Hardcoat film
A hard coating layer with specific resin composition and nanoparticles provides flexibility and scratch resistance, addressing the limitations of conventional layers by enabling repeated folding without separation or cracking in flexible display devices.
Patent Information
- Application Number
- KR1020247035610
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-05-03
- Filing Date
- 2022-11-30
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-11-30
AI Technical Summary
Conventional hard coating layers used in flexible display devices lack the combination of flexibility and scratch resistance necessary to withstand repeated folding without separating from the screen or cracking, as materials with high crosslinking density exhibit high shrinkage rates and reduced flexibility.
A hard coating layer composed of a resin composition containing a polyfunctional (meth)acrylic monomer and aliphatic urethane acrylate, with a glass transition temperature between 50°C and 100°C and a loss tangent between 0.07 and 0.15, optionally including metal oxide nanoparticles, to enhance flexibility and scratch resistance.
The hard coating layer can withstand at least 100,000 folds without cracking or losing optical properties, while maintaining excellent scratch resistance and flexibility, even in high-temperature environments.
Smart Images

Figure 112024116356608-PCT00006_ABST
Abstract
Description
Technology Field
[0001] The present disclosure relates to a hard coat film. Background Technology
[0002] Display devices such as liquid crystal displays (LCDs), plasma display panels (PDPs), or organic EL displays (OLEDs) are widely used in smartphones, mobile phones, portable personal computers, and automotive navigation devices. Generally, a protective film is provided on the outermost surface of the screen of a display device to prevent the screen from being scratched. The protective film comprises a substrate and a hard coating layer laminated on the substrate. Conventional hard coating layers are each made of a material having a high crosslinking density.
[0003] Currently, foldable flexible display devices equipped with flexible screens are being developed. Such flexible display devices are required to be folded repeatedly in one or more directions multiple times, such as hundreds of thousands of times. Accordingly, the protective film covering the screen of the flexible display device is also required to have enough flexibility to withstand the aforementioned multiple and repeated folding.
[0004] However, materials with high crosslinking density used in conventional hard coating layers possess hardness but have a high shrinkage rate, resulting in a lack of flexibility. Consequently, when a flexible display device is covered with a protective film having a conventional hard coating layer and the device is repeatedly folded over a number of cycles, such as hundreds of thousands, the hard coating layer and the protective film are prone to separating from the screen. Furthermore, if the crosslinking density of the hard coating layer material is high, the hard coating layer may break or crack even if the thickness of the hard coating layer itself is thin.
[0005] Thus, as a flexible hard coating layer, for example, Patent Document 1 discloses a hard coating layer with a thickness of 5 μm that can be bent without cracking around a mandrel with a diameter of 2 mm. Prior art literature
[0006] US 2009 / 0004478 A1 The problem to be solved
[0007] However, the above-mentioned patent document 1 does not disclose anything regarding repeatedly folding a hard coating layer multiple times, such as tens of thousands of times, the material of the hard coating layer required for such repeated folding, or the characteristics of the hard coating layer.
[0008] In addition, if the hard coating layer is made of a soft material to enable multiple foldings, the scratch resistance of the hard coating layer is reduced, and consequently, the hard coating layer becomes prone to scratching. Therefore, the hard coating layer used as a protective film for a flexible display device is required to have not only the performance to withstand multiple and repetitive foldings as described above, but also scratch resistance to prevent scratches.
[0009] Accordingly, the present invention has been made in consideration of the above-mentioned problems and aims to provide a hard coat film that combines performance capable of withstanding multiple and repetitive folding with scratch resistance. means of solving the problem
[0010] In order to solve the above problem, according to an embodiment of the present invention,
[0011] Listing; and
[0012] A hard coating layer laminated on a substrate comprising a cured product of a resin composition containing resin (A) and resin (B).
[0013] Includes,
[0014] Resin (A) is a polyfunctional (meth)acrylic monomer having a weighted average of 4 or more functional groups, and
[0015] The resin (B) is an aliphatic urethane acrylate, and
[0016] The glass transition temperature Tg of the hard coating layer is 50°C or higher and 100°C or lower, and
[0017] The loss tangent tangent tanδ at the glass transition temperature Tg is greater than or equal to 0.07 and less than or equal to 0.15, and
[0018] A hard coat film is provided, wherein the loss tangent tangent tanδ of the hard coating layer is measured by dynamic viscoelasticity measurement applying a dynamic load at a frequency of 1 Hz.
[0019] The resin composition may also additionally contain metal oxide nanoparticles having an average particle size of 100 nm or less.
[0020] In certain embodiments, the content of metal oxide nanoparticles contained in the resin composition may be 2 mass% or more and 5 mass% or less of the total solid content of the resin composition of the hard coating layer.
[0021] The metal oxide within the metal oxide nanoparticles can be either silica or alumina, or both.
[0022] Metal oxide nanoparticles can have a Mohs hardness greater than 6.
[0023] When abrasion is performed on the surface of a hard coating layer using a steel wool #0000 under conditions of load: 1000 g, speed: 50 mm / sec, reciprocating distance: 40 mm, and number of reciprocating cycles: 2500, the water contact angle of the surface of the hard coating layer after abrasion may be greater than 100°.
[0024] In certain embodiments, the water contact angle of the surface of the hard coating layer before wear may be greater than 110°.
[0025] In certain embodiments, the reduction in the water contact angle after wear relative to the water contact angle of the surface of the hard coating layer before wear may be less than 13%.
[0026] In a specific embodiment, the content of resin (A) contained in the resin composition may be greater than 2 times and less than 9 times the content of resin (B).
[0027] In a specific embodiment, the content of resin (A) contained in the resin composition may be 20 mass% or more and 40 mass% or less, and the content of resin (B) contained in the resin composition may be 2 mass% or more and 15 mass% or less.
[0028] The hard coat film may be configured to be foldable by either inbending or outbending at least 100,000 times without causing cracking, interlayer separation, or loss of optical properties.
[0029] The substrate may be a thermoplastic substrate with a thickness of 10 μm or more and 200 μm or less.
[0030] The resin composition may contain a fluorine compound, and the fluorine compound may be segregated in a first region located on the surface side of the hard coating layer.
[0031] In addition, segregated fluorine compounds may also provide an antifouling effect.
[0032] In certain embodiments, the fluorine compound may be segregated on the surface of the hard coating layer.
[0033] In a specific embodiment, the hard coat film may be configured to be foldable by either in-bending or out-bending at least 100,000 times without loss of optical properties, and the optical properties are one or more selected from the group consisting of total light transmittance (%), transmittance haze, glossiness, and chromaticity b* (intensity of color from blue to yellow).
[0034] In certain embodiments, there may be a second region located on the substrate side of the hard coating layer where the fluorine compound is not segregated. Effects of the invention
[0035] According to an embodiment of the present invention, a hard coat film can be provided that combines performance capable of withstanding multiple and repetitive folding with scratch resistance. Brief explanation of the drawing
[0036] [Fig. 1] Fig. 1 is a cross-sectional view showing a hard coat film according to one embodiment of the present invention. [Fig. 2] Fig. 2 is a cross-sectional view showing a hard coat film according to another embodiment of the present invention. [Fig. 3] Fig. 3 is a cross-sectional view showing a hard coat film according to another embodiment of the present invention. [Fig. 4] Fig. 4 is a schematic diagram showing a hard coat film manufacturing apparatus according to an embodiment. Specific details for implementing the invention
[0037] Detailed description of the embodiments
[0038] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. The dimensions, materials, specific numerical values, etc. described in these embodiments are merely examples to aid in understanding the present invention, and unless otherwise stated, the present invention is not limited thereto. It should be noted that in this specification and drawings, the same reference numerals are assigned to elements having substantially the same function and configuration, and repetitive descriptions thereof are omitted. Additionally, examples of elements not directly related to the present invention may be omitted.
