Silicone based thermoplastic elastomer composition and manufacturing method thereof

A silicone-based thermoplastic elastomer composition addresses the technological gap by enhancing compatibility and heat resistance, enabling stable production and improved mechanical properties for applications in automotive and wearable devices.

KR103046513B1Active Publication Date: 2026-11-11GRACE CONTINENTAL KOREA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020230169565
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2026-11-11
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

The domestic manufacturing technology for silicon-based thermoplastic elastomers lacks sufficient technical capability, resulting in a significant technological gap compared to overseas markets, leading to reliance on imports and difficulty in meeting performance requirements and securing price competitiveness.

Method used

A silicone-based thermoplastic elastomer composition comprising specific components such as polyorganosiloxane, silica, silicone oil, organohydrogenpolysiloxane curing agent, surface modifier, and platinum-based catalyst, which enhances compatibility, heat resistance, and mechanical properties, enabling stable product production and high melt viscosity for dynamic crosslinking and melt injection molding processes.

Benefits of technology

The composition achieves excellent miscibility and compatibility with thermoplastic materials, high heat resistance, light transmittance, chemical resistance, and wear resistance, with improved mechanical properties and flexibility, suitable for applications in automotive and wearable devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023133692564-PAT00012_ABST
    Figure 112023133692564-PAT00012_ABST
Patent Text Reader

Abstract

The present invention relates to a silicone-based thermoplastic elastomer composition and a method for manufacturing the same. In one embodiment, the silicone-based thermoplastic elastomer composition comprises 100 parts by weight of a polyorganosiloxane represented by the following chemical formula 1; 5 to 100 parts by weight of silica; 0.5 to 15 parts by weight of a silicone oil having a silanol group at one end; 1 to 20 parts by weight of an organohydrogenpolysiloxane curing agent; 0.5 to 15 parts by weight of a surface modifier; and 0.001 to 5 parts by weight of a platinum-based catalyst; wherein the surface modifier comprises a silane-based compound having one or more functional groups selected from epoxy groups, glycidoxy groups, phenyl groups, hydroxyl groups, isocyanate groups, vinyl groups, and acid anhydride groups: [Chemical Formula 1] (The above Chemical Formula 1 is as defined in the detailed description).
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a silicon-based thermoplastic elastomer composition and a method for manufacturing the same. Background Technology

[0003] Thermoplastic elastomers (TPEs) are materials used in various fields because they possess both the elastic properties of rubber and the thermoplastic properties of general plastics.

[0004] Meanwhile, silicone-based thermoplastic elastomers are thermoplastic elastomers that use silicone rubber as the cross-linked particles in the dispersed phase. Silicone-based thermoplastic elastomers have the advantage of excellent chemical resistance, scratch resistance, and a flexible tactile feel compared to general thermoplastic materials (TPE).

[0005] In this context, the smaller the size and the better the dispersibility of the cross-linked silicone rubber, the more effective it is in reinforcing the physical properties of thermoplastic elastomers. Therefore, the dispersibility between silicone rubber and TPE materials has become a critical factor for silicone-based thermoplastic elastomers, and there is a growing need to develop silicone rubber materials optimized for manufacturing processes that possess excellent compatibility with TPE materials.

[0006] With the recent expansion of applications for silicon-based thermoplastic elastomers in autonomous vehicles, electric vehicles, wearable devices, and human robots, there is an urgent need to secure domestic technology for silicon-based thermoplastic elastomers.

[0007] However, domestic manufacturing technology for silicon-based thermoplastic elastic materials lacks sufficient technical capability, resulting in a significant technological gap compared to overseas markets. Consequently, the industry cannot meet the performance requirements of the domestic market and relies heavily on imports, which makes it difficult to secure price competitiveness for products.

[0008] The background technology related to the present invention is disclosed in Korean Registered Patent Publication No. 10-0123018 (published Nov. 12, 1997, Title of Invention: Thermoplastic Material Composition). The problem to be solved

[0010] One objective of the present invention is to provide a silicone-based thermoplastic elastomer composition having excellent miscibility, compatibility, and heat resistance.

[0011] Another objective of the present invention is to provide a silicon-based thermoplastic elastomer composition having excellent light transmittance, chemical resistance, and wear resistance.

[0012] Another objective of the present invention is to provide a silicon-based thermoplastic elastomer composition having excellent stiffness, durability, and flexibility.

[0013] Another objective of the present invention is to provide a method for manufacturing the above-mentioned silicon-based thermoplastic elastomer composition.

[0014] Another objective of the present invention is to provide a molded article manufactured using the above-described silicon-based thermoplastic elastomer composition. means of solving the problem

[0016] One aspect of the present invention relates to a silicone-based thermoplastic elastomer composition. In one embodiment, the silicone-based thermoplastic elastomer composition comprises 100 parts by weight of a polyorganosiloxane represented by the following chemical formula 1; 5 to 100 parts by weight of silica; 0.5 to 15 parts by weight of a silicone oil having a silanol group at one end; 1 to 20 parts by weight of an organohydrogenpolysiloxane curing agent; 0.5 to 15 parts by weight of a surface modifier; and 0.001 to 5 parts by weight of a platinum-based catalyst; wherein the surface modifier comprises a silane-based compound having one or more functional groups selected from epoxy groups, glycidoxy groups, phenyl groups, hydroxyl groups, isocyanate groups, vinyl groups, and acid anhydride groups:

[0017] [Chemical Formula 1]

[0018]

[0019] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.)

[0020] In one embodiment, the silicone-based thermoplastic elastomer composition further comprises 50 to 1,000 parts by weight of a thermoplastic material per 100 parts by weight of the polyorganosiloxane, wherein the thermoplastic material may comprise one or more of a thermoplastic resin and a thermoplastic elastomer.

[0021] In one embodiment, the polyorganosiloxane may have an alkenyl group content of 0.01 mol% to 5 mol% and a weight-average molecular weight of 300,000 to 800,000 g / mol.

[0022] In one embodiment, the silane compound may include one or more of monomers, dimers, and oligomers.

[0023] In one embodiment, the silicone elastomer composition further comprises 0.01 to 5 parts by weight of a curing retardant per 100 parts by weight of the polyorganosiloxane, and the curing retardant may include one or more of alkyne alcohol-based, n-phosphorus-based, cyclosiloxane-based, and triazole-based curing retardants.

