bioelectrode

A laminated bioelectrode with a non-conductive fiber substrate and conductive carbon black layer addresses flexibility and conductivity issues, ensuring stable biosignal acquisition and comfort.

KR103046140B1Active Publication Date: 2026-11-10TORAY INDUSTRIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
KR1020227044722
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-29
Filing Date
2021-09-21
Publication Date
2026-11-10
Estimated Expiration
2041-09-21

AI Technical Summary

Technical Problem

Existing bioelectrodes, particularly those with conductive wire substrates like stainless steel or silicone rubber, suffer from low flexibility, skin peeling, and misalignment during biosignal acquisition due to wearer movement, while non-conductive fiber substrates lack sufficient conductivity.

Method used

A bioelectrode with a laminated structure comprising a non-conductive fiber substrate layer and a conductive layer made of carbon black, urethane resin, and a water-based thickener, with a mixed layer of fibers and conductors, achieving a volume resistivity of 1×10⁶ Ω·cm or smaller and a surface resistance value of 1×10⁹ Ω or greater.

Benefits of technology

The bioelectrode provides flexibility, high comfort, and excellent conductivity, reducing positional misalignment and enhancing biosignal acquisition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022137153974-PCT00003_ABST
    Figure 112022137153974-PCT00003_ABST
Patent Text Reader

Abstract

In order to make a textile-shaped bioelectrode that is flexible, highly comfortable to wear, and unlikely to cause positional misalignment, the bioelectrode has a laminated structure of a fiber substrate layer composed of non-conductive fibers and a conductive layer, wherein the conductive layer is a layer formed of a conductor containing carbon black, urethane resin, and a water-based thickener.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a bioelectrode. Background Technology

[0002] Various types of bioelectrodes are used to measure bioelectrical signals, such as brain waves, electrocardiograms, and electromyograms in humans or animals, or to apply electrical stimulation to the body, including gel electrodes, rubber electrodes, electrodes using metal foils, and electrodes using conductive fiber materials.

[0003] While the gel electrodes or rubber electrodes mentioned above have the advantage of being highly flexible and adhering to the surface of the body to enable stable acquisition of biological signals, they have problems such as poor ventilation, sweating at the contact points, and staining.

[0004] In addition, electrodes using metal sheets were hydrophobic, hard, and had a problem of being unsuitable for applications involving contact with flexible biological surfaces due to their high moisture content. To adhere to the body surface, high contact pressure was required, or a conductive paste (jelly) had to be used.

[0005] Textile-shaped electrodes with conductivity are considered effective as electrodes that can be directly attached to the surface of a living body without using conductive paste, and various proposals have been made. Textile electrodes are resistant to bending and can change shape to conform to the irregularities of the body surface.

[0006] In textile-shaped electrodes, metal plating, coating of conductive polymers, and the use of carbon materials have been proposed to impart conductivity. Carbon is widely used for industrial purposes because it is unlikely to cause allergic reactions or metal corrosion and is also inexpensive.

[0007] As a textile electrode using carbon, an electrode in which carbon black powder is added to silicone rubber has been proposed (see Patent Documents 1 and 2). Prior art literature

[0008] Japanese Patent Publication No. 2006-512128, International Publication No. 2017 / 199026 The problem to be solved

[0009] The bioelectrodes described in Patent Document 1 and Patent Document 2 both have a substrate composed of conductive wires, such as stainless steel, or a substrate composed of conductive wires. Additionally, the use of silicone rubber is exemplified for these bioelectrodes. Substrates composed of conductive wires, such as stainless steel, and substrates composed of conductive wires tend to have lower flexibility compared to substrates composed of non-conductive fibers. Furthermore, the silicone material included in these bioelectrodes has interfacial characteristics with excellent release properties. Consequently, these bioelectrodes are prone to skin peeling during use, which may cause misalignment of the bioelectrode due to the wearer's movement during biosignal acquisition, potentially leading to an arch defect in bioelectrodes that acquire or input weak signals. On the other hand, when non-conductive fibers are used, sufficient conductivity may not be obtained.

[0010] In light of the above, the present invention aims to provide a bioelectrode in the shape of a textile that is flexible, has high comfort when worn, and is unlikely to cause positional misalignment. means of solving the problem

[0011] The configuration of the invention for solving the above problem and achieving the objective is any one of the following.

[0012] (1) A bioelectrode having a laminated structure of a fiber substrate layer composed of non-conductive fibers and a conductive layer, wherein the conductive layer is a layer formed of a conductor containing carbon black, urethane resin and a water-based thickener.

[0013] (2)(1) In this case,

[0014] A bioelectrode having a mixed layer in which fibers and conductors are mixed between the fiber substrate layer and the conductor layer.

[0015] (3)(2) In this case,

[0016] A bioelectrode having a mixed layer ratio of 0.1 to 80%, wherein the value of the thickness of the mixed layer is obtained by multiplying the value obtained by dividing the value of the thickness of the mixed layer by the sum of the thicknesses of the conductor layer, the mixed layer, and the fiber substrate layer provided by the bioelectrode, and the thickness of the conductor layer is 1 to 200 μm.

[0017] (4) In any one of (1) to (3),

[0018] A bioelectrode in which the above-mentioned aqueous thickener is a polyacrylic acid-based compound.

[0019] (5)(1) to (4) any one of them,

[0020] A bioelectrode comprising at least one type of urethane resin selected from the group consisting of ether-based urethane resin and carbonate-based urethane resin.

[0021] (6) In any one of (1) to (5),

[0022] The volume resistivity of the above bioelectrode is 1×10 6 Bioelectrode with a Ω·cm or smaller.

[0023] (7) In any one of (1) to (6),

[0024] The surface resistance value of the above fiber substrate layer is 1×10 10 Bioelectrode with an Ω or greater. Effects of the invention

[0025] The present invention provides a bioelectrode in the shape of a textile, which is flexible, has high comfort when worn, has excellent conductivity, and is difficult to cause misalignment. Brief explanation of the drawing

[0026] FIG. 1 is a conceptual diagram of a cross-section of a bioelectrode representing one embodiment of the present invention. Specific details for implementing the invention

[0027] Hereinafter, embodiments of the bioelectrode according to the present invention will be described in detail. Furthermore, the present invention is not limited by these embodiments.