[0039] Please note that in the drawings referenced in the following description, the size of some components may be exaggerated for the sake of illustrative convenience. Therefore, the relative sizes of the components depicted in each drawing do not necessarily represent the exact proportional relationships between the actual components.
[0040] [1. Overall composition of hard coat film]
[0041] First, the overall configuration of a hard coat film (10) according to one embodiment of the present invention will be explained with reference to FIG. 1. FIG. 1 is a cross-sectional view showing a hard coat film (10) according to the present embodiment.
[0042] A hard coat film (10) according to the present embodiment is provided on the outermost surface of a flexible display device, for example, as a protective film to prevent scratches. As shown in FIG. 1, the hard coat film (10) according to the present embodiment comprises a substrate (11) and a hard coating layer (12). The hard coating layer (12) is laminated on the substrate (11). Each layer will be described below.
[0043] [Recording (11)]
[0044] The substrate (11) is made of a transparent material capable of transmitting light in the visible light range having a wavelength of 350 to 830 nm, for example.
[0045] The substrate (11) may be, for example, an inorganic material such as a glass film, or an organic material such as a plastic film.
[0046] The material of the plastic film is, for example, one or more selected from the group consisting of polyester resin, acetate resin, polyethersulfone resin, polycarbonate resin, polyamide resin, polyimide resin, polyolefin resin, poly(meth)acrylate resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl alcohol resin, polyarylate resin, and polyphenylene sulfide resin, and preferably, one or more of polyester resin, acetate resin, polycarbonate resin, polyimide resin, and polyolefin resin.
[0047] The thickness of the substrate (11) is preferably 10 μm or more and 200 μm or less in terms of handling, flexibility, cost, and characteristics, more preferably 20 μm or more and 100 μm or less, and even more preferably 40 μm or more and 60 μm or less.
[0048] When the thickness of the substrate (11) is 10 μm or more, at least one of the following advantages is achieved. Since the rigidity of the substrate (11) itself can be secured, it becomes difficult for wrinkles to form on the hard coat film (10) even when stress is applied to the hard coat film (10). Also, even if a hard coating layer (12) is continuously formed on the substrate (11), it is difficult for wrinkles to form on the hard coat film (10), so manufacturing problems related to the hard coat film (10) can be reduced. Also, as the curling of the hard coat film (10) is reduced, there is no need to laminate another coating layer on the back side of the substrate (11). Note that the back side of the substrate (11) represents a surface opposite to the surface on which the hard coating layer (12) is laminated.
[0049] When using a roll during the manufacture of the hard coat film (10), it is preferable that the thickness of the substrate (11) be 200 μm or less. If the thickness of the substrate (11) is 200 μm or less, the hard coat film (10) during manufacturing and the hard coat film (10) after manufacturing can be easily wound into a roll shape, and the hard coat film (10) can be manufactured efficiently. In addition, it is preferable that the substrate (11) be a thermoplastic substrate.
[0050] Surface treatment may be performed in advance on the substrate (11) for purposes such as improving adhesion. Surface treatment may include one or more treatments, such as corona treatment, plasma treatment, ultraviolet treatment, excimer treatment, and primer treatment. For improving adhesion, surface treatment including the use of a silane coupling agent is particularly preferred. Also, before forming a hard coating layer (12) on the substrate (11), it is also preferable to remove dust and clean the surface of the substrate (11) with a web cleaner or the like, if necessary.
[0051] [Hard coating layer (12)]
[0052] A hard coating layer (12) is provided on a substrate (11). The hard coating layer (12) may be, for example, a cured product of a resin composition. In a specific embodiment, the resin composition comprises a resin (A), a resin (B), an energy-ray active polymerization initiator, and a solvent.
[0053] Resins (A) and (B) may be energy beam curable resins such as ultraviolet curable resins, electron beam curable resins, and infrared curable resins.
[0054] It should be noted that it is preferable to use UV-curing resins as resins (A) and (B). This is because the need for post-treatment after curing is eliminated. For proper curing treatment, it is preferable to cure under a nitrogen atmosphere.
[0055] The resin (A) is a polyfunctional (meth)acrylic monomer having four or more weighted average functional groups. It is preferable that the number of weighted average functional groups of the resin (A) be greater than 4.2 and less than 5.1. In the present embodiment, the resin (A) contains, for example, a difunctional acrylic monomer and a hexafunctional acrylic monomer. Examples of the difunctional acrylic monomer may include the products "SR833S" (difunctional tricyclodecanedimethanol diacrylate) and "SR306" (tripropylene glycol diacrylate), both of which are available from SARTOMER. Examples of the hexafunctional acrylic monomer may include the products "DPHA" (dipentaerythritol hexaacrylate), available from DAICEL-ALLNEX LTD. Here, instead of or together with a difunctional acrylic monomer, at least one of a trifunctional acrylic monomer, a tetrafunctional acrylic monomer, or a pentafunctional acrylic monomer may be used. Examples of trifunctional monomers may include "SR351" (trimethylolpropane triacrylate) or "SR454" (ethoxylated trimethylolpropane triacrylate), both of which are available at SARTOMER. Examples of tetrafunctional monomers may include "SR295" (pentaerythritol tetraacrylate), "SR355" (di-trimethylolpropane tetraacrylate), or "SR494" (ethoxylated pentaerythritol tetraacrylate), all of which are available at SARTOMER. Examples of pentafunctional monomers may include "SR399" (dipentaerythritol pentaacrylate), which is available at SARTOMER.
[0056] In a specific embodiment, the resin (B) is an aliphatic urethane acrylate. The resin (B) is, for example, a trifunctional aliphatic urethane acrylate, a trifunctional aliphatic polyester urethane acrylate, etc. Specific examples of the resin (B) available on the market may include products "CN989" (trifunctional aliphatic urethane acrylate), "CN929" (trifunctional aliphatic polyester urethane acrylate), etc., all of which are available from SARTOMER.
[0057] By making the hard coating layer (12) into a cured product of a resin composition containing a resin (A) which is a polyfunctional (meth)acrylic monomer having a weighted average functional group of 4 or more and a resin (B) which is an aliphatic urethane acrylate, the glass transition temperature Tg of the hard coating layer (12) may be 50°C or higher and 100°C or lower. Additionally, by making the hard coating layer (12) similarly, the loss tangent tanδ of the hard coating layer (12) at the glass transition temperature Tg may be 0.07 or higher and 0.15 or lower. The loss tangent tanδ of the hard coating layer (12) at the glass transition temperature Tg is a value calculated through dynamic viscoelastic measurement applying a dynamic load at a frequency of 1 Hz. Furthermore, the loss tangent tanδ is the ratio between the storage modulus (E') and the loss modulus (E'') (tanδ = E'' / E'). Storage modulus (E') is the component of the increase in internal energy when an object undergoes deformation. Storage modulus (E') represents the elastic properties of the object. Loss modulus (E'') is the component of the energy loss when an object undergoes deformation. Energy loss is energy that diffuses out of the object as heat. Loss modulus (E'') represents the viscous properties of the object.
[0058] When the glass transition temperature Tg is less than 50°C, the hard coating layer (12) becomes soft in a vehicle or a similar high-temperature environment, and the scratch resistance of the hard coating layer (12) is significantly reduced. On the other hand, when the glass transition temperature Tg exceeds 100°C, the flexibility of the hard coating layer (12) cannot be secured, making it difficult to repeatedly fold the hard coating layer (12) multiple times.
[0059] Accordingly, it is preferable that the glass transition temperature Tg of the hard coating layer (12) be set to 50°C or higher and 100°C or lower. Accordingly, the scratch resistance of the hard coating layer (12) can be improved even in a vehicle or a similar high-temperature environment, and the hard coating layer (12) can be folded repeatedly more than 100,000 times.