[0024] In one embodiment, the silicone oil and surface modifier having a silanol group at the exponent may be included in a weight ratio of 1:0.5 to 1:3.

[0025] In one embodiment, the silicone oil having a silanol group at the exponent may have a hydroxyl group content of 1 to 10 weight% and a kinematic viscosity of 5,000 to 20,000 cSt.

[0026] Another aspect of the present invention relates to a method for preparing the above-mentioned silicone-based thermoplastic elastomer composition. In one embodiment, the method for preparing the above-mentioned silicone-based thermoplastic elastomer composition comprises the step of preparing a first mixture comprising a polyorganosiloxane represented by the following chemical formula 1, silica, a silicone oil having a silanol group at one end, and a surface modifier; The method comprises the step of preparing a second mixture comprising the first mixture, an organohydrogenpolysiloxane curing agent, and a platinum-based catalyst; wherein the silicone-based thermoplastic elastomer comprises 100 parts by weight of the polyorganosiloxane, 5 to 100 parts by weight of silica, 0.5 to 15 parts by weight of silicone oil having a silanol group at one end, 1 to 20 parts by weight of the organohydrogenpolysiloxane curing agent, 0.5 to 15 parts by weight of a surface modifier, and 0.001 to 5 parts by weight of a platinum-based catalyst, and wherein the surface modifier comprises a silane-based compound comprising one or more functional groups selected from epoxy groups, glycidoxy groups, phenyl groups, hydroxyl groups, isocyanate groups, vinyl groups, and acid anhydride groups:

[0027] [Chemical Formula 1]

[0028]

[0029] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.)

[0030] In one embodiment, the second mixture further comprises 50 to 1,000 parts by weight of a thermoplastic material based on 100 parts by weight of the polyorganosiloxane, and the thermoplastic material may comprise one or more of a thermoplastic resin and a thermoplastic elastomer.

[0031] In one embodiment, the silane compound may include one or more of monomers, dimers, and oligomers.

[0032] Another aspect of the present invention relates to a molded article manufactured using the above-described silicon-based thermoplastic elastomer composition. Effects of the invention

[0034] The silicone-based thermoplastic elastomer composition according to the present invention has excellent mixability and compatibility, excellent mixability with thermoplastic materials, excellent heat resistance, excellent light transmittance, chemical resistance and wear resistance, and may have excellent rigidity, durability and flexibility. Specific details for implementing the invention

[0036] In describing the present invention, if it is determined that a detailed description of related known technologies or configurations could unnecessarily obscure the essence of the invention, such detailed description will be omitted.

[0037] Furthermore, the terms described below are defined in consideration of their functions in the present invention; since these may vary depending on the intentions or practices of the user or operator, their definitions should be based on the content throughout this specification describing the present invention.

[0039] Silicone-based thermoplastic elastomer composition

[0040] One aspect of the present invention relates to a silicon-based thermoplastic elastomer composition.

[0041] The above-mentioned silicone-based thermoplastic elastic material has a wider range of applications than thermoplastic vulcanized rubber (TPV) due to its superior physical properties and flexible tactile feel. To respond to the expanded market, the present invention aims to secure basic technology applicable to the development of silicone-based thermoplastic elastic materials with stable physical properties by applying a silicone-based composition that has excellent compatibility with thermoplastic materials, such as thermoplastic elastomers, as a top priority.

[0042] The present invention applies a surface modifier having functional groups to manufacture a silicone-based material having compatibility and high heat resistance. In addition, when a silane-based oligomer compound is applied as the surface modifier imparting functional groups, the functional groups are efficiently imparted to the surface of the silane-based oligomer compound, and excellent effects of increasing adhesion and compatibility with thermoplastic materials can be achieved.

[0043] In addition, the silicon-based thermoplastic elastomer composition of the present invention has solved the problems of the prior art as follows.

[0044] (1) Compatibility: Conventional silicone rubber and thermoplastic elastomers (TPEs) have low compatibility, so when manufacturing silicone-based thermoplastic elastomers through dynamic crosslinking, there was a problem of reduced wear resistance. In addition, during the injection molding process, the silicone-based thermoplastic elastomer settles at the die exit, causing die drool and material adhesion phenomena that degrade the quality of the molded product. Due to these problems, it is difficult to achieve a deterioration in the physical properties of the molded product and stable product production. Furthermore, due to the characteristics of dynamic crosslinking and melt injection molding processes, high fluidity, i.e., high melt viscosity, is required to increase shear stress and ensure even dispersion and distribution. In particular, when silane-based oligomer compounds are applied, the compatibility of the composition is excellent, and due to high fluidity, the physical properties of the molded product and productivity can be achieved.

[0045] The present invention enables stable product production by minimizing the problem of reduced wear resistance and the die-droll phenomenon. In addition, by having high melt viscosity, it offers advantages that are more favorable for dynamic crosslinking and melt injection molding processes.

[0046] (2) Translucency: In addition, conventional silicone rubber has a problem in that the transparency of the material is reduced due to light blockage and scattering caused by fillers, additives, and impurities used to reinforce physical properties and increase compatibility. Therefore, to minimize the loss of transparency, products with a uniform nano-scale particle size distribution must be used when selecting fillers and additives. The present invention minimizes the reduction of transparency, thereby having a high self-transmittance, and increases compatibility to reduce the size distributed when dispersed in thermoplastic elastomers (TPE), so that a transparency of 15% or more can be secured even when mixed with thermoplastic elastomers.

[0047] (3) Heat resistance: Silicon-based thermoplastic elastic materials have a wide range of applications. In particular, when applied to the automotive industry, there are areas where sunlight is directly irradiated, so high light resistance and heat resistance are required. The present invention has high heat resistance and can maintain heat resistance characteristics even under conditions of 230°C.

[0049] In one embodiment, the silicone-based thermoplastic elastomer composition comprises 100 parts by weight of a polyorganosiloxane represented by the following chemical formula 1; 5 to 100 parts by weight of silica; 0.5 to 15 parts by weight of a silicone oil having a silanol group at one end; 1 to 20 parts by weight of an organohydrogenpolysiloxane curing agent; 0.5 to 15 parts by weight of a surface modifier; and 0.001 to 5 parts by weight of a platinum-based catalyst; wherein the surface modifier comprises a silane-based compound having one or more functional groups selected from epoxy groups, phenyl groups, hydroxyl groups, isocyanate groups, vinyl groups, and acid anhydride groups:

[0050] [Chemical Formula 1]

[0051]

[0052] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.)

