000 g / mol, 90,000 g / mol, 95,000 g / mol, 100,000 g / mol, 150,000 g / mol, 200,000 It may be g / mol, 250,000 g / mol, 300,000 g / mol, 350,000 g / mol, 400,000 g / mol, 450,000 g / mol, 500,000 g / mol, or a range between two of these values. If the total weight-average molecular weight is below the above range, the high-temperature properties of the modified asphalt composition may be degraded, and if it exceeds the above range, the viscosity may increase, resulting in reduced processability, reduced storage stability, or a decrease in the amount of additives that can be added to the asphalt.
[0078] The coupling efficiency of the additive composition for modified asphalt prepared by the above method may be 15 to 96%, preferably 15 to 40%, but is not limited thereto. For example, it may be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, or a range between two of these values. If the coupling efficiency is below the above range, high-temperature characteristics such as the softening point of the modified asphalt composition may be reduced, and if it exceeds the above range, storage stability may be reduced or processability may be reduced due to increased viscosity.
[0079] Modified asphalt composition
[0080] A modified asphalt composition according to another aspect of the present specification comprises asphalt; and an additive composition for modified asphalt.
[0081] The additive composition for modified asphalt may include a copolymer represented by Chemical Formula 1. In another example, the additive composition for modified asphalt may be prepared by the above manufacturing method, but is not limited thereto.
[0082] Based on 100 parts by weight of the asphalt, the content of the additive composition for the modified asphalt may be 0.5 to 40 parts by weight. For example, it may be 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, or a range between two of these values. If the content of the additive composition for modified asphalt is below the above range, the concentration of the polymer is too low, making it difficult to exhibit performance as a modifier; if it exceeds the above range, the viscosity increases, which reduces the dispersibility between the asphalt and the additive composition for modified asphalt and the flowability of the modified asphalt composition, thereby delaying the dispersion time.
[0083] The above modified asphalt composition exhibits excellent high and low temperature characteristics and storage stability, while simultaneously demonstrating excellent processability due to its low viscosity. Due to these excellent characteristics, the above modified asphalt composition may not contain sulfur-based crosslinking agents, and accordingly, may exhibit environmentally friendly characteristics.
[0084] The above modified asphalt composition may be used for road paving, waterproofing sheets, or sealants, but is not limited thereto.
[0085] The embodiments of this specification will be described in more detail below. However, the following experimental results represent only representative results among the above embodiments, and the scope and content of this specification should not be interpreted as being narrowed or limited by the embodiments. The respective effects of various embodiments of this specification not explicitly presented below will be described in detail in the relevant sections.
[0086] Example 1
[0087] The interior of a 5L internal pressure reactor was sufficiently purged with nitrogen gas. 2.4 kg of purified cyclohexane, 400 ppm of polar modifier, and 128 g of styrene were injected into the reactor, and after maintaining the temperature at 50 ℃, 14 g of butadiene was injected. 0.20 phm of n-butyllithium, an initiator, was introduced into the reactor to initiate a polymerization reaction to form a tapered butadiene / styrene block. 10 minutes after the polymerization temperature reached its maximum temperature, 258 g of butadiene was added to proceed with polymerization. 5 minutes after the polymerization temperature reached its maximum temperature, 0.04 phm of dichlorodimethylsilane, a coupling agent, was added to proceed with coupling. After 15 minutes, caprylic acid, a polymerization terminator, was added to the polymerization solution to completely remove the activity of the living polymer. An antioxidant was added to the terminated polymerization solution, and cyclohexane was removed using a roll mill to prepare a copolymer.
[0088] Example 2
[0089] A copolymer was prepared in the same manner as in Example 1 above, except that 0.13 phm of KER-950 (Kumho P&B Chemical, CAS No. 30583-72-3) was added as a coupling agent.
[0090] Example 3
[0091] The interior of a 5L internal pressure reactor was sufficiently purged with nitrogen gas. 2.4 kg of purified cyclohexane, 400 ppm of a polar modifier, and 14 g of butadiene were injected into the reactor, and the temperature was maintained at 50 ℃. 0.20 phm of n-butyllithium, an initiator, was introduced into the reactor to initiate the polymerization reaction. 5 minutes after the polymerization temperature reached its maximum, 128 g of styrene was injected to form a diblock structure in which butadiene blocks and styrene blocks were combined. 5 minutes after the polymerization temperature reached its maximum, 258 g of butadiene was introduced to proceed with polymerization. 5 minutes after the polymerization temperature reached its maximum, 0.04 phm of dichlorodimethylsilane, a coupling agent, was introduced to proceed with coupling. After 15 minutes, caprylic acid, a polymerization terminator, was added to the polymerization solution to completely eliminate the activity of the living polymer. An antioxidant was added to the completed polymerization solution, and cyclohexane was removed using a roll mill to prepare a copolymer.
