Electrode assambly and battery cell including the same

The electrode assembly with an insulating coating layer and protrusions addresses the issue of lithium ion precipitation by maintaining a safe N/P ratio, enhancing battery safety and capacity retention.

KR103046340B1Active Publication Date: 2026-11-10LG ENERGY SOLUTION LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020220136343
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-21
Filing Date
2022-10-21
Publication Date
2026-11-10
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

Existing electrode assemblies in secondary batteries face issues with lithium ion precipitation due to the reversal of the N/P ratio, leading to rapid deterioration in battery safety and capacity loss during high-rate charging and discharging.

Method used

An electrode assembly design featuring an anode with an insulating coating layer that includes protrusions towards the anode active material layer, covering a portion of the anode and minimizing the area where the N/P ratio can be reversed, while allowing lithium ions to move efficiently between the anode and cathode.

Benefits of technology

The design effectively prevents lithium ion precipitation by maintaining a safe N/P ratio, minimizing capacity loss, and ensuring stable battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112022111239915-PAT00002_ABST
    Figure 112022111239915-PAT00002_ABST
Patent Text Reader

Abstract

An electrode assembly according to one embodiment of the present invention comprises: an anode including an anode current collector and an anode active material layer located on the anode current collector; and a cathode including a cathode current collector and a cathode active material layer located on the cathode current collector, wherein the anode and the cathode are arranged in a direction in which the anode active material layer and the cathode active material layer face each other, and the anode includes an insulating coating layer covering from an end of the anode active material layer to at least a portion of the anode active material layer, and the insulating coating layer includes at least one protrusion protruding toward the center of the anode active material layer with respect to the end of the anode active material layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electrode assembly and a battery cell including the same, and more specifically, to an electrode assembly and a battery cell including the same that prevent lithium ion precipitation by preventing the reversal of the N / P ratio while minimizing capacity loss. Background Technology

[0002] With the increasing technological development and demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. In particular, secondary batteries are attracting significant interest as an energy source not only for mobile devices such as mobile phones, digital cameras, laptops, and wearable devices, but also for power devices such as electric bicycles, electric vehicles, and hybrid electric vehicles.

[0003] A secondary battery can be formed by inserting an electrode assembly, consisting of a positive electrode, a negative electrode, and a separator, into a case and then sealing it. Here, the electrode for the secondary battery, such as the positive or negative electrode, may have an active material layer and a non-active portion formed on a current collector where the active material layer is not formed. The active material layer may be formed by coating an active material slurry. Additionally, the active material layer may include a rolling process to increase adhesion to the electrode current collector and increase the active material capacity density. The problem to be solved

[0004] The problem to be solved by the present invention is to provide an electrode assembly that prevents lithium ion precipitation by preventing the reversal of the N / P ratio while minimizing capacity loss, and a battery cell including the same.

[0005] The problems that the present invention aims to solve are not limited to those described above, and problems not mentioned will be clearly understood by those skilled in the art from this specification and the attached drawings. means of solving the problem

[0006] An electrode assembly according to one embodiment of the present invention comprises: an anode including an anode current collector and an anode active material layer located on the anode current collector; and a cathode including a cathode current collector and a cathode active material layer located on the cathode current collector, wherein the anode and the cathode are arranged in a direction in which the anode active material layer and the cathode active material layer face each other, and the anode includes an insulating coating layer covering from an end of the anode active material layer to at least a portion of the anode active material layer, and the insulating coating layer includes at least one protrusion protruding toward the center of the anode active material layer with respect to the end of the anode active material layer.

[0007] The above positive current collector may include a first non-positive portion where the positive active material layer is not located, and the above negative current collector may include a second non-positive portion where the negative active material layer is not located.

[0008] The insulating coating layer may extend to at least a portion of the first unused portion based on the boundary line of the first unused portion and the positive active material layer.

[0009] At this time, the insulating coating layer may cover the first unused portion in a range of 10% to 50% based on the total area of ​​the first unused portion, and the ratio of the positive active material layer to the area covering the first unused portion may be an area ratio of 2:1 to 1:2.

