Method for manufacturing a vacuum-deposited rudorffite absorber and method for manufacturing a photovoltaic device comprising the same
Vacuum deposition of BiI3 and AgI powders with heat treatment and anhydrous PEDOT layers addresses the challenge of precise thickness control and large-area production of AgBiI-based photovoltaic devices, enhancing efficiency and uniformity.
Patent Information
- Application Number
- KR1020250061673
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-05-13
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2045-05-13
AI Technical Summary
Existing methods for manufacturing lead-free perovskite-like absorbers, such as AgBiI-based compounds, lack efficient vapor deposition processes for precise thickness control and large-area production, limiting their application in translucent devices for energy harvesting.
A method involving vacuum deposition of BiI3 and AgI powders to form an AgBiI4 layer, combined with a two-stage heat treatment for electron transport layers and use of anhydrous PEDOT for hole transport layers, enabling precise thickness control and uniform deposition on large substrates.
Enables precise nanometer-level thickness control and uniform deposition, facilitating mass production of efficient photovoltaic devices with improved efficiency and uniformity.
Smart Images

Figure 112025053088421-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing a vacuum-deposited ludorpite light absorber and a method for manufacturing a photovoltaic device including the same. More specifically, the invention relates to a method for manufacturing a light absorber capable of precise thickness control and large-area mass production through a vacuum deposition method, and a method for manufacturing a photovoltaic device including the same. Background Technology
[0002] With the advancement of Internet of Things (IoT) technology, the demand for self-powered and wireless devices is increasing. To operate without an external power supply, these devices require energy harvesting technology to collect energy from the surrounding environment; in particular, indoor lighting is attracting attention as an accessible and highly versatile ambient energy source.
[0003] In the development of optoelectronic devices utilizing such indoor light sources, organic-inorganic hybrid perovskite materials have been widely studied as light absorbers suitable for indoor photovoltaics (IPV) applications as well as outdoor ones, based on their excellent light absorption performance and high photoelectric conversion efficiency (PCE).
[0004] However, the toxicity of lead (Pb) contained in conventional perovskites is cited as a major factor hindering commercialization, particularly in relation to safety in indoor environments. Accordingly, the development of non-toxic and lead-free alternative absorbers is emerging as a key technology for the realization of IPV.
[0005] Against this backdrop, Rudorffite-based compounds (ABI) with various AgI:BiI3 compositional ratios, such as AgBi2I7, AgBiI4, Ag2BiI5, and Ag3BiI6, have been proposed as lead-free perovskite-like absorbers.
[0006] These ABI-type compounds possess a wide bandgap, enabling efficient light absorption within the indoor lighting spectrum and consequently achieving a high open-circuit voltage, thereby providing advantageous characteristics for optoelectronic devices for indoor lighting.
[0007] Meanwhile, although solution processes have been widely used as a method for manufacturing such light-absorbing layers, vapor deposition processes have advantages in that they enable precise control of thin film thickness, ease of forming multilayer structures, securing uniform thin films, and large-area mass production.
[0008] Furthermore, since the use of a vapor deposition process enables the precise formation of a thin light-absorbing layer, it is advantageous for the development of translucent devices that transmit a portion of incident light. The development of efficient translucent devices can also be effectively applied to specialized applications, such as integration into windows to harvest energy without significantly compromising transparency.
[0009] However, despite the advantages of the vapor deposition process mentioned above, research applying the vapor deposition process to fabricate ABI-based thin films has been very limited to date, and technological development in this area is required. The problem to be solved
[0010] The first technical problem to be achieved by the present invention is to provide a method for manufacturing a vacuum-deposited ludorpite light absorber.
[0011] In addition, the second technical objective of the present invention is to provide a method for manufacturing a photovoltaic device comprising a vacuum-deposited loudorfite light absorber. means of solving the problem
[0012] The present invention, for achieving the first technical objective described above, provides a method for manufacturing a vacuum-deposited rhodophyte light absorber comprising the steps of: supplying each of the separated BiI3 powder and AgI powder into a vacuum chamber; evaporating the supplied BiI3 powder and AgI powder using an evaporation source and forming a deposition layer of BiI3 and AgI on a substrate; and heat-treating the deposition layer of BiI3 and AgI to form an AgBiI4 layer.
