Method for preparing maleimide-based tetrapolymer and maleimide-based tetrapolymer prepared therefrom
A two-stage polymerization process with varying pressures and temperatures effectively addresses reflux and residual monomer issues in maleimide-based quaternary copolymer production, enhancing heat resistance and quality.
Patent Information
- Application Number
- KR1020240127926
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-09-23
AI Technical Summary
Existing methods for manufacturing maleimide-based quaternary copolymers face issues with reflux and scale formation in reactors, and high content of unreacted residual monomers, particularly when using monomers like acrylonitrile with low boiling points and fast polymerization rates.
A method involving a two-stage polymerization process under varying pressures and temperatures, starting with a first pressure and then increasing to a higher second pressure, along with a final stripping step, to minimize reflux and residual monomer content.
This approach reduces reflux and scale formation in the reactor while achieving high polymerization conversion rates and low oligomer content, resulting in a maleimide-based quaternary copolymer with excellent heat resistance and quality.
Abstract
Description
Technology Field
[0001] This specification relates to a method for manufacturing a maleimide-based quaternary copolymer and a maleimide-based quaternary copolymer manufactured therefrom. Background Technology
[0002] Maleimide copolymers are used as heat-resistant reinforcing materials for various resins because they exhibit high glass transition temperatures and excellent heat resistance due to the imide structure within the polymer chain. In particular, N-substituted maleimide monomers such as N-phenyl maleimide and N-cyclohexyl maleimide exhibit high heat resistance when copolymerized with other monomers; therefore, when these are mixed and used with diene-based graft copolymer resins such as ABS resin and ASA resin, they can exhibit high heat distortion temperatures and high heat resistance.
[0003] Maleimide-based quaternary copolymers are copolymers composed mainly of N-phenyl maleimide, styrene, α-methylstyrene, and acrylonitrile, and are known to have excellent compatibility with ABS resins and ASA resins compared to existing commercially available ternary copolymers of N-phenyl maleimide, styrene, and maleic anhydride or binary copolymers of N-phenyl maleimide and styrene.
[0004] Existing commercially available maleimide copolymer resins are manufactured primarily by bulk polymerization, solution polymerization, or reactive extrusion due to the limitations of technical issues and the material's characteristics, such as high viscosity and low melt flow index. However, manufacturing methods using such excessive solvents have the disadvantage of poor productivity and high manufacturing costs because they require complex production processes, such as recovering the solvent through a separate devolatilizer.
[0005] Meanwhile, the polymerization method utilizing suspension polymerization has the advantage of not requiring a complex production process including solvent recovery, and once polymerization is complete, the resin dispersed in the suspension can be immediately produced into a product through simple processing.
[0006] However, suspension polymerization is characterized by being significantly affected by physicochemical properties, including differences in the solubility of each monomer, and differences in the polymerization reaction rates of the monomers. Specifically, when monomers such as acrylonitrile, which have a low boiling point of 77°C and a high solubility in water of 7% at room temperature, are used as raw materials for copolymerization, there is a problem that can cause reflux and scale formation inside the reactor. In addition, when manufacturing maleimide-based quaternary copolymers, the polymerization reaction rate of N-substituted maleimide monomers is very fast compared to other monomers, so after the polymerization process, a large number of monomers other than N-substituted maleimide monomers remain as unreacted monomers, which has the disadvantage of making it difficult to manage RTVM (Residual total volatile matter).
[0007] Therefore, in the method for manufacturing maleimide-based quaternary copolymers by suspension polymerization, there is a need to develop a polymerization method that minimizes reflux and scale formation inside the reactor compared to conventional methods, while simultaneously minimizing the content of unreacted residual monomers. The problem to be solved
[0008] The details of this specification are intended to solve the problems of the aforementioned prior art, and one objective of this specification is to provide a method for manufacturing a maleimide-based quaternary copolymer that minimizes reflux and scale formation inside the reactor compared to the prior art, while simultaneously minimizing the content of unreacted residual monomers present in the final product.
[0009] Another objective of the present specification is to provide a maleimide-based quaternary copolymer with a high glass transition temperature and low oligomer content, which has excellent heat resistance and quality. means of solving the problem
[0010] According to one aspect, a method for producing a maleimide-based quaternary copolymer is provided, comprising: (a) introducing a monomer mixture comprising an N-substituted maleimide monomer, a styrene monomer, an α-alkylstyrene monomer, and a vinyl cyanide monomer into a reactor to prepare a suspension; and (b) polymerizing the suspension; wherein step (b) comprises: (b1) polymerizing the suspension under a first pressure; and (b2) polymerizing the product of step (b1) under a second pressure; wherein the second pressure is higher than the first pressure.
[0011] In one embodiment, the N-substituted maleimide monomer may be one selected from the group consisting of N-phenyl maleimide, N-methyl maleimide, N-ethyl maleimide, N-propyl maleimide, N-isopropyl maleimide, N-butyl maleimide, N-isobutyl maleimide, Nt-butyl maleimide, N-cyclohexyl maleimide, N-chlorophenyl maleimide, N-methylphenyl maleimide, N-bromophenyl maleimide, N-naphthyl maleimide, N-lauryl maleimide, N-hydroxyphenyl maleimide, N-methoxyphenyl maleimide, N-carboxyphenyl maleimide, N-nitrophenyl maleimide, N-benzyl maleimide, and combinations of two or more of these.
