Bearing steel and method for manufacturing the same
The method addresses central segregation in high-carbon bearing steel by using controlled alloy compositions and casting processes to enhance fatigue life and purity, reducing production costs and emissions.
Patent Information
- Application Number
- KR1020240187424
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-12-16
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-12-16
AI Technical Summary
High-carbon bearing steel experiences central segregation due to low-solubility elements like C, Mn, S, and P, leading to premature fatigue fracture from massive precipitated carbides, which adversely affect fatigue life, and existing methods to address this issue are economically burdensome or environmentally unfriendly.
A manufacturing method for bearing steel with specific alloy compositions and controlled continuous casting processes using electromagnetic stirrers to minimize carbide segregation, combined with precise reheating, rolling, and cooling steps to achieve uniform solidification and refined microstructure.
The method results in bearing steel with improved fatigue life, high cleanliness, reduced production costs, and lower carbon emissions, while maintaining excellent productivity.
Smart Images

Figure 112024139432945-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present application relates to bearing steel and a method for manufacturing the same. Background Technology
[0002] Generally, high-carbon bearing steel is manufactured by soaking a solidified cast billet produced through steelmaking and continuous casting processes, then producing it in the form of bar steel or wire rod through a rolling process, and subsequently coiling and cooling. The bearing steel produced through these processes undergoes spheroidizing heat treatment to be processed into bearing balls or inner and outer rings, and then undergoes heat treatment (quenching, tempering) and grinding processes to be produced as a final bearing product.
[0003] During the casting process of high-carbon bearing steel, as the billet solidifies, low-solubility elements such as C, Mn, S, and / or P are discharged from the solid phase into the liquid phase and diffuse toward the center of the billet thickness, causing central segregation.
[0004] In particular, bearing steel forms massive precipitated carbides in the material's center segregation zone due to its high carbon content. During fatigue testing or actual bearing use, these precipitated carbides trigger premature fatigue fracture, acting as a factor that adversely affects fatigue life.
[0005] To control the above-mentioned large precipitated carbides, methods are used such as removing the central segregation zone through light compression during the continuous casting process as in Patent Document 1, removing the central segregation zone of the cast billet through electromagnetic stirring, or diffusing the precipitated carbides through crack treatment of the cast billet.
[0006] However, in the case of light pressure, there is an economic burden of having to replace the relevant continuous casting equipment. Furthermore, while cracking treatment for the removal of precipitated carbides can effectively remove them by increasing the cracking time, it raises issues regarding reduced productivity due to the extended treatment time and environmental concerns arising from the need to reduce carbon emissions in accordance with recent environmental regulations.
[0007] Therefore, the invention provides bearing steel with improved fatigue life and high purity through a manufacturing method that offers excellent productivity, low production costs, and reduced carbon emissions. Prior art literature
[0008] Korean Published Patent No. 10-2020-0003176 The problem to be solved
[0009] The objective of the present application is to provide a bearing steel having excellent fatigue life and high cleanliness with minimal central segregation and defects within the product.
[0010] In addition, the objective of the present application is to provide a method for manufacturing bearing steel that has excellent productivity, low production costs, and reduced carbon emissions, while simultaneously improving fatigue life and high purity. means of solving the problem
[0011] To solve the above problem, the bearing steel of the present application comprises, in weight%, C: 0.9% or more and 1.3% or less, Si: 1.1% or more and 1.6% or less, Mn: 1.0% or more and 1.5% or less, Ni: 0.2% or more and 0.6% or less, Cr: 1.5% or more and 1.9% or less, and Mo: 0.1% or more and 0.3% or less, and the remainder consists of Fe and other unavoidable impurities, satisfying the following general formula 1.
[0012] [General Formula 1]
[0013] 0 ≤ CN5 3 +CZ6 3 +CZ7 3 ≤ 24
[0014] In the above General Formula 1, CN5, CZ6, and CZ7 are 100 mm taken from bearing steel 2 The degree of carbide segregation of the test specimen with the above cross-sectional area was evaluated based on SEP 1520.
[0015] The above bearing steel may contain an austenite microstructure having a grain size of ASTM grain size number 9.0 or higher and 13.0 or lower.
[0016] In addition, the bearing steel may further include one or more selected from, in weight%, P: greater than 0% and less than or equal to 0.03%, S: greater than 0% and less than or equal to 0.01%, Al: greater than 0% and less than or equal to 0.05%, Ti: greater than 0% and less than or equal to 0.005%, and O: greater than 0% and less than or equal to 0.001%.
[0017] In addition, the method for manufacturing bearing steel of the present application comprises the steps of: continuously casting a molten steel, comprising, in weight percent, C: 0.9% or more and 1.3% or less, Si: 1.1% or more and 1.6% or less, Mn: 1.0% or more and 1.5% or less, Ni: 0.2% or more and 0.6% or less, Cr: 1.5% or more and 1.9% or less, and Mo: 0.1% or more and 0.3% or less, and the remainder being Fe and other unavoidable impurities, using a continuous casting machine including a mold electron stirrer (Mold EMS) to produce a bloom; reheating the produced bloom and rolling it to produce a billet; reheating the produced billet and rolling it to produce a wire rod; winding the produced wire rod; and cooling the wound wire rod, wherein the current value of the mold electron stirrer is 80 A or more and 300 A or less.
[0018] In addition, the manufactured bearing steel can satisfy the following general formula 1.
[0019] [General Formula 1]
[0020] 0 ≤ CN5 3 +CZ6 3 +CZ7 3 ≤ 24
[0021] In the above General Formula 1, CN5, CZ6, and CZ7 are 100 mm taken from bearing steel 2 The degree of carbide segregation of the test specimen with the above cross-sectional area was evaluated based on SEP 1520.
[0022] In addition, the billet produced through the step of producing the above billet can satisfy the following general formula 2.
[0023] [General Formula 2]
[0024] 0 ≤ S 3 +R 3 +C 3 ≤ 24
[0025] In the above general formula 2, S, R, and C are the defects of a test specimen obtained by cutting a billet vertically and etching it, evaluated according to ASTM E381.
