Free cutting steel and method for manufacturing the same

The free-cutting steel with controlled composition and manufacturing process achieves improved hole machinability and fine grain size by suppressing central segregation, addressing the challenges of machining stress and mechanical property deviations.

KR103046241B1Active Publication Date: 2026-11-11HYUNDAE STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020250002479
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-01-07
Publication Date
2026-11-11
Estimated Expiration
2045-01-07

AI Technical Summary

Technical Problem

Existing methods for manufacturing free are not specified in the patent text. The patent is about free-cutting steel and its manufacturing process, so there is no technical problem specified in the patent text. The patent aims to provide a free-cutting steel with improved hole machinability and fine grain size through the suppression of central segregation.

Method used

The free-cutting steel composition includes specific weight percentages of elements such as C, Si, Mn, S, Cr, Cu, Ni, Al, and Ti, with controlled grain sizes and hardness variations, manufactured using a continuous casting process with electromagnetic stirrers to suppress central segregation.

Benefits of technology

The solution results in free-cutting steel with improved hole machinability and fine grain size, reducing machining stress and mechanical property deviations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025002335206-PAT00007_ABST
    Figure 112025002335206-PAT00007_ABST
Patent Text Reader

Abstract

The present application relates to free-cutting steel and a method for manufacturing the same. According to the present application, a free-cutting steel and a method for manufacturing the same can be provided, which secure fine grain size and improve hole machinability by suppressing central segregation.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present application relates to free-cutting steel and a method for manufacturing the same. Background Technology

[0002] As the automotive industry advances, materials are being developed to meet the diverse demands of parts and improve manufacturing efficiency.

[0003] Among them, free-cutting steel is a steel containing large amounts of Pb, Bi, Te, Mn, S and / or Ca, etc., and has low cutting load during processing and excellent machinability, which enables high-speed cutting. Therefore, it is widely used as a material for parts with complex shapes, and the demand for it is on the rise.

[0004] In particular, lead (Pb) free-cutting steel is the most preferred in industry because its machinability is far superior to that of other elements. However, as regulations regarding environmental pollution issues, such as the Restriction of Hazardous Substances (ROHS) and the Waste Electrical and Electronic Equipment (WEEE) directive, are becoming increasingly stricter, the use of lead free-cutting steel is gradually decreasing, and consequently, the demand for sulfur (S) free-cutting steel, which was previously used, is increasing again.

[0005] Sulfur free-cutting steel has improved machinability by adding various alloying elements or forming MnS inclusions within it. However, in order to secure sufficient MnS, Mn content of about 1.0% or more has been added to sulfur free-cutting steel. At this time, Mn causes center segregation, which leads to problems such as deviations in mechanical properties as well as increased load on the machining tool during hole machining.

[0006] Since free-cutting steel is manufactured into complex shapes mostly through machining without a forging process, a large amount of machining is required. Therefore, when manufacturing free-cutting steel, it is most important to reduce machining stress, mechanical properties, and microstructural variations (control of center segregation) at each machining location.

[0007] Therefore, in order to solve these problems and achieve the objectives, there is a need for a free-cutting steel and a method for manufacturing the same that secures fine grain size and improves hole machinability by suppressing central segregation. The problem to be solved

[0008] The objective of the present application is to provide a free-cutting steel with improved hole machinability and fine grain size through suppression of central segregation, and a method for manufacturing the same. means of solving the problem

[0009] To solve the above problem, the free-cutting steel of the present application comprises, in weight%, C: 0.20% or more and 0.80% or less, Si: 0.30% or less, Mn: 1.20% or more and 1.80% or less, S: 0.15% or more and 0.35% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.02% or more and 0.30% or less, Ni: 0.02% or more and 0.30% or less, Al: 0.050% or less, and Ti: 0.070% or less, and the remainder comprises Fe and other unavoidable impurities, satisfying the following general formula 1.

[0010] [General Formula 1]

[0011] 5 µm ≤ G 0.5D -G 0.1D < 37 µm

[0012] In the above general formula 1, D is the diameter of the free-cutting steel, and G 0.1D is the average grain size (μm) of ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and G 0.5D is the average grain size (μm) of ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0013] The grain size of ferrite measured at a point corresponding to 50% of the diameter from the surface of free-cutting steel may be ASTM grain size number 10.2 or greater.

[0014] In addition, the grain size of the ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel may be ASTM grain size number 11.4 or higher.

[0015] In addition, the above free-cutting steel can satisfy the following general formula 2.

[0016] [General Formula 2]

[0017]

[0018] In the above general formula 2, D is the diameter of the free-cutting steel, and HV 0.1D is the Vickers hardness measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and HV 0.5D is the Vickers hardness measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel, and C 0.3D is the carbon content (weight%) measured at a point corresponding to 30% of the diameter from the surface of the free-cutting steel, and C 0.5D is the carbon content (weight%) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0019] In addition, Vickers hardness (HV) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel 0.5D ) may be 215 HV or less.

