Environment-friendly polyamide resin composition and article comprising the same
The eco-friendly polyamide resin composition, combining recycled materials with specific additives, addresses adhesion and mechanical property issues, enhancing adhesion and impact resistance while reducing energy consumption in recycling.
Patent Information
- Application Number
- KR1020230114794
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-30
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2043-08-30
AI Technical Summary
Existing polyamide resins face challenges in adhesion to polyurethane adhesives, mechanical property deterioration due to resin aging, and high energy consumption in recycling processes, necessitating an eco-friendly composition with improved adhesion, disassembly properties, impact resistance, and heat resistance.
A polyamide resin composition comprising recycled polyamide resin, aliphatic and aromatic polyamide resins, glass fiber, polyetheresteramide block copolymer, and talc, optimized in specific ratios to enhance adhesion, impact resistance, and heat resistance.
The composition achieves excellent adhesion and disassembly properties with polyurethane adhesives, along with improved impact resistance and heat resistance, while reducing energy consumption in recycling processes.
Smart Images

Figure 112023095885745-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an eco-friendly polyamide resin composition and a molded article comprising the same. More specifically, the present invention relates to an eco-friendly polyamide resin composition having excellent eco-friendliness, adhesion and disassembly properties with polyurethane adhesives, impact resistance, heat resistance, rigidity, etc., and a molded article comprising the same. Background Technology
[0003] Polyamide resins possess excellent processability and impact resistance, making them useful for housings of various products or interior and exterior automotive materials. Furthermore, when mixed with inorganic fillers such as glass fibers, polyamide resins can further enhance mechanical properties such as rigidity and heat resistance; in line with the trends toward thin-film and lightweight materials, their application in electronic product housings is increasing.
[0004] Meanwhile, in the assembly process of components for electrical / electronic products and automobiles, the bonding process is carried out using adhesive tapes or adhesives. Polyurethane reactive (PUR) type adhesives are advantageous for increasing productivity due to the simpler process compared to adhesive tapes, and they also offer excellent adhesion. In particular, they are highly efficient when the bonding area is small.
[0005] However, the use of polyurethane adhesives is limited because their adhesion to polyamide resins is very poor.
[0006] Furthermore, driven by environmental issues such as the gradually increasing plastic waste and carbon reduction, interest in the market for eco-friendly products that recycle plastic waste is on the rise. Consequently, many companies are developing technological processes to convert waste plastics back into raw materials through methods like pyrolysis; however, due to the thermal energy consumed during this process, a significant amount of energy is currently being invested in the recycling systems. Therefore, there is a demand for a method that minimizes such energy loss and maximizes waste reuse by crushing the waste and utilizing it as a raw material for resin processing.
[0007] However, in the case of resins that are typically waste products, there is a problem in that mechanical properties and heat resistance deteriorate due to resin aging.
[0008] Therefore, there is a need to develop an eco-friendly polyamide resin composition by recycling plastic waste that is environmentally friendly and possesses excellent adhesion to polyurethane adhesives, disassembly properties, impact resistance, heat resistance, and rigidity.
[0009] The background technology of the present invention is disclosed in U.S. Patent Publication No. US 2014 / 0179850, etc. The problem to be solved
[0011] The objective of the present invention is to provide an eco-friendly polyamide resin composition having excellent eco-friendliness, adhesion and disassembly properties with polyurethane adhesives, impact resistance, heat resistance, and rigidity.
[0012] Another objective of the present invention is to provide a molded article formed from the above-mentioned eco-friendly polyamide resin composition.
[0013] The above and other objectives of the present invention can all be achieved by the present invention described below. means of solving the problem
[0015] 1. One aspect of the present invention relates to an eco-friendly polyamide resin composition. The eco-friendly polyamide resin composition comprises 100 parts by weight of a base material comprising 5 to 25 parts by weight of recycled polyamide resin, 1 to 30 parts by weight of an aliphatic polyamide resin excluding polyamide 6 and polyamide 6.6, 1 to 20 parts by weight of an aromatic polyamide resin, and 40 to 80 parts by weight of glass fiber; 5 to 15 parts by weight of a polyetheresteramide block copolymer; and 0.1 to 1 part by weight of talc; wherein the polyetheresteramide block copolymer is a block copolymer of a reaction mixture comprising an aminocarboxylic acid having 6 or more carbon atoms, a lactam or a diamine-dicarboxylate, polytetramethylene glycol, and a dicarboxylic acid having 4 to 20 carbon atoms.
[0016] 2. In the above 1 embodiment, the recycled polyamide resin may include one or more of marine waste-derived polyamide 6 and marine waste-derived polyamide 6.6.
[0017] 3. In the above 1 or 2 embodiments, the aliphatic polyamide resin may include one or more of polyamide 11, polyamide 12, polyamide 4.6, polyamide 6.10, polyamide 6.12, polyamide 10.10, and polyamide 10.12.
[0018] 4. In the above 1 to 3 embodiments, the aromatic polyamide resin may be a polymer of an aliphatic dicarboxylic acid and an aromatic diamine.
[0019] 5. In the above 1 to 4 embodiments, the glass fiber may have a rectangular or elliptical cross-section, the aspect ratio of the cross-section (major axis of the cross-section / minor axis of the cross-section) may be 1.5 to 10, and the minor axis may be 2 to 10 μm.