[0010] The end portion of the positive active material layer may become thinner than the thickness of the center portion of the positive active material layer as it moves toward the first unoccupied portion, and the end portion of the negative active material layer may become thinner than the thickness of the center portion of the negative active material layer as it moves toward the second unoccupied portion.

[0011] The length of the above protrusion may be the length from the anode active material layer to the region facing the region having a thickness of 0.9 or more to 1.0 or less relative to the thickness of the center of the cathode active material layer, based on the boundary line between the anode active material layer and the first unoccupied region. A part of the anode active material layer may have the same thickness as the thickness of the center of the anode active material layer.

[0012] The width of the above protrusion may be a range of absolute values ​​obtained by dividing a range of 20% to 50% relative to the width of the above positive active material layer by the number of protrusions.

[0013] The length of the first unworn portion may be the same as or greater than the length of the second unworn portion.

[0014] Two or more of the above protrusions may be formed and may be spaced apart from each other.

[0015] At this time, the distance between the protrusions may be equal to or smaller than the width of the protrusions.

[0016] The above insulating coating layer may be made of a material that prevents lithium ions from passing through.

[0017] A separator may be located between the anode and the cathode.

[0018] A battery cell according to another embodiment of the present invention includes the electrode assembly described above. Effects of the invention

[0019] According to the embodiments, the present invention relates to an electrode assembly comprising an insulating coating layer that covers an anode from an end portion of the anode active material layer to at least a portion of the anode active material layer, and a battery cell comprising the same, wherein the insulating coating layer comprises at least one protrusion that protrudes toward the center of the anode active material layer relative to the end portion of the anode active material layer, thereby preventing the precipitation of lithium ions by preventing the reversal of the N / P ratio while minimizing capacity loss.

[0020] The effects of the present invention are not limited to the effects described above, and unmentioned effects will be clearly understood by those skilled in the art from this specification and the accompanying drawings. Brief explanation of the drawing

[0021] Figure 1 is a cross-sectional view showing a conventional electrode assembly. FIG. 2 is a cross-sectional view showing a part of an electrode assembly according to one embodiment of the present invention. Figure 3 is a cross-sectional view showing the anode included in the electrode assembly of Figure 2. Figure 4 is a top view of the anode of Figure 3. Specific details for implementing the invention

[0022] Hereinafter, various embodiments of the present invention will be described in detail with reference to the attached drawings so that those skilled in the art can easily implement the present invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0023] To clearly explain the present invention, parts unrelated to the explanation have been omitted, and the same reference numerals are used for identical or similar components throughout the specification.

[0024] Furthermore, the size and thickness of each component shown in the drawings are depicted arbitrarily for convenience of explanation, and thus the present invention is not necessarily limited to what is illustrated. Thicknesses have been enlarged in the drawings to clearly represent various layers and regions. Additionally, for convenience of explanation, the thickness of some layers and regions has been exaggerated in the drawings.

[0025] Furthermore, throughout the specification, when a part is described as “comprising” a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0026] Additionally, throughout the specification, "planar" means when the subject part is viewed from above, and "cross-sectional" means when the cross-section obtained by vertically cutting the subject part is viewed from the side.

[0027] Hereinafter, an electrode assembly according to an embodiment of the present invention will be described. However, the description herein will be based on one positive electrode and one negative electrode among the electrode assemblies; the electrode assembly is not necessarily limited thereto, and the same or similar content may be described even in cases where a plurality of positive electrodes and a plurality of negative electrodes are arranged in an alternating manner.

[0028] Figure 1 is a cross-sectional view showing a conventional electrode assembly.

[0029] Referring to FIG. 1, a conventional electrode assembly includes a positive electrode (10) and a negative electrode (20), wherein the positive electrode (10) has a positive active material layer (15) located on a positive current collector (11) and the negative electrode (20) has a negative active material layer (25) located on a negative current collector (21).

[0030] Generally, for the positive electrode (10) and the negative electrode (20), the N / P ratio is measured as an indicator of the safety and capacity of the battery. Here, the N / P ratio is the value obtained by dividing the value obtained by subtracting the negative irreversible capacity from the negative electrode charging capacity by the value obtained by subtracting the larger value between the positive irreversible capacity and the negative irreversible capacity from the positive electrode charging capacity.