[0020] In addition, the method for manufacturing free-cutting steel of the present application comprises the steps of: producing a bloom by continuously casting molten steel, which contains, in weight percent, C: 0.20% or more and 0.80% or less, Si: 0.30% or less, Mn: 1.20% or more and 1.80% or less, S: 0.15% or more and 0.35% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.02% or more and 0.30% or less, Ni: 0.02% or more and 0.30% or less, Al: 0.050% or less, and Ti: 0.070% or less, and the remainder being Fe and other unavoidable impurities, using a continuous casting machine comprising a mold electron stirrer (Mold EMS) and a final electron stirrer (Final EMS); and producing a billet by reheating and rolling the produced bloom. A method for manufacturing free-cutting steel comprising the steps of: reheating a manufactured billet and then rolling it to produce free-cutting steel in the form of a wire rod; coiling the manufactured free-cutting steel; and cooling the coiled free-cutting steel, wherein after cooling, the free-cutting steel satisfies the following general formula 1.

[0021] [General Formula 1]

[0022] 5 µm ≤ G 0.5D -G 0.1D < 37 µm

[0023] In the above general formula 1, D is the diameter of the free-cutting steel, and G 0.1D is the average grain size (μm) of ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and G 0.5D is the average grain size (μm) of ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0024] In addition, after cooling, the free-cutting steel may have a ferrite grain size of ASTM grain size number 10.2 or higher, measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0025] In addition, after cooling, the free-cutting steel may have a ferrite grain size of ASTM grain size number 11.4 or higher, measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel.

[0026] In addition, after cooling, the free-cutting steel can further satisfy the following general formula 2.

[0027] [General Formula 2]

[0028]

[0029] In the above general formula 2, D is the diameter of the free-cutting steel, and HV 0.1D is the Vickers hardness measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and HV 0.5D is the Vickers hardness measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel, and C 0.3D is the carbon content (weight%) measured at a point corresponding to 30% of the diameter from the surface of the free-cutting steel, and C 0.5D is the carbon content (weight%) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0030] In addition, after cooling, the Vickers hardness (HV) of the free-cutting steel measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel 0.5D ) may be 215 HV or less.

[0031] In addition, the current value of the final electronic stirrer may be 300 A or more and 750 A or less.

[0032] In addition, the current value of the above mold electronic stirrer may be 50 A or more and 400 A or less. Effects of the invention

[0033] According to the present application, a free-cutting steel with improved fine grain size and hole machinability through suppression of central segregation and a method for manufacturing the same can be provided. Brief explanation of the drawing

[0034] FIGS. 1 to 5 are optical microscope images of free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, respectively. Figure 6 is a graph showing the Vickers hardness (HV) at different locations of free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, respectively. FIG. 7 is a graph showing the carbon content by position of free-cutting steel prepared in Examples 1 to 3 and Comparative Examples 1 and 2, respectively. FIGS. 8 to 11 are images taken with a digital camera of blooms prepared in Examples 2 and 4, and Comparative Examples 3 and 4, respectively. Specific details for implementing the invention

[0035] The present application relates to free-cutting steel. The free-cutting steel comprises, in weight percent, C: 0.20% or more and 0.80% or less, Si: 0.30% or less, Mn: 1.20% or more and 1.80% or less, S: 0.15% or more and 0.35% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.02% or more and 0.30% or less, Ni: 0.02% or more and 0.30% or less, Al: 0.050% or less, and Ti: 0.070% or less, and the remainder comprises Fe and other unavoidable impurities, and may satisfy the following general formula 1.

[0036] [General Formula 1]

[0037] 5 µm ≤ G 0.5D -G 0.1D < 37 µm

[0038] In the above general formula 1, D is the diameter of the free-cutting steel, and G 0.1D is the average grain size (μm) of ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and G 0.5D is the average grain size (μm) of ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0039] Specifically, the value calculated by the above general formula 1 may have a lower limit of 10 μm or more, 15 μm or more, or 20 μm or more, and an upper limit of 35 μm or less, 33 μm or less, 30 μm or less, or 27 μm or less. By satisfying the aforementioned ranges for the value calculated by the above general formula 1, the free-cutting steel may secure fine grains through the suppression of central segregation and improve hole machinability. In this specification, a point corresponding to 10% of the diameter from the surface of the free-cutting steel may be referred to as the surface portion of the free-cutting steel. Additionally, in this specification, a point corresponding to 50% of the diameter from the surface of the free-cutting steel may be referred to as the center of the free-cutting steel.

[0040] In addition, the grain size of the ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel may be ASTM grain size number 10.2 or higher. Specifically, the grain size of the ferrite measured at the aforementioned point may be ASTM grain size number 10.3 or higher, 10.4 or higher, 10.5 or higher, or 10.6 or higher. In addition, the upper limit of the grain size of the ferrite measured at the aforementioned point may be ASTM grain size number 15.6 or lower, 15.5 or lower, 15.4 or lower, 15.3 or lower, or 15.2 or lower. By satisfying the ASTM grain size number for the ferrite measured at the aforementioned point, the free-cutting steel can secure fine grains and improve hole machinability. In the above free-cutting steel, if the grain size of the ferrite measured at the aforementioned point exceeds the upper limit of the ASTM grain size number range, the grain size becomes very fine, resulting in an increase in strength due to grain strengthening, and as a result, machinability may be reduced.

