Apparatus and method for manufacturing positive electrode active material precursor

The apparatus and method address the issue of non-uniform growth in cathode active material precursors by using a two-stage impeller system to enhance sphericity and uniformity, reducing fine particles and impurities.

KR103046668B1Active Publication Date: 2026-11-10POSCO FUTURE M CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230023207
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2026-11-10
Estimated Expiration
2043-02-21

Smart Images

  • Figure 112023020469134-PAT00001_ABST
    Figure 112023020469134-PAT00001_ABST
Patent Text Reader

Abstract

A method for manufacturing a positive electrode active material precursor according to the present invention comprises: a reaction vessel; one or more input pipes for introducing a reaction solution into the reaction vessel; and a stirring means located at the inner center of the reaction vessel and stirring the reaction solution introduced from the input pipes; wherein the stirring means comprises a shaft and a two-stage impeller, and the impeller has an angle of 5 to 90° with respect to the horizontal direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an apparatus and method for manufacturing a positive electrode active material precursor. Background Technology

[0002] With the increasing demand for mobile devices such as smartphones and laptops, and the growth of the hybrid and electric vehicle markets, the demand for secondary batteries as an energy source is rapidly increasing. In particular, lithium-ion batteries, which exhibit high energy density and operating potential, long cycle life, and low self-discharge rates, are being widely used.

[0003] To manufacture the cathode active material for lithium secondary batteries, a lithium source, a cathode active material precursor, and a dopant are required. Among these, as a method for manufacturing the cathode active material precursor, the co-precipitation method is widely utilized. Instead of the conventional solid-state reaction method, this method involves precipitating chlorides, nitrides, or sulfides containing the raw material as hydroxides in a basic solution and growing them to a specific particle size.

[0004] When manufacturing cathode active material precursors using the co-precipitation method, production is primarily carried out in large-capacity reactors; however, as the reaction unit size increases, growth uniformity is compromised and fine particles are formed, making it very difficult to produce precursors with high sphericity and a uniform shape.

[0005] Therefore, there is a need to develop an apparatus and method for manufacturing a positive electrode active material precursor that can obtain a precursor with excellent sphericity and a uniform shape. The problem to be solved

[0006] The present invention aims to provide an apparatus and method for manufacturing a positive electrode active material precursor capable of suppressing fine particle formation and improving the growth uniformity and sphericity of the positive electrode active material precursor. means of solving the problem

[0007] The present invention provides an apparatus for manufacturing a positive electrode active material precursor, comprising: a reaction vessel; one or more input pipes for introducing a reaction solution into the reaction vessel; and a stirring means located at the inner center of the reaction vessel and stirring the reaction solution introduced from the input pipes; wherein the stirring means comprises a shaft and a two-stage impeller, and the impeller has an angle of 5 to 90° with respect to the horizontal direction.

[0008] In addition, the present invention provides a method for manufacturing a positive electrode active material precursor, comprising the steps of: introducing an initial solution into a reaction vessel; introducing a reaction solution into the reaction vessel into which the initial solution has been introduced; and stirring the initial solution and the reaction solution with a stirring means to obtain a positive electrode active material precursor, wherein the stirring means comprises a shaft and a two-stage impeller, the impeller having an angle of 5 to 90° with respect to the horizontal direction, and the initial solution is introduced so that the two-stage impeller is completely submerged. Effects of the invention

[0009] The apparatus and method for manufacturing a positive electrode active material precursor according to the present invention have the advantage of suppressing fine particle formation and improving the growth uniformity and sphericity of the positive electrode active material precursor. In addition, by improving internal concentration variation, there is the advantage of being able to control impurities and improve compositional accuracy. Brief explanation of the drawing

[0010] FIGS. 1 and 2 are drawings illustrating an apparatus for manufacturing a positive electrode active material precursor according to some embodiments of the present invention. FIG. 3 is a side view of a stirring means according to some embodiments of the present invention. FIG. 4 is a plan view of an apparatus for manufacturing a positive electrode active material precursor according to some embodiments of the present invention. Figures 5a and 5b show SEM images of cathode active material precursors prepared according to the examples and comparative examples. Figures 6a and 6b are diagrams showing the supernatant for measuring unreacted Ni of the cathode active material precursor prepared according to the examples and comparative examples. Specific details for implementing the invention

[0011] Hereinafter, embodiments of the present invention will be described in detail. However, these are presented as examples and are not intended to limit the present invention, and the present invention is defined only by the scope of the claims set forth below.

[0012] In the present invention, when it is stated that a certain member is located "on" another member, this includes not only cases where a certain member is in direct contact with another member, but also cases where another member is interposed between the two members.

[0013] In the present invention, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0015] <Manufacturing device for positive active material precursor>

[0016] One aspect of the present invention relates to an anode active material precursor manufacturing apparatus (100) comprising: a reaction vessel (10); one or more input pipes (20, 30, 40) for introducing a reaction solution into the reaction vessel (10); and a stirring means (60) located at the inner center of the reaction vessel (10) and stirring the reaction solution introduced from the input pipes (20, 30, 40); wherein the stirring means (60) comprises a shaft (61) and two impellers (62, 63), and the impellers (62, 63) have an angle of 5 to 90° with respect to the horizontal direction.

