A cylinderical secondary battery and a method for preparing the same
The cylindrical secondary battery design addresses high resistance and heat generation issues by eliminating the negative electrode active material layer and using a high-loading positive electrode, achieving high energy density and safety with a tab-less structure.
Patent Information
- Application Number
- KR1020230190501
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-23
- Filing Date
- 2023-12-22
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-12-22
AI Technical Summary
Cylindrical secondary batteries face issues such as high resistance, excessive heat generation, and poor current collection efficiency due to current concentration in strip-shaped electrode tabs, necessitating the development of high-energy-density batteries at a lower cost and with improved stability.
A cylindrical secondary battery design that includes a negative electrode without a negative electrode active material layer, utilizing a positive electrode with a high-loading amount of positive active material and a tab-less structure, along with a specific manufacturing process that omits the application of pressure to activate the battery.
The design achieves high energy density, reduces heat generation, and enhances safety in large cylindrical batteries while maintaining cost-effectiveness by utilizing a negative electrode without an active material layer and a tab-less structure.
Smart Images

Figure 112023144921583-PAT00004_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a cylindrical secondary battery and a method for manufacturing the same. Specifically, the present invention relates to a cylindrical secondary battery not having a negative electrode active material layer and a method for manufacturing the same.
[0002] This application is a priority claim application for Korean Patent Application No. 10-2022-0182927 filed on December 23, 2022, and all contents disclosed in the specification of said application are incorporated into this application by reference. Background Technology
[0004] With the technological advancement of electric vehicles, portable electronic devices, and the like, the demand for lithium-ion batteries as an energy source is rapidly increasing.
[0005] A lithium secondary battery is constructed by having a structure in which an electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive and negative electrodes is stacked or wound, and the electrode assembly is embedded in a battery case and an electrolyte is injected therein. The lithium secondary battery produces electrical energy through oxidation and reduction reactions when lithium ions are inserted into and extracted from the positive and negative electrodes.
[0006] With the recent surge in the price of raw materials for lithium secondary batteries, consumers are demanding secondary batteries that offer high performance at a low price. For example, among cathode active materials, lithium iron phosphate (LFP) is about 30% cheaper than nickel cobalt manganese oxide (NCM), but it has the disadvantage of having about 20% lower energy density. In other words, when using inexpensive LFP, it is necessary to design a system that increases energy density.
[0007] Meanwhile, lithium secondary batteries can be classified into cylindrical, prismatic, and pouch types depending on the shape of the battery case. Among these, the cylindrical battery is constructed by housing a jelly-roll type electrode assembly—manufactured by sequentially stacking sheet-shaped positive plates, separators, and negative plates and then winding them in one direction—into a cylindrical battery can, and then sealing the can by covering the top with a cap plate. The positive plate and negative plate are respectively equipped with strip-shaped positive and negative tabs, and these tabs are connected to electrode terminals to be electrically connected to an external power source. For reference, the positive electrode terminal is the cap plate, and the negative electrode terminal is the battery can.
[0008] However, cylindrical secondary batteries have problems such as high resistance, excessive heat generation, and poor current collection efficiency due to current concentration in the strip-shaped electrode tabs. Furthermore, with the recent advancement of electric vehicle technology and the increasing demand for high-capacity and high-energy-density batteries, there is a need to develop cylindrical batteries that offer high performance at a low price. The problem to be solved
[0010] Accordingly, the problem that the present invention aims to solve is to resolve the aforementioned issues and to provide a cylindrical secondary battery having high energy density per unit volume and improved cell performance, and a method for manufacturing the same.
[0011] Another objective of the present invention is to provide a cylindrical secondary battery with ensured stability and a method for manufacturing the same. means of solving the problem
[0013] The inventors have discovered that the above problem can be solved through the following cylindrical secondary battery and a method for manufacturing the same.
[0014] According to the first embodiment,
[0015] An electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; a battery can in which the electrode assembly is housed; and a sealing body for sealing an open end of the battery can.
[0016] The above positive electrode comprises a positive current collector and a positive active material layer comprising a positive active material on at least one surface of the positive current collector, and
[0017] The above-mentioned cathode relates to a cylindrical secondary battery that includes a cathode current collector but does not have a cathode active material layer.
[0018] According to the second embodiment, in the first embodiment,
[0019] The present invention relates to a cylindrical secondary battery characterized in that the above-mentioned negative electrode consists solely of a negative current collector.
[0020] According to the third embodiment, in the first embodiment or the second embodiment,
[0021] The present invention relates to a cylindrical secondary battery characterized in that the above-mentioned positive electrode active material comprises lithium iron phosphate oxide (LFP), lithium manganese iron phosphate (LMFP), lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese aluminum oxide (NCMA), lithium manganese oxide (LMO), overlithiated oxide (OLO), cobalt-free oxide, nickel-free oxide, manganese-free oxide, manganese-rich oxide, or a mixture thereof.
[0022] According to the fourth embodiment, in any one of the first to third embodiments,
[0023] The present invention relates to a cylindrical secondary battery characterized in that the positive electrode active material is included in an amount of 80 to 99 parts by mass relative to 100 parts by weight of the entire positive electrode active material layer.
[0024] According to the fifth embodiment, in any one of the first to fourth embodiments,
[0025] The present invention relates to a cylindrical secondary battery characterized in that the loading amount of the anode is 110 to 120% based on the loading amount of the anode of the cylindrical secondary battery having a negative electrode active material layer.
[0027] According to the 6th embodiment, in any one of the 1st to 5th embodiments,
[0028] The loading amount of the above anode is 500 to 600 mg / cm² 2 This relates to a cylindrical secondary battery characterized by being within the range of
[0029] According to the seventh embodiment, in any one of the first to sixth embodiments,
[0030] A cylindrical secondary battery characterized in that the thickness of the anode is 110 to 120% based on the thickness of the anode of a cylindrical secondary battery having a negative electrode active material layer.
[0031] According to the eighth embodiment, in any one of the first to seventh embodiments,
[0032] The present invention relates to a cylindrical secondary battery characterized in that the thickness of the anode is in the range of 190 to 220 μm.
[0033] According to the ninth embodiment, in any one of the first to eighth embodiments,
[0034] The present invention relates to a cylindrical secondary battery characterized by having a capacity of 140 to 180% increased based on the capacity of a cylindrical secondary battery having a negative electrode active material layer.
[0035] According to the 10th embodiment, in any one of the 1st to 9th embodiments,
[0036] The above-described cylindrical secondary battery relates to a cylindrical secondary battery characterized by having an energy density per unit volume of 850 Wh / L or more.
[0037] According to the 11th embodiment, in any one of the 1st to 10th embodiments,
[0038] A cylindrical secondary battery characterized in that the above-mentioned negative current collector has the structure of 1) or 2) below:
[0039] 1) A structure comprising a porous region and a non-porous region, wherein at least a portion of the porous region is in contact with at least one surface of the separation membrane;
[0040] 2) A multilayer structure comprising at least one porous sheet and at least one metal sheet.
[0041] According to the 12th embodiment, in any one of the 1st to 11th embodiments,
[0042] The above-described cylindrical secondary battery relates to a cylindrical secondary battery characterized by a form factor ratio of 0.25 or higher.
[0043] According to the 13th embodiment, in any one of the 1st to 12th embodiments,
[0044] The present invention relates to a cylindrical secondary battery characterized by the above-mentioned cylindrical secondary battery being 18650 cells, 21700 cells, 46110 cells, 48750 cells, 48110 cells, 48800 cells, or 46800 cells.
[0045] According to the 14th embodiment, in any one of the 1st to 13th embodiments,
[0046] The present invention relates to a cylindrical secondary battery characterized by the fact that the above-described cylindrical secondary battery is a tab-less battery structure that does not include an electrode tab.