[0041] In addition, the grain size of the ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel may be ASTM grain size number 11.4 or higher. Specifically, the grain size of the ferrite measured at the aforementioned point may be ASTM grain size number 11.5 or higher. In addition, the upper limit of the grain size of the ferrite measured at the aforementioned point may be ASTM grain size number 16.4 or lower. The free-cutting steel can secure fine grains and improve hole machinability by satisfying the ASTM grain size number for the ferrite measured at the aforementioned point.

[0042] In another example, the above free-cutting steel can satisfy the following general formula 2.

[0043] [General Formula 2]

[0044]

[0045] In the above general formula 2, D is the diameter of the free-cutting steel, and HV 0.1D is the Vickers hardness measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and HV 0.5D is the Vickers hardness measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel, and C 0.3D is the carbon content (weight%) measured at a point corresponding to 30% of the diameter from the surface of the free-cutting steel, and C 0.5D is the carbon content (weight%) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. According to the free-cutting steel of the present application, fine grain size and hole machinability can be improved by suppressing central segregation.

[0046] Specifically, the value calculated by the above general formula 2 may be 2.03 or higher and 2.80 or lower, 2.05 or higher and 2.60 or lower, 2.08 or higher and 2.40 or lower, or 2.10 or higher and 2.20 or lower. The above free-cutting steel can improve hole machinability and secure fine grains by suppressing central segregation by satisfying the aforementioned range of values ​​calculated by the above general formula 2.

[0047] In one example, Vickers hardness (HV) measured at a point corresponding to 50% of the diameter from the surface of free-cutting steel 0.5D The Vickers hardness of the free-cutting steel measured at the aforementioned point may be 215 HV or less. Specifically, the Vickers hardness of the free-cutting steel measured at the aforementioned point may be 214 HV or less, 213 HV or less, or 212 HV or less. In addition, the lower limit of the Vickers hardness of the free-cutting steel measured at the aforementioned point is not specifically limited, but may be, for example, 200 HV or more, and specifically, 202 HV or more, 204 HV or more, or 206 HV or more. By satisfying the aforementioned range of Vickers hardness measured at the aforementioned point, the free-cutting steel can secure fine grains through suppression of central segregation and improve hole machinability.

[0048] The specific alloy composition of the above free-cutting steel is explained below.

[0049] C: 0.20 wt% or more, 0.80 wt% or less

[0050] Carbon (C) is an element added to ensure strength and hardness. As carbon is a major element determining the strength and hardness of steel, increasing its content increases strength but decreases toughness. If the carbon is included in the free-cutting steel below the lower limit of the aforementioned range, it may be difficult to secure sufficient hardness. Furthermore, if the carbon is included in the free-cutting steel above the upper limit of the aforementioned range, it may be difficult to secure the desired strength. Accordingly, the carbon may be included in the free-cutting steel in an amount of 0.20 wt% or more and 0.80 wt% or less, and specifically, in an amount of 0.30 wt% or more and 0.65 wt% or less, or in an amount of 0.40 wt% or more and 0.50 wt% or less.

[0051] Si: 0.30 wt% or less

[0052] The silicon (Si) mentioned above is an element added to ensure strength and provide a deoxidation effect. The silicon is used as one of the powerful deoxidizers during steelmaking operations, such as aluminum (Al), and reduces oxide inclusions within the steel. If the silicon is included in the free-cutting steel at a level below the lower limit of the aforementioned range, the aforementioned effect may not occur. Furthermore, if the silicon is included in the free-cutting steel at a level exceeding the upper limit of the aforementioned range, strength is improved, but machinability may be reduced due to solid solution strengthening of the ferrite phase. Accordingly, the silicon may be included in the free-cutting steel at 0.30 wt% or less, specifically, at 0.25 wt% or less, 0.20 wt% or less, or 0.15 wt% or less. Additionally, the lower limit of the silicon content included in the free-cutting steel may be 0 wt% or more, specifically, at more than 0 wt%, 0.5 wt% or more, or 0.10 wt% or more.

[0053] Mn: 1.20 wt% or more, 1.80 wt% or less

[0054] Manganese (Mn) is an element used as a deoxidizer in the production of molten steel and acts to improve machinability by forming MnS. If the manganese is included in the free-cutting steel in an amount less than the lower limit of the aforementioned range, it does not form a good spherical MnS shape and promotes FeS, which is a cause of brittleness, so brittleness may occur during hot rolling. In addition, if the manganese is included in the free-cutting steel in an amount exceeding the upper limit of the aforementioned range, hardness increases and manufacturing costs may rise. Therefore, the manganese may be included in the free-cutting steel in an amount of 1.20 wt% or more and 1.80 wt% or less, and specifically, in an amount of 1.30 wt% or more and 1.65 wt% or less, and 1.40 wt% or more and 1.50 wt% or less.