[0012] In one embodiment, the styrene monomer may be one selected from the group consisting of styrene, t-butylstyrene, halogen-substituted styrene, 1,3-dimethylstyrene, 2,4-dimethylstyrene, ethylstyrene, and combinations of two or more of these.
[0013] In one embodiment, the α-alkylstyrene monomer may be one selected from the group consisting of α-methylstyrene, α-ethylstyrene, methyl α-methylstyrene, and combinations of two or more of these.
[0014] In one embodiment, the vinyl cyanide monomer may be one selected from the group consisting of acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, α-chloroacrylonitrile, and combinations of two or more of these.
[0015] In one embodiment, the monomer mixture may comprise 30 to 50 weight% of an N-substituted maleimide monomer, 1 to 40 weight% of a styrene monomer, 10 to 40 weight% of an α-alkylstyrene monomer, and 10 to 30 weight% of a vinyl cyanide monomer.
[0016] In one embodiment, the step (a) may include: (a1) introducing a monomer mixture comprising an N-substituted maleimide monomer, a styrene monomer, an α-alkylstyrene monomer, and a vinyl cyanide monomer into a reactor; and (a2) introducing a mixture comprising a polymerization initiator, a molecular weight regulator, an inert medium, and a dispersant into the reactor to prepare a suspension.
[0017] In one embodiment, the polymerization conversion rate of the product of step (b1) may be 80 to 90%.
[0018] In one embodiment, the step (b2) may include applying a pressure of 3.0 to 6.0 bar to the product of the step (b1).
[0019] In one embodiment, the polymerization of step (b1) is performed at a first temperature, and the polymerization of step (b2) is performed at a second temperature, and the second temperature may be higher than the first temperature.
[0020] In one embodiment, the step (b) further comprises (b3) a step of polymerizing the product of the step (b2) under a third pressure; wherein the third pressure may be higher than the second pressure.
[0021] In one embodiment, the polymerization of step (b2) is performed at a second temperature, and the polymerization of step (b3) is performed at a third temperature, and the third temperature may be higher than the second temperature.
[0022] In one embodiment, the method for manufacturing the maleimide-based quaternary copolymer may further include (c) a step of stripping the product of step (b).
[0023] According to another aspect, a maleimide-based quaternary copolymer prepared by the above method is provided.
[0024] In one embodiment, the weight-average molecular weight of the maleimide-based quaternary copolymer may be 100,000 to 250,000 g / mol.
[0025] In one embodiment, the glass transition temperature of the maleimide-based quaternary copolymer may be 170 to 190 ℃. Effects of the invention
[0026] A method for producing a maleimide-based quaternary copolymer according to one aspect of the present specification can minimize reflux and scale formation inside the reactor compared to conventional methods, while simultaneously minimizing the content of unreacted residual monomers present in the final product and exhibiting a high polymerization conversion rate.
[0027] In addition, a maleimide-based quaternary copolymer according to another aspect of this specification has a high glass transition temperature and a low oligomer content, which has excellent heat resistance and quality, and can be applied to the manufacture of high heat-resistant resins with a high heat distortion temperature.
[0028] The effects of one aspect of this specification are not limited to the effects described above, and should be understood to include all effects that can be inferred from the configurations described in the detailed description or claims of this specification. Specific details for implementing the invention
[0029] Hereinafter, one aspect of this specification will be described based on specific examples. However, the details described in this specification may be implemented in various different forms and are therefore not limited to the embodiments described herein.
[0030] Throughout the specification, when a part is described as "including" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but rather allows for the inclusion of additional components.
[0031] When a range of numerical values is described in this specification, unless a specific range is otherwise described, the value has the precision of significant figures provided according to the standard rules in chemistry for significant figures. For example, 10 includes a range of 5.0 to 14.9, and the number 10.0 includes a range of 9.50 to 10.49.
[0032] Terms including ordinal numbers, such as ‘first’ or ‘second’ as used in this specification, may be used to describe various components or steps, but such components or steps should not be limited by ordinal numbers. Terms including ordinal numbers should be interpreted solely for the purpose of distinguishing one component or step from other components or steps.
[0033] Method for manufacturing a maleimide-based quaternary copolymer
[0034] A method for preparing a maleimide-based quaternary copolymer according to one aspect of the present specification comprises: (a) a step of preparing a suspension by introducing a monomer mixture comprising an N-substituted maleimide monomer, a styrene monomer, an α-alkylstyrene monomer, and a vinyl cyanide monomer into a reactor; and (b) a step of polymerizing the suspension; wherein step (b) comprises: (b1) a step of polymerizing the suspension under a first pressure; and (b2) a step of polymerizing the product of step (b1) under a second pressure; wherein the second pressure is higher than the first pressure.
[0035] The above method for manufacturing a maleimide-based quaternary copolymer can minimize reflux and scale formation inside the reactor compared to conventional methods by additionally performing the polymerization of step (b2) at a higher pressure after the polymerization of step (b1), while simultaneously minimizing the content of unreacted residual monomers present in the final product and exhibiting a high final polymerization conversion rate.