[0092] Example 4
[0093] A copolymer was prepared in the same manner as in Example 3 above, except that 0.13 phm of KER-950 (Kumho P&B Chemical, CAS No. 30583-72-3) was added as a coupling agent.
[0094] Comparative Example 1
[0095] The interior of a 5L internal pressure reactor was sufficiently purged with nitrogen gas. 2.4 kg of purified cyclohexane, 400 ppm of a polar modifier, and 132 g of styrene were injected into the reactor, and after maintaining the temperature at 50 ℃, 0.21 phm of n-butyllithium, an initiator, was introduced into the reactor to initiate the polymerization reaction. 10 minutes after the polymerization temperature reached its maximum, 268 g of butadiene was introduced to proceed with polymerization. 5 minutes after the polymerization temperature reached its maximum, 0.04 phm of dichlorodimethylsilane, a coupling agent, was introduced to proceed with coupling. After 15 minutes, caprylic acid, a polymerization terminator, was added to the polymerization solution to completely eliminate the activity of the living polymer. An antioxidant was added to the terminated polymerization solution, and the cyclohexane was removed using a roll mill to produce a copolymer.
[0096] Experimental Example 1
[0097] The molecular weight, coupling efficiency, and composition of each copolymer prepared in Examples 1 to 4 and Comparative Example 1 were analyzed in the following manner, and the results are shown in Table 1 below.
[0098] 1) Molecular weight analysis
[0099] The weight-average molecular weight prior to coupling using a coupling agent (Mw before coupling), the weight-average molecular weight of the coupled structure formed after coupling (Mw after coupling), and the weight-average molecular weight of the total product (total Mw) were measured, respectively.
[0100] The weight-average molecular weight of each sample was analyzed using high-performance liquid chromatography (separation's module Waters 2690). The analysis was performed under conditions of a column temperature of 40°C, THF solvent, and a flow rate of 1.0 mL / min. Divinylbenzene Styragel HR 5E, HR 4, and HR 2 columns were connected in series, and the difference in refractive index was detected by a refractive index detector relative to a polystyrene standard sample.
[0101] 2) Coupling efficiency analysis
[0102] The coupling efficiency was analyzed according to Equation 1 below using the area of the polymer peaks observed in GPC (gel permeation chromatography).
[0103] <Equation 1>
[0104] Coupling efficiency (%) = {(Area of coupled polymer) / (Total area of polymer)} × 100
[0105] 3) Composition Analysis
[0106] The styrene content in the copolymer and the vinyl content of the butadiene block were analyzed.
[0107] Styrene and vinyl content analysis was performed using a nuclear magnetic resonance analyzer (Bruker NMR-400), and the samples were analyzed using chloroform-d as a solvent.
[0108] division Mw (g / mol) before coupling Mw (g / mol) after coupling Total Mw(g / mol) Coupling efficiency (%) Styrene content (weight%) Vinyl content (mol%) Example 1 50,400 111,900 64,600 23.1 33.3 61.2 Example 2 49,200 118,000 65,400 23.6 34.2 62.4 Example 3 52,600 115,700 67,600 23.3 33.1 61.0 Example 4 52,000 119,500 69,800 24.7 33.5 60.7 Comparative Example 1 54,300 119,400 68,900 23.9 32.1 63.5
[0109] Preparation Example
[0110] A modified asphalt composition was prepared by mixing the copolymer prepared in the above examples and comparative examples and molten pure asphalt with a high-speed shear mixer at 180°C for 2 hours. The composition ratio of the modified asphalt composition is shown in Table 2 below.
[0111] division Pure asphalt copolymer Content (parts by weight) type Content (parts by weight) Preparation Example 1 100 Example 1 7.5 Preparation Example 2 100 Example 2 7.5 Preparation Example 3 100 Example 3 7.5 Preparation Example 4 100 Example 4 7.5 Comparative Manufacturing Example 1 100 Comparative Example 1 7.5
[0112] Experimental Example 2
[0113] The physical properties of each modified asphalt composition prepared in Manufacturing Examples 1 to 4 and Comparative Manufacturing Example 1 were measured in the following manner, and the results are shown in Table 3 below.
[0114] 1) Softening point: Measured according to ASTM D36.
[0115] 2) Fraass breaking point: Measured according to EN 12593.
[0116] 3) Difference in softening point between phases: To evaluate storage stability, the difference in softening point between the top and bottom of the separated composition was measured according to ASTM D7173.
[0117] 4) Rotational viscosity @135 ℃: Measured according to ASTM D4402.
