Solid ion conductor, solid electrolyte and electrochemical device including the same, and method of preparing the solid ion conductor
A halide-based solid ion conductor with a distorted rock-salt structure addresses the limitations of existing materials by improving ion conductivity and stability, enhancing charge/discharge performance in electrochemical devices.
Patent Information
- Application Number
- KR1020200159096
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-24
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2040-11-24
AI Technical Summary
Existing solid ion conductors, such as oxide-based and sulfide-based materials, suffer from limitations in ion conductivity, electrochemical stability, and charge/discharge characteristics, with sulfides generating toxic gases and oxides having poor moldability and low conductivity.
A halide-based solid ion conductor with a distorted rock-salt type crystal structure, featuring metals with specific oxidation states substituted at lithium and indium sites, enhancing ion conductivity and electrochemical stability, is developed.
The new solid ion conductor exhibits improved ion conductivity and electrochemical stability over a wide potential window, leading to enhanced charge/discharge characteristics in electrochemical devices.
Smart Images

Figure 112020126534681-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The invention relates to a solid ion conductor, a solid electrolyte and an electrochemical device including the same, and a method for manufacturing the solid ion conductor. Background Technology
[0002] Electrochemical devices, such as all-solid-state secondary batteries, employ materials with high energy density, such as lithium metal, for the negative electrode to achieve high energy density, and use solid-state ion conductors as the electrolyte for safe operation.
[0003] Oxide-based and sulfide-based solid ion conductors are widely studied as solid ion conductors depending on the type of anion. However, while oxide-based solid ion conductors exhibit high chemical stability, their performance is inferior to that of sulfide-based solid ion conductors in terms of ion conductivity and moldability. Sulfide-based solid ion conductors possess high ion conductivity and excellent moldability, but they generate toxic gases upon reaction with water.
[0004] Therefore, there is a need for a solid ion conductor having improved ion conductivity, electrochemical stability over a wide potential window, and improved charge / discharge characteristics, a solid electrolyte and electrochemical device including the same, and a method for manufacturing the solid ion conductor. The problem to be solved
[0005] One aspect is to provide a solid ion conductor having enhanced ion conductivity, electrochemical stability over a wide potential window, and enhanced charge / discharge characteristics.
[0006] Another aspect is to provide a solid electrolyte comprising the above-mentioned solid ion conductor.
[0007] Another aspect is to provide an electrochemical device comprising the above-mentioned solid ion conductor.
[0008] Another aspect is to provide a method for manufacturing the above-mentioned solid ion conductor. means of solving the problem
[0009] Depending on one aspect,
[0010] A solid ionic conductor comprising a compound represented by the following chemical formula 1 is provided:
[0011] <Chemical Formula 1>
[0012] Li a M b In c X d
[0013] In the above chemical formula 1,
[0014] M may be one or more metals selected from metals with an oxidation number of +1 or metals with an oxidation number of +3, and
[0015] X may be one or more elements selected from among halogen elements, and
[0016] 2.5 < a < 3.5, 0 < b < 0.5, 0.5 < c < 1.5, 5 < d < 7.
[0017] The above compound may include a compound represented by the following chemical formula 2:
[0018] <Chemical Formula 2>
[0019] Li x-y (M1) y In 1-z (M2) z X' w
[0020] In the above chemical formula 2,
[0021] M1 can be a metal with an oxidation number of +1 having an ionic radius of 76 pm or more, and
[0022] M2 can be a metal with an oxidation number of +3, and
[0023] X' may be one or more elements selected from among halogen elements, and
[0024] 3 < x < 4, 0 < y < 0.5, 0 < z < 0.5, 5 < w < 7, 2.5 < xy < 3.5 may be possible.
[0025] The above compound may have a distorted rock-salt type structure.
[0026] The above compound may be a crystal structure having lithium ion transport channels extended in the x-axis, y-axis, and z-axis directions according to the spatial distribution of the ionic radius of the M element.
[0027] The above compound may include a crystal structure belonging to the C2 / m space group or the C2 / m-like space group.
[0028] Compared to the Li3InCl6 compound, the peak appearing in the region where the diffraction angle 2θ obtained by the XRD spectrum using CuKα rays is 51.5° to 52.0° in the above compound may be shifted to the left.
[0029] The above solid ion conductor is 3.5 x 10 at 25℃ -4 mS·cm -1 It can have an ionic conductivity greater than that.
[0030] Depending on other aspects of work,
[0031] A solid electrolyte comprising the solid ion conductor described above is provided.
[0032] The above solid electrolyte can be electrochemically stable in a voltage window of 0.6 V to 4.2 V (vs. Li).
[0033] Depending on other aspects of work,
[0034] An electrochemical device comprising an anode layer, a cathode layer, and a solid electrolyte layer, and comprising the solid electrolyte described above is provided.
[0035] The above solid electrolyte may be included in the solid electrolyte layer, the anode layer, the cathode layer, the anode layer protective film, the cathode layer protective film, or a combination thereof.
[0036] The above solid electrolyte layer may include the above solid electrolyte, a sulfide-based solid electrolyte, or a solid electrolyte selected from a combination thereof.
[0037] The above anode layer may include an anode active material selected from lithium transition metal oxide, lithium transition metal phosphate, sulfide, or a combination thereof, and the above solid electrolyte.
[0038] During the charging and discharging process of the above-mentioned positive electrode active material, cation mixing may occur in which metal ions with an oxidation state of +1 are inserted into the lithium ion transport pathway.
[0039] The above anode layer may further include an ion-conducting inorganic material.
[0040] The above cathode layer may include a metal-based cathode active material, a carbon-based cathode active material, or a combination thereof.
[0041] The above electrochemical device may be an all-solid-state secondary battery or a metal-air battery.
[0042] Depending on other aspects of work,
[0043] Step of preparing a precursor for forming a solid ion conductor;
[0044] A step of providing a precursor mixture for forming a solid ion conductor by performing mechanical milling on the precursor for forming a solid ion conductor; and
[0045] A method for manufacturing a solid ion conductor is provided, comprising the step of heat-treating the above-mentioned precursor mixture for forming a solid ion conductor at a temperature of 300°C or lower to manufacture a solid ion conductor comprising a compound represented by the following chemical formula 1:
[0046] <Chemical Formula 1>
[0047] Li a M b In c X d
[0048] In the above chemical formula 1,
[0049] M may be one or more metals selected from metals with an oxidation number of +1 or metals with an oxidation number of +3, and
[0050] X may be one or more elements selected from among halogen elements, and
[0051] 2.5 < a < 3.5, 0 < b < 0.5, 0.5 < c < 1.5, 5 < d < 7. Effects of the invention
[0052] A solid ion conductor according to one aspect is a halide-based solid ion conductor in which a metal having an oxidation state of +1 or / and a metal having an oxidation state of +3 is substituted at a Li site or / and an In site. The solid ion conductor may have enhanced ion conductivity. When the solid ion conductor is applied to an electrochemical device, the electrochemical device may have electrochemical stability over a wide potential window and enhanced charge / discharge characteristics.
[0053] The above solid ion conductor may be included in the solid electrolyte layer, anode layer, cathode layer, anode layer protective film, or cathode layer protective film of an electrochemical device, for example, an all-solid-state secondary battery or a metal-air battery. Brief explanation of the drawing
[0054] FIG. 1 is a schematic diagram showing the crystal structure of a solid ion conductor compound according to one embodiment. FIGS. 2 to 4 are cross-sectional views of an all-solid-state secondary battery according to one embodiment. Figure 5 shows the XRD spectrum experimental results for solid ion conductor compounds prepared according to Examples 1 to 4. Figure 6 is an enlarged result of the diffraction peak in the region where the diffraction angle 2θ is 51.5° to 52.0° in the XRD spectrum of solid ion conductor compounds prepared by Examples 1 to 4 and Comparative Example 1. Figure 7 is the evaluation result of the initial discharge capacity of the all-solid-state secondary battery prepared according to Example 14 and Comparative Example 3 when charged with a constant current of 0.1 C and discharged with a constant current of 0.01 C to 1.0 C (cut-off voltage: 4.0V~2.0V). Figures 8 and 9 are the charge-discharge evaluation results for all-solid-state secondary batteries prepared according to Example 14 and Comparative Example 3, respectively, when charged at a constant current of 0.1 C and discharged at a constant current of 0.05 C (cut-off voltage: 4.0V~2.0V). Figure 10 shows the results of the lifespan characteristic evaluation for the all-solid-state secondary batteries prepared by Example 25 and Comparative Example 5. Specific details for implementing the invention
[0055] Hereinafter, a solid ion conductor according to one embodiment of the present invention, a solid electrolyte and an electrochemical device including the same, and a method for manufacturing the solid ion conductor will be described in detail with reference to the attached drawings. The following is presented as an example and is not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.