[0028] Bioelectrodes

[0029] The bioelectrode of the present invention has a laminated structure comprising a fiber substrate layer composed of non-conductive fibers and a conductive layer, wherein the conductive layer serves as a contact surface with the body and acquires and transmits biological signals. Here, the laminated structure may be a laminated structure formed by directly laminating the fiber substrate layer and the conductive layer, or a laminated structure of three or more layers comprising a mixed layer in which fibers and conductors are mixed between the fiber substrate layer and the conductive layer. The conductive layer is a layer formed of a conductor comprising carbon black, urethane resin, and a water-based thickener, and the mixed layer is a layer in which fibers and conductors are mixed. Furthermore, the mixed layer is formed by impregnating the conductor into the non-conductive fibers. FIG. 1 is a conceptual diagram showing a cross-section of one form of the bioelectrode of the present invention, but it is a form obtained by, for example, applying a conductor (1) on a fiber substrate (2), and the bioelectrode has a structure in which a conductor layer (3) composed only of a conductor (i.e., not including a fiber substrate), a mixed layer (4) containing a conductor and a fiber substrate, and a fiber substrate layer (5) composed only of a fiber substrate (i.e., not including a conductor) are stacked.

[0030] <Challenge Layer>

[0031] In the present invention, the conductive layer is a layer that exhibits conductivity and is formed solely of a conductor (i.e., does not include a fiber substrate). The conductor referred to herein is a compound for imparting conductivity to a bioelectrode and comprises (A) carbon black, (B) urethane resin, and (C) a water-based thickener. Furthermore, the compound and the conductive layer may contain other components in addition to (A) carbon black, (B) urethane resin, and (C) a water-based thickener. Examples of other components include (D) a conductivity enhancer, (E) a flexibility enhancer, (F) a surfactant and / or leveling agent, a crosslinking agent, a catalyst, an antifoaming agent, etc., but are not limited thereto.

[0032] <(A) Carbon Black>

[0033] The carbon black used in the present invention (hereinafter referred to as CB) is a conductive material. When imparting conductivity using CB, it is essential to consider the particle diameter forming the base of the CB (the particle diameter of the particles constituting the structure; hereinafter, the particles may be referred to as primary particles and the particle diameter as primary particle diameter), the structure which is a chain structure of primary particles, and the particle surface characteristics. When preparing a solution containing CB and a binder, it is particularly important to increase the specific surface area by modifying the particle surface characteristics. A large specific surface area means that there are many pores on the particle surface, and the binder can enter the pores to reduce the distance between particles, which leads to obtaining high conductivity.

[0034] The specific surface area can be measured by the BET method, and it is preferable that the BET specific surface area of ​​carbon black be 400 to 2000 m² / g or higher. It is more preferable that the BET specific surface area of ​​carbon black be 600 to 1600 m² / g or higher. When the BET specific surface area of ​​carbon black is 400 m² / g or higher, the interparticle distance becomes sufficiently small, which is a range in which sufficient conductivity can be imparted to the bioelectrode, and an even higher conductivity performance is obtained when it is 600 m² / g or higher. By setting the upper limit to 2000 m² / g or lower, the structure can be maintained, and stable conductivity performance can be imparted to the bioelectrode. This effect becomes more pronounced when the BET specific surface area of ​​carbon black is 1600 m² / g or lower.

[0035] In addition, to obtain high conductivity, it is desirable that the primary particles of the CB be small. It is desirable that the average particle diameter of the primary particles of the CB be in the range of 1 to 200 nm, and more desirable that it be in the range of 5 to 100 nm. By making it 1 nm or larger, the robustness against friction of the bioelectrode is achieved, and by making it 5 nm or larger, high robustness is obtained. By making it 200 nm or smaller, sufficient conductivity performance is imparted to the bioelectrode, and by making it 100 nm or smaller, high conductivity is imparted. The primary particle diameter is obtained by observing an ultra-thin section cut from a conductor using a transmission electron microscope (TEM) at any magnification at which the primary particle diameter can be observed, determining the diameter of a circle circumscribing a plurality of arbitrarily selected primary particles from the acquired image, and averaging those values.

[0036] In addition, to obtain high conductivity, it is desirable for the structure to be highly developed, and it is desirable for the dibutyl phthalate (DBP) absorption amount, which is an indicator of the structure size, to be 100 to 600 cm³ / 100g, and more desirable for it to be 300 to 500 cm³ / 100g. By setting it to 100 cm³ / 100g or more, conductivity performance is realized through the development of the structure, and by setting it to 300 cm³ / 100g or more, conductivity performance is further improved. On the other hand, by setting it to 600 cm³ / 100g or less, viscosity can be kept high, allowing sufficient penetration into the interior of the fiber and providing sufficient conductivity performance to the bioelectrode. By setting it to 500 cm³ / 100g or less, the effect becomes more pronounced. The DBP absorption amount is measured using an absorb meter according to the method described in JIS K 6217-4 (2017).

[0037] In the bioelectrode of the present invention, (A) the content of carbon black is not particularly limited, but with respect to 100 parts by weight of solid content of the conductor, the content of CB is preferably 1 part by weight to 60 parts by weight, and more preferably 5 parts by weight to 40 parts by weight. By making it 1 part by weight or more, the conductive performance in the bioelectrode is realized due to the continuity of carbon black, and by making it 5 parts by weight or more, the conductive performance is further improved. In addition, by making the content of CB 60 parts by weight or less and 40 parts by weight or less, fastness against friction of the conductor layer is obtained.

[0038] <(B) Urethane Resin>

[0039] The conductor further contains (B) urethane resin in addition to the above (A) carbon black. Here, the role of (B) urethane resin is to serve as a binder that supports the composition constituting the conductor onto the fiber substrate. Since the flexibility of the bioelectrode is significantly influenced by the binder, it is important that the binder is urethane resin. Because urethane resin has superior flexibility compared to resins other than urethane resin, the bioelectrode of the present invention is flexible and offers excellent comfort when worn.

[0040] (B) Urethane resin can prevent the detachment of the compound constituting the conductor in the bioelectrode from the fiber substrate, reduce skin peeling of the bioelectrode, and improve biosignal acquisition capability. From this point, one of the features of the present invention is that the conductor comprises urethane resin.

[0041] The conductor may be a binder, and may be urethane resin alone or may include one or more other resins. Preferred specific examples of other resins include olefin resin, polyester resin, urethane resin, epoxy resin, silicone resin, vinyl chloride resin, nylon resin, and acrylic resin.

[0042] Urethane resins are classified according to the polyol of the raw material into ether-based, ester-based, carbonate-based, modified polyol, ester / carbonate-based, or polymers combining the same, but all of them can be used. From the perspective of hydrolytic resistance, it is particularly desirable to include at least one type selected from the group consisting of ether-based urethane resins and carbonate-based urethane resins.

[0043] The following commercially available products that can be used as urethane resins may be exemplified. Examples include ether-based urethane resins such as "Rezamin (trademark) D-2040" (DAINICHISEIKA) and "SUPERFLEX (registered trademark) E-4800" (DKS Co., Ltd.), carbonate-based urethane resins such as "EVAFANOL (registered trademark) HA-107C" (NICCA CHEMICAL CO., LTD.), "Rezamin (registered trademark) D-6300" (made by DAINICHISEIKA), "Rezamin (registered trademark) D-6065NP" (DAINICHISEIKA), and "SUPERFLEX (registered trademark) 460" (made by DKS Co., Ltd.), and also polyether / carbonate-based urethane resins such as "Rezamin (registered trademark) D-4080" (DAINICHISEIKA) and "Rezamin (registered trademark) D-4200" (DAINICHISEIKA).