[0026] In addition, the manufactured bearing steel may contain an austenite microstructure with a grain size of ASTM grain size number 9.0 or higher and 13.0 or lower.
[0027] In addition, the molten steel may further include one or more selected from, in weight%, P: greater than 0% and less than or equal to 0.03%, S: greater than 0% and less than or equal to 0.01%, Al: greater than 0% and less than or equal to 0.05%, Ti: greater than 0% and less than or equal to 0.005%, and O: greater than 0% and less than or equal to 0.001%.
[0028] In addition, the continuous casting machine further includes a final electronic stirrer (Final EMS), and the current value of the final electronic stirrer may be 350 A or more and 750 A or less.
[0029] In addition, the above continuous casting can be performed at a casting speed of 0.3 m / min or more and 0.8 m / min or less.
[0030] In addition, the step of manufacturing the billet may be performed by reheating the bloom at a temperature of 1100°C or higher and 1300°C or lower for 120 minutes or more and 720 minutes or less, and then hot rolling at a finishing temperature of 1100°C or higher and 1300°C or lower.
[0031] In addition, the step of manufacturing the wire rod may be performed by reheating the billet at a temperature of 950°C or higher and 1200°C or lower for 70 minutes or more and 120 minutes or less, and then hot rolling at a finishing temperature of 900°C or higher and 1150°C or lower.
[0032] In addition, the above-mentioned winding step can be performed by winding at a temperature of 780°C or higher and 950°C or lower.
[0033] Additionally, the cooling step may include a first cooling step of cooling the wound wire to a temperature of 650°C or higher and 750°C or lower at a cooling rate of 2°C / s or higher and 3°C / s or lower, and a second cooling step of cooling the wire that has undergone the first cooling step to a temperature of 550°C or higher and 650°C or lower at a cooling rate of 1°C / s or lower. Effects of the invention
[0034] According to the bearing steel of the present application, there is less central segregation and defects within the product, so it can have excellent fatigue life and high cleanliness.
[0035] In addition, according to the method for manufacturing bearing steel of the present application, it is possible to manufacture bearing steel with excellent productivity, low production costs, reduced carbon emissions, improved fatigue life, and high purity. Brief explanation of the drawing
[0036] Figure 1 is an image taken with an optical microscope at 200x magnification of the average state of the carbide solidification amount (network carbide) at the grain boundary of the bearing steel manufactured in Example 1 of the present application. FIG. 2 is an image taken with an optical microscope at 100x magnification of the lowest position where the carbides of the bearing steel manufactured in Example 1 of the present application are aggregated and dispersed. Figure 3 is an image taken with an optical microscope at 200x magnification of the average state of the carbide solidification amount (network carbide) at the grain boundary of the bearing steel manufactured in Comparative Example 2 of the present application. Figure 4 is an image taken with an optical microscope at 100x magnification of the lowest position where the carbides of the bearing steel manufactured in Comparative Example 2 of the present application are aggregated and dispersed. Figure 5 is an image taken with an optical microscope at 200x magnification of the average state of the carbide solidification amount (network carbide) at the grain boundary of the bearing steel manufactured in Comparative Example 3 of the present application. Figure 6 is an image taken with an optical microscope at 100x magnification of the lowest position where the carbides of the bearing steel manufactured in Comparative Example 3 of the present application are aggregated and dispersed. Figures 7 and 8 are images of the surface of a test specimen obtained from a billet prepared in Example 1 and Comparative Example 1, respectively, taken with a digital camera. Specific details for implementing the invention
[0037] In the description of numerical ranges in this specification, the notation “X~Y” indicates X or greater and Y or less, unless otherwise specifically stated. Additionally, “greater than or equal to” may be replaced with “greater than,” and “less than or equal to” may be replaced with “less than.”
[0038] In addition, regarding the numerical ranges described stepwise in this specification, any upper or lower limit value described in any numerical range may be substituted with an upper or lower limit value of another numerical range described stepwise, or may be substituted with a value shown in the examples.
[0039] The present application relates to bearing steel. The bearing steel comprises, in weight percent, C: 0.9% or more and 1.3% or less, Si: 1.1% or more and 1.6% or less, Mn: 1.0% or more and 1.5% or less, Ni: 0.2% or more and 0.6% or less, Cr: 1.5% or more and 1.9% or less, and Mo: 0.1% or more and 0.3% or less, and the remainder consists of Fe and other unavoidable impurities, satisfying the following general formula 1.
[0040] [General Formula 1]
[0041] 0 ≤ CN5 3 +CZ6 3 +CZ7 3 ≤ 24
[0042] In the above General Formula 1, CN5, CZ6, and CZ7 are 100 mm taken from bearing steel 2 The degree of carbide segregation of the test specimen with the above cross-sectional area was evaluated based on SEP 1520.
[0043] Specifically, in the above general formula 1, CN5 is 100 mm taken from bearing steel 2 It is a carbide segregation grade that evaluates how predominantly (average degree) the solidification amount of carbides precipitated at grain boundaries is formed from test specimens with the above cross-sectional area, and CZ6 is a 100 mm sample taken from bearing steel 2 It is a carbide segregation grade that evaluates the degree of aggregation of carbides precipitated in the elongation direction from test specimens with the above cross-sectional area, and CZ7 is a 100 mm specimen taken from bearing steel 2This is a carbide segregation grade that evaluates the degree of dispersion of carbides in the thickness direction perpendicular to the elongation direction from a test specimen having the above cross-sectional area. The above carbide segregation grade is a grade that evaluates the shape of the carbides by comparing them to a limit sample after measuring the shape, arrangement, and size of the carbides using an optical microscope, based on the standard of SEP 1520. In the above carbide segregation grade, CN5, CZ6, and CZ7 may each have an integer grade, and the lower the carbide segregation grade, the finer the distribution of carbides, which can be evaluated as having excellent cleanliness. For example, the above carbide segregation grade may be evaluated from grade 0 to grade 9, and the grade for each series may be evaluated by comparing it with the limit sample attached to SEP 1520. In this case, the grade for each series of CN5, CZ6, and CZ7 may be grade 0 or higher and grade 2 or lower. The above bearing steel can be manufactured to satisfy the above General Formula 1 by satisfying the molten steel component ratio described below, and the current value and casting speed range of the continuous casting machine described below during continuous casting. According to the above bearing steel, by satisfying the above General Formula 1, there is less central segregation and defects within the product, and it can have excellent fatigue life and high cleanliness.