[0053] Hereinafter, the constituent components of the above-mentioned silicone-based thermoplastic elastomer composition will be described in detail.

[0055] Polyorganosiloxane

[0056] The above polyorganosiloxane is represented by the following chemical formula 1:

[0057] [Chemical Formula 1]

[0058]

[0059] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.)

[0060] In one embodiment, the linear or branched alkyl groups having 1 to 10 carbon atoms include methyl, ethyl, normal propyl, isopropyl, normal butyl, isobutyl, tertiary butyl, normal pentyl, isopentyl, neopentyl, hexyl, heptyl, octyl, nonyl, and decyl.

[0061] In one embodiment, the aminoalkyl group having 1 to 10 carbon atoms includes a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, a dipropylamino group, and a dibutylamino group.

[0062] In one embodiment, the hydroxyalkyl group having 1 to 10 carbon atoms includes hydroxymethyl, hydroxyethyl, and hydroxypropyl.

[0063] In one embodiment, the above-mentioned haloalkyl groups having 1 to 20 carbon atoms include fluoroalkyl groups such as trifluoropropyl, heptafluoropentyl, heptafluoroisopentyl, tridecafluorooctyl, and heptadecafluorodecyl; and chloroalkyl groups such as chloromethyl, chloroethyl, and chloropropyl.

[0064] In one embodiment, the cycloalkyl group having 3 to 15 carbon atoms includes cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, cycloundecyl, cyclododecyl, butylcyclopropyl, methylcyclopentyl, dimethylcyclohexyl, ethyldimethylcycloheptyl, and dimethylcyclooctyl.

[0065] In one embodiment, the aryl group having 6 to 12 carbon atoms includes phenyl groups, tolyl groups, xyl groups, and naphthyl groups.

[0066] In one embodiment, the above aralkyl groups having 7 to 20 carbon atoms include methylphenyl groups, ethylphenyl groups, methylnaphthyl groups, and dimethylnaphthyl groups.

[0067] In one embodiment, the alkenyl groups having 2 to 20 carbon atoms include vinyl groups, propynyl groups, butynyl groups, fentinyl groups, hexinyl groups, octinyl groups, decinyl groups, hexadecinyl groups, and octadecinyl groups.

[0068] For example, the above-mentioned polyorganosiloxane may include polydimethylvinylsiloxane.

[0069] In one embodiment, the alkenyl group content of the polyorganosiloxane may be 0.01 mol% to 5 mol%. Within this range, the curing properties and the physical properties of the molded member of the present invention may be excellent.

[0070] In one embodiment, the weight-average molecular weight (Mw) of the polyorganosiloxane may be 300,000 g / mol to 800,000 g / mol. Within this range, the mechanical properties and processability of the present invention may be excellent.

[0071] In one embodiment, the polyorganosiloxane may have a viscosity of 10,000,000 cps to 150,000,000 cps measured at 25°C. At the viscosity under these conditions, excellent dispersibility and ease of processing may be achieved between the silica and other components described later.

[0072] In one embodiment, the polyorganosiloxane may use a mixture of two or more types of polyorganosiloxanes with different viscosities. In one embodiment, the polyorganosiloxane may comprise 60 to 80 weight% of a first polyorganosiloxane having an alkenyl group content of 0.01 to 0.05 mol% and a weight-average molecular weight of 600,000 to 750,000 g / mol, 10 to 30 weight% of a second polyorganosiloxane having an alkenyl group content of 1 to 5 mol% or 2 to 4.5 mol% and a weight-average molecular weight of 650,000 to 750,000 g / mol, and 3 to 15 weight% of a third polyorganosiloxane having an alkenyl group content of 0.05 to 0.5 mol% or 0.1 to 0.3 mol% and a weight-average molecular weight of 600,000 to 720,000 g / mol. In the above mixing range, the mechanical properties, dispersibility, and processability of the present invention may be excellent. For example, the alkenyl group is a vinyl group, and the first to third polyorganosiloxanes may each include polydimethylvinylsiloxane.

[0073] In another embodiment, the polyorganosiloxane may be used by mixing 90 to 99 weight% of a first polyorganosiloxane having an alkenyl group content of 0.01 to 0.05 mol% and a weight-average molecular weight of 600,000 to 750,000 g / mol, and 1 to 10 weight% of a second polyorganosiloxane having an alkenyl group content of 1 to 5 mol% or 2 to 4.5 mol% and a weight-average molecular weight of 650,000 to 750,000 g / mol. When mixed under the above conditions, the dispersibility and processability of the polyorganosiloxane with the silica described below may be excellent. For example, the alkenyl group may be a vinyl group, and the first and second polyorganosiloxanes may each be polydimethylvinylsiloxane.

[0075] silica

[0076] The above silica is included in the present invention for the purpose of improving mechanical strength. The silica may be amorphous or crystalline. The silica may include one or more of fumed silica and precipitated silica.

[0077] In one embodiment, the silica has a specific surface area (BET method) of 100 m² 2 / g to 400 m 2 A value of / g can be used. The mechanical properties of the present invention may be excellent at the above specific surface area. For example, 100 m 2 / g to 300 m 2 You can use / g.

[0078] In one embodiment, the silica has an average particle size of 5 nm to 30 µm and a specific gravity of 1.5 to 2.5 g / cm³ 3 It may be possible. Since dispersion is easy within the above range, workability and strength improvement may be excellent. Meanwhile, in the present invention, the particle "size" of silica is defined as meaning the "maximum length" of the silica particle.

[0079] In one embodiment, the silica may be surface-treated with one or more of a silane-based surface treatment agent and a silazane-based surface treatment agent. In one embodiment, the silane-based surface treatment agent may include one or more of methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, decyltrimethoxysilane, trifluoropropyltrimethoxysilane, hexamethyldisiloxane, trimethylmethoxysilane, ethyltrimethoxysilane, trimethylethoxysilane, and dimethyldiethoxysilane.

[0080] In one embodiment, the silazane-based surface treatment agent may include one or more of divinyltetramethyldisilazane, octamethylcyclotetrasilazane, and hexamethyldisilazane.

[0081] When the above-mentioned surface-treated silica is applied to silicone rubber, excellent mechanical properties, high transparency, and resistance to yellowing can be imparted, and the increase in plasticity can be controlled by suppressing the formation of hydrogen bonds through reaction with moisture in the air.

