Recyclable materials
A recyclable material with cellulose, protein binder, and additives allows for easy molding and composting, addressing the environmental issues of petroleum-based plastics by enhancing recyclability and biodegradability.
Patent Information
- Application Number
- KR1020247002997
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-29
- Filing Date
- 2022-06-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-06-23
AI Technical Summary
Existing disposable plastic products made from petroleum-based materials are not environmentally friendly due to low biodegradability, resource inefficiency, and competition with food resources, and recyclable alternatives like paper and cardboard are not suitable for mass production.
A recyclable material composed of 30-97% cellulose, 2-45% protein binder, 1-20% alcohol or ester, and 0-45% additive, which can be molded like thermoplastics and fully composted, allowing easy recycling into paper or cardboard cycles.
The material enables high recyclability, complete biodegradability, and thermoplastic processing, providing an environmentally friendly alternative to petroleum-based plastics for molded parts.
Abstract
Description
Technology Field
[0001] The present invention relates to a recyclable material suitable for producing a molded part, a method for producing a molded part from a recyclable material, and a molded part produced thereby. Background Technology
[0002] In 2017, approximately 348 million tons of petroleum-based plastic were produced globally. About half of this inexpensive and versatile material is processed into single-use products such as bags, straws, and disposable bottles. Considering all the energy, labor, and raw materials used to produce these products, the benefits are very short-lived. A significant portion of these disposable items are not properly disposed of and end up in the environment, particularly the ocean, where they remain for decades due to their low biodegradability. Furthermore, harmful chemicals, especially plasticizers, are washed away, leading to water and soil pollution. Even among plastic products that are properly disposed of, the majority are still incinerated or dumped in landfills.
[0003] Another problem is that manufacturing plastic products requires petroleum, large amounts of energy, and freshwater. Therefore, petroleum-based plastics have a poor balance between energy and the environment.
[0004] Therefore, for the past few years, plastics made from renewable natural materials have been increasingly used, particularly in the production of disposable products. The problem is that most of these plastics are made primarily from raw materials that are also used for food, such as potatoes, rice, and corn.
[0005] Many recyclable materials that can be used to produce disposable items, such as paper or cardboard, are not suitable for mass production because they cannot be molded as easily as plastic materials.
[0006] Therefore, it would be advantageous to use recyclable materials composed of natural raw materials that do not compete with food or compete only within a limited range, and which can be processed as easily and in as many ways as petroleum-based plastic materials. The problem to be solved
[0007] The objective of the present invention is to provide a recyclable material suitable for molding various molded parts, said material which is easy to form into various shapes and can be recycled or disposed of in an environmentally friendly manner, particularly through composting after use. means of solving the problem
[0008] This objective is solved by the features according to claim 1. According to the present invention, the recyclable material comprises 30 to 97 weight percent of a cellulose material, 2 to 45 weight percent of at least one protein binder, 1 to 20 weight percent of at least one alcohol or ester, and 0 to 45 weight percent of at least one additive.
[0009] This material is environmentally friendly as it is composed entirely of natural raw materials. Due to its high cellulose content, materials or molded parts made from it can be fed into the paper, cardboard, or board recycling cycle, allowing for easy and repeated recycling. Additionally, this material is fully compostable in household compost, enabling eco-friendly disposal. It can also be easily molded like thermoplastics using protein binders.
[0010] In this application, recyclable material is understood to mean a material that is processable and whose main component (in this case, cellulose material) can be used as a starting material for producing a new material (in this case, paper, cardboard, or board paper).
[0011] The recyclable material according to the present invention or the molded part formed therefrom can be dissolved in water, for example, in a pulper, thereby separating the cellulose material and allowing it to be further processed into paper, cardboard, or boards. Other components present in the recyclable material are completely biodegradable or present in small amounts that are not problematic, so that the material can be disposed of in an easy and environmentally friendly manner, particularly through wastewater. Additionally, the protein binder and other components of the recyclable material can be separated and reused using appropriate processing methods.