[0020] 6. In the above 1 to 5 embodiments, the weight ratio of the glass fiber and the polyetheresteramide block copolymer may be 1:0.05 to 1:0.3.
[0021] 7. In the above 1 to 6 embodiments, the weight ratio of the polyetheresteramide block copolymer and the talc may be 1:0.005 to 1:0.08.
[0022] 8. In the above 1 to 7 embodiments, the eco-friendly polyamide resin composition may be such that 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) is applied to a thickness of 1 mm at 110°C on a specimen of size 50 mm × 50 mm × 4 mm, a glass of size 25 mm × 25 mm × 0.7 mm is attached to the applied adhesive, and after curing for 72 hours under conditions of 25°C temperature and 50% humidity, a weight of 10 to 500 g is attached to the top of a drop weight evaluation device and the specimen is fixed to the bottom, and then the specimen is dropped from a height of 50 cm to measure the adhesive strength (potential energy) when the specimen detaches from the glass, which may be 700 to 990 mJ.
[0023] 9. In the above 1 to 8 embodiments, the eco-friendly polyamide resin composition may be formed by applying 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) to a thickness of 1 mm at 110°C onto a specimen of size 50 mm × 50 mm × 4 mm, attaching a glass of size 25 mm × 25 mm × 0.7 mm onto the applied adhesive, curing it for 72 hours under conditions of 25°C temperature and 50% humidity, heating it at 75°C for 15 minutes, and then using a Universal Testing Machine (UTM), fixing the specimen with the glass attached to the bottom of the machine and fixing a weight of 5 mm in diameter to the top jig, and dropping the weight at a speed of 20 mm / min so that when the glass and the specimen are detached, no adhesive remains on the specimen.
[0024] 10. In the above 1 to 9 embodiments, the eco-friendly polyamide resin composition may have a notched Izod impact strength of 12 to 30 kgf·cm / cm of a 1 / 8" thick specimen measured according to ASTM D256.
[0025] 11. In the above 1 to 10 embodiments, the eco-friendly polyamide resin composition may have a heat distortion temperature (HDT) of 175 to 195°C measured under conditions of a load of 1.82 MPa and a heating rate of 120°C / hr in accordance with ASTM D648.
[0026] 12. In the above embodiments 1 to 11, the eco-friendly polyamide resin composition has a flexural modulus of 90,000 to 180,000 kgf / cm² of a 6.4 mm thick specimen measured at a speed of 2.8 mm / min in accordance with ASTM D790. 2 It can be:
[0027] 13. Another aspect of the present invention relates to a molded article. The molded article is formed from an eco-friendly polyamide resin composition according to any one of 1 to 12.
[0028] 14. Another aspect of the present invention relates to an electronic device housing. The electronic device housing comprises a glass frame; and a plastic member in contact with at least one surface of the glass frame; wherein the plastic member is formed from an eco-friendly polyamide resin composition according to any one of 1 to 12. Effects of the invention
[0030] The present invention has the effect of providing an eco-friendly polyamide resin composition and a molded article formed therefrom, which have excellent eco-friendliness, adhesion and disassembly properties with polyurethane adhesives, impact resistance, heat resistance, and rigidity. Brief explanation of the drawing
[0032] FIG. 1 schematically illustrates a cross-section of an electronic device housing according to one embodiment of the present invention. Specific details for implementing the invention
[0033] The present invention will be described in detail below.
[0034] The eco-friendly polyamide resin composition according to the present invention comprises (A) recycled polyamide resin; (B) aliphatic polyamide resin; (C) aromatic polyamide resin; (D) glass fiber; (E) polyetheresteramide block copolymer; and (F) talc.
[0035] In this specification, "a to b" indicating a numerical range is defined as "≥a and ≤b".
[0037] (A) Recycled polyamide resin
[0038] A recycled polyamide resin according to one embodiment of the present invention is applied together with an aliphatic polyamide resin, an aromatic polyamide resin, glass fiber, a polyetheresteramide block copolymer, and talc, etc., thereby imparting eco-friendliness to the polyamide resin composition and improving adhesion and disassembly properties with polyurethane adhesives, impact resistance, heat resistance, rigidity, etc.
[0039] In a specific example, the recycled polyamide resin may include polyamide 6 derived from marine waste (waste polyamide), polyamide 6.6 derived from marine waste, combinations thereof, etc.
[0040] In a specific example, the recycled polyamide resin may have a weight-average molecular weight (Mw) measured by gel permeation chromatography (GPC) of 10,000 to 100,000 g / mol, for example, 20,000 to 40,000 g / mol.
[0041] In a specific example, the recycled polyamide resin may be included in an amount of 5 to 25 weight%, for example, 10 to 20 weight%, of the total 100 weight% of the base material including the recycled polyamide resin, the aliphatic polyamide resin, the aromatic polyamide resin, and the glass fiber. If the content of the recycled polyamide resin is less than 5 weight% of the total 100 weight% of the base material, there is a risk that the eco-friendliness of the eco-friendly polyamide resin composition may be reduced, and if it exceeds 25 weight%, there is a risk that the disassembly properties and impact resistance of the eco-friendly polyamide resin composition with the polyurethane adhesive may be reduced.
