AI Technical Summary
Lithium secondary batteries face safety issues due to the generation of oxygen at the positive electrode, leading to potential ignition and short circuits, especially in high-temperature environments, and all-solid-state batteries do not yet match the performance of liquid electrolyte-based batteries in terms of output, capacity, and lifespan.
Incorporating an inorganic solid electrolyte, specifically a NASICON-structured lithium aluminum titanium phosphate (LATP)-based compound, into the positive electrode, along with a gel-type electrolyte, ensuring uniform distribution and coverage of the electrode active material, and using a specific composition and distribution of the electrolyte layers to enhance safety.
The solution delays ignition and reduces explosive power by ensuring the inorganic solid electrolyte is uniformly distributed and covers over 50% of the positive electrode active material surface, enhancing safety even under heavy loading conditions.
Smart Images

Figure 112024137856875-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a lithium secondary battery with improved safety, and more specifically, to a lithium secondary battery comprising an inorganic solid electrolyte in the positive electrode and a gel-type electrolyte. Background Technology
[0002] Recently, as the application areas of lithium-ion batteries have rapidly expanded to include not only power supply for electronic devices such as electrical, electronic, telecommunications, and computers, but also power storage for large-area devices such as automobiles and power storage systems, there is a growing demand for high-capacity, high-output, and high-stability secondary batteries.
[0003] Generally, a lithium secondary battery comprises a positive electrode, a negative electrode, a separator interposed between the positive and negative electrodes, an electrolyte, an organic solvent, etc. Due to its unstable structure in the charged state, the positive electrode can generate oxygen; since the generation of oxygen poses a high risk of ignition, research and development are being conducted on methods to enhance the stability of lithium secondary batteries.
[0004] Separators are used to ensure electrical insulation between the anode and cathode, and thin membranes made of polyolefin are generally used. However, polyolefin-based separators can easily shrink in high-temperature environments, potentially failing to provide insulation between the anode and cathode. If electrical insulation between the anode and cathode becomes impossible, a short circuit occurs; this can react with oxygen generated by the unstable anode, leading to ignition. In other words, if a short circuit occurs within a charged lithium-ion battery in a high-temperature environment, the battery may ignite.
[0005] Accordingly, all-solid-state batteries utilizing solid electrolytes are being widely researched to ensure the safety of lithium-ion batteries, a field in which the industry is expanding; however, it is known that they have not yet achieved the same output, capacity, and lifespan performance as lithium-ion batteries using liquid electrolytes, and thus fall far short of the level for commercialization.
[0006] Therefore, the biggest issue in the industry is ultimately realizing batteries with enhanced safety that do not ignite even at significantly high temperatures; however, since it is very difficult to prevent ignition caused by the volatilization of the liquid electrolyte and oxygen generation at the cathode in lithium-ion batteries using liquid electrolytes at high temperatures, research is actively underway to reduce the explosive power of the battery to secure time for users to evacuate. The problem to be solved
[0007] The present invention aims to improve the safety of a secondary battery by delaying ignition and reducing explosive power of the lithium secondary battery. means of solving the problem
[0008] According to one embodiment of the present invention,
[0009] A positive electrode having a positive electrode composite layer comprising a positive electrode active material and an inorganic solid electrolyte formed on one or both sides of a positive electrode current collector,
[0010] A cathode having a cathode composite layer containing a cathode active material formed on one or both sides of a cathode current collector,
[0011] A separator interposed between the anode and the cathode, and
[0012] It includes a gel-type electrolyte,
[0013] A lithium secondary battery is provided in which the above-mentioned inorganic solid electrolyte is included in an amount of 0.5% to 2% by weight based on the total weight of the above-mentioned anode composite layer and is uniformly distributed within the above-mentioned anode composite layer.
[0014] Here, when the anode composite layer is divided in half based on the thickness direction, the inorganic solid electrolyte may be included in the upper layer at 40 to 60 weight% and the lower layer at 40 to 60 weight% based on the total weight of the inorganic solid electrolyte, and more specifically, when the upper layer and the lower layer are each divided in half, the inorganic solid electrolyte may be included in each layer at 20 to 30 weight% based on the total weight of the inorganic solid electrolyte.
[0015] In addition, as such, the inorganic solid electrolyte is distributed uniformly throughout, so that 50% to 90% of the total surface area of the positive active material may be covered by the inorganic solid electrolyte.
[0016] At this time, the inorganic solid electrolyte may be an oxide-based solid electrolyte having a NASICON structure, and more specifically, may be an oxide-based solid electrolyte represented by the following chemical formula 1.
[0017] [Chemical Formula 1]
[0018] Li 1+x M' 2-x M x (PO4)3
[0019] In the above chemical formula 1,
[0020] 0 <x<2 이고,
[0021] M' is one or more selected from the group consisting of Ti, Zr, Ge, Sn and Hf, and M is one or more selected from the group consisting of Cr, Al, Mg, Ga, Sc, Y, In and La.
[0022] More specifically, the oxide-based solid electrolyte may be a lithium aluminum titanium phosphate (LATP)-based compound in which M' is Ti and M is Al.
[0023] The loading amount of the anode composite layer of the above anode is 400 mg / 25 cm 2 Up to 600 mg / 25 cm2 It could be.
[0024] Meanwhile, the above-mentioned lithium secondary battery may include a gel-type electrolyte, and such gel-type electrolyte comprises i) a lithium salt, ii) a non-aqueous organic solvent, and
[0025] iii) comprising at least one polymerizable compound selected from the group consisting of polymerizable monomers, oligomers, or copolymers having polymerizable unsaturated functional groups, and
[0026] At least some of the above-mentioned polymerizable unsaturated functional groups may be hardened.
[0027] At this time, the polymerizable unsaturated functional group may be one or more selected from the group consisting of vinyl groups, epoxy groups, allyl groups and (meth)acrylic groups.
[0028] The above-mentioned non-aqueous organic solvent may be a carbonate-based organic solvent.
[0029] Furthermore, the gel-type electrolyte may further include a polymerization initiator, and the polymerization initiator may be a photoinitiator or a thermal initiator, and may be included in an amount of 0.01 to 20 parts by weight based on 100 parts by weight of a polymerizable compound.
[0030] In addition, the gel-type electrolyte may further contain a functional additive, and the functional additive may be one or more selected from the group consisting of sulfonate-based compounds, sulfite-based compounds, sulfone-based compounds, sulfate-based compounds, halogen-substituted carbonate-based compounds, nitrile-based compounds, cyclic carbonate-based compounds, phosphate-based compounds, borate-based compounds, and lithium salt-based compounds. Effects of the invention
[0031] The lithium secondary battery according to the present invention can exhibit the effect of improving the safety of the lithium secondary battery by delaying the ignition of the lithium secondary battery, lowering the explosive pressure, and increasing the reaction time to reduce explosive force, by ensuring that the inorganic solid electrolyte is not only uniformly distributed within the positive electrode but is also included in an amount greater than a predetermined amount to cover the surface of the positive electrode active material by more than 50%, and in addition, by gelling the electrolyte.