[0060] If the loss tangent tangent tan δ of the hard coating layer (12) at the glass transition temperature Tg is less than 0.07, the hardness of the hard coating layer (12) becomes too high, and the flexibility of the hard coating layer (12) will decrease. On the other hand, if the loss tangent tan δ of the hard coating layer (12) at the glass transition temperature Tg is greater than 0.15, the hardness of the hard coating layer (12) becomes too low, and the scratch resistance of the hard coating layer (12) will decrease.
[0061] Accordingly, it is preferable that the loss tangent tangent tan δ of the hard coating layer (12) at the glass transition temperature Tg be set to 0.07 or higher and 0.15 or lower. Accordingly, the scratch resistance of the hard coating layer (12) can be improved, and the hard coating layer (12) can be folded repeatedly over a number of times of 100,000 or more.
[0062] The content (mass%) of resin (A) contained in the resin composition is preferably greater than 2 times and less than 9 times the content (mass%) of resin (B), more preferably 4 times or more and less than 9 times, and even more preferably 4 times or more and 5 times or less. The content of resin (A) contained in the resin composition is preferably 20 mass% or more and 40 mass% or less, and more preferably 26 mass% or more and 33 mass% or less. The content of resin (B) contained in the resin composition is preferably 2 mass% or more and 15 mass% or less, and more preferably 4.5 mass% or more and 11.5 mass% or less.
[0063] In certain embodiments, the energy beam active polymerization initiator is a Norrish Type I photoinitiator or a Norrish Type II photoinitiator. Specific examples of energy beam active polymerization initiators available on the market may include products available from IGM RESINS (formerly BASF), such as "OMNIRAD 184 (IRGACURE 184)" (1-hydroxycyclohexyl-phenyl ketone), "OMNIRAD 500 (IRGACURE 500)" (a mixture of benzophenone and 1-hydroxycyclohexyl-phenyl ketone), "OMNIRAD TPO" (2,4,6-trimethylbenzoyl-diphenylphosphine oxide), etc.
[0064] The solvent is not particularly limited as long as it satisfies the coating properties of the resin composition, but it is preferable to select the solvent with safety in mind. In a specific embodiment, the solvent contains one or more selected from the group consisting of, for example, alcohol-based solvents such as ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, and diacetone alcohol; ketone-based solvents such as acetone, methyl ethyl ketone (hereinafter MEK), methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate (hereinafter PGMEA); and ether-based solvents such as propylene glycol monomethyl ether (hereinafter PGME), diethyl ether, and diisopropyl ether. The solvent preferably contains any one of MEK, PGME, and PGMEA. In particular, it is preferable to use either or both of PGME and PGMEA, and accordingly, the coating properties of the resin composition can be improved.
[0065] The thickness of the hard coating layer (12) is preferably 3 μm or more, for example, and more preferably 5 μm or more. When the thickness of the hard coating layer (12) is 3 μm or more, sufficient hardness is obtained, and the hard coating layer (12) is less likely to be scratched during the manufacturing process. Also, the thickness of the hard coating layer (12) is preferably 15 μm or less, and more preferably 10 μm or less. When the thickness of the hard coating layer (12) is 15 μm or less, microcracks that occur when the hard coat film (10) is bent during manufacturing are less likely to form in the hard coating layer (12), so the productivity of the hard coat film (10) is improved.
[0066] Metal oxide nanoparticles may be contained in a dispersed manner within the resin composition of the hard coating layer (12). When the resin composition contains metal oxide nanoparticles, the hardness of the hard coating layer (12) can be increased.
[0067] In addition, the average particle size of the metal oxide nanoparticles is preferably, for example, 100 nm or less, and more preferably 50 nm or less. It should be noted that in this embodiment, the average particle size refers to a value measured by the BET method.
[0068] If the average particle size of the metal oxide nanoparticles is greater than 100 nm, the light transmittance in the visible light range of the hard coating layer (12) may decrease. Therefore, by setting the average particle size of the metal oxide nanoparticles to 100 nm or less, the light transmittance in the visible light range of the hard coating layer (12) can be maintained. By setting the average particle size of the metal oxide nanoparticles to 50 nm or less, these advantages can be further enhanced. In the case where the substrate (11) is an opaque substrate, the hard coating layer (12) does not need to have high light transmittance, so the average particle size of the metal oxide nanoparticles may be greater than 100 nm.
[0069] The content of metal oxide nanoparticles (excluding monomers) in the resin composition is preferably 2 mass% or more and 5 mass% or less of the total solid content of the resin composition of the hard coating layer (12). If the content of metal oxide nanoparticles is greater than 5 mass%, the hard coating layer (12) tends to become brittle. Therefore, by setting the content of metal oxide nanoparticles according to the present embodiment within the above range, the flexibility of the hard coating layer (12) can be maintained. The solid content of the resin composition refers to the total content excluding the solvent, and the liquid monomer content is also included in the solid content.
[0070] In a specific embodiment, the metal oxide constituting the metal oxide nanoparticles is either or both of SiO2 (silica) and Al2O3 (alumina). This prevents the light transmittance in the visible light range of the hard coating layer (12) from being reduced.
[0071] It is preferable that the metal oxide nanoparticles have a Mohs hardness greater than 6. This allows the hardness of the hard coating layer (12) to be increased without reducing the flexibility of the hard coating layer (12).
[0072] [Anti-fouling layer (13)]
[0073] In a specific embodiment of the present invention, an antifouling layer (13) may be formed as part of a hard coating layer (12). FIG. 2 is a cross-sectional view showing a hard coat film (10) according to a specific embodiment. As shown in FIG. 2, a fluorine compound contained in the hard coating layer (12) is segregated in a first region (12a) located on the surface side of the hard coating layer (12) to form an antifouling layer (13). The fluorine compound is not segregated in a second region (12b) located on the substrate (11) side of the hard coating layer (12). That is, the amount of the fluorine compound in the second region (12b) is less than the amount of the fluorine compound in the first region (12a). The fluorine compound may be included in the second region (12b). The fluorine compound may be dispersed (dispersed) in the second region (12b). The first region (12a) has a thickness Ta of, for example, 10% of the total thickness T of the hard coating layer (12) at most. The second region (12b) is a region of the hard coating layer (12) other than the first region (12a). In this specification, the term “segregation” means that, upon curing of the resin composition, the distribution of fluorine compounds in the resin composition is greater on the surface side of the hard coating layer (12) than on the substrate (11) side. The antifouling layer (13) prevents the hard coating layer (12) from being contaminated. The antifouling layer (13) may or may not form a rigid layer depending on the segregation state of the fluorine compounds.
[0074] The antifouling layer (13) contains a fluorine compound. It is preferable that the fluorine compound has (meth)acrylic groups. Additionally, from the perspective of environmental regulations, it is preferable that the fluorine compound be a perfluoropolyether derivative rather than a fluoroalkyl derivative. The fluorine compound may be a hybrid material of organic and inorganic materials. Examples of hybrid materials may include fluorinated silsesquioxanes. In this embodiment, since the antifouling layer (13) contains a fluorine compound, the antifouling properties and chemical resistance of the hard coat film (10) can be improved. Chemical resistance is, for example, resistance to acids, bases, solvents, and oils.
[0075] Examples of fluorine compounds contained in the antifouling layer (13) may include products available from SHIN-ETSU CHEMICAL CO., LTD., "KY-1203", products available from DAIKIN INDUSTRIES, LTD., "OPTOOL DAC-HP", products available from SOLVAY SPECIALTY POLYMERS, "FLUOROLINK AD1700", products available from SARTOMER, etc.