[0013] The present invention, for achieving the second technical objective described above, provides a method for manufacturing a ludorpite photovoltaic device comprising the steps of: forming an electron transport layer on top of a first electrode; forming a light absorption layer on the electron transport layer; forming a hole transport layer on the light absorption layer; and forming a second electrode on the hole transport layer, wherein the step of forming the light absorption layer comprises: supplying each of the separated BiI3 powder and AgI powder into a vacuum chamber; evaporating the supplied BiI3 powder and AgI powder using an evaporation source and forming a deposited layer of BiI3 and AgI on the electron transport layer; and heat-treating the deposited layer of BiI3 and AgI to form an AgBiI4 layer. Effects of the invention
[0014] According to the present invention, a method for manufacturing a vacuum-deposited loudorpite light absorber and a method for manufacturing a photovoltaic device including the same are provided. Through this, not only can the deposition thickness be precisely controlled at the nanometer level, but uniform deposition on a large-area substrate is also possible, making mass production easier. Accordingly, the efficiency of the production process and the uniformity of the product can be improved. Brief explanation of the drawing
[0015] FIG. 1 is a schematic diagram showing the structure of a sequential deposition method according to one embodiment of the present invention and a loudorfite photovoltaic device manufactured therefrom. Figure 2 shows the transmission spectrum, photograph, and cross-sectional SEM image of a PEDOT / AgBiI4 / c-TiO2 / ITO coated glass thin film prepared according to one embodiment of the present invention. FIG. 3 shows the XRD pattern, absorption spectrum, and emission power spectrum of a WLED (6500K) of an AgBiI4 thin film prepared according to one embodiment and one comparative example of the present invention. Figure 4 shows the JV curve of a device having the highest performance under 1 sun and 1000 lx irradiance manufactured according to one embodiment and one comparative example of the present invention. Figure 5 shows the stability of a device manufactured according to one embodiment of the present invention. Specific details for implementing the invention
[0016] The present invention is susceptible to various modifications and may take various forms; therefore, specific embodiments are illustrated in the drawings and described in detail in the text. However, this is not intended to limit the invention to the specific disclosed forms, and it should be understood that the invention includes all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention. Similar reference numerals have been used for similar components in the description of each drawing.
[0017] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as generally understood by those skilled in the art to which the present invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this application.
[0018] Hereinafter, preferred embodiments of the present invention will be described in more detail with reference to the attached drawings.
[0020] Examples
[0021] One aspect of the present invention provides a method for manufacturing a vacuum-deposited rudorfite light absorber.
[0022] First, when the BiI3 powder and AgI powder supplied into the vacuum chamber are evaporated, the vaporized AgI and BiI3 are transferred to the surface of the substrate inside the vacuum chamber, and a deposited layer of AgI and BiI3 is formed.
[0023] At this time, the deposited layers of AgI and BiI3 can sequentially form individual layers, or they can form a mixed single layer.
[0024] After reaching the substrate surface, vaporized AgI and BiI3 molecules are fixed in a temporary stable state through physical or chemical adsorption.
[0025] Subsequently, as ions diffuse along the surface, thermodynamically stable nuclei begin to form. Following nucleation, interfacial reactions continuously occur along with the movement of surrounding adsorbed ions and particles, leading to particle growth.
[0026] Subsequently, when heat treatment is performed, an AgBiI4 crystal thin film is formed on the substrate surface.
[0027] Another aspect of the present invention provides a method for manufacturing a loudorfite photovoltaic device.
[0028] First, an electron transport layer is formed on the first electrode. At this time, a solution of isopropanol-based titanium diisopropoxide bis(acetylacetonate) diluted in n-butanol is spin-coated onto the first electrode and subjected to a two-step heat treatment to form a dense crystalline TiO2 (c-TiO2) layer.
[0029] When undergoing the first stage of heat treatment after spin coating, TiO2 may contain impurities such as organic matter or solvents in an amorphous structure, and in this state, electron transfer may be hindered by impurities, and electron transfer efficiency decreases.
[0030] Subsequently, through a two-stage heat treatment, the amorphous TiO2 is converted into crystalline TiO2 at high temperatures, and an anatase structure is formed. During this process, organic materials, solvents, and moisture vaporize or decompose to be converted into pure TiO2, and as a dense and uniform layer is formed, pinholes or pores are eliminated and adhesion to the substrate is improved. This helps with the efficient transfer of electrons and the blocking of leakage current.