[0043] (B) Aliphatic polyamide resin
[0044] The aliphatic polyamide resin according to one embodiment of the present invention can be applied together with the recycled polyamide resin, aromatic polyamide resin, glass fiber, polyetheresteramide block copolymer, and talc, etc., to improve the eco-friendliness of the polyamide resin composition, adhesion and disassembly properties with polyurethane adhesive, impact resistance, heat resistance, rigidity, etc., and can use conventional aliphatic polyamide resins excluding polyamide 6 and polyamide 6.6.
[0045] In a specific example, the aliphatic polyamide resin may include polyamide 11, polyamide 12, polyamide 4.6, polyamide 6.10, polyamide 6.12, polyamide 10.10, polyamide 10.12, combinations thereof, etc. For example, polyamide 10.12, etc. may be used.
[0046] In a specific example, the aliphatic polyamide resin is dissolved in a concentrated sulfuric acid solution (96%) at a concentration of 0.5 g / dL, and the relative viscosity [η] measured at 25°C using a Ubbelohde viscometer rel ] may be 2 to 3, for example, 2.3 to 2.8. Within the above range, the processability, impact resistance, etc. of the eco-friendly polyamide resin composition may be excellent.
[0047] In a specific example, the aliphatic polyamide resin may be included in an amount of 1 to 30 weight%, for example, 10 to 25 weight%, of 100 weight% of the base material (recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, and glass fiber). If the content of the aliphatic polyamide resin is less than 1 weight% of the 100 weight% of the base material, there is a risk that the impact resistance, etc., of the eco-friendly polyamide resin composition may be reduced, and if it exceeds 30 weight%, there is a risk that the disassembly properties, heat resistance, rigidity, and eco-friendliness of the eco-friendly polyamide resin composition with the polyurethane adhesive may be reduced.
[0048] In a specific example, the weight ratio of the recycled polyamide resin and the aliphatic polyamide resin may be 1:0.1 to 1:4, for example, 1:0.2 to 1:3, specifically 1:0.2 to 1:2.6. Within this range, the eco-friendliness of the eco-friendly polyamide resin composition, its disassembly properties with polyurethane adhesive, impact resistance, heat resistance, rigidity, etc., may be superior.
[0050] (C) Aromatic polyamide resin
[0051] An aromatic polyamide resin according to one embodiment of the present invention can be applied together with the recycled polyamide resin, aliphatic polyamide resin, glass fiber, polyetheresteramide block copolymer, and talc, etc., to improve the eco-friendliness of the polyamide resin composition, adhesion and disassembly properties with polyurethane adhesive, impact resistance, heat resistance, rigidity, etc., and an aromatic polyamide resin used in conventional polyamide resin compositions can be used.
[0052] In a specific example, the aromatic polyamide resin may be a polymer of an aliphatic dicarboxylic acid and an aromatic diamine prepared by reacting according to a known polymerization method.
[0053] In this specification, the term "dicarboxylic acid, etc." is used to include dicarboxylic acids, their alkyl esters (lower alkyl esters having 1 to 4 carbon atoms, such as monomethyl, monoethyl, dimethyl, diethyl, or dibutyl esters), and their acid anhydrides, etc., and reacts with diamines, etc., to form repeating units (dicarboxylic acid moiety) derived from dicarboxylic acids. In addition, in this specification, repeating units derived from dicarboxylic acids and repeating units derived from diamines (diamine moiety) refer to the residue remaining after hydrogen atoms (removed from the amine group), hydroxyl groups, or alkoxy groups (removed from the carboxylic acid group) are removed when dicarboxylic acids and diamines undergo a polymerization reaction.
[0054] In a specific example, the aliphatic dicarboxylic acid may be a linear, branched, or cyclic aliphatic dicarboxylic acid having 6 to 20 carbon atoms, such as adipic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, etc. Specifically, adipic acid, sebacic acid, etc. may be used.
[0055] In a specific example, one or more aromatic diamines having 6 to 30 carbon atoms may be used as the aromatic diamine. For example, phenylenediamine compounds such as m-phenylenediamine and p-phenylenediamine, xylenediamine compounds such as m-xylenediamine and p-xylenediamine, and naphthalenediamine compounds may be used.
[0056] In a specific example, the aromatic polyamide resin may have a molar ratio (diamine / dicarboxylic acid) of repeating units derived from the dicarboxylic acid and repeating units derived from the diamine of 0.95 to 1.15, for example, 1.00 to 1.10. Within this range, it is possible to manufacture a polyamide resin with a degree of polymerization suitable for molding, and to prevent a decrease in physical properties caused by unreacted monomers.
[0057] In a specific example, the aromatic polyamide resin may have a glass transition temperature of 30 to 100°C, for example, 40 to 80°C, as measured by differential scanning calorimetry (DSC). Within this range, the heat resistance, rigidity, impact resistance, etc. of the eco-friendly polyamide resin composition may be excellent.
[0058] In addition, the above aromatic polyamide resin may have an intrinsic viscosity [η] of 0.7 to 1.2 dL / g, for example, 0.8 to 1.0 dL / g, measured by a Ubbelohde viscometer at 25°C after being dissolved in a concentrated sulfuric acid solution (98%) at a concentration of 0.5 g / dL. Within this range, the heat resistance, rigidity, impact resistance, etc. of the eco-friendly polyamide resin composition may be excellent.