[0076] [2. Characteristics of the hard coating layer (12)]
[0077] Next, the characteristics of the hard coating layer (12) according to the present embodiment will be described. The hard coating layer (12) according to the present embodiment has, for example, at least one of the following characteristics (I) to (IV).
[0078] (I) Glass transition temperature Tg and loss tangent tangent tanδ
[0079] The glass transition temperature Tg of the hard coating layer (12) is 50°C or higher and 100°C or lower, preferably 60°C or higher and 90°C or lower. The loss tangent tanδ is 0.07 or higher and 0.15 or lower, preferably 0.09 or higher and 0.13 or lower.
[0080] Accordingly, the scratch resistance and wear resistance of the hard coating layer (12) can be improved even in a vehicle or a similar high-temperature environment, and the hard coating layer (12) can be folded repeatedly more than 100,000 times.
[0081] The glass transition temperature Tg and the loss tangent tangent tanδ can be measured, for example, using the DMA7100 kinetic analyzer available from HITACHI HIGH-TECH SCIENCE CORPORATION.
[0082] The measurement conditions for dynamic viscoelasticity measurements when calculating the glass transition temperature Tg and the loss tangent tangent tanδ are as follows.
[0083] Sinusoidal vibration induced by frequency: 1 Hz
[0084] Sample size: Length 20 mm × Width 4.4 mm × Thickness 0.10 mm
[0085] Test method: Temperature rise from 20℃ to 200℃ at a rate of 10℃ / min
[0086] (II) Number of folds
[0087] The hard coat film (10) is configured to be folded by either in-bending or out-bending at least 100,000 times without causing cracks, interlayer separation, or loss of optical properties. The optical properties mentioned here include, for example, total light transmittance (%), transmission haze, glossiness, and variations in chromaticity b* (intensity of color ranging from blue to yellow). By the above configuration, even when a flexible display device coated with the hard coat film (10) is repeatedly folded tens of thousands of times, the hard coat film (10) can avoid separating from the flexible display device.
[0088] The number of folds (number of bends) can be measured using a folding test device (mandrel diameter: 3 mm, bend radius: 1.5 mm) available from, for example, YUASA SYSTEM CO., LTD.
[0089] (III) Water Contact Angle (WCA)
[0090] The water contact angle is the angle formed by the surface of a water droplet and the surface of the hard coating layer (12) when a water droplet is brought into contact with the surface of the hard coating layer (12). The water contact angle is measured before and after the execution of the wear test.
[0091] The wear test is a test in which the surface of the hard coating layer (12) with steel wool is worn using a wear tester with steel wool #0000 under conditions of load: 1000 g, speed: 50 mm / sec, reciprocating distance: 40 mm, and number of reciprocating cycles: 2500 times.
[0092] It is preferable that the water contact angle θ1 of the surface of the hard coating layer (12) before the abrasion test (before abrasion) is greater than 110° and less than 120°. It is preferable that the water contact angle θ2 of the surface of the hard coating layer (12) after the abrasion test (after abrasion) is greater than 100° and less than the water contact angle θ1.
[0093] Before and after wear, the decrease in the water contact angle of the surface of the hard coating layer (12) is preferably less than 13%, and more preferably less than 7.6%. A low decrease in the water contact angle means that even when a wear test is performed on the hard coating layer (12), the hard coating layer (12) is hardly worn down, that is, the wear resistance is excellent. Here, the decrease in the water contact angle can be calculated by the formula (water contact angle before wear test - water contact angle after wear test) / water contact angle before wear test × 100.
[0094] The water contact angle can be measured, for example, using the automatic contact angle meter DM-501 Hi available from KYOWA INTERFACE SCIENCE CO., LTD.
[0095] (IV) Visibility Scratch
[0096] After performing the abrasion test on the hard coating layer (12) according to the present embodiment, no visible scratches were found on the hard coating layer (12). That is, in the hard coat film (10) according to the present embodiment, it can be seen that the hard coating layer (12) is resistant to scratches and has excellent scratch resistance.
[0097] [3. Manufacturing apparatus for hard coat film (10)]
[0098] FIG. 4 is a schematic diagram showing a film manufacturing apparatus (100) according to the present embodiment. As shown in FIG. 4, the film manufacturing apparatus (100) comprises a sending roll (110), a winding roll (112), guide rolls (114a to 114d), a coating device (120), a drying device (130), and a curing device (140). In FIG. 4, solid arrows indicate the rotation direction of the rolls. In FIG. 4, dashed arrows indicate the transport direction of the substrate (11).
[0099] A strip-shaped material (11) is wound in a roll shape on the discharge roll (110). The discharge roll (110) is arranged so that the material (11) can be continuously discharged by means of a guide roll (114a), etc.
[0100] A winding roll (112) is arranged to wind a strip-shaped hard coat film (10) manufactured by a film manufacturing device (100).
[0101] Guide rolls (114a to 114d) are arranged in a conveying path within a film manufacturing device (100) to convey a strip-shaped substrate (11) and a strip-shaped hard coat film (10). The material of the guide rolls (114a to 114b) is appropriately selected according to the desired roll characteristics. The material of the guide rolls (114a to 114b) is, for example, a metal such as stainless steel, rubber, silicone resin, etc.
[0102] A coating device (120) is provided between guide rolls (114a) and guide rolls (114b). The coating device (120) applies a resin composition (e.g., a resin composition) to a substrate (11). The coating device (120) is, for example, a gravure coater, a wire bar coater, a die coater, etc.
[0103] A drying device (130) is provided between guide rolls (114b) and guide rolls (114c). The drying device (130) heats a substrate (11) coated with a resin composition to dry the resin composition. The drying device (130) vaporizes the solvent contained in the resin composition. In this way, the solvent can be removed from the resin composition.
[0104] A curing device (140) is provided between a guide roll (114c) and a guide roll (114d). The curing device (140) comprises guide rolls (144, 146) and a light source (148) that irradiates energy rays onto a resin composition. Examples of energy rays include electron beams, ultraviolet rays, visible light, gamma rays, etc. The guide rolls (144 and 146) contact the back surface of a substrate (11) coated with a resin composition and feed the substrate (11) in the direction of the guide roll (114d).
[0105] Next, a method for manufacturing a hard coat film (10) using a film manufacturing device (100) is described. First, a substrate (11) is sent from a delivery roll (110). The delivered substrate (11) passes under a coating device (120) via a guide roll (114a). The coating device (120) applies a resin composition to the substrate (11) passing under the coating device (120). The substrate (11) coated with the resin composition is returned to a drying device (130) via a guide roll (114b). The drying device (130) dries the resin composition applied to the substrate (11).
[0106] A substrate (11) on which a dried resin composition is laminated is conveyed to a curing device (140) via a guide roll (114c), and an energy line from a light source (148) is irradiated onto the resin composition. As a result, the resin composition is cured, and a hard coat film (10) is manufactured in which a hard coating layer (12) is laminated on the substrate (11).
[0107] The hard coat film (10) manufactured in this way is wound onto a winding roll (112) via guide rolls (146 and 114d).
[0108] It should be noted that it is preferable for the resin composition to contain a fluorine compound. Accordingly, when the solvent is vaporized by the drying device (130), the fluorine compound rises to the surface of the resin composition along with the drying and rising of the solvent, thereby forming an antifouling layer (13).
[0109] Note that the antifouling layer (13) may be obtained by separately laminating a layer containing a fluorine compound after forming the hard coating layer (12). FIG. 3 is a cross-sectional view showing a hard coat film (10) according to a specific embodiment. As shown in FIG. 3, the antifouling layer (13) may be a separate layer from the hard coating layer (12). In this case, the antifouling layer (13) is formed on the hard coating layer (12). When forming the antifouling layer (13) by a separate process, methods such as coating, deposition, or sputtering may be used. When using a coating method, an apparatus similar to the film manufacturing apparatus (100) may be used. Thus, the antifouling layer (13) may be a part of the hard coating layer (12) or may be a different layer from the hard coating layer (12).