[0047] According to the 15th embodiment, in any one of the 1st to 14th embodiments,
[0048] The above-described cylindrical secondary battery relates to a cylindrical secondary battery characterized by including a liquid electrolyte.
[0049] According to the 16th embodiment,
[0050] Step of preparing the anode, cathode, and separator;
[0051] A step of forming an electrode-separator laminate by stacking the separator at least once so that the separator is interposed between the anode and the cathode;
[0052] A step of forming a jelly roll type electrode assembly by winding the above electrode-separator laminate in one direction;
[0053] A step of housing the electrode assembly in a can and injecting an electrolyte into the can housing the electrode assembly;
[0054] A step of manufacturing a battery by sealing the open end of the above can; and
[0055] The step of activating the battery under conditions of room temperature and atmospheric pressure; comprising
[0056] The above positive electrode comprises a positive current collector and a positive active material layer comprising a positive active material on at least one surface of the positive current collector, and
[0057] The present invention relates to a method for manufacturing a cylindrical secondary battery in which the above-mentioned cathode includes a cathode current collector but does not have a cathode active material layer. Effects of the invention
[0059] The cylindrical secondary battery according to the present invention can increase the energy density of the secondary battery by including a negative electrode that does not have a negative electrode active material layer.
[0060] The present invention is economical because it can exhibit a high energy density per unit volume even when a relatively low-energy-density and inexpensive cathode active material is applied to the cathode.
[0061] In addition, the present invention can effectively reduce heat generation inside a cylindrical secondary battery and can achieve excellent safety even in large cylindrical secondary batteries with increased volume.
[0062] The method for manufacturing a cylindrical secondary battery according to the present invention has the advantage of being convenient in process because the step of applying pressure to activate the secondary battery can be omitted. Brief explanation of the drawing
[0064] The following drawings attached to this specification illustrate preferred embodiments of the present invention and serve to further enhance understanding of the technical concept of the present invention together with the aforementioned description; therefore, the present invention should not be interpreted as being limited only to the matters described in such drawings. FIG. 1 is a drawing showing the stacked state of an electrode assembly provided in a cylindrical secondary battery according to one embodiment of the present invention before winding. FIG. 2 is a cross-sectional view showing the structure of a cylindrical battery with a tabless structure according to one embodiment of the present invention. FIG. 3 shows a cross-sectional view of a cylindrical battery with a tabless structure according to another embodiment of the present invention. FIG. 4 is a diagram showing the structure of a jelly roll type electrode assembly provided in a cylindrical secondary battery according to one embodiment of the present invention. FIG. 5 shows the results of the initial charge-discharge test of the cylindrical secondary batteries manufactured in Examples 1 and 2 and Comparative Example 1 of the present invention. Figure 6 shows the results of measuring the lifespan and Coulomb efficiency of cylindrical secondary batteries manufactured in Examples 1 and 2 and Comparative Example 1 of the present invention. Figure 7 shows the results of the Hot box safety evaluation of the cylindrical secondary battery manufactured in Example 1 of the present invention. Specific details for implementing the invention
[0065] The present invention will be described in detail below. Prior to this, terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings. Instead, based on the principle that the inventor can appropriately define the concepts of terms to best describe their invention, they should be interpreted in a meaning and concept consistent with the technical spirit of the present invention. Therefore, the configurations described in the embodiments of this specification are merely one preferred embodiment of the present invention and do not represent all aspects of the technical spirit of the present invention. It should be understood that various equivalents and modifications capable of replacing them may exist at the time of filing this application.
[0067] Throughout this specification, when a part is described as "comprising" or "having" a certain component, unless specifically stated otherwise, this means that it does not exclude other components but may additionally include or have other components.
[0068] Throughout this specification, the description “A and / or B” means “A or B or both.”
[0070] As a result of repeated research to develop an excellent large cylindrical battery, the inventors discovered that by including a negative electrode without a negative electrode active material layer, the safety of the large cylindrical battery can be ensured and cell performance improved with high energy density, thereby completing the present invention.
[0072] A cylindrical secondary battery according to one aspect of the present invention is,
[0073] An electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; a battery can in which the electrode assembly is housed; and a sealing body for sealing an open end of the battery can.
[0074] The above positive electrode comprises a positive current collector and a positive active material layer comprising a positive active material on at least one surface of the positive current collector, and
[0075] The above cathode includes a cathode current collector but does not have a cathode active material layer.
[0077] electrode assembly
[0078] The electrode assembly comprises an anode, a cathode, and a separator interposed between the anode and the cathode. The electrode assembly may be a jelly-roll type having a structure wound in one direction.
[0079] FIG. 1 illustrates a pre-winding stacked structure of an electrode assembly provided in a cylindrical secondary battery according to one embodiment of the present invention. Referring to FIG. 1, an electrode assembly (A) provided in a cylindrical secondary battery according to one embodiment of the present invention can be manufactured by winding an electrode-separator stack formed by sequentially stacking a separator (12), a positive electrode (10), a separator (12), and a negative electrode (11) at least once in one direction (X).
[0080] Specifically, FIG. 4 is a diagram showing the structure of a jelly roll type electrode assembly provided in a cylindrical secondary battery according to one embodiment of the present invention. Referring to FIG. 5, a separator (12), a positive electrode (10), a separator (12), and a negative electrode (11) are sequentially stacked, and the positive electrode (10) has a positive active material layer (10b) located on both sides of a positive current collector (10a), and the negative electrode (11) is composed only of a negative current collector (11a), so that a jelly roll type electrode assembly can be manufactured.
[0081] At this time, the negative electrode has a structure in which an active material layer is not formed, and the positive electrode has a structure in which an active material layer is formed on a long sheet-shaped current collector, and may include a non-active portion in which an active material layer is not formed in a part of the current collector. Preferably, the non-active portion of the positive electrode may be formed lengthwise along the winding direction (X) at one end of the current collector. By using a negative electrode in which an active material layer is not formed and a positive electrode in which a non-active portion is formed along the winding direction (X) at one end of the current collector in this manner, a tab-less battery structure without electrode tabs can be realized.
[0082] Specifically, a tab-less battery structure can be manufactured through the following method. First, a separator, a positive electrode, a separator, and a negative electrode are sequentially stacked and then wound in one direction to manufacture a jelly-roll type electrode assembly. Then, the non-positive portion (22) of the positive electrode is folded toward the core side, and current collection plates are welded to the non-positive portion of the positive electrode and the non-negative portion of the negative electrode to join them, and by connecting the current collection plates to the electrode terminals, a tab-less battery structure can be manufactured. Meanwhile, the current collection plates have a larger cross-sectional area compared to strip-type electrode tabs, and since resistance is proportional to the cross-sectional area of the current-carrying path, the cell resistance can be significantly reduced when the secondary battery is formed with such a structure.
[0084] Next, each component of the electrode assembly provided in a cylindrical secondary battery according to one embodiment of the present invention will be described in more detail.
[0085] (1) positive electrode
[0086] The above anode may be structured such that an anode active material layer is formed on at least one surface of a long sheet-shaped anode current collector, and the anode active material layer may include an anode active material, a conductive material, and a binder.
[0087] Specifically, the anode can be manufactured by applying an anode slurry, prepared by dispersing an anode active material, a conductive material, and a binder in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, onto one or both sides of a long sheet-shaped anode current collector, removing the solvent from the anode slurry through a drying process, and then rolling. Meanwhile, an anode including an uncoated portion can be manufactured by not applying the anode slurry to a portion of the anode current collector, for example, one end of the anode current collector, when applying the anode slurry.
[0089] The above positive active material includes lithium iron phosphate oxide (LiFePO4, LFP), and the above positive active material may specifically be lithium iron phosphate oxide (LiFePO4).