[0044] While urethane resins are derived from aromatic isocyanates and aliphatic isocyanates, from the perspective of toxicity and yellowing, it is preferable to use a urethane resin containing aliphatic isocyanates for applications requiring skin contact or durability, such as bioelectrodes.

[0045] In the bioelectrode of the present invention, from the perspective of the flexibility of the obtained bioelectrode, the glass transition temperature (Tg) of the urethane resin is preferably -60 to ±0°C. The glass transition temperature (Tg) is measured according to the following method. First, a resin solution is introduced into a stainless steel box, dried at 60°C for 1 hour and at 120°C for 2 hours, and a film with a thickness of about 0.3 mm is produced. Using this film, dynamic viscoelasticity is measured at -100 to 200°C using a viscoelasticity measuring device DMS6100 (manufactured by Seiko Instruments Inc.), and the peak temperature (T°C) of the obtained loss viscoelasticity is called the glass transition temperature (Tg). In addition, the measurement is performed at a heating rate of 5°C / min and a measurement frequency of 1 Hz.

[0046] In addition, from the perspective of the friction resistance of the obtained bioelectrode, it is preferable that the tensile strength of the urethane resin component be 5 to 50 MPa. Since the tensile strength of the urethane resin component is 5 MPa or higher, the frictional resistance of the bioelectrode is obtained, and since the tensile strength of the urethane resin component is 50 MPa or lower, the flexibility characteristic of textiles of the bioelectrode can be maintained more reliably.

[0047] In the bioelectrode of the present invention, the content of the urethane resin is not particularly limited, but it is preferably 40 to 98 parts by weight and more preferably 60 to 95 parts by weight per 100 parts by weight of the solid content of the conductor. When the content of the urethane resin is 40 parts by weight or more, the (A) carbon black contained in the bioelectrode becomes more difficult to detach. On the other hand, when the content of the urethane resin is 98 parts by weight or less, it is preferable to secure contact between the carbon blacks in the bioelectrode and to ensure sufficient conductivity when used as an electrode member.

[0048] <(C) Water-based thickener>

[0049] The conductor further contains (C) a water-based thickener in addition to the above (A) carbon black and (B) urethane resin. Here, the role of (C) the water-based thickener is to impart viscous properties to the solution (coating liquid) formed from the mixture constituting the conductor layer in order to control the coating thickness and the degree of penetration of the coating liquid into the fiber substrate when the coating liquid for forming the conductor layer is applied to the fiber substrate. Furthermore, by controlling the coating thickness, the thickness of the conductor layer can be controlled, and a bioelectrode with excellent conductivity can be obtained. Additionally, by controlling the degree of penetration of the coating liquid into the fiber substrate, the thickness of the mixture layer described later can be controlled, and a bioelectrode with excellent conductivity can be obtained.

[0050] (C) Water-based thickeners include water-based solvents for the purpose of reducing VOCs during manufacturing. One type of water-based thickener may be used, or two or more types may be used in combination.

[0051] Examples of water-based thickeners include the following. Examples of inorganic types include silicates and montmorillonite; examples of organic types include cellulose-based carboxymethylcellulose, methylcellulose, hydroxyethylcellulose; vinyl-based polyvinyl alcohol, polyvinylpyrrolidone, polyvinylbenzyl ether copolymers; polyacrylic acid-based polyacrylic acid or polyacrylate, poly(meth)acrylic acid-(meth)acrylic acid ester copolymers, cross-linked core-carboxylic acid emulsions; polyurethane-based polyether-modified urethane compounds, hydrophobic-modified polyoxyethylene polyurethane copolymers, and urea-based urethaneurea compounds.

[0052] Among these, polyacrylic acid-based compounds are preferably used because they can impart thixotropic properties in addition to thickening properties to the coating solution. The coating solution imparted with thickening and thixotropic properties by polyacrylic acid-based compounds obtains excellent characteristics, such as preventing sedimentation during storage and improving workability by reducing viscosity during application.

[0053] In the bioelectrode of the present invention, (C) the content of the aqueous thickener is not particularly limited, but it is preferable to have 0.1 to 10 parts by weight per 100 parts by weight of the solid content of the conductor, and more preferable to have 0.5 to 5 parts by weight. It is preferable to have a content of 0.1 parts by weight or more of the aqueous thickener so that the coating solution forming the conductor of the bioelectrode can be imparted with thickening and thixotropic properties to improve coating performance, and to have a content of 10 parts by weight or less so that coating defects caused by excessive thickening can be suppressed.

[0054] Other Mixtures

[0055] As described above, in the bioelectrode of the present invention, the conductor may contain other components in addition to (A) carbon black, (B) urethane resin, and (C) water-based thickener. Examples of other components include (D) conductivity enhancer, (E) flexibility imparting agent, (F) surfactant and / or leveling agent, crosslinking agent, catalyst, defoamer, etc.

[0056] <(D) Challenge Enhancer>

[0057] (D) A conductivity enhancer may be added to the conductor. (D) A conductivity enhancer is not particularly limited, but examples include a compound having a boiling point of 100°C or higher and having two or more hydroxyl groups in the molecule, a compound having a boiling point of 100°C or higher and having at least one sulfinyl group in the molecule, a compound having a boiling point of 60°C or higher and having at least one carbonyl group in the molecule, and a compound having a boiling point of 100°C or higher and having at least one amide group in the molecule. These (D) conductivity enhancers may be used alone or two or more may be used in combination.

[0058] Examples of compounds having a boiling point of 100°C or higher and having two or more hydroxyl groups in the molecule include ethylene glycol, diethylene glycol, propylene glycol, trimethylene glycol, β-thiodiglycol, triethylene glycol, tripropylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,3-butanediol, 1,6-hexanediol, neopentyl glycol, catechol, cyclohexanediol, cyclohexanedimethanol, glycerin, erythritol, inmatol, lactitol, maltitol, mannitol, sorbitol, xylitol, sucrose, etc. These may be used alone or in combination of two or more.

[0059] Examples of compounds having a boiling point of 100°C or higher and having at least one sulfinyl group in the molecule include dimethyl sulfoxide.

[0060] Examples of compounds having a boiling point of 60°C or higher and having at least one carbonyl group in the molecule include acrylic acid, methacrylic acid, methanoic acid, ethanoic acid, propanoic acid, butanoic acid, pentoic acid, hexanoic acid, octanoic acid, decanoic acid, dodecanoic acid, benzoic acid, p-toluic acid, p-chlorobenzoic acid, p-nitrobenzoic acid, 1-naphthoic acid, 2-naphthoic acid, phthalic acid, isophthalic acid, oxalic acid, malonic acid, succinic acid, adipic acid, maleic acid, fumaric acid, etc. These may be used alone or two or more may be used in combination.