[0032] Furthermore, the lithium secondary battery of the present invention allows the inorganic solid electrolyte to be uniformly distributed in the thickness direction even during heavy loading, making it effective in ensuring the safety of the lithium secondary battery even during heavy loading. Brief explanation of the drawing
[0033] Figure 1 is an SEM-EDS photograph of Experimental Example 1 according to Example 1. Figure 2 is an SEM-EDS photograph of Experimental Example 1 according to Comparative Example 3. Figure 3 is a graph showing the results of Experimental Example 2 according to Example 1. Figure 4 is a graph showing the results of Experimental Example 2 according to Example 2. Figure 5 is a graph showing the results of Experimental Example 2 according to Example 3. Figure 6 is a graph showing the results of Experimental Example 2 according to Comparative Example 1. Figure 7 is a graph showing the results of Experimental Example 2 according to Comparative Example 2. Figure 8 is a graph showing the results of Experimental Example 2 according to Comparative Example 3. Figure 9 is a graph of the capacity retention rate according to Experimental Example 3. Specific details for implementing the invention
[0034] Hereinafter, terms and words used in this specification and claims shall not be interpreted as being limited to their ordinary or dictionary meanings, but shall be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.
[0035] Unless otherwise defined, all terms used in this specification (including technical and scientific terms) may be used in a meaning that is commonly understood by those skilled in the art to which the present invention pertains. Additionally, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless explicitly and specifically defined otherwise.
[0036] The terms used herein are for describing the embodiments and are not intended to limit the invention. In this specification, the singular form includes the plural form unless specifically stated otherwise in the text. As used herein, "comprises" and / or "comprising" do not exclude the presence or addition of one or more other components in addition to the components mentioned.
[0037] In this specification, when a part is described as including a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0039] A lithium secondary battery according to one embodiment of the present invention is,
[0040] A positive electrode having a positive electrode composite layer comprising a positive electrode active material and an inorganic solid electrolyte formed on one or both sides of a positive electrode current collector,
[0041] A cathode having a cathode composite layer containing a cathode active material formed on one or both sides of a cathode current collector,
[0042] A separator interposed between the anode and the cathode, and
[0043] It includes a gel-type electrolyte,
[0044] The above-mentioned inorganic solid electrolyte is included in an amount of 0.5% to 2% by weight based on the total weight of the anode composite layer and is characterized by being uniformly distributed within the anode composite layer.
[0046] anode
[0047] The anode has a structure in which an anode composite layer comprising an anode active material and an inorganic solid electrolyte is formed on one or both sides of an anode current collector.
[0048] Here, the anode composite layer can be formed by applying, drying, and rolling an anode slurry comprising an anode active material and an inorganic solid electrolyte onto an anode current collector. At this time, in addition to the materials, the anode slurry may further include electrode materials such as a conductive material and a binder.
[0049] The above positive current collector may be conductive without causing chemical changes in the battery, and is not particularly limited. For example, the above current collector may be stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.
[0050] The positive current collector (121) may have a thickness of 3 μm to 500 μm, and may have fine irregularities formed on the surface of the positive current collector to increase adhesion to the positive active material layer. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0051] The above-mentioned cathode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium metal oxide containing lithium and one or more metals such as cobalt, manganese, nickel, or aluminum. More specifically, the lithium metal oxide is a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), or a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2(here, 0 <Y<1), LiMn 2-Z Ni Z O4 (where 0 < Z < 2), etc.), lithium-nickel-cobalt oxides (e.g., LiNi 1-Y1 Co Y1 O2(here, 0 <Y1<1) 등), 리튬-망간-코발트계 산화물(예를 들면, LiCo 1-Y2 Mn Y2 O2(here, 0 <Y2<1), LiMn 2-Z1 Co Z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-manganese-cobalt oxides (e.g., Li(Ni p Co q Mn r )O2(where, 0<p<1, 0<q<1, 0<r<1, p+q+r=1) or Li(Ni p1 Co q1 Mn r1 )O4 (where 0<p1<2, 0<q1<2, 0<r1<2, p1+q1+r1=2), etc.), or lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r2 M s2)O2(wherein M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r2, and s2 are the atomic fractions of independent elements, respectively, 0 < p2 < 1, 0 < q2 < 1, 0 < r2 < 1, 0 < s2 < 1, p2 + q2 + r2 + s2 = 1), etc.), lithium iron phosphate (e.g., Li 1+a Fe 1-x M x (PO 4-b )X b (Here, M is one or more selected from Al, Mg and Ti, and X is one or more selected from F, S and N, and -0.5≤a≤0.5, 0≤x≤0.5, 0≤b≤0.1) etc., and any one or more of these compounds may be included.
[0052] Among these, the lithium metal oxides mentioned above include LiCoO2, LiMnO2, LiNiO2, and lithium nickel manganese cobalt oxide (e.g., Li(Ni)) in that they can improve the capacity characteristics and stability of the battery. 1 / 3 Mn 1 / 3 Co 1 / 3 )O2, Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 and Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), lithium nickel-cobalt-aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.), or lithium nickel manganese cobalt aluminum oxide (e.g., Li(Ni 0.86 Co 0.05 Mn 0.07 Al 0.02It may be )O2), lithium iron phosphate (e.g., LiFePO4), etc., and any one or more of these may be used.
[0053] The above positive active material may be included in an amount of 60 to 98 weight%, preferably 80 to 98 weight%, and more preferably 90 to 98 weight% based on the total weight of the positive composite layer.
[0054] The above inorganic solid electrolyte may include one or more lithium metal oxides or lithium metal phosphates selected from Nasicon-type solid electrolytes, Lisicon-type solid electrolytes, Garnet-type solid electrolytes, Perovskite-type solid electrolytes, and LiPON-type solid electrolytes, and more specific examples may include one or more selected from the group consisting of LAGP (lithium aluminum germanium phosphate)-based compounds, LLZO (lithium lanthanum zirconium oxide)-based compounds, LATP (lithium aluminum titanium phosphate)-based compounds, LLZTO (lithium lanthanum zirconium tantalum oxide)-based compounds, LLTO (lithium lanthanum titanium oxide)-based compounds, LSTP (lithium silicon titanium phosphate)-based compounds, and LGPO (lithium germanium phosphate)-based compounds.
[0055] More specifically, the inorganic solid electrolyte may be a nasicon-type solid electrolyte among the examples above, and may be an oxide-based solid electrolyte having a nasicon structure, and more specifically, may be represented by the following chemical formula 1.
[0056] [Chemical Formula 1]
[0057] Li 1+x M' 2-x M x (PO4)3
[0058] In the above chemical formula 1,
[0059] 0 <x<2 이고,
[0060] M' is one or more selected from the group consisting of Ti, Zr, Ge, Sn and Hf, and M is one or more selected from the group consisting of Cr, Al, Mg, Ga, Sc, Y, In and La.
[0061] Most specifically, among these, it may be a lithium aluminum titanium phosphate (LATP)-based compound in which M' is Ti and M is Al.
[0062] This inorganic solid electrolyte may be included in an amount of 0.5% to 2% by weight based on the total weight of the anode composite layer, and more specifically, 0.5% to 1% by weight.
[0063] If the content is too low outside the above range, it is difficult to obtain the explosive power reduction effect intended by the present invention, and if the content is too high, it is undesirable as it causes a problem of increased resistance of the lithium secondary battery.
[0064] In addition, the inorganic solid electrolyte can be uniformly distributed within the anode composite layer.