[0090] If the above lithium iron phosphate oxide is used as a positive electrode active material, it can compensate for the irreversibility of the negative electrode during the activation process of the lithium secondary battery and act as a resistor during subsequent charging and discharging, thereby increasing the safety of the lithium secondary battery. In addition, it has the advantage of price competitiveness as it is cheaper than lithium nickel-cobalt-manganese oxide, which is a commonly used positive electrode active material.
[0091] However, the positive electrode active material in the present invention is not limited to lithium iron phosphate oxide, and any material that can be conventionally used as a positive electrode active material may be used as the positive electrode active material of the present invention. Representatively, the positive electrode active material may include lithium manganese iron phosphate (LMFP), lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese aluminum oxide (NCMA), lithium manganese oxide (LMO), overlithiated oxide (OLO), cobalt-free oxide, nickel-free oxide, manganese-free oxide, manganese-rich oxide, or a mixture thereof.
[0092] Meanwhile, when lithium iron phosphate oxide is used as the positive electrode active material, there is a problem with the relatively low energy density of the secondary battery. Accordingly, the inventors of the present invention have completed the invention so that the secondary battery can have a high level of energy density even when lithium iron phosphate oxide is used as the positive electrode active material.
[0093] In the present invention, the negative electrode active material layer is excluded from the negative electrode, and the volume resulting from excluding the negative electrode active material layer may additionally include a positive electrode active material. For example, since the volume resulting from excluding the negative electrode active material layer may additionally include about 40% of a positive electrode active material, it can have a higher energy density compared to a battery having a negative electrode equipped with a conventional negative electrode active material layer.
[0095] According to one embodiment of the present invention, the loading amount of the positive electrode may be 110 to 120% based on the loading amount of the positive electrode of a cylindrical secondary battery having a negative electrode active material layer.
[0096] In addition, according to one embodiment of the present invention, the thickness of the anode may be 110 to 120% based on the thickness of the anode of a cylindrical secondary battery having a negative electrode active material layer.
[0097] Specifically, the loading amount of the anode is 500 to 600 mg / cm² 2 , 520 to 580 mg / cm² 2 or 540 to 560 mg / cm² 2 It can be a range.
[0098] Additionally, specifically, the thickness of the anode may be in the range of 190 to 220 μm, or 200 to 220 μm, or 200 to 210 μm.
[0099] Since the loading amount and / or thickness of the anode falls within the above range, there is an advantage of being able to produce more capacity and energy, and the mobility of lithium ions is improved, which can improve lifespan characteristics.
[0100] In the present invention, the 'loading amount of the anode' refers to the content of the anode active material, binder polymer, and conductive material included in the anode active material layer.
[0101] Furthermore, in the present invention, the 'cylindrical secondary battery having a negative electrode active material layer' differs from the cylindrical secondary battery according to the present invention only in that it has a negative electrode active material layer. The negative electrode active material layer may include a negative electrode active material and a binder polymer commonly used in cylindrical secondary batteries, and the negative electrode active material layer is not specifically limited in the present invention.
[0102] Generally, a cylindrical battery houses a jellyroll-type electrode assembly in which a sheet-shaped positive plate, a separator, and a negative plate are sequentially laminated within a cylindrical battery can. Since the cylindrical secondary battery of the present invention does not have a negative active material layer, an extra space equivalent to the thickness of the negative active material layer may be created inside the battery can compared to a conventional cylindrical secondary battery equipped with a negative active material layer. In a cylindrical secondary battery comprising a negative plate equipped with a negative active material layer, the positive loading amount is approximately 400 to 500 mg / cm² 2The range is such that the thickness of the anode is in the range of about 150 to 180 μm, and it is common to have a lower loading amount and thinner thickness compared to the loading amount and thickness of the anode presented in the present invention.
[0103] Accordingly, the present invention can exhibit advantageous effects in terms of capacity and energy by utilizing the extra space that is not provided for the negative electrode active material layer to increase the loading amount of the positive electrode active material layer and / or increase its thickness.
[0105] According to one embodiment of the present invention, together with lithium iron phosphate oxide (LiFePO4, LFP) as the positive electrode active material, a positive electrode active material commonly used in secondary batteries, such as LCO, NCM, NCA, NCAM, LMO, or OLO as described above, may also be included. More specifically, as a positive electrode active material commonly used in secondary batteries, a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-x M x Lithium nickel oxide represented by O2 (where M = one or more selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and x = 0.01 to 0.9); chemical formula LiMn 2-x M xExamples include lithium manganese complex oxides represented by O2 (where M = Co, Ni, Fe, Cr, Zn or Ta and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which part of the Li in the chemical formula is substituted with alkaline earth metal ions; disulfide compounds; Fe2(MoO4)3, but are not limited to these.
[0107] The above positive active material may be included in an amount of 80 to 99 parts by weight, or 85 to 99 parts by weight, or 90 to 99 parts by weight, relative to 100 parts by weight of the entire positive active material layer.
[0109] Meanwhile, various positive current collectors used in the relevant technical field may be used as the positive current collector. For example, the positive current collector may be stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. The positive current collector may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the positive current collector to increase the adhesion of the positive active material. The positive current collector may be used in various forms, such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0111] The above conductive material is used to impart conductivity to the electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, carbon nanotube; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The above conductive material may typically be included in an amount of 1 to 30 weight%, preferably 1 to 20 weight%, and more preferably 1 to 10 weight% based on the total weight of the positive electrode active material layer.
[0113] The above binder serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used. The above binder may be included in an amount of 1 to 30 weight%, preferably 1 to 20 weight%, more preferably 1 to 10 weight% based on the total weight of the positive active material layer.
[0115] (2) Negative electrode
[0116] The above-mentioned cathode includes a cathode current collector and does not have a cathode active material layer formed on any one surface of the cathode current collector. Specifically, the above-mentioned cathode may consist solely of a cathode current collector. Since the above-mentioned cathode does not have a cathode active material layer, there is an advantage in that the unit cost of the battery can be lowered by reducing process and manufacturing time and costs compared to the case where a cathode active material layer is included, and energy density can also be increased.
[0117] As the above-mentioned negative current collector, negative current collectors generally used in the relevant technical field may be used, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. The above-mentioned negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the anode current collector, may have fine irregularities formed on the surface of the current collector, and may be used in various forms such as film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0119] According to one embodiment of the present invention, the negative current collector may have the structure of 1) or 2) below.
[0120] 1) a structure comprising a porous region and a non-porous region, wherein at least a portion of the porous region is in contact with at least one surface of the separation membrane; or
[0121] 2) A multilayer structure comprising at least one porous sheet and at least one metal sheet.
[0122] When the above-mentioned cathode current collector has a structure like that of 1), the non-porous region of the above-mentioned cathode current collector may be located in the central part of the above-mentioned cathode current collector.
[0123] In addition, the porosity of the above-mentioned negative electrode current collector may be 30 to 80%. Since the above-mentioned negative electrode current collector has a porosity within the above range, when lithium is electrodeposited from the positive electrode to the negative electrode, a deposition space can be created, so that there is almost no change in the volume of the cylindrical secondary battery sealed in the battery can, and stable charging and discharging can be performed.
[0124] In the present invention, “porosity” refers to the ratio of the volume occupied by pores to the total volume of the object being measured, and uses vol% as its unit; it can be used interchangeably with terms such as porosity and porosity.
[0125] Meanwhile, if the above-mentioned cathode current collector has a multilayer structure as in 2), it may have a sandwich structure in which the metal sheet is located between two porous sheets, and the porosity of the porous sheets may be 30 to 80%.