[0061] Examples of compounds having a boiling point of 100°C or higher and having at least one amide group in the molecule include N,N-dimethylacetamide, N-methylformamide, N,N-dimethylformamide, acetamide, N-ethylacetamide, N-phenyl-N-propylacetamide, benzamide, etc. These may be used alone or in combination of two or more types.

[0062] When the conductor contains (D) a conductivity enhancer, the content is not particularly limited, but 0.01 to 20 parts by weight is preferred per 100 parts by weight of the solid content of the conductor, and 0.1 to 10 parts by weight is more preferred. When the content of (D) a conductivity enhancer is 0.01 parts by weight or more, a sufficient conductivity enhancement effect is obtained, and when it is 20 parts by weight or less, the drying properties of the bioelectrode are good.

[0063] <(E)Flexibility Granting System>

[0064] (E) A flexible agent may be added to the conductor. (E) The flexible agent is not particularly limited, but examples include glycerol, sorbitol, polyglycerin, polyethylene glycol, and polyethylene glycol-polypropylene glycol copolymer. These may be used alone or in combination of two or more types.

[0065] When the conductor contains (E) a flexibility agent, the content is not particularly limited, but 0.01 to 20 parts by weight is preferred per 100 parts by weight of the solid content of the conductor, and 0.1 to 10 parts by weight is more preferred. When the content of (E) a flexibility agent is 0.01 parts by weight or more, sufficient flexibility is obtained, and when it is 20 parts by weight or less, the conductivity or strength of the bioelectrode is excellent and the washability is not significantly reduced.

[0066] <(F) Surfactants and / or leveling agents>

[0067] In the present invention, a surfactant to uniformly disperse the composition constituting the conductor within the conductor, or a leveling agent to homogenize the surface tension during drying of the bioelectrode may be added to the conductor. Furthermore, in the bioelectrode of the present invention, a single compound may correspond to either the surfactant or the leveling agent. Additionally, if the surfactant and the leveling agent are different compounds, the surfactant and the leveling agent may be used in combination.

[0068] As for the surfactant, it is preferable that it possesses dispersibility of the solid component in a solvent, and specific examples thereof include, for instance, siloxane-based compounds such as polyether-modified polydimethylsiloxane, polyether-modified siloxane, polyetherester-modified hydroxyl-containing polydimethylsiloxane, polyether-modified acrylic-containing polydimethylsiloxane, polyester-modified acrylic-containing polydimethylsiloxane, perfluoropolydimethylsiloxane, perfluoropolyether-modified polydimethylsiloxane, and perfluoropolyester-modified polydimethylsiloxane; fluorine-containing organic compounds such as perfluoroalkylcarboxylic acid and perfluoroalkyl polyoxyethyleneethanol; polyether-based compounds such as polyoxyethylenealkylphenyl ether, propylene oxide polymer, and ethylene oxide polymer; and carboxylic acids such as palm oil fatty acid amine salt and gum rosin. Examples include ester compounds such as castor oil sulfate esters, phosphate esters, alkyl ether sulfates, sorbitan fatty acid esters, sulfonic acid esters, and succinic acid esters; sulfonate compounds such as alkylarylsulfonate amine salts and sodium dioctyl sulfosuccinate; phosphate compounds such as sodium lauryl phosphate; amide compounds such as palm oil fatty acid ethanolamides; and acrylic compounds. These surfactants may be used alone or in combination of two or more types.

[0069] Leveling agents are not particularly limited and include, for example, siloxane-based compounds such as polyether-modified polydimethylsiloxane, polyether-modified siloxane, polyetherester-modified hydroxyl-containing polydimethylsiloxane, polyether-modified acrylic-containing polydimethylsiloxane, polyester-modified acrylic-containing polydimethylsiloxane, perfluoropolydimethylsiloxane, perfluoropolyether-modified polydimethylsiloxane, and perfluoropolyester-modified polydimethylsiloxane; fluorine-containing organic compounds such as perfluoroalkylcarboxylic acids and perfluoroalkylpolyoxyethyleneethanol; polyether-based compounds such as polyoxyethylenealkylphenyl ether, propylene oxide polymer, and ethylene oxide polymer; carboxylic acids such as palm oil fatty acid amine salts and gum rosin; and ester-based compounds such as castor oil sulfate esters, phosphate esters, alkyl ether sulfates, sorbitan fatty acid esters, sulfonic acid esters, and succinic acid esters. Examples include sulfonate compounds such as alkylarylsulfonate amine salts and sodium dioctyl sulfosuccinate; phosphate compounds such as sodium lauryl phosphate; and amide compounds such as palm oil fatty acid ethanolamide. These leveling agents may be used alone or in combination of two or more.

[0070] Fiber substrate layer

[0071] As the fiber constituting the fiber substrate layer provided by the bioelectrode of the present invention, metal fibers such as stainless steel, aluminum, aluminum alloy, or copper, metal film fibers coated with metals such as silver, or conductive fibers spun using a resin blended with metal or carbon are not used, and non-conductive fibers are used. The term "non-conductive" as used herein refers to 1×10⁻⁶ 10 It is to have a surface resistance value of Ω or greater. Non-conductive fibers tend to be easier to obtain compared to conductive fibers, and the bioelectrode of the present invention has excellent productivity.

[0072] The non-conductive fibers constituting the fiber substrate layer used in the present invention may be natural fibers or chemical fibers. Examples of natural fibers include cellulose-based fibers such as cotton or hemp, and protein fibers such as wool or silk. Examples of chemical fibers include regenerated fibers such as rayon, semi-synthetic fibers such as acetate, and synthetic fibers. From the perspective of processability, it is preferable that the fibers constituting the fiber substrate layer used in the present invention be synthetic fibers.

[0073] Examples of synthetic fibers include polyamide fibers such as nylon and aramid, polyester fibers such as polyethylene terephthalate, acrylic fibers such as polyacrylonitrile, polyolefin fibers such as polyethylene and polypropylene, polyvinyl alcohol fibers, polyvinyl chloride fibers, polyurethane fibers, polyimide fibers, and heterocyclic polymer fibers. In particular, it is preferable to use one or more types of polyamide fibers, polyester fibers, and polyolefin fibers from the perspective that high flexibility can be imparted by the bioelectrode.

[0074] In the bioelectrode of the present invention, the cross-sectional shape of the fiber constituting the fiber substrate layer may be a round cross-section, a triangular cross-section, a flat cross-section, a polygonal cross-section, a hollow shape, or other shapes with a high degree of irregularity, and is not particularly limited.