[0031] Next, a light absorption layer is formed on the electron transport layer.
[0032] To form a light-absorbing layer, a vacuum deposition method is used to form a film by evaporating two precursors.
[0033] In the present invention, vacuum deposition is used in combination with a vapor phase process.
[0034] The process of forming solid AgBiI4 through vacuum deposition is as described above.
[0035] Next, a solution containing anhydrous PEDOT is applied onto the light-absorbing layer to form a hole transport layer. In the present invention, a compound containing anhydrous PEDOT refers to a compound in which a compound performing a doping function or a specific function is bonded or mixed with anhydrous PEDOT. This is referred to as an anhydrous PEDOT complex. Hereinafter, in the present invention, expressions such as “containing anhydrous PEDOT” and similar expressions are used interchangeably with the expression “anhydrous PEDOT complex.”
[0036] The above-mentioned anhydrous PEDOT composite refers to a conductive polymer, specifically one that excludes PEDOT:PSS, is not dispersed in water, and is easily dispersed in nonpolar solvents other than water. Additionally, the above-mentioned PEDOT composite may have a form in which a doping agent is bonded to PEDOT.
[0037] Generally, the PEDOT:PSS solution used in the hole transport layer is dispersed in water. On the other hand, Ludorpite AgBiI4 in the light absorption layer is a water-soluble material, and contact with polar solvents such as water can lead to structural instability.
[0038] Specifically, when water molecules penetrate the ludorpite AgBiI4 crystal structure, silver ions (Ag + ) and bismuth ions (Bi 3+ ) dissolves, which can lead to the decomposition of AgBiI4. Also, iodide ions (I - Since it can be dissolved in water, there is a high possibility that changes in the crystal structure and chemical decomposition by water will occur.
[0039] Therefore, there are limitations to applying PEDOT:PSS in a water-dispersed form on top of a water-soluble light-absorbing layer.
[0040] On the other hand, a solution containing anhydrous PEDOT is in a dispersed form in toluene, and since it does not contain water, the above-mentioned problem does not occur even when applied to a water-soluble light-absorbing layer.
[0041] Subsequently, a second electrode is formed on the hole transport layer to manufacture a ludorfite photovoltaic device.
[0042] Embodiments of the present invention will be described in detail below with reference to the attached drawings.
[0043] FIG. 1 is a schematic diagram showing the structure of a sequential deposition method according to one embodiment of the present invention and a loudorfite photovoltaic device manufactured therefrom.
[0044] Referring to FIG. 1, the structure may include ITO coated glass (first electrode), c-TiO2 (electron transport layer), AgBiI4 (light absorption layer), PEDOT (hole transport layer), and Ag (second electrode).
[0045] First, an electron transport layer is formed on the upper part of the first electrode.
[0046] The first electrode may be a glass substrate comprising indium tin oxide (ITO), fluorine-doped tin oxide (FTO), indium zinc oxide (IZO), aluminum-doped zinc oxide (AZO), antimony-doped tin oxide (ATO), or gallium-doped zinc oxide (GZO).
[0047] The electron transport layer may be metal oxides such as TiO2, ZnO, MgO, SiO2, SnO2, WO3, ZrO2, HfO2, Ta2O5, BaTiO3, BaZrO3, Al2O3, Y2O3, or ZrSiO4, but it is preferable to use TiO2 to increase electron transfer efficiency and prevent leakage current.
[0048] To form the above-mentioned electron transport layer, c-TiO2, a TiO2 precursor solution is first formed by diluting titanium isopropoxide or titanium diisopropoxide bis(acetylacetonate) in a solvent such as alcohol. At this time, it is preferable to use a mixed solution of isopropanol-based titanium diisopropoxide bis(acetylacetonate) and n-butanol.
[0049] A TiO2 precursor solution mixed with isopropanol-based titanium diisopropoxide bis(acetylacetonate) and n-butanol is applied to the first electrode and heat-treated to form a dense crystalline TiO2 (c-TiO2) layer.
[0050] Specifically, when applying the above TiO2 precursor solution onto the first electrode, spin coating is preferred, and it is preferred to be performed at 500 rpm to 6000 rpm for 10 seconds to 60 seconds.