[0065] Here, 'uniformly distributed' means that when the anode composite layer is divided into two or more layers based on the thickness direction, the difference in the content of the inorganic solid electrolyte contained in the two or more layers does not differ by more than 20 weight% when the total weight of the inorganic solid electrolyte is 100 weight%.
[0066] In other words, when the anode composite layer is divided into two based on the thickness direction, the inorganic solid electrolyte content contained in the upper and lower layers, respectively, does not deviate from a ratio of 40:60 to 60:40 when the total inorganic solid electrolyte is 100% by weight.
[0067] Accordingly, when the anode composite layer is divided in half based on the thickness direction, the inorganic solid electrolyte may be included in the upper layer at 40 to 60 weight% and the lower layer at 40 to 60 weight% based on the total weight of the inorganic solid electrolyte.
[0068] More specifically, when the upper layer and the lower layer are each divided in half based on the thickness direction, the inorganic solid electrolyte may be included in each layer at a weight of 20 to 30% based on the total weight of the inorganic solid electrolyte.
[0069] Here, dividing the anode composite layer in half based on the thickness direction does not mean that the anode composite layer is formed in two or more layers, but rather means dividing the anode composite layer formed for analysis into an upper layer and a lower layer based on the thickness direction.
[0070] In addition, since the inorganic solid electrolyte is evenly distributed within the anode composite layer, the surface of the anode active material can be covered by more than 50% of the total surface area of the anode active material, specifically 50% to 90%, more specifically 50% to 80%, and most specifically 60% to 80%.
[0071] If the surface of the positive electrode active material is covered by less than 50% outside the above range, the safety intended by the present application cannot be sufficiently ensured and is therefore undesirable.
[0072] Furthermore, the average diameter (D50) of the inorganic solid electrolyte particles may be 50 nanometers to 10 micrometers, more specifically 50 nanometers to 5 micrometers, and even more specifically 50 nanometers to 1 micrometer.
[0073] If the particle size falls outside the above range and is too small, particle aggregation may occur due to reduced dispersibility; conversely, if it is too large, large pores are formed by the inorganic solid electrolyte, which is detrimental in terms of resistance. That is, when the above range is satisfied, the lithium ion conductivity of the anode is increased to reduce resistance, thereby enabling improved secondary battery performance.
[0074] The average diameter (D50) described above refers to the particle diameter corresponding to 50% of the volume accumulation in the particle diameter distribution curve. The D50 can be measured, for example, using a laser diffraction method. The laser diffraction method generally enables the measurement of particle diameters ranging from the submicron region to several millimeters, and can obtain results with high reproducibility and high resolution.
[0075] The above conductive material is a component for further improving the conductivity of the positive electrode active material, and such conductive material is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, carbon powder such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fibers such as carbon fibers or metal fibers; fluorocarbon powder; conductive powder such as aluminum powder or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. may be used.
[0076] The conductive material may be included in an amount of 0.1 to 20 weight%, specifically 0.5 to 10 weight%, and more specifically 0.5 to 5 weight% based on the total weight of the anode composite layer.
[0077] The above binder is a component that assists in the bonding between the conductive material, the positive active material, and the positive current collector. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polyethylene, polypropylene, ethylene-propylene-diene monomer, sulfonated ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.
[0078] Typically, the binder may be included in an amount of 0.5 to 20 weight%, more specifically 0.5 to 10 weight%, and more specifically 0.5 to 5 weight% based on the total weight of the anode composite layer.
[0079] In addition, the above-mentioned other additives may further include, for example, fillers as components that inhibit expansion. The above-mentioned filler is not particularly limited as long as it can inhibit the expansion of the electrode without causing chemical changes in the battery, and, for example, olifin-based polymers such as polyethylene and polypropylene; fibrous materials such as glass fibers and carbon fibers; etc. may be used.
[0080] Meanwhile, the loading amount of the above-mentioned anode composite layer of such an anode is 400 mg / 25 cm 2 Up to 600 mg / 25 cm 2 It could be, specifically, 450mg / 25cm 2 Up to 600 mg / 25 cm 2 It could be, and more specifically, 450mg / 25cm 2 Up to 550 mg / 25 cm 2 It could be.
[0081] In other words, in the case of the present invention, high secondary battery safety can be secured even when using a high-loading anode due to the uniform distribution of the inorganic solid electrolyte.
[0083] cathode
[0084] The above cathode has a structure in which a cathode composite layer is formed on one or both sides of a cathode current collector.
[0085] Here, the cathode composite layer can be formed by applying, drying, and rolling a cathode slurry containing a cathode active material onto a cathode current collector, and at this time, in addition to the cathode active materials, the cathode slurry may further include electrode materials such as a conductive material and a binder as described above.
[0086] The negative current collector (111) is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used.
[0087] The above negative current collector (111) can typically have a thickness of 3 μm to 500 μm, and, similar to the positive current collector, fine irregularities can be formed on the surface of the negative current collector to strengthen the bonding force of the negative active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0088] The above-mentioned negative electrode active material may include at least one selected from the group consisting of lithium metal, a carbon material capable of reversibly intercalating / deintercalating lithium ions, a metal or an alloy of these metals and lithium, a metal composite oxide, a material capable of doping and dedoping lithium, and a transition metal oxide.
[0089] As for the carbon material capable of reversibly intercalating / deintercalating the above lithium ions, any carbon-based negative electrode active material commonly used in lithium-ion secondary batteries may be used without particular limitation, and representative examples include crystalline carbon, amorphous carbon, or a combination thereof. Examples of the above crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the above amorphous carbon include soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0090] As the above metal or alloy of these metals and lithium, a metal selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn, or an alloy of these metals and lithium may be used.
[0091] The above metal composite oxides include PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5, LixFe2O3 (0≤x≤1), Li x WO2(0≤x≤1) and Sn x Me 1-x Me y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, Group 1, 2, and 3 elements of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 로 이루어진 군에서 선택되는 것이 사용될 수 있다.
[0092] Materials capable of doping and dedoping the above lithium include Si and SiO x(0 <x≤2), Si-Y 합금(상기 Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 및 이들의 조합으로 이루어진 군에서 선택되는 원소이며, Si은 아님), Sn, SnO2, Sn-Y(상기 Y는 알칼리 금속, 알칼리 토금속, 13족 원소, 14족 원소, 전이금속, 희토류 원소 및 이들의 조합으로 이루어진 군에서 선택되는 원소이며, Sn은 아님) 등을 들 수 있고, 또한 이들 중 적어도 하나와 SiO2를 혼합하여 사용할 수도 있다. 상기 원소 Y로는 Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po 및 이들의 조합으로 이루어진 군에서 선택될 수 있다.
[0093] Examples of the above transition metal oxides include lithium-containing titanium composite oxide (LTO), vanadium oxide, and lithium vanadium oxide.
[0094] The above-mentioned negative electrode active material may be included in an amount of 60 to 99 weight%, preferably 80 to 99 weight%, and more preferably 90 to 98 weight% based on the total weight of the negative electrode active material layer.
[0095] In cases where the metal itself is used without forming a cathode composite layer on the above cathode, it can be manufactured by physically bonding, rolling, or depositing the metal onto the metal thin film itself or onto the above cathode current collector. The deposition method may use an electro-deposition method or a chemical vapor deposition method.