[0059] In a specific example, the aromatic polyamide resin may be included in an amount of 1 to 20 weight%, for example, 5 to 15 weight%, of 100 weight% of the base material (recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, and glass fiber). If the content of the aromatic polyamide resin is less than 1 weight% of the 100 weight% of the base material, there is a risk that the disassembly properties, heat resistance, and rigidity of the eco-friendly polyamide resin composition with respect to the polyurethane adhesive will be reduced, and if it exceeds 20 weight%, there is a risk that the impact resistance of the eco-friendly polyamide resin composition will be reduced.
[0061] (D) Glass fiber
[0062] Glass fibers according to one embodiment of the present invention can be applied together with the recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, polyetheresteramide block copolymer, and talc, etc., to improve the eco-friendliness of the polyamide resin composition, adhesion and disassembly properties with polyurethane adhesive, impact resistance, heat resistance, rigidity, etc., and glass fibers used in conventional thermoplastic resin compositions can be used.
[0063] In a specific example, the glass fiber may have a cross-section of various shapes, such as circular, elliptical, or rectangular.
[0064] In a specific example, the glass fiber may be a flat glass fiber having a rectangular or elliptical cross-section. The aspect ratio of the cross-section (major axis of the cross-section / minor axis of the cross-section) of the flat glass fiber, measured using a Scanning Electron Microscope (SEM), may be 1.5 to 10, for example, 2 to 8; the minor axis of the cross-section may be 2 to 10 μm, for example, 4 to 8 μm; and the length before processing may be 1 to 15 mm, for example, 2 to 8 mm. Within the above range, the rigidity, processability, etc. of the eco-friendly polyamide resin composition may be improved.
[0065] In a specific example, the glass fiber may be treated with a conventional surface treatment agent.
[0066] In a specific example, the glass fiber may be included in an amount of 40 to 80 weight%, for example, 50 to 70 weight%, of 100 weight% of the base material (recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin and glass fiber). If the content of the glass fiber is less than 40 weight% of 100 weight% of the base material, there is a risk that the adhesion of the eco-friendly polyamide resin composition to the polyurethane adhesive, etc., will be reduced, and if it exceeds 80 weight%, there is a risk that the disintegration of the eco-friendly polyamide resin composition to the polyurethane adhesive, etc., will be reduced.
[0068] (E) Polyetheresteramide block copolymer
[0069] A polyetheresteramide block copolymer according to one embodiment of the present invention can be applied together with the recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, glass fiber, and talc, etc., to improve the eco-friendliness of the polyamide resin composition, adhesion and disassembly properties with polyurethane adhesive, impact resistance, heat resistance, rigidity, etc., and a block copolymer of a reaction mixture comprising an aminocarboxylic acid having 6 or more carbon atoms, a lactam, or a diamine-dicarboxylate; polytetramethylene glycol; and a dicarboxylic acid having 4 to 20 carbon atoms may be used.
[0070] In a specific example, the salt of the aminocarboxylic acid, lactam, or diamine-dicarboxylic acid having 6 or more carbon atoms may be exemplified as aminocarboxylic acids such as ω-aminocaproic acid, ω-aminoenanthic acid, ω-aminocaprilic acid, ω-aminofelconic acid, ω-aminocapric acid, 1,1-aminoundecanoic acid, 1,2-aminododecanoic acid; lactams such as caprolactam, enanthlactam, caprylactam, lauryllactam; and salts of diamines and dicarboxylic acids such as salts of hexamethylenediamine-adipic acid and hexamethylenediamine-isophthalic acid. For example, 1,2-aminododecanoic acid, caprolactam, and hexamethylenediamine-adipic acid may be used.
[0071] In a specific example, the dicarboxylic acid having 4 to 20 carbon atoms may be exemplified as terephthalic acid, 1,4-cyclohexacarboxylic acid, sebacic acid, adipic acid, dodecanocarboxylic acid, etc.
[0072] In a specific example, the bond between the aminocarboxylic acid, lactam, or diamine-dicarboxylic acid salt having 6 or more carbon atoms and the polytetramethylene glycol may be an ester bond, the bond between the aminocarboxylic acid, lactam, or diamine-dicarboxylic acid salt having 6 or more carbon atoms and the dicarboxylic acid having 4 to 20 carbon atoms may be an amide bond, and the bond between the polytetramethylene glycol and the dicarboxylic acid having 4 to 20 carbon atoms may be an ester bond.
[0073] In a specific example, the polyetheresteramide block copolymer may be prepared by a known synthesis method, for example, according to the synthesis method disclosed in Japanese Patent Publication No. 56-045419 and Japanese Patent Publication No. 55-133424.
[0074] In a specific example, the polyetheresteramide block copolymer may contain 10 to 95 weight percent of a polyether-ester block. Within this range, the impact resistance and other properties of the eco-friendly polyamide resin composition may be excellent.
[0075] In a specific example, the polyetheresteramide block copolymer may be included in an amount of 5 to 15 parts by weight, for example, 6 to 12 parts by weight, per 100 parts by weight of the base material (recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, and glass fiber). If the content of the polyetheresteramide block copolymer is less than 5 parts by weight per 100 parts by weight of the base material, there is a risk that the adhesion and impact resistance of the eco-friendly polyamide resin composition with the polyurethane adhesive will be reduced, and if it exceeds 15 parts by weight, there is a risk that the disintegration resistance, heat resistance, and rigidity of the eco-friendly polyamide resin composition with the polyurethane adhesive will be reduced.