[0056] In this specification, expressions such as "at least one," "one or more," or "one or more" preceding components are to supplement the list of all components and do not mean that they are to supplement the individual components described above. In this specification, the term "combination" includes mixtures, alloys, reaction products, etc., unless specifically stated otherwise.
[0057] In this specification, the term "includes" means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0058] In this specification, terms such as "first," "second," etc., are used to distinguish one element from another without indicating order, quantity, or importance. Unless otherwise indicated in this specification or clearly contradicted by the context, they should be interpreted to include both singular and plural forms. "Or" means "and / or" unless otherwise specified.
[0059] Throughout this specification, terms such as “one embodiment,” “an embodiment,” etc., mean that specific elements described in relation to an embodiment are included in at least one embodiment described herein and may or may not be present in other embodiments. Furthermore, it should be understood that the described elements may be combined in any appropriate manner in various embodiments.
[0060] Unless otherwise defined, technical and scientific terms used herein have the same meaning as generally understood by those skilled in the art to which this application pertains. All cited patents, patent applications, and other references are incorporated herein by reference in their entirety. However, in the event that terms in this specification contradict or conflict with terms in the incorporated reference, terms from this specification shall prevail over conflicting terms in the incorporated reference. Although specific embodiments and embodiments have been described, alternatives, modifications, variations, improvements, and substantial equivalents that are not currently anticipated or cannot be anticipated may arise to the applicant or those skilled in the art. Accordingly, the appended claims and subject to amendment are intended to include all such alternatives, variations, improvements, and substantial equivalents.
[0061] Solid ion conductors are used as solid electrolytes. However, solid electrolytes cannot possess high ionic conductivity compared to liquid electrolytes. Therefore, when solid electrolytes are applied to electrochemical devices, these devices exhibit poor charge and discharge characteristics at room temperature.
[0062] Among solid ion conductors, sulfide-based and oxide-based solid ion conductors are being widely studied. Sulfide-based solid ion conductors exhibit excellent ion conductivity, but their chemical and electrochemical stability are degraded due to factors such as gas generation. Oxide-based solid ion conductors have excellent chemical stability but poor moldability and low ion conductivity, resulting in poor charge-discharge characteristics when applied to electrochemical devices. Therefore, to compensate for these shortcomings, a process for crystallizing oxide-based solid ion conductors at high temperatures exceeding 1000°C is required.
[0063] Recently, halide-based solid electrolytes are being studied as solid ion conductors. Halide-based solid electrolytes can be molded by pressurization alone and do not generate gas. Among halide-based solid electrolytes, Li3InCl6 is widely used as a solid electrolyte for the anode. However, when Li3InCl6 is applied to electrochemical devices as a solid electrolyte, its ion conductivity remains low, resulting in poor charge-discharge characteristics.
[0064] Based on these points, the inventors of the present invention propose a solid ion conductor, a solid electrolyte and an electrochemical device including the same, and a method for manufacturing the solid ion conductor.
[0065] Hereinafter, a solid ion conductor, a solid electrolyte and an electrochemical device including the same, and a method for manufacturing the solid ion conductor are described in detail.
[0067] Solid ion conductors
[0068] A solid ion conductor according to one embodiment may include a compound represented by the following chemical formula 1:
[0069] <Chemical Formula 1>
[0070] Li a M b In c X d
[0071] In the above chemical formula 1,
[0072] M may be one or more metals selected from metals with an oxidation number of +1 or metals with an oxidation number of +3, and
[0073] X may be one or more elements selected from among halogen elements, and
[0074] 2.5 < a < 3.5, 0 < b < 0.5, 0.5 < c < 1.5, 5 < d < 7.
[0075] The compound represented by the above chemical formula 1 may include a compound represented by the following chemical formula 2:
[0076] <Chemical Formula 2>
[0077] Li x-y (M1) y In 1-z (M2) z X' w
[0078] In the above chemical formula 2,
[0079] M1 can be a metal with an oxidation number of +1 having an ionic radius of 76 pm or more, and
[0080] M2 can be a metal with an oxidation number of +3, and
[0081] X' may be one or more elements selected from among halogen elements, and
[0082] 3 < x < 4, 0 < y < 0.5, 0 < z < 0.5, 5 < w < 7, 2.5 < xy < 3.5 may be possible.
[0083] The above compound is a halide-based solid ion conductor in which a metal with an oxidation state of +1 or / and a metal with an oxidation state of +3 is substituted at the Li site or / and the In site. The above halide-based solid ion conductor may have improved ion conductivity compared to a Li3InCl6 halide-based solid ion conductor. When the above solid ion conductor is applied to an electrochemical device, the electrochemical device may have electrochemical stability over a wide potential window and improved charge / discharge characteristics.
[0084] The reason why the above compound has improved ionic conductivity compared to Li3InCl6 halide-based solid ionic conductors is explained in more detail below, but this is intended to aid in understanding the present invention and the scope of the present invention is not limited to the scope of the following description.
[0085] FIG. 1 is a schematic diagram showing the crystal structure of a solid ion conductor compound according to one embodiment.
[0086] As shown in FIG. 1, the solid ion conductor compound according to one embodiment has a distorted rock-salt type crystal structure. The compound is In 3+ Metal as the central element and some In 3+ The metal is In substituted with a metallic element (M or M2) other than In with an oxidation number of +3. 3+ 6 Cl in (100) - (200) coordinated octahedron (InCl6 3- It is composed of the above octahedron (InCl6 3- Li around ) + Li, in which the metal and some parts are substituted with metal elements other than lithium (M or M1) having an oxidation state of +1. + (300) is a layered crystal structure in which the above octahedron (InCl6) is located. 3- Li around ) + The metal is substituted with a metal other than lithium with an oxidation state of +1 (M or M1), for example, a metal with an oxidation state of +1 (M or M1) having an ionic radius of 76 pm or greater. Li + The metal is Cl - LiCl can have ionic bonds depending on the distance from. Li + Li on the site + Li is substituted with a metal (M or M1) cation with an ionic radius greater than that of Li +A space in which ions can move freely can be secured. The compound may have a crystal structure having lithium ion movement channels extended in the x-axis, y-axis, and z-axis directions according to the spatial distribution of the ionic radius of the M element (or M1 element). As a result, it is believed that lithium ion conductivity is improved.
[0087] The above compound may include a crystal structure belonging to the C2 / m space group or the C2 / m-like space group. The C2 / m space group refers to ICSD No. 04-009-9027, and the C2 / m-like space group refers to a crystal structure similar to the C2 / m space group crystal structure and having a peak pattern similar to the peak pattern of the C2 / m space group crystal structure in the XRD spectrum. For example, the C2 / m space group crystal structure may have diffraction peaks in the region where the diffraction angle 2θ is 28° to 29°, the region where it is 29° to 30°, the region where it is 32.5° to 35°, the region where it is 37° to 38.5°, the region where it is 42.5° to 45°, the region where it is 47.5° to 50°, and the region where it is 51.5° to 52.0°.
[0088] Compared to the Li3InCl6 compound, the peak appearing in the region where the diffraction angle 2θ obtained by the XRD spectrum using CuKα lines is 51.5° to 52.0° in the above compound may be shifted to the left. In other words, compared to the Li3InCl6 compound, the crystal lattice size of the above compound may be larger in the x-axis direction, the y-axis direction, or / and the z-axis direction. A solid ion conductor containing the above compound may have enhanced ion conductivity.
[0089] For example, the above M (or M1) may be one or more metals selected from Na, K, Rb, Cs, Ag, Au, Cu, Hg, Tl, Ga, Tl, Sc, Y, La, Lu, or Gd.
[0090] For example, the above X may be Cl, Br, I, or a combination thereof.