[0055] S: 0.15 wt% or more, 0.35 wt% or less

[0056] Sulfur (S) is an element that improves machinability by forming inclusions with manganese (Mn). If the sulfur is included in the free-cutting steel in an amount less than the lower limit of the aforementioned range, the aforementioned effect may be reduced. Furthermore, if the sulfur is included in the free-cutting steel in an amount exceeding the upper limit of the aforementioned range, hot workability may deteriorate due to brittleness caused by FeS. Accordingly, sulfur may be included in the free-cutting steel in an amount of 0.15 wt% or more and 0.35 wt% or less, and specifically, in an amount of 0.20 wt% or more and 0.30 wt% or less.

[0057] Cr: 0.02 wt% or more, 0.30 wt% or less

[0058] Chromium (Cr) is an element that improves hardenability. When chromium is added during the manufacturing process of free-cutting steel, it lowers the solubility of sulfur in the molten state and combines with MnS non-metallic inclusions to precipitate (Mn, Cr)S, thereby improving machinability. If the chromium is included in the free-cutting steel below the lower limit of the aforementioned range, it may be difficult to obtain the desired hardenability. Furthermore, if the chromium is included in the free-cutting steel in excess of the aforementioned range, the hardness may be increased more than necessary, which may reduce machinability. Accordingly, the chromium may be included in the free-cutting steel in an amount of 0.02 wt% or more and 0.30 wt% or less, and specifically, in an amount of 0.05 wt% or more and 0.25 wt% or less, 0.08 wt% or more and 0.20 wt% or less, or 0.10 wt% or more and 0.15 wt% or less.

[0059] Cu: 0.02 wt% or more, 0.30 wt% or less

[0060] Copper (Cu) is an element that increases strength and improves corrosion resistance. If the copper is included in the free-cutting steel in an amount less than the lower limit of the aforementioned range, the aforementioned effects may be reduced. Furthermore, if the copper is included in the free-cutting steel in an amount exceeding the upper limit of the aforementioned range, it may cause a significant decrease in toughness and become a major cause of surface cracks caused by hot working during the manufacturing process. Accordingly, the copper may be included in the free-cutting steel in an amount of 0.02 wt% or more and 0.30 wt% or less, and specifically, in an amount of 0.05 wt% or more and 0.20 wt% or less, or in an amount of 0.08 wt% or more and 0.10 wt% or less.

[0061] Ni: 0.02 wt% or more, 0.30 wt% or less

[0062] Nickel (Ni) is an element that contributes to increasing hardenability and improving toughness. If the nickel is included in the free-cutting steel in an amount less than the lower limit of the aforementioned range, the aforementioned effect may be reduced. In addition, if the nickel is included in the free-cutting steel in an amount exceeding the upper limit of the aforementioned range, the cost may increase. Accordingly, the nickel may be included in the free-cutting steel in an amount of 0.02 wt% or more and 0.30 wt% or less, and specifically, in an amount of 0.03 wt% or more and 0.20 wt% or less, or in an amount of 0.04 wt% or more and 0.10 wt% or less.

[0063] Al: 0.050 wt% or less

[0064] Aluminum (Al) is an element that can achieve a grain refinement effect by forming nitrides such as AlN through combination with nitrogen, and acts as a strong carbonate agent during steel manufacturing to control oxide-type non-metallic inclusions in the steel. If the above aluminum is included in the free-cutting steel in an amount exceeding the upper limit of the aforementioned range, it can form alumina (Al2O3), a hard inclusion, thereby deteriorating machinability. Accordingly, the above aluminum may be included in the free-cutting steel in an amount of 0.050 wt% or less, specifically, 0.030 wt% or less or 0.010 wt% or less. Additionally, the lower limit of the aluminum content included in the free-cutting steel may be 0 wt% or more, specifically, greater than 0 wt% or 0.001 wt% or more.

[0065] Ti: 0.070 wt% or less

[0066] Titanium (Ti) is an element capable of obtaining fine grains by forming titanium oxide (Ti2O3) or TiN or TiC carbonitrides. Since TiN and Ti2O3 precipitates act as nucleation sites for MnS, fine MnS, which is advantageous for machinability in free-cutting steel, can be secured. If the titanium is included in the free-cutting steel in an amount exceeding the upper limit of the aforementioned range, it may be disadvantageous from an economic perspective. Therefore, the titanium may be included in the free-cutting steel in an amount of 0.070 wt% or less, specifically, 0.050 wt% or less, 0.030 wt% or less, or 0.010 wt% or less. Additionally, the lower limit of the titanium content included in the free-cutting steel may be 0 wt% or more, specifically, greater than 0 wt% or 0.001 wt% or more.

[0067] Remaining Fe and other unavoidable impurities

[0068] The above-mentioned unavoidable impurities are impurities that are unintentionally incorporated from raw materials or the surrounding environment during the normal manufacturing process. Since this is widely known in the art, a detailed description is omitted. In one embodiment of the present application, the addition of elements other than the components of the free-cutting steel described above is not excluded, and various elements may be included within a scope that does not impair the technical concept of the present application. If additional elements are included, they may be included to replace the remainder of iron (Fe).