[0012] It has been demonstrated that using the recyclable material according to the present invention allows a high proportion of cellulose material to be supplied to the recycling cycle. In a series of tests performed by the applicant, the recyclability of the cellulose material showed a value of 95% or higher.
[0013] If recyclable materials or molded parts made from these materials are not recycled, they can be completely decomposed in compost. The materials used can be completely decomposed in both domestic and industrial compost according to the standard of DIN / EN 13432:2000. In addition, recyclable materials or molded parts made from them decompose harmlessly in nature and water according to the specifications of ISO 16221:2001.
[0014] Recyclable materials exhibit thermoplastic properties during processing, particularly when solvents such as water are added or when exposed to heat, so they can be processed into molded parts using methods known in polymer processing, such as injection molding, extrusion molding, press molding, casting, rotational molding, or vacuum molding. These materials can also be processed into molded parts using sintering or a 3D printer.
[0015] Therefore, the recyclable material according to the present invention provides an environmentally friendly alternative to petroleum-based plastics.
[0016] The cellulose material is preferably in the form of fibers or powder. When the cellulose material is present as a powder, the average particle size of the powder is 100 to 1000 μm, preferably 150 to 250 μm.
[0017] It is desirable that the cellulose material be present in the recyclable material in an amount of preferably 30 to 97 weight percent, particularly preferably 40 to 90 weight percent, particularly preferably 51 to 85 weight percent, and most preferably 60 to 80 weight percent.
[0018] In this application, a protein binder is understood to be a protein or a protein mixture that has adhesive properties and can be cured. The protein binder softens when heat is applied or water is added, thereby allowing the shape of the recyclable material to be modified. Thus, by using at least one protein binder, the thermoplastic behavior of the recyclable material according to the present invention can be characterized.
[0019] It is desirable that at least one protein binder be present in the recyclable material at a concentration of 2 to 45 weight percent, more preferably 10 to 30 weight percent, and particularly preferably 15 to 25 weight percent.
[0020] At least one alcohol and / or at least one ester improves the fluidity of the recyclable material according to the present invention, thereby facilitating the processing of the recyclable material into a molded part.
[0021] The recyclable material comprises 1 to 20 weight percent, preferably 3 to 17 weight percent, particularly preferably 6 to 15 weight percent of at least one alcohol and / or ester.
[0022] Depending on the application, the recyclable material according to the present invention may comprise at least one additive. The at least one additive may be used to add additional physical, optical, tactile, or chemical properties to the recyclable material or to specifically modify such properties. For example, the recyclable material may be colored with a dye or pigment. It is preferable that the at least one additive be biodegradable and / or recyclable.
[0023] Preferably, at least one coloring agent or at least one pigment is used as an additive, and in particular, charcoal, vegetable coloring agents, preferably extracted from vegetables or fruits such as beets or carrots.
[0024] The recyclable material according to the present invention can be used to produce all molded parts, in particular packaging materials, fillers, furniture parts, daily necessities, decorative items, cutlery, plates, bags, etc.
[0025] The cellulose material preferably comprises cellulose, cellulose derivatives, lignin, paper or cardboard, or a mixture thereof.
[0026] Accordingly, used paper and / or cardboard may also be used in the recyclable material according to the present invention. As a result, the recyclable material or molded parts manufactured therefrom can be integrated into the recycling cycle of paper and cardboard, particularly to conserve resources and enable environmentally friendly production. Preferably, a cellulose material derived from the recyclable material according to the present invention or a molded part manufactured by it and dissolved in water may be used as the cellulose material. Accordingly, the cellulose material of the recyclable material according to the present invention may be reused in the production of the new recyclable material according to the present invention.
[0027] Preferably, methylcellulose or hydroxymethylcellulose is used as a cellulose derivative. The cellulose may be in the form of cellulose fibers, microcrystalline cellulose, or hemicellulose.
[0028] Preferably, at least one protein binder comprises a plant-based protein binder, in particular grains, soybeans, almonds, hemp, peas, lupine, pumpkin, cassava, sunflower, or a mixture thereof.