[0075] Examples of the form of the fiber substrate layer according to the present invention include mesh, paper, woven fabric, knitted fabric, nonwoven fabric, ribbon, string, etc. The form may be suitable for the intended use and is not particularly limited, but nonwoven fabric or woven fabric is preferred from the perspective of conductivity and processability.

[0076] In the case of nonwoven fabric, it is desirable to have high water pressure resistance. It is more desirable to have a performance of 50 mmH2O (490 Pa) or higher, and 100 mmH2O (980 Pa) or higher. As a means of achieving water pressure resistance, the above range can be achieved by a laminated structure of a spun bond layer and a melt blow layer, an increase in weight per unit area of ​​the nonwoven fabric, and embossing.

[0077] In the case of a fabric, it is preferable that the sum of the cover factors of the warp and weft yarns, respectively, is 1500 or more and 3000 or less, with respect to the cover factor calculated by multiplying the square root of the fineness by the yarn density. If the cover factor is small, the coating agent may reach the back side, and there is a risk that the fiber base layer will not function as an insulating layer. On the other hand, fabrics with a cover factor exceeding 3000 have reduced weaving performance.

[0078] The form of the fiber can be monofilament, multifilament, or staple yarn.

[0079] The single fiber fineness is not particularly limited, and for example, 0.0001 dtex to 300 dtex is exemplified.

[0080] In addition to fiber bonding and napping, many treatments such as shrinkage treatment, shape fixing treatment, compression treatment, dyeing finishing treatment, oiling treatment, heat setting treatment, solvent removal, shape fixing agent removal, combing treatment, polishing treatment, flat (roll) breath treatment, and high-performance short cut shirring treatment (hair cutting) are appropriately combined in each process on the fiber substrate layer, but the implementation is not limited as long as the performance as an electrode is not impaired.

[0081] In addition, it is preferable that the fiber substrate layer has a unit per unit area of ​​5 g / m² or more and 500 g / m² or less. Since the unit per unit area is 5 g / m² or more, the fabric is not excessively thin and the bioelectrode has sufficient strength, and since the unit per unit area is 500 g / m² or less, it has good flexibility. More preferably, it is 10 g / m² or more and 250 g / m² or less.

[0082] In addition, when the surface resistance value of the fiber substrate layer is measured in the fiber substrate unit by the method described below, it is 1×10 10 It is preferable that it be Ω or greater. The above surface resistance value is 1×10 10 By having a value of Ω or higher, the occurrence of stiffness in the bioelectrode when a conductive layer is applied can be further suppressed, and consequently, the wearing comfort becomes superior. Furthermore, if conductive threads or conductive wires such as stainless steel are used, the resistance value in the fiber substrate alone is reduced, and the surface resistance value is 1×10 10 It tends to be less than Ω. In addition, the surface resistance value is 1×10 10 If the conductivity is Ω or higher, meaning the conductivity of the fiber substrate itself is low, the fiber substrate layer can be utilized more effectively as an insulating layer. In addition, if the surface resistance value is 1×10 18 An example is provided of using a fluorine-based polymer as a fiber substrate exceeding Ω. In addition to the above, in the view that the applicability of the processing agent becomes better, the surface resistance value is 1×10⁻⁶ 18 It is desirable that the value be Ω or less. In addition, the surface resistance value of such fiber substrates can be controlled by selecting the polymer that forms the fiber substrate or by limiting the application of conductive material during or after the formation of the substrate.

[0083] Mixed layer

[0084] In the present invention, the conductive layer is supported on the fiber substrate layer, but it is preferable to have a mixed layer between the conductive layer and the fiber substrate layer. Here, the mixed layer is a layer in which fibers and conductors are mixed, and the conductors are inserted into the fiber gaps. By having the mixed layer, the adhesion between the conductive layer and the fiber substrate layer becomes strong, and delamination between the layers during use becomes difficult. It is preferable to install the mixed layer such that the mixed layer ratio, measured by the method described below, is 80% or less. The mixed layer ratio is more preferably 0.1% or more and 80% or less, and even more preferably 0.5% or more and 50% or less. Here, as described below, the mixed layer ratio refers to a value obtained by multiplying the value obtained by dividing the thickness of the mixed layer by the sum of the thicknesses of the conductive layer, the mixed layer, and the fiber substrate layer provided by the bioelectrode by 100.

[0085] <Other Components of the Bioelectrode>

[0086] In the bioelectrode of the present invention, a resin layer may be laminated on the surface opposite to the conductive layer which is the bio-contact surface, or fibers or films may be laminated. The resin, fibers, or films may be laminated for purposes such as insulation of electrical stimulation, moisture permeability, and moisturization.

[0087] <Mixed layer ratio and conductor layer thickness in bioelectrodes>

[0088] The ratio of the mixed layer and the thickness of the conductive layer of the bioelectrode of the present invention can be controlled by the selection of a thickener, the amount of thickener mixed in the coating solution, and the selection, fineness, and density of the polymer constituting the fiber substrate. When the ratio of the mixed layer is measured by the measurement method described in the section of the examples below, it is preferable that the ratio of the mixed layer be 0.1% or more and 80% or less, and more preferable that it be 0.5% or more and 50% or less.

[0089] The mixed layer ratio mentioned here specifically refers to a value obtained by multiplying the value of the thickness of the mixed layer provided by the bioelectrode by 100, divided by the sum of the thicknesses of the conductor layer, the mixed layer, and the fiber substrate layer provided by the bioelectrode.

[0090] If the ratio of the mixed layer is excessively high, the resistance value of the bioelectrode increases due to the insulating properties of the fiber substrate, and consequently, conductivity is reduced, which is undesirable. By setting the ratio of the mixed layer to 80% or less, the bioelectrode of the present invention can suppress the resistance value to a low level and provide an electrode with better conductivity. More preferably, it is 50% or less. On the other hand, if the ratio of the mixed layer is low, it is undesirable because delamination tends to occur between the layers of the conductor and the fiber substrate. By setting the ratio of the mixed layer to 0.1% or more, more preferably 0.5% or more, the bioelectrode of the present invention can suppress the occurrence of delamination between the conductor layer and the fiber substrate layer.

[0091] In addition, when measuring the thickness of the conductive layer using the measurement method described in the section of the embodiments below, it is preferable that the thickness be 1 to 200 μm. If the thickness of the conductive layer is excessively thin, the influence of the insulating properties of the fiber substrate becomes strong, which tends to increase the resistance value of the bioelectrode and, consequently, tends to reduce conductivity, so this is undesirable. If the thickness of the conductive layer is excessively thick, the flexibility of the fiber substrate is easily damaged, resulting in rigidity, and there is a risk that the comfort of wearing may be compromised. By setting the thickness of the conductive layer of the bioelectrode of the present invention to 1 to 200 μm, it is possible to provide an electrode that achieves both conductivity and flexibility at a higher level.