[0036] The above N-substituted maleimide monomer may be one selected from the group consisting of N-phenyl maleimide, N-methyl maleimide, N-ethyl maleimide, N-propyl maleimide, N-isopropyl maleimide, N-butyl maleimide, N-isobutyl maleimide, Nt-butyl maleimide, N-cyclohexyl maleimide, N-chlorophenyl maleimide, N-methylphenyl maleimide, N-bromophenyl maleimide, N-naphthyl maleimide, N-lauryl maleimide, N-hydroxyphenyl maleimide, N-methoxyphenyl maleimide, N-carboxyphenyl maleimide, N-nitrophenyl maleimide, N-benzyl maleimide, and combinations of two or more of these, but is not limited thereto.
[0037] The above styrene monomer may be one selected from the group consisting of styrene, t-butylstyrene, halogen-substituted styrene, 1,3-dimethylstyrene, 2,4-dimethylstyrene, ethylstyrene, and combinations of two or more of these, but is not limited thereto.
[0038] The above α-alkylstyrene monomer may be one selected from the group consisting of α-methylstyrene, α-ethylstyrene, methyl α-methylstyrene, and combinations of two or more of these, but is not limited thereto.
[0039] The vinyl cyanide monomer mentioned above may be one selected from the group consisting of acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, α-chloroacrylonitrile, and combinations of two or more of these, but is not limited thereto.
[0040] The above monomer mixture may comprise 30 to 50 weight% of an N-substituted maleimide monomer, 1 to 40 weight% of a styrene monomer, 10 to 40 weight% of an α-alkylstyrene monomer, and 10 to 30 weight% of a vinyl cyanide monomer.
[0041] The content of the N-substituted maleimide monomer may be 30 to 50 wt% based on the total weight of the monomer mixture. For example, it may be 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, 50 wt%, or a range between two of these values. If the content of the N-substituted maleimide monomer is below the above range, the heat resistance of the copolymer may be reduced, and if it exceeds the above range, the polymerization rate increases, which may cause the weight-average molecular weight of the copolymer to decrease excessively or the content of unreacted residual monomer present in the final product to increase.
[0042] The content of the above styrene-based monomer may be 1 to 40 weight percent based on the total weight of the monomer mixture. For example, it may be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, or a range between two of these values. If the content of the styrene-based monomer is below the above range, the final polymerization conversion rate may decrease, and the polymerization rate may decrease, which may increase the weight-average molecular weight of the copolymer. If the content of the styrene-based monomer exceeds the above range, the heat resistance of the copolymer may decrease.
[0043] The content of the α-alkylstyrene monomer may be 10 to 40 wt% based on the total weight of the monomer mixture. For example, it may be 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, or a range between two of these values. If the content of the α-alkylstyrene monomer is below the above range, the polymerization rate may increase, the weight-average molecular weight of the copolymer may increase excessively, or it may become difficult to control the reaction temperature, and the glass transition temperature and heat resistance of the copolymer may decrease. If the content of the α-alkylstyrene monomer exceeds the above range, the polymerization rate decreases, the weight-average molecular weight of the copolymer decreases, the reaction time increases, and the final polymerization conversion rate may decrease.
[0044] The content of the vinyl cyanide-based monomer may be 10 to 30 wt% based on the total weight of the monomer mixture. For example, it may be 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, or a range between two of these values. If the content of the vinyl cyanide-based monomer exceeds the above range, the content of unreacted residual monomer present in the final product may increase excessively.
[0045] The above suspension may further include one selected from the group consisting of a polymerization initiator, a molecular weight regulator, an inert medium, a dispersant, and a combination of two or more of these.
[0046] The above step (a) may include: (a1) introducing a monomer mixture comprising an N-substituted maleimide monomer, a styrene monomer, an α-alkylstyrene monomer, and a vinyl cyanide monomer into a reactor; and (a2) introducing a mixture comprising a polymerization initiator, a molecular weight regulator, an inert medium, and a dispersant into the reactor to prepare a suspension.
[0047] The above polymerization initiator is azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanopentoic acid), 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(1-cyclohexanecarbonitrile), benzoyl peroxide, t-butylperoxybenzoate, t-butylhydroperoxide, 1,1,3,3-tetramethylbutylhydroperoxide, succinic acid peroxide, peroxymaleic acid t-butyl ester, cumene hydroperoxide, lauroyl peroxide, isopropyl-t-butylperoxycarbonate, butyl perbenzoate, 1,1-bis(alkylperoxy)3,3,5-trimethylcyclohexane, It may be one selected from the group consisting of 1,1-bis(t-butylperoxy)cyclohexane and combinations of two or more of these, but is not limited thereto.
[0048] The content of the polymerization initiator may be 0.01 to 1 part by weight based on 100 parts by weight of the monomer mixture. For example, it may be 0.01 parts by weight, 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, 0.05 parts by weight, 0.06 parts by weight, 0.07 parts by weight, 0.08 parts by weight, 0.09 parts by weight, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or a range between two of these values. If the content of the polymerization initiator is below the above range, the final polymerization conversion rate may decrease, and if it exceeds the above range, the physical properties of the copolymer may decrease due to residual initiator.
[0049] The above molecular weight regulator may be one selected from the group consisting of t-dodecyl mercaptan, t-butyl mercaptan, n-dodecyl mercaptan, n-amyl mercaptan, n-hexyl mercaptan, n-octyl mercaptan, n-nonyl mercaptan, and combinations of two or more of these, but is not limited thereto.