[0017] The cathode active material precursor manufacturing apparatus (100) according to the present invention can control the formation of fine particles by suppressing the scattering of the reaction solution using two-stage impellers (62, 63). Therefore, there is an advantage in that the growth uniformity and sphericity of the cathode active material precursor can be improved.

[0018] The cathode active material precursor manufacturing apparatus (100) according to the present invention may be a co-precipitation reactor for manufacturing a catalyst or a cathode active material precursor for a lithium secondary battery, including a continuous stirred reactor (CSTR) based on a batch type reactor.

[0020] FIG. 1 briefly illustrates an apparatus (100) for manufacturing a positive electrode active material precursor according to some embodiments of the present invention.

[0021] The apparatus (100) for manufacturing a positive electrode active material precursor according to the present invention includes a reaction vessel (10). The reaction vessel (10) may be formed in the shape of a tube with an open top into which a reaction solution is introduced. Alternatively, although not illustrated, the reaction vessel (10) may be in the form of a structure in which a central cylindrical body, a bottom, and an upper cover portion are assembled via a flange structure, but is not limited thereto.

[0022] The reaction vessel (10) contains the reaction solution inside and reacts it. The reaction vessel (10) may include a drain portion for discharging the generated positive active material precursor to the outside, but is not limited thereto.

[0024] The anode active material precursor manufacturing apparatus (100) according to the present invention includes one or more input pipes (20, 30, 40) for introducing a reaction solution into the reaction vessel (10).

[0025] In one embodiment of the present invention, the input pipes (20, 30, 40) may include a first input pipe (20) for introducing a first solution containing NH4OH, a second input pipe (30) for introducing a second solution containing NaOH, and a third input pipe (40) for introducing a metal solution.

[0026] The above-mentioned input pipes (20, 30, 40) are not illustrated but can be connected to each storage tank in which the reaction solution is stored.

[0027] The above-mentioned input pipes (20, 30, 40) may be equipped with a flow meter, but are not limited thereto.

[0028] The material of the above-mentioned input pipes (20, 30, 40) is not limited as long as it has corrosion resistance and chemical resistance to the above-mentioned first solution, second solution, and metal solution. The material of the above-mentioned input pipes (20, 30, 40) may be provided with at least one material among, for example, stainless steel, PP, PVC, PE, and PVDF.

[0029] The diameter and thickness of the above-mentioned input pipes (20, 30, 40) can be designed to be appropriately changed according to the capacity of the reaction vessel (10).

[0030] For example, in the case of the reaction vessel (10) having a volume of 10 to 30 tons, the input pipe (20, 30, 40) may have a diameter of 5 to 80 mm, preferably 10 to 65 mm, more preferably 15 to 50 mm, but is not limited thereto. It is preferable that the diameter of the input pipe (20, 30, 40) be within the above range because it facilitates the input of the first solution, the second solution, and the metal solution.

[0031] For example, in the case of the reaction vessel (10) having a volume of 10 to 30 tons, the thickness of the input pipe (20, 30, 40) may be 1 to 15 mm, preferably 1.5 to 10 mm, more preferably 2 to 5 mm, but is not limited thereto. It is desirable for the thickness of the input pipe (20, 30, 40) to satisfy the above range because the durability of the input pipe (20, 30, 40) is excellent.

[0032] In another embodiment of the present invention, the first input pipe (20) and the third input pipe (40) may be arranged adjacently.

[0033] Specifically, when the first input pipe (20) and the third input pipe (40) are arranged adjacently, it is advantageous for the formation of a complex compound between the metal solution introduced through the third input pipe (40) and the NH4OH of the first solution introduced through the first input pipe (20), thereby allowing the reaction rate to be controlled and aiding in uniform growth. More specifically, when the metal solution reacts with the NH4OH of the first solution, a complex compound is formed, which then reacts with the NaOH of the second solution to proceed with a co-precipitation reaction. Therefore, by arranging the first input pipe (20) and the third input pipe (40) adjacently, the reaction rate can be controlled to ensure a fast reaction. Additionally, the formation of aggregates that cause clogging at the ends of the input pipes (20, 40) can be suppressed.

[0034] In another embodiment of the present invention, the input pipes (20, 30, 40) may be branched into 3 to 4 branches from a branching point. Specifically, referring to FIG. 2, the input pipes (20, 30, 40) may be branched into 3 branches from a branching point.

[0035] It is desirable that the above-mentioned input pipes (20, 30, 40) branch into 3 to 4 branches from the branching point, as this can improve the internal diffusion of the reaction solution.

[0036] Specifically, if the input pipes (20, 30, 40) are branched, the internal diffusivity of the reaction solution can be improved, thereby inducing uniform particle growth, controlling impurities, and improving the accuracy of the composition. Additionally, it is desirable to be able to improve the concentration variation within the reaction solution.

[0037] FIG. 4 is a plan view illustrating an apparatus (100) for manufacturing an anode active material precursor according to some embodiments of the present invention. Referring to FIG. 4, the first input pipe (20) and the third input pipe (40) may be branched into 3 to 4 branches from a branching point, and in this case, the branch pipe of the first input pipe (20) may be arranged adjacent to the branch pipe of the third input pipe (40). When the input pipes (20, 40) are branched, it is preferable that the distance between adjacent branch pipes be the same. For example, when the first input pipe (20) is branched into three branch pipes, the three branch pipes may be branched to have the same distance.