[0091] For example, in the above chemical formula 1, 0 < b ≤ 0.3 may be possible.
[0092] For example, in Chemical Formula 1, 0.7 < c < 1.2 may be possible.
[0093] For example, the above compound is Li 3-p K p InCl6(0 < p ≤ 0.3), Li 3-p Cu p InCl6(0 < p ≤ 0.3), Li 3-p Na p InCl6(0 < p ≤ 0.3), Li 3-p Rb p InCl6(0 < p ≤ 0.3), Li 3-p Cs p InCl6(0 < p ≤ 0.3), Li 3-p Ag p InCl6(0 < p ≤ 0.3), Li 3-p Hg p InCl6(0 < p ≤ 0.3), Li 3-p Tl p InCl6(0 < p ≤ 0.3), Li 3-p K p InCl5Br (0 < p ≤ 0.3), Li 3-p Cu p InCl5Br (0 < p ≤ 0.3), Li 3-p Na p InCl5Br (0 < p ≤ 0.3), Li 3-p Rb p InCl5Br (0 < p ≤ 0.3), Li 3-p Cs p InCl5Br (0 < p ≤ 0.3), Li 3-p Ag p InCl5Br (0 < p ≤ 0.3), Li 3-p Hgp InCl5Br (0 < p ≤ 0.3), Li 3-p Tl p InCl5Br (0 < p ≤ 0.3), Li 3-p K p InClBr5(0 < p ≤ 0.3), Li 3-p The p InClBr5(0 < p ≤ 0.3), Li 3-p The p InClBr5(0 < p ≤ 0.3), Li 3-p Rb p InClBr5(0 < p ≤ 0.3), Li 3-p Cs p InClBr5(0 < p ≤ 0.3), Li 3-p Ag p InClBr5(0 < p ≤ 0.3), Li 3-p Hg p InClBr5(0 < p ≤ 0.3), Li 3-p Tl p InClBr5(0 < p ≤ 0.3), Li 3-p K p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Rb p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cs p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Agp And 1-q Him q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Hg p And 1-q Him q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Soil p And 1-q Him q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p K p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cu p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p On p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Rb p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cs p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Ag p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Hg p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Soil p And 1-q Him qCl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p K p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Cu p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Na p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Rb p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Cs p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Ag p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Hg p In 1-q Ga q ClBr5(0 < p ≤ 0.3, 0 < q ≤ 0.3), or Li 3-p Tl p In 1-q Ga q It may include one or more compounds selected from ClBr5 (0 < p ≤ 0.3, 0 < q ≤ 0.3).
[0094] For example, the above compound is Li 3-p K p InCl6(0 < p ≤ 0.3), Li 3-p Cu p InCl6(0 < p ≤ 0.3), Li 3-p Na p InCl6(0 < p ≤ 0.3), Li3-p Rb p InCl6(0 < p ≤ 0.3), Li 3-p Cs p InCl6(0 < p ≤ 0.3), Li 3-p Ag p InCl6(0 < p ≤ 0.3), Li 3-p Hg p InCl6(0 < p ≤ 0.3), Li 3-p Tl p InCl6(0 < p ≤ 0.3), Li 3-p K p InCl5Br (0 < p ≤ 0.3), Li 3-p The p InCl5Br (0 < p ≤ 0.3), Li 3-p The p InCl5Br (0 < p ≤ 0.3), Li 3-p Rb p InCl5Br (0 < p ≤ 0.3), Li 3-p Cs p InCl5Br (0 < p ≤ 0.3), Li 3-p Ag p InCl5Br (0 < p ≤ 0.3), Li 3-p Hg p InCl5Br (0 < p ≤ 0.3), Li 3-p Tl p InCl5Br (0 < p ≤ 0.3), Li 3-p K p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga qCl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Rb p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cs p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Ag p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Hg p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Tl p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p K p You 1-q Ga q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Rb p You 1-q Ga q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cs p You 1-q Ga q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Ag p You 1-qGa q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Hg p In 1-q Ga q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), or Li 3-p Tl p In 1-q Ga q It may include one or more compounds selected from Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3).
[0095] The above compound can maintain the crystal structure of the halide compound within the range of types and amounts of the metal having an oxidation number of +1 or / and the metal having an oxidation number of +3 that is substituted. Within the crystal structure, the metal having an oxidation number of +1 or / and the metal having an oxidation number of +3 can be easily substituted. As a result, a solid ion conductor containing the above compound can have enhanced ion conductivity.
[0096] The above solid ion conductor is 3.5 x 10 at 25℃ -4 S·cm -1 It can have an ionic conductivity greater than or equal to 3.6 x 10⁻⁶ at 25°C. For example, the solid ionic conductor has 3.6 x 10⁻⁶ at 25°C -4 S·cm -1 More than or equal to 3.7 x 10 -4 S·cm -1 or more than 3.8 x 10 -4 S·cm -1 or more than 3.9 x 10 -4 S·cm -1 or more than 4.0 x 10 -4 S·cm -1 or more than 4.1 x 10 -4 S·cm -1 or more than 4.2 x 10 -4 S·cm -1 or more than 4.3 x 10 -4 S·cm -1 or more than 4.4 x 10 -4 S·cm-1 or more than 4.5 x 10 -4 S·cm -1 or more than 4.6 x 10 -4 S·cm -1 or more than 4.7 x 10 -4 S·cm -1 or more than 4.8 x 10 -4 S·cm -1 or more than 4.9 x 10 -4 S·cm -1 or more than 5.0 x 10 -4 S·cm -1 or more than 5.1 x 10 -4 S·cm -1 or more than 5.2 x 10 -4 S·cm -1 or more than 5.3 x 10 -4 S·cm -1 It can have an ionic conductivity greater than that.
[0098] Solid Electrolytes and Electrochemical Devices
[0099] A solid electrolyte according to another embodiment may include the solid ion conductor described above. The solid electrolyte may be electrochemically stable in a voltage window of 0.6 V to 4.2 V (vs. Li). An electrochemical device comprising the solid electrolyte may have improved ion conductivity and charge / discharge characteristics.
[0100] An electrochemical device according to another embodiment includes an anode layer, a cathode layer, and a solid electrolyte layer, and may include the solid electrolyte described above.
[0101] The above solid electrolyte may be included in the solid electrolyte layer, the anode layer, the cathode layer, the anode layer protective film, the cathode layer protective film, or a combination thereof.
[0102] The above solid electrolyte layer may include the above solid electrolyte, a sulfide-based solid electrolyte, or a solid electrolyte selected from a combination thereof.
[0103] The above sulfide-based solid electrolyte may include a solid electrolyte represented by the following chemical formula 3:
[0104] <Chemical Formula 3>
[0105] Li + 12-n-r A n+ X 2- 6-r Y' - r
[0106] In the above chemical formula 3,
[0107] A can be P, As, Ge, Ga, Sb, Si, Sn, Al, In, Tl, V, Nb, or Ta, and
[0108] X can be S, Se, or Te, and
[0109] Y' can be Cl, Br, I, F, CN, OCN, SCN, or N3, and
[0110] 1 < n < 5, 0 < r < 2.
[0111] The above sulfide-based solid ion conductor is Li 7-x PS 6-x Cl x (0≤x≤2), Li 7-x PS 6-x Br x (0≤x≤2), and Li 7-x PS 6-x I x It may be an azirodite-type compound containing one or more selected from (0≤x≤2). For example, the sulfide-based solid ion conductor may be an azirodite-type compound containing one or more selected from Li6PS5Cl, Li6PS5Br, and Li6PS5I.
[0112] If necessary, the above sulfide-based solid ion conductor is Li2S-P2S5, Li2S-P2S5-LiX (where X is a halogen element), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z m S n (m, n are positive numbers, Z is one of Ge, Zn, or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, or Li2S-SiS2-Li p MO q (p, q are positive numbers, M is one of P, Si, Ge, B, Al, Ga, In, etc.) may be included. For example, the sulfide-based solid ion conductor may include Li2S-P2S5. If the sulfide-based solid ion conductor is Li2S-P2S5, the molar ratio of Li2S and P2S5 may be, for example, in the range of Li2S:P2S5 = 50:50 to 90:10.