[0126] The porous sheet may be copper; stainless steel; aluminum; nickel; titanium; calcined carbon; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, chromium, etc.; aluminum-cadmium alloy; or may comprise two or more of these.
[0127] The metal sheet may comprise lithium, a lithium alloy, or a mixture thereof.
[0128] The thickness of the metal sheet may be 0.1 to 10 μm. A metal sheet having a thickness within this range can provide appropriate energy density and is desirable in terms of economy.
[0130] (3) Separator
[0131] The above separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions; any separator typically used as a separator in a lithium secondary battery can be used without any special restrictions. Specifically, the above separator may be a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength.
[0132] In another embodiment of the separation membrane according to the present invention, at least one side may further include a porous coating layer comprising inorganic particles and a binder polymer.
[0133] In the porous coating layer, inorganic particles can be bound together by the binder polymer while in a state of being filled and in contact with each other, and as a result, an interstitial volume is formed between the inorganic particles, and the interstitial volume between the inorganic particles becomes an empty space, thereby forming pores.
[0134] The inorganic particles used to form the above porous coating layer are inorganic particles, that is, the operating voltage range of the electrochemical device (e.g., Li / Li +Inorganic particles that do not undergo oxidation and / or reduction reactions at a voltage of 0 to 5V (based on 0~5V) can be added and used. In particular, when using inorganic particles with ion transport capabilities, the ion conductivity within the electrochemical device can be increased to improve performance. Additionally, when using inorganic particles with a high dielectric constant, it contributes to increasing the degree of dissociation of electrolyte salts, such as lithium salts, within the liquid electrolyte, thereby improving the ion conductivity of the electrolyte.
[0135] For the reasons mentioned above, it is preferable that the inorganic particles include high dielectric constant inorganic particles having a dielectric constant of 5 or more, preferably 10 or more, inorganic particles having lithium ion transfer ability, or a mixture thereof.
[0136] Non-limiting examples of inorganic particles with a permittivity constant of 5 or greater include BaTiO3, Pb(Zr,Ti)O3 (PZT), and Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg 1 / 3 Nb 2 / 3 There are )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC, or mixtures thereof.
[0137] In particular, the aforementioned BaTiO3, Pb(Zr,Ti)O3(PZT), and Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg 1 / 3 Nb 2 / 3Inorganic particles such as O3-PbTiO3 (PMN-PT) and hafnia (HfO2) not only exhibit high dielectric constant characteristics with a dielectric constant of 100 or more, but also possess piezoelectricity, in which a charge is generated and a potential difference is created between the two surfaces when subjected to tension or compression by applying a certain pressure. This prevents internal short circuits between the two electrodes caused by external shocks, thereby enhancing the safety of electrochemical devices. Furthermore, when the aforementioned high dielectric constant inorganic particles are combined with inorganic particles capable of transporting lithium ions, their synergistic effects can be doubled.
[0138] Inorganic particles possessing lithium ion transport capability refer to inorganic particles that contain lithium elements but do not store lithium, instead having the function of transporting lithium ions. Since inorganic particles possessing lithium ion transport capability can transport and move lithium ions due to a type of defect existing within their particle structure, the lithium ion conductivity within the battery is enhanced, thereby enabling improved battery performance. Non-limiting examples of the aforementioned inorganic particles possessing lithium ion transport capability include lithium phosphate (Li3PO4) and lithium titanium phosphate (Li x Ti y (PO4)3, 0 <x<2, 0<y<3), 리튬알루미늄티타늄포스페이트(Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), such as (LiAlTiP) 14Li2O-9Al2O3-38TiO2-39P2O5 x O y Series glass (0 < x < 4, 0 < y < 13), lithium lanthanum titanate (Li x La y TiO3, 0<x<2, 0<y<3), Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4, etc.x Ge y P z S w Lithium nitrides such as , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), Li3N, etc. (Li x N y , 0 < x < 4, 0 < y < 2), SiS2-based glass such as Li3PO4-Li2S-SiS2 (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4), P2S5 series glass such as LiI-Li2S-P2S5 (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7) or mixtures thereof, etc.
[0139] There is no limit to the size of the inorganic particles in the porous coating layer, but it is preferable that it be 0.001 to 10 μm to form a coating layer of uniform thickness and appropriate porosity. If it is less than 0.001 μm, the dispersibility of the inorganic particles may decrease, and if it exceeds 10 μm, the thickness of the porous coating layer increases, which may degrade mechanical properties, and also, due to the excessively large pore size, the probability of an internal short circuit occurring during battery charging and discharging increases.
[0140] Binder polymers forming the porous coating layer include polyvinylidene fluoride-co-hexafluoropropylene (PVdF), polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, and cyanoethylflurane. Any one binder polymer selected from the group consisting of cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxylmethylcellulose, or a mixture of two or more of these may be used, but is not limited thereto.
[0141] The compositional ratio of inorganic particles and binder polymer used in the porous coating layer is preferably in the range of, for example, 50:50 to 99:1, and more preferably 70:30 to 95:5. If the content ratio of inorganic particles to binder polymer is less than 50:50, the content of binder polymer increases, which may reduce the improvement in the thermal safety of the separator. In addition, the reduction in voids formed between inorganic particles leads to a decrease in pore size and porosity, which may result in a degradation of the final battery performance. If the content of inorganic particles exceeds 99 parts by weight, the binder polymer content is too low, which may weaken the peel resistance of the porous coating layer. There are no specific limitations on the thickness of the porous coating layer, but a range of 0.01 to 20 µm is preferred. Furthermore, there are no specific limitations on pore size and porosity, but a pore size in the range of 0.001 to 10 µm is preferred, and a porosity in the range of 10 to 90% is preferred. Pore size and porosity mainly depend on the size of inorganic particles; for example, when inorganic particles with a particle size of 1 μm or less are used, the formed pores also exhibit a size of approximately 1 μm or less. This pore structure is subsequently filled with an electrolyte, and the electrolyte thus filled acts as an ion transporter. If the pore size and porosity are less than 0.001 μm and 10%, respectively, it can function as a resistive layer, and if the pore size and porosity exceed 10 μm and 90%, respectively, mechanical properties may deteriorate.
[0142] The porous coating layer described above can be formed by dissolving or dispersing a binder polymer in a dispersion medium, adding inorganic particles to obtain a slurry for forming a porous coating layer, and then coating and drying this slurry on at least one surface of a substrate. It is preferable that the dispersion medium has a solubility index similar to that of the binder polymer to be used and has a low boiling point. This is to facilitate uniform mixing and subsequent removal of the dispersion medium. Non-limiting examples of usable dispersion media include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or mixtures thereof.
[0143] It is preferable to add inorganic particles to a dispersion in which the binder polymer is dispersed in a dispersion medium, and then crush the inorganic particles. At this time, the crushing time is appropriately 1 to 20 hours, and the particle size of the crushed inorganic particles is preferably 0.001 to 10 μm as described above. Conventional methods may be used for crushing, and the ball mill method is particularly preferred.
[0144] Then, a binder polymer dispersion in which inorganic particles are dispersed is coated onto at least one surface of a porous polymer substrate under humidity conditions of 10 to 80% and dried. The method of coating the dispersion onto the porous polymer substrate may use conventional coating methods known in the industry, such as dip coating, die coating, roll coating, comma coating, or a combination thereof.
[0145] In addition to the aforementioned inorganic particles and binder polymers, the porous coating layer components may further include other additives such as conductive agents.
[0146] The final separator produced according to the present invention may have a thickness of 1 to 100 μm or 5 to 50 μm. If the thickness is less than 1 μm, the function of the separator may not be fully exerted and deterioration of mechanical properties may occur, and if it exceeds 100 μm, the characteristics of the battery may deteriorate during high-rate charging and discharging. In addition, it may have a porosity of 40 to 60% and an air permeability of 150 to 300 seconds / 100 mL.