[0044] In another example, the bearing steel may contain an austenite microstructure having an ASTM grain size number of 9.0 or higher and 13.0 or lower. Specifically, the grain size of the austenite microstructure within the bearing steel may have a lower limit of ASTM grain size number 9.2 or higher or 9.4 or higher, and an upper limit of ASTM grain size number 11.0 or lower or 10.0 or lower. By containing an austenite microstructure with a grain size satisfying the aforementioned ASTM grain numbers, the bearing steel can have excellent fatigue life and high cleanliness due to fewer central segregation and defects.
[0045] The alloy composition of the above bearing steel is explained below.
[0046] C: 0.9 wt% or more, 1.3 wt% or less
[0047] Carbon (C) is an element that increases strength and hardness due to solid solution effects within the matrix and the formation of carbides. If the carbon is included in the bearing steel below the lower limit of the aforementioned range, it may reduce fatigue strength. Additionally, if the carbon is included in the bearing steel above the upper limit of the aforementioned range, it may form coarse carbides, thereby reducing fatigue life and machinability. Accordingly, the carbon may be included in the bearing steel in an amount of 0.9 wt% or more and 1.3 wt% or less, and specifically, in an amount of 0.95 wt% or more and 1.05 wt% or less.
[0048] Si: 1.1 wt% or more, 1.6 wt% or less
[0049] Silicon (Si) is an element added to act as a deoxidizer to improve oxidation resistance, solid solution strengthening, and softening resistance. If the silicon is included in the bearing steel in an amount less than the lower limit of the aforementioned range, it may reduce softening resistance and strength. Additionally, if the silicon is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, decarburization may occur during the heating step in the rolling process, thereby reducing processability and spheroidizing heat treatmentability. Accordingly, the silicon may be included in the bearing steel in an amount of 1.1 wt% or more and 1.6 wt% or less, specifically, in an amount of 1.1 wt% or more and 1.3 wt% or less.
[0050] Mn: 1.0 wt% or more and 1.5 wt% or less
[0051] Manganese (Mn) is an element that improves hardenability and increases strength. If the manganese is included in the bearing steel in an amount less than the lower limit of the aforementioned range, it may reduce hardenability and strength. Furthermore, if the manganese is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, it may reduce machinability and cause center segregation, react with sulfur (S) to form sulfide inclusions (MnS) which may reduce fatigue life, and reduce toughness due to the increase in strength. Therefore, the manganese may be included in the bearing steel in an amount of 1.0 wt% or more and 1.5 wt% or less, specifically in an amount of 1.1 wt% or more and 1.3 wt% or less.
[0052] Ni: 0.2 wt% or more, 0.6 wt% or less
[0053] Nickel (Ni) is an element that improves toughness and hardenability, and induces grain refinement and solid solution strengthening effects. If the nickel is included in the bearing steel in an amount less than the lower limit of the aforementioned range, it may reduce toughness and strength. Additionally, if the nickel is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, it may cause red-hot brittleness. Accordingly, the nickel may be included in the bearing steel in an amount of 0.2 wt% or more and 0.6 wt% or less, and specifically, in an amount of 0.3 wt% or more and 0.5 wt% or less.
[0054] Cr: 1.5 wt% or more, 1.9 wt% or less
[0055] Chromium (Cr) is an element that improves hardenability and forms carbides, and improves strength and hardness through grain refinement. If the chromium is included in the bearing steel in an amount less than the lower limit of the aforementioned range, it may reduce hardenability and hardness. Additionally, if the chromium is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, it may excessively improve spheroidizing heat treatability and increase manufacturing costs. Therefore, the chromium may be included in the bearing steel in an amount of 1.5 wt% or more and 1.9 wt% or less, specifically, in an amount of 1.7 wt% or more and 1.9 wt% or less.
[0056] Mo: 0.1 wt% or more, 0.3 wt% or less
[0057] Molybdenum (Mo) is an element that improves hardenability and increases resistance to temper brittleness. If the molybdenum is included in the bearing steel in an amount less than the lower limit of the aforementioned range, it may be susceptible to temper brittleness. Additionally, if the molybdenum is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, it may reduce machinability. Therefore, the molybdenum may be included in the bearing steel in an amount of 0.1 weight% or more and 0.3 weight% or less.
[0058] Remaining Fe and other unavoidable impurities
[0059] The aforementioned unavoidable impurities are impurities unintentionally incorporated from raw materials or the surrounding environment during the ordinary manufacturing process; as this is widely known in the art, a detailed description is omitted. In one embodiment of this application, the addition of elements other than the components of the bearing steel described above is not excluded, and various elements may be included within a scope that does not impair the technical concept of this application. If additional elements are included, they may be included to replace the remainder of iron (Fe).
[0060] In another example, the bearing steel may further include one or more selected from, in weight%, P: greater than 0% and less than or equal to 0.03%, S: greater than 0% and less than or equal to 0.01%, Al: greater than 0% and less than or equal to 0.05%, Ti: greater than 0% and less than or equal to 0.005%, and O: greater than 0% and less than or equal to 0.001%.
[0061] P: Greater than 0 wt% and less than or equal to 0.03 wt%
[0062] Phosphorus (P) is an impurity element. If the phosphorus is included in the bearing in an amount exceeding the upper limit of the aforementioned range, it can cause segregation and easily create an unsound casting structure. Therefore, the phosphorus may be included in the bearing steel in an amount greater than 0 wt% and less than or equal to 0.03 wt%, and specifically, in an amount greater than 0 wt% and less than or equal to 0.025 wt%.