[0113] The above oxide-based solid ion conductor is Garnet-based ceramics Li 3+x La3M2O 12 (M = Te, Nb, or Zr, x is an integer from 1 to 10), lithium phosphorus oxynitride (Li x PO y N z )(0< x <1, 0< y <1, 0< z <1)(LiPON: Lithium Phosphorus Oxynitride), Li x P y O z N k (2.7 ≤ x ≤3.3, 0.8≤ y ≤1.2, 3.5≤ z ≤3.9, 0.1≤ k ≤0.5), Li w PO x N y S z(0< w <1, 0< x <1, 0< y <1, 0< z <1), Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0< x <2, 0 ≤ y <3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0 ≤ x <1, 0≤ y <1), Pb(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, SiC, Lithium Phosphate (Li3PO4), Lithium Titanium Phosphate (Li x Ti y (PO4)3, 0< x <2, 0< y <3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0< x <2, 0< y <1, 0< z <3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤ x ≤1, 0≤ y ≤1), lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0< x <4, 0< y <1, 0< z <1, 0< w <5), lithium nitride glass (Li x N y , 0< x <4, 0< y <2), SiS2(Li x Si y S z, 0< x <3, 0< y <2, 0< z <4), P2S5 series glass (Li x P y S z , 0< x <3, 0< y <3, 0< z <7), Li2O, LiF, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2-based ceramics, Garnet-based ceramics Li 3+x La3M2O 12 (M = Te, Nb, or Zr, where x is an integer from 1 to 10), or a combination thereof may be used. For example, the oxide-based solid ion conductor may use a garnet-based oxide-based solid electrolyte that exhibits excellent reduction stability when in contact with a lithium anode. Garnet-based ceramics Li 3+x La3M2O 12 (M = Te, Nb, or Zr), for example LLZO(Li 6.5 La3Zr 1.5 Ta 0.5 O 12 ) can be used.
[0114] The above solid electrolyte may further include a binder. For example, the binder included in the above solid electrolyte may be styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, or a combination thereof. However, it is not limited thereto, and any binder used in the relevant technical field is acceptable.
[0115] If necessary, the solid electrolyte may further comprise an organic solid electrolyte. Examples of the organic solid electrolyte may include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate ester polymers, poly-adhesion lysines, polyester sulfides, polyvinyl alcohols, polyvinylidene fluoride, or polymers containing ionic dissociators. If necessary, the solid electrolyte may further comprise an amorphous solid electrolyte. The solid electrolyte may comprise a mixed solid electrolyte comprising a mixture of a crystalline solid electrolyte and an amorphous solid electrolyte. If necessary, the solid electrolyte may further comprise a lithium salt or / and an ionic liquid.
[0116] If necessary, the solid electrolyte may further include an ion-conducting inorganic material.
[0117] Ion-conducting inorganic materials include one or more selected from glass or amorphous metal ion conductors, ceramic active metal ion conductors, and glass ceramic active metal ion conductors, but are not necessarily limited to these, and any material used as an ion-conducting inorganic material in the relevant technical field is acceptable. The ion-conducting inorganic materials are, for example, in the form of ion-conducting inorganic particles or sheets thereof.
[0118] Ionic conductive inorganic materials include, for example, BaTiO3, Pb(Zr,Ti)O3(PZT), and Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1, 0≤y<1), Pb(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, SiC, Lithium Phosphate (Li3PO4), Lithium Titanium Phosphate (Li x Ti y(PO4)3, 0 <x<2, 0<y<3), 리튬알루미늄티타늄포스페이트 (Li x Al y Ti z (PO4)3, 0 <x<2, 0<y<1, 0<z<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0≤x≤1, 0≤y≤1), lithium lanthanum titanate(Li x La y TiO3, 0 <x<2, 0<y<3), 리튬게르마늄티오포스페이트(Li x Ge y P z S w , 0 <x<4, 0<y<1, 0<z<1, 0<w<5), 리튬나이트라이드(Li x N y , 0 <x<4, 0<y<2), SiS2(Li x Si y S z , 0 <x<3,0<y<2, 0<z<4) 계열 글래스, P2S5(Li x P y S z , 0 <x<3, 0<y<3, 0<z<7) 계열 글래스, L i2 O, LiF, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2-based ceramics, Garnet-based ceramics (Li 3+x La3M2O 12 It is one or more selected from (M = Te, Nb, Zr)) or a combination thereof.
[0119] The above-mentioned solid electrolyte may be in the form of a powder or a molded article. The solid electrolyte in the form of a molded article may be, for example, in the form of pellets, sheets, thin films, etc., but is not necessarily limited to these and may have various forms depending on the application.
[0120] The thickness of the solid electrolyte layer may be 10 micrometers (μm) to 1 millimeter (mm). The solid electrolyte layer may be a single layer or a multilayer structure of two or more layers.
[0121] For example, the solid electrolyte may comprise a solid ion conductor comprising a compound represented by Chemical Formula 1 alone in the solid electrolyte layer. Alternatively, the solid electrolyte layer may comprise an oxide-based solid ion conductor or a sulfide-based solid ion conductor as a separate layer in addition to the solid ion conductor.
[0122] For example, the solid electrolyte may comprise, alone, a solid ion conductor comprising a compound represented by Formula 1 in the anode layer or / and cathode layer. Alternatively, in addition to the solid ion conductor, the anode layer or / and cathode layer may comprise a sulfide-based solid ion conductor, an oxide-based solid ion conductor solid electrolyte, or / and an ionic liquid-containing electrolyte in a separate single-layer or multi-layer structure. For example, the electrochemical element may comprise, in the order of an anode layer, an ionic liquid-containing electrolyte, an oxide-based solid ion conductor solid electrolyte (or a sulfide-based solid ion conductor solid electrolyte), a solid ion conductor solid electrolyte containing a compound represented by Formula 1, an oxide-based solid ion conductor solid electrolyte (or a sulfide-based solid ion conductor solid electrolyte), and a cathode layer.
[0123] The above electrochemical device may be an all-solid-state secondary battery or a metal-air battery. However, it is not limited thereto, and any electrochemical device usable in the relevant technical field is acceptable.
[0124] For example, the above electrochemical device may be an all-solid-state secondary battery.
[0125] FIGS. 2 to 4 are cross-sectional views of an all-solid-state secondary battery according to one embodiment.
[0126] Referring to FIGS. 2 to 4, the all-solid-state secondary battery (1) comprises a positive electrode layer (10) including a positive current collector (11) and a positive active material layer (12); a negative electrode layer (20); and a solid electrolyte layer (30) disposed between the positive electrode layer (10) and the negative electrode layer (20). The negative electrode layer (20) comprises a negative electrode current collector (21) and a negative electrode active material layer (22) disposed on the negative electrode current collector (21), wherein the negative electrode active material layer (22) comprises lithium metal, an alloy with lithium, or a negative electrode active material that forms a compound. One or more of the positive electrode layer (10); the negative electrode layer (20); and the solid electrolyte layer (30) of the all-solid-state secondary battery (1) comprise a solid ion conductor comprising a compound represented by the above chemical formula 1.
[0127] For the positive current collector (11), for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof may be used. The positive current collector (11) may be omitted.
[0128] The positive active material layer (12) may include a positive active material and / or a solid electrolyte. The solid electrolyte included in the positive layer (10) may be the same as or different from the solid electrolyte included in the solid electrolyte layer (30).
[0129] The cathode active material may be a cathode active material capable of reversibly absorbing and releasing lithium ions. The cathode active material may be selected from lithium transition metal oxides, lithium transition metal phosphates, sulfides, or combinations thereof. For example, the cathode active material may be formed using lithium cobalt oxide (hereinafter referred to as LCO), lithium nickel oxide, lithium nickel cobalt oxide, lithium nickel cobalt aluminum oxide (hereinafter referred to as NCA), lithium nickel cobalt manganese oxide (hereinafter referred to as NCM), lithium manganate, lithium iron phosphate, nickel sulfide, copper sulfide, lithium sulfide, iron oxide, or vanadium oxide, etc. Each of these cathode active materials may be used individually or in combination of two or more types. For example, the cathode active material may be LiNi x Co y Al z O2(NCA) or LiNi x Co y Mn z Examples include lithium salts of ternary transition metal oxides such as O2(NCM) (where 0 < x < 1, 0 < y < 1, 0 < z < 1, x + y + z = 1).