[0092] In addition, from the perspective that it is possible to provide an electrode with better conductivity by keeping the resistance value low and preventing delamination between the conductor layer and the fiber substrate layer, and also excellent flexibility, it is particularly desirable that the ratio of the mixed layer be 0.1 to 80% and the thickness of the conductor layer be 1 to 200 μm.

[0093] Method for manufacturing bioelectrodes

[0094] The bioelectrode of the present invention is obtained by forming a laminated structure of a fiber substrate layer and a conductive layer by applying a conductive coating solution, for example, containing (A) carbon black, (B) urethane resin, and (C) a water-based thickener, onto the surface of a fiber substrate layer. Furthermore, as the coating solution, it is preferable to use a dispersion solution containing (A) carbon black, (B) urethane resin, and (C) a water-based thickener, or a solution containing (A) carbon black, (B) urethane resin, and (C) a water-based thickener, and apply it onto the surface of the fiber substrate layer. Additionally, in this specification, there is no particular distinction between a substance that completely dissolves all components contained in the conductor (i.e., "solvent") and a substance that disperses insoluble components (i.e., "dispersion medium"), and both are referred to as "solvent." The solvent will be described below.

[0095] <Solvent>

[0096] The above solvent is not particularly limited and, for example, water; alcohols such as methanol, ethanol, 2-propanol, 1-propanol, and glycerin; ethylene glycols such as ethylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mononormal butyl ethyl ether, diethylene glycol monomethyl ether, ethylene glycol diethyl ether, and diethylene glycol dimethyl ether; glycol ether acetates such as ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate; and propylene glycols such as propylene glycol, dipropylene glycol, and tripropylene glycol. Examples include propylene glycol ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, propylene glycol diethyl ether, and dipropylene glycol diethyl ether; propylene glycol ether acetates such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, dipropylene glycol monomethyl ether acetate, and dipropylene glycol monoethyl ether acetate; tetrahydrofuran; acetone; acetonitrile, etc. These solvents may be used alone or in combination of two or more types.

[0097] The solvent is preferably water or a mixture of water and an organic solvent. When water is included as the solvent, the amount of water is not particularly limited, but 10 to 1,000 parts by weight is preferred and 20 to 500 parts by weight is more preferred per 100 parts by weight of the solid content of the conductor. By having a water content of 10 parts by weight or more, the fluidity of the mixture in the solution is ensured, and handling is improved. By having a water content of 1,000 parts by weight or less, the concentration of the mixture does not become excessively low, and the amount of coating solution used does not increase excessively.

[0098] In the present invention, when applying a conductive coating solution onto a fiber substrate layer, conventional methods such as immersion, coating, or spraying may be used, and a bioelectrode can be obtained by laminating the coating solution onto the fiber substrate and then heating. A coating method is preferred in that it allows the conductive coating solution to be applied with a uniform thickness.

[0099] (A) It is preferable that the carbon black be mixed with (E) a surfactant in advance and be uniformly dispersed in the solvent, and also that the dispersibility is maintained even when (B) a urethane resin is mixed. Examples of methods for uniformly dispersing the carbon black in the solvent include, but are not limited to, mechanical stirring methods using a ball mill, bead mill, planetary ball mill, vibrating ball mill, sand mill, colloid mill, atrium, roll mill, high-speed impeller dispersion, disperser, homogenizer, high-speed impact mill, ultrasonic dispersion, stirring blades, stirrers, etc.

[0100] <Forms of Use of Bioelectrodes>

[0101] A preferred form of use for the bioelectrode of the present invention is exemplified by a form capable of acquiring electrical signals and / or providing electrical signals or electrical stimulation by making direct contact with a living body. Examples include electrode members such as electrocardiograms, muscle potentials, and brain waves that acquire electrical signals from a living body, or electrode members such as low frequency, high frequency, and EMS that provide electrical stimulation to a living body.

[0102] Specific examples of products that come into direct contact with the skin include, but are not limited to, electrodes containing the bioelectrode, wires, wear, pants, gloves, socks, bras, headbands, wristbands, scarves, hats, girdle belts, supporters, shoes, seats, glasses, headbands, fur-decorated members, headphones, watches, chairs, toilet seats, handles, beds, carpets, various covers, etc. By attaching, for example, a sensor or an electrical stimulation device to a part of these products so as to establish conductivity with the bioelectrode, they can be made into various products that function as electrode members.

[0103] In the case of the electrode, the form of the electrode alone and / or in combination with the one directly in contact with the skin can be suitably used. The shape of the electrode alone may be any shape, such as a circle or a polygon, and is not limited to any other shape.

[0104] The size of the electrode should be a contact area capable of acquiring the desired biological signal, but it is not limited to that. Since it improves adhesion to the body, a standard flat electrode may be made into a three-dimensional structure, such as a loop shape, to facilitate movement, or it may be inflated with air.

[0105] When used as an electrode in combination with other structures such as clothing, wiring may be attached to the bioelectrode so as to acquire electrical signals from a desired area, and the bioelectrode may also be suitably used in a form that can be attached to clothing by attaching buttons, hooks, magnets, or cotton fasteners such as "Magic Tape" (registered trademark) to the bioelectrode.

[0106] Static friction resistance of bioelectrodes

[0107] The bioelectrode of the present invention can control static friction resistance by appropriately selecting a binder resin. When measuring the static friction resistance (Fs) described below, it is preferable that it be 0.16 N / cm² or higher. If the static friction resistance of the bioelectrode is low, the movement of the wearer during biosignal acquisition may cause misalignment of the bioelectrode, and there is a risk of causing artifacts in bioelectrodes that acquire or input weak signals. Since the bioelectrode of the present invention has high static friction resistance, it can prevent the occurrence of misalignment of the bioelectrode caused by the movement of the wearer.

[0108] Volume resistivity of bioelectrodes

[0109] The volume resistivity of the bioelectrode of the present invention can be controlled by the properties of CB (BET specific surface area or DBP attachment amount), the amount of CB incorporated in the conductor, the ratio of the mixed layer, etc.

[0110] The volume resistivity of the bioelectrode of the present invention is 1×10 when measured by the method described below. 6 It is preferable that it be Ω·cm or less. More preferably, 1×10⁻⁶ -2 Ω·cm or more 1×10 6 It is Ω·cm or less. The volume resistivity is 1×10⁻⁶ 6 Since it is Ω·cm or less, the bioelectrode's biosignal acquisition capability becomes superior. Meanwhile, the volume resistivity is 1×10 -2 By being Ω·cm or higher, the amount of binder containing CB increases, and as a result, the retention power of CB in the bioelectrode is improved, and the detachment of CB from the bioelectrode is further suppressed.

[0111] Examples

[0112] Next, the bioelectrode of the present invention will be described in detail by way of examples. The bioelectrode of the present invention is not limited to these examples. The measured values ​​in the examples and comparative examples were obtained by the following method.