[0096] For example, the metal thin film itself or the metal bonded / rolled / deposited on the negative current collector may include one metal selected from the group consisting of lithium (Li), nickel (Ni), tin (Sn), copper (Cu), and indium (In), or an alloy of two metals.
[0098] Separator
[0099] The separator can be used without special restrictions as long as it is typically used as a separator in a lithium secondary battery, and it is particularly desirable that it has low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capability.
[0100] For example, as a separator, a porous polymer film comprising polyolefin-based polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fibers, polyethylene terephthalate fibers, etc., may also be used as a separator.
[0101] Alternatively, it may be a Safety Reinforced Separator (SRS) membrane having a coating layer containing a binder and inorganic particles formed on one or both sides of a polymer substrate as described above.
[0102] The above-described SRS separator is as described above. Specifically, the polyolefin substrate of the SRS separator is as described above, and the coating layer comprises inorganic particles and a binder.
[0103] Here, the inorganic particles serve the dual role of forming micropores by enabling the formation of empty spaces between the inorganic particles and acting as a kind of spacer that maintains a physical shape. In addition, since the inorganic particles generally have the characteristic that their physical properties do not change even at high temperatures of 200°C or higher, the formed organic-inorganic mixed layer has excellent heat resistance.
[0104] The above-mentioned inorganic particles are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present invention are not particularly limited as long as they do not undergo oxidation and / or reduction reactions within the operating voltage range of the applied battery. In particular, when using inorganic particles with ion-transfer capabilities, it is desirable to have as high an ion conductivity as possible, as this can improve performance by increasing the ion conductivity within the electrochemical device. Furthermore, if the inorganic particles have a high density, it is desirable to have as low a density as possible, as this not only makes it difficult to disperse them during manufacturing but also causes problems with weight increase during the production of secondary batteries. Additionally, in the case of inorganic materials with high dielectric constant, they can improve the ion conductivity of the electrolyte by contributing to an increased degree of dissociation of electrolyte salts, such as lithium salts, within the liquid electrolyte. Finally, in the case of inorganic particles with thermal conductivity, it is even more desirable because their excellent heat-endoscopy ability suppresses the phenomenon where heat is concentrated locally to form heat points, which leads to thermal runaway.
[0105] For the reasons stated above, the inorganic particles are preferably one or more selected from the group consisting of (a) high dielectric constant inorganic particles having a dielectric constant of 1 or more, 5 or more, preferably 10 or more, (b) inorganic particles having piezoelectricity, (c) thermally conductive inorganic particles, and (d) inorganic particles having lithium ion transfer ability.
[0106] The above-mentioned piezoelectric inorganic particles refer to materials that are insulators at atmospheric pressure but possess the property of conducting electricity due to changes in their internal structure when a certain pressure is applied. In addition to exhibiting high dielectric constant characteristics with a dielectric constant of 100 or more, when subjected to tension or compression by applying a certain pressure, electric charge is generated, causing one side to become positively charged and the opposite side to become negatively charged, thereby creating a potential difference between the two sides.
[0107] Examples of the above-mentioned inorganic particles having piezoelectric properties include BaTiO3, Pb(Zr,Ti)O3 (PZT), and Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT) hafnia (H f O2) or mixtures thereof, but are not limited thereto.
[0108] The inorganic particles having the above lithium ion transfer capability refer to inorganic particles that contain lithium elements but do not store lithium and have the function of moving lithium ions. Since the inorganic particles having the lithium ion transfer capability can transfer and move lithium ions due to a type of defect existing within the particle structure, a decrease in lithium mobility can be prevented, thereby preventing a decrease in battery capacity.
[0109] Examples of inorganic particles having the above-mentioned lithium ion transfer ability include lithium phosphate (Li3PO4) and lithium titanium phosphate (Li x Ti y (PO4)3, 0 <x<2, 0<y<3), 리튬알루미늄티타늄포스페이트(Li x Al y Ti z (PO4)3, 0 <x<2, 0<y<1, 0<z<3), 14Li2O-9Al2O3-38TiO2-39P2O5등과 같은 (LiAlTiP)x O y Series glass (0 <x<4, 0<y<13), 리튬란탄티타네이트(Li x La y TiO3, 0 <x<2, 0<y<3), Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4, etc. x Ge y P z S w , 0 <x<4, 0<y<1, 0<z<1, 0<w<5), Li3N 등과 같은 리튬나이트라이드(Li x N y , 0 <x<4, 0<y<2), Li3PO4-Li2S-SiS2등과 같은 SiS2계열 glass (Li x Si y S z , 0 <x<3, 0<y<2, 0<z<4), LiI-Li2S-P2S5등과 같은 P2S5계열 glass (Li x P y S z , 0 <x<3, 0<y<3, 0<z<7), 또는 이들의 혼합물 등이 있으나, 이에 한정되는 것은 아니다.
[0110] In addition, examples of inorganic particles with a dielectric constant of 1 or greater include SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC, or mixtures thereof, but are not limited thereto.
[0111] The above thermally conductive inorganic particles are materials that provide low thermal resistance but do not provide electrical conductivity, thus having insulating properties, and may be one or more selected from the group consisting of, for example, aluminum nitride (AlN), boron nitride (BN), alumina (Al2O3), silicon carbide (SiC), and beryllium oxide (BeO), but are not limited thereto.
[0112] When the aforementioned high dielectric constant inorganic particles, piezoelectric inorganic particles, thermally conductive inorganic particles, and inorganic particles capable of transporting lithium ions are mixed, their synergistic effect can be doubled.
[0113] There is no limit to the size of the inorganic particles, but it is preferable that they be in the range of 0.001 to 10 μm to ensure an appropriate porosity between the inorganic particles. If the size is less than 0.001 μm, dispersibility is reduced, making it difficult to control physical properties; if the size exceeds 10 μm, the thickness increases, leading to a decrease in mechanical properties, and furthermore, due to the excessively large pore size, it fails to perform the function of a sufficient coating layer, increasing the probability of an internal short circuit occurring during battery charging and discharging.
[0114] There are no specific limitations on the content of the above inorganic particles, but a range of 1 to 99 weight% per 100 weight% of the mixture of inorganic particles and binder is preferred, and particularly 10 to 95 weight% is more preferred. If it is less than 1 weight%, the content of the binder becomes excessively high, which may reduce the pore size and porosity due to a decrease in the empty space formed between the inorganic particles, thereby reducing the mobility of lithium ions. Conversely, if it exceeds 99 weight%, the mechanical properties of the coating layer deteriorate due to weakened adhesion between the inorganic particles because the binder content is too low.
[0115] Meanwhile, the above-mentioned binder is not limited as long as it does not cause adverse reactions with the electrolyte, but in particular, one with a glass transition temperature (Tg) as low as possible can be used, preferably in the range of -200 to 200°C. This is because it can improve the mechanical properties of the final insulating film.
[0116] In addition, the above-mentioned binder does not necessarily have to possess ion conductivity, but it is more preferable to use a polymer that possesses ion conductivity.