[0031] At this time, since the N / P ratio has a significant impact on safety and capacity, it should generally be 100 or higher. In other words, if the N / P ratio is less than 100, it can be said that the N / P ratio is reversed, and lithium ions are prone to precipitating on the surface of the negative electrode (20) during charging and discharging, and there is a problem that the safety of the battery deteriorates rapidly during high-rate charging and discharging.

[0032] Accordingly, for the positive electrode (10) and the negative electrode (20), it is necessary to design the size, position, shape, etc. of the positive electrode (10) and the negative electrode (20) so that the N / P ratio is 100 or more.

[0033] Referring to FIG. 1, lithium ions move from the positive active material layer (15) to the negative active material layer (25). At this time, generally, due to the flowability of the positive slurry or negative slurry in the process, the ends of the positive active material layer (15) and the negative active material layer (25) gradually become thinner.

[0034] At this time, due to differences in position and / or thickness between the end of the positive active material layer (15) and the end of the negative active material layer (25), a problem occurs in which the N / P ratio is reversed at the position where the end of the positive active material layer (15) and the end of the negative active material layer (25) face each other. In particular, if the degree to which the end of the negative active material layer (25) becomes thinner is greater than the degree to which the end of the positive active material layer (15) becomes thinner, this problem is more likely to occur.

[0035] In this case, when the N / P ratio is reversed, lithium ions cannot completely move from the positive active material layer (15) to the negative active material layer (25), and some of the lithium ions are deposited on the surface of the negative electrode (20).

[0036] Accordingly, unlike conventional electrode assemblies, there is a need to develop an electrode assembly that prevents lithium ion precipitation by preventing the reversal of the N / P ratio while minimizing capacity loss, and a battery cell containing the same.

[0038] FIG. 2 is a cross-sectional view showing a part of an electrode assembly according to one embodiment of the present invention.

[0039] Referring to FIG. 2, an electrode assembly according to one embodiment of the present invention comprises: a positive electrode (100) comprising a positive current collector (110) and a positive active material layer (150) located on the positive current collector (110); and a negative electrode (200) comprising a negative current collector (210) and a negative active material layer (250) located on the negative current collector (210).

[0040] More specifically, the positive electrode (100) and the negative electrode (200) may be arranged such that the positive active material layer (150) and the negative active material layer (250) face each other. Additionally, although not shown in FIG. 2, a separator (not shown) may be positioned between the positive electrode (100) and the negative electrode (200). More specifically, the separator (not shown) may be positioned between the positive active material layer (150) and the negative active material layer (250) that face each other.

[0041] The positive current collector (110) is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used.

[0042] The positive active material layer (150) can be manufactured in a form in which a positive slurry containing a positive active material is attached or coated on a positive current collector (110), and the positive slurry may further include a conductive material and a polymer material in addition to the positive active material.

[0043] The above positive active material may include, for example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2); lithium manganese oxide; lithium copper oxide (Li2CuO2); vanadium oxide; Ni-site type lithium nickel oxide; lithium manganese complex oxide; spinel structure lithium manganese complex oxide; LiMn2O4 in which part of the chemical formula Li is substituted with alkaline earth metal ions; disulfide compounds; Fe2(MoO4)3, etc.

[0044] The negative current collector (210) is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used.

[0045] The negative electrode active material layer (250) can be manufactured in a form in which a negative electrode slurry containing a negative electrode active material is attached or coated on a negative electrode current collector (210), and the negative electrode slurry may further include a conductive material and a polymer material in addition to the negative electrode active material.

[0046] The above negative electrode active material may be a negative electrode active material for lithium secondary batteries that is conventional in the industry, and for example, materials such as lithium metal, lithium alloy, petroleum coke, activated carbon, graphite, silicon, tin, metal oxide, or other carbons may be used.