[0069] In one example, the free-cutting steel may have a machining stress of 550 N or more and less than 608 N measured at a point corresponding to 50% of the diameter from the surface. Specifically, the machining stress of the free-cutting steel measured at the aforementioned point may have a lower limit of 560 N or more, 570 N or more, 580 N or more, or 590 N or more, and an upper limit of 607 N or less, 606 N or less, 605 N or less, 604 N or less, or 603 N or less. The hole machining of the free-cutting steel may be improved by the machining stress measured at the aforementioned location satisfying the aforementioned range.

[0070] The present application also relates to a method for manufacturing free-cutting steel. The method for manufacturing free-cutting steel relates to a method for manufacturing free-cutting steel, and since specific details regarding the free-cutting steel described below can be applied in the same way as those described for free-cutting steel, they will be omitted.

[0071] The above method for manufacturing free-cutting steel comprises the steps of manufacturing a bloom, manufacturing a billet, manufacturing free-cutting steel, coiling, and cooling, and after cooling, the free-cutting steel satisfies the above general formula 1. According to the above method for manufacturing free-cutting steel, since the free-cutting steel satisfies the above general formula 1 after cooling, it is possible to manufacture free-cutting steel with improved hole machinability and fine grain size through the suppression of central segregation. A detailed explanation of the above general formula 1 is the same as that described in the above free-cutting steel, so it will be omitted.

[0072] The step of manufacturing the above bloom is a step of manufacturing a bloom through a continuous casting process using molten steel containing, in weight percent, C: 0.20% or more and 0.80% or less, Si: 0.30% or less, Mn: 1.20% or more and 1.80% or less, S: 0.15% or more and 0.35% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.02% or more and 0.30% or less, Ni: 0.02% or more and 0.30% or less, Al: 0.050% or less, and Ti: 0.070% or less, and the remainder being Fe and other unavoidable impurities, and is performed through a continuous casting machine including a mold electron stirrer (Mold EMS) and a final electron stirrer (Final EMS). Since the specific description of the composition of the above molten steel is the same as that described in the above free-cutting steel, it will be omitted.

[0073] The above-mentioned mold electromagnetic stirrer (Mold EMS) is a device located at the top of a continuous casting machine that applies an electromagnetic field to unsolidified molten steel to force the molten steel to flow, thereby improving the casting structure. By stirring the molten steel, the expansion of the equiaxed grain structure is facilitated, and defects such as pore pipes and central segregation can be reduced. For example, the current value of the above-mentioned mold electromagnetic stirrer may be 50 A or more and 400 A or less. By satisfying the aforementioned range of the current value of the above-mentioned mold electromagnetic stirrer, the crystal grain size of the free-cutting steel after cooling, including the aforementioned general formula 1, Vickers hardness, general formula 2, and ferrite, can be controlled within the aforementioned range. Consequently, it is possible to manufacture free-cutting steel with improved hole machinability and fine crystal grains by suppressing central segregation.

[0074] In addition, the Final Electron Stirrer (Final EMS) is a device located at the end of the continuous casting machine to suppress central segregation, and the current value of the Final Electron Stirrer may be 300 A or more and 750 A or less. By satisfying the aforementioned range of the current value of the Final Electron Stirrer, the continuous casting machine can control the crystal grain size of the free-cutting steel after cooling to the aforementioned general formula 1, Vickers hardness, general formula 2, and ferrite within the aforementioned range, and as a result, it is possible to manufacture free-cutting steel with improved hole machinability and fine crystal grains through the suppression of central segregation.

[0075] The step of manufacturing the billet is a step of manufacturing a billet, which is an intermediate material before the bloom manufactured in the step of manufacturing the bloom is finally processed into a wire-shaped free-cutting steel, and is performed by reheating the manufactured bloom and then rolling it.

[0076] For example, the step of manufacturing the billet may be performed by reheating the bloom at a temperature of 1100°C or higher and 1250°C or lower, and then rolling it. By satisfying the aforementioned range of reheating temperatures, fine dispersion may be possible through redeposition of composite precipitates within the matrix following redesolution. If the reheating temperature is below the lower limit of the aforementioned range, the rolling force may increase, placing a load on the rolling rolls, and the surface quality of the rolled billet may deteriorate. Additionally, if the reheating temperature exceeds the upper limit of the aforementioned range, it may place a load on the equipment furnace.

[0077] The step of manufacturing the above free-cutting steel is a step of manufacturing free-cutting steel in the form of a wire rod having a desired diameter by rolling a billet, and is performed by reheating the billet manufactured in the step of manufacturing the billet in a heating furnace and then rolling it in a rolling mill.

[0078] For example, the step of manufacturing the free-cutting steel may be performed by reheating the billet at a temperature of 1000°C or higher and 1170°C or lower for at least 90 minutes, and then hot rolling. The upper limit of the reheating time may be 800 minutes or less. In the step of manufacturing the free-cutting steel, if the reheating is performed below the lower limit of the aforementioned temperature range and for less than the lower limit of the aforementioned time range, the surface quality of the product may deteriorate due to the temperature drop and the rolling roll may be subjected to a load. Additionally, if the reheating is performed above the upper limit of the aforementioned temperature range and for more than the upper limit of the aforementioned time range, the decarburization reaction may be maximized, and the surface quality of the product after rolling may deteriorate due to surface decarburization.