[0130] A coating layer may be formed on the cathode active material. Any coating layer that is used as a coating layer for the cathode active material of an all-solid-state secondary battery may be used. Examples of coating layers include, for instance, Li2O-ZrO2.
[0131] In addition, if the positive active material is formed from a lithium salt of a ternary transition metal oxide such as NCA or NCM and includes nickel (Ni) as the positive active material, the capacity density of the all-solid-state secondary battery (1) can be increased, thereby reducing the metal leaching of the positive active material in the charged state. The all-solid-state secondary battery (1) can improve long-term reliability and cycle characteristics in the charged state.
[0132] Examples of the shapes of the above positive active material include particle shapes such as oval and spherical. In addition, the particle size of the positive active material is not limited and can be used as long as it is within a range applicable to the positive active material of an all-solid-state secondary battery. The content of the positive active material of the positive layer (10) is also not limited and can be used as long as it is within a range applicable to the positive of an all-solid-state secondary battery.
[0133] During the charging and discharging process of the above-mentioned positive electrode active material, cation mixing may occur in which metal ions with an oxidation state of +1 are inserted into the lithium ion transport pathway.
[0134] The anode layer (10) may further include an ion-conducting inorganic material. The types of ion-conducting inorganic materials are the same as those described above, so further explanation is omitted.
[0135] The anode layer (10) may appropriately incorporate additives such as, for example, a conductive agent, a binder, a filler, a dispersant, and an ion-conducting aid, in addition to the anode active material or / and solid electrolyte described above.
[0136] Examples of conductive agents that can be incorporated into the anode layer (10) include graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or metal powder. Examples of binders that can be incorporated into the anode layer (10) include styrene butadiene rubber (SBR), polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Known materials generally used in electrodes of all-solid-state secondary batteries can be used as coating agents, dispersants, and ion-conducting aids that can be incorporated into the anode layer (10).
[0137] The negative electrode layer (20) may include a negative electrode current collector (21) and a negative electrode active material layer (22).
[0138] Materials constituting the negative electrode current collector (21) may include copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), or nickel (Ni). The negative electrode current collector (21) may be composed of one type of metal, or may be composed of an alloy of two or more types of metals or a coating material. The negative electrode current collector (21) may be formed, for example, in a plate shape or a thin shape.
[0139] The negative electrode active material layer (22) may include a metal-based negative electrode active material, a carbon-based negative electrode active material, or a combination thereof.
[0140] The above-mentioned negative electrode active material may include a metal-based negative electrode active material, a carbon-based negative electrode active material, or a combination thereof. For example, the negative electrode active material may use lithium or an alloy comprising one or more selected from lithium and indium (In), silicon (Si), gallium (Ga), tin (Sn), aluminum (Al), titanium (Ti), zirconium (Zr), niobium (Nb), germanium (Ge), antimony (Sb), bismuth (Bi), gold (Au), platinum (Pt), palladium (Pd), magnesium (Mg), palladium (Pd), silver (Ag), and zinc (Zn). However, it is not limited thereto, and any metal or metalloid capable of forming an alloy with lithium available in the relevant technical field may be used.
[0141] The above carbon-based cathode active material may be graphite, carbon black (CB), acetylene black (AB), furnace black (FB), ketjen black (KB), graphene, carbon nanotube, or carbon nanofiber.
[0142] The negative electrode active material layer (22) may also appropriately incorporate additives such as a conductive agent, binder, filler, dispersant, and ion conductivity aid.
[0143] If necessary, the cathode active material layer (22) may be a non-cathode coating layer. For example, the non-cathode coating layer may have a structure containing a metal such as silicon and carbon, and a conductive binder disposed around the metal and carbon. The thickness of the non-cathode coating layer may be 1 μm to 20 μm.
[0144] The solid electrolyte layer (30) can be manufactured by depositing using known film deposition methods, such as aerosol deposition, cold spray, or sputtering. Alternatively, the solid electrolyte layer (30) can be manufactured by pressurizing a single solid electrolyte particle. Alternatively, the solid electrolyte layer (30) can be manufactured by mixing the solid electrolyte, solvent, and binder, applying the mixture, drying, and pressurizing.
[0145] As shown in FIG. 5, a thin film (24) may be formed on the surface of the negative current collector (21). The thin film (24) may contain elements capable of forming an alloy with lithium. Elements capable of forming an alloy with lithium may include, for example, gold, silver, zinc, tin, indium, silicon, aluminum, and bismuth. The thin film (24) may be composed of one of these metals or may be composed of several types of alloys. By having the thin film (24), the precipitation pattern of the metal layer (23) shown in FIG. 6 may be further flattened, and the characteristics of the solid secondary battery (1) may be further improved.
[0146] The thickness of the thin film (24) may be 1 nm to 500 nm, but is not limited thereto. When the thickness of the thin film (24) is within the above range, the function of the thin film (24) is sufficiently performed, and the amount of lithium precipitated in the negative electrode layer is appropriate, so the characteristics of the all-solid-state secondary battery (1) are excellent. The thin film (24) can be formed on the negative electrode current collector (21) by, for example, vacuum deposition, sputtering, plating, etc.
[0148] Method for manufacturing a solid ion conductor
[0149] A method for manufacturing a solid ion conductor according to one embodiment may include: a step of preparing a precursor for forming a solid ion conductor; a step of performing mechanical milling on the precursor for forming a solid ion conductor to provide a precursor mixture for forming a solid ion conductor; and a step of heat-treating the precursor mixture for forming a solid ion conductor at a temperature of 300°C or lower to manufacture a solid ion conductor comprising a compound represented by the following chemical formula 1:
[0150] <Chemical Formula 1>
[0151] Li a M b In c X d
[0152] In the above chemical formula 1,
[0153] M may be one or more metals selected from metals with an oxidation number of +1 or metals with an oxidation number of +3, and
[0154] X may be one or more elements selected from among halogen elements, and
[0155] 2.5 < a < 3.5, 0 < b < 0.5, 0.5 < c < 1.5, 5 < d < 7.
[0156] The above method for manufacturing a solid ion conductor allows for the easy production of a solid ion conductor at low temperatures that has enhanced ion conductivity, electrochemical stability over a wide potential window when applied to an electrochemical device, and improved charge / discharge characteristics.
[0157] When preparing the above-mentioned precursor mixture for forming a solid ion conductor, a lithium precursor, an M precursor, an indium precursor, and a halogen element precursor may be mixed. The M precursor may be a precursor of a metal element with an oxidation number of +1 or / and a precursor of a metal element with an oxidation number of +3.
[0158] The lithium precursor and the M precursor may include chlorides, halides, oxides, nitrides, oxynitrides, nitrates, hydroxides, and carbonates of lithium. For example, the lithium precursor may be lithium chloride. For example, the M precursor may include chlorides, oxides, nitrides, oxynitrides, nitrates, hydroxides, and carbonates of one element selected from sodium, potassium, rubidium, cesium, silver, gold, copper, mercury, thallium, gallium, scandium, yttrium, lanthanum, lutetium, and gadolinium. For example, the M precursor may be a chloride of one element selected from sodium, potassium, rubidium, cesium, silver, gold, copper, mercury, thallium, and gallium. For example, the M precursor may be a chloride of one element selected from sodium, potassium, copper, and gallium.
[0159] The above compound can be used to prepare a mixture by contacting the starting material in an appropriate amount, for example, a stoichiometric amount. Mechanical milling is performed on the mixture.
[0160] The mechanical milling described above may utilize a ball mill, airjet mill, bead mill, roll mill, planetary mill, hand milling, high energy ball mill, planetary ball mill, stirred ball mill, vibrating mill, mechanofusion milling, shaker milling, planetary milling and atritor milling, disk milling, shape milling, nauta milling, nobilta milling, high speed mix, or a combination thereof. For example, the mechanical milling may be planetary milling and may be performed at room temperature. The method may further include a forming step after performing the mechanical milling.
[0162] Examples and comparative examples of the present invention are described below. However, the following examples are merely one example of the present invention, and the present invention is not limited to the following examples.