[0082] In one embodiment, the silica is included in an amount of 5 to 100 parts by weight per 100 parts by weight of the polyorganosiloxane. Within this range, the mechanical strength and dispersibility of the present invention are excellent. If the silica is included in an amount less than 5 parts by weight, the mechanical properties of the present invention are poor, and if it is included in an amount exceeding 100 parts by weight, the mechanical properties may deteriorate, and productivity and workability may be reduced due to severe crepe hardening. For example, it may be included in an amount of 10 to 70 parts by weight. As another example, it may be included in an amount of 25 to 65 parts by weight, 30 to 55 parts by weight, or 30 to 45 parts by weight.

[0084] Silicone oil having silanol groups on one end

[0085] The silicone oil having a silanol group at one end of the above-mentioned exponent may refer to a silicone oil containing a siloxane (Si-O) bond and having a silanol group (Si-O-H) at one or more ends of the molecule.

[0086] When a silicone oil having silanol groups is applied to the above-mentioned end, the mechanical properties of the composition, such as mixability and heat resistance, can be excellent.

[0087] In one embodiment, the siloxane oil having a silanol group at one end may have a hydroxyl group content of 1 to 10 weight% and a kinematic viscosity of 5,000 to 20,000 cSt. Under these conditions, moldability and mixability may be excellent.

[0088] In one embodiment, 0.5 to 15 parts by weight of a siloxane oil having a silanol group at one end is included with respect to 100 parts by weight of the polyorganosiloxane. If the siloxane oil having a silanol group at one end is included in an amount less than 0.5 parts by weight, the mixability and moldability of the composition are reduced and mechanical properties such as heat resistance are reduced; if it is included in an amount exceeding 15 parts by weight, the mixability and moldability are reduced and the mechanical properties of the composition may be reduced. For example, it may be included in an amount of 0.5 to 10 parts by weight, 1 to 8 parts by weight, or 1 to 5 parts by weight.

[0090] thermoplastic materials

[0091] The above thermoplastic material may be included to reinforce durability and mechanical properties. The above thermoplastic material includes one or more of a thermoplastic resin and a thermoplastic elastomer.

[0092] In one embodiment, the thermoplastic resin may include one or more of polyolefin resin, (meth)acrylic resin, polyvinyl chloride (PVC) resin, and polyvinyl alcohol (PVA) resin.

[0093] The above polyolefin resin may include one or more of polyethylene resin and polypropylene resin. The above "(meth)acrylic" may include one or more of "acrylic" and "methacrylic".

[0094] The above thermoplastic elastomer possesses both plasticity and rubber elasticity and may be capable of injection molding at high temperatures. In one embodiment, the thermoplastic elastomer may include one or more of a polyurethane elastomer (TPU), a styrene copolymer, and a polyolefin elastomer (POE).

[0095] In one embodiment, the polyolefin elastomer may include one or more of an ethylene-alpha-olefin copolymer, a propylene-alpha-olefin copolymer, an ethylene-vinyl acetate (EVA) copolymer, an ethylene-methyl acrylate (EMA) copolymer, an ethylene-ethyl acrylate (EEA) copolymer, an ethylene glycol dimethacrylate (EDM) copolymer, and an ethylene-propylene-diene monomer (EPDM) copolymer.

[0096] The above styrene-based copolymer may include styrene-based block copolymers (SBC), etc. For example, the above styrene-based copolymer may include one or more of styrene-butadiene-styrene (SBS), styrene-ethylene-butadiene-styrene (SEBS), and acrylonitrile-styrene-acrylate (ASA).

[0097] In one embodiment, the silicone-based thermoplastic elastomer composition may further include 50 to 1,000 parts by weight of a thermoplastic material per 100 parts by weight of the polyorganosiloxane. When included within the above range, excellent mixability and compatibility are achieved, and mechanical properties such as heat resistance, flexibility, and durability may be excellent without reducing light transmittance. For example, it may be included in an amount of 100 to 500 parts by weight, 150 to 300 parts by weight, or 150 to 250 parts by weight.

[0099] Organohydrogenpolysiloxane curing agent

[0100] The above organohydrogenpolysiloxane curing agent is included to form an addition-type curing in the presence of the catalyst of the present invention.

[0101] In one embodiment, the organohydrogenpolysiloxane curing agent may have an average of two or more silicon-bonded hydrogen atoms (Si-H) per molecule. For example, it may have an average of two or more silicon-bonded hydrogen atoms per molecule and an average of one or fewer silicon-bonded hydrogen atoms per silicon atom. The silicon-bonded hydrogen atoms may be located at the terminal or side chain of the organohydrogenpolysiloxane, or at both the terminal and side chain positions.

[0102] The siloxane unit that may be included in the above organohydrogenpolysiloxane is HR2SiO 1 / 2 , R3SiO 1 / 2 , HRSiO 2 / 2 , R2SiO 2 / 2 , RSiO 3 / 2 and SiO 4 / 2 There are units, etc. In the above chemical formula, R may each independently be an alkyl group having 1 to 20 carbon atoms, a haloalkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an alkenyl group having 2 to 20 carbon atoms. For example, R may be a methyl group. For example, the organohydrogenpolysiloxane may contain 50 mol% or more of methyl groups.

[0103] In one embodiment, the organohydrogenpolysiloxane may be a single organohydrogenpolysiloxane or a mixture of two or more different organohydrogenpolysiloxanes.

[0104] In one embodiment, the organohydrogenpolysiloxane may include 1-octadecyl-1,3,5,7,9-pentamethylcyclopentasiloxane.

[0105] As another example, the above organohydrogenpolysiloxane may include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, methylhydrogensiloxane cyclic polymer, dimethylsiloxane-methylhydrogensiloxane copolymer blocked by trimethylsiloxy groups at both ends, methylhydrogensiloxane-diphenylsiloxane copolymer blocked by trimethylsiloxy groups at both ends, and polymethylhydrogensiloxane.

[0106] In one embodiment, the organohydrogenpolysiloxane curing agent is included in an amount of 1 to 20 parts by weight per 100 parts by weight of the polyorganosiloxane. When included within this range, the curing of the composition can be easily achieved. If the organohydrogenpolysiloxane curing agent is included in an amount of less than 1 part by weight, curing does not occur easily, resulting in a decrease in the mechanical strength of the present invention, and if included in an amount exceeding 20 parts by weight, the durability, etc., of the present invention may be reduced. For example, it may be included in an amount of 1 to 15 parts by weight, 1 to 10 parts by weight, or 3 to 8 parts by weight.