[0047] The above separator (not shown) separates the positive electrode (100) and the negative electrode (200) and provides a passage for the movement of lithium ions. It can be used without special limitations as long as it is used as a separator in a lithium secondary battery, and it is particularly desirable that it has low resistance to the movement of ions in the electrolyte and excellent electrolyte retention capacity.

[0049] Referring to FIG. 2, the positive current collector (110) may include a first non-positive portion (110a) where the positive active material layer (150) is not located, and the negative current collector (210) may include a second non-positive portion (210a) where the negative active material layer (250) is not located. Here, a positive tab (not shown) may be attached to a part of the first non-positive portion (110a), and a negative tab (not shown) may be attached to a part of the second non-positive portion (210a). Accordingly, the positive (100) and the negative (200) may be electrically connected to different positive (100) or negative (200) and electrically connected to external components through the positive tab (not shown) and the negative tab (not shown).

[0051] More specifically, the length of the first unoccupied portion (110a) may be equal to or greater than the length of the second unoccupied portion (210a). In other words, the distance between the end of the positive active material layer (150) and the end of the positive current collector (110) may be equal to or greater than the distance between the end of the negative active material layer (250) and the end of the negative current collector (210). That is, the end of the negative active material layer (250) is located further outward than the end of the positive active material layer (150), so that the area of ​​the negative active material layer (250) may be larger than the area of ​​the positive active material layer (150).

[0052] Accordingly, in the electrode assembly according to the present embodiment, the reaction area of ​​the negative active material layer (250) facing the end of the positive active material layer (150) is relatively large, so that lithium ions can easily move from the end of the positive active material layer (150) to the negative active material layer (250). That is, the present embodiment can minimize the risk of the N / P ratio being reversed and can also prevent lithium ion precipitation.

[0054] FIG. 3 is a cross-sectional view showing the anode included in the electrode assembly of FIG. 2. FIG. 4 is a top view of the anode of FIG. 3.

[0055] Referring to FIGS. 3 and 4, the anode (100) includes an insulating coating layer (115) that covers at least a portion of the anode active material layer (150) from the end of the anode active material layer (150). In other words, the insulating coating layer (115) can cover at least a portion of the anode active material layer (150) based on the boundary line between the first uncoated portion (110a) and the anode active material layer (150).

[0056] Here, the insulating coating layer (115) may be made of a material that prevents lithium ions from passing through. For example, the insulating coating layer (115) may be made of a material such as PVDF (Polyvinylidene fluoride), a mixture of PVDF and ceramic, or a mixture of ceramic and SBR (Styrene Butadiene Rubber). However, it is not limited to this, and any material that prevents lithium ions from passing through may be included in this embodiment.

[0057] Accordingly, the electrode assembly according to the present embodiment can control the area of ​​the positive active material layer (150) facing the end of the negative active material layer (250) through an insulating coating layer (115) that covers a part of the positive active material layer (150). That is, the reaction area of ​​the negative active material layer (250) facing the end of the positive active material layer (150) can be relatively controlled to prevent the N / P ratio from being reversed.

[0058] Additionally, the insulating coating layer (115) may extend to at least a portion of the first unused portion (110a) based on the boundary line between the first unused portion (110a) and the positive active material layer (150). In other words, the insulating coating layer (115) may extend toward the first unused portion (110a) and the positive active material layer (150), respectively, based on the boundary line between the first unused portion (110a) and the positive active material layer (150).

[0059] At this time, the insulating coating layer (115) can cover the first unused portion (110a) in a range (S1) of 10% to 50% based on the total area (S) of the first unused portion (110a).

[0060] If the insulating coating layer (115) covers too much of the first unused portion (110a) outside the above range, the insulating coating layer (115) may be formed in the area where the tab is attached, which may affect conductivity, and if it is too small, the boundary line between the positive active material layer (150) and the first unused portion (110a) may be exposed, which is undesirable.

[0061] Additionally, if the shape covers a part of the positive active material layer (150) and a part of the first non-positive portion (110a), the area ratio is not limited, but for example, the ratio covering the positive active material layer (150) and the first non-positive portion (110a) may be an area ratio (S2:S1) of 2:1 to 1:2.

