Frame used in expanded type mask-frame assembly for forming OLED pixels and producing method thereof

The frame design with extended support and precise etching methods addresses mask deformation and alignment issues in OLED manufacturing, enhancing the production of ultra-high definition OLEDs by stabilizing the mask and improving alignment precision.

KR103046257B1Active Publication Date: 2026-11-11OLUM MATERIAL CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020250052412
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-04-24
Filing Date
2025-04-22
Publication Date
2026-11-11
Estimated Expiration
2045-04-22

AI Technical Summary

Technical Problem

Conventional OLED manufacturing processes face challenges with mask deformation, such as sagging and twisting, and poor alignment due to the thinness and large surface area of masks, leading to alignment errors that exceed the micrometer level, especially in ultra-high definition OLEDs, resulting in low yield and product failure.

Method used

A frame design with an extended support portion and cell sheet portions, utilizing materials like invar, super invar, and nickel-cobalt, and a manufacturing method involving multiple etching steps to form precise mask patterns, ensuring stable support and alignment without deformation.

Benefits of technology

The solution prevents mask deformation and ensures clear alignment of mask cells, improving the manufacturing process for ultra-high definition OLEDs by reducing alignment errors and enhancing the precision of mask patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025045635576-PAT00034_ABST
    Figure 112025045635576-PAT00034_ABST
Patent Text Reader

Abstract

The present invention relates to a frame used in a connection between an expanded type mask and a frame for forming an OLED pixel, and a method for manufacturing the same. The frame according to the present invention is a frame used in a connection between an expanded type mask and a frame for forming an OLED pixel, wherein the frame comprises an expanded support member and a plurality of cell sheet members, wherein the expanded support member comprises an expanded edge member having a hollow region; and at least one support grid bar connected to the expanded edge member; wherein the plurality of cell sheet members are connected on the expanded support member, and the expanded support member provides a plurality of module regions, and each of the cell sheet members is connected to correspond to each of the module regions.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a frame used in a connection between an extended-type mask and a frame for forming OLED pixels, and a method for manufacturing the same. More specifically, the invention relates to a frame used in a connection between a mask and a frame for forming OLED pixels, comprising a mask having a high-resolution mask pattern formed thereon, capable of stably forming the mask without deformation, and capable of clearly aligning the mask cells with each other, and a method for manufacturing the same. Background Technology

[0002] As a technology for forming pixels in the OLED manufacturing process, the Fine Metal Mask (FMM) method is mainly used, in which a thin metal mask (Shadow Mask) is attached to a substrate to deposit organic material at a desired location.

[0003] In conventional OLED manufacturing processes, masks are manufactured in stick or plate forms and then welded and fixed to an OLED pixel deposition frame for use. A single mask can be equipped with multiple cells corresponding to a single display. Additionally, for the manufacturing of large-area OLEDs, multiple masks may be fixed to the OLED pixel deposition frame; during this fixing process, tension is applied to each mask to ensure it becomes flat. Controlling the tension force to ensure the entire mask is flat is a very difficult task. In particular, to flatten all cells while aligning mask patterns that are only a few to tens of micrometers in size requires a highly sophisticated operation involving finely adjusting the tension force applied to each side of the mask and monitoring the alignment status in real time.

[0004] Nevertheless, during the process of fixing multiple masks to a single frame, there was a problem with poor alignment between the masks and between the mask cells. In addition, during the process of welding the masks to the frame, there were problems such as the masks sagging or twisting due to the load because the mask film was too thin and had a large surface area, and the alignment of the mask cells becoming misaligned due to wrinkles and burrs occurring in the welded area during the welding process.

[0005] In the case of ultra-high definition OLEDs, current QHD resolution has a pixel size of approximately 30–50㎛ with a resolution of 500–600 PPI (pixels per inch), while 4K UHD and 8K UHD resolutions have higher resolutions of approximately 860 PPI and 1600 PPI, respectively. Considering the pixel size of such ultra-high definition OLEDs, the alignment error between cells must be reduced to a few micrometers; errors exceeding this limit can lead to product failure and consequently a very low yield. Therefore, there is a need to develop technologies that prevent deformation such as sagging or twisting of the mask and ensure clear alignment, as well as technologies for fixing the mask to the frame. The problem to be solved

[0006] Accordingly, the present invention has been devised to solve the various problems of the prior art as described above, and aims to provide a frame used in a connection between an OLED pixel forming mask and a frame, and a method for manufacturing the same, which can stably support and move the mask without deformation, prevent deformation such as sagging or twisting of the mask, and ensure clear alignment.

[0007] In addition, the present invention aims to provide a frame used in a connection between an OLED pixel forming mask and a frame, which can clearly align the mask cells and simultaneously form the bezel edge portion more clearly, and a method for manufacturing the same.

[0008] However, these tasks are exemplary and do not limit the scope of the invention. means of solving the problem

[0009] The above objective of the present invention is achieved by a frame used in a connection of an extended type mask and a frame for forming an OLED pixel, wherein the frame comprises an extended support portion and a plurality of cell sheet portions, the extended support portion comprises an extended edge portion having a hollow region; and at least one support grid bar connected to the extended edge portion; wherein the plurality of cell sheet portions are connected on the extended support portion, and the extended support portion provides a plurality of module regions, and each of the cell sheet portions is connected to correspond to each of the module regions.

[0010] The above-mentioned extension support may have a plurality of module regions formed along a first direction or a second direction perpendicular to the first direction, or along the first direction and the second direction.

[0011] Each of the above cell sheet portions can be connected to the expansion support portion with mutual spacing.

[0012] The above frame may have the dimensions of (1) or (2) below. (1) The length in the first direction is at least greater than 1,700 mm, (2) The length in the second direction is at least greater than 1,100 mm.

[0013] A plurality of mask cell regions are formed in each of the above cell sheet portions, and the side shape of the mask cell region and the side shape of the outer edge of the cell sheet portion may include a curvature shape formed by isotropic etching.

[0014] The difference in average surface roughness between the side of the mask cell area and the side of the outer edge of the cell sheet portion may be 10% or less.

[0015] The side shape of the outer edge of the cell sheet portion above may differ from the side shape of a comparative example in which at least a portion of the outer edge of the cell sheet portion is mechanically cut, physically cut, or laser cut.

[0016] The above expansion frame portion is made of at least one of invar, super invar, nickel, and nickel-cobalt, and the above expansion support portion and the above cell sheet portion may be composed of the same material.

[0017] And, the above objective of the present invention is achieved by a method for manufacturing a frame used in a connection of an extended type mask and a frame for forming an OLED pixel, comprising: (a) providing an extended edge portion having a hollow region; (b) connecting at least one support grid bar to the extended edge portion to provide an extended support portion including a plurality of module regions; and (c) corresponding and connecting a cell sheet portion to each of the module regions.

[0018] Prior to step (c) above, the method further includes (1) a step of preparing the cell sheet portion; and step (1) may include (1-1) a step of adhering a first surface of a metal sheet to a moving plate; and (1-2) a step of manufacturing the cell sheet portion by forming a plurality of mask cell regions on a second surface opposite to the first surface of the metal sheet. Effects of the invention

[0019] According to the present invention configured as described above, it is possible to stably support and move the mask without deformation, and it is possible to prevent deformation such as sagging or twisting of the mask and to clearly align it.

[0020] In addition, according to the present invention, there is an effect of clearly aligning the mask cells and simultaneously forming the bezel border portion more clearly.

[0021] Of course, the scope of the present invention is not limited by these effects. Brief explanation of the drawing

[0022] FIG. 1 is a front view and a side cross-sectional view showing a connection between a mask and a frame according to one embodiment of the present invention. FIG. 2 is a front view and a side cross-sectional view showing a frame according to one embodiment of the present invention. FIG. 3 is a schematic diagram showing a mask according to one embodiment of the present invention. Figure 4 is a schematic diagram showing the manufacturing process of a conventional mask. FIGS. 5 to 7 are schematic diagrams illustrating the manufacturing process of a mask according to one embodiment of the present invention. FIG. 8 is a schematic diagram showing the degree of etching of a mask according to a comparative example of the present invention. FIG. 9 is a schematic diagram showing the degree of etching of a mask according to one embodiment of the present invention. FIG. 10 is a schematic diagram showing taper angle adjustment according to one embodiment of the present invention. FIGS. 11 to 15 are schematic diagrams illustrating the manufacturing process of a frame according to one embodiment of the present invention. FIG. 16 is a schematic diagram showing the elongation state of the cell sheet portion and the moving plate with respect to a change in process temperature according to one embodiment of the present invention. FIGS. 17 to 18 are schematic diagrams illustrating the manufacturing process of a cell sheet portion according to one embodiment of the present invention. FIG. 19 is a schematic diagram showing a cell pattern of a cell sheet portion according to one embodiment of the present invention. FIG. 20 is a schematic diagram showing a form in which a mask is connected on a cell sheet portion according to one embodiment of the present invention. FIG. 21 is an electron microscope image showing a cell pattern according to one embodiment of the present invention. FIG. 22 is a schematic diagram showing the manufacturing process of a cell sheet and a frame according to a comparative example. FIG. 23 is a partially enlarged schematic diagram of FIG. 22 according to a comparative example. FIG. 24 is a schematic diagram showing the process of connecting a cell sheet portion according to the first comparative example to a border frame portion. FIG. 25 is a schematic diagram showing the process of connecting a cell sheet portion according to the second comparative example to a border frame portion. Figures 26 and 27 are electron microscope images showing the side of the outer edge of the cell sheet portion according to the first comparative example. Figures 28 and 29 are electron microscope images showing the side of the outer edge of the cell sheet portion according to the second comparative example. FIG. 30 is a schematic diagram showing the process of connecting a cell sheet portion to a border frame portion according to one embodiment of the present invention. FIG. 31 is a schematic diagram showing a side cross-section of a border sheet portion among cell sheet portions according to one embodiment of the present invention. FIG. 32 is an electron microscope image showing the side of the outer edge of the cell sheet portion according to one embodiment of the present invention. FIG. 33 is a schematic plan view showing the shape of an extended support member according to one embodiment of the present invention. FIG. 34 is a schematic plan view showing a frame in which a cell sheet portion is connected on an expansion support portion according to one embodiment of the present invention. FIG. 35 is an enlarged side schematic view of part I of FIG. 34, showing a form in which a support grid bar and a cell sheet part are connected to the extended edge part. FIG. 36 is a schematic plan view showing the shape of an extended support member according to another embodiment of the present invention. FIG. 37 is a schematic plan view showing a frame in which a cell sheet portion is connected on an extension support portion according to another embodiment of the present invention. Specific details for implementing the invention

[0023] The following detailed description of the invention refers to the accompanying drawings, which illustrate specific embodiments in which the invention may be practiced. These embodiments are described in sufficient detail to enable those skilled in the art to practice the invention. It should be understood that various embodiments of the invention are different but need not be mutually exclusive. For example, specific shapes, structures, and characteristics described herein may be implemented in other embodiments without departing from the spirit and scope of the invention in relation to one embodiment. It should also be understood that the location or arrangement of individual components within each disclosed embodiment may be changed without departing from the spirit and scope of the invention. Accordingly, the following detailed description is not intended to be limiting, and the scope of the invention is limited only by the appended claims, including all equivalents to those claimed therein, provided they are appropriately described. Similar reference numerals in the drawings refer to the same or similar functions across various aspects, and lengths, areas, thicknesses, etc., and shapes may be exaggerated for convenience.

[0024] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the attached drawings in order to enable a person skilled in the art to easily practice the present invention.

[0025] FIG. 1 is a front view [Fig. 1 (a)] and a side cross-sectional view [Fig. 1 (b)] showing a frame-integrated mask according to one embodiment of the present invention. FIG. 2 is a front view [Fig. 2 (a)] and a side cross-sectional view [Fig. 2 (b)] showing a frame according to one embodiment of the present invention.