[0038] At this time, referring to FIG. 4, in the case of the first input pipe (20) and the third input pipe (40), the angle θ2 formed by the line extending from the first branch pipe to the shaft (61), which is the central axis of the impeller (62, 63) to be described later, and the line extending from the last branch pipe to the shaft (61) may be within 135°, preferably between 90° and 135°. In addition, in the case of the second input pipe (30), the angle θ3 formed by the line extending from the first branch pipe to the shaft (61) and the line extending from the last branch pipe to the shaft (61) may be within 120°, preferably between 60° and 120°. Preferably, each of the branch pipes may be arranged at equal intervals within the angle range.

[0039] The above θ2 and When θ3 satisfies the above range, the solutions in the input pipes (20, 30, 40) can be uniformly diffused within the reaction solution, which can improve internal concentration variation and suppress non-uniform growth of particles and impurities, which is desirable.

[0040] Specifically, when the first injection pipe (20) into which the first solution containing NH4OH is introduced and the third injection pipe (40) into which the metal solution is introduced are arranged adjacently, it is desirable to suppress the phenomenon of aggregation forming at the end of the third injection pipe (40).

[0041] The second injection pipe (30) into which the second solution containing the above NaOH is introduced may be provided on the opposite side of the first injection pipe (20) and the third injection pipe (40).

[0042] Generally, when a metal solution is introduced into a reaction solution within a pH range, specifically between pH 10 and 13, precipitation occurs immediately. However, as the amount of solution introduced increases over time, precipitation proceeds without uniform diffusion of ions such as metal ions, sodium, and sulfate ions. For this reason, concentration variations occur within the reaction solution, leading to a problem where the concentration of impurities, such as unreacted metals, Na, and S ions, increases within the synthesized cathode active material precursor. In particular, if unreacted metals are present, overall process loss increases, which has the disadvantage of resulting in higher processing costs.

[0043] When the second input pipe (30) is positioned on the opposite side of the first input pipe (20) and the third input pipe (40), specifically when the centers of θ2 and θ3 are positioned to satisfy 180° with respect to the shaft (61), it is desirable because the metal ions form a complex compound, making it easy to control the reaction rate, which has the advantage of suppressing the aforementioned problem.

[0044] The diameters of the branch pipes may all be the same or different. It is preferable that the diameters of each input pipe (20, 30, 40) after branching are the same. It is desirable that the diameters after branching are all the same, as this helps with flow control in the pipes after branching, that is, in other words, in the branch pipes. Specifically, if the first input pipe (20) includes a branch pipe that branches into three branches, it is preferable that the diameters of the branch pipes are all the same. Additionally, referring to FIG. 2, it is preferable that the diameter of the input pipe (20, 30, 40) before branching is greater than or equal to the diameter of the branch pipe after branching.

[0045] The above branch point may be provided at 1 / 20 to 1 / 5, preferably 1 / 10 to 1 / 7 from the top of the input pipe (20, 30, 40), but is not limited thereto.

[0047] In another embodiment of the present invention, the input pipes (20, 30, 40) may further include a deionized water (DI water) input pipe and a nitrogen input pipe (50).

[0048] The above-mentioned deionized water inlet pipe may be provided to introduce deionized water included in the initial solution to be described later. Since the deionized water introduced through the above-mentioned deionized water inlet pipe does not need to be introduced during the manufacturing process of the anode active material precursor, the location of the above-mentioned deionized water inlet pipe is not specifically limited.

[0049] The nitrogen injection pipe (50) may be provided for nitrogen purging to remove dissolved oxygen in the initial solution and to create a non-oxidizing atmosphere inside the reaction vessel (10). Referring to FIG. 4, the nitrogen injection pipe (50) may be provided relatively close to the first injection pipe (20), but is not limited thereto.

[0050] The ends of the above-mentioned input pipes (20, 30, 40) may be positioned at a point 1 / 20 to 2 / 5 of the way from the bottom of the reaction vessel (10), preferably at a point 1 / 10 to 1 / 7 of the way. When the ends of the above-mentioned input pipes (20, 30, 40) are positioned within the above range, the spacing and arrangement with the stirring means (60) described later are appropriate, making stirring easy and allowing for uniform diffusion according to the flow of the vortex, which is desirable.

[0051] It is preferable that the ends of the above-mentioned input pipes (20, 30, 40) be located at the same point from the bottom of the reaction vessel (10) (see FIG. 2).

[0053] The anode active material precursor manufacturing apparatus (100) according to the present invention comprises a stirring means (60) located at the inner center of the reaction vessel (10) and stirring the reaction solution introduced from the introduction pipes (20, 30, 40); the stirring means (60) comprises a shaft (61) and two impellers (62, 63), and the impellers (62, 63) have an angle of 5 to 90° with respect to the horizontal direction.

[0054] Conventional mass-production reactors increase the input amount of the reaction solution for large-scale synthesis and set the spacing of multi-stage impellers of three or more stages relative to simple volume to stir the solution. In this case, as the reaction unit increases, uniformity is compromised and fine particles are formed, making it very difficult to produce a uniform precursor.

[0055] Furthermore, as the liquid level of the reaction solution rises during the reaction, the solution is scattered whenever it comes into contact with the impeller. While the scattered reaction solution remains on the wall, it is deprived of a supply of reaction raw materials such as metal ions, NaOH, and NH4OH, which inhibits the particle growth of the cathode active material precursor and causes non-uniform growth. Consequently, fine particles are formed, leading to some issues regarding reduced particle uniformity and sphericity.