[0117] Therefore, it is desirable for the above-mentioned binder to have a high possible dielectric constant, and since the degree of dissociation of the salt in the electrolyte actually depends on the dielectric constant of the electrolyte solvent, the higher the dielectric constant of the above-mentioned polymer, the higher the degree of dissociation of the salt in the electrolyte can be improved. The dielectric constant of the above-mentioned polymer can be 1 or higher, specifically in the range of 1.0 to 100 (measurement frequency = 1 kHz), and it is particularly desirable that it be 10 or higher.
[0118] In addition to the aforementioned functions, the binder may have the characteristic of gelling upon liquid electrolyte impregnation to exhibit a high degree of swelling. In practice, if the binder is a polymer with excellent electrolyte impregnation, the electrolyte injected after battery assembly permeates into the polymer, and the polymer retaining the absorbed electrolyte acquires electrolyte ion conductivity. Therefore, if possible, the solubility index is 15 to 45 MPa 1 / 2 A phosphorus polymer is preferred, with a value of 15 to 25 MPa 1 / 2 and 30 to 45 MPa 1 / 2 The range is more desirable. The solubility index is 15 MPa 1 / 2 Less than and 45 MPa 1 / 2 If it exceeds, it becomes difficult to swell with a conventional liquid electrolyte for batteries.
[0119] Examples of such binders include polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate copolymer, polyimide, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, and cyanoethylpullulan. It may be one or more selected from the group consisting of cyanoethylpolyvinyl alcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxyl methyl cellulose, and polyvinyl alcohol.
[0120] The total thickness of the separator may be 5 micrometers to 20 micrometers, more specifically 5 micrometers to 15 micrometers, and even more specifically 6 micrometers to 13 micrometers. When the thickness of the separator satisfies the above range, it is possible to effectively prevent a short circuit between the positive and negative electrodes while minimizing the resistance value of the lithium secondary battery. As a result, it is possible to prevent a decrease in the energy density of the lithium secondary battery and improve its lifespan characteristics.
[0122] Gel-type electrolyte
[0123] The above gel-type electrolyte comprises i) a lithium salt, ii) a non-aqueous organic solvent, and
[0124] iii) comprising at least one polymerizable compound selected from the group consisting of polymerizable monomers, oligomers, or copolymers having polymerizable unsaturated functional groups, and
[0125] At least some of the above polymerizable unsaturated functional groups may be hardened.
[0126] Here, the lithium salt is used as a medium for transferring ions within a lithium secondary battery. The lithium salt is, for example, Li as a cation + It includes, and as anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , B 10 Cl 10 - , AlCl4 - , AlO2 - , PF6 - , CF3SO3 - , CH3CO2 - , CF3CO2 - , AsF6 - , SbF6 - , CH3SO3 -, (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - , BF2C2O4 - , BC4O8 - , PF4C2O4 - , PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , C4F9SO3 - , CF3CF2SO3 - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CF3(CF2)7SO3 - and SCN - At least one selected from the group consisting of can be cited.
[0127] Specifically, the lithium salt is LiCl, LiBr, LiI, LiBF4, LiClO4, LiB 10 Cl 10 It may include a single substance or a mixture of two or more substances selected from the group consisting of LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiFSI (Lithium bis(fluorosulfonyl) imide, LiN(SO2F)2), LiBETI (lithium bis(perfluoroethanesulfonyl) imide, LiN(SO2CF2CF3)2)2 and LiTFSI (lithium bis(trifluoromethanesulfonyl) imide, LiN(SO2CF3)2), but it is preferable to include Li(N(SO2CF3)2 for excellent stability.
[0128] In addition to these, lithium salts commonly used in the electrolytes of lithium secondary batteries can be used without restriction.
[0129] The above lithium salt can be appropriately modified within a range that is typically usable, but in order to obtain the effect of forming a corrosion-preventing film on the optimal electrode surface, it may be included in the electrolyte at a concentration of 0.5 M to 3 M, specifically at a concentration of 1 M to 2.5 M, and more specifically at a concentration of 1 M to 2 M. When the concentration of the lithium salt satisfies the above range, the effect of improving cycle characteristics during high-temperature storage of the lithium secondary battery is sufficient, and the viscosity of the electrolyte is appropriate, so the electrolyte impregnation can be improved.
[0130] The above-mentioned non-aqueous organic solvent is not limited to any specific type, provided that it minimizes decomposition due to oxidation reactions, etc., within the voltage range of the charging and discharging process of a lithium secondary battery and can exhibit characteristics together with additives. For example, carbonate-based organic solvents, ether-based organic solvents, or ester-based organic solvents may be used individually or in a mixture of two or more types, and specifically, carbonate-based organic solvents may be used.
[0131] Among the above organic solvents, the carbonate-based organic solvent may include at least one of a cyclic carbonate-based organic solvent and a linear carbonate-based organic solvent. Specifically, the cyclic carbonate-based organic solvent may include at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and fluoroethylene carbonate (FEC). Specifically, it may include a mixed solvent of ethylene carbonate having a high dielectric constant and propylene carbonate having a relatively low melting point compared to ethylene carbonate.
[0132] In addition, the linear carbonate-based organic solvent is a solvent having low viscosity and low dielectric constant, and may include at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethylmethyl carbonate (EMC), methylpropyl carbonate, and ethylpropyl carbonate, and more specifically may include dimethyl carbonate.
[0133] The above ether-based organic solvent may be any one selected from the group consisting of ethylene glycol dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methylpropyl ether, and ethyl propyl ether, or a mixture of two or more of these, but is not limited thereto.
[0134] The above ester-based organic solvent may include at least one selected from the group consisting of linear ester-based organic solvents and cyclic ester-based organic solvents.
[0135] The above linear ester-based organic solvent may be represented by any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, or a mixture of two or more of these, but is not limited thereto.
[0136] The above-mentioned cyclic ester-based organic solvent may be any one selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, or a mixture of two or more of these, but is not limited thereto.
[0137] Among the above ester-based solvents, cyclic carbonate compounds can be preferably used as high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts in the electrolyte. Furthermore, if low-viscosity, low-dielectric constant linear carbonate compounds such as dimethyl carbonate and diethyl carbonate, and linear ester compounds are mixed in appropriate proportions with such cyclic carbonate compounds, a gel-type electrolyte with high electrical conductivity can be produced, making it even more preferable to use.
[0138] Meanwhile, the polymerizable compound of the above polymerizable monomer, oligomer, or copolymer is a substance having a polymerizable unsaturated functional group, for example, having a polymerizable unsaturated functional group selected from the group consisting of vinyl groups, epoxy groups, allyl groups, and (meth)acrylic groups, and is a compound that can be changed into a gel form by polymerization or crosslinking, and is not particularly limited as long as it is used as a polymerizable monomer, oligomer, or polymer for the manufacture of conventional gel-type electrolytes.
[0139] More specifically, the polymerizable monomer or oligomer is, as a non-limiting example, tetraethyleneglycoldiacrylate, polyethylene glycol diacrylate (molecular weight 50–20,000), 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxylate triacrylate, trimethylolpropane propoxylate triacrylate, ditrimethylolpropane tetraacrylate, and pentaerythritol. Tetraacrylate (pentaerythritol tetraacrylate), Pentaerythritol ethoxylate tetraacrylate, Dipentaerythritol pentaacrylate, Dipentaerythritol hexaacrylate, Poly(ethyleneglycol) diglycidyl ether, 1,5-hexadiene diepoxide, Glycerol propoxylate triglycidyl ether, Vinylcyclohexenedioxide, 1,2,7,8-diepoxyoctane,Examples include, butyl glycidyl ether, diglycidyl 1,2-cyclohexanedicarboxylate, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and glycidyl methacrylate, but are not limited thereto; these compounds may be used alone or in a mixture of two or more.