[0118] division Softening point (°C) Plasma embrittlement point (°C) Difference in softening point between phases (°C) Rotational viscosity (cps) Preparation Example 1 75.8 -19.6 4.8 2200 Preparation Example 2 77.6 -19.4 2.4 2100 Preparation Example 3 77.9 -17.5 14.5 2350 Preparation Example 4 79.8 -17.7 12.5 2275 Comparative Manufacturing Example 1 82.2 -19.1 23.3 2725
[0119] Referring to Table 3 above, it was confirmed that the modified asphalt compositions of Preparation Examples 1 and 2 have a slightly lower softening point compared to the modified asphalt composition of Comparative Preparation Example 1, but have a lower plastic embrittlement point, resulting in excellent low-temperature characteristics, and have excellent storage stability and low viscosity due to a very small difference in phase separation softening point compared to the modified asphalt composition of Comparative Preparation Example 1.
[0120] It was confirmed that the modified asphalt compositions of Manufacturing Examples 3 and 4 had a slightly lower softening point and a slightly higher plastic embrittlement point compared to the modified asphalt composition of Comparative Manufacturing Example 1, but had excellent storage stability and low viscosity due to the small difference in phase separation softening point compared to the modified asphalt composition of Comparative Manufacturing Example 1.
[0121] The foregoing description of this specification is for illustrative purposes only, and those skilled in the art to which one aspect of this specification pertains will understand that other specific forms can be easily modified without altering the technical concept or essential features described in this specification. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0122] The scope of this specification is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of this specification.
Claims
Claim 1 Additive composition for modified asphalt comprising a copolymer represented by the following chemical formula 1, having a coupling efficiency of 40% or less: <Chemical Formula 1> (AB) n - In the above chemical formula 1, A is a block composed of a conjugated diene monomer and an aromatic vinyl monomer, B is a block composed of a conjugated diene monomer, X is a coupling agent, n is an integer from 2 to 4, and the coupling agent is a hydrogenated bisphenol A type epoxy resin having two or more epoxy groups. Claim 2 An additive composition for modified asphalt according to claim 1, wherein the block composed of the conjugated diene monomer and the aromatic vinyl monomer has a diblock, random, or tapered structure. Claim 3 An additive composition for modified asphalt according to claim 1, wherein, based on the total weight of the conjugated diene monomers included in the copolymer, the content of the conjugated diene monomer included in the block composed of the conjugated diene monomer and the aromatic vinyl monomer is 1 to 10 weight percent. Claim 4 The additive composition for modified asphalt according to claim 1, wherein the conjugated diene monomer is one selected from the group consisting of 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, 2-chloro-1,3-butadiene, 3-butyl-1,3-octadiene, octadiene, and combinations of two or more of these. Claim 5 In claim 1, the aromatic vinyl monomer is styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-(p-methylphenyl)styrene, 5-tert-butyl-2-methylstyrene, tert-butoxystyrene, 2-tert-butylstyrene, 3-tert-butylstyrene, 4-tert-butylstyrene, N,N-dimethylaminoethylstyrene, 1-vinyl-5-hexylnaphthalene, 1-vinylnaphthalene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, vinylpyridine, vinylxylene, diphenylethylene, diphenylethylene including tertiary amines, primary, secondary, or An additive composition for modified asphalt, comprising styrene containing a tertiary amine and one selected from the group consisting of a combination of two or more of these. Claim 6 delete Claim 7 delete Claim 8 An additive composition for modified asphalt according to claim 1, wherein the content of the aromatic vinyl monomer in the copolymer is 10 to 60 weight%. Claim 9 An additive composition for modified asphalt according to claim 1, wherein the vinyl content of the block composed of the conjugated diene monomer is 10 to 80 mol%. Claim 10 An additive composition for modified asphalt according to claim 1, wherein the weight-average molecular weight (Mw) of the copolymer is 20,000 to 1,000,000 g / mol. Claim 11 A method for preparing an additive composition for modified asphalt, comprising: (a) a step of polymerizing a conjugated diene monomer and an aromatic vinyl monomer simultaneously or sequentially in the presence of an initiator; (b) a step of polymerizing the product of step (a) by introducing a conjugated diene monomer; and (c) a step of reacting the product of step (b) by introducing a coupling agent, wherein the coupling agent is a hydrogenated bisphenol A type epoxy resin having two or more epoxy groups, wherein the coupling efficiency is 40% or less. Claim 12 A method for preparing an additive composition for modified asphalt according to claim 11, wherein, based on the total weight of the conjugated diene monomer polymerized in step (a) and step (b), the weight ratio of the conjugated diene monomer polymerized in step (a) is 1 to 10 weight percent. Claim 13 delete Claim 14 A modified asphalt composition comprising asphalt; and the additive composition for modified asphalt of claim 1. Claim 15 A modified asphalt composition according to claim 14, wherein, based on 100 parts by weight of the asphalt, the content of the additive composition for the modified asphalt is 0.5 to 40 parts by weight.
Citation Information
Patent Citations
Asphalt modifier and asphalt composition comprising the same
KR1020160052310A
Block copolymer composition, method for preparing the same and asphalt composition comprising the same
KR1020210036149A