[0051] In addition, the heat treatment can be performed in two stages. In the first stage, heat treatment is performed at 80°C to 150°C for 2 to 30 minutes to remove residual solvent, and in the subsequent second stage, heat treatment is performed at 400°C to 600°C for 10 to 60 minutes to induce crystallization of TiO2, and at the same time, a c-TiO2 layer is formed.
[0052] Next, a light absorption layer is formed on the electron transport layer.
[0053] To form a light-absorbing layer, a vacuum deposition method can be used to form a film by evaporating two precursors.
[0054] At this time, the formation of a film via vacuum deposition can be achieved through co-evaporation (codeposition) or sequential deposition. Co-evaporation has the advantage of ensuring fast process times, while sequential deposition has the advantage of enabling precise control of compositional ratios because heat treatment is performed after sequentially depositing each material.
[0055] Therefore, those skilled in the art need to selectively use the two types of methods described in this specification as needed.
[0056] First, AgI powder and BiI3 powder are introduced into an evaporation source as precursors of silver (Ag) and bismuth (Bi).
[0057] Here, the temperature of the evaporation source into which BiI3 powder is introduced may be 250°C to 450°C, and the temperature of the evaporation source into which AgI powder is introduced may be 400°C to 600°C.
[0058] If the temperature of the evaporation source is too low, the material does not vaporize sufficiently, resulting in a very low deposition rate; conversely, if the temperature of the evaporation source is too high, the vaporization rate becomes excessively high, making it difficult to control the film thickness.
[0059] Next, a deposition layer of BiI3 and AgI with a constant thickness is formed while controlling the evaporation rate.
[0060] At this time, the evaporation rate of BiI3 may be 0.1 Å / s to 10 Å / s, and the evaporation rate of AgI may be 0.1 Å / s to 10 Å / s.
[0061] The thickness of the BiI3 layer among the deposition layers formed using a sequential deposition method may be 10 nm to 500 nm, and the thickness of the AgI layer among the deposition layers may be 10 nm to 500 nm.
[0062] In addition, the thickness of the deposition layer formed using the simultaneous deposition method may be 20 nm to 1000 nm.
[0063] If the above range is exceeded, photoelectric performance may be significantly degraded.
[0064] Meanwhile, heat treatment can be performed in the formation of the light absorption layer. The heat treatment 5 to 30 minutes at 100℃ to 300℃ By being performed during, AgBiI4 compounds are formed through interdiffusion and reaction, thereby achieving the effect of improved crystallinity.
[0065] The thickness of the light absorption layer may be 20 nm to 1 µm.
[0066] If the light absorption layer is too thin, sufficient light absorption does not occur, and the photoelectric conversion efficiency (PCE) decreases; if it becomes too thick, the charge transport path becomes longer, increasing charge recombination, which in turn decreases the photoelectric conversion efficiency (PCE).
[0067] Subsequently, a solution containing anhydrous PEDOT is applied onto the light absorption layer to form a hole transport layer.
[0068] The hole transport layer above may include an anhydrous PEDOT complex dispersed in toluene.
[0069] Generally, PEDOT:PSS used in hole transport layers is in a water-dispersed form. On the other hand, the light absorber Ludorpite AgBiI4 is a water-soluble material that reacts readily with water. Due to these characteristics, applying a water-dispersed PEDOT:PSS layer on top of the light absorption layer can affect the structural stability of the light absorption layer.
[0070] To solve the above problem, an anhydrous PEDOT complex dispersed in toluene that does not contain water was used as a hole transport layer material.
[0071] Next, a second electrode is formed on the hole transport layer to manufacture a ludorpite photovoltaic device.
[0072] The second electrode may be aluminum (Al), calcium (Ca), silver (Ag), zinc (Zn), gold (Au), platinum (Pt), copper (Cu), or chromium (Cr), etc.
[0074] Hereinafter, preferred manufacturing examples and measurement examples are presented to aid in understanding the present invention. However, the following manufacturing examples and measurement examples are intended only to aid in understanding the present invention, and the present invention is not limited by the following measurement examples.
[0076] [Manufacturing Example: Manufacture of Ludorpite Photovoltaic Device]
[0077] Preparation of the first electrode
[0078] An ITO (Sn-doped In2O3) coated glass substrate was sequentially cleaned with isopropanol and deionized water in an ultrasonic cleaner.