[0026] In this specification, the configuration of the mask-frame connector (or frame-integrated mask) is briefly described below; however, the structure and manufacturing process of the mask-frame connector may be understood as incorporating the contents of Korean Patent Application No. 2018-0016186 in its entirety.

[0027] Referring to FIGS. 1 and 2, the connection (10) of the mask and frame (or the frame-integrated mask) may include a plurality of masks (100) and a single frame (200). In other words, the plurality of masks (100) are each attached to the frame (200). For convenience of explanation, a square-shaped mask (100) is described below as an example, but the masks (100) may be in the form of stick masks having protrusions that are clamped on both sides before being attached to the frame (200), and the protrusions may be removed after being attached to the frame (200).

[0028] A plurality of mask patterns (P) are formed on each mask (100), and a single cell (C) can be formed on one mask (100). A single mask cell (C) can correspond to a display such as a smartphone.

[0029] The mask (100) may be made of materials such as invar, super invar, nickel (Ni), or nickel-cobalt (Ni-Co). The mask (100) may use a gold sheet produced by a rolling process or electroforming.

[0030] The frame (200) is formed to allow multiple masks (100) to be attached. The frame (200) is preferably composed of a material such as Invar, Super Invar, nickel, or nickel-cobalt, which has the same coefficient of thermal expansion as the mask, taking into account thermal deformation. The frame (200) may include a border frame portion (210) in the shape of a roughly square or square frame. The interior of the border frame portion (210) may be hollow.

[0031] In addition, the frame (200) may include a plurality of mask cell regions (CR) and a cell sheet portion (220) connected to the border frame portion (210). The cell sheet portion (220) may be composed of a border sheet portion (221) and first and second grid sheet portions (223, 225). The border sheet portion (221) and the first and second grid sheet portions (223, 225) refer to each portion partitioned from the same sheet, and they are formed integrally with each other.

[0032] The thickness of the border frame portion (210) may be formed to a thickness of several mm to several cm, which is thicker than the thickness of the cell sheet portion (220). The cell sheet portion (220) may have a thickness of about 0.1 mm to 1 mm, which is thinner than the thickness of the border frame portion (210) but thicker than the mask (100). The width of the first and second grid sheet portions (223, 225) may be formed to a width of about 1 to 5 mm.

[0033] A plurality of mask cell regions (CR: CR11~CR56) may be provided by excluding the area occupied by the border sheet portion (221) and the first and second grid sheet portions (223, 225) in the flat sheet. In this specification, the formation of 6 x 5 mask cell regions (CR: CR11~CR56) is described as an example. There may be five first grid sheet portions (223) and four second grid sheet portions (225).

[0034] The frame (200) is provided with a plurality of mask cell regions (CR), and each mask (100) may have one mask cell (C) attached to it so that it corresponds to the mask cell region (CR). The mask cell (C) corresponds to the mask cell region (CR) of the frame (200), and part or all of the dummy may be attached to the frame (200) [cell sheet portion (220)]. Accordingly, the mask (100) and the frame (200) can form an integrated structure.

[0035] The manufacturing process of the specific frame (200) is described in FIGS. 11 to 15, and the formation process of the mask cell region (CR) portion of the cell sheet portion (220) is described later in FIGS. 17 and below.

[0036] FIG. 3 is a schematic diagram showing a mask (100) according to one embodiment of the present invention.

[0037] Each mask (100) may include a mask cell (C) having a plurality of mask patterns (P) formed thereon and a dummy around the mask cell (C) [corresponding to the portion of the mask film (110) excluding the cell (C)]. The dummy may include only the mask film (110) or may include a mask film (110) having a predetermined dummy pattern formed thereon that is similar in shape to the mask pattern (P). The mask cell (C) corresponds to the mask cell region (CR) of the frame (200), and part or all of the dummy may be attached to the frame (200) [cell sheet portion (220)]. Accordingly, the mask (100) and the frame (200) can form an integrated structure.

[0038] Meanwhile, according to another embodiment, the frame may be manufactured by not attaching a cell sheet portion (220) to a border frame portion (210), but by directly forming a grid frame [corresponding to the grid sheet portion (223, 225)] that is integral with the border frame portion (210) in the hollow area (R) of the border frame portion (210). This type of frame also includes at least one mask cell area (CR), and a mask (100) may be aligned with the mask cell area (CR) to manufacture a connection body (10) between the mask and the frame.

[0039] Below, the process of manufacturing a mask (100) is described.

[0040] Figure 4 is a schematic diagram showing the manufacturing process of a conventional mask.

[0041] Referring to Fig. 4, the manufacturing process of a conventional mask is performed solely by wet etching.

[0042] First, a patterned photoresist (M) can be formed on a planar film (sheet; 110') as in FIG. 4 (a). Next, wet etching (WE) is performed through the space between the patterned photoresists (M) as in FIG. 4 (b). After wet etching (WE), a portion of the space of the film (110') can be penetrated to form a mask pattern (P'). Next, the photoresist (M) is washed to complete the manufacture of the film (110') with the mask pattern (P'), i.e., the mask (100').

[0043] As shown in FIG. 4(b), the conventional mask (100') has the problem that the sizes of the mask patterns (P') are not uniform. Since wet etching (WE) is performed isotropically, the etched shape is bound to be approximately an arc shape. In addition, because it is very difficult to perform the etching at the same rate in each part during the wet etching (WE) process, the widths (R1', R1", R1"') of the pierced patterns after the film (110') is pierced are bound to be different. In particular, in patterns where many undercuts (UC) occur, not only the lower width (R1") but also the upper width (R2") of the mask pattern (P') can be formed wide, while in patterns where fewer undercuts (UC) occur, the lower width (R1', R1"') and the upper width (R2', R2"') can be formed relatively narrow.

[0044] Ultimately, the conventional mask (100') had the problem that the size of each mask pattern (P') was not uniform. In the case of ultra-high definition OLEDs, current QHD quality has a pixel size of about 30 to 50 μm with a resolution of 500 to 600 PPI (pixels per inch), and 4K UHD and 8K UHD quality have higher resolutions such as ~860 PPI and ~1600 PPI, so even a minor difference in size is at risk of leading to product failure.

[0045] Accordingly, the present invention is characterized by performing wet etching twice to improve the pattern precision of the insulating mask during the wet etching process.

[0046] FIGS. 5 to 7 are schematic diagrams illustrating the manufacturing process of a mask according to one embodiment of the present invention.

[0047] Referring to FIG. 5(a), first, a metal sheet (sheet; 110) for manufacturing a mask can be provided. As previously mentioned, the material of the metal sheet (110) may be invar, super invar, nickel (Ni), nickel-cobalt (Ni-Co), etc.

[0048] Next, a patterned first insulating portion (M1) can be formed on one side (upper surface) of the metal sheet (110). The first insulating portion (M1) can be formed from a photoresist material using a printing method or the like.

[0049] The first insulating part (M1) may be a black matrix photoresist or a photoresist material having a metal coating film formed on its upper surface. The black matrix photoresist may be a material containing a black matrix resin used to form the black matrix of a display panel. The black matrix photoresist may have a greater light-blocking effect than a general photoresist. Additionally, the photoresist having a metal coating film formed on its upper surface may also have a greater effect in blocking light irradiated from above due to the metal coating film.

[0050] Next, referring to FIG. 5(b), a first mask pattern (P1) can be formed to a predetermined depth by wet etching (WE1) on one side (top surface) of the metal sheet (110). When performing wet etching (WE1), the metal sheet (110) must not be penetrated. Thus, the first mask pattern (P1) can be formed in an approximately arc shape without penetrating the metal sheet (110). That is, the depth value of the first mask pattern (P1) can be less than the thickness of the metal sheet (110).

[0051] Since the wet etching (WE1) has isotropic etching characteristics, the width (R2) of the first mask pattern (P1) does not have the same width as the spacing (R3) between patterns of the first insulating part (M1), but can have a wider width than the spacing (R3) between patterns of the first insulating part (M1). In other words, since an undercut (UC) is formed on both lower sides of the first insulating part (M1), the width (R2) of the first mask pattern (P1) can be larger than the spacing (R3) between patterns of the first insulating part (M1) by the width of the undercut (UC).

[0052] Next, referring to FIG. 5(c), a second insulating portion (M2) can be formed on one side (upper surface) of the metal sheet (110). The second insulating portion (M2) can be formed from a photoresist material using a printing method or the like. Since the second insulating portion (M2) must be left in the space where the undercut (UC) described later is formed, it is preferable that it be a positive type photoresist material.

[0053] Since a second insulating portion (M2) is formed on one side (upper surface) of the metal sheet (110), some of it is formed on the first insulating portion (M1), and some of it can be filled within the first mask pattern (P1).

[0054] The second insulating part (M2) may use a photoresist diluted in a solvent. If a high-concentration photoresist solution is formed on the metal sheet (110) and the first insulating part (M1), it may react with the photoresist of the first insulating part (M1) and cause a portion of the first insulating part (M1) to dissolve. Thus, to avoid affecting the first insulating part (M1), the second insulating part (M2) may use a photoresist with a lower concentration diluted in a solvent.

[0055] Next, referring to FIG. 6(d), baking can be performed to volatilize a portion of the second insulating part (M2). By baking, the solvent of the second insulating part (M2) volatilizes, leaving only the photoresist component. Thus, the second insulating part (M2') can be left thin, like a film coated on the exposed portion of the first mask pattern (P1) and the surface of the first insulating part (M1). It is preferable that the thickness of the remaining second insulating part (M2') be less than a few micrometers so as not to affect the pattern width (R3) of the first insulating part (M1) or the pattern width (R2) of the first mask pattern (P1).

[0056] Next, referring to FIG. 6(e), exposure (L) can be performed on one side (top side) of the metal sheet (110). When exposure (L) is performed on the top of the first insulating part (M1), the first insulating part (M1) can act as an exposure mask. Since the first insulating part (M1) is a black matrix photoresist or a photoresist material with a metal coating film formed on top, it can have an excellent light-blocking effect. Thus, the second insulating part (M2) [see FIG. 6(f)] located vertically below the first insulating part (M1) may not be exposed (L), and the remaining insulating part (M2') may be exposed (L).

[0057] Next, referring to (f) of FIG. 6, when developed after exposure (L), the portion of the second insulating part (M2") that is not exposed (L) remains, and the remaining second insulating part (M2') can be removed. Since the second insulating part (M2') is a positive type photoresist, the exposed (L) portion can be removed. The space where the second insulating part (M2") remains can correspond to the space where an undercut (UC) is formed on both lower sides of the first insulating part (M1) [refer to step (b) of FIG. 5].

[0058] Next, referring to (g) of FIG. 7, wet etching (WE2) can be performed on the first mask pattern (P1) of the metal sheet (110). The wet etching solution can penetrate into the space between the patterns of the first insulating part (M1) and the space of the first mask pattern (P1) to perform wet etching (WE2). The second mask pattern (P2) can be formed by penetrating the metal sheet (110). That is, it can be formed by penetrating the other side of the metal sheet (110) from the bottom of the first mask pattern (P1).

[0059] At this time, a second insulating portion (M2") remains in the first mask pattern (P1). The remaining second insulating portion (M2") can act as a mask for wet etching. That is, the second insulating portion (M2") masks the etching solution, preventing the etching solution from being etched in the lateral direction of the first mask pattern (P1) and causing it to be etched in the lower direction of the first mask pattern (P1).

[0060] Since the second insulating part (M2) is placed in the undercut (UC) space vertically below the first insulating part (M1), the pattern width of the second insulating part (M2) substantially corresponds to the pattern width (R3) of the first insulating part (M1). Accordingly, the second mask pattern (P2) is equivalent to having performed wet etching (WE2) on the gap (R3) between the patterns of the first insulating part (M1). Therefore, the width (R1) of the second mask pattern (P2) can be formed narrower than the width (R2) of the first mask pattern (P1).