[0076] In a specific example, the weight ratio (D:E) of the glass fiber and the polyetheresteramide block copolymer may be 1:0.05 to 1:0.3, for example, 1:0.1 to 1:0.2. Within this range, the adhesion and disassembly properties, impact resistance, heat resistance, rigidity, etc., of the eco-friendly polyamide resin composition with the polyurethane adhesive may be superior.
[0078] (F) Talc
[0079] Talc according to one embodiment of the present invention is applied together with the recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, glass fiber, and polyetheresteramide block copolymer, etc., to improve the eco-friendliness of the polyamide resin composition, adhesion and disassembly properties with polyurethane adhesive, impact resistance, heat resistance, rigidity, etc., and can use talc used in conventional thermoplastic resin compositions.
[0080] In a specific example, the talc is a plate-shaped inorganic filler, and the average particle size measured by a particle size measuring device (Malvern mastersizer 300) may be 0.5 to 10 μm, for example, 1 to 7 μm. Within this range, the adhesion and disassembly properties, heat resistance, etc., of the eco-friendly polyamide resin composition with the polyurethane adhesive may be excellent.
[0081] In a specific example, the talc may be included in an amount of 0.1 to 1 part by weight, for example, 0.15 to 0.5 parts by weight, per 100 parts by weight of the base material (recycled polyamide resin, aliphatic polyamide resin, aromatic polyamide resin, and glass fiber). If the content of the talc is less than 0.1 parts by weight per 100 parts by weight of the base material, there is a risk that the bonding properties of the eco-friendly polyamide resin composition with the polyurethane adhesive will be reduced, and if it exceeds 1 part by weight, there is a risk that the impact resistance properties of the eco-friendly polyamide resin composition will be reduced.
[0082] In a specific example, the weight ratio (D:E) of the polyetheresteramide block copolymer and the talc may be 1:0.005 to 1:0.08, for example, 1:0.01 to 1:0.07. Within this range, the adhesion and disassembly properties, impact resistance, heat resistance, rigidity, etc., of the eco-friendly polyamide resin composition with respect to the polyurethane adhesive may be superior.
[0084] An eco-friendly polyamide resin composition according to one embodiment of the present invention may further include conventional additives as needed, within a range that does not impede the effects of the present invention. Such additives include, but are not limited to, heat stabilizers, flame retardants, antioxidants, lubricants, release agents, nucleating agents, colorants, and mixtures thereof. When using such additives, the content thereof may be 0.001 to 40 parts by weight, for example, 0.1 to 20 parts by weight, per 100 parts by weight of the base material.
[0086] An eco-friendly polyamide resin composition according to one embodiment of the present invention may be in the form of pellets produced by mixing the above components and melt-extruding them using a conventional twin-screw extruder at 240 to 320°C, for example, 250 to 310°C.
[0087] In a specific example, the above-described eco-friendly polyamide resin composition may be applied to a specimen of size 50 mm × 50 mm × 4 mm with a thickness of 1 mm using 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) at 110°C, a glass of size 25 mm × 25 mm × 0.7 mm attached to the applied adhesive, and cured for 72 hours under conditions of 25°C temperature and 50% humidity, and then the specimen is fixed to the top of a drop weight evaluation device with a weight of 10 to 500 g attached to the bottom and the specimen dropped from a height of 50 cm to measure the adhesive strength (potential energy) when the specimen detaches from the glass, which may be 700 to 990 mJ, for example, 750 to 950 mJ.
[0088] In a specific example, the above-described eco-friendly polyamide resin composition may be formed by applying 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) to a thickness of 1 mm at 110°C onto a specimen of size 50 mm × 50 mm × 4 mm, attaching a glass of size 25 mm × 25 mm × 0.7 mm onto the applied adhesive, curing it for 72 hours under conditions of 25°C temperature and 50% humidity, heating it at 75°C for 15 minutes, and then using a Universal Testing Machine (UTM), fixing the specimen with the glass attached to the bottom of the machine and fixing a weight of 5 mm in diameter to the top jig, and dropping the weight at a speed of 20 mm / min so that when the glass and the specimen are detached, no adhesive remains on the specimen.
[0089] In a specific example, the eco-friendly polyamide resin composition may have a notched Izod impact strength of 12 to 30 kgf·cm / cm, for example, 14 to 25 kgf·cm / cm, of a 1 / 8" thick specimen measured according to ASTM D256.
[0090] In a specific example, the above-described eco-friendly polyamide resin composition may have a heat distortion temperature (HDT) of 175 to 195°C, for example 177 to 193°C, measured under conditions of a load of 1.82 MPa and a heating rate of 120°C / hr in accordance with ASTM D648.
[0091] In a specific example, the eco-friendly polyamide resin composition has a flexural modulus of 90,000 to 180,000 kgf / cm² of a 6.4 mm thick specimen measured at a speed of 2.8 mm / min in accordance with ASTM D790. 2 , for example, 100,000 to 170,000 kgf / cm² 2 It could be.
[0093] The molded article according to the present invention is formed from the above-mentioned eco-friendly polyamide resin composition.
[0094] In a specific example, the molded article may be a plastic member of an electronic device housing comprising a glass frame and a plastic member in contact with at least one surface of the glass frame.
[0095] FIG. 1 schematically illustrates a cross-section of an electronic device housing according to one embodiment of the present invention. The sizes of the components constituting the invention in the drawings are exaggerated for clarity of the specification and are not limited thereto. As shown in FIG. 1, an electronic device housing according to one embodiment of the present invention comprises a glass frame (10); and one or more plastic members (20) in contact with at least one surface of the glass frame (10), wherein the plastic members are formed from the environmentally friendly polyamide resin composition.