[0107] In one embodiment, the silicone-based thermoplastic elastomer composition may include a siloxane oil having a silanol group at one end and an organohydrogenpolysiloxane curing agent in a weight ratio of 1:1 to 1:6. When included in the above weight ratio, the mixability and formulation stability are excellent, and the heat resistance, durability, and mechanical properties of the composition may be excellent. For example, it may be included in a weight ratio of 1:1.5 to 1:4. As another example, it may be included in a weight ratio of 1:2 to 1:4.

[0109] Surface modifier

[0110] The above surface modifier is included to increase compatibility and heat resistance with the thermoplastic material and the components of the silicone-based elastomer composition.

[0111] The above surface modifier comprises a silane-based compound having one or more functional groups selected from epoxy, glycidoxy, phenyl, hydroxy, isocyanate, vinyl, and acid anhydride groups. Under the above conditions, it exhibits excellent miscibility with components of silicone-based thermoplastic elastomer compositions, such as thermoplastic materials, and can increase light transmittance, compatibility, and heat resistance.

[0112] In one embodiment, the silane compound is glycidoxypropyl trimethoxysilane, glycidoxypropyl triethoxysilane, gamma-isocyanatopropyl trimethoxysilane, gamma-isocyanatopropyl triethoxysilane, hydroxymethyl triethoxysilane, hydroxyethylaminopropyl triethoxysilane, hydroxyethyl-N-methylaminopropyl trimethoxysilane, 3-(Triethoxysilyl)propylsuccinic anhydride, It may include one or more of trimethoxyphenylsilane and triethoxyphenylsilane.

[0113] In one embodiment, the silane compound may include one or more of monomers, dimers, and oligomers.

[0114] In one embodiment, the silane monomer may include one or more of a phenyl group-containing silane compound and an epoxy group-containing silane compound. For example, it may include a silane oligomer.

[0115] The above silane-based oligomer can be prepared by hydrolyzing one or more of the above silane monomers in the presence of a catalyst. The manufacturing process of the above silane-based oligomer will be described later.

[0116] The above silane-based oligomer may include one or more functional groups per molecule selected from epoxy, glycidoxy, phenyl, hydroxy, isocyanate, vinyl, and acid anhydride groups. Under these conditions, the composition may exhibit excellent compatibility and miscibility, as well as excellent mechanical properties such as light transmittance and heat resistance.

[0117] In one embodiment, the silane-based oligomer may have a weight-average molecular weight (Mw) of 500 to 10,000 g / mol. Under these conditions, mechanical properties such as miscibility, light transmittance, and heat resistance of the composition may be excellent. For example, the silane-based oligomer may have a weight-average molecular weight of 1,000 to 5,000 g / mol or 1,500 to 4,000 g / mol.

[0118] In one embodiment, the silane-based oligomer may have a number average molecular weight (Mn) of 300 to 7,000 g / mol. In another example, the number average molecular weight may be 1,200 to 3,500 g / mol.

[0119] In one embodiment, the surface modifier is included in an amount of 0.5 to 15 parts by weight per 100 parts by weight of the polyorganosiloxane. If the surface modifier is included in an amount less than 0.5 parts by weight, the mixability and compatibility are reduced, and the mechanical strength and light transmittance of the composition are reduced; if it is included in an amount exceeding 15 parts by weight, the mixability and compatibility are reduced, and the heat resistance and mechanical strength of the composition may be reduced. For example, it may be included in an amount of 0.5 to 10 parts by weight, 0.5 to 8 parts by weight, 1 to 6 parts by weight, or 1 to 4 parts by weight.

[0120] In one embodiment, the silicone oil having a silanol group at one end and the surface modifier may be included in a weight ratio of 1:0.5 to 1:3. When included in the above weight ratio, the mixability and formulation stability are excellent, and the heat resistance, durability, and mechanical properties of the composition may be excellent. For example, it may be included in a weight ratio of 1:0.5 to 1:2. As another example, it may be included in a weight ratio of 1:1 to 1:2.

[0121] In another embodiment, the silicone-based thermoplastic elastomer composition may include a siloxane oil having a silanol group at one end, a surface modifier, and an organohydrogenpolysiloxane curing agent in a weight ratio of 1:0.5 to 3:1 to 6. When included in the above weight ratios, the mixability and formulation stability are excellent, and the transparency, heat resistance, durability, and mechanical properties of the composition may be excellent. For example, it may be included in a weight ratio of 1:0.5 to 2:1.5 to 4. As another example, it may be included in a weight ratio of 1:1 to 2:2 to 4.

[0123] platinum-based catalysts

[0124] The above catalyst is included in the present invention for the purpose of promoting a curing reaction (reacting a siloxane having an unsaturated bond such as an alkenyl group with a Si-O type siloxane, thereby generating a cross-linking reaction by adding a Si-H bond to the alkenyl group (vinyl group)).

[0125] In one embodiment, the catalyst may comprise a platinum-based catalyst. In one embodiment, the platinum-based catalyst may comprise one or more of finely powdered platinum, platinum black, chloroplatinic acid, alcohol-modified chloroplatinic acid, chloroplatinic acid-olefin complex, chloroplatinic acid-alkenylsiloxane complex, and chloroplatinic acid-divinyltetramethyldisiloxane complex. For example, the reaction product of chloroplatinic acid and 1,3-diethenyl-1,1,3,3-tetramethyldisiloxane may be used.

[0126] In one embodiment, the catalyst is included in an amount of 0.001 to 5 parts by weight per 100 parts by weight of the polyorganosiloxane. Within this range, the curing reaction rate of the present invention may be easily controlled. If the catalyst is included in an amount less than 0.001 parts by weight, the curing reaction does not occur easily, and if it is included in an amount exceeding 5 parts by weight, it may be difficult to control the curing rate. For example, it may be included in an amount of 0.001 to 2 parts by weight. As another example, it may be included in an amount of 0.01 to 0.1 parts by weight.

[0128] Hardening retardant

[0129] The above-mentioned curing retardant may be further included for the purpose of controlling the manufacturing time of the above-mentioned silicone-based thermoplastic elastomer composition. In one embodiment, the above-mentioned curing retardant may be a compound having a carbon-carbon double bond or a carbon-carbon triple bond at the terminal end.