[0029] The grain is preferably wheat, rye, barley, oats, rice, corn, millet, or a mixture thereof.
[0030] Preferably, the protein binder comprises at least one animal protein binder, in particular gluten glue, gelatin, collagen, keratin, casein, albumin, or a mixture thereof.
[0031] Gluten glue is preferably bone glue, leather glue, rabbit glue, fish glue, or a mixture thereof.
[0032] At least one alcohol preferably has 1 to 50 carbon atoms. The alcohol is preferably an alcohol having 2 to 30 carbon atoms, particularly an alcohol having 2 to 15 carbon atoms.
[0033] At least one alcohol may be a linear alcohol or a branched alcohol. At least one alcohol may be a monohydric alcohol, but a polyhydric alcohol having 2 to 15 hydroxyl groups, preferably 2 to 10 hydroxyl groups, and particularly 2 to 6 hydroxyl groups is preferred.
[0034] Preferably, at least one alcohol is selected from polyglycerol-3 (CAS 25618-55-7), glycerol ethoxylate (CAS 316954-55-0), pentaerythriol ethoxylate (CAS 30599-15-6), polyethylene glycol E400 (CAS 25322-68-3), glycerol (CAS 56-81-5), 1,2-propanediol (CAS 57-55-6), dipentaerythritol (CAS 126-58-9), pentaerythritol (CAS 115-77-5), ethylene glycol (CAS 107-21-1), diethylene glycol (CAS 111-46-6), triethylene glycol (CAS 112-27-6), or a mixture thereof.
[0035] At least one ester is preferably a carboxylic acid ester, having 2 to 22 carbon atoms, particularly 6 to 12 carbon atoms. At least one ester may be a monoester, but is preferably a polyester. In particular, at least one ester is preferably an alkyl citrate or glycerol acetate, particularly triethyl citrate (CAS 77-93-0) or glycerol triacetate (CAS 102-76-1).
[0036] Preferably, the recyclable material according to the present invention comprises starch, at least one monosaccharide, at least one oligosaccharide, or at least one polysaccharide, or a mixture thereof, as at least one additive. Such sugar compounds act as additional binders in the recyclable material, thereby increasing the strength of the recyclable material or maintaining the same strength while reducing the amount of at least one protein binder.
[0037] Preferably, at least one additive is selected from wheat starch, potato starch, rice starch, tapioca starch, dextrin, agar, alginates, pectin, chitin, cyclodextrin, or a mixture thereof. More preferably, the additive may include sugars extracted from extracts of algae, fruits, vegetables and / or grains.
[0038] Preferably, at least one additive may include glucose, fructose, galactose, sucrose, maltose, lactose, maltodextrin, dextrose, isomalt, erythritol, mannitol, xylitol, sugar syrup, invert sugar syrup, or a mixture thereof.
[0039] Preferably, at least one additive comprises sorbitol (CAS 50-70-4), xylitol (CAS 87-99-0), mannitol (CAS 69-65-8), sucrose (CAS 57-50-1), trehalose (CAS 6138-23-4), or a mixture thereof.
[0040] Preferably, at least one additive of the recyclable material comprises urea and / or allantoin. This improves the flow characteristics of the recyclable material before it is dried or cured, thereby enabling the recyclable material to be easily processed into a molded part, for example, during casting.
[0041] At least one additive to the recyclable material preferably includes a preservative. This allows the recyclable material to be stored for a longer period of time before being processed into molded parts.
[0042] Preferably, the additive is selected from ascorbic acid or citric acid or their salts, sorbate, plant extract, or a mixture thereof.
[0043] Alternatively, the additive includes methyl 4-hydroxybenzoate or propyl 4-hydroxybenzoate. However, since these materials are not biodegradable, only a small amount of up to 0.3 weight percent is used, so the entire recyclable material can be composted according to standards, and the environment and water are not at risk.
[0044] Preferably, the recyclable material includes at least one animal or vegetable fat as at least one additive. Adding fat can improve the granulation of the recyclable material.
[0045] At least one fat is preferably linseed oil, castor oil, rapeseed oil, sunflower oil, fat powder, medium-chain triglycerides, or a mixture thereof.