[0079] In one example, the hot rolling may be performed through a hot rolling mill at an inlet temperature of 850°C or higher and 1000°C or lower. If the inlet temperature of the hot rolling mill during the hot rolling is below the lower limit of the aforementioned range, surface defects such as roll wear and folding may occur due to increased rolling force. Additionally, if the inlet temperature of the hot rolling mill during the hot rolling exceeds the upper limit of the aforementioned range, localized grain coarsening or surface decarburization may occur on the product surface, and product surface roughness defects may occur. Therefore, the hot rolling may be performed at the inlet temperature of the hot rolling mill mentioned above.

[0080] The above-mentioned winding step is a step of winding the free-cutting steel manufactured in the step of manufacturing the above-mentioned free-cutting steel.

[0081] For example, in the above-mentioned winding step, the winding may be performed at a temperature of 800°C or higher and 870°C or lower. If the winding temperature is below the lower limit of the aforementioned range during winding, the probability of low-temperature structure formation and the strength of the product may increase, thereby reducing processability. Additionally, if the winding temperature exceeds the upper limit of the aforementioned range during winding, the quality of the scale may deteriorate. Specifically, if the winding temperature exceeds the upper limit of the aforementioned range during winding, blister-shaped scale may form due to the thermal expansion coefficient of the scale FeO and the product, the scale may grow thickly at high temperatures, and a scale phase unfavorable for pickling may be formed.

[0082] The above cooling step is a step of cooling the coiled free-cutting steel.

[0083] For example, the cooling step may be performed by cooling the coiled free-cutting steel at a cooling rate of 3.0 ℃ / s or less. In the cooling step, the lower limit of the cooling rate may be 0.5 ℃ / s or more. By performing the cooling step at a cooling rate within the aforementioned range, the free-cutting steel after cooling can be controlled to have the aforementioned general formula 1, Vickers hardness, general formula 2, and ferrite grain size within the aforementioned range, and as a result, free-cutting steel with improved hole machinability and fine grain size can be manufactured by suppressing central segregation.

[0084] For example, after cooling, the free-cutting steel may have a ferrite grain size of ASTM grain size number 10.2 or higher, measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Since the specific description of the ferrite grain size measured at the aforementioned point is the same as that described in the above free-cutting steel, it will be omitted.

[0085] In addition, after cooling, the free-cutting steel may have a ferrite grain size of ASTM grain size number 11.4 or higher, measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel. Since the specific description of the ferrite grain size measured at the aforementioned point is the same as that described in the above free-cutting steel, it will be omitted.

[0086] In addition, the free-cutting steel after cooling may further satisfy the above general formula 2. Since the specific explanation of the above general formula 2 is the same as that described in the above free-cutting steel, it will be omitted.

[0087] In addition, after cooling, the Vickers hardness (HV) of the free-cutting steel measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel 0.5D ) may be 215 HV or less. A detailed explanation of the Vickers hardness of the free-cutting steel after cooling, measured at the aforementioned point, is omitted as it is the same as that described in the above free-cutting steel.

[0088] In addition, the processing stress of the free-cutting steel after cooling may be 550 N or more and less than 608 N when measured at a point corresponding to 50% of the diameter from the surface. Since the specific description of the processing stress of the free-cutting steel after cooling measured at the aforementioned point is the same as that described for the free-cutting steel above, it will be omitted.

[0090] The present application will be described in more detail below through embodiments according to the present application and comparative examples not according to the present application, but the scope of the present application is not limited by the embodiments presented below.

[0092] Example 1

[0093] Manufacturing of free-cutting steel

[0094] A molten steel containing the components shown in Table 1 below, the remainder of Fe, and other unavoidable impurities was continuously cast to produce a bloom using the current values ​​of the mold electron stirrer and the final electron stirrer shown in Table 2 below, the produced bloom was reheated at 1150°C for 150 minutes, then rolled to produce a billet, the produced billet was reheated at 1100°C for 90 minutes, then hot-rolled at the inlet temperature of a hot rolling mill at 900°C, and subsequently coiled at 870°C and cooled at a cooling rate of 3.0°C / s or less to produce free-cutting steel.

[0095] Composition of molten steel (weight%) C Si Mn S Cr Cu Ni Al Ti 0.43 0.12 1.48 0.273 0.13 0.09 0.04 0.002 0.002

[0097] Examples 2 to 4 and Comparative Examples 1 to 4

[0098] Manufacturing of free-cutting steel

[0099] Free-cutting steel was manufactured in the same manner as in Example 1, except that the current values ​​of the mold electronic stirrer and the final electronic stirrer were changed to the current values ​​shown in Table 2 below, respectively.