[0148] Cylindrical lithium secondary battery
[0149] Next, a cylindrical lithium secondary battery according to the present invention will be described.
[0150] A cylindrical battery according to the present invention may include an electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; a battery can in which the electrode assembly is housed; and a sealing body that seals an open end of the battery can.
[0152] The cylindrical lithium secondary battery according to the present invention may be a cylindrical battery having a form factor ratio (defined as the ratio of the diameter of the cylindrical battery to the height, i.e., the ratio of the diameter (Ф) to the height (H)) of 0.25 or higher, or 0.4 or higher. Here, the form factor refers to a value representing the diameter and height of the cylindrical battery.
[0153] The cylindrical battery according to the present invention may be, for example, an 18650 cell (diameter 18 mm, height 65 mm, form factor ratio 0.277), a 21700 cell (diameter 21 mm, height 70 mm, form factor ratio 0.300), a 46110 cell (diameter 46 mm, height 110 mm, form factor ratio 0.418), a 48750 cell (diameter 48 mm, height 75 mm, form factor ratio 0.640), a 48110 cell (diameter 48 mm, height 110 mm, form factor ratio 0.418), a 48800 cell (diameter 48 mm, height 80 mm, form factor ratio 0.600), or a 46800 cell (diameter 46 mm, height 80 mm, form factor ratio 0.575). In the figures representing the form factor, the first two digits represent the diameter of the cell, the next two digits represent the height of the cell, and the last digit O represents that the cross-section of the cell is circular.
[0154] A cylindrical lithium secondary battery according to the present invention can exhibit a high energy density per unit volume by including a negative electrode that excludes a negative electrode active material layer. According to one embodiment of the present invention, the capacity of the cylindrical lithium secondary battery according to the present invention may be increased by 140 to 180% based on the capacity of a cylindrical secondary battery having a negative electrode active material layer. Specifically, it may exhibit an energy density per unit volume of 850 or 900 Wh / L or higher. This can be calculated by multiplying the design capacity of the secondary battery by the average voltage and then dividing by the volume of the battery size.
[0156] In addition, the cylindrical lithium secondary battery according to the present invention can achieve excellent safety even in cylindrical batteries with a form factor ratio of 0.25 or 0.4 or higher. In particular, when the negative electrode active material layer is excluded, the negative electrode accumulates in the form of lithium metal when charged; nevertheless, the present invention facilitates gas discharge in a certain direction, which is advantageous for thermal stability.
[0158] Meanwhile, the cylindrical battery according to the present invention may preferably be a tab-less battery that does not include an electrode tab, but is not limited thereto.
[0159] The above-described tabless battery structure may, for example, have a positive electrode and a negative electrode each having a non-active material layer formed therein, a positive electrode non-active portion and a negative electrode non-active portion located at the top and bottom of an electrode assembly, respectively, a current collection plate coupled to the positive electrode non-active portion and the negative electrode non-active portion, and a current collection plate connected to an electrode terminal.
[0161] FIG. 2 shows a cross-sectional view of a cylindrical battery with a tabless structure according to an embodiment of the present invention. Hereinafter, a cylindrical battery according to an embodiment of the present invention will be described with reference to FIG. 2. However, FIG. 2 is merely an example of an embodiment of the present invention, and the structure of the cylindrical battery of the present invention is not limited to the range disclosed in FIG. 2.
[0162] A cylindrical battery (140) according to one embodiment of the present invention comprises a jelly-roll type electrode assembly (141) described above, a battery can (142) in which the electrode assembly (141) is housed, and a sealing body (143) that seals the open end of the battery can (142).
[0163] At this time, the positive and negative electrodes of the electrode assembly may each include a non-active portion in which an active material layer is not formed, and may be stacked and wound such that the positive non-active portion and the negative non-active portion are located at the top and bottom of the electrode assembly, respectively. Since the electrode assembly has been described above, only the remaining components excluding the electrode assembly will be described below.
[0164] The battery can (142) is a cylindrical container with an opening formed at the top and is made of a conductive metal material such as aluminum or steel. The battery can accommodates an electrode assembly (141) in the inner space through the top opening and also accommodates an electrolyte (not shown).
[0166] The electrolyte used in the present invention may be any of the various electrolytes usable in lithium secondary batteries, such as liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., and the types thereof are not particularly limited.
[0167] Specifically, the electrolyte may be a liquid electrolyte and may include an organic solvent and a lithium salt.
[0168] The above organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. For example, the above organic solvent may be an ester, ether, imide, linear carbonate, cyclic carbonate, etc., used individually or in a mixture of two or more types.
[0169] Specifically, as the ester among the above organic solvents, any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone, or a mixture of two or more of these may be used, but is not limited thereto.
[0170] In addition, specifically, the ether among the organic solvents is a linear ether system such as dimethyl ether, diethyl ether, dipropyl ether, dibutyl ether, diisobutyl ether, ethylmethyl ether, ethylpropyl ether, ethyl tert-butyl ether, dimethoxymethane, trimethoxymethane, dimethoxyethane, diethoxyethane, dimethoxypropane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, dipropylene glycol dimethylene ether, butylene glycol ether, diethylene glycol ethylmethyl ether, diethylene glycol isopropylmethyl ether, diethylene glycol butylmethyl ether, diethylene glycol tert-butylethyl ether, ethylene glycol ethylmethyl ether, etc.; Cyclic ethers such as dioxolane, methyldioxolane, dimethyldioxolane, vinyldioxolane, methoxydioxolane, ethylmethyldioxolane, oxane, dioxane, trioxane, tetrahydrofuran, methyltetrahydrofuran, dimethyltetrahydrofuran, dimethoxytetrahydrofuran, ethoxytetrahydrofuran, dihydropyran, tetrahydropyran, furan, 2-methylfuran, etc. Fluorinated ether compounds such as 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether (TTE), bis(fluoromethyl) ether, 2-fluoromethyl ether, bis(2,2,2-trifluoroethyl) ether, propyl 1,1,2,2-tetrafluoroethyl ether, isopropyl 1,1,2,2-tetrafluoroethyl ether, 1,1,2,2-tetrafluoroethyl isobutyl ether, 1,1,2,3,3,3-hexafluoropropyl ethyl ether, 1H,1H,2'H,3H-decafluorodipropyl ether, 1H,1H,2'H-perfluorodipropyl ether, or mixtures thereof may be included.
[0172] The above lithium salt can be used without special limitations as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably used within the range of 0.1 to 5.0 M, more preferably 0.1 to 3.0 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively.
[0173] In addition to the electrolyte components, the above electrolyte may further include additives for the purpose of improving the lifespan characteristics of the battery, suppressing the reduction of battery capacity, and improving the discharge capacity of the battery. For example, the above additives may include haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, either alone or in combination, but are not limited thereto. The above additives may be included in an amount of 0.1 to 10 weight%, preferably 0.1 to 5 weight%, based on the total weight of the electrolyte.
[0175] The battery can (142) is electrically connected to the non-electrical portion (146) of the negative plate and functions as a negative terminal that contacts an external power source to transmit current applied from the external power source to the negative plate.
[0176] If necessary, a beading portion (147) and a crimping portion (148) may be provided on the top of the battery can (142). The beading portion (147) may be formed by pressing the outer circumference of the battery can (142). The beading portion (147) prevents the electrode assembly (141) housed inside the battery can (142) from escaping through the top opening of the battery can (142) and may function as a support portion on which the seal (142) is seated.
[0177] The above-mentioned crimping portion (148) may be formed on the upper part of the above-mentioned beading portion (147) and has an extended and bent shape to wrap around the outer surface of the cap plate (143a) placed on the beading portion (147) and a part of the upper surface of the cap plate (143a).