[0140] In addition, the above copolymer may include at least one copolymer selected from the group consisting of allyl 1,1,2,2-tetrafluoroethyl ether (TFE)-(2,2,2-trifluoroethyl acrylate) polymer, TFE-vinyl acetate, TFE-(2-vinyl-1,3-dioxoran) polymer, TFE-vinyl methacrylate polymer, TFE-acrylonitrile polymer, TFE-vinyl acrylate polymer, TFE-methyl acrylate polymer, TFE-methyl methacrylate (MMA) polymer, and TFE-2,2,2-trifluoroethyl acrylate (FA) polymer as representative examples.
[0141] The polymer formed by curing the above materials may be included in an amount of 0.01% to 10% by weight based on the total weight of the gel-type electrolyte. If the content of the polymer exceeds 10% by weight, the amount of polymerizable material increases during the preparation of the gel-type electrolyte, which results in gelation occurring too quickly or being formed too densely, thus having the disadvantage of obtaining a gel with high resistance; conversely, if the content is less than 0.01% by weight, the effect of gelation cannot be obtained, which is undesirable.
[0142] Meanwhile, the gel-type electrolyte of the present invention may further include a polymerization initiator for the polymerization of the polymerizable unsaturated functional group, and conventional thermal or photoinitiators known in the art may be used. For example, the initiator may decompose by heat to form radicals and react with polymerizable monomers, oligomers, or polymers, etc., by free radical polymerization to form a gel-type electrolyte.
[0143] More specifically, examples of the polymerization initiators include organic peroxides or hydroperoxides such as benzoyl peroxide, acetyl peroxide, dilauryl peroxide, di-tert-butyl peroxide, t-butyl peroxy-2-ethyl-hexanoate, cumyl hydroperoxide, and hydrogen peroxide, and 2,2'-azobis(2-cyanobutane), 2,2'-azobis(methylbutyronitrile), and 2,2'-azobis(isobutyronitrile) (AIBN; 2,2'-Azobis(iso-butyronitrile)). There are, but are not limited to, one or more azo compounds selected from the group consisting of 2,2'-azobisdimethyl-valeronitrile (AMVN).
[0144] The above polymerization initiator may decompose within a lithium secondary battery by heat, for example, heat of 30°C to 100°C, or by decomposing at room temperature (5°C to 30°C) to form radicals, and the polymerizable monomer, oligomer, or polymerizable unsaturated functional group of the polymer may react through free radical polymerization to form a gel-type electrolyte.
[0145] The above polymerization initiator may be included in an amount of 0.01 to 20 parts by weight, specifically 0.01 to 1 part by weight, based on 100 parts by weight of the polymerizable compound.
[0146] When the above polymerization initiator is in the range of 0.01 to 20 parts by weight, the gel conversion rate can be increased to secure gel-type electrolyte characteristics, and the pre-gel reaction can be prevented, thereby improving the electrolyte wetting properties of the electrode.
[0147] Furthermore, the gel-type electrolyte may further include a functional additive, and the functional additive may be included to prevent cathode breakdown in a high-power environment or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, prevention of overcharging, and swelling improvement effects during high-temperature storage.
[0148] Specifically, the functional additive may include one or more functional additives selected from the group consisting of sulfonate compounds, sulfite compounds, sulfone compounds, sulfate compounds, halogen-substituted carbonate compounds, nitrile compounds, cyclic carbonate compounds, phosphate compounds, borate compounds, and lithium salt compounds as representative examples.
[0149] The above sulfone-based compound may be at least one compound selected from the group consisting of 1,3-propane sulfone (PS), 1,4-butane sulfone, ethene sulfone, 1,3-propene sulfone (PRS), 1,4-butene sulfone, and 1-methyl-1,3-propene sulfone, and may be included in an amount of 0.3% to 5% by weight, specifically 1% to 5% by weight, based on the total weight of the gel electrolyte. If the content of the sulfone-based compound in the gel electrolyte exceeds 5% by weight, an excessively thick film may be formed on the electrode surface, causing an increase in resistance and output degradation, and the resistance may also increase due to the excess amount of additive, which may lead to a deterioration in output characteristics.
[0150] The above sulfite-based compounds may include one or more compounds selected from the group consisting of ethylene sulfite, methyl ethylene sulfite, ethyl ethylene sulfite, 4,5-dimethyl ethylene sulfite, 4,5-diethyl ethylene sulfite, propylene sulfite, 4,5-dimethyl propylene sulfite, 4,5-diethyl propylene sulfite, 4,6-dimethyl propylene sulfite, 4,6-diethyl propylene sulfite, and 1,3-butylene glycol sulfite, and may be included in an amount of 3% by weight or less based on the total weight of the gel-type electrolyte.
[0151] The above sulfone-based compounds may include one or more compounds selected from the group consisting of divinylsulfone, dimethyl sulfone, diethyl sulfone, methyl ethyl sulfone, and methylvinyl sulfone, and may be included in an amount of 3% by weight or less based on the total weight of the gel-type electrolyte.
[0152] The above sulfate-based compounds may include ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS), and may be included in an amount of 3% by weight or less based on the total weight of the gel electrolyte.
[0153] In addition, the above-mentioned halogen-substituted carbonate compound may be fluoroethylene carbonate (FEC), and may be included in an amount of 5% by weight or less based on the total weight of the gel electrolyte. If the content of the halogen-substituted carbonate compound in the gel electrolyte exceeds 5% by weight, the cell swelling performance may deteriorate.
[0154] In addition, the nitrile-based compound may include at least one compound selected from the group consisting of succinonitrile, adiponitrile (Adn), acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanitrile, cyclopentane carbonitrile, cyclohexane carbonitrile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.
[0155] The above-mentioned cyclic carbonate-based compound may be vinylene carbonate (VC) or vinylethylene carbonate, and may be included in an amount of 3% by weight or less based on the total weight of the gel-type electrolyte. If the content of the cyclic carbonate-based compound in the gel-type electrolyte exceeds 3% by weight, the cell swelling inhibition performance may deteriorate.
[0156] The above phosphate-based compound may be one or more compounds selected from the group consisting of lithium difluoro(bisoxalato)phosphate, lithium difluorophosphate, tetramethyl trimethylsilyl phosphate, trimethylsilyl phosphite, tris(2,2,2-trifluoroethyl)phosphate, and tris(trifluoroethyl)phosphite, and may be included in an amount of 3% by weight or less based on the total weight of the gel-type electrolyte.
[0157] The above borate-based compound may be lithium oxalyl difluoroborate, and may be included in an amount of 3% by weight or less based on the total weight of the gel-type electrolyte.
[0158] The above lithium salt-based compound is a compound different from the lithium salt included in the gel-type electrolyte, and may include one or more compounds selected from the group consisting of LiPO2F2, LiODFB, LiBOB (lithium bisoxalate toborate (LiB(C2O4)2) and LiBF4), and may be included in an amount of 3% by weight or less based on the total weight of the gel-type electrolyte.