[0130] For example, the above-mentioned curing retardant may include one or more of alkyne alcohol-based, n-phosphorus-based, cyclosiloxane-based, and triazole-based curing retardants.

[0131] In one embodiment, the alkyne alcohol-based curing retardant may use 3-methyl-1-hexin-3-ol, 3-methyl-1-penten-3-ol, 2-methyl-3-butyn-2-ol, 2-methyl-3-butyn-2-ol, 2-phenyl-3-butyn-2-ol, 3,5-dimethyl-1-hexin-3-ol, and 1-ethynyl-1-cyclohexanol, etc. For example, it may include one or more of 3-methyl-1-hexin-3-ol and 1-ethynyl-1-cyclohexanol.

[0132] In one embodiment, the cyclosiloxane-based curing retardant may be 1,3,5,7-tetravinyltetramethylcyclotetrasiloxane, 1,3-divinyl-1,3-diphenyldimethyldisiloxane, and methyltris(3-methyl-1-butyne-3-oxy)silane.

[0133] In one embodiment, the curing retardant may be included in an amount of 0.01 to 5 parts by weight per 100 parts by weight of the polyorganosiloxane. Within this range, the curing speed control effect may be excellent without impairing the physical properties of the present invention. For example, it may be included in an amount of 0.01 to 0.5 parts by weight. For another example, it may be included in an amount of 0.01 to 0.2 parts by weight.

[0135] Method for manufacturing a silicon-based thermoplastic elastomer composition

[0136] Another aspect of the present invention relates to a method for preparing the above-mentioned silicone-based thermoplastic elastomer composition. In one embodiment, the method for preparing the above-mentioned silicone-based thermoplastic elastomer composition comprises: a step of preparing a first mixture comprising a polyorganosiloxane represented by the following chemical formula 1, silica, a silicone oil having a silanol group at one end, and a surface modifier; and a step of preparing a second mixture comprising the first mixture, an organohydrogenpolysiloxane curing agent, and a platinum-based catalyst.

[0137] The above silicone-based thermoplastic elastomer comprises 100 parts by weight of the polyorganosiloxane, 5 to 100 parts by weight of silica, 1 to 20 parts by weight of a silicone oil having a silanol group at one end, 1 to 20 parts by weight of an organohydrogenpolysiloxane curing agent, 0.5 to 15 parts by weight of a surface modifier, and 0.001 to 5 parts by weight of a platinum-based catalyst, wherein the surface modifier comprises a silane-based compound having one or more functional groups selected from epoxy groups, glycidoxy groups, phenyl groups, hydroxyl groups, isocyanate groups, vinyl groups, and acid anhydride groups:

[0138] [Chemical Formula 1]

[0139]

[0140] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.)

[0141] The constituent components used in the above-mentioned silicone-based thermoplastic elastomer composition may be the same as those described above.

[0142] In one embodiment, the first mixture can be prepared by mixing the polyorganosiloxane, silica, silicone oil, and surface modifier at 120 to 220°C. Under these conditions, mixability and dispersibility may be easily achieved. The first mixture can be prepared by mixing the polyorganosiloxane, silica, silicone oil, and surface modifier at 120 to 220°C for 10 minutes to 12 hours.

[0143] In one embodiment, the silane compound may include one or more of monomers, dimers, and oligomers.

[0144] In one embodiment, the silane-based oligomer compound can be prepared by including the step of hydrolyzing the silane-based monomer compound.

[0145] The above hydrolysis may be carried out in the presence of a catalyst. In one embodiment, the catalyst may include one or more of an acid catalyst and a base catalyst.

[0146] For example, the acid catalyst may include one or more of acetic acid, formic acid, hydrochloric acid, nitric acid, sulfuric acid, hydrofluoric acid, and phosphoric acid. For example, the basic catalyst may include one or more of ammonium hydroxide, ammonium chloride, and methylamine.

[0147] For example, the above hydrolysis can be carried out under pH conditions of 3.5 to 6.0. When hydrolyzing under these conditions, a silane oligomer compound can be easily prepared. For example, the above hydrolysis can be carried out under pH conditions of 3.5 to 6.0 of a mixed composition comprising a silane monomer compound, water, and a catalyst.

[0148] The above hydrolysis may be carried out by including the step of raising the temperature of the above mixed composition to 40 to 60°C by an exothermic reaction; the step of cooling the above mixed composition to room temperature and stirring; and the step of heating the stirred mixed composition to 60 to 75°C. Under the above conditions, a silane oligomer compound can be easily prepared.

[0149] The above second mixture can be prepared by adding and mixing the above first mixture, an organohydrogenpolysiloxane curing agent, and a platinum-based catalyst.

[0150] For example, the second mixture above can be prepared by adding the first mixture, an organohydrogenpolysiloxane curing agent, and a platinum-based catalyst and heating at 140 to 200°C to produce a silicone-based thermoplastic elastomer composition in the form of a cured product.

[0151] In one embodiment, the second mixture further comprises 50 to 1,000 parts by weight of a thermoplastic material based on 100 parts by weight of the polyorganosiloxane, and the thermoplastic material may comprise one or more of a thermoplastic resin and a thermoplastic elastomer.

[0152] In one embodiment, the second mixture further comprises 0.01 to 5 parts by weight of a curing retardant per 100 parts by weight of the polyorganosiloxane, and the curing retardant may include one or more of alkyne alcohol-based, n-phosphorus-based, cyclosiloxane-based, and triazole-based curing retardants.

[0153] In one embodiment, the silicone-based thermoplastic elastomer composition may include a siloxane oil having a silanol group at one end and an organohydrogenpolysiloxane curing agent in a weight ratio of 1:1 to 1:6. When included in the above weight ratio, the mixability and formulation stability are excellent, and the heat resistance, durability, and mechanical properties of the composition may be excellent. For example, it may be included in a weight ratio of 1:1.5 to 1:4. As another example, it may be included in a weight ratio of 1:2 to 1:4.

[0154] In one embodiment, the silicone oil having a silanol group at one end and the surface modifier may be included in a weight ratio of 1:0.5 to 1:3. When included in the above weight ratio, the mixability and formulation stability are excellent, and the heat resistance, durability, and mechanical properties of the composition may be excellent. For example, it may be included in a weight ratio of 1:0.5 to 1:2. As another example, it may be included in a weight ratio of 1:1 to 1:2.