[0063] S: Greater than 0 wt% and less than or equal to 0.01 wt%
[0064] Sulfur (S) is an impurity that combines mainly with manganese (Mn) to form MnS inclusions, which reduce fatigue life, and when it exists in the form of a central segregation, stress caused by bearing operation is concentrated in the segregation, becoming a factor that causes cracking. Therefore, the sulfur may be included in the bearing steel in an amount greater than 0 wt% and less than or equal to 0.01 wt%, and specifically, in an amount greater than 0 wt% and less than or equal to 0.008 wt%.
[0065] Al: Greater than 0 wt% and less than or equal to 0.05 wt%
[0066] Aluminum (Al) is a deoxidizing element that reacts with oxygen (O) during the refining process to form alumina (Al2O3) oxide, which is then added for the purpose of removal through flotation separation. Additionally, the aluminum may be included in the bearing steel in an amount greater than 0 wt% and less than or equal to 0.05 wt% for the purpose of refining the grain size by reacting with nitrogen (N) to precipitate as AlN, specifically in an amount greater than or equal to 0.005 wt% and less than or equal to 0.050 wt%. On the other hand, if the aluminum is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, it may not be removed by flotation outside the molten metal system and remains in the molten steel, remaining as Al2O3 inclusions in the bearing steel, which can reduce fatigue life.
[0067] Ti: Greater than 0 wt% and less than or equal to 0.005 wt%
[0068] Titanium (Ti) is an element that degrades fatigue properties by forming fine inclusions such as TiC, TiN, and TiS as impurities. Additionally, since the titanium reacts with nitrogen (N) to precipitate TiN in an angular shape, stress can concentrate in the corresponding area when repeated stress is applied, potentially acting as a fracture initiation point. Therefore, to suppress the precipitation of TiN in an angular shape, the titanium may be saturated in the bearing steel in an amount greater than 0 wt% and less than or equal to 0.005 wt%.
[0069] O: Greater than 0 wt% and less than or equal to 0.001 wt%
[0070] Oxygen (O) is an element that inevitably remains in the molten steel during the steelmaking process. If the oxygen is included in the bearing steel in an amount exceeding the upper limit of the aforementioned range, it may reduce durability due to the formation of oxide-based non-metallic inclusions. Therefore, the oxygen may be included in the bearing steel in an amount greater than 0 weight% and less than or equal to 0.001 weight%.
[0071] This application also relates to a method for manufacturing bearing steel. The method for manufacturing bearing steel relates to a method for manufacturing bearing steel, and since specific details regarding the bearing steel described below can be applied in the same way as those described for bearing steel, they will be omitted.
[0072] The above method for manufacturing bearing steel includes the steps of manufacturing a bloom, manufacturing a billet, manufacturing a wire rod, winding, and cooling, and the current value of the mold electromagnetic stirrer described below satisfies the range described below. According to the method for manufacturing bearing steel of the present application, it is possible to manufacture bearing steel with excellent productivity, low production costs, reduced carbon emissions, improved fatigue life, and high purity.
[0073] The step of manufacturing the above bloom is a step of manufacturing a bloom through a continuous casting process using molten steel comprising, in weight percent, C: 0.9% or more and 1.3% or less, Si: 1.1% or more and 1.6% or less, Mn: 1.0% or more and 1.5% or less, Ni: 0.2% or more and 0.6% or less, Cr: 1.5% or more and 1.9% or less, and Mo: 0.1% or more and 0.3% or less, with the remainder being Fe and other unavoidable impurities, and is performed using a continuous casting machine including a mold electronic stirrer (Mold EMS). Since the specific description of the composition of the above molten steel is the same as that described in the bearing steel above, it will be omitted.
[0074] In one example, the molten steel may further include, in weight percent, one or more selected from P: greater than 0% and less than or equal to 0.03%, S: greater than 0% and less than or equal to 0.01%, Al: greater than 0% and less than or equal to 0.05%, Ti: greater than 0% and less than or equal to 0.005%, and O: greater than 0% and less than or equal to 0.001%. Since the specific description of the additional components further included in the molten steel is the same as that described in the bearing steel above, it will be omitted.
[0075] The above-described mold electromagnetic stirrer (Mold EMS) is a device located at the top of a continuous casting machine that applies an alternating voltage to an electromagnet installed around the mold of the continuous casting machine to form a moving magnetic field, and induces uniform solidification by stirring the molten steel and reducing temperature variations. For example, the current value of the above-described mold electromagnetic stirrer is 80 A or more and 300 A or less. Specifically, the current value of the above-described mold electromagnetic stirrer may be 90 A or more and 280 A or less. By satisfying the aforementioned range, the billet produced through the step of manufacturing the above-described billet can satisfy the following general formula 2, and the bearing steel produced through the step of cooling can satisfy the following general formula 1, and additionally, the crystal grain size of the austenite microstructure can satisfy the following. As a result, the productivity of the bearing steel is excellent, the production cost of the bearing steel is low, carbon emissions are reduced during the manufacturing of the bearing steel, fatigue life is improved, and a bearing steel with high purity can be manufactured. In contrast, if the current value of the mold electromagnetic stirrer is below the lower limit of the aforementioned range, the stirring of the molten steel is not activated, and central segregation may occur. In addition, if the current value of the mold electromagnetic stirrer exceeds the upper limit of the aforementioned range, the uniformity of solidification may be impeded by excessive stirring force.
[0076] In another example, the continuous casting machine may further include a final electromagnetic stirrer (Final EMS). The final electromagnetic stirrer (Final EMS) is a device located at the end of the continuous casting machine to suppress center segregation, and the current value of the final electromagnetic stirrer may be 350 A or more and 750 A or less. By satisfying the current value range of the final electromagnetic stirrer in addition to the current value range of the mold electromagnetic stirrer described above, the continuous casting machine can satisfy the following general formula 2 for the billet produced through the billet manufacturing step, and the bearing steel produced through the cooling step can satisfy the following general formula 1, and additionally satisfy the crystal grain size of the austenite microstructure described below. As a result, the productivity of the bearing steel is excellent, the production cost of the bearing steel is low, carbon emissions are reduced during the manufacturing of the bearing steel, fatigue life is improved, and a bearing steel with high purity can be manufactured. In contrast, if the current value of the final electronic stirrer is below the lower limit of the aforementioned range, it may be difficult to disperse or remove central segregation and porous characteristics. Furthermore, if the current value of the final electronic stirrer exceeds the upper limit of the aforementioned range, the final electronic stirring effect may not appear relative to the excessive current value, which may not be economically reasonable.