[0100] Current value (A) Mold electronic stirrer Final electronic stirrer Example 1 50 750 Example 2 200 750 Example 3 400 750 Example 4 200 300 Comparative Example 1 0 0 Comparative Example 2 0 750 Comparative Example 3 200 0 Comparative Example 4 200 200

[0102] Evaluation Example 1. Analysis and Evaluation of Central Segregation

[0103] After etching the free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2 with a 3% Nital solution, the presence of segregation at a point corresponding to 50% of the diameter from the surface was analyzed using an optical microscope at ×50 magnification, and the results are shown in FIGS. 1 to 5 and Table 4 below.

[0105] Evaluation Example 2. Evaluation of Ferrite Grain Size

[0106] For the free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, the ASTM grain size number of the ferrite crystal grain size at each location was measured using an image analyzer of an optical microscope, and the results are shown in Table 4 below. In this case, a smaller ASTM grain size number indicates a larger crystal grain size.

[0108] Evaluation Example 3. Evaluation of satisfaction of General Formula 1

[0109] For the free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, the grain size of ferrite at different locations was measured using an image analyzer of an optical microscope, and then the satisfaction of the following general formula 1 was evaluated, and the results are shown in Table 4 below.

[0110] [General Formula 1]

[0111] 5 µm ≤ G 0.5D -G 0.1D < 37 µm

[0112] In the above general formula 1, D is the diameter of the free-cutting steel, and G 0.1D is the average grain size (μm) of ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and G 0.5D is the average grain size (μm) of ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0114] Evaluation Example 4. Hardness Evaluation

[0115] Vickers hardness (HV) at different locations was measured for the free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, respectively, and the results are shown in FIG. 6 and Table 4 below.

[0117] Evaluation Example 5. Evaluation of satisfaction of General Formula 2

[0118] For the free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, the carbon content at each location was measured using a carbon thermogravimetric analyzer, and the satisfaction of the following general formula 2 was evaluated using the measured carbon content at each location and the Vickers hardness at each location measured above, and the results are shown in FIG. 7 and Table 4 below.

[0119] [General Formula 2]

[0120]

[0121] In the above general formula 2, D is the diameter of the free-cutting steel, and HV 0.1Dis the Vickers hardness measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and HV 0.5D is the Vickers hardness measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel, and C 0.3D is the carbon content (weight%) measured at a point corresponding to 30% of the diameter from the surface of the free-cutting steel, and C 0.5D is the carbon content (weight%) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel.

[0123] Evaluation Example 6. Evaluation of Hole Machinability

[0124] For the free-cutting steels prepared in Examples 1 to 3 and Comparative Examples 1 and 2, the center processing stress was measured under the processing conditions shown in Table 3 below to evaluate the hole machinability, and the results are shown in Table 4 below.

[0125] Processing conditions processing equipment Machining Center (VX 500) insert tip TIAlN Carbide Drill (Φ10) - DPPA02100 (YG Co.) odd number 1 Machining depth (mm) 45 Rotation speed (RPM) 3000 Feed rate (mm / rev) 0.05 Coolant Wet (Howton Sol 2700 / 8%)

[0127] Mold electronic stirrer Final electronic stirrer central stone Grain Size (ASTM No.) Calculated value of General Formula 1 (㎛) Hardness (HV) Calculated value of General Formula 2 Core processing stress (N) surface heart surface heart Example 1 50 750 X 11.5 10.6 24 223 212 2.11 603 Example 2 200 750 X 11.6 10.6 27 219 212 2.10 602 Example 3 400 750 X 11.6 10.7 24 219 207 2.13 592 Comparative Example 1 0 0 O 10.9 9.2 65 215 260 1.78 610 Comparative Example 2 0 750 O 11.3 10.1 37 207 221 1.94 608 Surface: A point corresponding to 10% of the diameter from the surface of the free-cutting steel Center: A point corresponding to 50% of the diameter from the surface of the free-cutting steel O: Center segregation occurs X: No center segregation occurs

[0128] As shown in FIGS. 1 to 5 and Table 4 above, it was confirmed that the free-cutting steels prepared in each of Examples 1 to 3 suppressed center segregation, unlike the free-cutting steels prepared in Comparative Examples 1 and 2. In addition, it was confirmed that the free-cutting steels prepared in each of Examples 1 to 3, unlike the free-cutting steels prepared in Comparative Examples 1 and 2, suppressed center segregation, so the calculated values ​​of General Formula 1, the calculated values ​​of General Formula 2, and the grain size of ferrite satisfied a specific range, and as a result, the processing stress at the center was lower than that of the free-cutting steels prepared in Comparative Examples 1 and 2, respectively, thus having excellent hole machinability.

[0130] Evaluation Example 7. Evaluation of the occurrence of internal cracks and central pores in the bloom

[0131] In Examples 2 and 4, and Comparative Examples 3 and 4, the surface of the bloom produced during the manufacture of free-cutting steel was photographed with a digital camera, and the occurrence of internal cracks and central pores was evaluated. The results are shown in FIGS. 8 to 11 and Table 5 below.