[0050] The content of the molecular weight regulator may be 0.01 to 1 part by weight based on 100 parts by weight of the monomer mixture. For example, it may be 0.01 parts by weight, 0.02 parts by weight, 0.03 parts by weight, 0.04 parts by weight, 0.05 parts by weight, 0.06 parts by weight, 0.07 parts by weight, 0.08 parts by weight, 0.09 parts by weight, 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, or a range between two of these values.
[0051] A mixture containing the above-mentioned inert medium and dispersant can form a dispersion system.
[0052] The above-mentioned inert medium may be an aqueous liquid, such as water, for example, ion-exchanged water, but is not limited thereto.
[0053] The content of the above inert medium may be 100 to 200 parts by weight based on 100 parts by weight of the monomer mixture. For example, it may be 100 parts by weight, 110 parts by weight, 120 parts by weight, 130 parts by weight, 140 parts by weight, 150 parts by weight, 160 parts by weight, 170 parts by weight, 180 parts by weight, 190 parts by weight, 200 parts by weight, or a range between two of these values.
[0054] The above dispersant may include a phosphate-based inorganic salt.
[0055] The above-mentioned dispersant may be one selected from the group consisting of tricalcium phosphate, dicalcium phosphate, calcium phosphate, trisodium phosphate, disodium phosphate, sodium phosphate, calcium carbonate, ammonium persulfate, and combinations of two or more of these, but is not limited thereto.
[0056] The content of the dispersant may be 0.1 to 10 parts by weight based on 100 parts by weight of the monomer mixture. For example, it may be 0.1 parts by weight, 0.5 parts by weight, 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, or a range between two of these values.
[0057] Step (b) above can be performed using a conventional suspension polymerization method. The method for manufacturing the maleimide-based quaternary copolymer using suspension polymerization can achieve a high final polymerization conversion rate despite a lower polymerization temperature compared to manufacturing through conventional bulk polymerization or solution polymerization methods, allows for free control of the weight-average molecular weight of the copolymer, and is easy to manufacture as it does not involve complex production processes including separate solvent recovery.
[0058] The polymerization conversion rate of the product in step (b1) above may be 80 to 90%. For example, it may be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, or a range between two of these values. If the polymerization conversion rate of the product in step (b1) above is below the above range, the energy efficiency of the polymerization process and the final polymerization conversion rate may decrease, and if it exceeds the above range, the oligomer content of the final product may increase.
[0059] The above step (b2) may include a step of applying pressure to the product of the above step (b1). For example, the above step (b2) may include a step of injecting nitrogen into the reactor. The method for manufacturing the above maleimide-based quaternary copolymer can achieve a high level of reaction conversion rate by performing a multi-stage polymerization reaction including a pressurization process.
[0060] The conventional method for manufacturing maleimide-based quaternary copolymers using suspension polymerization had problems such as causing reflux and scale formation inside the reactor because monomers like acrylonitrile, which have a low boiling point of 77°C and a high solubility in water of 7% at room temperature, were used as raw materials for copolymerization. Additionally, because the polymerization reaction rate of N-substituted maleimide monomers was very fast compared to other monomers, there was a problem where a large amount of unreacted monomers of the remaining monomers remained in the polymer after the polymerization process.
[0061] The method for manufacturing the above maleimide-based quaternary copolymer involves performing a pressurization process after the polymerization of step (b1), so that even if the subsequent polymerization step is performed at a reaction temperature above the boiling point of acrylonitrile, the acrylonitrile does not vaporize, thereby minimizing the reflux or scale formation of acrylonitrile in the reactor. In addition, the unreacted acrylonitrile phase exists as a liquid, thereby inducing copolymerization with unreacted radical sites of the maleimide-based quaternary copolymer, which can minimize the content of unreacted residual monomers present in the final product.
[0062] The above step (b2) may include a step of applying a pressure of 3.0 to 6.0 bar to the product of the above step (b1). For example, it may include a step of applying a pressure of 3.0 bar, 3.5 bar, 4.0 bar, 4.5 bar, 5.0 bar, 5.5 bar, 6.0 bar, or a range between two of these values to the product of the above step (b1). If the magnitude of the pressure applied to the product of the above step (b1) is less than the above range, the final polymerization conversion rate may decrease, and the residual monomer content and oligomer content of the final product may increase. If the magnitude of the pressure applied to the product of the above step (b1) exceeds the above range, subsequent polymerization may become difficult due to destabilization of the system.
[0063] The above step (b2) may include (b2-1) a step of applying a pressure of 3.0 to 6.0 bar to the product of the above step (b1); and (b2-2) a step of polymerizing under a second pressure.
[0064] The above step (b2-1) may be performed by injecting nitrogen into the reactor, but is not limited thereto.
[0065] The polymerization of step (b1) above is performed at a first temperature, and the polymerization of step (b2) above is performed at a second temperature, and the second temperature may be higher than the first temperature.