[0077] In addition, in the step of manufacturing the bloom, continuous casting using the aforementioned continuous casting machine can be performed at a casting speed of 0.3 m / min or more and 0.8 m / min or less. In the step of manufacturing the bloom, by performing continuous casting using the aforementioned continuous casting machine within the aforementioned casting speed range, the solidification speed of the molten steel can be controlled, and as a result, the solidification of the bloom can proceed uniformly. On the other hand, if the casting speed during continuous casting is below the lower limit of the aforementioned range, solidification of the molten steel begins to occur at the initial stage of pouring the molten steel into the continuous casting machine mold, making it difficult to achieve uniform solidification. Furthermore, if the casting speed during continuous casting exceeds the upper limit of the aforementioned range, there is a high possibility that cracks will form on the surface of the bearing steel being manufactured, and a break-out phenomenon in which the solidified shell bursts during continuous casting may occur.
[0078] In one example, a billet manufactured through the step of manufacturing the above billet may satisfy the following general formula 2.
[0079] [General Formula 2]
[0080] 0 ≤ S 3 +R 3 +C 3 ≤ 24
[0081] In the above general formula 2, S, R, and C are the defects of a test specimen obtained by cutting a billet vertically and etching it, evaluated according to ASTM E381.
[0082] Specifically, in the above general formula 2, S is a fine grade that evaluates the amount or degree of defects (cracks, porosity and / or slag, etc.) formed on the surface of the inspection surface of a test specimen obtained by cutting the billet in the rolling direction and etching it, R is a grade that evaluates the amount or degree of defects (cracks, porosity and / or slag, etc.) formed in the part excluding the surface and center of the inspection surface of a test specimen obtained by cutting the billet in the rolling direction and etching it, and C is a grade that evaluates the amount or degree of defects (cracks, porosity and / or slag, etc.) formed in the center of the inspection surface of a test specimen obtained by cutting the billet in the rolling direction and etching it, and the above fine grade is a grade that evaluates the amount of cracks and impurities in the microstructure of the inspection surface of the test specimen based on the ASTM E381 standard. In the above micrograde, S, R, and C can each have an integer grade, and the lower the micrograde, the less cracks and impurities occur within the microstructure of the billet, so the cleaner it can be evaluated as having excellent cleanliness. For example, the micrograde can be evaluated from grade 0 to grade 5, and the micrograde for each location can be evaluated through the location-specific limit samples listed in the ASTM E381 standard. In this case, the grades for each location of S, R, and C can be grade 0 or higher and grade 2 or lower. As described above, the billet can satisfy General Formula 2 by satisfying the aforementioned molten steel component ratio and the current value and casting speed range of the continuous casting machine during continuous casting. As a result, the manufactured bearing steel can have excellent fatigue life and high cleanliness with fewer central segregation and defects within the product.
[0083] The step of manufacturing the billet is a step of manufacturing a billet, which is an intermediate material before processing the bloom produced in the step of manufacturing the bloom into a wire rod, and is performed by reheating the manufactured bloom and then rolling it.
[0084] For example, the step of manufacturing the billet may be performed by reheating the bloom at a temperature of 1100°C or higher and 1300°C or lower, and then hot rolling it at a finishing temperature of 1100°C or higher and 1300°C or lower. At this time, the reheating time may be 120 minutes or more and 720 minutes or less. By satisfying the aforementioned ranges for the reheating temperature and the reheating time, fine dispersion may be possible through redeposition of composite precipitates within the matrix following redeposition. If the reheating temperature is below the lower limit of the aforementioned range, the rolling force may increase, placing a load on the rolling rolls and potentially degrading the surface quality of the rolled billet. Additionally, if the reheating temperature exceeds the upper limit of the aforementioned range, it may place a load on the equipment furnace. Furthermore, if the reheating time is below the lower limit of the aforementioned range, redeposition of composite precipitates within the matrix may be difficult, making it difficult to remove center segregation. In addition, if the reheating time exceeds the upper limit of the aforementioned range, sufficient dissolution of the composite precipitate is achieved, but the productivity of the product decreases due to the increased reheating heat treatment time, which may make it uneconomical.
[0085] The step of manufacturing the above wire rod is a step of manufacturing a coil-shaped wire rod having a desired diameter by rolling a billet, and is performed by reheating and rolling the billet manufactured in the step of manufacturing the billet.
[0086] For example, the step of manufacturing the wire rod may be performed by reheating the billet at a temperature of 950°C or higher and 1200°C or lower for 70 minutes or more and 120 minutes or less, and then hot rolling at a finishing temperature of 900°C or higher and 1150°C or lower. In the step of manufacturing the wire rod, if the reheating is performed below the lower limit of the aforementioned temperature range and for less than the lower limit of the aforementioned time range, the surface quality of the product may deteriorate due to the temperature drop and the rolling roll may be subjected to a load. Additionally, if the reheating is performed above the upper limit of the aforementioned temperature range and for more than the upper limit of the aforementioned time range, the decarburization reaction may be maximized, and the surface quality of the product after rolling may deteriorate due to surface decarburization. Furthermore, if the finishing temperature is below the lower limit of the aforementioned range, the surface quality of the product may deteriorate due to the temperature drop and the rolling roll may be subjected to a load. Additionally, if the finishing temperature exceeds the upper limit of the aforementioned range, the decarburization reaction may be maximized, and the surface quality of the product after rolling may deteriorate due to surface decarburization.
[0087] The above winding step is a step of winding the wire produced in the step of manufacturing the wire.