[0155] In another embodiment, the silicone-based thermoplastic elastomer composition may include a siloxane oil having a silanol group at one end, a surface modifier, and an organohydrogenpolysiloxane curing agent in a weight ratio of 1:0.5 to 3:1 to 6. When included in the above weight ratios, the mixability and formulation stability are excellent, and the transparency, heat resistance, durability, and mechanical properties of the composition may be excellent. For example, it may be included in a weight ratio of 1:0.5 to 2:1.5 to 4. As another example, it may be included in a weight ratio of 1:1 to 2:2 to 4.

[0157] A molded body manufactured using a silicone-based thermoplastic elastomer composition

[0158] Another aspect of the present invention relates to a molded article manufactured using the above-described silicon-based thermoplastic elastomer composition.

[0159] In one embodiment, the molded body may be manufactured by including the step of molding the silicone-based thermoplastic elastomer composition. For example, the molding may be carried out by various methods such as extrusion, injection, and compression.

[0161] Hereinafter, the structure and operation of the present invention will be explained in more detail through preferred embodiments. However, these are presented as preferred examples of the present invention and should not be interpreted in any way as limiting the present invention. Details not described herein can be sufficiently technically inferred by those skilled in the art, so such descriptions will be omitted.

[0163] Examples and Comparative Examples

[0164] The components used in the above examples and comparative examples are as follows.

[0165] (A) Polyorganosiloxane: (A1) Polyorganosiloxane with a vinyl group content of 0.032 mol%, a weight-average molecular weight (Mw) of 600,000–700,000 g / mol, and having dimethylvinylsilyl groups at both ends (Grace Continental Korea, T722TM) was used. (A2) Polyorganosiloxane with a vinyl group content of 4 mol%, a weight-average molecular weight (Mw) of 650,000–700,000 g / mol, and having dimethylvinylsilyl groups at both ends (Grace Continental Korea, T4.5TM) ​​was used. (A3) Polyorganosiloxane (Grace Continental Korea, T5™) with a vinyl group content of 0.16 mol%, a weight-average molecular weight (Mw) of 600,000 to 700,000 g / mol, and having dimethylvinylsilyl groups at both ends was used.

[0166] (B) Silica: Average particle size is 5 nm to 30 µm, and specific surface area (BET method) is 100 to 300 m² 2 Silica with a content of / g was used.

[0167] (C) Silicone oil having silanol groups on one end: Silicone oil having silanol groups on one end was used, having a hydroxyl group content of 1 to 10 wt% and a kinematic viscosity of 5,000 to 20,000 cSt measured at 25°C.

[0168] (D) Surface modifier: (D1) A glycidoxy group-containing silane monomer compound (glycidoxypropyl triethoxysilane) was used. (D2) A phenyl group-containing silane monomer compound (trimethoxyphenylsilane) was used.

[0169] (D3) A silane-based oligomer compound was used. Specifically, the silane-based monomer compounds (D1) and (D2) were placed in a reaction vessel, and after adding an acid catalyst, distilled water was slowly added while stirring to prepare a mixed composition. The mixed composition maintained a pH of 3.5 to 6.0, and the temperature rose to 50°C due to the exothermic hydrolysis reaction. After cooling to room temperature, it was stirred for 4 hours. Then, the mixed composition was heated to 70°C and the reaction was carried out to prepare the silane-based oligomer compound (D3). The silane-based oligomer compound (D3) contained glycidoxy groups and phenyl groups, and had a number average molecular weight (Mn) of 2186.1 g / mol and a weight average molecular weight (Mw) of 3574.5 g / mol.

[0170] (E) Thermoplastic materials: (E1) Thermoplastic polyurethane (Dongsung Corporation, Neothane 90A) was used. (E2) Propylene-alpha-olefin copolymer (Mitsui Chemical, Tafmer XM-5070) was used. (E3) Styrene-ethylene-butadiene-styrene (SEBS) copolymer (Kraton, KG1645) was used. (E4) Polypropylene homopolymer (Lyondellbasell, HP522) was used.

[0171] (F) A platinum-based catalyst was used.

[0172] (G) Organohydrogen polysiloxane (1-octadecyl-1,3,5,7,9-pentamethylcyclopentasiloxane) was used as a curing agent.

[0173] (H) Curing retardant: 1-ethynyl-1-cyclohexanol was used.

[0175] Examples 1-6

[0176] Polyorganosiloxane, silica, siloxane oil, and a surface modifier were introduced into a reactor and mixed at 200°C for 8 hours to prepare a first mixture. The first mixture, a thermoplastic material, a platinum-based catalyst, a curing agent, and a curing retardant were introduced and mixed and cured at 140°C to prepare a second mixture (silicone-based thermoplastic elastomer composition).

[0178] Example 7

[0179] A second mixture (silicon-based thermoplastic elastomer composition) was prepared in the same manner as in Example 1, except that the above thermoplastic material was not applied. The components and content included in the silicon-based thermoplastic elastomer compositions of Examples 1 to 7 are shown in Table 1 below.

[0181] Comparative Examples 1~10

[0182] A silicone-based thermoplastic elastomer composition was prepared in the same manner as in Example 1, except that no surface modifier was added. The components and contents included in Comparative Examples 1 to 5 are shown in Table 2 below.

[0183]

[0184]

[0186] Experimental Example

[0187] (1) Compatibility: For the above examples and comparative examples, compatibility and mixability were visually observed and evaluated according to the following criteria, and the results are shown in Tables 3 and 4 below (◎: Very good, ○: Very partially undispersed, △: Partially undispersed, X: Not dispersed).

[0188] (2) Specific gravity (g / cm²) 3 For the above examples and comparative examples, the specific gravity was measured using ALFA MIRAGE’s MD-300S (product name), and the results are shown in Tables 3 and 4 below.

[0189] (3) Hardness (shore A / shore D): The hardness of the above examples and comparative examples was measured according to ASTM D 2240, and the results are shown in Tables 3 and 4 below.

[0190] (4) Tensile strength (MPa), elongation (%) and 100% modulus (MPa): Tensile strength and elongation were measured for the above examples and comparative examples according to ASTM D 624. In addition, the modulus (100% modulus, MPa) was measured for representative examples 1 to 4 and comparative examples 1 to 3 according to ASTM D 412, and the results are shown in Tables 3 and 4 below.