[0159] The above functional additives may be mixed in two or more types and included in an amount of 20% by weight or less, specifically 0.1% to 10% by weight, based on the total weight of the gel-type electrolyte. If the content of the above functional additives exceeds 20% by weight, there is a possibility that excessive side reactions may occur within the gel-type electrolyte during the charging and discharging of the battery. In particular, they may not decompose sufficiently at high temperatures and may remain as unreacted substances or precipitates within the gel-type electrolyte at room temperature. Consequently, side reactions that degrade the lifespan or resistance characteristics of the lithium secondary battery may occur.
[0161] Hereinafter, a lithium secondary battery according to one embodiment of the present invention will be described with reference to an example to demonstrate that it exhibits an enhanced effect.
[0163] <Example 1>
[0164] Manufacturing of anodes
[0165] An aluminum (Al) metal thin film with a thickness of 15 micrometers is prepared as an anode current collector, and Li(Ni) is prepared as an anode active material on one surface of the aluminum metal thin film. 0.8 Mn 0.1 Co 0.1 )O2: As an inorganic solid electrolyte, Li 1.4 Al 0.4 Ti 1.6 An anode slurry prepared by dispersing (PO4)3(LATP) as a conductive material, carbon nanotubes as a conductive material, and PVDF as a binder in an NMP solvent at a weight ratio of 95:1:1:3, is coated, dried, and rolled to a thickness of 60 micrometers (loading amount 450 mg / 25 cm²). 2 Manufactured ).
[0166] Manufacturing of the cathode
[0167] Next, a copper (Cu) metal thin film with a thickness of 20 micrometers was prepared as a negative electrode current collector, and a negative electrode slurry was prepared by dispersing graphite as a negative electrode active material, carbon black as a conductive material, carboxymethylcellulose (CMC) as a thickening material, and styrene-butadiene rubber (SBR) as a binder in water in a weight ratio of 95:1:1.5:2.5 on one side of the copper metal thin film, and then coating, drying, and rolling the resulting slurry to a thickness of 75 micrometers to produce a negative electrode.
[0168] Manufacturing of electrode assemblies
[0169] An electrode assembly was manufactured by interposing a polyolefin separator (thickness: 15 micrometers) between the anode and the cathode.
[0170] Manufacturing of lithium secondary batteries
[0171] LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent having a composition of ethylene carbonate (EC) : ethylmethyl carbonate (EMC) = 30 : 70 (volume ratio). A composition for a gel polymer electrolyte was prepared by adding 4% by weight of trimethylolpropane triacrylate as a polymerizable compound based on the total weight, and 0.02% by weight of azobisisobutyronitrile (AIBN, V59) as a polymerization initiator based on 100 parts by weight of the polymerizable compound.
[0172] The electrode assembly manufactured above was inserted into a battery case, and the gel polymer electrolyte composition manufactured above was injected to manufacture a secondary battery. Subsequently, the battery case was subjected to wetting with the electrolyte at room temperature for 2 days, and then the gel polymer electrolyte composition was left in a 60°C chamber for 5 hours to polymerize, thereby manufacturing a lithium secondary battery.
[0174] <Example 2>
[0175] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the polymerizable compound in the gel polymer electrolyte composition of Example 1 was 10 wt% of the total weight.
[0177] <Example 3>
[0178] In the anode of Example 1 above, Li(Ni as the anode active material 0.8 Mn 0.1 Co 0.1 )O2: As an inorganic solid electrolyte, Li 1.4 Al 0.4 Ti 1.6 A lithium secondary battery was manufactured in the same manner as in Example 1 above, except that the weight ratio of carbon nanotubes as (PO4)3(LATP) as a conductive material and PVDF as a binder was 94:2:1:3.
[0180] <Comparative Example 1>
[0181] In the anode of Example 1 above, Li(Ni as the anode active material 0.8 Mn 0.1 Co 0.1 A lithium secondary battery was manufactured in the same manner as in Example 1 above, except that carbon nanotubes as a conductive material and PVDF as a binder were mixed in a weight ratio of 96:1:3, and instead of a composition for a gel polymer electrolyte, a liquid electrolyte solution was prepared by dissolving LiPF6 to a concentration of 1.0 M in a non-aqueous organic solvent having a composition of ethylene carbonate (EC) : ethyl methyl carbonate (EMC) = 30:70 (volume ratio) and pouring it in to perform only the impregnation process.
[0183] <Comparative Example 2>
[0184] A lithium secondary battery was manufactured in the same manner as in Example 1, except that the same cathode as in Example 1 was used, and instead of the gel polymer electrolyte composition of Example 1, a liquid electrolyte in which LiPF6 was dissolved to a concentration of 1.0 M in a non-aqueous organic solvent having a composition of ethylene carbonate (EC) : ethylmethyl carbonate (EMC) = 30 : 70 (volume ratio) was injected to perform only the impregnation process.
[0186] <Comparative Example 3>
[0187] In the anode of Example 1 above, Li(Ni as the anode active material 0.8 Mn 0.1 Co 0.1 A lithium secondary battery was manufactured in the same manner as in Example 1 above, except that carbon nanotubes as a conductive material and PVDF as a binder were mixed in a weight ratio of 96:1:3.
[0189] <Comparative Example 4>
[0190] In the anode of Example 1 above, Li(Ni as the anode active material 0.8 Mn 0.1 Co 0.1 )O2: As an inorganic solid electrolyte, Li 1.4 Al 0.4 Ti 1.6 A lithium secondary battery was manufactured in the same manner as in Example 1 above, except that the weight ratio of carbon nanotubes as (PO4)3(LATP) as a conductive material and PVDF as a binder was 93:3:1:3.
[0192] <Experimental Example 1>
[0193] SEM images of the cross-sections were taken by cutting the anodes prepared in Example 1, Comparative Example 3, and 4 in the thickness direction through the center, and EDS analysis was performed.
[0194] At this time, the analysis was conducted by dividing the upper and lower layers in the thickness direction, and the results are shown in Figures 1 and 2 and Table 1 below.
[0195] Example 1 Comparative Example 3 Upper layer (wt%) Lower layer (wt%) Bare C 6.93 7.28 8.05 O 28.21 29.27 31.78 F 2.11 2.2 2.27 Al 0.64 0.67 0.61 P 0.48 0.45 0.07 Ti 0.4 0.35 0 Mn 4.82 4.72 4.45 Co 3.21 3.13 3.06 Ni 52.59 51.92 49.72 Total 100 100 100
[0196] Referring to Figures 1 and 2 below and Table 1 above, it can be seen that the inorganic solid electrolyte is distributed in very similar amounts in both the upper and lower layers of the anode composite layer according to the present invention.
[0198] <Experimental Example 2>
[0199] The lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 3 were fully charged at 25°C with a constant current of 0.33C until they reached 4.2V. A heating pad made of mica was attached to these lithium secondary batteries and the temperature was raised at 300W / min for 1 minute, after which the 300W was maintained to create an external ignition environment. While maintaining these conditions, the voltage, pressure, and temperature of the lithium secondary batteries were measured over time and are shown in Figures 3 to 8 below.
[0200] The difference between the maximum pressure measured at the time of explosion of the above lithium secondary batteries and the initially set atmospheric pressure was defined as the explosion pressure, and the time from the point at which the pressure begins to change to the maximum pressure was defined as the reaction time.