[0079] Formation of electron transport layer
[0080] 0.12M and 0.24M solutions of isopropanol-based titanium diisopropoxide bis(acetylacetonate) (75 wt% in isopropanol, 55 μL and 110 μL) mixed with n-butanol (1 mL), respectively A dense crystalline TiO2 (compact TiO2, c-TiO2) layer was formed by spin coating on the first electrode at 3000 rpm for 30 seconds, heat treating at 120°C for 5 minutes, and then heat treating at 500°C for 30 minutes.
[0081] Formation of a light absorption layer
[0082] A light absorption layer was formed on the electron transport layer by sequentially evaporating BiI3 powder and AgI powder using two effusion cells heated independently within a vacuum chamber.
[0083] The amount of BiI3 and AgI powders introduced into the evaporation source was fixed at 450 mg to 500 mg, and the evaporation temperature was controlled to maintain the evaporation rates of BiI3 and AgI during deposition at 1.1 Å / s to 1.2 Å / s and 1.0 Å / s to 1.1 Å / s, respectively.
[0084] As a result, a BiI3 layer with a thickness of 45 nm and an AgI layer with a thickness of 35 nm were formed.
[0085] Afterwards, the light absorption layer was heat-treated at 160°C for 15 minutes in a room temperature atmosphere.
[0086] Formation of a hole transport layer
[0087] A hole transport layer was formed by spin-coating an anhydrous PEDOT complex solution (Clevios™ HTL Solar 3; Ossila) dispersed in toluene onto the light-absorbing layer at 3000 rpm for 30 seconds in air.
[0088] Second electrode formation
[0089] Finally, a second electrode was formed by depositing a 150 nm thick Ag layer on the hole transport layer at a rate of 10 Å / s using a thermal evaporation deposition system.
[0091] [Comparative Example 1]
[0092] A photoelectric device was fabricated by performing the same procedure as in the preparation example, except that the light absorption layer was not applied.
[0094] [Comparative Example 2]
[0095] A photovoltaic device was fabricated in the same manner as in the preparation example, except that a BiI3 layer with a thickness of 90 nm and an AgI layer with a thickness of 70 nm were formed, and then heat-treated at 200°C for 15 minutes in a room temperature atmosphere.
[0097] [Measurement Example 1: Structural Analysis of Photovoltaic Devices]
[0098] Figure 2 shows the transmission spectrum, photograph, and cross-sectional SEM image of a PEDOT / AgBiI4 / c-TiO2 / ITO coated glass thin film prepared according to one embodiment of the present invention.
[0099] Here, the light absorption and transmission spectra of the thin film were measured using an ultraviolet-visible (UV-vis) spectrophotometer (V-780; Jasco), and the morphology and thickness of the thin film were measured using a field emission scanning electron microscope (FESEM, S-4300; Hitachi).
[0100] The possibility of a translucent device based on a thin light-absorbing layer formed through a vapor phase process was explored, and the results are shown in Fig. 2. Referring to Fig. 2(a), the transmission spectrum and actual photograph of a PEDOT / AgBiI4 / c-TiO2 thin film deposited on a glass substrate coated with ITO of the preparation example are shown, and the translucency of the AgBiI4 light-absorbing layer prepared by the vapor phase process can be confirmed.
[0101] Referring to Figure 2(b), the thicknesses of AgBiI4 and PEDOT were estimated to be approximately 65 nm each through cross-sectional scanning electron microscope (SEM) images.
[0102] FIG. 3 shows the XRD pattern, absorption spectrum, and emission power spectrum of a WLED (6500K) of an AgBiI4 thin film prepared according to one embodiment and one comparative example of the present invention.
[0103] Here, the crystal structure of the thin film was measured using XRD (MiniFlex 600; Rigaku).
[0104] Referring to Fig. 3(a), AgBiI4 has been reported to have both cubic and hexagonal crystal structures, and the final phase formed varies significantly depending on the synthesis method.
[0105] For example, when synthesized via a solid-state reaction when the composition ratio of Ag / Bi is within the range of 1:1 to 2:1, a hexagonal Ag2BiI5 phase is consistently formed regardless of the initial composition ratio.