[0096] In a specific embodiment, the shapes of the glass frame (10) and the plastic member (20) are not limited to those in the drawing and may have various shapes. However, the glass frame (10) and the plastic member (20) have a structure in which at least one surface is in contact with each other. The contact structure can be realized by bonding with a polyurethane adhesive.
[0097] In a specific example, the glass frame (10) may be a product that is applied to a standard electronic device housing and is readily available for commercial purchase.
[0098] In a specific embodiment, the plastic member (20) can be formed from the eco-friendly polyamide resin composition through various molding methods such as injection molding, extrusion molding, vacuum molding, and casting molding. Specifically, the plastic member (20) may be a plastic member of an electronic device housing, an internal material for an electrical or electronic device, etc.
[0100] The present invention is to be explained more specifically through the following examples, but these examples are for illustrative purposes only and should not be interpreted as limiting the invention.
[0102] Examples
[0103] The specifications of each component used in the following examples and comparative examples are as follows.
[0104] (A) Recycled polyamide resin
[0105] Polyamide 6 derived from marine waste (Manufacturer: Jinjiang-Yonghong Regeneration Resource, Product Name: YH-005) was used.
[0106] (B) Aliphatic polyamide resin
[0107] Polyamide 10.12 (Manufacturer: Shandong Guangyin New Materials, Product Name: B150) was used.
[0108] (C) Aromatic polyamide resin
[0109] Polyamide MXD10 (Manufacturer: Mitsubishi Gas Chemical, Product name: LEXTER8000) was used.
[0110] (D) Glass fiber
[0111] Flat glass fiber (Manufacturer: NITTOBO, Product name: CSG 3PA-820) was used.
[0112] (E) Polyetheresteramide block copolymer
[0113] (E1) Polyamide 12-polytetramethylene oxide block copolymer (Manufacturer: Evonik, Product name: Vestamid E62-S3) was used.
[0114] (E2) Polyamide 6-polyethylene oxide block copolymer (PA6-b-PEO, manufacturer: Sanyo chemical, product name: Pelestat 1251) was used.
[0115] (F) Talc
[0116] Talc (Manufacturer: KOCH, Product Name: KCM-6300C) was used.
[0118] Examples 1 to 12 and Comparative Examples 1 to 10
[0119] Each of the above components was added in the amounts listed in Tables 1, 2, 3, and 4 below, and pellets were prepared by extrusion at 260°C. A twin-screw extruder with L / D=44 and a diameter of 45 mm was used for extrusion. The prepared pellets were dried at 80°C for at least 4 hours, and then injection molded in a 6 oz injection molding machine (molding temperature: 280°C, mold temperature: 80°C) to produce specimens. The physical properties of the prepared specimens were evaluated by the following method, and the results are shown in Tables 1, 2, 3, and 4 below.
[0121] Methods for evaluating physical properties
[0122] (1) Adhesion strength (potential energy, unit: mJ): 0.018 g of polyurethane-based adhesive (HB Fuller, EH9777BS) was applied to a thickness of 1 mm at 110°C on a specimen of size 50 mm × 50 mm × 4 mm, and a glass of size 25 mm × 25 mm × 0.7 mm was attached to the applied adhesive. After curing for 72 hours under conditions of 25°C temperature and 50% humidity, a weight of 10 to 500 g was attached to the top of the drop weight evaluation equipment and the specimen was fixed to the bottom. Then, the weight was dropped from a height of 50 cm to measure the adhesion strength (potential energy) when the specimen detached from the glass.
[0123] (Potential Energy (Ep) = Mass (Weight of weight upon detachment) × 9.8 (Gravitational acceleration) × 50 (Height of weight upon detachment))
[0124] (2) Evaluation of Detachability: 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) was applied to a thickness of 1 mm at 110°C onto a specimen measuring 50 mm × 50 mm × 4 mm. A piece of glass measuring 25 mm × 25 mm × 0.7 mm was then attached to the applied adhesive. The specimen was cured for 72 hours under conditions of 25°C and 50% humidity, and then heated at 75°C for 15 minutes. Subsequently, a Universal Testing Machine (UTM) was used. The specimen with the attached glass was fixed to the bottom of the machine, and a weight with a diameter of 5 mm was fixed to the top jig. The weight was dropped at a speed of 20 mm / min, and the presence of any remaining adhesive on the specimen was checked when the glass and specimen detached. (OK: No adhesive remaining, NG: Adhesive remaining)
[0125] (3) Notched Izod impact strength (unit: kgf·cm / cm): The notched Izod impact strength of a 1 / 8" thick specimen was measured according to ASTM D256.
[0126] (4) Heat distortion temperature (unit: ℃): According to ASTM D648, the heat distortion temperature (HDT) of the specimen was measured under conditions of a load of 1.82 MPa and a heating rate of 120℃ / hr.
[0127] (5) Flexural modulus (unit: kgf / cm²) 2 According to ASTM D790, the flexural modulus of a 6.4 mm thick specimen was measured at a speed of 2.8 mm / min.