[0061] Since the width of the second mask pattern (P2) defines the width of the pixel, it is preferable that the width of the second mask pattern (P2) be smaller than 35 μm. In addition, if the thickness of the second mask pattern (P2) is too thick, it is difficult to control the width (R1) of the second mask pattern (P2), the uniformity of the widths (R1) decreases, and a problem may occur where the shape of the mask pattern (P) does not appear as a tapered / inverse tapered shape overall; therefore, it is preferable that the thickness of the second mask pattern (P2) be smaller than the thickness of the first mask pattern (P1). It is preferable that the thickness of the second mask pattern (P2) be as close to 0 as possible, and considering the size of the pixel, for example, it is preferable that the thickness of the second mask pattern (P2) be about 0.5 to 3.0 μm, and more preferable that it be 0.5 to 2.0 μm.

[0062] The sum of the shapes of the consecutive first mask pattern (P1) and second mask pattern (P2) can form a mask pattern (P).

[0063] Next, referring to (h) of FIG. 7, the manufacturing of the mask (100) can be completed by removing the first insulating part (M1) and the second insulating part (M2). Since the first and second mask patterns (P1) are formed including a slanted surface and the height of the second mask pattern (P2) is formed very low, the shapes of the first mask pattern (P1) and the second mask pattern (P2) combined can show an overall tapered shape or an inverse tapered shape.

[0064] FIG. 8 is a schematic diagram showing the degree of etching of a mask according to a comparative example of the present invention.

[0065] Referring to FIG. 8, since wet etching is performed isotropically, the etched shape is bound to be approximately an arc shape. Furthermore, it is difficult for the etching speed to be perfectly identical in each part during the wet etching process, and the deviation may be even greater when the mask pattern is formed by penetrating the metal sheet (110) by performing wet etching only once. For example, there is a difference in wet etching speed between the mask pattern (111) and the mask pattern (112), but the difference in the upper width (undercut) is not that large. However, the difference between the lower width (PD1) of the metal sheet (110) penetrating through the mask pattern (111) and the lower width (PD2) of the metal sheet (110) penetrating through the mask pattern (112) becomes much larger than the difference in the upper width. This is a result that occurs because wet etching is performed isotropically. In other words, since the width determining the pixel size is the lower width (PD1, PD2) rather than the upper width of the mask pattern (111, 112), performing two wet etchings instead of one wet etching makes it easier to control the lower width (PD1, PD2). An embodiment applying the present invention is further explained below with reference to FIG. 9.

[0066] FIG. 9 is a schematic diagram showing the degree of etching of a mask according to one embodiment of the present invention.

[0067] The process up to FIG. 9(a) is the same as the process described in FIG. 5(a) and (b). However, FIG. 9(a) explains the first mask pattern (P1-1) and the first mask pattern (P1-2) by comparing them, in which a difference in the degree of etching is shown during wet etching (WE1) through the first insulating part (M1).

[0068] Referring to FIG. 9(a), even with the same wet etching (WE1-1, WE1-2), there may be differences in the degree of etching depending on the part, such as between the first mask pattern (P1-1) and the first mask pattern (P1-2). The pattern width (R2-1) of the first mask pattern (P1-1) is smaller than the pattern width (R2-2) of the first mask pattern (P1-2), and such a difference in pattern widths (R2-1, R2-2) may be a difference that adversely affects the resolution of the pixels.

[0069] Next, referring to FIG. 9(b), it can be seen that after performing the process described in FIG. 5(c) to FIG. 6(f), a second insulating part (M2"-1, M2"-2) is formed in the vertical lower space of the first insulating part (M1). Due to the difference in the size of the undercut space below the first insulating part, the size of the second insulating part (M2"-1, M2"-2) formed may differ. Although the size of the second insulating part (M2"-2) formed is larger than that of the second insulating part (M2"-1), the pattern width of the second insulating part (M2"-1, M2"-2) may be the same. The pattern width of each second insulating part (M2"-1, M2"-2) may be the same to correspond to the pattern width (R3) of the first insulating part (M1).

[0070] Next, referring to FIG. 9 (c), a second wet etching (WE2) can be performed using each second insulating part (M2"-1, M2"-2) as a wet etching mask to penetrate the metal sheet (110). As a result, the deviation in the width (R1-1, R1-2) of the second mask pattern (P2-1, P2-2) formed can be significantly smaller than the deviation in the width (R2-1, R2-2) of the first mask pattern (P1-1, P1-2). This is because the metal sheet (110) is wet-etched first by the depth of the first mask pattern (P1-1, P1-2), and wet-etched secondly on the thickness of the remaining metal sheet (110), and at the same time, the pattern width of the second insulating part (M2"-1, M2"-2) that performs the second wet-etching is substantially the same as the pattern width of the first insulating part (M1) that performs the first wet-etching.

[0071] As described above, the present invention has the effect of forming a mask pattern (P) of a desired size by performing wet etching twice in a mask manufacturing method. In particular, by leaving a portion of the second insulating portion (M2), the second wet etching is performed for a thinner width and thinner thickness than the first wet etching, so there is an advantage in that it is easy to control the width (R1) of the second mask pattern (P2). Furthermore, since a slanted surface can be formed by wet etching, it is possible to realize a mask pattern (P) that prevents shadow effects.

[0072] FIG. 10 is a schematic diagram showing the adjustment of taper angles (a1, a2) according to one embodiment of the present invention.

[0073] Meanwhile, the mask manufacturing method of the present invention has the advantage that the mask pattern (P), composed of the first and second mask patterns (P1, P2), is advantageous for forming a taper angle. In addition, it has the effect of making it easy to adjust the taper angle (a1, a2). Referring to FIG. 10 (a), if the thickness (T1) of the second mask pattern (P2) becomes thinner, the taper angle (a1) can increase. In other words, if the thickness of the first mask pattern (P1) is thick and the thickness (T1) of the second mask pattern (P2) becomes thinner, the taper angle (a1) can increase as a result of isotropic wet etching (indicated by radius R1) being performed. Conversely, referring to FIG. 10 (b), if the thickness (T2) of the second mask pattern (P2) becomes thicker, the taper angle (a2) can decrease. In other words, compared to the case of FIG. 10 (a), if the thickness of the first mask pattern (P1) is thinner and the thickness (T2) of the second mask pattern (P2) becomes thicker, the taper angle (a2) can be increased as a result of performing isotropic wet etching (indicated by radius R1). Accordingly, there is an advantage in being able to adjust the taper angle (a1, a2) by adjusting the thickness of the second mask pattern (P2).

[0074] Below, the process of manufacturing the connection (10) of the mask and frame of the present invention is further explained.

[0075] FIGS. 11 to 15 are schematic diagrams illustrating the manufacturing process of a frame according to one embodiment of the present invention.

[0076] To manufacture a connection between a mask (100) and a frame (200) (or a frame-integrated mask), a frame (200) may be provided first. First, the frame (200) may be manufactured by manufacturing a cell sheet portion (220) and connecting the cell sheet portion (220) to a border frame portion (210). Alternatively, the border frame portion (210) may be prepared first, and then the cell sheet portion (220) may be manufactured and connected to the border frame portion (210).

[0077] Referring to FIG. 11, a metal sheet (220') for manufacturing the cell sheet portion (220) of the frame (200) can be prepared. The material of the metal sheet (220') may be invar, super invar, nickel (Ni), nickel-cobalt (Ni-Co), etc., similar to the metal sheet (110) for manufacturing the mask [see FIG. 5 (a)].

[0078] Since the metal sheet (220') is to be used as a cell sheet portion (220) that supports the mask (100), a thickness greater than that of the mask (100) may be used. The thickness of the metal sheet (220') may be approximately 70 µm to 200 µm within the range thicker than the mask (100).

[0079] Additionally, a moving plate (90) may be prepared. The moving plate (90) is a medium that can move the first surface (bottom surface) of the metal sheet (220') while it is bonded and supported. To ensure that the metal sheet (220') is supported as a whole, the size of the moving plate (90) may be a flat plate shape with an area equal to or larger than that of the metal sheet (220').

[0080] For example, 6G may have a width x height of approximately 1,500mm x 1,800mm, and 6G half may have a size of approximately 1,500mm x 900mm. In the connection (10) [see FIG. 1] of the mask (100) and frame (200), the size of the plurality of masks (100) excluding the border frame portion (210) and the cell sheet portion (220) to which the plurality of masks (100) are attached may be the size of 6G half. Considering this, it is preferable that the size of the movable plate (90) supporting the cell sheet portion (220) be equal to or larger than a width x height of approximately 1,500mm x 900mm.

[0081] The moving plate (90) can be made of a material through which the laser (L) can pass. Materials such as glass, silica, quartz, alumina (Al2O3), borosilicate glass, and zirconia can be used.

[0082] Among these, the moving plate (90) is preferably made of a glass material that is easy to configure with a large area corresponding to the 6G half, easy to process, and inexpensive, and is even more preferably made of borosilicate glass. In particular, among borosilicate glass, BOROFLOAT, which has excellent heat resistance, chemical durability, mechanical strength, transparency, etc. ® 33 materials can be used. Also, BOROFLOAT ® 33 has a thermal expansion coefficient of about 3.3, so the difference in thermal expansion coefficient with the metal sheet (220') made of Invar material is small, which has the advantage of being easy to control the metal sheet (220').

[0083] A temporary adhesive portion (95) may be interposed between the movable plate (90) and the metal sheet (220'). The temporary adhesive portion (95) may use means that provide adhesive force to allow the metal sheet (220') to be adhered to the movable plate (90). In particular, the temporary adhesive portion (95) may be provided as a dry film resist layer (DFR layer; 95). The dry film resist layer (95) may be provided as a photoresist in the form of a film. For example, a soft baking process may be performed at approximately 60°C for 60 seconds, and then a lamination process may be carried out immediately. The photoresist layer of the DFR may be laminated onto the first surface (bottom surface) of the metal sheet (220') while peeling off the protective film of the DFR. Lamination may be performed under a predetermined roller pressure and a low-temperature process of approximately 60°C or less. It is preferable to perform lamination under a vacuum. By performing lamination in a vacuum, it is possible to prevent bubbles from being interposed on the interface between the dry film resist layer (95), the metal sheet (220') / moving plate (90).

[0084] The present invention utilizes a dry film resist layer (95) to perform adhesion and lithography processes in a low-temperature region of about 60°C or lower, thereby preventing the metal sheet (220') from being deformed by heat during the process step. Additionally, since a dry film resist layer (95) is used, the baking time and exposure processing time are significantly reduced compared to using a liquid photoresist. While a liquid photoresist requires approximately 1 hour for baking and exposure for outgassing, using a dry film resist requires only about 2 minutes, thus significantly reducing the process time.

[0085] According to FIG. 11 of Korean Patent Application No. 2020-0043485, liquid wax is conventionally used to bond a mask metal film to a substrate supporting it. The liquid wax layer undergoes baking at approximately 100–160°C to vaporize the solvent during use, and the lamination process is also performed at approximately 110°C. Consequently, there is a problem in that thermal deformation of the mask metal film or metal sheet may occur in high-temperature regions above 100°C. In addition, a liquid photoresist is also used separately from the liquid wax to form a pattern for etching. That is, conventionally, a liquid wax layer and a liquid photoresist layer are used between the mask metal film and the substrate supporting it.

[0086] On the other hand, since the present invention uses a dry film resist layer (95), it has the effect of enabling the adhesion process to be performed in a low temperature range of about 60°C or lower. In addition, it has the effect of enabling adhesion, etching pattern formation, etc., to be performed using only the dry film resist layer (95) without using a liquid wax layer and a liquid photoresist layer separately. Furthermore, as described below, the dry film resist layer (95) can provide etch resistance and adhesion to the metal sheet (220') during the process of forming the third cell pattern (Cc).

[0087] Meanwhile, although the city is omitted in FIG. 11, a configuration such as the adsorption chuck (80) shown in FIG. 14 may be adsorbed to the moving plate (90) in the step of FIG. 11 to control the movement of the moving plate (90).

[0088] Next, referring to FIG. 12, a patterned insulating portion (MM) can be formed on a metal sheet (220'). The insulating portion (MM) can be formed from a photoresist material using a printing method or the like.