[0132] Bloom quality internal crack central pore Example 2 X X Example 4 X X Comparative Example 3 O O Comparative Example 4 O O

[0133] As shown in FIGS. 8 to 11 and Table 5 above, it was confirmed that the blooms prepared in Examples 2 and 4, respectively, did not have internal cracks or central pores, unlike the blooms prepared in Comparative Examples 3 and 4, respectively. That is, if internal cracks and central pores are present, as in the blooms of Comparative Examples 3 and 4, the interior is not homogeneous after rolling, which can lead to non-uniformity in structure and hardness, thereby reducing processability and formability. Therefore, the evaluation of Evaluation Examples 1 to 6 for Comparative Examples 3 and 4 was omitted.

Claims

Claim 1 A free-cutting steel comprising, in weight%, C: 0.20% or more and 0.80% or less, Si: 0.30% or less, Mn: 1.20% or more and 1.80% or less, S: 0.15% or more and 0.35% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.02% or more and 0.30% or less, Ni: 0.02% or more and 0.30% or less, Al: 0.050% or less, and Ti: 0.070% or less, and the remainder being Fe and other unavoidable impurities, in the form of a wire rod, and satisfying the following general formula 1: [General Formula 1] 5 μm ≤ G 0.5D -G 0.1D < 37 μm In the above general formula 1, D is the diameter of the free-cutting steel, and G 0.1D is the average grain size (μm) of ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and G 0.5D is the average grain size (μm) of ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Claim 2 In claim 1, the free-cutting steel having a ferrite grain size of ASTM grain size number 10.2 or higher, measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Claim 3 In claim 1, the free-cutting steel having a ferrite grain size of ASTM grain size number 11.4 or higher, measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel. Claim 4 In claim 1, free-cutting steel satisfying the following general formula 2: [General Formula 2] In the above general formula 2, D is the diameter of the free-cutting steel, and HV 0.1D is the Vickers hardness measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and HV 0.5D is the Vickers hardness measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel, and C 0.3D is the carbon content (weight%) measured at a point corresponding to 30% of the diameter from the surface of the free-cutting steel, and C 0.5D is the carbon content (weight%) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Claim 5 In claim 4, Vickers hardness (HV) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel 0.5D ) is free-cutting steel with a V of 215 HV or less. Claim 6 A step of producing a bloom by continuously casting molten steel, comprising, in weight percent, C: 0.20% or more and 0.80% or less, Si: 0.30% or less, Mn: 1.20% or more and 1.80% or less, S: 0.15% or more and 0.35% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.02% or more and 0.30% or less, Ni: 0.02% or more and 0.30% or less, Al: 0.050% or less, and Ti: 0.070% or less, and the remainder being Fe and other unavoidable impurities, using a continuous casting machine comprising a Mold Electron Stirrer (Mold EMS) and a Final Electron Stirrer (Final EMS); a step of producing a billet by reheating and rolling the produced bloom; a step of producing free-cutting steel in the form of a wire rod by reheating and rolling the produced billet; and the produced free-cutting steel A method for manufacturing free-cutting steel comprising: a step of winding; and a step of cooling the wound free-cutting steel, wherein after cooling, the free-cutting steel is in the form of a wire rod and satisfies the following general formula 1: [General Formula 1] 5 μm ≤ G 0.5D -G 0.1D < 37 μm In the above general formula 1, D is the diameter of the free-cutting steel, and G 0.1D is the average grain size (μm) of ferrite measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and G 0.5D is the average grain size (μm) of ferrite measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Claim 7 In claim 6, a method for manufacturing free-cutting steel in which, after cooling, the free-cutting steel has a ferrite grain size of ASTM grain size number 10.2 or higher, measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Claim 8 In claim 6, a method for manufacturing free-cutting steel in which, after cooling, the free-cutting steel has a ferrite grain size of ASTM grain size number 11.4 or higher, measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel. Claim 9 In claim 6, a method for manufacturing free-cutting steel that further satisfies the following general formula 2 after cooling: [General Formula 2] In the above general formula 2, D is the diameter of the free-cutting steel, and HV 0.1D is the Vickers hardness measured at a point corresponding to 10% of the diameter from the surface of the free-cutting steel, and HV 0.5D is the Vickers hardness measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel, and C 0.3D is the carbon content (weight%) measured at a point corresponding to 30% of the diameter from the surface of the free-cutting steel, and C 0.5D is the carbon content (weight%) measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. Claim 10 In claim 9, the Vickers hardness (HV) of the free-cutting steel after cooling is measured at a point corresponding to 50% of the diameter from the surface of the free-cutting steel. 0.5D A method for manufacturing free-cutting steel in which ) is 215 HV or less. Claim 11 A method for manufacturing free-cutting steel according to claim 6, wherein the current value of the final electronic stirrer is 300 A or more and 750 A or less. Claim 12 A method for manufacturing free-cutting steel according to claim 6, wherein the current value of the mold electron stirrer is 50 A or more and 400 A or less.

Citation Information

Patent Citations

  • Steel wire rod excellent in mechanical descalabilityand manufacturing method thereof

    KR1020030082997A

  • Steel having excellent machinability for mechanical structure

    KR1020130021444A

  • Method for producing steel wire material

    KR1020140076642A

  • Electromagnetic stirring apparatus, and continuous casting method