[0179] Next, the seal (143) is intended to seal the open end of the battery can (142) and includes a cap plate (143a), a first gasket (143b) that provides airtightness and insulation between the cap plate (143a) and the battery can (142), and, if necessary, may further include a connecting plate (143c) electrically and mechanically coupled to the cap plate (143a). The cap plate (143a) is pressed onto a beading portion (147) formed on the battery can (142) and may be secured by a crimping portion (148).
[0180] The cap plate (143a) is a component made of a conductive metal material and covers the upper opening of the battery can (142). The cap plate (143a) is electrically connected to the positive plate of the electrode assembly (141) and is electrically insulated from the battery can (142) through the first gasket (143b). Thus, the cap plate (143a) can function as a positive terminal of a cylindrical secondary battery. The cap plate (143a) may have a formed protrusion (143d) protruding upward from its center, and the protrusion (143d) may come into contact with an external power source to allow current to be applied from the external power source.
[0181] A first gasket (143b) may be interposed between the cap plate (143a) and the crimping portion (148) to ensure airtightness of the battery can (142) and to provide electrical insulation between the battery can (142) and the cap plate (143a).
[0182] Meanwhile, the cylindrical battery (140) according to the present invention may further include a current collection plate (144, 145) as needed. The current collection plate is coupled to the non-positive portion (146a) of the positive plate and the non-positive portion (146b) of the negative plate, and is connected to electrode terminals (i.e., positive terminal and negative terminal).
[0183] Specifically, the cylindrical battery (140) according to the present invention may include a first current collecting plate (144) coupled to the upper part of an electrode assembly (141) and a second current collecting plate (145) coupled to the lower part of the electrode assembly (141).
[0184] The first current collector plate (144) is coupled to the upper part of the electrode assembly (141). The first current collector plate (144) is made of a conductive metal material such as aluminum, copper, nickel, etc., and is electrically connected to the non-conductive portion (146a) of the positive plate. A lead (149) may be connected to the first current collector plate (144). The lead (149) may extend upward from the electrode assembly (141) and be coupled to the connecting plate (143c) or directly coupled to the lower surface of the cap plate (143a). The coupling of the lead (149) and other parts may be achieved through welding. Preferably, the first current collector plate (144) may be formed integrally with the lead (149). In this case, the lead (149) may have an elongated plate shape extending outward from the center of the first current collector plate (144).
[0185] Meanwhile, the first current collector plate (144) is coupled to the end of the non-conforming portion (146a) of the positive plate, and the coupling can be achieved by methods such as, for example, laser welding, resistance welding, ultrasonic welding, or soldering.
[0186] The second current collector plate (145) is coupled to the lower part of the electrode assembly (141). The second current collector plate (145) is made of a conductive metal material such as aluminum, copper, nickel, etc., and is electrically connected to the non-conductive portion (146b) of the negative electrode plate. One side of the second current collector plate (145) can be coupled to the non-conductive portion (146b) of the negative electrode plate, and the opposite side can be coupled to the inner bottom surface of the battery can (142). At this time, the coupling can be achieved by methods such as laser welding, resistance welding, ultrasonic welding, or soldering.
[0187] Meanwhile, the cylindrical battery (140) according to the present invention may further include an insulator (146) as needed. The insulator (146) may be positioned to cover the upper surface of the first current collector plate (144). By the insulator (146) covering the first current collector plate (144), direct contact between the first current collector plate (144) and the inner surface of the battery can (142) can be prevented.
[0188] The insulator (146) is provided with a lead hole (151) so that a lead (149) extending upward from the first current collection plate (144) can be drawn out. The lead (149) is drawn out upward through the lead hole (151) and coupled to the lower surface of the connecting plate (143c) or the lower surface of the cap plate (143a).
[0189] The insulator (146) may be made of an insulating polymer resin, such as polyethylene, polypropylene, polyimide, or polybutylene terephthalate.
[0190] Meanwhile, the cylindrical battery (140) according to the present invention may further include a venting portion (152) formed on the lower surface of the battery can (142) as needed. The venting portion (152) corresponds to an area on the lower surface of the battery can (142) that has a thinner thickness compared to the surrounding area. Because the venting portion (152) has a thin thickness, it is structurally weaker compared to the surrounding area. Therefore, when the pressure inside the cylindrical battery (140) increases above a certain level, the venting portion (152) ruptures, allowing the gas inside the battery can (152) to be discharged to the outside, thereby preventing the battery from exploding.
[0192] FIG. 3 shows a cross-sectional view of a cylindrical battery with a tabless structure according to another embodiment of the present invention. Hereinafter, a cylindrical battery according to another embodiment of the present invention will be described with reference to FIG. 3. However, FIG. 3 is merely an example of an embodiment of the present invention, and the structure of the cylindrical battery of the present invention is not limited to the scope disclosed in FIG. 3.
[0194] Referring to FIG. 3, a cylindrical battery (170) according to another embodiment of the present invention has a different structure of the battery can and seal compared to the cylindrical battery (140) shown in FIG. 2, and the composition of the electrode assembly and electrolyte is substantially the same.
[0195] Specifically, the cylindrical battery (170) includes a battery can (171) through which a rivet terminal (172) is installed. The rivet terminal (172) is installed on the closed surface (upper surface of the drawing) of the battery can (171). The rivet terminal (172) is riveted into the through hole of the battery can (171) with an insulating second gasket (173) interposed therein. The rivet terminal (172) is exposed to the outside in a direction opposite to the direction of gravity.
[0196] The rivet terminal (172) includes a terminal exposure portion (172a) and a terminal insertion portion (172b). The terminal exposure portion (172a) is exposed to the outside of the closed surface of the battery can (171). The terminal exposure portion (172a) may be located approximately in the center of the closed surface of the battery can (171). The maximum diameter of the terminal exposure portion (172a) may be formed to be larger than the maximum diameter of the through hole formed in the battery can (171). The terminal insertion portion (172b) may penetrate approximately in the center of the closed surface of the battery can (171) and be electrically connected to the non-existent portion (146a) of the positive plate. The terminal insertion portion (172b) may be rivet-bonded onto the inner surface of the battery can (171). That is, the end of the terminal insertion portion (172b) may have a curved shape toward the inner surface of the battery can (171). The maximum diameter of the end of the terminal insertion part (172b) may be larger than the maximum diameter of the through hole of the battery can (171).
[0197] The lower surface of the terminal insertion portion (172b) can be welded to the first current collector plate (144) connected to the non-contained portion (146a) of the positive plate. An insulating cap (172) made of an insulating material can be interposed between the first current collector plate (144) and the inner surface of the battery can (171). The insulating cap (174) covers the upper portion of the first current collector plate (144) and the upper edge portion of the electrode assembly (141). This prevents the outer non-contained portion (B3) of the electrode assembly (141) from coming into contact with the inner surface of the battery can (171) having a different polarity and causing a short circuit. The terminal insertion portion (172b) of the rivet terminal (172) can be welded to the first current collector plate (144) by penetrating the insulating cap (174).
[0198] The second gasket (173) is interposed between the battery can (171) and the rivet terminal (172) to prevent the battery can (171) and the rivet terminal (172), which have opposite polarities, from coming into electrical contact. This allows the upper surface of the battery can (171), which has a roughly flat shape, to function as the positive terminal of the cylindrical battery (170).
[0199] The second gasket (173) includes a gasket exposure portion (173a) and a gasket insertion portion (173b). The gasket exposure portion (173a) is interposed between the terminal exposure portion (172a) of the rivet terminal (172) and the battery can (171). The gasket insertion portion (173b) is interposed between the terminal insertion portion (172b) of the rivet terminal (172) and the battery can (171). The gasket insertion portion (173b) can be deformed together with the terminal insertion portion (172b) during riveting and adhere to the inner surface of the battery can (171). The second gasket (173) may be made of, for example, an insulating polymer resin.