[0089] Next, etching (EC) of the metal sheet (220') can be performed. Methods such as dry etching and wet etching can be used without limitation, and the portion of the metal sheet (220') exposed as a void between the insulating portions (MM) as a result of the etching can be etched (EC). The etched portion of the metal sheet (220') may be the size of the mask cell area (CR), the size of the mask (100), or a size corresponding to the display on which OLED pixel formation is to be performed.

[0090] Next, referring to FIG. 13, the insulating portion (MM) can be removed. After etching (EC), the metal sheet (220') can become a cell sheet portion (220) in which the edge sheet portion (221) and the first and second grid sheet portions (223, 225) are formed. The cell sheet portion (220) in which the edge sheet portion (221) and the first and second grid sheet portions (223, 225) are formed can be provided in a form bonded by interposing a temporary adhesive portion (95) [or a dry film resist layer (95)].

[0091] Next, referring to FIG. 14, a movable plate (90) with a cell sheet portion (220) attached can be loaded onto a border frame portion (210). The movable plate (90) can be transported by a chuck (not shown). For example, the opposite side of the movable plate (90) with the cell sheet portion (220) attached can be adsorbed and transported by a suction chuck (80).

[0092] The cell sheet portion (220) can be in contact with the border frame portion (210). That is, the border sheet portion (221) of the cell sheet portion (220) can be in contact with the upper surface of the border frame portion (210). By loading the movable plate (90) onto the border frame portion (210), the cell sheet portion (220) can be placed on the border frame portion (210). Since the movable plate (90) compresses the cell sheet portion (220), the cell sheet portion (220) and the border frame portion (210) can be in close contact.

[0093] Next, a laser (L) can be irradiated between the cell sheet portion (220) [or, the border sheet portion (221)] and the border frame portion (210) to connect the cell sheet portion (220) to the border frame portion (210) by laser welding. A welding bead (WB) is formed between the laser-welded border sheet portion (221) and the border frame portion (210), and the cell sheet portion (220) can be connected to the border frame portion (210) through the welding bead (WB).

[0094] Next, referring to FIG. 15, after connecting the cell sheet portion (220) and the edge frame portion (210), the moving plate (90) can be debonded from the cell sheet portion (220). The debonding of the cell sheet portion (220) and the moving plate (90) can be performed by applying heat, chemical treatment, ultrasonic treatment, or UV treatment to the temporary adhesive portion (95) [or, dry film resist layer (95)]. When at least one of applying heat, chemical treatment, ultrasonic treatment, or UV treatment is applied to the temporary adhesive portion (95), the adhesive force between the cell sheet portion (220) and the moving plate (90) is weakened, and the moving plate (90) can be debonded from the cell sheet portion (220). After the moving plate (90) is debonded, the temporary adhesive portion (95) remaining on the cell sheet portion (220) can be removed through cleaning, etc.

[0095] Accordingly, as shown in FIG. 15 (a) [side view] and FIG. 15 (b) [front view], the cell sheet portion (220) is connected to the border frame portion (210). This can be provided as a frame (200).

[0096] According to another embodiment, a connection can be made using a metal connector without performing laser welding between the welded edge sheet portion (221) and the edge frame portion (210). As shown in FIG. 14, a movable plate (90) with a cell sheet portion (220) adhesively supported can be loaded onto the edge frame portion (210). At this time, a metal connector (not shown) between the cell sheet portion (220) [or the edge sheet portion (221)] and the edge frame portion (210) can be interposed. The metal connector (not shown) can be formed on the lower surface of the edge sheet portion (221) facing the edge frame portion (210). Alternatively, the metal connector (not shown) can be formed on the upper surface of the edge frame portion (210) facing the edge sheet portion (221).

[0097] The metal joint may include at least one material selected from Cu, Ni, Au, Ag, Al, Sn, In, Bi, Zn, Sb, Ge, and Cd. It is preferable to form the metal joint using a sputtering method, a brazing method, or the like, which allows for the easy formation of a thin film without material limitations, but the method is not limited thereto.

[0098] Next, at least one of heat and pressure may be applied to the metal connection portion. Heat treatment may be performed by applying heat to the cell sheet portion (220), the metal connection portion, and the edge frame portion (210). Alternatively, heat treatment may be performed by applying less heat by simultaneously applying heat and pressure to the cell sheet portion (220), the metal connection portion, and the edge frame portion (210).

[0099] Heat treatment by applying heat and pressure can be performed within a range where the metal connection part can connect the cell sheet part (220) and the edge frame part (210). For example, the metals of the metal connection part can be connected as they are melted by heat treatment and then solidified again, thereby connecting the cell sheet part (220) and the edge frame part (210). For another example, the connection can be performed by changing the interface state of the cell sheet part (220) and the edge frame part (210) in such a way that the metal components of the metal connection part diffuse into the cell sheet part (220) and the edge frame part (210), or conversely, the components of the cell sheet part (220) and the edge frame part (210) diffuse into the metal connection part, or mutual components diffuse.

[0100] The heat treatment can be performed at a temperature of about 200°C to 800°C, and more preferably at a low temperature range of about 200°C to 400°C.

[0101] After connecting the cell sheet portion (220) and the border frame portion (210), the moving plate (90) can be separated from the cell sheet portion (220). The separation process of the moving plate (90) described above can be applied as is.

[0102] FIG. 16 is a schematic diagram showing the elongation state of the cell sheet portion and the moving plate with respect to a change in process temperature according to one embodiment of the present invention.

[0103] Conventionally, in the process of aligning the cell sheet portion (220) with the border frame portion (210), all sides of the cell sheet portion (220) were stretched to flatten the cell sheet portion (220) and the border sheet portion (221) was aligned with the border frame portion (210). After that, the process of connecting the border sheet portion (221) to the border frame portion (210) was performed. Alternatively, after stretching a flat sheet and attaching it to the border frame portion (210), the cell sheet portion (220) was formed by removing the mask cell region (CR) portion through laser scribing, etching, etc. However, the above conventional method has the problem that the alignment error of the mask cell regions (CR) increases because a gripping means, such as a gripper, is connected to the side of the cell sheet portion (220) to apply tension directly.

[0104] On the other hand, the present invention forms a mask cell region (CR) with the metal sheet (220') adhesively supported on the movable plate (90), and connects the manufactured cell sheet portion (220) to the border frame portion (210) while it is adhesively supported through the movable plate (90) without applying tension, thereby having the effect of reducing alignment error.

[0105] The present invention allows internal tensile force to be applied to a metal sheet (220') on a moving plate (90) solely through temperature control via the difference in the coefficient of thermal expansion between the moving plate (90) and the metal sheet (220'), without applying tension by directly connecting a gripping means, such as a gripper, to the side of the cell sheet portion (220). A large-area metal sheet (220') can have tensile force applied uniformly in all directions or in a radial direction on a large-area moving plate (90). Below, with reference to FIG. 16, the behavior during the process of contacting the metal sheet (220') on the moving plate (90) will be examined.

[0106] According to one embodiment, the degree of elongation or tensile force (IT) of the metal sheet (220') can be controlled by controlling the process temperature as shown in FIG. 16. In FIG. 16 (a), the initial lengths are shown as equal to the metal sheet (220') and the movable plate (90) to compare the degree of elongation, but the movable plate (90) may be equal to or larger than the metal sheet (220'), or vice versa.

[0107] Referring to FIG. 16(a), a moving plate (90) and a metal sheet (220') [or a cell sheet portion (220) in which a mask cell region (CR) is formed] are prepared at a room temperature (RT) of about 25°C. In FIG. 16, the metal sheet (220') is described as a sheet made of Invar material, and the moving plate (90) is described as quartz, which has a lower coefficient of thermal expansion than Invar. A temporary adhesive portion (95) [or a dry film resist layer (95)] may be formed on one side of the moving plate (90) and / or the metal sheet (220').

[0108] Next, referring to FIG. 16(b), the process temperature such that the push-pull strength of the temporary adhesive part (95) is 0 to 5 kgf / cm 2 It can be raised to a first process temperature (TS1). The first process temperature (TS1) may be approximately 50 to 70°C. At the first process temperature (TS1), the temporary adhesive portion (95) is 0 to 5 kgf / cm 2In this case, the temporary adhesive portion (95) is in a state where it lacks the adhesive force to bond the metal sheet (220') and the movable plate (90). That is, in a state where the temporary adhesive portion (95) lacks viscosity, it is difficult for the metal sheet (220') and the movable plate (90) to bond, and it can be understood that the metal sheet (220') and the movable plate (90) can easily separate even without the application of a load or external force. Accordingly, the metal sheet (220') and the movable plate (90) only come into contact through the temporary adhesive portion (95) [and the first insulating portion (23)], but they do not bond. The metal sheet (220') can be extended linearly with the temperature rise without being hindered by the temporary adhesive portion (95). In addition, since the coefficient of thermal expansion of the moving plate (90) is lower than that of the metal sheet (220'), at the first process temperature (TS1), the metal sheet (220') can be expanded (L1) relatively more than the degree (L2) of expansion of the moving plate (90).

[0109] Next, referring to FIG. 16 (c), with the metal sheet (220') and the movable plate (90) in contact, the process temperature is such that the adhesive strength of the temporary adhesive part (95) is at least 5 kgf / cm 2 The temperature can be lowered to a second process temperature (TS2) that is larger. The second process temperature (TS2) may be lower than the first process temperature (TS1), approximately 40 to 60°C, and higher than room temperature. As adhesive force appears on the temporary adhesive portion (95) at the second process temperature (TS2), the metal sheet (220') and the movable plate (90) can be bonded. As the temperature decreases, the movable plate (90) shrinks (L2->L3), and the metal sheet (220') can also shrink in response.

[0110] However, when the process temperature is lowered from step (b) to step (c) in FIG. 16 (TS1 -> TS2), the temporary adhesive portion (95) cools and hardens first, and the metal sheet (220') may have a slower rate of temperature reduction than the temporary adhesive portion (95). Accordingly, the metal sheet (220') can be adhered to the movable plate (90) in a longer elongated state. In other words, rather than adhering the metal sheet (220') and the movable plate (90) after raising the temperature from room temperature (RT) directly to the second process temperature (TS2), as in FIG. 16, by adding an additional step of raising the temperature to the first process temperature (TS1) between room temperature (RT) and the second process temperature (TS2), it is possible to achieve the metal sheet (220') being adhered to the movable plate (90) in a longer elongated state. When the metal sheet (220') and the movable plate (90) are bonded after being raised directly from room temperature (RT) to the second process temperature (TS2), the adhesive force is significantly present in the temporary adhesive portion (95), so the metal sheet (220') may not be stretched linearly with respect to the temperature rise due to resistance from the temporary adhesive portion (95). The fact that the metal sheet (220') is stretched further corresponds to the tensile force (IT) contained in the metal sheet (220') supported on the movable plate (90) becoming greater, and means that the cell sheet portion (220) can have a more taut state even after the cell sheet portion (220) is attached to / attached to the edge frame portion (210) in a subsequent process.

[0111] However, it should be noted that this does not mean that bonding the metal sheet (220') and the moving plate (90) after raising the temperature from room temperature (RT) directly to the second process temperature (TS2) is excluded.

[0112] Next, referring to FIG. 16 (e), the process temperature can be lowered to room temperature (RT). As the temperature is lowered, the movable plate (90) shrinks (by L3), and the metal sheet (220') can also shrink accordingly. The movable plate (90) returns to its length at the initial room temperature (RT) state of FIG. 16 (a), but the metal sheet (220') can be bonded to the movable plate (90) to an extent that is elongated (L5) compared to the initial room temperature (RT) state. This degree of elongation (L5) and the tensile force (IT) contained in the metal sheet (220') are greater than the process of bonding the metal sheet (220') and the movable plate (90) after raising the temperature from the aforementioned room temperature (RT) directly to the second process temperature (TS2).