[0046] Preferably, at least one additive of the recyclable material comprises at least one natural wax, in particular carnauba wax, candelilla wax, sugarcane wax, beeswax or stearin, or a mixture thereof.
[0047] Preferably, at least one additive of the recyclable material comprises at least one inorganic material. Preferably, at least one inorganic material may be mica, wollastonite, iron oxide, bentonite, hydromagnesite, chalk, gypsum, lithopone, huntite, talc, magnesium oxide, magnesium carbonate, kaolin, calcium carbonate, vermiculite, silicates, perlite, or a mixture thereof.
[0048] Adding at least one inorganic material can affect the mechanical properties of a recyclable material or a molded part made therefrom. Additionally, adding at least one inorganic material can achieve pigment formation or coloring of the recyclable material and improve the homogeneity of the surface of the molded part made therefrom. Furthermore, the flow properties of the recyclable material can be specifically improved by at least one inorganic material.
[0049] The present application also relates to a method for manufacturing a molded part from a recyclable material. In the first step, 30 to 97 weight percent of a cellulose material, 2 to 45 weight percent of at least one protein binder, 1 to 20 weight percent of at least one alcohol or ester, and 0 to 45 weight percent of at least one additive are provided to a mixer with water as a solvent. The components are then mixed in the mixer to form a recyclable material and then a molded part.
[0050] Depending on the protein binder, it must first be dissolved in warm or boiling water. For components in powder form, it is preferable to dissolve them in water first with heating and / or stirring, depending on the type of component.
[0051] The mixer is preferably a planetary agitator, an eccentric screw pump, a propeller agitator, a disc agitator, an extruder, or a magnetic stirrer.
[0052] It is preferable to mix the components for 1 to 40 minutes, preferably 1 to 10 minutes.
[0053] Preferably, the recyclable material is extruded into a strand after mixing, then a molded part is formed from the strand of the recyclable material, and then the formed molded part is dried.
[0054] Preferably, the recyclable material is mixed and then preferably extruded into a strand, the strand is crushed into granules, a molded part is formed from the granules, and the formed molded part is subsequently dried.
[0055] The granules are preferably dried. It is preferable to store the granules before the molded part is formed. The granules can be transported during storage. This has the advantage of allowing the granules and the molded part to be produced at different geographical locations at different times.
[0056] For example, the granules may be heated to form a molded part, and eventually, the molded part may be formed under high pressure. Alternatively, the granules may be liquefied using a suitable solvent, preferably water, before molding.
[0057] Preferably, extrusion molding is performed at a pressure of 40 to 180 bar, preferably 60 to 140 bar, and particularly preferably 80 to 120 bar.
[0058] Preferably, the recyclable material is dried after mixing and ground into a powder, particularly into a powder with a particle size of less than 0.10 mm, particularly less than 0.05 mm, and a molded part is formed from the powder.
[0059] Preferably, the powder is stored before the molded part is formed. The powder can be transported during storage. This has the advantage of allowing the powder and the molded part to be produced at different geographical locations at different times.
[0060] For example, a molded part can be formed by heating the powder even under applied pressure. Alternatively, the powder may be liquefied using a suitable solvent (preferably water) before molding. If the material is liquefied before the molded part is formed, the molded part dries after formation.
[0061] The powder made of recyclable material according to the present invention is particularly suitable for forming molded parts through 3D printing, especially multi-jet modeling.
[0062] Preferably, the molded part is formed by press molding, casting molding, extrusion molding, rotational molding, vacuum molding, injection molding, sintering, or 3D printing.
[0063] This application also relates to a molded part made of a recyclable material as described above.
[0064] The molded parts are preferably packaging materials, fillers, furniture parts, utility items, decorative items, cutlery, plates, or bags. Specific details for implementing the invention
[0065] Further advantageous embodiments and combinations of the features of the present invention are derived from the following detailed description and the entire scope of the claims.