[0200] The gasket exposure portion (173a) of the second gasket (173) may have an extended shape to cover the outer surface of the terminal exposure portion (172a) of the rivet terminal (172). When the second gasket (173) covers the outer surface of the rivet terminal (172), it is possible to prevent a short circuit from occurring during the process of connecting electrical connection components, such as a busbar, to the upper surface of the battery can (171) and / or the rivet terminal (172). Although not shown in the drawing, the gasket exposure portion (173a) may have an extended shape to cover not only the outer surface of the terminal exposure portion (172a) but also a part of the upper surface.
[0201] In the case where the second gasket (173) is made of a polymer resin, the second gasket (173) can be joined to the battery can (171) and the rivet terminal (172) by heat fusion. In this case, the airtightness at the joint interface between the second gasket (173) and the rivet terminal (172) and the joint interface between the second gasket (173) and the battery can (171) can be enhanced. Meanwhile, in the case where the gasket exposure portion (173a) of the second gasket (173) has a shape that extends to the upper surface of the terminal exposure portion (172a), the rivet terminal (172) can be joined integrally with the second gasket (173) by insert injection.
[0202] The remaining area (185) of the upper surface of the battery can (171), excluding the area occupied by the rivet terminal (172) and the second gasket (173), corresponds to a negative terminal having opposite polarity to the rivet terminal (172).
[0203] The second current collector plate (176) is coupled to the lower part of the electrode assembly (141). The second current collector plate (176) is made of a conductive metal material such as aluminum, steel, copper, or nickel, and is electrically connected to the non-conductive portion (146b) of the negative plate.
[0204] Preferably, the second current collector plate (176) is electrically connected to the battery can (171). To this end, at least a portion of the edge portion of the second current collector plate (176) may be interposed and fixed between the inner surface of the battery can (171) and the first gasket (178b). In one example, at least a portion of the edge portion of the second current collector plate (176) may be fixed to the beading portion (180) by welding while being supported on the bottom surface of the beading portion (180) formed at the bottom of the battery can (171). In a variation, at least a portion of the edge portion of the second current collector plate (176) may be directly welded to the inner wall surface of the battery can (171).
[0205] The second current collector plate (176) may have a plurality of irregularities (not shown) formed radially on a surface facing the non-contact portion (146b). When irregularities are formed, the second current collector plate (176) can be pressed to press the irregularities into the non-contact portion (146b).
[0206] Preferably, the ends of the second current collector plate (176) and the non-current portion (146b) can be joined by welding, for example, laser welding.
[0207] A sealing body (178) that seals the lower open end of a battery can (171) includes a cap plate (178a) and a first gasket (178b). The first gasket (178b) electrically separates the cap plate (178a) from the battery can (171). A crimping portion (181) secures the edge of the cap plate (178a) and the first gasket (178b) together. The cap plate (178a) is provided with a vent portion (179). The configuration of the vent portion (179) is substantially the same as that of the above-described embodiment.
[0208] Preferably, the cap plate (178a) is made of a conductive metal material. However, since a first gasket (178b) is interposed between the cap plate (178a) and the battery can (171), the cap plate (178a) does not have electrical polarity. The seal (178) seals the open end of the lower part of the battery can (171) and functions to release gas when the internal pressure of the battery cell (170) increases above a critical value.
[0209] Preferably, the rivet terminal (172) electrically connected to the non-bonded portion (146a) of the positive plate is used as the positive terminal. Additionally, the portion (175) of the upper surface of the battery can (171), which is electrically connected to the non-bonded portion (146b) of the negative plate through the second current collector plate (176), excluding the rivet terminal (172), is used as the negative terminal. Thus, when two electrode terminals are located on the upper part of the cylindrical battery, electrical connection components such as busbars are used on the cylindrical battery
[0210] It is possible to place it on only one side of (170). This can lead to a simplification of the battery pack structure and an improvement in energy density. Additionally, the portion (175) used as the negative terminal has a roughly flat shape, so a sufficient contact area can be secured for joining electrical connection components such as busbars. Accordingly, the cylindrical battery (170) can reduce the resistance at the joining site of the electrical connection components to a desirable level.
[0212] When a cylindrical lithium secondary battery is formed with a tabless structure as described above, current concentration is less compared to a conventional battery equipped with electrode tabs, so heat generation inside the battery can be effectively reduced, and accordingly, the thermal safety of the battery can be improved.
[0214] A method for manufacturing a cylindrical secondary battery according to one aspect of the present invention is,
[0215] Step of preparing the anode, cathode, and separator;
[0216] A step of forming an electrode-separator laminate by stacking the separator at least once so that the separator is interposed between the anode and the cathode;
[0217] A step of forming a jelly roll type electrode assembly by winding the above electrode-separator laminate in one direction;
[0218] A step of housing the electrode assembly in a battery can and injecting an electrolyte into the battery can housing the electrode assembly;
[0219] A step of manufacturing a battery by sealing the open end of the battery can; and
[0220] The step of activating the battery under conditions of room temperature and atmospheric pressure; is included.
[0222] A detailed description of each component is as explained above.
[0223] In particular, the present invention is characterized by the fact that the activation of the battery is performed under conditions of room temperature and atmospheric pressure during the activation step of the battery.
[0224] In the battery activation stage, initial charging is performed to activate the electrode active material and form an SEI film on the electrode surface. Generally, since gas generation inside the battery is inevitable during the activation stage due to factors such as the decomposition reaction of the electrolyte, it is customary to remove the internally generated gas by performing battery activation under specific high-pressure conditions.
[0225] However, in the present invention, the cylindrical secondary battery can self-pressurize as the lithium metal is generated with a can acting as an outer wall on the outside of the jelly roll, causing the pressure to come into contact with the can when the volume expands. In other words, the cylindrical secondary battery of the present invention can self-pressurize by performing initial charging and discharging. Accordingly, since separate high-pressure conditions, specifically conditions such as pressurizing with a jig, are not required during the battery activation stage, there is an advantage of process convenience.
[0227] Hereinafter, the present invention will be described in detail with reference to examples to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described below. The embodiments of the present invention are provided to more completely explain the invention to those with average knowledge in the art.
[0229] Example 1
[0230] An anode slurry was prepared by mixing 497 parts by weight of LiFePO4 as the anode active material, 1.5 parts by weight of carbon nanotubes as the conductive material, and 1.5 parts by weight of polyvinylidene fluoride (PVdF, Kureha) as the binder, adding the mixture to an N-methyl-2-pyrrolidone solvent, and mixing. The anode slurry was applied to one side of an aluminum current collector sheet with a thickness of 15 μm, dried at 120°C, and then rolled to obtain an anode loading amount of 560 mg / 25 cm². 2 And, an anode plate with a thickness of 200㎛ was prepared.
[0231] A copper foil with a thickness of 10 μm was prepared as the cathode plate.
[0232] A jelly-roll type electrode assembly was manufactured by interposing a separator between the positive plate and the negative plate prepared as described above, stacking them in the order of separator / positive plate / separator / negative plate, and then winding them. A cylindrical secondary battery with 21,700 cells was manufactured by inserting the electrode assembly manufactured as described above into a cylindrical battery can and injecting an electrolyte.
[0234] Comparative Example 1
[0235] A negative electrode slurry was prepared by mixing a negative electrode active material (a mixture of graphite and SiO₂ in a weight ratio of 95:5), a conductive material (super C), styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) in water in a weight ratio of 96:2:1.5:0. A negative electrode was prepared by applying the negative electrode slurry to one side of a copper foil with a thickness of 10 μm, drying it at 150°C, and rolling it; and a positive plate was prepared with different amounts of positive active material, positive thickness, and positive loading amount as shown in Table 1 below. A cylindrical secondary battery with 21,700 cells was manufactured in the same manner as in Example 1.