[0066] The first temperature above may be 50 to 80 ℃. For example, it may be 50 ℃, 51 ℃, 52 ℃, 53 ℃, 54 ℃, 55 ℃, 56 ℃, 57 ℃, 58 ℃, 59 ℃, 60 ℃, 61 ℃, 62 ℃, 63 ℃, 64 ℃, 65 ℃, 66 ℃, 67 ℃, 68 ℃, 69 ℃, 70 ℃, 71 ℃, 72 ℃, 73 ℃, 74 ℃, 75 ℃, 76 ℃, 77 ℃, 78 ℃, 79 ℃, 80 ℃, or a range between two of these values. If the first temperature is below the above range, the polymerization rate and polymerization conversion rate may decrease. If the first temperature exceeds the above range, the oligomer content in the product increases excessively, which may lower the glass transition temperature and gloss of the copolymer, and when combined with diene-based graft copolymer resins such as ABS resin and ASA resin, the kneading properties and heat resistance may be reduced.
[0067] Acrylonitrile, a type of vinyl cyanide monomer, has a low boiling point of about 77°C. If polymerization is carried out at a temperature higher than this, acrylonitrile vapor may be generated, which can increase the pressure inside the polymerization reactor and produce polyacrylonitrile through the condensation of acrylonitrile gas and homopolymerization. The formation of scale containing polyacrylonitrile can increase the cleaning cycle of the polymerization reactor and degrade the physical properties of the polymer.
[0068] The polymerization of step (b1) above may be performed for 2 to 6 hours. For example, it may be performed for 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, or for a time between two of these values.
[0069] The second temperature may be 70 to 100 ℃. For example, it may be 70 ℃, 75 ℃, 80 ℃, 85 ℃, 90 ℃, 95 ℃, 100 ℃, or a range between two of these values. If the second temperature is below the above range, the polymerization conversion rate may decrease, and if it exceeds the above range, the oligomer content in the product may increase, and the glass transition temperature may decrease.
[0070] The polymerization of step (b2) above may be performed for 1 to 4 hours. For example, it may be performed for 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, or for a time between two of these values.
[0071] The above step (b) further comprises (b3) a step of polymerizing the product of the above step (b2) under a third pressure; wherein the third pressure may be higher than the second pressure.
[0072] The polymerization of step (b2) above is performed at a second temperature, and the polymerization of step (b3) above is performed at a third temperature, and the third temperature may be higher than the second temperature.
[0073] The third temperature may be 100 to 150 ℃. For example, it may be 100 ℃, 105 ℃, 110 ℃, 115 ℃, 120 ℃, 125 ℃, 130 ℃, 135 ℃, 140 ℃, 145 ℃, 150 ℃, or a range between two of these values. If the third temperature is below the above range, the final polymerization conversion rate may be reduced, and if it exceeds the above range, the glass transition temperature of the copolymer may be reduced.
[0074] The polymerization of step (b3) above may be performed for 1 to 4 hours. For example, it may be performed for 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, or for a time between two of these values.
[0075] The polymerization in step (b) above can be performed while stirring at 100 to 600 rpm.
[0076] The polymerization of step (b) above may be performed for a total of 4 to 12 hours. For example, it may be performed for 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, or for a time between two of these values.
[0077] The polymerization conversion rate of the product in step (b) above may be 98% or more or 99% or more. If the polymerization conversion rate of the product in step (b) is below the above range, a large amount of gas may be generated when compounded with diene-based graft copolymer resins such as ABS resin and ASA resin due to the high residual monomer content in the product, the composition may be carbonized during resin extrusion due to a rapid decrease in thermal stability, and the heat distortion temperature of the heat-resistant resin composition may be lowered.
[0078] The above method for manufacturing the maleimide-based quaternary copolymer is by suspension polymerization, and unlike the conventional methods for manufacturing maleimide-based copolymers, such as bulk polymerization and solution polymerization, it does not undergo a devolatilization process by vacuum and high temperature. That is, suspension polymerization is a polymerization method in which the polymer product is obtained as is after dehydration and drying, and since the manufactured polymer product itself is the finished product, the content of residual monomer in the product must be very low, and it is required to achieve a high polymerization conversion rate compared to other polymerization methods.
[0079] The oligomer content of the product of step (b) above may be 3 mol% or less. For example, it may be 3 mol% or less, 2.9 mol% or less, 2.8 mol% or less, 2.7 mol% or less, 2.6 mol% or less, 25 mol% or less, 2.4 mol% or less, 2.3 mol% or less, 22 mol% or less, 2.1 mol% or less, or 2.0 mol% or less. Oligomers, which are one of the factors that impair the physical properties of a polymer, are mainly generated when monomers initiated by heat fail to grow sufficiently into polymers with high molecular weights. If the oligomer content of the product of step (b) exceeds the above range, the glass transition temperature and gloss of the quaternary copolymer may decrease, and the kneading ability may decrease when compounded with diene-based graft copolymer resins such as ABS resin and ASA resin. The oligomer content may be measured using a gel permeation chromatography (GPC) instrument.
[0080] The method for manufacturing the above maleimide-based quaternary copolymer may further include (c) a step of stripping the product of step (b). By performing the stripping process of step (c), the residual monomer content present in the final product can be further reduced in a simple manner, thereby achieving a high yield.
[0081] The above method for manufacturing a maleimide-based quaternary copolymer may further include one or more of the steps of removing a dispersant; and separating solids and liquids, dehydrating, and drying.