[0201] A relatively lower explosion pressure and a longer reaction time indicate that the explosive power of the lithium secondary battery is smaller. The results are shown in Table 2 below.
[0202] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Explosive pressure (bar) 1.29 1.35 1.31 1.46 1.47 1.48 Reaction time (sec) 10.1 10.3 10.1 8.3 7.5 8.1 Explosion pressure / reaction time 0.128 0.131 0.130 0.176 0.196 0.183
[0203] Referring to Figures 3 to 8 below and Table 2 above, lithium secondary batteries according to the embodiments using LATP in the cathode and a gel-type electrolyte according to the present invention showed the highest values for explosion pressure and reaction time, with an explosion pressure of 1.29 bar and a reaction time of 10.1 s. In the case of Comparative Example 1, the explosion pressure was 1.46 bar and the reaction time was 8.3 s, indicating that compared to Comparative Example 1, the explosion pressure of Example 1 decreased by 11.6% and the reaction time increased by 21.7%. When converted to explosion pressure per reaction time, Example 1 showed 0.128 bar / sec and Comparative Example 1 showed 0.176 bar / sec, indicating a difference of 27.4%. Similarly, Comparative Example 2, which does not use a gel-type electrolyte, and Comparative Example 3, which does not use LATP in the cathode, also showed results similar to Comparative Example 1.
[0205] <Experimental Example 3>
[0206] For the lithium secondary batteries of Example 1 and Comparative Examples 1 to 3 above, the process of CC-CV charging at 25°C at 0.33C and CC discharging at 0.33C was repeated for 300 cycles, and the discharge capacity retention rate at 300 cycles was calculated with the discharge capacity of 1 cycle set to 100%, and the results are shown in Table 3 and Figure 9 below.
[0207] In addition, DC resistance was measured for the lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 4 using the HPPC (Hybrid pulse power characterization) method, and the results are shown in Table 3 below.
[0208] The above DC resistance measurement was performed by checking the capacity of the lithium secondary batteries by CC / CV charging under conditions of 0.33C, 4.2V, and 0.05C cut-off, and CC discharging under conditions of 0.33C and 2.5V cut-off, and then discharging the fully charged lithium secondary batteries under the same charging conditions to 50% of their capacity to adjust the SOC to 50, and subsequently measuring the DC resistance at that SOC through 2.5C and 10-second discharge.
[0209] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Cell resistance (mohm) 1.86 2.05 1.88 1.88 1.80 1.98 1.90 Dose retention rate (%) 95.5 - - 95.5 95.7 95.7 -
[0210] Referring to Table 3 above, it can be seen that the resistance of Example 1 and Comparative Example 2, in which LATP is added, is relatively low. In this case, it can be seen that the resistance of the lithium secondary battery decreases by about 2 to 3% compared to the case where it is not added. However, from Example 1 and Comparative Example 4, it can be seen that when the LATP content is 3 wt%, the resistance actually increases. Meanwhile, since the capacity retention rate is similar, it can be seen that there is no other degradation of the lithium secondary battery performance according to the present invention.
[0212] A person skilled in the art to which this invention pertains will be able to make various applications and modifications within the scope of this invention based on the above content.
Claims
Claim 1 A lithium secondary battery comprising: a positive electrode having a positive electrode composite layer including a positive electrode active material and an inorganic solid electrolyte formed on one or both sides of a positive electrode current collector; a negative electrode having a negative electrode composite layer including a negative electrode active material formed on one or both sides of a negative electrode current collector; a separator interposed between the positive electrode and the negative electrode; and a gel-type electrolyte, wherein the inorganic solid electrolyte is included in an amount of 0.5% to 2% by weight based on the total weight of the positive electrode composite layer and is uniformly distributed within the positive electrode composite layer. Claim 2 A lithium secondary battery according to claim 1, wherein when the anode composite layer is divided in half based on the thickness direction, the inorganic solid electrolyte is included in the upper layer at 40 to 60 weight% and the lower layer at 40 to 60 weight% based on the total weight of the inorganic solid electrolyte. Claim 3 A lithium secondary battery according to claim 2, wherein when the upper layer and the lower layer are each divided in half based on the thickness direction, the inorganic solid electrolyte is included in each layer at a weight% of 20 to 30% based on the total weight of the inorganic solid electrolyte. Claim 4 A lithium secondary battery according to claim 1, wherein 50% to 90% of the total surface area of the positive electrode active material is covered by the inorganic solid electrolyte. Claim 5 In claim 1, the above-mentioned inorganic solid electrolyte is an oxide-based solid electrolyte having a NASICON structure, in a lithium secondary battery. Claim 6 In claim 1, the lithium secondary battery wherein the inorganic solid electrolyte is an oxide-based solid electrolyte represented by the following chemical formula 1: [Chemical Formula 1]Li 1+x M' 2-x M x (PO4)3 In the above chemical formula 1, 0 <x<2 이고, M’는 Ti, Zr, Ge, Sn 및 Hf으로 이루어진 군에서 선택되는 하나 이상이고, M은 Cr, Al, Mg, Ga, Sc, Y, In, 및 La로 이루어진 군에서 선택되는 하나 이상이다. Claim 7 In claim 6, the oxide-based solid electrolyte is a lithium secondary battery in which the lithium aluminum titanium phosphate (LATP)-based compound is M' being Ti and M being Al. Claim 8 In claim 1, the loading amount of the anode composite layer is 400 mg / 25 cm 2 Up to 600 mg / 25 cm 2 lithium secondary battery. Claim 9 In claim 1, the gel-type electrolyte comprises i) a lithium salt, ii) a non-aqueous organic solvent, and iii) at least one polymerizable compound selected from the group consisting of polymerizable monomers, oligomers, and copolymers having polymerizable unsaturated functional groups, and at least some of the polymerizable unsaturated functional groups are a cured lithium secondary battery. Claim 10 A lithium secondary battery according to claim 9, wherein the polymerizable unsaturated functional group is one or more selected from the group consisting of vinyl groups, epoxy groups, allyl groups, and (meth)acrylic groups. Claim 11 In claim 9, the above-mentioned non-aqueous organic solvent is a carbonate-based organic solvent for a lithium secondary battery. Claim 12 A lithium secondary battery according to claim 9, wherein the gel-type electrolyte further comprises a polymerization initiator, and the polymerization initiator is a photoinitiator or a thermal initiator. Claim 13 A lithium secondary battery according to claim 12, wherein the polymerization initiator is included in an amount of 0.01 to 20 parts by weight based on 100 parts by weight of the polymerizable compound. Claim 14 A lithium secondary battery according to claim 9, wherein the gel-type electrolyte further comprises a functional additive, and the functional additive is one or more selected from the group consisting of sulfonate-based compounds, sulfite-based compounds, sulfone-based compounds, sulfate-based compounds, halogen-substituted carbonate-based compounds, nitrile-based compounds, cyclic carbonate-based compounds, phosphate-based compounds, borate-based compounds, and lithium salt-based compounds.
Citation Information
Patent Citations
Lithium secondary battery, and electrode for lithium secondary battery
JP2008117542A
Solid electrolytic material and all-solid battery arranged by use thereof
JP2015076324A