[0113] Meanwhile, between steps (c) and (e) of FIG. 16, a process of lowering the process temperature to a process temperature (TS3) lower than room temperature (RT) may be performed. Afterward, the temperature may be raised back to room temperature (RT). As the temperature is lowered to the process temperature (TS3), the moving plate (90) shrinks (L4) more than in the room temperature state, and the metal sheet (220') may also shrink accordingly. The process temperature (TS3) may be approximately 5 to 15°C. Additionally, the holding time at the process temperature (TS3) may be at least equal to or longer than the holding time at the process temperatures (TS1, TS2) of FIG. 16 (b) and (c). For example, if the holding time at TS1 is 1 minute and the holding time at TS2 is 1 minute, the holding time at TS3 may be 2 minutes or more. In this way, the viscosity of the temporary adhesive part (95) increases through rapid cooling rather than slow cooling, and the adhesive strength may be increased. As the adhesive strength of the temporary adhesive portion (95) is maximized, the metal sheet (220') and the movable plate (90) are more firmly bonded, and the length of the metal sheet (220') that is further extended in step (b) of FIG. 16 can be maintained even after the temperature drops.

[0114] Figure 16 described above illustrates an embodiment in which an internal tensile force (IT) is applied to a metal sheet (220') on a moving plate (90) through temperature control, but is not limited thereto, and an internal tensile force (IT) may be applied to the metal sheet (220') by applying other temperature control methods.

[0115] According to another embodiment, the metal sheet (220') is a sheet made of Invar material, and the movable plate (90) is BOROFLOAT having a higher coefficient of thermal expansion than Invar. ® 33 can be used. In this case, temperature control can be performed in reverse compared to the embodiment of FIG. 16. First, the process temperature can be lowered to a temperature lower than at least room temperature (20±5℃). The temperature lower than room temperature may include a range from below zero to room temperature.

[0116] In the next step, the metal sheet (220) and the movable plate (90) can be bonded together by interposing a temporary adhesive portion (95) made of a dry film resist layer material.

[0117] In the next step, the process temperature can be raised to room temperature. As the process temperature rises to room temperature, the thermal expansion coefficient of the moving plate (90) is high, so the degree of relative elongation becomes greater than that of the metal sheet (220'). Since the metal sheet (220') is bonded to the moving plate (90), tensile force can be applied to all lateral directions of the metal sheet (220') to the extent that the moving plate (90) elongates more than the metal sheet (220'). The metal sheet (220') can be bonded and supported on the moving plate (90) while tensile force is applied in the lateral directions.

[0118] According to another embodiment, if the metal sheet (220') is directly subjected to tension on the moving plate (90) and then bonded, the large-area moving plate (90) may be bent by the tension force of the large-area metal sheet (220'). When the metal sheet (220') [or cell sheet portion (220)] is bonded to the moving plate (90), it may be bent concavely in the direction of the metal sheet (220'). That is, the moving plate (90) located at the bottom may be bent downwards. In this case, the moving plate (90) is flipped over and aligned with the edge frame portion (210), and the moving plate (90) that is bent upwards is straightened by its own weight, and the bonded metal sheet (220') [or cell sheet portion (220)] is pressed to straighten the bent part together. Through this, the metal sheet (220') [or cell sheet part (220)] can be connected to the border frame part (210) while being stretched taut.

[0119] In addition, the adsorption chuck (80) described above in FIG. 14 may further include means for generating heat. As the adsorption chuck (80) generates heat and transfers this heat to the metal sheet (220') and the moving plate (90), tensioning of the metal sheet (220') through temperature control may be performed as described above in FIG. 16.

[0120] Meanwhile, apart from forming the aforementioned mask pattern (P) in a fine size, it is considered important that multiple mask cell regions (CR) in the cell sheet portion (220) are accurately aligned along the X-axis and Y-axis directions. An organic material for forming an OLED pixel passing through a single mask cell region (CR) can pass through multiple mask patterns (P) of the mask (100) to form a pixel of a single display. In other words, each mask cell region (CR) can correspond to a display. For the mass production quality of OLED pixels, the error range of the X-axis and Y-axis lengths between the mask cell regions (CR) is considered to be approximately ±30 to 40 μm or less. As OLED technology evolves, there is a trend toward minimizing bezels, and to minimize the bezel width, it is necessary for the width of the border of the mask cell region (CR), which is the periphery of the mask (100) through which the organic material forming the pixel passes, to become more uniform.

[0121] In addition, when wet etching is performed during the process of forming a mask cell region (CR) in the cell sheet portion (220), the difference in size between the etching solution entry surface and the opposite surface is inevitably large due to isotropic etching, similar to what is described above in FIG. 8. In terms of bezel minimization, it is necessary to minimize dead space at the edges of the mask cell region (CR) caused by wet etching.

[0122] Accordingly, the following describes a manufacturing method that can reduce the boundary error between mask cell regions (CR) while simultaneously minimizing dead space.

[0123] FIGS. 17 and 18 are schematic diagrams illustrating the manufacturing process of a cell sheet portion according to an embodiment of the present invention. FIG. 19 is a schematic diagram illustrating the cell pattern of a cell sheet portion according to an embodiment of the present invention.

[0124] In the following description, for convenience of explanation, the formation of a single mask cell region (CR) in the cell sheet portion (220) is described as an example, but it can be understood that multiple mask cell regions (CR) must be formed simultaneously.

[0125] Referring to FIG. 17 (a), first, a metal sheet (220') for manufacturing the cell sheet portion (220) of the frame (200) can be prepared. As described above in FIG. 11, the metal sheet (220') may be adhered to the movable plate (90) via a temporary adhesive portion (95) [or a dry film resist layer (95)].

[0126] Since the metal sheet (220') is to be used as a cell sheet portion (220) supporting the mask (100), a thickness greater than that of the mask (100) may be used. According to one embodiment, the thickness of the metal sheet (220') may be approximately 70 μm to 200 μm. The thickness of the metal sheet (220') may be at least twice as thick as the thickness of the mask (100). Meanwhile, within the range thicker than the mask (100), or within the range thicker than twice, the thickness of the metal sheet (220') may be set to approximately 50 μm to 200 μm. For example, when the thickness of the mask (100) is approximately 2 μm to 50 μm, the metal sheet (220') is several times to tens of times thicker, and the width of the mask cell region (CR) [or cell pattern (CP)] is much larger than the width of the mask pattern (P), which is approximately tens of μm, on a scale of tens of mm to hundreds of mm. Therefore, it is necessary to form a mask cell region (CR) [or cell pattern (CP)] by applying a different wet etching process. Accordingly, the cell sheet portion (220) applies a process to form three or more cell patterns (Ca, Cb, Cc). In the following description, the mask cell region (CR) is formed using three cell patterns (Ca, Cb, Cc) with a thickness of approximately 150 μm, but depending on the thickness of the cell sheet portion (220), an additional etching process may be performed to form a mask cell region (CR) using four or more cell patterns.

[0127] A patterned first insulating portion (Ma) can be formed on one side (upper surface) of a metal sheet (220'). The first insulating portion (Ma) can be formed from a photoresist material using a printing method or the like. The material and method of forming the first insulating portion (Ma) can be the same as the process of forming the first insulating portion (M1) in FIG. 5 (a).

[0128] Next, referring to FIG. 17(b), a first cell pattern (Ca) can be formed to a predetermined depth by a first wet etching (WEa) on one side (top side) of the metal sheet (220'). When performing the first wet etching (WEa), the metal sheet (220') must not be penetrated. Thus, the first cell pattern (Ca) can be formed in an approximately arc shape without penetrating the metal sheet (220'a).

[0129] Since the first wet etching (WEa) has isotropic etching characteristics, the width (Rb) of the first cell pattern (Ca) does not have the same width as the spacing (Ra) between patterns of the first insulating part (Ma), but can have a wider width than the spacing (Ra) between patterns of the first insulating part (Ma). In other words, since an undercut is formed on both lower sides of the first insulating part (Ma), the width (Rb) of the first cell pattern (Ca) can be larger than the spacing (Ra) between patterns of the first insulating part (Ma) by the width of the undercut. The spacing (Ra) between patterns can correspond to approximately tens of millimeters to hundreds of millimeters, which corresponds to the width of the mask cell area (CR) [or cell pattern (CP)].

[0130] The formation depth of the first cell pattern (Ca) may be about 60 to 70% of the thickness of the metal sheet (220'). For example, when using a metal sheet (220') with a thickness of about 150 μm, the formation depth of the first cell pattern (Ca) may be about 90 to 105 μm, so the difference between the width (Rb) of the first cell pattern (Ca) and the gap (Ra) between the pattern of the first insulating part (Ma) due to the undercut may be equal to or smaller than the formation depth of the first cell pattern (Ca).

[0131] Next, referring to FIG. 17 (c), a second insulating portion (Mb) can be formed within at least the first cell pattern (Ca). The process of forming the second insulating portion (Mb) while the first cell pattern (Ca) is formed can apply the process described above from FIG. 5 (c) to FIG. 6 (f). The second insulating portion (Mb) is formed on one side (upper surface) of the metal sheet (220'a), and baking is performed to volatilize a portion of the second insulating portion (Mb). Then, exposure (L) is performed from the top to apply the first insulating portion (Ma) as an exposure mask. Since the second insulating portion (Mb) is a positive type photoresist, the exposed (L) portion can be removed. The space where the second insulating portion (Mb) remains can correspond to the space where undercuts are formed on both lower sides of the first insulating portion (Ma) [refer to step FIG. 5 (b)]. The spacing (Ra) between patterns of the second insulating part (Mb) may be the same as the spacing (Ra) between patterns of the first insulating part (Ma).

[0132] Next, referring to FIG. 18 (d), a second wet etching (WEb) can be performed on the first cell pattern (Ca) of the metal sheet (220'b). The wet etching solution can penetrate into the space between the patterns of the first insulating part (Ma) and the space of the first cell pattern (Ca) to perform the second wet etching (WEb). A second cell pattern (Cb) can be formed to a predetermined depth by the second wet etching (WEb). When performing the second wet etching (WEb), the metal sheet (220'a) must not be penetrated. Thus, the second cell pattern (Cb) can be formed in an approximately arc shape without penetrating the metal sheet (220'b).

[0133] Since the second wet etching (WEb) has isotropic etching characteristics, the width (Rc) of the second cell pattern (Cb) does not have the same width as the spacing (Ra) between patterns of the second insulating part (Mb), but can have a wider width than the spacing (Ra) between patterns of the second insulating part (Mb). In other words, since an undercut is formed on both lower sides of the second insulating part (Mb), the width (Rc) of the second cell pattern (Cb) can be larger than the spacing (Ra) between patterns of the second insulating part (Mb) by the width of the undercut.

[0134] The formation depth of the second cell pattern (Cb) may be about 20 to 30% of the thickness of the metal sheet (220'). For example, when using a metal sheet (220') with a thickness of about 150 μm, the formation depth of the second cell pattern (Cb) may be about 30 to 45 μm, so the difference between the width (Rc) of the second cell pattern (Cb) due to the undercut and the gap (Ra) between the pattern of the second insulating part (Mb) may be equal to or smaller than the formation depth of the second cell pattern (Cb).

[0135] In addition, since the formation depth of the first cell pattern (Ca) is thicker than the formation depth of the second cell pattern (Cb), the difference between the width (Rb) of the first cell pattern and the gap (Ra) between the patterns of the first and second insulating parts (Ma, Mb) may be greater than the difference between the width (Rc) of the second cell pattern and the gap (Ra) between the patterns of the first and second insulating parts (Ma, Mb).

[0136] Next, referring to FIG. 18 (e), a third insulating part (Mc) can be formed within at least the second cell pattern (Cb). The process of forming the third insulating part (Mc) while the second cell pattern (Cb) is formed may be the same as the process of forming the second insulating part (Mb) described above in FIG. 17 (c). The space left by the third insulating part (Mc) may correspond to the space where undercuts are formed on both lower sides of the second insulating part (Mb). The spacing (Ra) between the patterns of the third insulating part (Mc) may be the same as the spacing (Ra) between the patterns of the first insulating part (Ma).