[0110] [Example]
[0111] Hereinafter, embodiments and comparative examples of the present invention are described in detail. The embodiments described below are merely examples, and the hard coat film according to the present invention is not limited to the following embodiments.
[0112] Examples 1 to 13 and Comparative Examples 1 to 8 were prepared as hard coating layers and antifouling layers. When preparing the hard coating layer and the antifouling layer, resin compositions were prepared containing resin (A), resin (B), an energy beam active polymerization initiator, a solvent, and a fluorine compound, respectively. The compositions of the resin compositions of Examples 1 to 5 are shown in Table 1 below. The compositions of the resin compositions of Examples 6 to 10 are shown in Table 2 below. The compositions of the resin compositions of Examples 11 to 13 are shown in Table 3 below. The compositions of the resin compositions of Comparative Examples 1 to 5 are shown in Table 4 below. The compositions of the resin compositions of Comparative Examples 6 to 8 are shown in Table 5 below. Note that the unit of the mixing ratios in Tables 1 to 5 is mass%.
[0113] The glass transition temperature Tg, the loss tangent tangent tan δ (tan Delta, peak) at the glass transition temperature Tg, the number of folds, the water contact angle (WCA) before and after the abrasion test, and the visibility scratch were measured for the hard coat films according to Examples 1 to 13 and Comparative Examples 1 to 8.
[0114] The glass transition temperature Tg and the loss tangent tangent tanδ at the glass transition temperature Tg were measured using the DMA7100 dynamic measuring device available from HITACHI HIGH-TECH SCIENCE CORPORATION. In addition, the measurement conditions for the dynamic viscoelasticity measurement when calculating the loss tangent tanδ were similar to those of the above embodiment.
[0115] The number of folds was measured using a folding test device (mandrel diameter: 3 mm, bending radius: 1.5 mm) available from YUASA SYSTEM CO., LTD. In Tables 1 to 5, the evaluation of the folding test results is shown on a scale of 1 to 3. In Tables 1 to 5, Grade "3" indicates an excellent grade with no change even after 200,000 (200K) folds. In Tables 1 to 5, Grade "2" indicates a grade within the acceptable range with no change even after 100,000 (100K) folds. In Tables 1 to 5, Grade "1" indicates a poor grade where change occurs before 100,000 folds.
[0116] The water contact angle was measured by dropping 2.0 μL of pure water onto the surface of the hard coat film according to each experimental example before and after abrasion using a steel wool abrasion tester. Abrasion was performed on the surface of the hard coat film under the conditions of a load of 1000 g, a speed of 50 mm / sec, a reciprocating distance of 40 mm, and a number of reciprocating cycles of 2500. In addition, the average value was calculated by measuring the water contact angle 10 times at the center of the abraded area. The water contact angles shown in Tables 1 to 5 below are average values. The water contact angle was measured using the DM-501 Hi automatic contact angle meter available from KYOWA INTERFACE SCIENCE CO., LTD.
[0117] After conducting the above abrasion test, the surface of the hard coat film according to each experimental example was visually inspected to see if any scratches had formed.
[0118] [Table l]
[0119]
[0120] [Example 1]
[0121] As shown in Table 1, the resin composition of Example 1 comprises 5.64 mass% of "SR833S" available from SARTOMER and 22.56 mass% of "DPHA" available from DAICEL-ALLNEX LTD. as resin (A), 9.4 mass% of "CN989" available from SARTOMER as resin (B), 5.64 mass% of "OMNIRAD 500" available from IGM RESINS and 1.41 mass% of "OMNIRAD TPO" available from IGM RESINS as energy beam active polymerization initiator, 46.984 mass% of "PGME" available from SIGMA-ALDRICH as solvent, 7.52 mass% of "AL2260" available from NANOPHASE TECHNOLOGIES CORPORATION as metal oxide nanoparticles, and SHIN-ETSU as a fluorine compound. It contained 0.846 mass% of "KY-1203" available from CHEMICAL. CO., LTD.
[0122] Here, "AL2260" contains 30 mass% of alumina particles and 70 mass% of a difunctional monomer (TPGDA). For this reason, the "weighted average of functionality" and the content ratio between resin (A) and resin (B) (hereinafter referred to as "A / B") of Examples 1 to 13 and Comparative Examples 1 to 8 shown in Tables 1 to 5 reflect the content of the difunctional monomer.
[0123] In Example 1, the weighted average functional group of the resin (A) was 4.70, and A / B was 3.56.
[0124] In Example 1, the glass transition temperature Tg was 60.4°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1046.
[0125] In the folding test of Example 1, there was no change in the hard coat film even after 200K folding (Grade "3"). In Example 1, the water contact angle before the abrasion test was 114.7°, and the water contact angle after the abrasion test was 106°.
[0126] No visible scratches were found.
[0127] [Example 2]
[0128] As shown in Table 1, the resin composition of Example 2 contained 7.52 mass% of "SR833S" and 22.56 mass% of "DPHA" as resin (A), and 7.52 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 2 were similar to those in Example 1.
[0129] In Example 2, the weighted average functional group of the resin (A) was 4.55, and A / B was 4.70.
[0130] In Example 2, the glass transition temperature Tg was 54.4°C. The loss tangent tangent tangent tan δ at the glass transition temperature Tg was 0.1126.
[0131] In the folding test of Example 2, there was no change even after folding the hard coat film 200K times. In Example 2, the water contact angle before the abrasion test was 115.2°, and the water contact angle after the abrasion test was 100.8°. No visible scratches were observed.
[0132] [Example 3]
[0133] As shown in Table 1, the resin composition of Example 3 contained 7.52 mass% of "SR833S" and 18.8 mass% of "DPHA" as resin (A), and 11.28 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 3 were similar to those in Example 1.
[0134] In Example 3, the weighted average functional group of the resin (A) was 4.38, and A / B was 2.80.
[0135] In Example 3, the glass transition temperature Tg was 68.5°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1246.
[0136] In the folding test of Example 3, there was no change even after folding the hard coat film 200K times. In Example 3, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 105.1°. No visible scratches were observed.
[0137] [Example 4]
[0138] As shown in Table 1, the resin composition of Example 4 contained 9.4 mass% of "SR833S" and 20.68 mass% of "DPHA" as resin (A), and 7.52 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 4 were similar to those in Example 1.
[0139] In Example 4, the weighted average functional group of the resin (A) was 4.34, and A / B was 4.70.
[0140] In Example 4, the glass transition temperature Tg was 68.5°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1274.
[0141] In the folding test of Example 4, there was no change even after folding the hard coat film 200K times. In Example 4, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 106.7°. No visible scratches were observed.
[0142] [Example 5]
[0143] As shown in Table 1, the resin composition of Example 5 contained 5.64 mass% of "SR833S" and 24.44 mass% of "DPHA" as resin (A), and 7.52 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 5 were similar to those in Example 1.
[0144] In Example 5, the weighted average functional group of the resin (A) was 4.77, and A / B was 4.70.
[0145] In Example 5, the glass transition temperature Tg was 76.8°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1017.
[0146] In the folding test of Example 5, there was no change even after folding the hard coat film 200K times. In Example 5, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 106.5°. No visible scratches were observed.
[0147] [Table 2]
[0148]
[0149] [Example 6]
[0150] As shown in Table 2, the resin composition of Example 6 contained 9.4 mass% of "SR833S" and 18.8 mass% of "DPHA" as resin (A), and 9.4 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 6 were similar to those in Example 1.
[0151] In Example 6, the weighted average functional group of the resin (A) was 4.25, and A / B was 3.56.
[0152] In Example 6, the glass transition temperature Tg was 73.4°C. The loss tangent tangent tangent tan δ at the glass transition temperature Tg was 0.1125.