[0056] However, the present invention has the advantage of being able to control the formation of fine particles by suppressing scattering of the reaction solution through the use of a two-stage impeller (62, 63), and to improve growth uniformity and sphericity.

[0058] The impeller (62, 63) according to the present invention has an angle of 5 to 90° with respect to the horizontal direction.

[0059] FIG. 3 shows a side view of a stirring means (60) according to some embodiments of the present invention.

[0060] Specifically, referring to FIG. 3, the impeller (62, 63) may be provided to be inclined such that θ1, defined with respect to the horizontal direction, is 5 to 90°, preferably 15 to 70°, and more preferably 30 to 45°. In short, the impeller (62, 63) may be in a shape in which the angle of the blade is inclined from the upper left to the lower right at 5 to 90°.

[0061] By having the above impellers (62, 63) configured to have an angle of the above range, a vortex can be formed from the bottom to the top of the reaction vessel (10). At this time, the rotation direction of the impellers (62, 63) may be clockwise.

[0062] Since the impeller (62, 63) forms the vortex, the diffusion of ions within the reaction solution is facilitated, and concentration variations can be eliminated. As a result, there is an advantage that the growth of the positive active material precursor can be carried out uniformly.

[0064] In another embodiment of the present invention, the two-stage impellers (62, 63) may be configured such that the vertical center of the lower impeller (63) located at the bottom is located at a point 1 / 15 to 1 / 5 of the way from the bottom of the reaction vessel (10), preferably at a point 1 / 8 to 1 / 6 of the way.

[0065] In another embodiment of the present invention, the two-stage impeller (62, 63) may be configured such that the vertical center of the upper impeller (62) located at the top is located at a point 1 / 4 to 1 / 2, preferably 1 / 4 to 1 / 3, with respect to the vertical direction from the bottom of the reaction vessel (10).

[0066] Specifically, the positions of the upper impeller (62) and the lower impeller (63) may be based on the vertical center of each of the impellers (62, 63).

[0067] More specifically, with reference to FIG. 3, in the side view of the stirring means (60), the vertical center points of the upper impeller (62) and the lower impeller (63) may be positioned at 1 / 4 to 1 / 2 and 1 / 15 to 1 / 5 points, respectively, relative to the vertical direction from the bottom of the reaction vessel (10).

[0068] When the upper impeller (62) and the lower impeller (63) are positioned to satisfy the above range, the flow of the vortex formed by stirring is optimized, and the uniformity and sphericity of the manufactured positive active material precursor are excellent, which is desirable.

[0070] The diameter of the impeller (62, 63) can be designed to be appropriately changed according to the capacity of the reaction vessel (10). For example, in the case of the reaction vessel (10) having a volume of 3 to 30 tons, the diameter of the impeller (62, 63) may be 400 to 1550 mm, preferably 700 to 1200 mm, and more preferably 800 to 1050 mm. It is desirable for the diameter of the impeller (62, 63) to satisfy the above range, as it is possible to manufacture a positive active material precursor with uniform particle size and excellent sphericity while minimizing the number of impellers (62, 63).

[0071] The upper impeller (62) and the lower impeller (63) may have different or identical diameters. In terms of optimizing the flow of the vortex, it is preferable that the upper impeller (62) and the lower impeller (63) have the same diameter.

[0073] In another embodiment of the present invention, the two-stage impellers (62, 63) may have the same angle with respect to the horizontal direction. For instance, referring to FIG. 3, the upper impeller (62) and the lower impeller (63) may be tilted to have the same angle with respect to the horizontal direction. When the upper impeller (62) and the lower impeller (63) have the same angle with respect to the horizontal direction, the formation of vortices within the reaction solution is optimized, allowing ions within the reaction solution to diffuse uniformly, thereby making it desirable to obtain a positive active material precursor with excellent uniformity and sphericity.

[0075] The apparatus (100) for manufacturing a positive electrode active material precursor according to the present invention may further include known pumps, heaters, coolers, drain lines, etc., provided that such pumps, heaters, coolers, drain lines, etc., are not illustrated but do not impede the purpose of the present invention. For example, the reaction vessel (10) may be provided with a drain line at the bottom for recovering the manufactured positive electrode active material precursor, and the outer edge of the reaction vessel (10) may further be provided with a heater and a cooler for controlling the temperature of the solution inside the reaction vessel (10), and the upper or lower side of the reaction vessel (10) may further be provided with a sensing tank, etc., for discharging and circulating the solution from the reaction vessel (10) using a circulation pump, but is not limited thereto. In addition, the drain line may be connected to a filtration device, but is not limited thereto.

[0077] The apparatus (100) for manufacturing a positive electrode active material precursor according to the present invention has the advantage of being able to manufacture a positive electrode active material precursor with excellent uniformity and sphericity and minimized impurities without using additional additives. In particular, it has the advantage of being able to easily obtain a desired positive electrode active material precursor regardless of composition.