[0164] [Example]
[0166] Example 1: Li 2.99 K 0.01 InCl 6 Manufacturing of solid ion conductors
[0167] A precursor mixture for forming a solid-state ion conductor was prepared by introducing and mixing lithium precursor LiCl, potassium precursor KCl, and indium precursor InCl3 into a reactor in a stoichiometric ratio of 2.99:0.01:1. The precursor mixture was obtained by repeatedly performing a cycle of mixing for 10 minutes followed by a 5-minute rest at 500 rpm for a total of 24 hours using a planetary mill (Pulverisette 7 premium line) equipped with 10 mm diameter zirconia (YSZ) balls. The precursor mixture was placed into a 1-inch diameter pelletizer, and a weight of 5 tons was applied using uniaxial pressure for 2 minutes to form LiCl in the shape of a circular disc. 2.99 K 0.01 InCl6 solid ion conductor pellets were prepared.
[0168] Example 2: Li 2.97 K 0.03 InCl 6 Manufacturing of solid ion conductors
[0169] Except for adjusting the lithium precursor LiCl, the potassium precursor KCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.97:0.03:1, Li was prepared in the same manner as in Example 1. 2.97 K 0.03 InCl6 solid ion conductor pellets were prepared.
[0170] Example 3: Li 2.95 K 0.05 InCl 6 Manufacturing of solid ion conductors
[0171] Except for adjusting the lithium precursor LiCl, the potassium precursor KCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.95:0.05:1, Li was prepared in the same manner as in Example 1.2.95 K 0.05 InCl6 solid ion conductor pellets were prepared.
[0172] Example 4: Li 2.9 K 0.1 InCl 6 Manufacturing of solid ion conductors
[0173] Except for adjusting the lithium precursor LiCl, the potassium precursor KCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.9:0.1:1, Li was prepared in the same manner as in Example 1. 2.9 K 0.1 InCl6 solid ion conductor pellets were prepared.
[0174] Example 5: Li 2.99 Cu 0.01 InCl 6 Manufacturing of solid ion conductors
[0175] Except for adjusting the lithium precursor LiCl, the copper precursor CuCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.99:0.01:1, Li was prepared in the same manner as in Example 1. 2.99 Cu 0.01 InCl6 solid ion conductor pellets were prepared.
[0176] Example 6: Li 2.95 Cu 0.05 InCl 6 Manufacturing of solid ion conductors
[0177] Except for adjusting the lithium precursor LiCl, the copper precursor CuCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.95:0.05:1, Li was prepared in the same manner as in Example 1. 2.95 Cu 0.05 InCl6 solid ion conductor pellets were prepared.
[0178] Example 7: Li 2.7 Cu 0.3 InCl 6 Manufacturing of solid ion conductors
[0179] Except for adjusting the lithium precursor LiCl, the copper precursor CuCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.7:0.3:1, Li was prepared in the same manner as in Example 1. 2.7 Cu 0.3 InCl6 solid ion conductor pellets were prepared.
[0180] Example 8: Li 2.97 Na 0.03 InCl 6 Manufacturing of solid ion conductors
[0181] Except for adjusting the lithium precursor LiCl, the sodium precursor NaCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.97:0.03:1, Li was prepared in the same manner as in Example 1. 2.97 Na 0.03 InCl6 solid ion conductor pellets were prepared.
[0182] Example 9: Li 2.95 Na 0.05 InCl 6 Manufacturing of solid ion conductors
[0183] Except for adjusting the lithium precursor LiCl, the sodium precursor NaCl, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.95:0.05:1, Li was prepared in the same manner as in Example 1. 2.95 Na 0.05 InCl6 solid ion conductor pellets were prepared.
[0184] Example 10: Li 2.95 K 0.05 In 0.95 Ga 0.05 Cl 6 Manufacturing of solid ion conductors
[0185] Except for adjusting the lithium precursor LiCl, potassium precursor KCl, indium precursor InCl3, and gallium precursor GaCl3 in the reactor at a stoichiometric ratio of 2.95:0.05:0.95:0.05, Li was prepared in the same manner as in Example 1. 2.95 K 0.05 In 0.95 Ga 0.05 Cl6 solid ion conductor pellets were manufactured.
[0186] Example 11: Li 2.95 K 0.05 InCl 5 Br Manufacturing of solid ion conductors
[0187] Except for adjusting the lithium precursor LiCl, the potassium precursor KBr, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.95:0.05:1, Li was prepared in the same manner as in Example 1. 2.95 K 0.05 InCl5Br Solid ion conductor pellets were manufactured.
[0188] Comparative Example 1: Li 3 InCl 6 Manufacturing of solid ion conductors
[0189] Li3InCl6 solid ion conductor pellets were prepared in the same manner as in Example 1, except that the lithium precursor LiCl and the indium precursor InCl3 were placed in a reactor in a stoichiometric ratio of 3:1.
[0190] Comparative Example 2: Li 2.8 Mg 0.1 In 0.9 Cl 6 Manufacturing of solid ion conductors
[0191] Except for adjusting the lithium precursor LiCl, the magnesium precursor MgCl2, and the indium precursor InCl3 in the reactor at a stoichiometric ratio of 2.8:0.1:1, Li was prepared in the same manner as in Example 1. 2.8 Mg 0.1 InCl6 solid ion conductor pellets were prepared.
[0193] Example 12: Preparation of an all-solid-state secondary battery
[0194] (Manufacturing of the cathode layer)
[0195] A cathode layer was prepared by placing a Cu current collector with a thickness of 10 μm on the bottom surface of a tubular cell case with an inner diameter of 13 mm, and sequentially placing a foil with a thickness of 20 μm of In deposited on one surface of the Cu current collector.
[0196] (Manufacturing of cathode layer / solid electrolyte layer laminate)
[0197] Li prepared according to Example 1 on the above cathode layer 2.99 K 0.01 150 mg of InCl6 solid ion conductor pellets were placed, and 250 MPa was applied at 25°C using the Cold Isotactic Pressing (CIP) method to form a Cu current collector layer / In layer / Li 2.99 K 0.01 A laminate of InCl6 solid electrolyte layers (thickness: approximately 500 μm) was prepared.
[0198] (Manufacturing of the anode layer)
[0199] LiNi as a positive electrode active material 0.9 Co 0.07 Mn 0.03 O2(NCM), Li prepared according to Example 1 as a solid electrolyte 2.99 K 0.01 InCl6 solid ion conductor pellets and carbon nanofibers (CNF) as a conductive agent were mixed in a mass ratio of 60:35:5. 15 mg of the mixture was placed on an 18 μm thick aluminum foil current collector to prepare an anode layer.
[0200] (Manufacturing of all-solid-state secondary batteries)
[0201] A torque cell type all-solid-state secondary battery was manufactured by placing the anode layer on the above cathode layer / solid electrolyte layer laminate and applying a weight of 4 tons for 2 minutes.
[0202] Examples 13 to 22: Preparation of all-solid-state secondary batteries
[0203] An all-solid-state secondary battery was manufactured in the same manner as in Example 12, except that the solid-state ion conductor pellets prepared according to Examples 2 to 11 were used.
[0204] Comparative Examples 3 to 4: Manufacturing of all-solid-state secondary batteries
[0205] An all-solid-state secondary battery was manufactured in the same manner as in Example 12, except that solid-state ion conductor pellets prepared according to Comparative Examples 1 and 2 were used.
[0207] Example 23: Preparation of an all-solid-state secondary battery
[0208] (Manufacturing of the cathode layer)
[0209] A cathode layer was prepared by placing a Cu current collector with a thickness of 10 μm on the bottom surface of a tubular cell case with an inner diameter of 13 mm, and sequentially placing a foil with a thickness of 20 μm of Li deposited on one surface of the Cu current collector.
[0210] (Preparation of solid electrolyte layer)
[0211] An argyrodite-type Li6PS5Cl solid ion conductor pellet (Mitusi, S33) was prepared.
[0212] (Manufacturing of cathode layer / solid electrolyte layer laminate)
[0213] 150 mg of the azirodite-type Li6PS5Cl solid ion conductor pellet was placed on the above cathode layer, and 250 MPa was applied at 25°C by cold isotactic pressing (CIP) to prepare a Cu current collector layer / Li layer / Li6PS5Cl solid electrolyte layer (thickness: about 500 μm).