[0153] In the folding test of Example 6, there was no change even after folding the hard coat film 200K times. In Example 6, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 107.3°. No visible scratches were observed.
[0154] [Example 7]
[0155] As shown in Table 2, the resin composition of Example 7 contained 5.64 mass% of "SR833S" and 20.68 mass% of "DPHA" as resin (A), and 11.28 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 7 were similar to those in Example 1.
[0156] In Example 7, the weighted average functional group of the resin (A) was 4.62, and A / B was 2.80.
[0157] In Example 7, the glass transition temperature Tg was 50.6°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1152.
[0158] In the folding test of Example 7, there was no change even after folding the hard coat film 200K times. In Example 7, the water contact angle before the abrasion test was 113.2°, and the water contact angle after the abrasion test was 102.3°. No visible scratches were observed.
[0159] [Example 8]
[0160] As shown in Table 2, the resin composition of Example 8 contained 4.7 mass% of "SR833S" and 25.38 mass% of "DPHA" as resin (A), and 7.52 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 8 were similar to those in Example 1.
[0161] In Example 8, the weighted average functional group of the resin (A) was 4.87, and A / B was 4.70.
[0162] In Example 8, the glass transition temperature Tg was 58.3°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.0912.
[0163] In the folding test of Example 8, there was no change even after folding the hard coat film 200K times. In Example 8, the water contact angle before the abrasion test was 114.5°, and the water contact angle after the abrasion test was 105.6°. No visible scratches were observed.
[0164] [Example 9]
[0165] As shown in Table 2, the resin composition of Example 9 contained 3.76 mass% of "SR833S" and 26.32 mass% of "DPHA" as resin (A), and 7.52 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 9 were similar to those in Example 1.
[0166] In Example 9, the weighted average functional group of the resin (A) was 4.98, and A / B was 4.70.
[0167] In Example 9, the glass transition temperature Tg was 91.7°C. The loss tangent tangent tangent tan δ at the glass transition temperature Tg was 0.1003.
[0168] In the folding test of Example 9, there was no change even after folding the hard coat film 200K times. In Example 9, the water contact angle before the abrasion test was 115.8°, and the water contact angle after the abrasion test was 107.1°. No visible scratches were observed.
[0169] [Example 10]
[0170] As shown in Table 2, the resin composition of Example 10 contained 2.82 mass% of "SR833S" and 27.26 mass% of "DPHA" as resin (A), and 7.52 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 10 were similar to those in Example 1.
[0171] In Example 10, the weighted average functional group of the resin (A) was 5.09, and A / B was 4.70.
[0172] In Example 10, the glass transition temperature Tg was 85.3°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1007.
[0173] In the folding test of Example 10, there was no change even after folding the hard coat film 200K times. In Example 10, the water contact angle before the abrasion test was 116.1°, and the water contact angle after the abrasion test was 109.6°. No visible scratches were observed.
[0174] [Table 3]
[0175]
[0176] [Example 11]
[0177] As shown in Table 3, the resin composition of Example 11 contained 5.64 mass% of "SR833S" and 27.26 mass% of "DPHA" as resin (A), and 4.7 mass% of "CN989" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Example 11 were similar to those in Example 1.
[0178] In Example 11, the weighted average functional group of the resin (A) was 4.86, and A / B was 8.12.
[0179] In Example 11, the glass transition temperature Tg was 58.3°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.0912.
[0180] In the folding test of Example 11, there was no change even after folding the hard coat film 200K times. In Example 11, the water contact angle before the abrasion test was 116.7°, and the water contact angle after the abrasion test was 110.2°. No visible scratches were observed.
[0181] [Example 12]
[0182] As shown in Table 3, the resin composition of Example 12 contained 8.064 mass% of "SR833S" and 24.192 mass% of "DPHA" as resin (A), 8.064 mass% of "CN929" available from SARTOMER as resin (B), 1.613 mass% of "OMNIRAD 184" available from IGM RESINS as energy beam active polymerization initiator, 49.693 mass% of "PGME" as solvent, 8.064 mass% of "AL2260" as metal oxide nanoparticles, and 0.31 mass% of "KY-1203" as a fluorine compound.
[0183] In Example 12, the weighted average functional group of the resin (A) was 4.55, and A / B was 4.70.
[0184] In Example 12, the glass transition temperature Tg was 69.4°C. The loss tangent tangent tangent tan δ at the glass transition temperature Tg was 0.09.
[0185] In the folding test of Example 12, there was no change even after folding the hard coat film more than 250,000 times (250K). In Example 12, the water contact angle before the abrasion test was 115.3°, and the water contact angle after the abrasion test was 107.7°. No visible scratches were observed.
[0186] [Example 13]
[0187] As shown in Table 3, the resin composition of Example 13 contained 8.014 mass% of "SR833S" and 22.04 mass% of "DPHA" as resin (A), 10.02 mass% of "CN989" as resin (B), 1.603 mass% of "OMNIRAD 184" as an energy beam active polymerization initiator, 50 mass% of "PGME" as a solvent, 8.014 mass% of "AL2260" as metal oxide nanoparticles, and 0.31 mass% of "KY-1203" as a fluorine compound.
[0188] In Example 13, the weighted average functional group of the resin (A) was 4.47, and A / B was 3.56.
[0189] In Example 13, the glass transition temperature Tg was 80°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.099.
[0190] In the folding test of Example 13, there was no change even after folding the hard coat film more than 250K. In Example 13, the water contact angle before the abrasion test was 114.9°, and the water contact angle after the abrasion test was 105.9°. No visible scratches were observed.
[0191] As explained above, in Examples 1 to 13, the weighted average functional group of the resin (A) was 4 or higher. Accordingly, the glass transition temperature Tg of Examples 1 to 13 was within the range of 50°C or higher and 100°C or lower, and the loss tangent tangent tanδ at the glass transition temperature Tg was within the range of 0.07 or higher and 0.15 or lower. For this reason, it is presumed that the number of folds in Examples 1 to 13 was 200° or higher. In addition, it is presumed that the water contact angle before the abrasion test of Examples 1 to 13 was greater than 110° and the water contact angle after the abrasion test was greater than 100°. Furthermore, in Examples 1 to 13, it is presumed that the decrease in the water contact angle after the abrasion test relative to the water contact angle before the abrasion test was less than 13%. In addition, it appears that no visible scratches were observed in Examples 1 to 13. In summary, Examples 1 to 13 were confirmed to have the ability to withstand repeated folding over a long period of time, and to improve scratch resistance and wear resistance even in a vehicle or under similar high-temperature environments.
[0192] [Table 4]
[0193]
[0194] [Comparative Example 1]
[0195] As shown in Table 4, the resin composition of Comparative Example 1 contained 7.515 mass% of "SR833S" available from SARTOMER, 5.01 mass% of "SR306 (TPGDA)" available from SARTOMER, and 9.018 mass% of "DPHA" as resin (A), 16.032 mass% of "CN929" as resin (B), 2.004 mass% of "OMNIRAD 184" as an energy beam active polymerization initiator, 50.09 mass% of "PGME" as a solvent, 10.02 mass% of "AL2460" available from NANOPHASE TECHNOLOGIES CORPORATION as a metal oxide nanoparticle, and 0.31 mass% of "KY-1203" as a fluorine compound.
[0196] In Comparative Example 1, the weighted average functional group of resin (A) was 2.77, and A / B was 1.78.
[0197] In Comparative Example 1, the glass transition temperature Tg was 59.5°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.1516.
[0198] In the folding test of Comparative Example 1, there was no change even after folding the film more than 250K. The water contact angle before the abrasion test was 115°, and the water contact angle after the abrasion test was 106°. Meanwhile, visible scratches were confirmed.