[0079] <Method for manufacturing a positive electrode active material precursor>

[0080] Another aspect of the present invention relates to a method for manufacturing an anode active material precursor, comprising the steps of: introducing an initial solution into a reaction vessel (10); introducing a reaction solution into the reaction vessel (10) into which the initial solution has been introduced; and stirring the initial solution and the reaction solution with a stirring means (60) to obtain an anode active material precursor, wherein the stirring means (60) includes a shaft (61) and two-stage impellers (62, 63), the impellers (62, 63) have an angle of 5 to 90° with respect to the horizontal direction, and the initial solution is introduced so that the two-stage impellers (62, 63) are completely submerged.

[0081] In short, another aspect of the present invention relates to a method for manufacturing a positive electrode active material precursor using the aforementioned positive electrode active material precursor manufacturing apparatus (100).

[0083] A method for manufacturing a positive electrode active material precursor according to the present invention includes the step of introducing an initial solution into a reaction vessel (10).

[0084] The above reaction vessel (10), the above stirring means (60), and the input pipes (20, 30, 40) to be described later may be applied according to the above description.

[0085] In another embodiment of the present invention, the initial solution may include deionized water.

[0086] The above initial solution is introduced so that the two-stage impellers (62, 63), namely the upper impeller (62) and the lower impeller (63), are both submerged. That is, the method for manufacturing a positive active material precursor according to the present invention starts the reaction with the two-stage impellers (62, 63) both submerged, thereby suppressing non-uniform diffusion within the reaction solution and suppressing scattering of the reaction solution.

[0087] In the case of conventional multi-stage impellers with three or more stages, there was a problem in that it was practically difficult to submerge all of the multi-stage impellers. Consequently, as the water level of the reaction solution rose during the reaction, a phenomenon occurred in which the reaction solution splashed out whenever it came into contact with the multi-stage impellers, which inhibited the growth of the cathode active material precursor particles.

[0088] However, the method for manufacturing a positive electrode active material precursor according to the present invention has the advantage of being able to control the formation of fine particles and improve the growth uniformity and sphericity of the positive electrode active material precursor by suppressing the scattering of the reaction solution and suppressing the phenomenon of the reaction solution remaining on the wall of the reaction vessel (10), etc., since the reaction is initiated with both of the two impellers (62, 63) submerged.

[0089] The above initial solution may further include one or more selected from the group consisting of NH4OH and NaOH. In short, the above initial solution may include a first solution containing NH4OH and a portion of a second solution containing NaOH.

[0090] The above NH4OH may be included in an amount of 0 to 10 weight%, preferably 0 to 5 weight%, and more preferably 0.1 to 3 weight% with respect to the total weight% of the initial solution.

[0091] The above NaOH may be included in an amount of 0 to 10 weight%, preferably 0 to 5 weight%, and more preferably 0.1 to 3 weight% with respect to the total weight% of the initial solution.

[0092] The above deionized water may be included as the remainder to satisfy 100% by weight of the entire initial solution.

[0093] It is desirable that the above NH4OH and the above NaOH are each included within the above ranges, as this can further enhance the reaction effect. Specifically, it is desirable that the above NH4OH and the above NaOH are each included within the above ranges, as this results in an appropriate and uniform initial particle size of the cathode active material precursor being manufactured.

[0094] The amount of the initial solution is not limited as long as it is sufficient to submerge both of the two impellers (62, 63).

[0095] The method for manufacturing a positive electrode active material precursor according to the present invention may further include the step of stirring the initial solution.

[0097] The method for manufacturing a positive electrode active material precursor according to the present invention may further include, but is not limited to, the step of purging the initial solution with nitrogen (N2 purge).

[0098] The step of stirring the initial solution and the step of purging the initial solution with nitrogen can be performed simultaneously.

[0099] Specifically, the method for manufacturing a positive electrode active material precursor according to the present invention may further include the step of purging with nitrogen while stirring the initial solution.

[0100] Since purging the initial solution with nitrogen while stirring can remove dissolved oxygen within the initial solution and improve the uniformity of the cathode active material precursor being manufactured, it is preferable to further include the step of purging the initial solution with nitrogen while stirring.

[0101] The above-mentioned supply amount of nitrogen, supply time, etc., are not limited in the present invention.

[0103] A method for manufacturing a positive electrode active material precursor according to the present invention comprises: a step of introducing a reaction solution into a reaction vessel (10) into which the initial solution is introduced; and a step of stirring the initial solution and the reaction solution with a stirring means (60) to obtain a positive electrode active material precursor.

[0104] In another embodiment of the present invention, the reaction solution may include a first solution containing NH4OH, a second solution containing NaOH, and a metal solution.

[0105] The first solution, the second solution, and the metal solution may be included in appropriate proportions according to the composition of the positive active material precursor to be manufactured, and specifically, by controlling the flow rates of the first solution, the second solution, and the metal solution, a positive active material precursor of the desired form can be obtained.

[0106] The above metal solution may contain salts of one or more metals selected from the group consisting of nickel, cobalt, and manganese.

[0107] For example, the nickel (Ni) may be included in the metal solution as Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, nickel salts of fatty acids, or nickel halides, and at least one of these may be used.

[0108] The above cobalt may be included in the metal solution as Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or CoSO4·7H2O, and at least one of these may be used.

[0109] In addition, the manganese (Mn) may be included in the metal solution as manganese oxides such as Mn2O3, MnO2, and Mn3O4; manganese salts such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid salts; oxyhydroxide, and manganese chloride, etc., and at least one or more of these may be used.