[0066] example
[0067] Example 1
[0068] In the first example, about 134g of rabbit glue was mixed with 250g of boiling water and heated in a water bath at 70°C for 20 minutes. Then, 101g of casein extracted from cow's milk (nitrogen content 13.5 to 15%) was added to the mixture and vigorously mixed to form a binder component.
[0069] 40g of glucose and 16g of magnesium sulfate were dissolved in boiling water (glucose in 40g of water and magnesium sulfate in 20g of water) and added to the binder components and mixed. When the mixture became homogeneous, 1.6g of methyl 4-hydroxybenzoate and propyl 4-hydroxybenzoate (69:31) were added and mixed.
[0070] The intermediate was mixed with liquid additives and fibers. Specifically, 64 g of sorbitol and 12 g of castor oil were added to the mixture and mixed vigorously. Finally, 432 g of fibers (hydroxypropylmethylcellulose and cellulose of about 200 μm, in a 50:50 ratio) were added and mixed vigorously in an oil stirrer (rotor stirrer 10 L).
[0071] This material was extruded into strands in a hydraulic press (Lindenberg press 60 tons) at a pressure of approximately 140 bar through a compression device consisting of a piston and a ram equipped with a nozzle with a diameter of 2 mm. After drying, the strands were cut into pieces 2 mm long, and the resulting granules were injection molded into molded parts and then dried.
[0072] ingredient Weight percentage relative to total amount Amount [g] rabbit glue 16.7 133.608 casein 12.6 100.792 Hydroxypropylmethylcellulose HPMC 27 216 Cellulose 200μm 27 216 Paraben 0.2 1.6 Sorbitol 8 64 Glucose 5 40 Magnesium sulfate MgSO4 2 16 Castor oil 1.5 12 Total of all components 100 800
[0073] Example 2
[0074] In the second example, 1.6g of potassium benzoate and 16g of magnesium sulfate were dissolved in 250g of boiling water. Then, 116g of glycerol was added to the mixture.
[0075] 234g of gluten protein (general nutritional information: protein 80wt%, fiber 3.8wt%, fat 5.8wt%, carbohydrate 4.7wt%, salt 0.13wt%) was mixed with 416g of cellulose fiber (approx. 150μm).
[0076] A binder component is obtained by mixing the powder mixture and the liquid mixture together.
[0077] Finally, 16g of nut oil was added and mixed vigorously in an oil stirrer.
[0078] This material was extruded into a strand in a hydraulic press at a pressure of approximately 140 bar through a compression device comprising a piston and a plunger with a nozzle of 2 mm in diameter. After drying, the strand was cut into pieces 2 mm long, and the resulting granules were injection molded into molded parts and then dried.
[0079] ingredient Weight percentage relative to total amount Amount [g] gluten 29.3 234.4 Cellulose 150 μm 52 416 Potassium benzoate 0.2 1.6 Glycerol 14.5 116 Magnesium sulfate MgSO4 2 16 Nut oil 2 16 Total components 100 800
[0080] Example 3
[0081] In the third example, 109.2g of isolated soy protein (general nutritional information: protein 90wt%, fat 1.5wt%, carbohydrate 1.8wt%, salt 0.5wt%) was mixed in a bowl with 109.2g of tapioca starch (general nutritional information: protein 0.2wt%, fat <0.1wt%, carbohydrate 87.8wt%, salt <0.1wt%), 40g of xanthan gum, 2g of a mixture of methyl 4-hydroxybenzoate and propyl 4-hydroxybenzoate (69:31), and 416g of cellulose fiber (approx. 150 μm).
[0082] 28g of glucose and 16g of magnesium sulfate were dissolved in boiling water (glucose in 50g of water, magnesium sulfate in 20g of water), added to the powder mixture, and mixed well. Then, 71g of sorbitol and 8g of coconut oil were added and mixed vigorously.
[0083] 300g of boiling water was added to the previously mixed components and mixed with a sufficiently powerful oil stirrer.
[0084] This material was extruded into strands in a hydraulic press at a pressure of approximately 140 bar through a compression device consisting of a piston and a punch with a nozzle of 2 mm in diameter. After drying, the strands were cut into pieces 2 mm long, and the resulting granules were injection molded into molded parts and then dried.