[0062] If the positive active material layer (150) is covered too much, the capacity loss may increase, and if it is covered too little, the effect of preventing N / P ratio reversal cannot be sufficiently obtained. Therefore, it is more preferable for the insulating coating layer (115) to cover the positive active material layer (150) and the first unprotected portion (110a) with the above-mentioned area ratio.

[0063] Accordingly, in the electrode assembly according to the present embodiment, the insulating coating layer (115) covers the boundary line between the first uninsulated portion (110a) and the positive active material layer (150), so the effect of preventing the reversal of the N / P ratio by the insulating coating layer (115) can be further enhanced.

[0065] Referring to FIGS. 3 and 4, the insulating coating layer (115) includes at least one protrusion that protrudes toward the center of the positive active material layer (150) with respect to the end of the positive active material layer (150). For example, the at least one protrusion may have a rectangular shape as shown in FIG. 4. However, the shape of the at least one protrusion is not limited thereto, and any shape that can cover the positive active material layer (150) while being spaced apart from each other may be included in this embodiment.

[0066] Accordingly, the electrode assembly according to the present embodiment can control the area of ​​the positive active material layer (150) facing the end of the negative active material layer (250) through the size and / or shape of the protrusion included in the insulating coating layer (115). That is, by controlling the reaction area of ​​the negative active material layer (250) facing the end of the positive active material layer (150), it is possible to prevent the N / P ratio from being reversed.

[0067]

[0068] Referring to FIG. 2, the end portion of the positive active material layer (150) becomes thinner than the thickness of the center portion of the positive active material layer (150) as it moves toward the first unoccupied portion (110a), and the end portion of the negative active material layer (250) becomes thinner than the thickness of the center portion of the negative active material layer (250) as it moves toward the second unoccupied portion (210a). More specifically, as the positive slurry is applied to the positive current collector (110), the positive active material layer (150) located at the boundary between the positive active material layer (150) and the first unoccupied portion (110a) may gradually become thinner due to the flowability of the positive slurry. This can be explained in the same way for the negative electrode (200).

[0069] Additionally, in the positive active material layer (150), the remainder excluding both ends of the positive active material layer (150) may refer to the center of the positive active material layer (150). Here, the center of the positive active material layer (150) may have a flat thickness, unlike the ends of the positive active material layer (150). Here, a flat thickness may mean having the same or similar thickness. This can be explained in the same way for the negative electrode (200).

[0070] Referring to FIGS. 2 and FIGS. 4, the protrusion may extend from the end of the positive active material layer (150) to a part of the positive active material layer (150). Here, the part of the positive active material layer (150) may have the same thickness as the center of the positive active material layer (150).

[0071] Here, the length (d1) of the protrusion can be determined based on the thickness of the negative active material layer (250) facing the positive active material layer (150).

[0072] Generally, the electrode assembly is designed such that the N / P ratio is 110 or higher based on a flat portion, such as the center of the positive active material layer (150), and a flat portion, such as the center of the negative active material layer (250), and this value can be referred to as the pre-designed N / P ratio. At this time, the thickness of the negative active material layer (250) facing the flat portion, such as the center of the positive active material layer (150), relative to the thickness of the center of the negative active material layer (250), must satisfy 100 / a (A = pre-designed N / P ratio) or higher. For example, when the pre-designed N / P ratio is 110, the thickness of the negative active material layer (250) facing the flat portion, such as the center of the positive active material layer (150), relative to the thickness of the center of the negative active material layer (250), must be approximately 0.9 or higher.

[0073] Accordingly, if the thickness of the negative active material layer (250) facing the positive active material layer (150) is 0.9 or more compared to the thickness of the center of the negative active material layer (250), the N / P ratio in that part can be seen as having a value of 100 or more.

[0074] More specifically, referring to FIGS. 3 and 4, the length (d1) of the protrusion may be the length from the positive active material layer (150) to the region facing the region having a thickness of 0.9 or more to 1.0 or less relative to the thickness of the center of the negative active material layer (250), based on the boundary line between the positive active material layer (150) and the first unoccupied portion (110a).