[0237] Example 2
[0238] A cylindrical secondary battery with 21,700 cells was manufactured in the same manner as in Example 1, except that a positive plate with different amounts of positive active material, positive thickness, and positive loading amount was prepared as shown in Table 1 below.
[0240] Amount of positive active material (g) Anode thickness (㎛) Anode loading amount (mg / 25cm) 2 ) Charge capacity (mAh) Single discharge capacity (mAh) Energy density per unit volume (Wh / L) 20-dose retention rate (%) Comparative Example 1 26 180 490 4933 4526 607 93.6 Example 1 38 200 560 7014 6711 901 95.9 Example 2 37 210 540 6919 6621 889 95.3
[0242] Evaluation example
[0243] 1. Charge / Discharge Capacity
[0244] For the cylindrical secondary batteries prepared in Examples 1 and 2 and Comparative Example 1, the initial charge / discharge capacity was measured by charging in CC / CV mode at 25°C with a constant current of 0.1C to 3.9V (termination current 0.1C), and then discharging in CC mode until the voltage reached 2.5V. The results are shown in FIG. 5.
[0245] In the operating range of the cylindrical secondary battery of Comparative Example 1, the amount of positive active material can be up to 26g, but when a negative electrode that does not include a negative active material layer is applied as in Examples 1 and 2, the amount of positive active material that can be inserted into the cell increases, thereby maximizing the energy density per volume. The charge capacity and discharge capacity of Examples 1 and 2 can be increased by about 50% compared to Comparative Example 1.
[0247] 2. Life Assessment
[0248] To verify the life characteristics of the cylindrical secondary batteries prepared in Examples 1 and 2 and Comparative Example 1, the first cycle at 25°C was charged to 3.9V at 0.1C under constant current / constant voltage (CC / CV) conditions, and then charged to 0.1C under constant current (CC) conditions. After leaving it for 30 minutes, it was discharged to 2.5V at 0.1C, and the discharge capacity was measured.
[0249] Subsequently, the cycle was repeated for up to 25 cycles of charging and discharging at 0.1C in the 3.9V-2.5V voltage range, and the discharge capacity retention rate was measured for each cycle. The results are shown in Fig. 6. It can be confirmed that Examples 1 and 2 exhibit superior charging and discharging capacities compared to Comparative Example 1, while the capacity retention rate is equivalent to that of Comparative Example 1.
[0251] 3. Hot Box Review
[0252] To verify the safety of the cylindrical secondary battery prepared in Example 1, a hot box test was performed. In the hot box test, the charged battery was placed in a chamber capable of convection, and the cell temperature of the secondary battery was checked by reaching 130°C at a heating rate of 5°C / min, maintaining the temperature for 30 minutes, and then reaching 200°C at a heating rate of 5°C / min and maintaining the temperature for 1 hour. The results are shown in Fig. 7.
[0253] The cylindrical secondary battery manufactured in Example 1 was confirmed to maintain a temperature of approximately 30 minutes at 130°C and 1 hour at 200°C as a result of hot box evaluation. This is similar to the hot box evaluation results of a cylindrical secondary battery with a negative electrode coating layer, indicating that Example 1 can secure excellent safety equivalent to that of a battery with a negative electrode coating layer, even without a negative electrode coating layer.
Claims
Claim 1 A cylindrical secondary battery comprising: an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; a battery can in which the electrode assembly is housed; and a sealing body for sealing an open end of the battery can, wherein the positive electrode comprises a positive current collector and a positive active material layer comprising a positive active material on at least one surface of the positive current collector, the negative electrode comprises a negative current collector but does not comprise a negative active material layer, and the negative current collector has a structure of 1) or 2) below: 1) a structure comprising a porous region and a non-porous region, wherein at least a portion of the porous region contacts one surface of the separator, or 2) a structure wherein at least one metal sheet is positioned between two porous sheets. Claim 2 A cylindrical secondary battery according to claim 1, characterized in that the negative electrode is composed solely of a negative current collector. Claim 3 A cylindrical secondary battery according to claim 1, wherein the positive electrode active material comprises lithium iron phosphate oxide (LFP), lithium manganese iron phosphate (LMFP), lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), lithium nickel cobalt manganese aluminum oxide (NCMA), lithium manganese oxide (LMO), overlithiated oxide (OLO), cobalt-free oxide, nickel-free oxide, manganese-free oxide, manganese-rich oxide, or a mixture thereof. Claim 4 A cylindrical secondary battery according to claim 1, characterized in that the positive active material is included in an amount of 80 to 99 parts by weight relative to 100 parts by weight of the entire positive active material layer. Claim 5 A cylindrical secondary battery according to claim 1, characterized in that the loading amount of the positive electrode is 110 to 120% based on the loading amount of the positive electrode of a cylindrical secondary battery having a negative electrode active material layer. Claim 6 In claim 1, the loading amount of the anode is 500 to 600 mg / cm² 2 A cylindrical secondary battery characterized by being within the range of Claim 7 A cylindrical secondary battery according to claim 1, characterized in that the thickness of the positive electrode is 110 to 120% based on the thickness of the positive electrode of a cylindrical secondary battery having a negative electrode active material layer. Claim 8 A cylindrical secondary battery according to claim 1, characterized in that the thickness of the anode is in the range of 190 to 220 μm. Claim 9 A cylindrical secondary battery according to claim 1, characterized in that the capacity of the cylindrical secondary battery is increased by 140 to 180% based on the capacity of the cylindrical secondary battery having a negative electrode active material layer. Claim 10 The cylindrical secondary battery according to claim 1, characterized in that the cylindrical secondary battery has an energy density per unit volume of 850 Wh / L or more. Claim 11 delete Claim 12 In claim 1, the cylindrical secondary battery is characterized by having a form factor ratio of 0.25 or higher. Claim 13 A cylindrical secondary battery according to claim 1, characterized in that the cylindrical secondary battery is an 18650 cell, a 21700 cell, a 46110 cell, a 48750 cell, a 48110 cell, a 48800 cell, or a 46800 cell. Claim 14 A cylindrical secondary battery according to claim 1, characterized in that the cylindrical secondary battery is a tab-less battery that does not include an electrode tab. Claim 15 A cylindrical secondary battery according to claim 1, characterized in that the cylindrical secondary battery comprises a liquid electrolyte. Claim 16 A method for manufacturing a cylindrical secondary battery according to claim 1, comprising the steps of: preparing a positive electrode, a negative electrode, and a separator; forming an electrode-separator laminate by stacking the separator at least once such that the separator is interposed between the positive electrode and the negative electrode; forming a jelly roll type electrode assembly by winding the electrode-separator laminate in one direction; housing the electrode assembly in a can and injecting an electrolyte into the can housing the electrode assembly; sealing the open end of the can to manufacture a battery; and performing activation of the battery under conditions of room temperature and atmospheric pressure; wherein the positive electrode comprises a positive current collector and a positive active material layer comprising a positive active material on at least one side surface of the positive current collector, and the negative electrode comprises a negative current collector but does not comprise a negative active material layer.
Citation Information
Patent Citations
Porous lithium metal anode, preparation and application in lithium metal battery
CN110867559A
Lithium-ion batteries
US20220302495A1
Multifunctional cathode additives for battery technologies
WO2015126932A1
Cylindrical secondary battery comprising flexible input port
KR1020210077968A
Negative electrode comprising porous matrix and current collector, and lithium secondary battery comprising the same
KR1020220011408A