[0082] The weight-average molecular weight of the maleimide-based quaternary copolymer prepared by the above method for preparing the maleimide-based quaternary copolymer may be 100,000 to 250,000 g / mol.
[0083] The glass transition temperature of the maleimide-based quaternary copolymer prepared by the above method for preparing the maleimide-based quaternary copolymer may be 170 to 190 ℃.
[0084] Maleimide-based quaternary copolymer
[0085] A maleimide-based quaternary copolymer according to another aspect of this specification may be manufactured by the method for manufacturing the maleimide-based quaternary copolymer described above.
[0086] The above maleimide-based quaternary copolymer has a high glass transition temperature and a low oligomer content, resulting in excellent heat resistance and quality. It also has excellent compatibility with other resins, so it can be applied to the manufacture of high-heat resistant resins with high heat distortion temperatures. In particular, it can be applied to products in various fields requiring a high level of heat resistance through formulation with diene-based graft copolymer resins such as ABS resin and ASA resin.
[0087] The weight-average molecular weight of the above maleimide-based quaternary copolymer may be 100,000 to 250,000 g / mol. For example, it may be 100,000 g / mol, 110,000 g / mol, 120,000 g / mol, 130,000 g / mol, 140,000 g / mol, 150,000 g / mol, 160,000 g / mol, 170,000 g / mol, 180,000 g / mol, 190,000 g / mol, 200,000 g / mol, 210,000 g / mol, 220,000 g / mol, 230,000 g / mol, 240,000 g / mol, 250,000 g / mol, or a range between two of these values.
[0088] The glass transition temperature of the above maleimide-based quaternary copolymer may be 170 to 190 ℃. For example, it may be 170 ℃, 171 ℃, 172 ℃, 173 ℃, 174 ℃, 175 ℃, 176 ℃, 177 ℃, 178 ℃, 179 ℃, 180 ℃, 181 ℃, 182 ℃, 183 ℃, 184 ℃, 185 ℃, 186 ℃, 187 ℃, 188 ℃, 189 ℃, 190 ℃, or a range between two of these values.
[0089] The embodiments of this specification will be described in more detail below. However, the following experimental results represent only representative results among the above embodiments, and the scope and content of this specification should not be interpreted as being narrowed or limited by the embodiments. The respective effects of various embodiments of this specification not explicitly presented below will be described in detail in the relevant sections.
[0090] Example 1
[0091] 100 parts by weight of a monomer mixture comprising 38% by weight of N-phenyl maleimide monomer, 30% by weight of α-methylstyrene monomer, 16% by weight of styrene monomer, and 16% by weight of acrylonitrile monomer was added to a stirred reactor with a reactor capacity of 100 L, and an organic mixture comprising an initiator comprising 0.10 parts by weight of azobisisobutyronitrile, 0.12 parts by weight of benzoyl peroxide, and 0.15 parts by weight of t-butylperoxybenzoate, and 0.35 parts by weight of t-dodecylmercaptan, a molecular weight regulator, was further added and heated, mixed, and homogenized at a temperature of 35 to 45 ℃. After that, a dispersion system composed of ion-exchange water and as a dispersant tricalcium phosphate, trisodium phosphate, calcium carbonate, and ammonium persulfate was heated and mixed at a temperature of 35 to 50 ℃ and introduced into the reactor to prepare a suspension.
[0092] The first stage of polymerization was carried out for 4 hours while maintaining the suspension in the reactor at a stirring speed of 180 rpm and a temperature of 65 ℃.
[0093] After the first stage of polymerization was completed, nitrogen was injected into the reactor to apply a pressure of 5 bar. Subsequently, the polymerization temperature was raised to 90 ℃ over 30 minutes, and then the second stage of polymerization was carried out for 2 hours.
[0094] After that, the polymerization temperature was raised to 125 ℃ for 1 hour, and then a three-stage polymerization was carried out for 3 hours to complete the polymerization.
[0095] After the polymerization was completed, the slurry was cooled to 94 to 96 °C and stripped of residual monomers for 2 hours. Subsequently, hydrochloric acid was added to adjust the pH to 2.0 to remove residual dispersant, and then a quaternary copolymer was obtained through solid-liquid separation by centrifugation, dehydration, and drying in a fluidized bed dryer.
[0096] Example 2
[0097] A quaternary copolymer was prepared in the same manner as in Example 1, except that after the first stage of polymerization was completed, nitrogen was injected into the reactor and a pressure of 6 bar was applied.
[0098] Example 3
[0099] A quaternary copolymer was prepared in the same manner as in Example 1, except that after the first stage of polymerization was completed, nitrogen was injected into the reactor and a pressure of 3 bar was applied.
[0100] Comparative Example 1
[0101] After the first stage of polymerization was completed, a quaternary copolymer was prepared in the same manner as in Example 1, except that no pressure was applied.
[0102] Comparative Example 2
[0103] A quaternary copolymer was prepared in the same manner as in Example 1, except that after the first stage of polymerization was completed, nitrogen was injected into the reactor and a pressure of 1 bar was applied.
[0104] Comparative Example 3
[0105] A quaternary copolymer was prepared in the same manner as in Example 1, except that after the first stage of polymerization was completed, nitrogen was injected into the reactor and a pressure of 2 bar was applied.