[0199] As described above, in Comparative Example 1, the weighted average functional group of the resin (A) contained in the resin composition was 2.77. Therefore, the loss tangent tan δ at the glass transition temperature Tg of Comparative Example 1 increased to 0.1516, which means that the flexibility of the film was slightly lowered. For this reason, it is presumed that visible scratches were observed in Comparative Example 1.
[0200] [Comparative Example 2]
[0201] As shown in Table 4, the resin composition of Comparative Example 2 contained 16.65 mass% of "SR444" available from SARTOMER as resin (A), 30.91 mass% of "PU610" available from MIWON SPECIALTY CHEMICAL as resin (B), 2.37 mass% of "OMNIRAD 184" as an energy beam active polymerization initiator, 49.76 mass% of "PGME" as a solvent, and 0.31 mass% of "KY-1203" as a fluorine compound. It should be noted that the resin composition of Comparative Example 2 did not contain metal oxide nanoparticles. Furthermore, "SR444" is a monomer containing a tetrafunctional group with a trifunctional group as the main component.
[0202] In Comparative Example 2, the weighted average functional group of resin (A) was 3.00, and A / B was 0.54.
[0203] In Comparative Example 2, the glass transition temperature Tg was 100°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.055.
[0204] In the folding test of Comparative Example 2, cracks formed in the sample during the process of folding the film 100 times. In Comparative Example 2, the water contact angle before the abrasion test was 110°, and the water contact angle after the abrasion test was 95°. No visible scratches were observed.
[0205] As described above, in Comparative Example 2, the weighted average functional group of the resin (A) contained in the resin composition was 3.00. Therefore, the loss tangent tangent tanδ at the glass transition temperature Tg of Comparative Example 2 was lowered to 0.055, and the hardness of the film became too high. For this reason, it is presumed that the number of folds in Comparative Example 2 was 100 or less. In general, in Comparative Example 2, scratches were not observed because the crosslinking density was increased to improve abrasion resistance, whereas it is thought that good results were not obtained in the folding test because the crosslinking density was increased excessively, resulting in a lack of flexibility.
[0206] As shown in Table 4, the resin composition of Comparative Example 3 contained 7.35 mass% of "SR444" as resin (A) and 24.51 mass% of "IBOA(SR506-A)" available from SARTOMER, 9.81 mass% of "CN9047" available from SARTOMER as resin (B), 0.98 mass% of "OMNIRAD 184" as an energy beam active polymerization initiator, 49.75 mass% of "PGME" as a solvent, 7.35 mass% of "AL2260" as metal oxide nanoparticles, and 0.25 mass% of "KY-1203" as a fluorine compound. Here, "IBOA(SR506-A)" is a monofunctional monomer.
[0207] In Comparative Example 3, the weighted average functional group of resin (A) was 1.54, and A / B was 3.77.
[0208] In Comparative Example 3, the glass transition temperature Tg was 129.6℃. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.25.
[0209] In the folding test of Comparative Example 3, there was no change even after folding the film 200K. However, in Comparative Example 3, the water contact angle before the abrasion test was 113.4°, and the water contact angle after the abrasion test was 87.3°. Visible scratches were confirmed.
[0210] As described above, in Comparative Example 3, the weighted average functional group of the resin (A) contained in the resin composition was 1.54. Accordingly, the glass transition temperature Tg of Comparative Example 3 increased to 129.6°C. The loss tangent tangent tanδ at the glass transition temperature Tg of Comparative Example 3 increased to 0.25. That is, since Comparative Example 3 has a high tanδ, the crosslinking density is low and it has flexibility, so it showed good results in the folding test, but it is presumed that visible scratches were confirmed after the wear test because the hardness became too low.
[0211] [Comparative Example 4]
[0212] As shown in Table 4, the resin composition of Comparative Example 4 contained 7.35 mass% of "SR444" and 22.06 mass% of "IBOA (SR506-A)" as resin (A), and 12.26 mass% of "CN9047" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Comparative Example 4 were similar to those in Comparative Example 3.
[0213] In Comparative Example 4, the weighted average functional group of resin (A) was 1.57, and A / B was 2.82.
[0214] In Comparative Example 4, the glass transition temperature Tg was 117.8℃. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.208.
[0215] In the folding test of Comparative Example 4, there was no change even after folding the film 200K. However, in Comparative Example 4, the water contact angle before the abrasion test was 113.7°, and the water contact angle after the abrasion test was 73.9°. Visible scratches were confirmed.
[0216] As described above, in Comparative Example 4, the weighted average functional group of the resin (A) contained in the resin composition was 1.57. Accordingly, the glass transition temperature Tg of Comparative Example 4 increased to 117.8°C. The loss tangent tangent tanδ at the glass transition temperature Tg of Comparative Example 4 increased to 0.208. That is, since Comparative Example 4 has a high tanδ, the crosslinking density is low and it has flexibility, so it showed good results in the folding test, but it is presumed that visible scratches were confirmed after the wear test because the hardness became too low.
[0217] [Comparative Example 5]
[0218] As shown in Table 4, the resin composition of Comparative Example 5 contained 7.35 mass% of "SR444" and 19.61 mass% of "IBOA (SR506-A)" as resin (A), and 14.71 mass% of "CN9047" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Comparative Example 5 were similar to those in Comparative Example 3.
[0219] In Comparative Example 5, the weighted average functional group of resin (A) was 1.62, and A / B was 2.18.
[0220] In Comparative Example 5, the glass transition temperature Tg was 106.3℃. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.194.
[0221] In the folding test of Comparative Example 5, there was no change even after folding the film 200K. However, in Comparative Example 5, the water contact angle before the abrasion test was 114.1°, and the water contact angle after the abrasion test was 76.1°. Visible scratches were confirmed.
[0222] As described above, in Comparative Example 5, the weighted average functional group of the resin (A) contained in the resin composition was 1.62. Accordingly, the glass transition temperature Tg of Comparative Example 5 increased to 106.3°C. The loss tangent tangent tanδ at the glass transition temperature Tg of Comparative Example 5 increased to 0.194. That is, since Comparative Example 5 has a high tanδ, the crosslinking density is low and it has flexibility, so it showed good results in the folding test, but it is presumed that visible scratches were confirmed after the wear test because the hardness became too low.
[0223] [Table 5]
[0224]
[0225] [Comparative Example 6]
[0226] As shown in Table 5, the resin composition of Comparative Example 6 contained 4.9 mass% of "SR444" and 24.51 mass% of "IBOA (SR506-A)" as resin (A), and 12.26 mass% of "CN9047" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Comparative Example 6 were similar to those in Comparative Example 3.
[0227] In Comparative Example 6, the weighted average functional group of resin (A) was 1.43, and A / B was 2.82.
[0228] In Comparative Example 6, the glass transition temperature Tg was 111.9℃. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.2791.
[0229] In the folding test of Comparative Example 6, there was no change even after folding the film 200K. However, in Comparative Example 6, the water contact angle before the abrasion test was 113.5°, and the water contact angle after the abrasion test was 77.4°. Visible scratches were confirmed.
[0230] As described above, in Comparative Example 6, the weighted average functional group of the resin (A) contained in the resin composition was 1.43. Accordingly, the glass transition temperature Tg of Comparative Example 6 increased to 111.9°C. The loss tangent tangent tanδ at the glass transition temperature Tg of Comparative Example 6 increased to 0.2791. That is, since Comparative Example 6 has a high tanδ, the crosslinking density is low and it has flexibility, so it showed good results in the folding test, but it is presumed that visible scratches were confirmed after the wear test because the hardness became too low.
[0231] [Comparative Example 7]
[0232] As shown in Table 5, the resin composition of Comparative Example 7 contained 4.9 mass% of "SR444" and 22.06 mass% of "IBOA (SR506-A)" as resin (A), and 14.71 mass% of "CN9047" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Comparative Example 7 were similar to those in Comparative Example 3.