[0113] Static friction resistance of bioelectrodes

[0114] The bioelectrode measured static friction resistance using the method shown below.

[0115] Using a surface texture measuring instrument tribo gear (TYPE: HEIDON-14DR) manufactured by Shinto Scientific Co., Ltd., electrodes were fixed to a flat indenter (area 30×28 mm) with a moving speed of 60 mm / min and a load of 255 g (2.50 N), and static friction resistance (N) was measured by sliding a SUS plate with a surface roughness of 0.8 μm, which was used for imaging, in a perpendicular direction. Three points were measured, and the averaged static friction resistance was divided by the surface area of ​​the flat indenter to obtain the static friction resistance per unit area (N / ㎠). In addition, the load was set to the above load in order to apply an equivalent pressure per area of ​​the flat indenter.

[0116] Surface resistance value of the fiber substrate layer

[0117] The surface resistance (Ω) of the fiber substrate layer of the bioelectrode was measured using a surface electric resistor (Megaresta H0709 manufactured by SHISHIDO ELECTROSTATIC, LTD.) at 500V for 60 seconds under conditions of 20℃ and 40% RH. Three measurements were taken and averaged.

[0118] <Mixed layer ratio of bioelectrodes>

[0119] The ratio of the mixed layer in the bioelectrode was measured by the following method. The electrode was cut with one blade, and a cross-sectional image was acquired at a magnification of 100x using a microscope (KEYENCE CORPORATION VHX-2000). Using measurement mode, the thickness of the conductor layer formed solely by the conductor (μm), the thickness of the fiber substrate layer formed solely by the fiber substrate layer (μm), and the thickness of the mixed layer (μm) in which the conductor and fiber are mixed between the conductor layer and the fiber substrate layer were measured, respectively.

[0120] A specific method for measuring the thickness of each layer from a cross-sectional image is explained in detail with reference to FIG. 1. Any three locations where the conductor penetrates from the surface side of the conductor layer toward the fiber substrate layer are selected, and at each location, the combined thickness of the conductor layer and the mixed layer is measured and the average value is denoted as A. Additionally, any three other locations where the conductor penetrates the fiber substrate are selected, and the combined thickness of the fiber substrate layer and the mixed layer is measured and the average value is denoted as B. Additionally, any three other locations are selected, and the thickness from the surface on the conductor layer side to the surface on the fiber substrate layer side is measured as the sum of the conductor layer, the mixed layer, and the fiber substrate layer (bioelectrode thickness), and the average value is denoted as C. The thickness of the mixed layer is calculated as (A+B)-C and is denoted as D. The thickness of the conductor layer is calculated as AD. The thickness of the fiber substrate layer is calculated as BD. In addition, the mixed layer ratio (%) refers to a value obtained by multiplying the value obtained by dividing the thickness of the mixed layer by the sum of the thicknesses of the conductor layer, the mixed layer, and the fiber substrate layer provided by the bioelectrode, by 100. In addition, if there are irregularities such as embossing on the surface of the substrate and the layer thickness varies depending on the location, an image is acquired at the part in contact with the body and the layer thickness is measured.

[0121] <Resistance and Volume Resistivity of Bioelectrodes>

[0122] Measurements were taken using the five-point measurement method specified in JIS K 7194 (1994). The resistance value (Ω) of the bioelectrode was measured using a resistance meter (Mitsubishi Chemical Analytech Co., Ltd. 4-probe resistance meter Loresta-AX MCP-T370) under conditions of 20°C and 40% RH. Additionally, the thickness value of the bioelectrode used to calculate the volume resistivity was the sum of the thicknesses of the conductor layer and the mixed layer. The electrode was cut with one blade, and an image was acquired at a magnification of 100x using a microscope (KEYENCE CORPORATION VHX-2000). Using the measurement mode, the thickness of the conductor layer formed solely of the conductor (μm) and the thickness of the mixed layer (μm) between the conductor layer and the fiber substrate layer, where the conductor and fiber are mixed, were measured. The volume resistivity (Ω·cm) was calculated from the obtained resistance value, thickness, and the correction factor specified in JIS.

[0123] <Ratio of change in stiffness of bioelectrode>

[0124] The magnification of the change in stiffness of the bioelectrode was calculated by measuring the stiffness of the bioelectrode (mm) and the stiffness of the fiber substrate before conductive processing (mm) respectively according to the stiffness A method (45° cantilever method) of JIS L 1096 (Test method for raw fabrics of woven and knitted fabrics) (1999), dividing the stiffness of the bioelectrode by the stiffness of the fiber substrate, and calculating the magnification of the change in stiffness of the bioelectrode. Meanwhile, the stiffness measurement samples were taken such that the length was in the longitudinal direction or the well direction, and measurements were performed on the front and back sides and then averaged.

[0125] Strong peeling of the entire conductive layer

[0126] The following method was performed by reference to the peel strength test method of JIS L 1066 (2004). Three test specimens measuring 15 × 2.5 cm were prepared with the longitudinal direction of the sample as the length direction. For each test specimen, with the conductive layer accurately peeled 5 cm in the longitudinal direction of the test specimen, a low-speed elongation type tensile testing machine equipped with a magnetic recording device was used. The peeled portion of the conductive layer and the remaining portion of the substrate were gripped at a distance of 5 cm, and the conductive layer was peeled another 5 cm at a tensile speed of 10 cm / min, and the load (N) at that time was measured. From the load-peel distance curve, three points with the largest maximum value (N) and three points with the smallest minimum value (N) were taken, and their average value was calculated. This was performed for each test specimen, and the average was calculated and referred to as peel strength. A case where the peel strength is 30 cN / cm or more is denoted as A, and a case where the peel strength is less than 30 cN / cm is denoted as B, and in the case of A, it is determined that it maintains sufficient peel strength as a bioelectrode.

[0127] [Example 1]

[0128] Polyester filament of 84dtex-72F was used, and a circular knitted fabric with a smooth structure was knitted using a circular knitting machine. The obtained circular knitted fabric was scoured with a 3 mass% aqueous solution of sodium hydroxide (at 80°C for 20 minutes), washed with water (at 50°C for 10 minutes), and heat-set in a dry heat treatment machine (at 180°C for 1 minute) to obtain a fiber substrate. The obtained fiber substrate had a weight of 150 g / m² per unit area. A mixed solution comprising (A) 400 g / L of “LION PASTE (registered trademark) W-311N” (KETJENBLACK dispersion manufactured by LION SPECIALTY CHEMICALS CO., Ltd., containing carbon black as a conductive material), (B) 500 g / L of “EVAFANOL (registered trademark) HA-107C” (water-based urethane resin manufactured by NICCA CHEMICAL CO., LTD., as a binder), and (C) 40 g / L of “SN Thickener 920” (acrylate from Sanop Corporation, as a water-based thickener) as a water-based thickener was applied to the obtained fiber substrate using a bar coater and heated at 130°C to obtain a bioelectrode. The characteristics of the material used and the obtained bioelectrode are shown in Table 1.