[0106] Experimental Example 1
[0107] In the above Examples 1 to 3 and Comparative Examples 1 to 3, the residual monomer content and polymerization conversion rate were measured at the end of the first stage of polymerization, at the end of the third stage of polymerization, and after stripping.
[0108] Residual monomer content and polymerization conversion rate were measured using a gas chromatograph (GC, GC2010, Shimadzu). An HP FFAP 0.530 mm * 1 μm, 30 m column was used; the temperature was maintained isothermally at an initial temperature of 35 ℃ for 5 minutes, followed by a heating rate of 5 ℃ / min, and a flame ionization detector maintained at 240 ℃ was used. The gases used for analysis were He, H2, and Air, of high purity grade with a purity of 99.9999% or higher. After sufficiently removing moisture from the polymer, samples were prepared by dissolving the polymer in DMF or THF along with normal butanol as a standard substance, and the conversion rate was measured through residual monomer content analysis.
[0109] Experimental Example 1-1
[0110] In Example 1 above, the residual monomer content and polymerization conversion rate at the end of the first stage of polymerization were measured and are shown in Table 1 below.
[0111] division Polymerization conversion rate (%) Residual styrene monomer content (ppm) Residual α-methylstyrene monomer content (ppm) Residual acrylonitrile monomer content (ppm) Total residual monomer content (ppm) Step 1 polymerization 84.7 83205 39730 30469 153404
[0112] Experimental Example 1-2
[0113] In the above Examples 1 to 3 and Comparative Examples 1 to 3, the residual monomer content and polymerization conversion rate at the end of the three-step polymerization were measured and are shown in Table 2 below.
[0114] division Polymerization conversion rate (%) Residual styrene monomer content (ppm) Residual α-methylstyrene monomer content (ppm) Residual acrylonitrile monomer content (ppm) Total residual monomer content (ppm) Example 1 99.3 ND ND 7075 7075 Example 2 99.3 ND ND 6900 6900 Example 3 98.1 3248 6548 9058 18854 Comparative Example 1 96.8 3638 10970 17645 32253 Comparative Example 2 96.7 4598 10268 17898 32764 Comparative Example 3 97.0 5428 9987 14268 29683
[0115] Referring to Table 2 above, it was confirmed that Examples 1 to 3, in which a pressure of 3 to 6 bar was applied after the completion of the first stage of polymerization, had a higher polymerization conversion rate at the end of the third stage of polymerization and a lower residual monomer content of all monomers compared to Comparative Example 1, in which no pressurization process was performed, and Comparative Examples 2 and 3, in which a pressure of 1 to 2 bar was applied. In particular, Examples 1 and 2, in which a pressure of 5 to 6 bar was applied after the completion of the first stage of polymerization, showed a high polymerization conversion rate of over 99%, and at the same time, it was confirmed that the residual monomer content of styrene and α-methylstyrene was below the detection limit and was not detected (Not Detected; ND).
[0116] Experimental Example 1-3
[0117] In the above Examples 1 to 3 and Comparative Examples 1 to 3, the residual monomer content after stripping was measured and is shown in Table 3 below.
[0118] division Residual styrene monomer content (ppm) Residual α-methylstyrene monomer content (ppm) Residual acrylonitrile monomer content (ppm) Total residual monomer content (ppm) Example 1 ND ND 4939 4939 Example 2 ND ND 4688 4688 Example 3 3228 6434 8055 17717 Comparative Example 1 3528 10076 15658 29262 Comparative Example 2 4548 10058 15558 30164 Comparative Example 3 5420 9922 13255 28597
[0119] Referring to Tables 2 and 3 above, it was confirmed that the residual monomer content of all monomers was reduced after the stripping process. In particular, it was confirmed that the final residual monomer content of all monomers in Examples 1 to 3, in which a pressure of 3 to 6 bar was applied after the completion of the first stage polymerization, was significantly lower compared to Comparative Example 1, in which no pressurization process was performed, and Comparative Examples 2 and 3, in which a pressure of 1 to 2 bar was applied.
[0120] Experimental Example 2
[0121] The glass transition temperature, weight-average molecular weight, and oligomer content of the quaternary copolymers prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were measured and are shown in Table 4 below.
[0122] (1) Glass transition temperature (°C): It was measured using a differential scanning calorimeter (DSC, DSC200 F3 Maia, NETZSCH). After adding 10 mg of the polymer to an aluminum dish and preparing the sample using an aluminum pierced lid, the temperature was raised to 275°C at a rate of 20°C / min, then cooled to 50°C at a rate of 20°C / min and kept constant for 5 minutes. Afterward, the temperature was raised to 275°C at a rate of 10°C / min, and the glass transition temperature was measured through the change in heat quantity analyzed during the second raising.
[0123] (2) Weight-average molecular weight (g / mol): Measured using a gel permeation chromatography (GPC, HLC-8320GPC, TOSOH) instrument. The sample was prepared by dissolving the polymer in THF at a concentration of 1 mg / mL, and then measured under constant temperature conditions of 40 ℃.
[0124] (3) Oligomer content (mol%): Measured using a gel permeation chromatography (GPC, HLC-8320GPC, TOSOH) instrument. Samples were prepared by dissolving the polymer in THF at a concentration of 1 mg / mL, and then measured under constant temperature conditions of 40 ℃.