[0214] (Manufacturing of the anode layer)
[0215] LiNi as a positive electrode active material 0.8 Co 0.15 Mn 0.05 O2(NCM), Li prepared according to Example 1 as a solid electrolyte 2.99 K 0.01 InCl6 solid ion conductor pellets, LiF as an ion-conducting inorganic material, and carbon nanofibers (CNF) as a conductive agent were mixed in a mass ratio of 60:30:5:5. An anode layer was prepared by placing 15 mg of the mixture onto an 18 μm thick aluminum foil current collector.
[0216] (Manufacturing of all-solid-state secondary batteries)
[0217] A torque cell type all-solid-state secondary battery was manufactured by placing the anode layer on the above cathode layer / solid electrolyte layer laminate and applying a weight of 4 tons for 2 minutes.
[0218] Examples 24 to 33: Preparation of all-solid-state secondary batteries
[0219] An all-solid-state secondary battery was manufactured in the same manner as in Example 23, except that solid-state ion conductor pellets prepared according to Examples 2 to 11 were used.
[0220] Comparative Examples 5 to 6: Manufacturing of all-solid-state secondary batteries
[0221] An all-solid-state secondary battery was manufactured in the same manner as in Example 23, except that solid-state ion conductor pellets manufactured according to Comparative Examples 1 and 2 were used.
[0223] Analysis Example 1: XRD Experiment
[0224] XRD spectral experiments using CuKα rays were performed on the solid ion conductor compounds prepared according to Examples 1 to 4 and Comparative Example 1. The XRD spectral experiments were conducted at a rate of 5° / min in the range of a diffraction angle 2θ of 25° to 60°. Part of the results are shown in Fig. 5. Fig. 6 shows the results of magnifying the diffraction peaks in the region where the diffraction angle 2θ is 51.5° to 52.0° in the XRD spectrum.
[0225] As shown in FIG. 5, it was confirmed that all solid ion-conducting compounds prepared according to Examples 1 to 4 have diffraction peaks in regions where the diffraction angle 2θ is 28° to 29°, 29° to 30°, 32.5° to 35°, 37° to 38.5°, 42.5° to 45°, 47.5° to 50°, and 51.5° to 52.0°. From this, it was confirmed that all solid ion-conducting compounds prepared according to Examples 1 to 4 have K + It can be seen that even if substituted with cations, there is no change in the crystal structure, and it belongs to the C2 / m space group or the C2 / m-like space group.
[0226] As shown in FIG. 6, it was confirmed that the diffraction peaks of the solid ion conductor compounds prepared according to Examples 1 to 3 were shifted to the left in the region where the diffraction angle 2θ was 51.5° to 52.0° compared to the Li3InCl6 solid ion conductor compound prepared according to Comparative Example 1. From this, it can be seen that the crystal lattice size of the solid ion conductors prepared according to Examples 1 to 3 increased compared to the Li3InCl6 solid ion conductor.
[0228] Evaluation Example 1: Measurement of ion conductivity
[0229] Solid-state ion conductor pellets with a thickness of approximately 700 μm were prepared according to Examples 1 to 11 and Comparative Examples 1 to 2, respectively. Platinum (Pt) electrodes were formed by depositing a 10 nm thick platinum (Pt) paste on both sides of the solid-state ion conductor pellets using the sputtering method. Wires were connected to the platinum (Pt) electrodes on both sides of the specimens, and analysis was performed using electrochemical impedance spectroscopy (EIS). The amplitude was approximately 10 mV, and the frequency was 0.1 Hz to 10 6 The test was conducted in the Hz range. The impedance of the pellet was measured at room temperature (25°C) using the 2-probe method with a potentiostat / galvanostat and a 1455 frequency response analyzer (FRA) multi-channel test module (Solatron Analytical, UK) as the impedance analyzer. The resistance value was determined from the arc of the Nyquist plot of the impedance measurement results, and the ionic conductivity was calculated by correcting for the electrode area and pellet thickness. The results are shown in Table 1 below.
[0230] Ionic conductivity (S / cm, @ 25℃) Example 1 6.0 X10 -4 Example 2 5.3 X10 -4 Example 3 1.4 X10 -3 Example 4 8.3 X10 -4 Example 5 1.2 X10 -3 Example 6 1.1 X10 -3 Example 7 7.4 X10 -4 Example 8 1.1 X10 -3 Example 9 7.5 X10 -4 Example 10 1.1 X10 -3 Example 11 1.0 X10 -3 Comparative Example 1 3.4 X10 -4 Comparative Example 2 2.7 X10 -4
[0231] As shown in Table 1, the solid ion conductors prepared according to Examples 1 to 11 had higher ion conductivity compared to the solid ion conductors prepared according to Comparative Examples 1 to 2, and 3.5 x 10 -4 S·cm -1 The above ionic conductivity was shown.
[0233] Evaluation Example 2: Charge / Discharge Experiment
[0234] Evaluation Example 2-1: (Initial) Discharge Capacity
[0235] The initial discharge capacity was tested on the all-solid-state secondary batteries prepared according to Example 14 and Comparative Example 3. The cutoff potential was 4.0 V to 2.0 V (vs. Li / Li + ) and a constant current of 0.1 C was applied. The discharge current was performed under conditions of 0.01 C, 0.05 C, 0.5 C, 0.75 C, and 1.0 C at the constant current (CC), respectively. The results are shown in FIG. 7. In addition, the results of performing the discharge under the condition that the discharge current was 0.05 C at the constant current are shown in FIG. 8 and FIG. 9.
[0236] As shown in Fig. 7, the all-solid-state secondary battery manufactured according to Example 14 had a larger initial discharge capacity compared to the all-solid-state secondary battery manufactured according to Comparative Example 3.
[0237] As shown in FIG. 8, the all-solid-state secondary battery prepared according to Example 14 achieved a discharge capacity of 175 mAh / g or more under conditions where the discharge current is 0.05 C. As shown in FIG. 9, the all-solid-state secondary battery prepared according to Comparative Example 3 achieved a discharge capacity of 135 mAh / g or less under the same discharge current conditions.
[0238] Evaluation Example 2-2: Life Characteristics
[0239] Lifetime characteristics were evaluated for the all-solid-state secondary batteries prepared according to Example 25 and Comparative Example 5. Lifetime characteristics were evaluated by the following charge-discharge test.
[0240] One cycle was defined as charging with a constant current of 0.1 C until the battery voltage reached 4.0 V, and then discharging with a constant current of 0.1 C until the battery voltage reached 2.0 V. The results of repeating the above one cycle of charging and discharging are shown in FIG. 10. The capacity retention rate was calculated using Equation 2 below and is shown in Table 3 below.
[0241] <Equation 2>
[0242] Capacity retention rate (%) = [30 th Discharge capacity per cycle / 1 st Discharge capacity per cycle] x 100
[0243] Dose retention rate (%) Example 25 99.5% Comparative Example 5 99.3%
[0244] As shown in Table 3, the all-solid-state secondary battery prepared according to Example 25 had a higher capacity retention rate compared to the all-solid-state secondary battery prepared according to Comparative Example 5.
[0245] As shown in FIG. 10, the all-solid-state secondary battery prepared according to Example 25 operated stably with a discharge capacity of 149 mAh / g or more up to 30 cycles. In comparison, the all-solid-state secondary battery prepared according to Comparative Example 5 also operated stably up to 30 cycles, but the discharge capacity was 120 mAh / g or less. Explanation of the symbols
[0246] 1, 1a: All-solid-state secondary battery 10: Cathode layer 11: Positive current collector 12: Positive active material layer 20: Cathode layer 21: Cathode current collector 22: Cathode active material layer 23: Metal layer 24: Thin film 30: Solid electrolyte layer 100: In 3+ or In substituted with a metal element other than In (M or M2) having an oxidation number of +3. 3+ , 200: Cl - , 300: Li + or Li substituted with a metal element other than lithium (M or M1) having an oxidation number of +1. +
Claims
Claim 1 Solid ionic conductor comprising a compound represented by the following chemical formula 1: <Chemical Formula 1>Li a M b In c X d In the above chemical formula 1, M is one or more metals selected from Na, K, Rb, Cs, Ag, Au, Cu, Hg, Tl, Ga, Sc, La, or Lu, X is one or more elements selected from halogen elements, and 2.5 < a < 3.5, 0 < b ≤ 0.3, 0.5 < c < 1.5, 5 < d < 7. Claim 2 In claim 1, the solid ionic conductor comprising a compound represented by the following chemical formula 2: <Chemical Formula 2>Li x-y (M1) y In 1-z (M2) z X' w In the above chemical formula 2, M1 is a metal with an oxidation number of +1 having an ionic radius of 76 pm or more, M2 is a metal with an oxidation number of +3, X' is one or more elements selected from halogen elements, and 3 < x < 4, 0 < y < 0.5, 0 < z < 0.5, 5 < w < 7, 2.5 < xy < 3.