[0106] The XRD pattern obtained from the experiment is consistent with the hexagonal Ag2BiI5 structure (JCPDS 35-1025), and a distinct diffraction peak is observed, particularly in the (101) plane. No peaks of the secondary phases, AgI or BiI3, were observed.
[0107] In the energy dispersive spectroscopy (EDS) analysis performed on the AgBiI4 thin film formed via the vapor phase process, the average elemental composition was analyzed to be AgBi(0.96±0.01)I(4.4±0.4).
[0108] Considering the error limits of EDS analysis, the deposition thickness ratio of AgI and BiI3 is determined to have a composition suitable for the formation of AgBiI4.
[0109] Referring to Fig. 3(b), assuming AgBiI4 is a direct bandgap material capable of transitioning only by energy change, the optical bandgap estimated from the Tauc plot of the absorption spectrum was measured to be 1.89 eV in the preparation example.
[0110] In addition, the spectrum of the 6500K WLED is generally concentrated between 400 nm and 700 nm (visible light region), and shows relatively strong output in the blue region (about 450 nm to 490 nm). On the other hand, other colors are included in relatively small amounts, and a red region (600 nm to 700 nm) and a green region (500 nm to 570 nm) are also included.
[0111] In other words, this means that an AgBiI4 light absorber with a wide bandgap can effectively capture the indoor light spectrum concentrated in the visible light region.
[0113] [Measurement Example 2: Verification of Photovoltaic Device Performance]
[0114] In order to evaluate the performance of the optoelectronic devices prepared in the above Preparation Example and Comparative Example 2, the photocurrent density ( J SC , Short-Circuit Current Density), Open-circuit voltage( V OC Open-Circuit Voltage, Fill Factor (FF), and Power Conversion Efficiency (PCE) were measured, and the average and standard deviation of the performance of the optoelectronic device were compared and shown in Figure 4 and Table 1, where the values in parentheses in Table 1 represent the performance values of the highest-performing device.
[0115] Figure 4 shows the JV curve of a device having the highest performance under 1 sun and 1000 lx irradiance manufactured according to one embodiment of the present invention.
[0116] Table 1 summarizes the average photovoltaic parameters (forward scan) measured at 1 sun and 1000 lx for the photovoltaic devices of Manufacturing Example and Comparative Example 2.
[0117] Photoelectric conversion performance was measured using a solar simulator (PEC-L01; Peccell Technologies) and an indoor light test system (K3000 WLED100; Mcscience).
[0118] To observe changes in photoelectric efficiency and determine the causal relationship, the performance was evaluated by applying it to a photoelectric device in a solar light environment (1 sun) and a WLED (White Light Emitting Diode) at 1000 lx.
[0119] Light absorption layer thickness light source J SC (㎃ / ㎠) V OC (V) FF PCE(%) Preparation Example AgI 35 nm BiI 345 nm 1 sun 2.85±0.24(2.81) 0.35±0.11(0.57) 0.42±0.06(0.57) 0.42±0.17(0.91) 1000 lx 0.036±0.004(0.037) 0.18±0.09(0.35) 0.39±0.01(0.55) 0.87±0.62(2.12) Comparative Example 2 AgI 70 nm BiI 390 nm 1 sun 2.85±0.44 0.40±0.08 0.44±0.08 0.53±0.22 1000 lx 0.038±0.006 0.09±0.06 0.27±0.02 0.33±0.26
[0120] Referring to Figure 4 and Table 1, the photocurrent density at 1 sun ( J SC ) is 2.81 mA / cm², open-circuit voltage ( V OC ) was observed to be 0.57V.
[0121] Photocurrent density at 1000 lx ( J SC ) is 37 µA / cm², open-circuit voltage( V OC ) was observed to be 0.35V.
[0122] The packing factor (FF) was observed to be 0.57 at 1 sun and 0.55 at 1000 lx.
[0123] As a result, the photoelectric conversion efficiency (PCE) of the device with the highest performance at 1 sun reached 0.91%, while at 1000 lx it achieved 2.12%, indicating that the PCE was significantly improved under indoor lighting conditions.
[0124] In addition, when the thickness of the light absorption layer was doubled, at 1000 lx V OC The efficiency decreased significantly as FF decreased, indicating severe trap-assisted recombination.