[0137] Next, referring to (f) of FIG. 18, a third wet etching (WEc) can be performed on the second cell pattern (Cb) of the metal sheet (220'b). The wet etching solution can penetrate the space between the patterns of the third insulating part (Mc) and the space of the second cell pattern (Cb) to perform the third wet etching (WEc). The third wet etching (WEc) can form the third cell pattern (Cc) by penetrating the metal sheet (220'b). That is, the third cell pattern (Cc) can be formed by opening through the other side of the metal sheet (220'c) from the bottom of the second cell pattern (Cb).

[0138] Meanwhile, if liquid wax or photoresist is used to bond the moving plate (90) and the metal sheet (220') as in the conventional method, during the third wet etching (WEc) process, the portion of the metal sheet (220'c) around the third cell pattern (Cc) may not adhere to the liquid wax / photoresist layer and a lifted portion may appear. The lifted portion may be further caused by the low adhesion of the liquid wax / photoresist layer. In this case, if the third wet etching solution penetrates through the lifted portion, a problem may occur in which the desired third cell pattern (Cc) is not formed.

[0139] However, the dry film resist layer (95) used for bonding the moving plate (90) and the metal sheet (220') in the present invention has superior adhesion and etch resistance compared to conventional liquid wax / photoresist layers. Since the metal sheet (220') adheres to the dry film resist layer (95) with strong adhesion, there are no lifted parts of the metal sheet (220'c) around the third cell pattern (Cc). Since there are no lifted parts, the third cell pattern (Cc) can be clearly formed as desired.

[0140] Since the third wet etching (WEc) has isotropic etching characteristics, the width (Rd) of the third cell pattern (Cc) does not have the same width as the spacing (Ra) between patterns of the third insulating part (Mc), but can have a wider width than the spacing (Ra) between patterns of the third insulating part (Mc). In other words, since an undercut is formed on both lower sides of the third insulating part (Mc), the width (Rd) of the third cell pattern (Cc) can be larger than the spacing (Ra) between patterns of the third insulating part (Mc) by the width of the undercut.

[0141] The formation depth of the third cell pattern (Cc) may be about 10 to 20% of the thickness of the metal sheet (220'). For example, when using a metal sheet (220') with a thickness of about 150 μm, the formation depth of the third cell pattern (Cc) may be about 15 to 30 μm.

[0142] In addition, since the formation depth of the second cell pattern (Cb) is thicker than the formation depth of the third cell pattern (Cc), the difference between the width (Rc) of the second cell pattern and the spacing (Ra) between the patterns of the first, second, and third insulating parts (Ma, Mb, Mc) may be greater than the difference between the width (Rd) of the third cell pattern and the spacing (Ra) between the patterns of the first, second, and third insulating parts (Ma, Mb, Mc).

[0143] Since the lower width of the third cell pattern (Cc) defines the width of the mask cell region (CR), the smaller the difference between the width (Rd) of the third cell pattern and the gap (Ra) between the patterns of the first, second, and third insulating parts (Ma, Mb, Mc), the smaller the error range of the X-axis and Y-axis widths between the mask cell regions (CR). Therefore, it is desirable that the difference between the width (Rd) of the third cell pattern and the gap (Ra) between the patterns of the first, second, and third insulating parts (Ma, Mb, Mc) be about 30 μm or less.

[0144] Next, referring to FIG. 19, the first, second, and third insulating parts (Ma, Mb, Mc) can be removed to complete the manufacture of the cell sheet part (220). The sum of the shapes of the subsequent first cell pattern (Ca), second cell pattern (Cb), and third cell pattern (Cc) can form a cell pattern (CP) [or, mask cell region (CR)].

[0145] As described above, the thickness (Tc) of the first cell pattern (Ca) may be about 60% to 70% of the thickness (T) of the cell sheet portion (220), the thickness (Tb) of the second cell pattern (Cb) may be 20% to 30% of the thickness (T) of the cell sheet portion (220), and the thickness (Ta) of the third cell pattern (Cc) may be 10% to 20% of the thickness of the cell sheet portion (220). The sum of the thicknesses of the first cell pattern (Ca), the second cell pattern (Cb), and the third cell pattern (Cc) may correspond to the thickness (T) of the cell sheet portion (220).

[0146] Meanwhile, according to another embodiment, the thicknesses (Tc, Tb) of the first cell pattern (Ca) and the second cell pattern (Cb) may be the same. Even in this case, it is more desirable for reducing the error range of the aperture [mask cell region (CR)] width that the thickness (Ta) of the third cell pattern (Cc) is not greater than the thicknesses (Tc, Tb) of the first and second cell patterns (Ca, Cb).

[0147] Both sides of the cell pattern (CP) [mask cell region (CR)] may be formed to have curvature. The first, second, and third cell patterns (Ca, Cb, Cc) may each be formed to have sides with curvature and may be formed to have concave curvature. Overall, both sides of the cell pattern (CP) may exhibit a tilted shape.

[0148] More specifically, the slope between an arbitrary straight line (L1) from the upper edge (Ca1) of the first cell pattern (Ca) to the upper edge (Cb1) of the second cell pattern (Cb) and the horizontal plane, and the slope between an arbitrary straight line (L2) from the upper edge (Cb1) of the second cell pattern (Cb) to the upper edge (Cc1) of the third cell pattern (Cc) and the horizontal plane may have a non-vertical, inclined angle. Additionally, since the thickness of the first cell pattern (Ca) is thicker than that of the second cell pattern (Cb), considering the isotropic etching shape, the slope between an arbitrary straight line (L2) from the upper edge (Cb1) of the second cell pattern (Cb) to the upper edge (Cc1) of the third cell pattern (Cc) and the horizontal plane may be greater than the slope between an arbitrary straight line (L1) from the upper edge (Ca1) of the first cell pattern (Ca) to the upper edge (Cb1) of the second cell pattern (Cb) and the horizontal plane.

[0149] FIG. 20 is a schematic diagram showing a form in which a mask (100) is connected on a cell sheet portion (220) according to one embodiment of the present invention.

[0150] Referring to FIG. 20, a cell sheet portion (220) can be connected to a border frame portion (210) by forming a weld bead (WB1) through welding. Additionally, a mask (100) can be connected to the cell sheet portion (220) by forming a weld bead (WB2) through welding on each mask cell area (CR) of the cell sheet portion (220). Based on FIG. 20, the mask (100) can be connected to the upper part of the third cell pattern (Cc). That is, the open width of the third cell pattern (Cc) can substantially be provided as a mask cell area (CR).

[0151] The mask (100) can cover the entire mask cell area (CR). Additionally, the cell (C) [see FIG. 3] in which the multiple mask patterns (P) of the mask (100) are formed must be within the width of the mask cell area (CR), and the dummy of the mask (100) can be supported on the mask cell area (CR). Accordingly, the exposed area [open width] of the third cell pattern (Cc) can have a larger area than the cell (C), which is the area of ​​the multiple mask patterns (P) formed on the mask (100).

[0152] Since the width of the mask cell region (CR) [or cell pattern (CP)] in the X-axis and Y-axis directions is on a scale of tens of mm to hundreds of mm, the organic materials deposited in the OLED pixel deposition process that enter the central part of the mask cell region (CR) have high uniformity, however, the entry of organic materials from the edge part of the mask cell region (CR) may be considered. According to one embodiment, the slope (a3) ​​[see FIG. 19] between any straight line (L1) from the upper edge (Ca1) of the first cell pattern (Ca) to the upper edge (Cb1) of the second cell pattern (Cb) and the horizontal plane may be 50° or less. That is, since the organic materials deposited in the OLED pixel deposition process can enter along a relatively low-slope and wide plane having a slope of 50° or less in the first cell pattern (Ca) through which they pass first [the direction of entry of the organic materials is indicated by an arrow], the amount of organic materials scattered from the inner wall of the first cell pattern (Ca) and incident toward the center can be reduced. As a result, the amount of organic matter entering the corner portion of the cell pattern (CP) increases, so there is an effect that organic matter can enter more uniformly across the entire area of ​​the mask cell region (CR) before passing through the mask pattern (P) of the mask (100).

[0153] In addition, as described above in FIG. 19, since the slope between the horizontal plane and the arbitrary straight line (L2) from the upper edge (Cb1) of the second cell pattern (Cb) to the upper edge (Cc1) of the third cell pattern (Cc) is greater than the slope between the horizontal plane and the arbitrary straight line (L1) from the upper edge (Ca1) of the first cell pattern (Ca), the deposited organic materials can enter along the wide plane of the first cell pattern (Ca) and gradually concentrate on the edge portion of the mask cell region (CR), thereby enabling the organic materials to enter more uniformly across the entire area of ​​the mask cell region (CR) before passing through the mask pattern (P) of the mask (100).

[0154] FIG. 21 is an electron microscope image showing a cell pattern according to one embodiment of the present invention.

[0155] Referring to FIG. 21, the thickness of the mask (100) is approximately 140 μm, and it can be seen that the first cell pattern (Ca), the second cell pattern (Cb), and the third cell pattern (Cc) have a shape with side curvature due to isotropic etching. The layer with a darker color on the upper part of the cell pattern (CP) corresponds to the first, second, and third insulating parts (Ma, Mb, Mc). The angle (a3) ​​of an arbitrary straight line (L1) from the upper corner (Ca1) of the first cell pattern (Ca) to the upper corner (Cb1) of the second cell pattern (Cb) is approximately 47.8°, and since the slope in the lower part is larger, it can be seen that organic materials entering the corner part of the first cell pattern (Ca) can be more uniformly concentrated into the third cell pattern (Cc). Organic materials that have passed through the third cell pattern (Cc) [or, mask cell region (CR)] can pass through the mask pattern (P) of the mask (100) to form an OLED pixel on a target substrate for forming an OLED pixel.

[0156] Meanwhile, the present invention may also exhibit a characteristic structure on the side (CS) of the outer portion of the cell sheet portion (220) [see (b) of FIG. 30] in addition to the cell pattern (CP) [or, mask cell region (CR)].

[0157] FIG. 22 is a schematic diagram showing the manufacturing process of a cell sheet portion and a frame according to a comparative example. FIG. 23 is a partially enlarged schematic diagram of FIG. 22 according to a comparative example. FIG. 23 is an enlarged view of the upper right portion of FIG. 22 (b).

[0158] Referring to FIG. 22 (a), the manufacturing process of a frame according to a comparative example first provides a border frame portion (210). The border frame portion (210) may be a rectangular frame shape including a hollow area (R).

[0159] Next, referring to FIG. 22(b), a cell sheet portion (220') is manufactured. The cell sheet portion (220') can be manufactured by manufacturing a flat sheet using electroplating or other film forming processes, and then removing the mask cell region (CR) portion [or forming a cell pattern (CP)]. For example, if a 6 x 5 mask cell region (CR: CR11~CR56) is formed, there may be five first grid sheet portions (223) and four second grid sheet portions (225).

[0160] Next, the cell sheet portion (220') can be aligned with the border frame portion (210). In the alignment process, each side of the cell sheet portion (220') is stretched (F1~F4) so ​​that the cell sheet portion (220') is flattened and the border sheet portion (221') can be aligned with the border frame portion (210).

[0161] Next, referring to FIG. 22 (b) and FIG. 23, if the cell sheet portion (220') corresponds to the border frame portion (210), the border sheet portion (221') of the cell sheet portion (220) can be connected by welding. A weld bead (WB) may be formed at the welded portion, and it may serve as a medium that integrally connects the border frame portion (210) and the cell sheet portion (220') using the same material as the cell sheet portion (220').

[0162] According to the comparative example or prior art, the cell sheet portion (220') can be connected to the border frame portion (210), but since a process of tensioning the side of the cell sheet portion (220) is essential, a part is required to grip and tension the cell sheet portion (220'). As a part to grip when tensioning each side of the cell sheet portion (220') (F1~F4), a part that is removed after connecting the cell sheet portion (220') to the border frame portion (210) is required. This part may be provided as a protrusion (PT). Alternatively, this part may be provided as an outer border portion of the border sheet portion (221'), and the outer border portion may be provided with a wider width than the border sheet portion (221') connected to the final frame (200), so that a predetermined width may be removed later.