5. Claim 3 In claim 1, the compound is a solid ion conductor having a distorted rock-salt type structure. Claim 4 A solid ion conductor according to claim 1, wherein the compound is a crystal structure having lithium ion transport channels extended in the x-axis, y-axis, and z-axis directions in a spatial distribution according to the ionic radius of the M element. Claim 5 A solid ion conductor according to claim 1, wherein the compound comprises a crystal structure belonging to the C2 / m space group or the C2 / m-like space group. Claim 6 In claim 1, the compound is a solid ion conductor in which the peak appearing in the region where the diffraction angle 2θ obtained by the XRD spectrum using CuKα-rays is 51.5° to 52.0° is shifted to the left compared to the Li3InCl6 compound. Claim 7 delete Claim 8 A solid ion conductor according to claim 1, wherein X is Cl, Br, I, or a combination thereof. Claim 9 delete Claim 10 A solid ion conductor according to claim 1, wherein 0.7 < c < 1.2 in the above chemical formula 1. Claim 11 In claim 1, the compound is Li 3-p K p InCl6(0 < p ≤ 0.3), Li 3-p Cu p InCl6(0 < p ≤ 0.3), Li 3-p Na p InCl6(0 < p ≤ 0.3), Li 3-p Rb p InCl6(0 < p ≤ 0.3), Li 3-p Cs p InCl6(0 < p ≤ 0.3), Li 3-p Ag p InCl6(0 < p ≤ 0.3), Li 3-p Hg p InCl6(0 < p ≤ 0.3), Li 3-p Tl p InCl6(0 < p ≤ 0.3), Li 3-p K p InCl5Br (0 < p ≤ 0.3), Li 3-p Cu p InCl5Br (0 < p ≤ 0.3), Li 3-p Na p InCl5Br (0 < p ≤ 0.3), Li 3-p Rb p InCl5Br (0 < p ≤ 0.3), Li 3-p Cs p InCl5Br (0 < p ≤ 0.3), Li 3-p Ag p InCl5Br (0 < p ≤ 0.3), Li 3-p Hg p InCl5Br (0 < p ≤ 0.3), Li 3-p Tl p InCl5Br (0 < p ≤ 0.3), Li 3-p K p InClBr5(0 < p ≤ 0.3), Li 3-p Cu p InClBr5(0 < p ≤ 0.3), Li 3-p The p InClBr5(0 < p ≤ 0.3), Li 3-p Rb p InClBr5(0 < p ≤ 0.3), Li 3-p Cs p InClBr5(0 < p ≤ 0.3), Li 3-p Ag p InClBr5(0 < p ≤ 0.3), Li 3-p Hg p InClBr5(0 < p ≤ 0.3), Li 3-p Tl p InClBr5(0 < p ≤ 0.3), Li 3-p K p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p The p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Rb p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cs p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Ag p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Hg p You 1-q Ga q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Tl p And 1-q Him q Cl6(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p K p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cu p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p On p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Rb p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cs p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Ag p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Hg p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Soil p And 1-q Him q Cl5Br (0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p K p And 1-q Him q ClBr5(0 < p ≤ 0.3, 0 < q ≤ 0.3), Li 3-p Cu p And 1-q Him q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Na p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Rb p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Cs p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Ag p In 1-q Ga q ClBr5(0 <p ≤ 0.3, 0 <q ≤ 0.3), Li 3-p Hg p In 1-q Ga q ClBr5(0 < p ≤ 0.3, 0 < q ≤ 0.3), or Li 3-p Tl p In 1-q Ga q A solid ion conductor comprising one or more compounds selected from ClBr5 (0 < p ≤ 0.3, 0 < q ≤ 0.3). Claim 12 In claim 1, the solid ion conductor is 3.5 x 10 at 25°C -4 S·cm -1 A solid ion conductor having an ion conductivity greater than or equal to the above. Claim 13 A solid electrolyte comprising a solid ion conductor according to any one of claims 1 to 6, 8, and 10 to 12. Claim 14 In claim 13, the solid electrolyte is an electrochemically stable solid electrolyte in a voltage window of 0.6 V to 4.2 V (vs. Li). Claim 15 An electrochemical device comprising an anode layer, a cathode layer, and a solid electrolyte layer, and a solid electrolyte according to claim 14. Claim 16 An electrochemical device according to claim 15, wherein the solid electrolyte comprises the solid electrolyte layer, the anode layer, the cathode layer, the anode layer protective film, the cathode layer protective film, or a combination thereof. Claim 17 In claim 15, the electrochemical device comprising a solid electrolyte layer comprising a solid electrolyte, a sulfide-based solid electrolyte, or a combination thereof. Claim 18 In claim 17, the electrochemical device comprising a solid electrolyte represented by the following chemical formula 3, wherein the sulfide-based solid electrolyte is: <Chemical Formula 3>Li + 12-n-r A n+ X 2- 6-r Y' - r In the above chemical formula 3, A is P, As, Ge, Ga, Sb, Si, Sn, Al, In, Tl, V, Nb, or Ta, X is S, Se, or Te, Y' is Cl, Br, I, F, CN, OCN, SCN, or N3, and 1 < n < 5, 0 < r < 2. Claim 19 In claim 15, an electrochemical device having a thickness of 10 micrometers (㎛) to 1 millimeter (㎜) of the solid electrolyte layer. Claim 20 An electrochemical device according to claim 15, wherein the anode layer comprises an anode active material selected from lithium transition metal oxide, lithium transition metal phosphate, sulfide, or a combination thereof, and the solid electrolyte. Claim 21 An electrochemical device according to claim 20, wherein cation mixing occurs in which a metal ion with an oxidation state of +1 is inserted into the lithium ion transport path during the charging and discharging process of the above-mentioned positive active material. Claim 22 In claim 15, the electrochemical device wherein the anode layer further comprises an ion-conducting inorganic material. Claim 23 In claim 15, the electrochemical device wherein the cathode layer comprises a metal-based cathode active material, a carbon-based cathode active material, or a combination thereof. Claim 24 In paragraph 15, the electrochemical device is an all-solid-state secondary battery or a metal-air battery. Claim 25 A method for manufacturing a solid ion conductor comprising: a step of preparing a precursor for forming a solid ion conductor; a step of performing mechanical milling on the precursor for forming a solid ion conductor to provide a precursor mixture for forming a solid ion conductor; and a step of heat-treating the precursor mixture for forming a solid ion conductor at a temperature of 300°C or lower to manufacture a solid ion conductor comprising a compound represented by the following chemical formula 1: <Chemical Formula 1>Li a M b In c X d In the above chemical formula 1, M is one or more metals selected from Na, K, Rb, Cs, Ag, Au, Cu, Hg, Tl, Ga, Sc, La, or Lu, X is one or more elements selected from halogen elements, and 2.5 < a < 3.5, 0 < b ≤ 0.3, 0.5 < c < 1.5, 5 < d < 7. Claim 26 A method for manufacturing a solid ion conductor according to claim 25, wherein the mechanical milling is a ball mill, airjet mill, bead mill, roll mill, planetary mill, hand milling, high energy ball mill, planetary mill ball mill, stirred ball mill, vibrating mill, mechanofusion milling, shaker milling, planetary milling, atritor milling, disk milling, shape milling, nauta milling, nobilta milling, high speed mix, or a combination thereof. Claim 27 In claim 25, the mechanical milling is planetary milling and is a method for manufacturing a solid ion conductor performed at room temperature. Claim 28 A method for manufacturing a solid ion conductor according to claim 25, further comprising the step of forming after performing the above mechanical milling.
Citation Information
Patent Citations
Solid electrolyte material and battery using the same
JP2020109047A