[0110] In addition, the metal solution may further include a salt of at least one metal selected from the group consisting of Al, Zr, B, W, Mo, Cr, Ta, Nb, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y. For example, the metal solution may further include at least one acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide selected from the group consisting of Al, Zr, B, W, Mo, Cr, Ta, Nb, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and Y.

[0111] The flow rate of the above reaction solution can be appropriately varied according to the input pipe (20, 30, 40) into which the above reaction solution is introduced.

[0112] In another embodiment of the present invention, the metal solution may be introduced at a flow rate of 80 to 3200 kg / h, preferably 104 to 2250 kg / h, more preferably 120 to 1950 kg / h.

[0113] In the case where the third injection pipe (40) into which the metal solution is introduced is branched into three branches, the metal solution can be introduced into each branch pipe at a flow rate of 30 to 1000 kg / h, preferably 38 to 750 kg / h, more preferably 40 to 650 kg / h, and in the case where the third injection pipe (40) is branched into four branches, the metal solution can be introduced into each branch pipe at a flow rate of 20 to 800 kg / h, preferably 25 to 680 kg / h, more preferably 30 to 550 kg / h.

[0114] In the case of the second solution mentioned above, the flow rate can be appropriately adjusted and injected according to the morphology.

[0115] In another embodiment of the present invention, the second solution may be introduced at a flow rate of 40 to 1800 kg / h, preferably 60 to 1650 kg / h, more preferably 70 to 1330 kg / h.

[0116] In the case where the second injection pipe (30) into which the second solution is injected is branched into three branches, the second solution can be injected into each branch pipe at a flow rate of 15 to 550 kg / h, preferably 20 to 480 kg / h, and more preferably 22 to 430 kg / h.

[0117] In the case where the second input pipe (30) is branched into four branches, the second solution can be injected into each branch pipe at a flow rate of 10 to 450 kg / h, preferably 15 to 370 kg / h, and more preferably 17 to 330 kg / h.

[0118] In the case of the first solution above, the flow rate can be appropriately adjusted and introduced according to the morphology. For example, the first solution above can be introduced at a flow rate of 10 to 1320 kg / h, preferably 20 to 1200 kg / h, and more preferably 24 to 690 kg / h.

[0119] In the case where the first injection pipe (20) into which the first solution is injected is branched into three branches, the first solution can be injected into each branch pipe at a flow rate of 5 to 400 kg / h, preferably 8 to 230 kg / h.

[0120] In the case where the first input pipe (20) is branched into four branches, the first solution may be injected into each branch pipe at a flow rate of 3 to 330 kg / h, preferably 5 to 180 kg / h, but is not limited thereto.

[0122] In another embodiment of the present invention, the molar ratio of the metal ions in the metal solution to the NH4OH may be 1:0.2 to 1:0.9, preferably 1:0.2 to 1:0.7. It is desirable that the molar ratio of the metal in the metal solution to the NH4OH satisfies the above range, as this can suppress the formation of unreacted transition metals.

[0123] In another embodiment of the present invention, the molar ratio of the metal ions in the metal solution to the NaOH may be 1:1.5 to 1:2.5, preferably 1:1.8 to 1:2.3, and more preferably 1:1.94 to 1:2.05. It is desirable that the molar ratio of the metal in the metal solution to the NaOH satisfies the above range, as this can suppress the induction of unreacted transition metals.

[0124] If the above initial solution contains the above NH4OH and / or NaOH, the above first solution containing the above NH4OH and the above second solution containing the above NaOH may each be included to satisfy the molar ratio with respect to the metal in the metal solution.

[0125] The method for manufacturing a positive electrode active material precursor according to the present invention has the advantage of improving process loss caused by unreacted metal, as the concentration variation of the reaction solution during the reaction is suppressed, making it easy to add the first solution and the second solution in appropriate ratios. In addition, by inducing uniform diffusion, the compositional accuracy of the manufactured positive electrode active material precursor can be improved.

[0127] In another embodiment of the present invention, the step of introducing the reaction solution; and the step of stirring the initial solution and the reaction solution with a stirring means (60) to obtain an anode active material precursor may be performed simultaneously.

[0128] In summary, the method for manufacturing a positive electrode active material precursor according to the present invention can obtain a positive electrode active material precursor by stirring the initial solution and the reaction solution with the stirring means (60) while introducing the reaction solution.

[0129] The stirring speed of the stirring means (60) is not limited in the present invention. For example, the initial solution and the reaction solution may be stirred at 30 to 1500 rpm, preferably 50 to 1200 rpm, and more preferably 60 to 800 rpm.

[0131] The above-mentioned positive active material precursor may be recovered through the drain line provided at the bottom of the reaction vessel (10) and further undergo steps such as filtration, washing, and drying. The recovery, filtration, washing, and drying may be performed using conventional methods and are not limited thereto in the present invention.

[0133] The method for manufacturing a positive electrode active material precursor according to the present invention has the advantage of being able to suppress unreacted materials, and the positive electrode active material precursor manufactured by the method according to the present invention has excellent uniformity and sphericity and has the advantage of having a low impurity content.

[0134] In another embodiment of the present invention, the cathode active material precursor may have a Na content of 550 ppm or less, specifically 300 ppm or less, more specifically 100 ppm or less, most specifically 52 ppm or less.