[0085] ingredient Weight percentage relative to total amount Amount [g] Soy protein 13.65 109.2 tapioca starch 13.65 109.2 Cellulose 150 μm 52 416 Paraben 0.3 2 Sorbitol 8.9 71 Glucose 3.5 28 Magnesium sulfate MgSO4 2 16 Xanthan sword 5 40 coconut oil 1 8 Total components 100 800
[0086] Example 4
[0087] In the fourth example, 16g of lactose, 24g of maltodextrin, 1.6g of potassium benzoate, and 16g of magnesium sulfate were dissolved in 330g of boiling water. Then, 107.2g of fish glue was added and mixed, and then heated in a water bath at 70°C for 20 minutes.
[0088] 107.2g of gluten protein (general nutrient information: protein 80wt%, fiber 3.8wt%, fat 5.8wt%, carbohydrate 4.7wt%, salt 0.13wt%) was mixed with 480g of cellulose fiber (approx. 150μm).
[0089] 40g of 1,2-propanediol and 8g of nut oil were added to the liquid mixture.
[0090] The powder mixture and the liquid mixture were mixed together.
[0091] This material was extruded into a strand in a hydraulic press at a pressure of approximately 140 bar through a compression device including a piston and a punch with a nozzle of 2 mm in diameter. After drying, the strand was cut into 2 mm lengths, and the resulting granules were injection molded into a molded part and then dried.
[0092] ingredient Weight percentage relative to total amount Amount [g] gluten protein 13.4 107.2 fish glue 13.4 107.2 Cellulose 150 μm 60 480 Potassium benzoate 0.2 1.6 1,2-propanediol 5 40 Lactose 2 16 Magnesium sulfate MgSO4 2 16 Maltodextrin 3 24 Nut oil 1 8 Total components 100 800
[0093] Example 5
[0094] In the fifth example, 134g of gelatin was mixed with 310g of boiling water and then heated in a water bath at 70℃ for 20 minutes.
[0095] Then, 100.8g of albumin was mixed in a 1:1 ratio with isolated pea protein (general nutrient information: protein 80wt%, fat 5.5wt%, carbohydrate 2.6wt%, salt 1.9wt%) and about 38g of maltodextrin.
[0096] A binder component was obtained by mixing the powder mixture and the liquid mixture together.
[0097] Dissolve 16g of magnesium sulfate in 20g of boiling water, add it to a mixture with 80g of 1,2-propanediol, and mix.
[0098] Finally, 432g of fiber (cellulose, approximately 200μm) was added and vigorously mixed with an oil stirrer.
[0099] This material was extruded into a strand in a hydraulic press at a pressure of approximately 140 bar through a compression device including a piston and a punch with a nozzle of 2 mm in diameter. After drying, the strand was cut into 2 mm lengths, and the resulting granules were injection molded into a molded part and then dried.
[0100] ingredient Weight percentage relative to total amount Amount [g] gelatin 16.7 133.61 albumin 6.3 50.40 isolated pea protein 6.3 50.40 Cellulose 200 μm 54 432 1,2-propanediol 10 80 Maltodextrin 4.7 37.6 Magnesium sulfate MgSO4 2 16 Total components 100 800.01
[0101] Processing recyclable materials through sintering
[0102] A certain amount of granules of recyclable material was placed into a pressing tool having the contour of the molded part to be produced. The tool was heated to a temperature of 150°C in a heated press, and after filling with granules, it was compressed for 2 minutes at a pressure of 1 kg / ㎠. Then, the tool containing the molded part was removed from the press, cooled to a temperature of 50°C, and the manufactured molded part was removed.
[0103] Alternatively, the powder can be sintered and used for processing.
[0104] Processing Recyclable Materials via Extrusion
[0105] Granules of recyclable material were processed into profiles with various cross-sections using an extrusion molding system (Weber ES45) with a short compression screw at an operating temperature of 120 to 140°C.