[0129] [Example 2]

[0130] A bioelectrode was prepared by performing the same treatment as in Example 1, except that the fiber substrate was changed to nylon jersey. The nylon jersey was produced by making a circular knit using nylon 6 filaments of 70d-24F and 78T / 2-24F in a well and course, and the fiber substrate was obtained by performing the same treatment as in Example 1. The obtained fiber substrate had a weight of 260 g / m² per unit area. The characteristics of the materials used and the obtained bioelectrode are shown in Table 1.

[0131] [Example 3]

[0132] A bioelectrode was manufactured by performing the same treatment as in Example 1, except that a three-layer laminated nonwoven fabric of a polypropylene-based melt-blown fiber web, a spunbond fiber web, and a melt-blown fiber web was used as the fiber substrate. The weight per unit area of ​​the fiber substrate was 65 g / m². The water pressure resistance was 1091 mmH2O. The characteristics of the materials used and the obtained bioelectrode are shown in Table 1.

[0133] [Example 4]

[0134] A bioelectrode was prepared by the same method as in Example 3, except that the binder was changed to “SUPERFLEX (registered trademark) E-4800” (DKS Co., Ltd., polyether-based urethane resin). The materials used and the characteristics of the obtained bioelectrode are shown in Table 1.

[0135] [Example 5]

[0136] A bioelectrode was prepared by the same manufacturing method as in Example 4, except that the ratio of the mixed layer was changed to 0.4%. The characteristics of the materials used and the obtained bioelectrode are shown in Table 1.

[0137] [Example 6]

[0138] A bioelectrode was prepared by the same manufacturing method as in Example 1, except that the ratio of the mixed layer was changed to 57%. The characteristics of the materials used and the obtained bioelectrode are shown in Table 1.

[0139] [Example 7]

[0140] A bioelectrode was manufactured by the same manufacturing method as in Example 1, except that the fiber substrate was changed to a polyester fabric and the blending layer ratio was changed to 24%. Polyester filaments of 84dtex-72F were used as the fiber substrate, and a plain weave fabric was produced using a loom. The obtained fabric was scoured with an aqueous solution of 0.5 g / L surfactant and 0.7 g / L sodium hydroxide (at 80°C for 20 minutes), washed with water (at 50°C for 10 minutes), and heat-set in a dry heat treatment machine (at 180°C for 1 minute) to obtain a fiber substrate. The weight of the obtained fiber substrate was 110 g / m² per unit area. The cover factor of the obtained fiber substrate was 2300. The characteristics of the materials used and the obtained bioelectrode are shown in Table 1.

[0141] [Comparative Example 1]

[0142] A bioelectrode was prepared by performing the same treatment as in Example 1, except that no thickener was added. The materials used and the characteristics of the obtained bioelectrode are shown in Table 2.

[0143] [Comparative Example 2]

[0144] A bioelectrode was prepared by the same manufacturing method as in Example 3, except that the binder was changed to "High Resin SD-319" (TAKAMATSU OIL&FAT CO., LTD., silicone resin). The materials used and the characteristics of the obtained bioelectrode are shown in Table 2.

[0145] [Comparative Example 3]

[0146] A bioelectrode was prepared by the same manufacturing method as in Example 3, except that the binder was changed to "KM-9772" (Shin-Etsu Chemical Co., Ltd., silicone rubber). The materials used and the characteristics of the obtained bioelectrode are shown in Table 2.

[0147]

[0148]

[0149] Since the bioelectrode of the example contains a water-based thickener, the ratio of the mixed layer within the electrode is reduced, thereby realizing an excellent volume resistivity. This is thought to enable biosignal acquisition at high sensitivity. Furthermore, because the static friction resistance is very high, it is expected to prevent positional misalignment when worn and prevent the occurrence of artifacts during biosignal acquisition. Additionally, since a non-conductive fiber substrate is used and a flexible urethane resin is used as a binder, it offers excellent wearing comfort. On the other hand, since Comparative Example 1 does not contain a thickener, the ratio of the mixed layer within the electrode is high, resulting in a high volume resistivity, and there is concern regarding a decrease in biosignal acquisition performance compared to the example. Moreover, since Comparative Examples 2 and 3 do not use a urethane-based binder, the static friction resistance is low, causing positional misalignment when worn and raising concerns about the occurrence of artifacts during biosignal acquisition.

[0150] (Industrial Applicability)

[0151] The bioelectrode of the present invention is suitablely used as a bioelectrode for measuring bioelectrical signals, such as brain waves, electrocardiograms, and electromyograms, in humans or animals, or for applying electrical stimulation to the body. Explanation of the symbols

[0152] 1: Conductor 2: Fiber substrate 3: Conductor layer 4: Mixed layer 5: Fiber substrate layer

Claims

Claim 1 A bioelectrode having a laminated structure of a fiber substrate layer composed of non-conductive fibers and a conductor layer, wherein the conductor layer is a layer formed of a conductor containing carbon black, urethane resin, and a water-based thickener, and having a mixed layer between the fiber substrate layer and the conductor layer in which fibers and conductors are mixed, wherein the value of the thickness of the mixed layer is a value obtained by multiplying the value obtained by dividing the value of the thickness of the conductor layer, the mixed layer, and the fiber substrate layer provided by the bioelectrode by 100, and the ratio of the mixed layer is 0.1 to 80%, and the thickness of the conductor layer is 1 to 200 μm. Claim 2 In claim 1, the form of the fiber substrate layer is one of woven, knitted, or nonwoven fabric, the ratio of the blended layer is 0.5 to 50%, and the static friction resistance (Fs) is 0.16 N / cm 2 Bioelectrode with abnormal characteristics. Claim 3 A bioelectrode according to claim 1 or 2, wherein the aqueous thickener is a polyacrylic acid-based compound. Claim 4 A bioelectrode according to claim 1 or 2, wherein the urethane resin comprises at least one type selected from the group consisting of ether-based urethane resin and carbonate-based urethane resin. Claim 5 In claim 1 or 2, the volume resistivity of the bioelectrode is 1×10 6 Bioelectrode with a Ω·cm or smaller. Claim 6 In claim 1 or 2, the surface resistance value of the fiber substrate layer is 1×10 10 Bioelectrode with an Ω or greater. Claim 7 delete

Citation Information

Patent Citations

  • Biomedical electrode structural body

    JP2001190694A

  • Electrode configuration

    JP2006512128A

  • Conductive polymer fibers, and biological electrode

    JP2015037695A

  • Multifilament yarn and fiber structure prepared using the same

    JP2015140493A

  • Fabric electrode

    JP2017218690A