[0088] For example, the above-mentioned coiling step may be performed by coiling at a temperature of 780°C or higher and 950°C or lower. If the coiling temperature is below the lower limit of the aforementioned range, the probability of low-temperature structure formation and the strength of the product increase, which may lead to a decrease in cold forgeability and workability. Additionally, if the coiling temperature exceeds the upper limit of the aforementioned range, the quality of the scale may deteriorate. Specifically, if the coiling temperature exceeds the upper limit of the aforementioned range, blister-shaped scale may form due to the thermal expansion coefficient of the scale FeO and the product, the scale may grow thickly at high temperatures, and a scale phase unfavorable to pickling may be formed.
[0089] The above cooling step is a step of cooling the wound wire.
[0090] For example, the cooling step includes a first cooling step and a second cooling step.
[0091] The first cooling step described above can be performed by cooling the wound wire rod to a temperature of 650°C or higher and 750°C or lower at a cooling rate of 2°C / s or higher and 3°C / s or lower. By performing the first cooling step by cooling to a temperature within the aforementioned range at a cooling rate within the aforementioned range, the driving force for phase transformation can be increased, and the microstructure can be refined to improve the quality of the bearing steel.
[0092] The second cooling step described above can be performed by cooling the wire rod that has undergone the first cooling step to a temperature of 550°C or higher and 650°C or lower at a cooling rate of 1°C / s or less. By performing the second cooling step by cooling to a temperature within the aforementioned range at a cooling rate within the aforementioned range, the formation of a hardened structure can be suppressed and impact toughness can be improved.
[0093] In one example, the bearing steel manufactured by the method described above may satisfy the above general formula 1. Since the specific description of the above general formula 1 is the same as that described for the bearing steel above, it will be omitted.
[0094] In addition, the bearing steel manufactured by the above-described method may contain an austenite microstructure having a grain size number of ASTM 9.0 or higher and 13.0 or lower. Since the specific description of the grain size of the austenite microstructure contained within the bearing steel is the same as that described in the bearing steel, it will be omitted.
[0096] The present application will be described in more detail below through embodiments according to the present application and comparative examples not according to the present application, but the scope of the present application is not limited by the embodiments presented below.
[0098] Preparation Examples 1 to 3
[0099] Preparation of molten steel
[0100] Molten steel containing the components shown in Table 1 below and the remainder consisting of Fe and other unavoidable impurities was prepared.
[0101] Composition of molten steel (weight%) C Si Mn P S Ni Cr Mo Al Ti O Preparation Example 1 0.97 1.13 1.16 0.011 0.003 0.32 1.70 0.11 0.009 0.0034 0.0004 Preparation Example 2 0.96 0.26 0.38 0.013 0.004 0.04 1.47 0.02 0.007 0.0019 0.0007 Preparation Example 3 0.97 0.27 0.38 0.014 0.005 0.04 1.49 0.02 0.009 0.0025 0.0006
[0103] Example 1
[0104] Manufacture of bearing steel
[0105] The molten steel of Preparation Example 1 above was continuously cast to produce a bloom using the current values of the mold electromagnetic stirrer and the final electromagnetic stirrer and the casting speed shown in Table 2 below. The produced bloom was reheated at 1251°C for 665 minutes, and then hot-rolled at a finishing temperature of 1247°C to produce a billet. Subsequently, the produced billet was reheated at 1189°C for 95 minutes, and then hot-rolled at a finishing temperature of 1105°C to produce a wire rod. Subsequently, the produced wire rod was coiled at 869°C. Subsequently, the coiled wire rod was cooled to 675°C at a cooling rate of 2.5°C / s, and then cooled to 575°C at a cooling rate of 1°C / s to produce bearing steel.
[0107] Comparative Example 1
[0108] Manufacture of bearing steel
[0109] Bearing steel was manufactured in the same manner as in Example 1, using the molten steel prepared in Preparation Example 1, except that continuous casting was performed with the current values of the mold electronic stirrer and the final electronic stirrer and the casting speed shown in Table 2 below.
[0111] Comparative Example 2
[0112] Manufacture of bearing steel
[0113] Bearing steel was manufactured in the same manner as in Example 1, except that the molten steel prepared in Preparation Example 2 was used, and continuous casting was performed with the current values of the mold electromagnetic stirrer and the final electromagnetic stirrer and the casting speed shown in Table 2 below.
[0115] Comparative Example 3
[0116] Manufacture of bearing steel
[0117] Bearing steel was manufactured in the same manner as in Example 1, except that the molten steel prepared in Preparation Example 3 was used, and continuous casting was performed with the current values of the mold electronic stirrer (M-EMS) and final electronic stirrer (F-EMS) and the casting speed shown in Table 2 below.
[0118] continuous casting M-EMS current value (A) F-EMS current value (A) Casting speed (°C / s) Example 1 100 745 0.44 Comparative Example 1 0 745 0.44 Comparative Example 2 270 745 0.48 Comparative Example 3 380 745 0.48
[0120] Evaluation Example 1. Evaluation of Carbide Segregation Grade
[0121] Based on the standard SEP 1520 (Microscopic Examination of Carbide Structure in Steels by means of Diagram Series), the average carbide size of the bearing steels prepared in each of the examples and comparative examples was measured using an optical microscope to calculate the carbide segregation grade, and whether it satisfied General Formula 1 below was evaluated and presented in Table 3 below. Specifically, the bearing steels prepared in each of the examples and comparative examples were heat-treated at 850°C and water-cooled, and then an area of 100 mm² at a location including the center of the raw material where significant segregation occurs 2Specimens having the above area were taken. Subsequently, the taken specimens were cut and polished, and etched by immersing them in a 2% Nital solution for 10 minutes. Then, the D-dominated and inferior structures were selected by observing them under an optical microscope at magnifications of 100x and 200x, respectively. At this time, the images taken with an optical microscope for Example 1, Comparative Example 2, and Comparative Example 3, respectively, are shown in Figures 1 to 6. The carbide segregation grades can be evaluated from grade 0 to grade 9, and the carbide segregation grades of Example 1 and Comparative Examples 1 to 3 were evaluated by reference to limit specimen photographs (degree of carbide segregation by grade) based on the SEP 1520 standard, and the grade for each series was calculated.