[0135] In another embodiment of the present invention, the positive active material precursor may have an S content of 5000 ppm, specifically 3500 ppm or less, more specifically 1590 ppm or less.

[0137] Preferred embodiments and comparative examples of the present invention are described below. However, the following examples are merely preferred embodiments of the present invention, and the present invention is not limited to the following examples.

[0139] Examples

[0140] Deionized water, NaOH, and NH4OH were introduced as an initial solution into a reaction vessel equipped with a stirring means having two impellers located in the center of the interior, such that both impellers were submerged. At this time, based on 100% by weight of the total initial solution, 1.5% by weight of NaOH, 1.5% by weight of NH4OH, and the remainder of the deionized water were introduced and stirred. Both impellers had an angle of 45° relative to the horizontal direction, and the vertical center of the upper impeller was located at 1 / 3 of the way down from the bottom of the reaction vessel, and the vertical center of the lower impeller (63) was located at 1 / 6 of the way down from the bottom of the reaction vessel.

[0141] Afterwards, dissolved oxygen in the initial solution was removed by purging nitrogen at a rate of 10 L / min through the nitrogen injection pipe while maintaining stirring.

[0142] NiSO4, CoSO4, and MnSO4 were mixed in deionized water such that the molar ratio of nickel:cobalt:manganese was 0.89:0.04:0.07 to prepare a metal solution with a concentration of 2.5 M.

[0143] Subsequently, an aqueous NH4OH solution, an aqueous NaOH solution, and a metal solution were introduced as reaction solutions while maintaining stirring. At this time, each pipe for introducing the NH4OH solution, NaOH solution, and metal solution utilized a three-branched input pipe. The aqueous NH4OH solution was introduced at a flow rate of 23 kg / h, the aqueous NaOH solution at 210 kg / h, and the metal solution at 400 kg / h, ensuring that the ratio of NH4OH to the total molar amount of metal ions was 1:0.6 and the ratio of NaOH was 1:1.97. Stirring was performed at 550 rpm, and the reaction was maintained for 28 hours to obtain a cathode active material precursor using the co-precipitation method.

[0145] Comparative example

[0146] A positive electrode active material precursor was prepared using the same method as in the example, except that a conventional positive electrode active material precursor manufacturing apparatus (a three-stage impeller and unbranched input piping) was used.

[0148] Experimental Example

[0149] (1) SEM measurement results

[0150] The cathode active material precursors prepared according to the examples and comparative examples were measured using SEM images, and the results are shown in Figures 5a (Example) and 5b (Comparative Example), respectively.

[0152] (2) ICP analysis

[0153] Inductively coupled plasma (ICP) analysis was performed using an Agilent ICP 720-ES to determine the impurity content of the cathode active material precursors prepared according to the examples and comparative examples.

[0154] 2 g of precursor powder was dissolved in 10 mL of high-purity hydrochloric acid in an Erlenmeyer flask. The flask was covered with glass and heated on a hot plate to ensure complete dissolution of the precursor. After cooling to room temperature, the solution was transferred to a 100 mL volumetric flask, which had been washed 3 to 4 times with distilled (DI) water. Subsequently, the volumetric flask was filled with DI water to the 100 mL mark and then completely homogenized. 5 mL of the solution was withdrawn using a 5 mL pipette and transferred to a 50 mL volumetric flask for secondary dilution. The volumetric flask was then filled with 10% hydrochloric acid to the 50 mL mark and homogenized. This 50 mL solution was then used for ICP measurement, and the results are shown in Table 1 below.

[0156] Unit: ppm Examples Comparative example Na content 52 184 S content 1587 3066

[0158] (3) Measurement of unreacted Ni

[0159] The unreacted Ni in the cathode active material precursors prepared according to the examples and comparative examples was measured. After the co-precipitation reaction was completed, 15 g of the reaction solution of the cathode active material precursor was weighed and placed in a vial. Then, the vial was left for 1 hour to precipitate the cathode active material precursor, and the supernatant of the cathode active material precursor was obtained. Approximately 5 g of the supernatant of the cathode active material precursor was analyzed using inductively coupled plasma (ICP) analysis with an Agilent ICP 720-ES, and the results are shown in Table 2 below. Figures 6a and 6b show the supernatant of the cathode active material precursors prepared according to the examples and comparative examples, respectively.

[0161] Unit: ppm Examples Comparative example Unreacted Ni content 17 1906

[0163] Referring to FIGS. 5a to 6b and Tables 1 and 2, it can be seen that the cathode active material precursor prepared according to the example has excellent uniformity and sphericity, and has low levels of unreacted metal and impurities. Specifically, referring to FIGS. 6a and 6b, when nickel ions and ammonia form a coordinate bond, they exhibit a blue color; in the case of FIG. 6b, the supernatant appears dark, indicating that a large amount of unreacted transition metal remains.