[0191] (5) Heat resistance: For the above examples and comparative examples, specifically Examples 5 to 7 and Comparative Examples 5 to 10, the samples were heated in a chamber at 230°C for 72 hours according to KS M 6518, then removed and left to room temperature, after which the change in hardness and the rate of change in tensile strength of the examples and comparative examples were measured.

[0192] Next, the rate of change was calculated based on the hardness change values ​​(hardness value after heat resistance test - hardness value before heat resistance test) and the initial tensile strength measurements of the above examples and comparative examples, and the results are shown in Tables 3 and 4 below:

[0193] [ceremony]

[0194] Change in tensile strength (%) = ((A2-A1) / A1)*100

[0195] (In the above formula, A1 is the tensile strength of the example and comparative example before the heat resistance test, and A2 is the tensile strength of the example and comparative example after the heat resistance test).

[0196]

[0198]

[0199] Referring to the results of Tables 3 and 4 above, it was found that in the case of Examples 1 to 4, which used thermoplastic materials, the compatibility of the composition was superior compared to Comparative Examples 1 to 4, which used the same type of thermoplastic materials, and the tensile strength and elongation were excellent.

[0200] In addition, Examples 5 to 7 of the present invention showed superior compatibility, tensile strength, and elongation compared to Comparative Examples 5 to 10, and the change in hardness and the rate of change in tensile strength before and after the heat resistance test were measured to be low, indicating excellent heat resistance even in a high-temperature environment of 230°C.

[0202] The present invention has been described above with reference to embodiments. Those skilled in the art will understand that the present invention may be embodied in modified forms without departing from the essential characteristics of the invention. Therefore, the disclosed embodiments should be considered in an illustrative rather than a restrictive sense. The scope of the invention is defined by the claims, not by the foregoing description, and all variations within the scope of equivalents should be interpreted as being included in the invention.

Claims

Claim 1 A silicone-based thermoplastic elastomer composition comprising: 100 parts by weight of a polyorganosiloxane represented by the following chemical formula 1; 5 to 100 parts by weight of silica; 0.5 to 15 parts by weight of a silicone oil having a silanol group on one end; 1 to 20 parts by weight of an organohydrogenpolysiloxane curing agent; 0.5 to 15 parts by weight of a surface modifier; and 0.001 to 5 parts by weight of a platinum-based catalyst; wherein the silicone oil having a silanol group on one end and the surface modifier are included in a weight ratio of 1:1 to 1:3, and the surface modifier comprises a silane-based oligomer having a weight-average molecular weight of 1,500 to 4,000 g / mol, and including a glycidoxy group and a phenyl group as functional groups: [Chemical Formula 1] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.) Claim 2 In claim 1, the silicone-based thermoplastic elastomer composition further comprises 50 to 1,000 parts by weight of a thermoplastic material per 100 parts by weight of the polyorganosiloxane, wherein the thermoplastic material comprises one or more of a thermoplastic resin and a thermoplastic elastomer. Claim 3 The silicone-based thermoplastic elastomer composition according to claim 1, wherein the polyorganosiloxane has an alkenyl group content of 0.01 mol% to 5 mol% and a weight-average molecular weight of 300,000 to 800,000 g / mol. Claim 4 delete Claim 5 The silicone-based thermoplastic elastomer composition according to claim 1 further comprises 0.01 to 5 parts by weight of a curing retardant per 100 parts by weight of the polyorganosiloxane, wherein the curing retardant comprises one or more of alkyne alcohol-based, n-phosphorus-based, cyclosiloxane-based, and triazole-based curing retardants. Claim 6 delete Claim 7 The silicone-based thermoplastic elastomer composition according to claim 1, wherein the silicone oil having a silanol group at one end has a hydroxyl group content of 1 to 10 weight% and a kinematic viscosity of 5,000 to 20,000 cSt. Claim 8 A step of preparing a first mixture comprising a polyorganosiloxane represented by the following chemical formula 1, silica, a silicone oil having a silanol group at one end, and a surface modifier; A method for manufacturing a silicone-based thermoplastic elastomer comprising the step of preparing a second mixture comprising the first mixture, an organohydrogenpolysiloxane curing agent, and a platinum-based catalyst; wherein the silicone-based thermoplastic elastomer comprises 100 parts by weight of the polyorganosiloxane, 5 to 100 parts by weight of silica, 0.5 to 15 parts by weight of a silicone oil having silanol groups on one end, 1 to 20 parts by weight of the organohydrogenpolysiloxane curing agent, 0.5 to 15 parts by weight of a surface modifier, and 0.001 to 5 parts by weight of a platinum-based catalyst, wherein the silicone oil having silanol groups on one end and the surface modifier are included in a weight ratio of 1:1 to 1:3, and the surface modifier comprises a silicone-based thermoplastic elastomer comprising a silane-based oligomer having a weight-average molecular weight of 1,500 to 4,000 g / mol and including glycidoxy groups and phenyl groups as functional groups. Manufacturing method: [Chemical Formula 1] (In the above formula 1, R1, R2, R3, R4, R5, R6, R7, and R8 are each independently selected from linear or branched C1 to C10 alkyl groups, C1 to C10 aminoalkyl groups, C1 to C10 hydroxyalkyl groups, C1 to C20 haloalkyl groups, C3 to C15 cycloalkyl groups, C6 to C12 aryl groups, C7 to C20 aralkyl groups, and C2 to C20 alkenyl groups, wherein a is an integer from 1 to 100, and at least one of R1 to R8 is a vinyl group.) Claim 9 A method for preparing a silicone-based thermoplastic elastomer composition, wherein, in claim 8, the second mixture further comprises 50 to 1,000 parts by weight of a thermoplastic material based on 100 parts by weight of the polyorganosiloxane, and the thermoplastic material comprises one or more of a thermoplastic resin and a thermoplastic elastomer. Claim 10 delete Claim 11 A molded body manufactured using a silicone-based thermoplastic elastomer composition according to any one of claims 1 to 3, 5, and 7.

Citation Information

Patent Citations

  • Oil-Resistant Thermoplastic Elastomer Composition andMoldings Using the Same

    KR100606308B1

  • Silicone rubber composition

    KR1020010092360A

  • Curable polyorganosiloxane composition

    KR1020150099581A

  • A water repellent coating composition having excellent slip with water repellent property and manufacturing method thereof

    KR1020210089298A

  • A composition for wiper blade for vehicle and manufacturing method for wiper blade for vehicle using the same