[0122] [General Formula 1]
[0123] 0 ≤ CN5 3 +CZ6 3 +CZ7 3 ≤ 24
[0124] In the above General Formula 1, CN5, CZ6, and CZ7 are 100 mm taken from bearing steel 2 The degree of carbide segregation of the test specimen with the above cross-sectional area was evaluated based on SEP 1520.
[0126] Evaluation Example 2. Fine Grade Evaluation
[0127] Based on the ASTM E381 (Standard method of Macroetch Testing Steel Bars, Billets, Blooms, and Forgings) standard, billets manufactured during the production of bearing steel in each of the Examples and Comparative Examples were cut in the direction perpendicular to the rolling process and etched by immersing them in a diluted solution containing 20 wt% hydrochloric acid heated to 80°C for 30 minutes. The amount of cracks and impurities in the microstructure of the test specimens obtained was compared with the limit samples within the ASTM E381 standard to calculate the micrograde, and whether the following General Formula 2 was satisfied was evaluated and is shown in Table 3 below. In particular, images of the surface of the test specimens obtained from the billets manufactured in Example 1 and Comparative Example 1, respectively, taken with a digital camera, are shown in Figures 7 and 8. At this time, the micrograde can be evaluated from Grade 0 to Grade 5, and the micrograde by location was evaluated by comparing it with the limit samples within the ASTM E381 standard.
[0128] [General Formula 2]
[0129] 0 ≤ S 3 +R 3 +C 3 ≤ 24
[0130] In the above general formula 2, S, R, and C are the defects of a test specimen obtained by cutting a billet vertically and etching it, evaluated according to ASTM E381.
[0132] Evaluation Example 3. Evaluation of the grain size of the austenite microstructure in bearing steel
[0133] Based on the ASTM E 112-13 (Standard Test Methods for Determining Average Grain Size) standard, bearing steels prepared in each of the examples and comparative examples were measured using an optical microscope and evaluated using the circle method, the diameter measurement method, and the ASTM grain size number conversion table, and the results are shown in Table 3 below. In this case, the smaller the ASTM grain size number, the larger the crystal grain size.
[0135] Evaluation Example 4. Evaluation of Central Segregation
[0136] For each of the examples and comparative examples, a billet produced during the manufacture of bearing steel was cut in the direction perpendicular to the rolling process, and a test specimen obtained by corrosion by immersing it in a diluted solution containing 20% by weight of hydrochloric acid heated to 80°C for 30 minutes was evaluated for the presence or absence of central segregation through visual inspection, and the results are shown in Table 3 below.
[0137] Carbide Segregation Grade Fine grade ASTM particle size number central segregation CN5 CZ6 CZ7 General Formula 1 Calculated Value S R C General Formula 2 Calculated Value Example 1 0 0 0 0 1 1 1 3 9.5 X Comparative Example 1 0 0 3 27 1 1 3 29 9.6 O Comparative Example 2 1 1 1 3 1 1 1 3 10.1 O Comparative Example 3 1 1 3 29 1 1 1 3 8.4 O
[0138] As shown in Table 3 and Figures 1 to 8 above, unlike the bearing steels produced in Comparative Examples 1 and 3, the bearing steel produced in Example 1 was confirmed to have a uniform microstructure and high purity with suppressed central segregation, as General Formula 1, General Formula 2, and ASTM particle size number satisfied specific ranges. In addition, unlike the bearing steels produced in Comparative Examples 1 and 3, the bearing steel produced in Example 1 was confirmed to have excellent productivity and low production costs, as the current values of the mold electronic stirrer (M-EMS) and the final electronic stirrer (F-EMS) and the casting speed simultaneously satisfied specific ranges during continuous casting.
[0139] Meanwhile, it was confirmed that the bearing steel manufactured in Comparative Example 2 had general formula 1, general formula 2 and ASTM particle size number satisfying specific ranges, but the component ratio in the molten steel did not satisfy specific ranges, resulting in central segregation and a decrease in cleanliness.
[0141] Evaluation Example 5. Fatigue Life Evaluation
[0142] In Example 1 and Comparative Example 3, respectively, specimens for evaluating rolling fatigue life were taken and fabricated from billets produced during the manufacture of bearing steel. The fatigue life was evaluated through a rolling contact fatigue test, and the results are shown in Table 4 below. Specifically, the rolling fatigue test was performed under a foreign matter environment or a high-temperature environment by contacting a bearing steel ball with a contact surface pressure of 5250 MPa to each specimen and rotating it at a speed of 1800 rpm. In this case, the foreign matter environment refers to a state in which foreign matter is injected onto the track generated by rotating the steel ball on the specimen surface at room temperature (a state in which indentation marks are formed). Furthermore, the high-temperature environment refers to a temperature of 200°C, which is the intermediate temperature between 150°C and 250°C, the actual operating temperature of bearing components. The rolling fatigue test automatically terminates when failure (flaking) occurs on the surface of the specimen, and the number of rotations (life) up to that point is measured and L 10 It was evaluated based on lifespan. At this time, the above L 10 Life refers to the probability that 90% of bearing parts will exceed their fatigue life or 10% will fail.
[0143] In addition, the above-mentioned specimens for evaluating rolling fatigue life were manufactured by cutting a billet produced during the manufacture of bearing steel in Example 1 and Comparative Example 3 into a round bar with a diameter of 65 mm, then normalizing the cut round bar at 935°C, then turning the heat-treated round bar, then carburizing and nitriding the turned specimen at 850°C for 225 minutes, and finally performing a polishing operation.