[0129] Examples 1 2 3 4 5 6 (A) (Weight%) 10 11 14 20 10 17.5 (B) (Weight%) 22 21 18 12 25 22.5 (C) (weight%) 8 8 8 8 5 10 (D) (Weight%) 60 60 60 60 60 50 (E1) (weight part) 9 9 9 9 9 9 (E2) (weight part) - - - - - - (F) (parts by weight) 0.2 0.2 0.2 0.2 0.2 0.2 adhesive strength 850 850 900 950 850 850 Deconstruction assessment OK OK OK OK OK OK Notch Izod impact strength 18.0 17.5 16.0 14.0 19.0 15.7 Heat distortion temperature 183 182 185 190 181 178 Flexural modulus 138,000 135,000 140,000 155,000 135,000 125,000
[0130] * Parts by weight: Parts by weight relative to 100 parts by weight of base material (A+B+C+D)
[0132] Examples 7 8 9 10 11 12 (A) (Weight%) 10.5 15 14 14 14 14 (B) (Weight%) 13.5 20 18 18 18 18 (C) (weight%) 6 8 8 8 8 8 (D) (Weight%) 70 57 60 60 60 60 (E1) (weight part) 9 9 6 12 9 9 (E2) (weight part) - - - - - - (F) (parts by weight) 0.2 0.2 0.2 0.2 0.15 0.5 adhesive strength 800 850 750 950 850 850 Deconstruction assessment OK OK OK OK OK OK Notch Izod impact strength 20.0 16.9 15.3 18.7 17.1 16.4 Heat distortion temperature 191 181 188 178 185 185 Flexural modulus 165,000 140,000 155,000 135,000 158,000 153,000
[0133] * Parts by weight: Parts by weight relative to 100 parts by weight of base material (A+B+C+D)
[0135] Comparative example 1 2 3 4 5 (A) (Weight%) 4 14.5 30 22.75 5.25 (B) (Weight%) 35.5 0.5 2 29.25 6.75 (C) (weight%) 0.5 25 8 13 3 (D) (Weight%) 60 60 60 35 85 (E1) (weight part) 9 9 9 9 9 (E2) (weight part) - - - - - (F) (parts by weight) 0.2 0.2 0.2 0.2 0.2 adhesive strength 670 840 1,100 680 1,050 Deconstruction assessment OK OK NG OK NG Notch Izod impact strength 19.4 11.0 8,5 13.2 18.8 Heat distortion temperature 174 180 194 175 199 Flexural modulus 85,000 135,000 150,000 90,000 180,000
[0136] * Parts by weight: Parts by weight relative to 100 parts by weight of base material (A+B+C+D)
[0138] Comparative example 6 7 8 9 10 (A) (Weight%) 14 14 14 14 14 (B) (Weight%) 18 18 18 18 18 (C) (weight%) 8 8 8 8 8 (D) (Weight%) 60 60 60 60 60 (E1) (weight part) 1 20 - 9 9 (E2) (weight part) - - 9 - - (F) (parts by weight) 0.2 0.2 0.2 0.01 2 adhesive strength 300 1,200 1,050 650 850 Deconstruction assessment OK NG NG OK OK Notch Izod impact strength 10.0 22.5 16.5 19.5 9.5 Heat distortion temperature 189 168 181 171 184 Flexural modulus 150,000 80,000 135,000 140,000 125,000
[0139] * Parts by weight: Parts by weight relative to 100 parts by weight of base material (A+B+C+D)
[0141] From the above results, it can be seen that the eco-friendly polyamide resin composition according to the present invention is eco-friendly by using a specific amount or more of recycled polyamide resin (at least 5% by weight of the total 100% by weight of the base material), and has excellent adhesion (adhesion strength) and disassembly properties with polyurethane adhesive, impact resistance (notched Izod impact strength), heat resistance (heat distortion temperature), and stiffness (flexural modulus).
[0142] On the other hand, in Comparative Example 1, in which a small amount of recycled polyamide resin and aromatic polyamide resin is applied and an excessive amount of aliphatic polyamide resin is applied, it can be seen that the eco-friendliness, adhesion to polyurethane adhesive, heat resistance, and rigidity are reduced; in Comparative Example 2, in which an excessive amount of aromatic polyamide resin is applied and a small amount of aliphatic polyamide resin is applied, it can be seen that the impact resistance is reduced; and in Comparative Example 3, in which an excessive amount of recycled polyamide resin is applied, it can be seen that the disintegration resistance with polyurethane adhesive and impact resistance are reduced. In Comparative Example 4, in which a small amount of glass fiber is applied, it can be seen that the adhesion to polyurethane adhesive is reduced; and in Comparative Example 5, in which an excessive amount of glass fiber is applied, it can be seen that the disintegration resistance with polyurethane adhesive is reduced. In Comparative Example 6, in which a small amount of polyetheresteramide block copolymer was applied, it was found that adhesion to the polyurethane adhesive and impact resistance were reduced; in Comparative Example 7, in which an excessive amount of polyetheresteramide block copolymer was applied, it was found that disintegration resistance, heat resistance, and rigidity with the polyurethane adhesive were reduced; and in Comparative Example 8, in which a polyamide 6-polyethylene oxide block copolymer (E2) was applied instead of the polyetheresteramide block copolymer of the present invention, it was found that disintegration resistance with the polyurethane adhesive was reduced. Additionally, in Comparative Example 9, in which a small amount of talc was applied, it was found that adhesion to the polyurethane adhesive was reduced, and in Comparative Example 10, in which an excessive amount of talc was applied, it was found that impact resistance was reduced.