[0165] The present invention is not limited to the above embodiments and can be manufactured in various different forms, and those skilled in the art will understand that the invention can be implemented in other specific forms without changing the technical concept or essential features of the invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. Explanation of the symbols

[0167] 10: Reaction vessel 20: First inlet pipe 30: Second input pipe 40: Third input pipe 50: Nitrogen injection piping 60: Stirring means 61: Shaft 62: Top impeller 63: Bottom impeller 100: Cathode active material precursor manufacturing device

Claims

Claim 1 A reaction vessel; one or more inlet pipes for introducing a reaction solution into the reaction vessel; and a stirring means located on the inner central side of the reaction vessel and stirring the reaction solution introduced from the introduction pipe; wherein the stirring means includes a shaft and a two-stage impeller, and the impeller has an angle of 5° to 90° with respect to the horizontal direction, and the introduction pipe includes a first introduction pipe for introducing a first solution containing NH4OH, a second introduction pipe for introducing a second solution containing NaOH, and a third introduction pipe for introducing a metal solution, wherein the first introduction pipe and the third introduction pipe are arranged adjacent to each other, and the second introduction pipe is arranged opposite the first introduction pipe and the third introduction pipe, and the first introduction pipe and the third introduction pipe each branch into three or four branches from a branching point, and the first introduction pipe and the third introduction pipe include a line extending from the first branched first introduction pipe and the third introduction pipe to the shaft, and from the last branched first introduction pipe and the third introduction pipe to the shaft A positive electrode active material precursor manufacturing apparatus arranged such that the angle formed by the extended line is 90° to 135°. Claim 2 An apparatus for manufacturing an anode active material precursor, wherein, in claim 1, the vertical center of the lower impeller located at the bottom is located at a point 1 / 15 to 1 / 5 of the way from the bottom of the reaction vessel. Claim 3 An apparatus for manufacturing an anode active material precursor, wherein, in claim 1, the vertical center of the upper impeller located at the top is located at a point 1 / 4 to 1 / 2 from the bottom of the reaction vessel. Claim 4 A positive electrode active material precursor manufacturing apparatus according to claim 1, wherein the two-stage impeller is inclined to have the same angle with respect to the horizontal direction. Claim 5 An apparatus for manufacturing a positive active material precursor according to claim 1, wherein the two-stage impeller has a diameter of 400 to 1550 mm. Claim 6 A cathode active material precursor manufacturing apparatus according to claim 1, wherein the input pipe has a diameter of 5 to 80 mm. Claim 7 An anode active material precursor manufacturing apparatus according to claim 1, wherein the input pipe has a thickness of 1 to 15 mm. Claim 8 delete Claim 9 A cathode active material precursor manufacturing apparatus according to claim 1, wherein the input piping further includes a deionized water input piping and a nitrogen input piping. Claim 10 A cathode active material precursor manufacturing apparatus according to claim 1, wherein the input piping is made of at least one material selected from stainless steel, PP, PVC, PE, and PVDF. Claim 11 delete Claim 12 delete Claim 13 A step of introducing an initial solution into a reaction vessel; a step of introducing a reaction solution into the reaction vessel into which the initial solution has been introduced; and a step of obtaining a positive electrode active material precursor by stirring the initial solution and the reaction solution with a stirring means; wherein the stirring means includes a shaft and a two-stage impeller, the impeller has an angle of 5° to 90° with respect to the horizontal direction, the initial solution is introduced so that the two-stage impeller is completely submerged, the reaction solution includes a first solution containing NH4OH, a second solution containing NaOH, and a metal solution, the first solution and the metal solution are introduced into the reaction vessel adjacent to each other by a first input pipe and a third input pipe, respectively, and the second solution is introduced into the reaction vessel on the opposite side of the first solution and the metal solution by a second input pipe, the first input pipe and the third input pipe are each branched into three or four branches from a branching point, and the first solution and the metal solution are a line extending from the first branched first input pipe and the third input pipe to the shaft, and the last branched first input pipe and the third A method for manufacturing an anode active material precursor, wherein the first input pipe and the third input pipe are introduced adjacent to each other into the reaction vessel such that the angle formed by the line extending from the input pipe to the shaft is 90° to 135°. Claim 14 A method for manufacturing a positive electrode active material precursor according to claim 13, wherein the initial solution comprises deionized water. Claim 15 delete Claim 16 A method for manufacturing a positive active material precursor according to claim 13, wherein the initial solution further comprises a portion of the first solution and the second solution. Claim 17 A method for manufacturing a positive active material precursor according to claim 13, wherein the step of introducing the reaction solution; and the step of stirring the initial solution and the reaction solution with a stirring means to obtain a positive active material precursor are performed simultaneously. Claim 18 A method for preparing an anode active material precursor according to claim 13, wherein the molar ratio of the metal ions in the metal solution to the NH4OH is 1:0.2 to 1:0.

9. Claim 19 A method for preparing an anode active material precursor according to claim 13, wherein the molar ratio of the metal ions in the metal solution and the NaOH is 1:1.5 to 1:2.

5. Claim 20 A method for manufacturing a positive electrode active material precursor according to claim 13, wherein the second solution is introduced at a flow rate of 40 to 1800 kg / h. Claim 21 A method for manufacturing an anode active material precursor according to claim 13, wherein the metal solution is introduced at a flow rate of 80 to 3200 kg / h. Claim 22 A method for manufacturing a positive active material precursor according to claim 13, wherein the positive active material precursor has a Na content of 550 ppm or less. Claim 23 A method for manufacturing a positive active material precursor according to claim 13, wherein the positive active material precursor has an S content of 5000 ppm or less.

Citation Information

Patent Citations

  • Batch reactor for preparing electrode active material and electrode active material precursor

    KR1020140074102A

  • Reaction Apparatus and Method

    KR1020180130241A