[0233] In Comparative Example 7, the weighted average functional group of resin (A) was 1.47, and A / B was 2.18.
[0234] In Comparative Example 7, the glass transition temperature Tg was 102.7℃. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.2455.
[0235] In the folding test of Comparative Example 7, there was no change even after folding the film 200K. However, in Comparative Example 7, the water contact angle before the abrasion test was 113.5°, and the water contact angle after the abrasion test was 70.3°. Visible scratches were confirmed.
[0236] As described above, in Comparative Example 7, the weighted average functional group of the resin (A) contained in the resin composition was 1.47. Accordingly, the glass transition temperature Tg of Comparative Example 7 was increased to 102.7°C. The loss tangent tangent tanδ at the glass transition temperature Tg of Comparative Example 7 was increased to 0.2455. That is, since Comparative Example 7 has a high tanδ, the crosslinking density is low and it has flexibility, so it showed good results in the folding test, but it is presumed that visible scratches were confirmed after the wear test because the hardness became too low.
[0237] [Comparative Example 8]
[0238] As shown in Table 5, the resin composition of Comparative Example 8 contained 4.9 mass% of "SR444" and 19.61 mass% of "IBOA (SR506-A)" as resin (A), and 17.16 mass% of "CN9047" as resin (B). The energy beam active polymerization initiator, solvent, metal oxide nanoparticles, and fluorine compound contained in the resin composition of Comparative Example 8 were similar to those in Comparative Example 3.
[0239] In Comparative Example 8, the weighted average functional group of resin (A) was 1.50, and A / B was 1.73.
[0240] In Comparative Example 8, the glass transition temperature Tg was 93.2°C. The loss tangent tangent tan δ at the glass transition temperature Tg was 0.2183.
[0241] In the folding test of Comparative Example 8, there was no change even after folding the film 200K. However, in Comparative Example 8, the water contact angle before the abrasion test was 107°, and the water contact angle after the abrasion test was 65°. Visible scratches were confirmed.
[0242] As described above, in Comparative Example 8, the weighted average functional group of the resin (A) contained in the resin composition was 1.50. Consequently, the loss tangent tan δ at the glass transition temperature Tg of Comparative Example 8 increased to 0.2183, and the hardness became too low. Because of this, the water contact angle after the wear test of Comparative Example 8 was lowered to 65°, and it is presumed that visible scratches were confirmed.
[0243] As described above, according to the present embodiment, a hard coat film (10) can be provided that has the ability to withstand repeated folding multiple times, as well as scratch resistance and abrasion resistance.
[0244] The embodiments of the present invention have been described above with reference to the accompanying drawings. However, the invention disclosed herein is not limited thereto, and those skilled in the art will understand that various changes and modifications may be made within the scope of this disclosure and claims.
[0245] The hard coat film (10) of the present invention can be employed as a protective film in all devices requiring a protective film, such as display screens, screens, goggles, eye shields, and face shields of display devices. The hard coat film (10) disclosed above is particularly suitable for flexible displays used in a bendable (foldable) manner, electronic devices such as information terminals, and all other similar articles.
[0246] When the hard coat film (10) of the present disclosure is employed in a display device, the hard coat film (10) may have a functional material layer and / or an adhesive layer for improving visibility. Examples of the functional material layer may include a diffusion layer, an anti-reflection layer, etc. Examples of the adhesive layer may include an optical elastic resin layer, etc. Explanation of the symbols
[0247] 10 Hard Coat Film 11 entries 12 hard coating layers 12a First region 12b Second area 13 Antifouling layer 100 manufacturing devices 110 Streaming Roll 112 coil roll 114a~d Guide Roll 120 dispensing device 130 drying device 140 curing device 144 Guide Roll 146 Guide Roll 148 light sources
Claims
Claim 1 A hard coat film comprising: a substrate; and a hard coating layer laminated on the substrate, the hard coat film comprising a cured product of a resin composition containing resin (A) and resin (B), wherein the resin (A) is a polyfunctional (meth)acrylic monomer having a weighted average functional group of 4 or more, and the resin (B) is an aliphatic urethane acrylate, wherein the glass transition temperature Tg of the hard coating layer is 50°C or higher and 100°C or lower, and the loss tangent tanδ at the glass transition temperature Tg is 0.07 or higher and 0.15 or lower, and the loss tangent tanδ of the hard coating layer is measured by dynamic viscoelasticity measurement applying a dynamic load at a frequency of 1 Hz. Claim 2 A hard coat film according to claim 1, wherein the resin composition further comprises metal oxide nanoparticles having an average particle size of 100 nm or less. Claim 3 A hard coat film according to claim 2, wherein the content of the metal oxide nanoparticles contained in the resin composition is 2 mass% or more and 5 mass% or less of the total solid content of the resin composition of the hard coating layer. Claim 4 A hard coat film according to claim 2, wherein the metal oxide constituting the metal oxide nanoparticles is either or both of silica and alumina. Claim 5 In claim 2, the metal oxide nanoparticles are a hard coat film having a Mohs hardness greater than 6. Claim 6 A hard coat film according to claim 1, wherein when abrasion is performed by using a wear tester with steel wool #0000 and abrading the surface of the hard coating layer with the steel wool under conditions of load: 1000 g, speed: 50 mm / sec, reciprocating distance: 40 mm, and number of reciprocating cycles: 2500, the water contact angle of the surface of the hard coating layer after abrasion is greater than 100°. Claim 7 In claim 6, a hard coat film in which the water contact angle of the surface of the hard coating layer before wear is greater than 110°. Claim 8 A hard coat film according to claim 7, wherein the reduction in the water contact angle after wear relative to the water contact angle of the surface of the hard coating layer before wear is less than 13%. Claim 9 A hard coat film according to claim 7, wherein the content of the resin (A) contained in the resin composition is greater than 2 times and less than 9 times the content of the resin (B). Claim 10 A hard coat film according to claim 9, wherein the content of the resin (A) contained in the resin composition is 20 mass% or more and 40 mass% or less, and the content of the resin (B) contained in the resin composition is 2 mass% or more and 15 mass% or less. Claim 11 A hard coat film according to claim 1, wherein the hard coat film is configured to be foldable by either in-bending or out-bending at least 100,000 times without causing cracking, interlayer separation, or loss of optical properties. Claim 12 A hard coat film according to claim 1, wherein the substrate is a thermoplastic substrate having a thickness of 10 μm or more and 200 μm or less. Claim 13 A hard coat film according to claim 1, wherein the resin composition contains a fluorine compound, and the fluorine compound is segregated in a first region located on the surface side of the hard coating layer. Claim 14 In claim 13, the segregated fluorine compound provides an antifouling effect, a hard coat film. Claim 15 In claim 13, the fluorine compound is segregated on the surface of the hard coating layer, a hard coat film. Claim 16 In claim 11, the hard coat film is configured to be foldable by either in-bending or out-bending at least 100,000 times without loss of optical properties, wherein the optical properties are one or more selected from the group consisting of total light transmittance (%), transmittance haze, glossiness, and chromaticity b* (intensity of color from blue to yellow). Claim 17 In claim 13, a hard coat film in which the fluorine compound is not segregated in the second region located on the substrate side of the hard coating layer.
Citation Information
Patent Citations
Polymer gels and polymer gel sheets
JP5775475B2
Flexible hardcoat compositions, articles, and methods
US20090004478A1
Hard coat film, polarizing plate and liquid crystal display device
US20120295040A1
Method for measuring dynamic viscoelasticity of particulate material
US20140102223A1
Pressure sensitive adhesive, curable pressure sensitive adhesive composition, pressure sensitive adhesive sheet and method for manufacturing thereof
US20190233681A1