[0144] The present invention has been described above with reference to embodiments. Those skilled in the art will understand that the present invention may be embodied in modified forms without departing from the essential characteristics of the invention. Therefore, the disclosed embodiments should be considered in an illustrative rather than a restrictive sense. The scope of the invention is defined by the claims, not by the foregoing description, and all variations within the scope of equivalents should be interpreted as being included in the invention.
Claims
Claim 1 An eco-friendly polyamide resin composition comprising 100 parts by weight of a base material including 5 to 25 parts by weight of recycled polyamide resin, 1 to 30 parts by weight of an aliphatic polyamide resin excluding polyamide 6 and polyamide 6.6, 1 to 20 parts by weight of an aromatic polyamide resin, and 40 to 80 parts by weight of glass fiber; 5 to 15 parts by weight of a polyetheresteramide block copolymer; and 0.1 to 1 part by weight of talc; wherein the polyetheresteramide block copolymer is a block copolymer of a reaction mixture comprising an aminocarboxylic acid having 6 or more carbon atoms, a lactam or a diamine-dicarboxylate, polytetramethylene glycol, and a dicarboxylic acid having 4 to 20 carbon atoms. Claim 2 An eco-friendly polyamide resin composition according to claim 1, characterized in that the recycled polyamide resin comprises one or more of marine waste-derived polyamide 6 and marine waste-derived polyamide 6.
6. Claim 3 An eco-friendly polyamide resin composition according to claim 1, characterized in that the aliphatic polyamide resin comprises one or more of polyamide 11, polyamide 12, polyamide 4.6, polyamide 6.10, polyamide 6.12, polyamide 10.10, and polyamide 10.
12. Claim 4 An eco-friendly polyamide resin composition according to claim 1, characterized in that the aromatic polyamide resin is a polymer of an aliphatic dicarboxylic acid and an aromatic diamine. Claim 5 An eco-friendly polyamide resin composition according to claim 1, wherein the glass fiber has a rectangular or elliptical cross-section, the aspect ratio of the cross-section (major axis of the cross-section / minor axis of the cross-section) is 1.5 to 10, and the minor axis is 2 to 10 μm. Claim 6 An eco-friendly polyamide resin composition according to claim 1, characterized in that the weight ratio of the glass fiber and the polyetheresteramide block copolymer is 1:0.05 to 1:0.
3. Claim 7 An eco-friendly polyamide resin composition according to claim 1, characterized in that the weight ratio of the polyetheresteramide block copolymer and the talc is 1:0.005 to 1:0.
08. Claim 8 The eco-friendly polyamide resin composition according to claim 1 is characterized by applying 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) to a thickness of 1 mm at 110°C onto a specimen of size 50 mm × 50 mm × 4 mm, attaching glass of size 25 mm × 25 mm × 0.7 mm onto the applied adhesive, curing for 72 hours under conditions of 25°C temperature and 50% humidity, and then attaching a weight of 10 to 500 g to the top of a drop weight evaluation device and fixing the specimen to the bottom, and then dropping the weight from a height of 50 cm to measure the adhesive strength (potential energy) when the specimen detaches from the glass, which is 700 to 990 mJ. Claim 9 The eco-friendly polyamide resin composition according to claim 1 is characterized by applying 0.018 g of a polyurethane-based adhesive (HB Fuller, EH9777BS) to a thickness of 1 mm at 110°C onto a specimen of size 50 mm × 50 mm × 4 mm, attaching a glass of size 25 mm × 25 mm × 0.7 mm onto the applied adhesive, curing for 72 hours under conditions of 25°C temperature and 50% humidity, heating the specimen at 75°C for 15 minutes, and then using a Universal Testing Machine (UTM), fixing the specimen with the attached glass to the bottom of the machine and fixing a weight with a diameter of 5 mm to the top jig, and dropping the weight at a speed of 20 mm / min so that when the glass and the specimen are detached, no adhesive remains on the specimen. Claim 10 The eco-friendly polyamide resin composition according to claim 1, characterized in that the notched Izod impact strength of a 1 / 8" thick specimen measured according to ASTM D256 is 12 to 30 kgf·cm / cm. Claim 11 The eco-friendly polyamide resin composition according to claim 1, characterized in that the heat distortion temperature (HDT) measured under conditions of a load of 1.82 MPa and a heating rate of 120℃ / hr in accordance with ASTM D648 is 175 to 195℃. Claim 12 In claim 1, the eco-friendly polyamide resin composition has a flexural modulus of 90,000 to 180,000 kgf / cm² of a 6.4 mm thick specimen measured at a speed of 2.8 mm / min in accordance with ASTM D790. 2 An eco-friendly polyamide resin composition characterized by being. Claim 13 A molded article characterized by being formed from an eco-friendly polyamide resin composition according to any one of claims 1 to 12. Claim 14 An electronic device housing comprising: a glass frame; and a plastic member in contact with at least one surface of the glass frame; wherein the plastic member is formed from an eco-friendly polyamide resin composition according to any one of claims 1 to 12.
Citation Information
Patent Citations
Recycling polyamide resin composition
JP2007262259A
Light-weight recycled resin composition using recycled resin and preparation method therof
KR1020180084244A
Thermoplastic resin composition and article produced therefrom
KR1020230046439A
Polyamide resin composition and article comprising the same
KR1020200082436A
A Recycled polyamide-based resin composition and a molded article prepared therefrom