[0075] Accordingly, the length (d1) of the above-mentioned protrusion is included in the range described above, so that the N / P ratio can have a value of 100 or more, and lithium ion precipitation can also be prevented.

[0076] In contrast, if the length (d1) of the protrusion is the length from the positive active material layer (150) to the region facing the region having a thickness of less than 0.9 relative to the thickness of the center of the negative active material layer (250) among the negative active material layers (250), based on the boundary line between the positive active material layer (150) and the first unoccupied portion (110a), the N / P ratio may have a value of less than 100. That is, in this case, the N / P ratio may be reversed, and a problem may occur in which lithium ions are easily precipitated.

[0077] Additionally, the width (d3) of the protrusion may be a range of absolute values ​​obtained by dividing the range of 20% to 50% relative to the width of the positive active material layer (150), that is, relative to the direction of the boundary surface between the positive active material layer (150) and the first non-positive part (110a), by the number of protrusions.

[0078] For example, when two protrusions are formed, the width (d3) of each protrusion may be 10% (20 / 2) to 25% (50 / 2) of the width of the positive active material layer (150), and when five protrusions are formed as shown in FIG. 4, the width (d3) of each protrusion may be in the range of 4% (20 / 5) to 10% (50 / 5) of the width of the positive active material layer (150).

[0079] In addition, in the electrode assembly according to the present embodiment, an insulating coating layer (115) is located on the positive electrode (100), so that lithium ions moving from the positive electrode active material layer (150) toward the negative electrode active material layer (250) can move to the positive electrode active material layer (150) where the insulating coating layer (115) is not formed, as shown in FIG. 2, and move outside the positive electrode active material layer (150).

[0080] However, in this case, as the travel distance of lithium ions is extended by the insulating coating layer (115), some of the lithium ions in the positive active material layer (150) may not participate in the reaction during charging and discharging, and there may be a problem of capacity loss.

[0081] In consideration of this, the electrode assembly according to the present embodiment may have two or more protrusions formed in the insulating coating layer (115) as shown in FIG. 4, and these may be spaced apart from each other. In other words, by forming two or more protrusions, the positive active material layer (150) located between the protrusions may be exposed toward the negative active material layer (250).

[0082] Accordingly, some of the lithium ions in the positive active material layer (150) can move to the negative active material layer (250) through the positive active material layer (150) exposed between the at least one protrusion of the insulating coating layer (115).

[0083] That is, the electrode assembly according to the present embodiment can prevent the reversal of the N / P ratio by covering a portion of the positive active material layer (150) with an insulating coating layer (115), while exposing a portion of the positive active material layer (150) toward the negative active material layer (250) between the at least one protrusion of the insulating coating layer (115), thereby minimizing the capacity loss caused by the insulating coating layer (115).

[0084] Also, referring to FIG. 4, in the insulating coating layer (115), the distance (d2) between the protrusions may be equal to or smaller than the width (d3) of the protrusions.

[0085] For example, the distance (d2) between the at least one protrusion may be greater than 2 / 3 * the width (d3) of the protrusion or less than the width (d3) of the protrusion. This is calculated by taking into account the fact that the lithium ions contained in the positive active material layer (150) where the insulating coating layer (115) is located can move to the left, right, and downward directions, and that the lithium ions can move from both sides.

[0086] However, it is not limited thereto, and the distance (d2) at least one protrusion is spaced apart from each other may be included in this embodiment as long as it is sufficient to maximize the effect of preventing the reversal of the N / P ratio of the insulating coating layer (115) while minimizing the capacity loss caused by the insulating coating layer (115).

[0087] Accordingly, the distance (d2) at least one protrusion is spaced apart from each other is included in the range described above, so that the N / P ratio is prevented by the insulating coating layer (115), while the capacity loss caused by the insulating coating layer (115) can be minimized.

[0088] In contrast, if the distance (d2) between the at least one protrusion is excessively small, the area of ​​the positive active material layer (150) exposed toward the negative active material layer (250) is excessively reduced, and the capacity loss due to the insulating coating layer (115) may increase. Additionally, if the distance (d2) between the at least one protrusion is excessively large, the area of ​​the positive active material layer (150) covered by the insulating coating layer (115) is excessively reduced, and the effect of preventing the reversal of the N / P ratio of the insulating coating layer (115) may be reduced.