[0125] division Glass transition temperature (°C) Weight-average molecular weight (g / mol) Oligomer content (mol%) Example 1 176.4 149000 2.2 Example 2 177.4 147000 2.0 Example 3 178.8 155000 2.4 Comparative Example 1 182.5 170000 3.2 Comparative Example 2 181.4 165000 2.8 Comparative Example 3 180.2 160000 2.5
[0126] Referring to Table 4 above, it was confirmed that the quaternary copolymers prepared in Examples 1 to 3 have excellent quality due to their low oligomer content, and at the same time exhibit excellent heat resistance characteristics due to their high glass transition temperature.
[0127] The foregoing description of this specification is for illustrative purposes only, and those skilled in the art to which one aspect of this specification pertains will understand that other specific forms can be easily modified without altering the technical concept or essential features described in this specification. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0128] The scope of this specification is defined by the claims set forth below, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of this specification.
Claims
Claim 1 (a) a step of preparing a suspension by introducing a monomer mixture comprising 30-50 wt% of an N-substituted maleimide monomer, 1-40 wt% of a styrene monomer, 10-40 wt% of an α-alkylstyrene monomer, and 10-30 wt% of a vinyl cyanide monomer into a reactor; and (b) a step of polymerizing the suspension; wherein step (b) comprises: (b1) a step of polymerizing the suspension at a first temperature under a first pressure; and (b2) a step of polymerizing the product of step (b1) at a second temperature under a second pressure by applying a pressure of 3.0-6.0 bar. and (b3) a step of polymerizing the product of step (b2) at a third temperature under a third pressure; wherein the second pressure is higher than the first pressure, the third pressure is higher than the second pressure, the second temperature is higher than the first temperature, and the third temperature is higher than the second temperature, a method for producing a maleimide-based quaternary copolymer. Claim 2 A method for preparing a maleimide-based quaternary copolymer according to claim 1, wherein the N-substituted maleimide monomer is one selected from the group consisting of N-phenyl maleimide, N-methyl maleimide, N-ethyl maleimide, N-propyl maleimide, N-isopropyl maleimide, N-butyl maleimide, N-isobutyl maleimide, Nt-butyl maleimide, N-cyclohexyl maleimide, N-chlorophenyl maleimide, N-methylphenyl maleimide, N-bromophenyl maleimide, N-naphthyl maleimide, N-lauryl maleimide, N-hydroxyphenyl maleimide, N-methoxyphenyl maleimide, N-carboxyphenyl maleimide, N-nitrophenyl maleimide, N-benzyl maleimide, and combinations of two or more of these. Claim 3 A method for preparing a maleimide-based quaternary copolymer according to claim 1, wherein the styrene-based monomer is one selected from the group consisting of styrene, t-butylstyrene, halogen-substituted styrene, 1,3-dimethylstyrene, 2,4-dimethylstyrene, ethylstyrene, and combinations of two or more of these. Claim 4 A method for preparing a maleimide-based quaternary copolymer according to claim 1, wherein the α-alkylstyrene monomer is one selected from the group consisting of α-methylstyrene, α-ethylstyrene, methyl α-methylstyrene, and combinations of two or more of these. Claim 5 A method for preparing a maleimide-based quaternary copolymer according to claim 1, wherein the vinyl cyanide-based monomer is one selected from the group consisting of acrylonitrile, methacrylonitrile, ethacrylonitrile, phenylacrylonitrile, α-chloroacrylonitrile, and combinations of two or more of these. Claim 6 delete Claim 7 A method for producing a maleimide-based quaternary copolymer according to claim 1, wherein step (a) comprises: (a1) introducing a monomer mixture comprising 30 to 50 wt% of an N-substituted maleimide monomer, 1 to 40 wt% of a styrene monomer, 10 to 40 wt% of an α-alkylstyrene monomer, and 10 to 30 wt% of a vinyl cyanide monomer into a reactor; and (a2) introducing a mixture comprising a polymerization initiator, a molecular weight regulator, an inert medium, and a dispersant into the reactor to produce a suspension. Claim 8 A method for producing a maleimide-based quaternary copolymer according to claim 1, wherein the polymerization conversion rate of the product of step (b1) is 80 to 90%. Claim 9 delete Claim 10 delete Claim 11 delete Claim 12 delete Claim 13 A method for manufacturing a maleimide-based quaternary copolymer, comprising, in claim 1, (c) a step of stripping the product of step (b). Claim 14 A maleimide-based quaternary copolymer produced by the method of claim 1. Claim 15 A maleimide-based quaternary copolymer according to claim 14, wherein the weight-average molecular weight of the maleimide-based quaternary copolymer is 100,000 to 250,000 g / mol. Claim 16 A maleimide-based quaternary copolymer according to claim 14, wherein the glass transition temperature of the maleimide-based quaternary copolymer is 170 to 190 ℃.
Citation Information
Patent Citations
Two-step polymerization process
EP1448633B2
Nitrile-based copolymer having improved color stability and preparing process thereof
KR100160174B1
Alphamethylstyrene-based copolymer having excellent heat resistance and method for preparing the same
KR101185633B1
Styrenic tetrapolymer, method for preparing the same and thermoplastic resin composition comprising thereof
KR101739621B1
A tetra-copolymer and a method for manufacturing the same
KR101957231B1