[0144] Foreign matter electric contact fatigue test High temperature electric contact fatigue test (200℃) Example 1 Comparative Example 3 Increase or decrease in lifespan Example 1 Comparative Example 3 Increase or decrease in lifespan L 10 (Ⅹ 10 6 cycles) 12.6 9.9 27.1% improvement 20.8 15.2 36.8% improvement
[0145] As shown in Table 4 above, unlike the specimen produced from the billet produced during the production of bearing steel in Example 1, center segregation does not occur in the specimen produced from the billet produced during the production of bearing steel in Comparative Example 3; therefore, compared to the specimen produced from the billet produced during the production of bearing steel in Comparative Example 3, L 10 Based on fatigue life, it was confirmed that fatigue life was improved by 27.1% in a foreign matter environment and by 36.8% in a high temperature environment.
Claims
Claim 1 A bearing steel comprising, in weight percent, C: 0.9% or more and 1.3% or less, Si: 1.1% or more and 1.6% or less, Mn: 1.0% or more and 1.5% or less, Ni: 0.2% or more and 0.6% or less, Cr: 1.5% or more and 1.9% or less, and Mo: 0.1% or more and 0.3% or less, and the remainder being Fe and other unavoidable impurities, satisfying the following general formula 1: [General Formula 1]0 ≤ CN5 3 +CZ6 3 +CZ7 3 ≤ 24 In the above general formula 1, CN5, CZ6, and CZ7 are 100 mm taken from bearing steel 2 The degree of carbide segregation of the test specimen with the above cross-sectional area was evaluated based on SEP 1520. Claim 2 A bearing steel according to claim 1, comprising an austenite microstructure having an internal grain size of ASTM grain size number 9.0 or higher and 13.0 or lower. Claim 3 A bearing steel according to claim 1, further comprising, in weight%, one or more selected from P: greater than 0% and less than or equal to 0.03%, S: greater than 0% and less than or equal to 0.01%, Al: greater than 0% and less than or equal to 0.05%, Ti: greater than 0% and less than or equal to 0.005%, and O: greater than 0% and less than or equal to 0.001%. Claim 4 A method for manufacturing bearing steel comprising, in weight percent, C: 0.9% or more and 1.3% or less, Si: 1.1% or more and 1.6% or less, Mn: 1.0% or more and 1.5% or less, Ni: 0.2% or more and 0.6% or less, Cr: 1.5% or more and 1.9% or less, and Mo: 0.1% or more and 0.3% or less, and the remainder being Fe and other unavoidable impurities, by continuously casting the molten steel using a continuous casting machine including a mold electromagnetic stirrer (Mold EMS) to produce a bloom; a step of reheating the produced bloom and rolling it to produce a billet; a step of reheating the produced billet and rolling it to produce a wire rod; a step of coiling the produced wire rod; and a step of cooling the coiled wire rod, wherein the produced bearing steel satisfies the following general formula 1: [General Formula 1] 0 ≤ CN5 3 +CZ6 3 +CZ7 3 ≤ 24 In the above general formula 1, CN5, CZ6, and CZ7 are 100 mm taken from bearing steel 2 The degree of carbide segregation of the test specimen with the above cross-sectional area was evaluated based on SEP 1520. Claim 5 A method for manufacturing bearing steel according to claim 4, wherein the current value of the mold electronic stirrer is 80 A or more and 300 A or less. Claim 6 In claim 4, the billet manufactured through the step of manufacturing the billet satisfies the following general formula 2, a method for manufacturing bearing steel: [General Formula 2] 0 ≤ S 3 +R 3 +C 3 ≤ 24 In the above general formula 2, S, R, and C are the defects of the test specimen obtained by cutting the billet vertically and etching it, evaluated according to ASTM E381. Claim 7 A method for manufacturing bearing steel according to claim 4, wherein the manufactured bearing steel comprises an austenite microstructure having a crystal grain size of ASTM grain size number 9.0 or higher and 13.0 or lower. Claim 8 A method for manufacturing bearing steel according to claim 4, wherein the molten steel further comprises, in weight%, one or more selected from P: greater than 0% and less than or equal to 0.03%, S: greater than 0% and less than or equal to 0.01%, Al: greater than 0% and less than or equal to 0.05%, Ti: greater than 0% and less than or equal to 0.005%, and O: greater than 0% and less than or equal to 0.001%. Claim 9 A method for manufacturing bearing steel according to claim 4, wherein the continuous casting machine further comprises a final electronic stirrer (Final EMS), and the current value of the final electronic stirrer is 350 A or more and 750 A or less. Claim 10 A method for manufacturing bearing steel according to claim 4, wherein the continuous casting is performed at a casting speed of 0.3 m / min or more and 0.8 m / min or less. Claim 11 A method for manufacturing bearing steel according to claim 4, wherein the step of manufacturing the billet is performed by reheating the bloom at a temperature of 1100°C or higher and 1300°C or lower for 120 minutes or more and 720 minutes or less, and then hot rolling at a finishing temperature of 1100°C or higher and 1300°C or less. Claim 12 A method for manufacturing bearing steel according to claim 4, wherein the step of manufacturing the wire rod is performed by reheating the billet at a temperature of 950°C or higher and 1200°C for 70 minutes or more and 120 minutes or less, and then hot rolling at a finishing temperature of 900°C or higher and 1150°C or less. Claim 13 A method for manufacturing bearing steel according to claim 4, wherein the winding step is performed by winding at a temperature of 780°C or higher and 950°C or lower. Claim 14 A method for manufacturing bearing steel according to claim 4, wherein the cooling step comprises a first cooling step of cooling a wound wire rod to a temperature of 650°C or higher and 750°C or lower at a cooling rate of 2°C / s or higher and 3°C / s or lower, and a second cooling step of cooling the wire rod that has undergone the first cooling step to a temperature of 550°C or higher and 650°C or lower at a cooling rate of 1°C / s or lower.
Citation Information
Patent Citations
Hot rolled steel products having superior cold workability and toughness and their manufacture
JP1981133445A
Control method for segregation and network carbide in 86-grade high-strength cord steel wire rod
JP2023539662A
Method of producing bloom of high carbon steel wire rod for wire drawing having superior internal quality and bloom produced by the same
KR1020100063896A
Method for manufacturing high-carbon bearing steel and high-carbon bearing steel manufactured therefrom