[0163] FIG. 22(b) and FIG. 23 illustrate a protrusion (PT) that protrudes outward from the edge sheet portion (221') in an extended form of the first and second grid sheet portions (223', 225') of the cell sheet portion (220'). A gripper (not shown) grips the protrusion (PT) and then applies a tensile force. For example, in the case of a cell sheet portion (220') corresponding to a 6G half size, 100 mask cell regions (CR) may be provided, with 6 first grid sheet portions (223') and 20 second grid sheet portions (225'). Here, if a protrusion (PT) is formed between two mask cell regions (CR), a total of 44 protrusions (PT) may be formed on the outer side of the edge sheet portion (221') spaced apart from each other in a 4 x 11 configuration.

[0164] After gripping the protrusions (PT) on the four sides [or the four sides of the border sheet (221')] of the cell sheet portion (220') which has an overall square shape, a tensile force (F1~F4) is applied. As the border sheet portion (221') and the first and second grid sheet portions (223', 225') are tensioned by the application of the protrusions (PT), the cell sheet portion (220') is connected to the border frame portion (210) in a taut state overall.

[0165] FIG. 24 is a schematic diagram illustrating the process of connecting a cell sheet portion according to the first comparative example to a border frame portion. Hereinafter, the process of connecting a cell sheet portion (220') further equipped with a protrusion (PT) to a border frame portion (210) is described as an example. For convenience of explanation, the first and second grid sheet portions (223', 225') and the border frame portion (210) are omitted from the illustration, and a part of the border sheet portion (221') and the mask cell area (CR) are illustrated and described.

[0166] First, referring to FIG. 24 (a), a cell sheet portion (220') in which a border frame portion (210) and a mask cell region (CR) are formed can be prepared as described in FIG. 22 (a) and (b). Next, a protrusion (PT) protruding outward from the border sheet portion (221') is gripped by a gripper, and a tensile force (F) is applied. Then, as shown in FIG. 24 (b), when the border sheet portion (221') corresponds to an appropriate position on the border frame portion (210), welding is performed to form a weld bead (WB). The border sheet portion (221') is connected to the border frame portion (210) via the weld bead (WB). The tensile force (F) must be applied until the welding process is completed.

[0167] Next, as shown in (c) of FIG. 24, the protrusion (PT) is removed. The area between the protrusion (PT) and the outer edge of the border sheet portion (221') is set as the cutting line (CL). The removal of the protrusion (PT) is performed by physical cutting, mechanical cutting, or laser cutting. The protrusion (PT) can be removed in a single process, but as shown in the enlarged portion of (c) of FIG. 24, after forming a half notch (NC) first, an additional cutting process can be performed along the cutting line (CL), or the protrusion (PT) can be pulled outward from the half notch (NC) to cut it off.

[0168] Next, as shown in (d) of FIG. 24, when the protrusion (PT) is removed, a cut surface (CS1) appears at the part where the protrusion (PT) of the edge sheet part (221') was connected. Since the cut surface (CS1) [or the outer edge side of the cell sheet part (220')] appears by physical cutting, mechanical cutting, or laser cutting, its shape may be irregular. That is, the shape of the half notch (NC) of the cut surface (CS1) is maintained to some extent, but the shape of the cut surface (CS1) is irregular in the remaining part due to reasons such as being pulled and broken, and the cut surface (CS1) may even remain in an elongated state.

[0169] FIG. 25 is a schematic diagram illustrating the process of connecting a cell sheet portion according to a second comparative example to a border frame portion. FIG. 25 illustrates the process of connecting a cell sheet portion (220') having a protrusion (PT) to a border frame portion (210) as an example, but it should be noted that the border sheet portion (221') is provided with a wider width instead of the protrusion (PT) and can be applied to a comparative example that is later removed by a predetermined width.

[0170] Figures 25 (a) and (b) are identical to Figures 24 (a) and (b).

[0171] Next, as shown in (c) of FIG. 25, the border sheet portion (221') is removed. When a predetermined width is removed from the outer edge of the border sheet portion (221'), the protrusion (PT) is also removed. A cutting line (CL) is set inward by a predetermined width from the outer edge of the border sheet portion (221'). The cutting of the cutting line (CL) is performed by physical cutting, mechanical cutting, or laser cutting. The cutting of the cutting line (CL) may be performed in a single process, but as shown in the enlarged portion of (c) of FIG. 25, after forming a half notch (NC) first, an additional cutting process may be performed along the cutting line (CL), or the border sheet portion (221') on the outer part of the cutting line (CL) may be pulled outward and cut off based on the half notch (NC).

[0172] Next, as shown in (d) of FIG. 25, when a portion of the edge sheet portion (221') and the protrusion (PT) are removed, a cut surface (CS2) appears. Since the cut surface (CS2) [or the outer edge side of the cell sheet portion (220')] is formed by physical cutting, mechanical cutting, or laser cutting, its shape may be irregular. That is, while the shape of the half notch (NC) of the cut surface (CS2) is maintained to some extent, the shape of the cut surface (CS2) is irregular in the remaining parts due to reasons such as being pulled and broken, and the cut surface (CS2) may even remain in an elongated state.

[0173] FIGS. 26 and 27 are electron microscope images showing the side of the outer edge of the cell sheet portion according to the first comparative example. FIG. 26 (a) shows a cross-sectional view (CS1) of the cell sheet portion (220'), and FIG. 26 (b) is a magnified image of the cross-sectional view (CS1) portion in FIG. 26 (a).

[0174] Referring to FIG. 26, it can be seen that the upper part (CSa) of the cut surface (CS1) remains in an elongated state as a result of pulling the protrusion (PT) outward and cutting it off. It can be seen that the lower part (CSb) of the cut surface (CS1) retains the shape of the notch (NC).

[0175] Figure 27 is a frontal view of the cross-section (CS1) of Figure 26. The boundary between the upper (CSa) and lower (CSb) sections of the cross-section (CS1) is clearly visible as a horizontal line. In particular, as shown in Figure 27 (b), the average surface roughness (Ra) of the lower section (CSb) is low and the surface roughness appears relatively uniform, whereas the upper section (CSa) has a high average surface roughness and a large variation in surface roughness. There is a distinct difference in the average surface roughness between the upper (CSa) and lower (CSb) sections, and the value exceeds at least 10%. This is the result of pulling and cutting the remaining part of the notch (NC) as described above.

[0176] FIGS. 28 and 29 are electron microscope images showing the side of the outer edge of the cell sheet portion according to the second comparative example. FIG. 28 (a) shows the cross-sectional plane (CS2) of the cell sheet portion (220'), and FIG. 28 (b) is a magnified image of the cross-sectional plane (CS2) portion in FIG. 28 (a).

[0177] Referring to FIG. 28, it can be seen that the upper part (CSa) of the cut surface (CS2) remains in an elongated state as a result of pulling and cutting the outer part of the edge sheet portion (221') beyond the cutting line (CL). It can be seen that the lower part (CSb) of the cut surface (CS2) maintains the shape of the notch (NC). In particular, FIG. 26 shows a relatively small elongated state because only the protrusion (PT) part is pulled, whereas FIG. 28 shows a relatively larger elongated state because each side of the edge sheet portion (221'), including the protrusion (PT), is pulled outward.

[0178] FIG. 29 is a frontal view of the cross-section (CS2) of FIG. 28. The boundary between the upper (CSa) and lower (CSb) sections of the cross-section (CS2) is clearly visible as a horizontal line. In particular, it can be seen that the average surface roughness of the lower section (CSb) is low and relatively uniform, while the upper section (CSa) has a high average surface roughness and a large variation in surface roughness. This is the result of pulling and cutting the remaining part of the notch (NC) as described above.

[0179] FIG. 30 is a schematic diagram showing the process of connecting a cell sheet portion to a border frame portion according to one embodiment of the present invention.

[0180] Referring to FIG. 30(a), as described above in FIG. 11 to 15, a cell sheet portion (220) having a plurality of mask cell regions (CR) [or cell pattern (CP)] formed thereon can be attached to a movable plate (90) and corresponded to a border frame portion (210). As described above in FIG. 16, since a tensile force (IT) is applied to the cell sheet portion (220) on the movable plate (90), there is no need to apply a tensile force to the cell sheet portion (220) using a separate means such as a gripper.

[0181] Referring to (b) of FIG. 30, similar to the step described above in FIG. 14, the cell sheet portion (220) is aligned with the border frame portion (210), and then welding is performed to connect the border frame portion (210) and the cell sheet portion (220) through the weld bead (WB).

[0182] Since the cell sheet portion (220) of the present invention does not need to provide a gripping portion such as a protrusion (PT), the cutting process of the protrusion (PT) is not performed. Therefore, the cut surface (CS) of the outer edge of the border sheet portion (221) is not formed after the cell sheet portion (220) is connected to the border frame portion (210), but can be formed at the manufacturing stage of the cell sheet portion (220). That is, when the mask cell area (CR) [or cell pattern (CP)] is formed, the outer edge of the cell sheet portion (220) can also be processed together, so the side (CRS) of the mask cell area (CR) can have a shape substantially identical to the cut surface (CS) of the outer edge of the cell sheet portion (220).

[0183] FIG. 31 is a schematic diagram showing a side cross-section of a border sheet portion among cell sheet portions according to one embodiment of the present invention.

[0184] The side (CRS) of the mask cell region (CR) can have the same cross-sectional shape, surface characteristics, material characteristics, physical properties, etc., as the side (CS) of the outer edge of the cell sheet portion (220) through the same process.

[0185] The mask cell region (CR) [or cell pattern (CP)] can be formed using wet etching. Additionally, not only the mask cell region (CR) but also the outer edge of the cell sheet portion (220) can be processed simultaneously in the wet etching (EC) process described above in FIG. 12. Accordingly, the side shape of the mask cell region (CR) or the shape of the cell pattern (CP) may include a curvature shape resulting from isotropic wet etching, similar to the shape of the side (CS). Alternatively, the side shape of the mask cell region (CR) or the shape of the cell pattern (CP) may be identical to the shape of the side (CS).

[0186] As in FIG. 31 (a), the side shape of the mask cell region (CR), or the shape of the cell pattern (CP) and the outer edge side (CS) of the cell sheet portion (220) may include a single curvature, or as in FIG. 31 (b), the process of FIG. 17 to FIG. 19 may be performed to include a plurality of curvatures.

[0187] On the other hand, in the case of Comparative Examples 1 and 2 above, the side shape of the mask cell region (CR) or the shape of the cell pattern (CP) can be formed by wet etching during the manufacturing stage of the cell sheet portion (220'), but since the outer edge shape of the cell sheet portion (220') is formed by physical, mechanical, or laser cutting methods rather than wet etching, the shape of the outer cut surface (CS1, CS2) appears completely different. Even if the outer edge shape of the cell sheet portion (220') is formed by wet etching, it must be performed at a different stage from the formation stage of the mask cell region (CR), so a difference in the side / cut surface shape is inevitable. The shape of the outer side (CS) of the edge sheet portion (221) according to the embodiment of the present invention exhibits curvature due to wet etching, and unlike mechanical / physical cutting, the cell sheet portion (220) is etched by a chemical reaction, so a different result in material properties is inevitable.

[0188] FIG. 32 is an electron microscope image showing the side of the outer edge of the cell sheet portion according to one embodiment of the present invention.

[0189] Referring to FIG. 32, the shape of the outer side (CS) of the edge sheet portion (221) can be seen to have a curvature shape resulting from isotropic wet etching. Additionally, since the side (CS) does not have a part that is arbitrarily pulled and stretched for cutting, it can be seen that no part protruding above the upper horizontal plane of the cell sheet portion (220) appears.