[0125] The reasons for the increase in defects in thick light-absorbing layers are as follows. In sequential deposition, each material is evaporated and deposited individually, after which the desired compound is formed through interdiffusion during heat treatment. In processes requiring interdiffusion, it becomes more difficult for sufficient diffusion to occur as the thickness increases. Consequently, defects may increase due to non-uniform composition, lattice mismatch, and the occurrence of regions where the reaction is incomplete.
[0127] [Measurement Example 3: Verification of Photovoltaic Element Stability]
[0128] Figure 5 shows the stability of a device manufactured according to one embodiment of the present invention.
[0129] The devices were stored without encapsulation under dark room conditions (temperature 20°C to 25°C, relative humidity 25% to 46%), and the data from four devices measured at 1 sun and 1000 lx illuminance were averaged.
[0130] Referring to Figure 5, when measured under 1 sun conditions, the device maintained 75.3% of its initial photoelectric conversion efficiency (PCE) even after 34 days.
[0131] On the other hand, under low light intensity conditions of 1000 lx, faster performance degradation was observed, and after 34 days, only 48.4% of the initial PCE was maintained. This means that the device exhibits higher sensitivity to aging at low light intensity.
[0132] A point to note is the open voltage ( V OC The fact that it did not degrade even after aging suggests that the AgBiI4 light absorption layer was maintained stably.
[0133] Efficiency degradation is mainly due to photocurrent density ( J SC This was attributed to a decrease in ), which was observed under all lighting conditions. Additionally, a decrease in the filling factor (FF) was observed under 1000 lx illuminance conditions, suggesting that the charge extraction efficiency may have decreased due to the deterioration of the charge extraction layers.
[0134] Here, the charge extraction layer can be used in combination with the electron transport layer or the hole transport layer.
[0136] According to the present invention described above, a method for manufacturing a vacuum-deposited loudorpite light absorber and a method for manufacturing a photovoltaic device including the same are provided. Through this, not only can the deposition thickness be precisely controlled at the nanometer level, but uniform deposition on a large-area substrate is also possible, making mass production easier. Accordingly, the efficiency of the production process and the uniformity of the product can be improved.
Claims
Claim 1 delete Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 delete Claim 7 A method for manufacturing a Ludorpite photovoltaic device, comprising the steps of: forming an electron transport layer on a first electrode; forming a light absorption layer on the electron transport layer; forming a hole transport layer by applying a solution containing anhydrous PEDOT dispersed in toluene onto the light absorption layer; and forming a second electrode on the hole transport layer, wherein the step of forming the light absorption layer comprises: supplying each of the separated BiI3 powder and AgI powder into a vacuum chamber; evaporating the supplied BiI3 powder and AgI powder using an evaporation source and forming a deposited layer of BiI3 and AgI on the electron transport layer; and heat-treating the deposited layer of BiI3 and AgI to form an AgBiI4 layer. Claim 8 A method for manufacturing a ludorfite photovoltaic device according to claim 7, wherein the step of forming the electron transport layer comprises: a step of forming a TiO2 precursor solution by mixing isopropanol-based titanium diisopropoxide bis(acetylacetonate) and n-butanol; and a step of forming a dense crystalline TiO2 (c-TiO2) layer by spin-coating the TiO2 precursor solution onto the first electrode and heat-treating it. Claim 9 delete Claim 10 delete Claim 11 A method for manufacturing a ludorpite photovoltaic device according to claim 7, wherein, in the step of forming the light absorption layer, the formation of the deposition layer is implemented through a simultaneous deposition method or a sequential deposition method. Claim 12 A method for manufacturing a loudorfite photovoltaic device according to claim 11, characterized in that the thickness of the BiI3 layer among the deposition layers formed using the above sequential deposition method is 10 nm to 500 nm and the thickness of the AgI layer is 10 nm to 500 nm. Claim 13 A method for manufacturing a loudorfite photovoltaic device according to claim 11, characterized in that the thickness of the deposition layer formed using the above simultaneous deposition method is 20 nm to 1000 nm. Claim 14 A method for manufacturing a loudorfite photovoltaic device according to claim 7, wherein, in the step of forming the light absorption layer, the heat treatment is performed at 100°C to 300°C for 5 minutes to 30 minutes.
Citation Information
Patent Citations
Preparation method and application of novel non-lead-based perovskite film
CN113192843A
Formation of lead-free perovskite film
KR1020180042277A