[0090] Meanwhile, a battery cell according to another embodiment of the present invention includes the electrode assembly described above. Additionally, the battery cell may be included in a battery module in a stacked form. Furthermore, one or more of the battery modules may be packaged in a pack case to form a battery pack.

[0091] The battery module and battery pack containing the same described above can be applied to various devices. Such devices may be applied to means of transportation such as electric bicycles, electric vehicles, and hybrid vehicles, but the present invention is not limited thereto and can be applied to various devices capable of using the battery module and battery pack containing the same, and this also falls within the scope of the rights of the present invention.

[0092] Although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims also fall within the scope of the present invention. Explanation of the symbols

[0093] 100: Anode 110: Positive current collector 110a: First thumb 115: Insulating coating layer 150: Positive active material layer 210: Cathode current collector 210a: Second thumbless part 250: Cathode active material layer 200: Cathode

Claims

Claim 1 A positive electrode comprising a positive current collector and a positive active material layer located on the positive current collector; The cathode comprises a cathode current collector and a cathode active material layer located on the cathode current collector, wherein the anode and the cathode are arranged in a direction in which the anode active material layer and the cathode active material layer face each other, the anode comprises an insulating coating layer covering from the end of the anode active material layer to at least a portion of the anode active material layer, the insulating coating layer comprises at least one protrusion protruding toward the center of the anode active material layer with respect to the end of the anode active material layer, the anode current collector comprises a first non-existent portion where the anode active material layer is not located, the cathode current collector comprises a second non-existent portion where the cathode active material layer is not located, the insulating coating layer extends to at least a portion of the first non-existent portion with respect to the boundary line between the first non-existent portion and the anode active material layer, the ratio of the insulating coating layer covering the anode active material layer and the first non-existent portion is an area ratio of 2:1 to 1:2, the end of the anode active material layer becomes thinner than the thickness of the center of the anode active material layer as it moves toward the first non-existent portion, and the cathode active material layer An electrode assembly comprising: an end portion that becomes thinner than the thickness of the center of the cathode active material layer as it moves toward the second unoccupied portion; a protrusion whose length is, based on the boundary line between the positive active material layer and the first unoccupied portion, extends from the positive active material layer to a region facing the region having a thickness of 0.9 or more to 1.0 or less relative to the thickness of the center of the negative active material layer among the positive active material layers; and an insulating coating layer made of a material that prevents lithium ions from passing through, and comprising one or more of polyvinylidene fluoride (PVDF), a mixture of PVDF and ceramic, and a mixture of ceramic and styrene-butadiene rubber (SBR). Claim 2 delete Claim 3 delete Claim 4 In claim 1, the insulating coating layer covers the first unused portion in a range of 10% to 50% based on the total area of ​​the first unused portion, forming an electrode assembly. Claim 5 delete Claim 6 delete Claim 7 delete Claim 8 In claim 1, the electrode assembly having a portion of the positive active material layer having the same thickness as the center of the positive active material layer. Claim 9 An electrode assembly according to claim 1, wherein the width of the protrusion is a range of absolute values ​​obtained by dividing a range of 20% to 50% relative to the width of the positive active material layer by the number of protrusions. Claim 10 In claim 1, the electrode assembly in which the length of the first uninhibited portion is equal to or greater than the length of the second uninhibited portion. Claim 11 In claim 1, the electrode assembly in which two or more of the above-mentioned protrusions are formed and are spaced apart from each other. Claim 12 In claim 11, the electrode assembly in which the distance between the protrusions is equal to or smaller than the width of the protrusions. Claim 13 delete Claim 14 An electrode assembly having a separator located between the anode and the cathode in claim 1. Claim 15 A battery cell comprising an electrode assembly according to claim 1.

Citation Information

Patent Citations

  • Cylindrical nonaqueous electrolyte secondary battery

    JP2007080795A

  • Secondary batteries

    JP6621765B2