[0106] Processing Recyclable Materials via 3D Printing
[0107] Powder made from recyclable materials was filled into a designated container of a 3D printer (3DSystems' ZPrinter ⓒ 150) operating according to the multi-jet modeling process, and Z-Corp's original binder was replaced with water. After the printing process, the molded part was removed and dried.
Claims
Claim 1 A recyclable material for molding comprises: a) 30 to 97 weight percent of a cellulose material; b) 2 to 45 weight percent of at least one protein binder; c) 1 to 20 weight percent of at least one alcohol and / or at least one ester; and d) up to 45 weight percent of at least one additive; wherein the at least one additive comprises at least one inorganic material, and the at least one inorganic material comprises magnesium sulfate. Claim 2 A recyclable material according to claim 1, characterized in that the cellulose material comprises cellulose, a cellulose derivative, lignin, paper or cardboard, or a mixture thereof. Claim 3 A recyclable material according to claim 1 or 2, characterized in that at least one of the protein binders comprises a plant-based protein binder. Claim 4 A recyclable material according to claim 1 or 2, wherein the protein binder comprises at least one animal protein binder. Claim 5 A recyclable material according to claim 1 or 2, characterized in that at least one of the alcohols has 1 to 50 carbon atoms. Claim 6 A recyclable material according to claim 1 or 2, characterized in that the recyclable material comprises starch, at least one monosaccharide, at least one oligosaccharide, or at least one polysaccharide, or a mixture thereof as the additive. Claim 7 A recyclable material according to claim 1 or 2, characterized in that the material comprises urea and / or allantoin as the additive. Claim 8 A recyclable material according to claim 1 or 2, characterized in that the recyclable material comprises a preservative as an additive. Claim 9 A recyclable material according to claim 1 or 2, characterized in that the recyclable material comprises at least one animal fat or vegetable fat as the additive. Claim 10 A recyclable material according to claim 1 or 2, characterized in that the recyclable material comprises at least one natural wax. Claim 11 A recyclable material according to claim 1 or 2, wherein at least one inorganic material further comprises mica, wollastonite, iron oxide, bentonite, hydromagnesite, chalk, gypsum, lithopone, huntite, talc, magnesium oxide, magnesium carbonate, kaolin, calcium carbonate, vermiculite, silicates, perlite, or a mixture thereof. Claim 12 A method for producing a molded part from a recyclable material according to claim 1, comprising: a) providing 30 to 97 weight percent of a cellulose material, 2 to 45 weight percent of at least one protein binder, 1 to 20 weight percent of at least one alcohol or ester, and up to 45 weight percent of at least one additive to a mixer with water as a solvent, wherein the at least one additive comprises at least one inorganic material, and the at least one inorganic material comprises magnesium sulfate; b) mixing the components in the mixer to produce the recyclable material; and c) forming the molded part from the recyclable material; the method. Claim 13 A method according to claim 12, characterized in that the recyclable material is extruded into a strand after mixing, then a molded part is formed from the strand of the recyclable material, and then the molded part is dried. Claim 14 A method according to claim 12, characterized in that the recyclable material is extruded into a strand after mixing, the strand is crushed into granules, the molded part is then formed from the granules, and the molded part is then dried. Claim 15 A method according to claim 13 or 14, characterized in that the extrusion molding is performed at a pressure of 40 to 180 bar. Claim 16 A method according to claim 12, characterized in that the recyclable material is dried and ground into powder after mixing. Claim 17 A method according to claim 12 or 13, characterized in that the molded part is formed by press molding, casting molding, extrusion molding, rotational molding, vacuum molding, injection molding, sintering, or 3D printing. Claim 18 A molded part produced from a recyclable material according to claim 1 or 2. Claim 19 In claim 1 or 2, the recyclable material comprises 2 weight percent magnesium sulfate.
Citation Information
Patent Citations
Environmentally friendly materials, or molded articles made therefrom, methods for manufacturing the same, and their use
JP1997500924A
Biodegradable thermoplastic composition mainly composed of protein and starch
JP2002512929A
Biodegradable material made of biological components
KR1020140145153A