[0190] Since the side (CS) is the result of the same process throughout, the average surface roughness can be constant even if an arbitrary area is set, not just the top and bottom. In addition, since the outer side (CS) of the border sheet portion (221) and the side of the mask cell area (CR) are the result of the same process, the average surface roughness is constant, and even if there is a difference, it can be less than 10%. The side shape of the mask cell area (CR) can also include a high-ratio shape as in FIG. 32.

[0191] As described above, the present invention manufactures a frame (200) by manufacturing a cell sheet portion (220) on a moving plate (90) and connecting it to a border frame portion (210), so the steps of complex tensioning with a gripper and removing protruding parts can be omitted, thus having the advantage of a simple process. In addition, the present invention has the advantage of being able to infer the manufacturing process of the cell sheet portion (220) and the process of forming the frame (220) by connecting it to the border frame portion (210) by examining the shape of the outer side (CS) of the border sheet portion (221) and the side (CRS) of the mask cell region (CR) [or cell pattern portion (CP)].

[0192] FIG. 33 is a planar schematic diagram showing the shape of an extension support member (310) according to an embodiment of the present invention. FIG. 34 is a planar schematic diagram showing a frame (300) with a cell sheet member (220) connected on an extension support member (310) according to an embodiment of the present invention. FIG. 35 is an enlarged side schematic diagram of part I of FIG. 34, showing a shape in which a support grid bar (315) and a cell sheet member (220) are connected to an extension edge member (311).

[0193] The size of each cell sheet portion (220) may be a 6G half size. A 6G may have a width x height of approximately 1,500mm x 1,800mm, and a 6G half may have a size of approximately 1,500mm x 900mm. Up to the size of one cell sheet portion (220), a connection body (10) of a mask and a frame can be manufactured by connecting it to the frame (200) described above in FIG. 2. However, if the substrate size increases further to 7G, 8G, or larger, severe sagging of the cell sheet portion (220) and alignment errors of the masks (100) may occur. It becomes very difficult to achieve a resolution of 500 to 600 PPI or higher while simultaneously satisfying productivity.

[0194] Accordingly, the present invention proposes a structure that can perform a pixel process on an extra-large substrate of 7G, 8G or more by connecting a plurality of cell sheet portions (220) to the extended frame (300) as an embodiment applying a frame (300) that is extended beyond the frame (200) of FIG. 2.

[0195] Referring to FIG. 33, an extension support member (310) can be prepared first. The extension support member (310) may include an extension edge member (311) and at least one support grid bar (315). The extension edge member (311) may include a hollow area in the form of a square frame, etc.

[0196] It is preferable that the extended edge portion (311) of the extended support portion (310) has a higher rigidity than or at least the same as the edge frame portion (210) described above in FIG. 2 so as to be able to support a plurality of cell sheet portions (220). Accordingly, it is preferable that the unit frames constituting each edge of the extended edge portion (311) of the extended support portion (310) have a width equal to or greater than the width of the unit frames constituting each edge of the edge frame portion (210).

[0197] Referring to FIGS. 33 and 35, as a support grid bar (315) is connected to the extended edge portion (311), the hollow area of ​​the extended edge portion (311) can be partitioned. One or more support grid bars (315) may be connected to the extended edge portion (311). The support grid bar (315) may have a thinner thickness and a thinner width than the extended edge portion (311).

[0198] Each support grid bar (315: 315-1, 315-2) is formed to extend along a first direction (X-axis direction), and the support grid bars (315: 315-1, 315-2) are connected on an extended edge portion (311) so as to be parallel and spaced apart from each other, thereby providing a plurality of module areas (320: 320-1, 320-2, 320-3). For example, two support grid bars (315: 315-1, 315-2) are connected on the extended edge portion (311), thereby providing three module areas (320: 320-1, 320-2, 320-3), which is one more than the number provided, but is not limited thereto.

[0199] A predetermined groove (312) may be formed on the expanded edge portion (311), and a support grid bar (315) may be inserted into the groove (312) to connect the support grid bar (315) to the expanded edge portion (311). Alternatively, during the process of forming the hollow area of ​​the expanded edge portion (311), only the portion of the support grid bar (315) may be left so that the expanded edge portion (311) and the support grid bar (315) are formed integrally during the manufacturing process. It is preferable to form the upper surface of the expanded edge portion (311) and the upper surface of the support grid bar (315) so that they share the same surface.

[0200] Referring to FIGS. 33 and 34, each module area (320: 320-1, 320-2, 320-3) may correspond to the size and shape of a single cell sheet portion (220). Alternatively, each module area (320) may be provided to correspond to the size and shape of a single movable plate (90), or may be provided to have a larger size than the movable plate (90). That is, the expansion support portion (310) may have a size corresponding to the combined size of a plurality of cell sheet portions (220).

[0201] For example, as illustrated in FIG. 34, a pair of vertically adjacent cell sheet sections (220) can be connected on a single support grid bar (315). For instance, the upper side and left / right side of a cell sheet section (220-1) may be connected to an extended edge section (311), and the lower side may be connected to a support grid bar (315-1). The upper side of a cell sheet section (220-2) may be connected to a support grid bar (315-1), the lower side to a support grid bar (315-2), and the left / right side to an extended edge section (311). The lower side and left / right side of a cell sheet section (220-3) may be connected to an extended edge section (311), and the upper side may be connected to a support grid bar (315-2).

[0202] The support grid bar (315-1) (315-2) can block the gap between adjacent pairs of cell sheet portions (220-1, 220-2) (220-2, 220-3). Accordingly, organic materials for forming OLED pixels can pass only through the mask cell region (CR) of the cell sheet portion (220) and prevent passing between adjacent cell sheet portions (220) from adversely affecting the deposition quality.

[0203] As described above in FIGS. 12 to 14, after forming a cell sheet portion (220) on a movable plate (90), a connection process can be performed by aligning it with each module area (320) of an expansion support portion (310). According to the example of FIG. 34, after preparing the expansion support portion (310), the cell sheet portion (220) in a state bonded to the movable plate (90) can be aligned with the expansion support portion (310), and the cell sheet portion (220) can be connected to the corresponding module area (320) by irradiating a laser (L). For example, if there are three module areas (320: 320-1, 320-2, 320-3), the alignment and connection process of the cell sheet portion (220) three times can be performed to manufacture an expanded frame (300) of 8G Half or higher class.

[0204] The expanded frame (300) may have multiple 6G half cell sheet sections (220) connected to it. The 6G may have a width of approximately 1,500mm x 1,800mm and the 6G half may have a width of approximately 1,500mm x 900mm. Each unit frame constituting the edge of the expanded support section (310) of the frame (300) may have a width of approximately 20mm to 100mm. Therefore, the size of the expanded frame (300) needs to be at least larger than approximately 1,700mm x 1,100mm.

[0205] For example, if the frame (300) has multiple module areas (320) only in the first direction (X-axis), the length in the X-axis direction may be at least 1,700 mm, and may have a length that is a multiple of approximately 1,700 mm. For another example, if the frame (300) has multiple module areas (320) only in the second direction (Y-axis), the length in the Y-axis direction may be at least 1,100 mm, and may have a length that is a multiple of approximately 1,100 mm.

[0206] FIG. 36 is a schematic plan view showing the shape of an extension support member (310') according to another embodiment of the present invention. FIG. 37 is a schematic plan view showing a frame (300') with a cell sheet member (220) connected on an extension support member (310') according to another embodiment of the present invention.

[0207] Referring to FIGS. 36 and 37, the frame (300') [or, the extension support (310') may have a plurality of module areas (320': 320'-1 to 320'-4) along the first direction (horizontal) and the second direction (vertical). In this case, the frame (300') can be manufactured by sequentially connecting cell sheet portions (220) along the first direction and the second direction on the extension support (310').

[0208] For example, if the frame (300') has a plurality of module areas (320) in a first direction (X-axis) and a second direction (Y-axis), the length in the X-axis direction may be at least 1,700 mm and may have a length corresponding to a multiple of approximately 1,700 mm, and the length in the Y-axis direction may be at least 1,100 mm and may have a length corresponding to a multiple of approximately 1,100 mm.

[0209] Although the present invention has been illustrated and described with reference to preferred embodiments as described above, it is not limited to the above embodiments, and various modifications and changes can be made by those skilled in the art within the scope of the invention without departing from the spirit of the invention. Such modifications and changes should be deemed to fall within the scope of the present invention and the appended claims. Explanation of the symbols

[0210] 10: Connection between mask and frame 80: Suction Chuck 90: Moving plate 95: Temporary adhesive, dry film resist layer 100: Mask 110: Mask film, metal sheet 200: Frame 210: Border frame section 220: Cell Sheet Section 220': Metal sheet for manufacturing cell sheet parts 221: Border sheet section 223: 1st Grid Sheet Section 225: Second grid sheet section 300: Extended Frame 310: Extension support 311: Extended border 315: Support Grid Bar 1000: OLED pixel deposition device C: Cell, Mask Cell Ca, Cb, Cc: 1st, 2nd, and 3rd cell patterns CP: Cell pattern CR: Mask cell area CS: Outer border side of the cell sheet CS1, CS2: Cut edges of the cell sheet sections of the comparative examples Ma, Mb, Mc: 1st insulation part R: Hollow area of ​​the rim frame P: Mask pattern P1, P1-1, P1-2: First mask pattern P2, P2-1, P2-2: Second mask pattern

Claims

Claim 1 A frame used in a connection of an extended type mask and a frame for forming an OLED pixel, wherein the frame comprises an extended support portion and a plurality of cell sheet portions, wherein the extended support portion comprises an extended edge portion having a hollow region; and at least one support grid bar connected to the extended edge portion; wherein the plurality of cell sheet portions are connected on the extended support portion, and the extended support portion provides a plurality of module regions, wherein the plurality of module regions are formed along a first direction or a second direction perpendicular to the first direction, or along both the first direction and the second direction, and wherein each of the cell sheet portions is connected to each of the cell sheet portions so as to correspond to each of the module regions with mutual spacing. Claim 2 delete Claim 3 delete Claim 4 In claim 1, the frame is a frame having the dimensions of (1) or (2) below. (1) The length in the first direction is at least 1,700 mm, (2) The length in the second direction is at least 1,100 mm. Claim 5 A frame according to claim 1, wherein each of the cell sheet portions has a plurality of mask cell regions formed therein, and the side shape of the mask cell region and the side shape of the outer edge of the cell sheet portion include a curvature shape formed by isotropic etching. Claim 6 A frame according to claim 5, wherein the difference in average surface roughness between the side of the mask cell region and the side of the outer edge of the cell sheet portion is 10% or less. Claim 7 In paragraph 5, the outer edge side shape of the cell sheet portion is a frame that is different from the side shape of a comparative example in which at least a portion of the outer edge of the cell sheet portion is mechanically cut, physically cut, or laser cut. Claim 8 A frame according to claim 1, wherein the expansion frame portion is made of at least one of invar, super invar, nickel, and nickel-cobalt, and the expansion support portion and the cell sheet portion are made of the same material. Claim 9 A method for manufacturing a frame used in a connection of an extended type mask and a frame for forming an OLED pixel, comprising: (a) providing an extended edge portion having a hollow region; (b) connecting at least one support grid bar to the extended edge portion to provide an extended support portion including a plurality of module regions; (c) corresponding and connecting a cell sheet portion to each of the module regions; wherein, in step (b), the extended support portion provides a plurality of module regions, provided along a first direction or a second direction perpendicular to the first direction, or along both the first direction and the second direction, and in step (c), each of the cell sheet portions is connected to correspond to each of the module regions with mutual spacing. Claim 10 A method for manufacturing a frame according to claim 9, further comprising, prior to step (c), (1) a step of preparing the cell sheet portion; wherein step (1) comprises: (1-1) a step of adhering a first surface of a metal sheet to a moving plate; and (1-2) a step of manufacturing the cell sheet portion by forming a plurality of mask cell regions on a second surface opposite to the first surface of the metal sheet.

Citation Information

Patent Citations

  • Extended-type mask integrated frame and producing method thereof

    KR1020220145592A

  • Producing method of mask-support assembly

    KR1020240041217A