Lead―Free Piezoelectric Textured Ceramic Using 2―Dimensionally―Dispersed (2DD) Template Grain Growth and Method for Manufacturing the Same

The cross-stacking and RTGG method for lead-free piezoelectric ceramics addresses non-uniform orientation issues, achieving high crystal orientation and improved piezoelectric properties by aligning template particles and forming a homogeneous phase, resulting in superior electromechanical performance.

KR103046677B1Active Publication Date: 2026-11-10KOREA INST OF CERAMIC ENG & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
KR1020250068137
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-05-26
Publication Date
2026-11-10
Estimated Expiration
2045-05-26

AI Technical Summary

Technical Problem

Conventional Templated Grain Growth (TGG) methods for lead-free piezoelectric ceramics face issues with non-uniform orientation of plate-shaped template particles, leading to degraded piezoelectric and dielectric properties, and interlayer defects in multilayer structures, hindering the production of high-performance piezoelectrics.

Method used

A method involving the cross-stacking of a matrix piezoelectric ceramic sheet with a template sheet containing plate-shaped seeds, where the template sheet is thinner than the matrix, ensuring aligned growth without collisions, and a Reactive Templated Grain Growth (RTGG) process where the template reacts with the matrix to form a homogeneous phase.

Benefits of technology

This approach achieves over 99% crystal orientation and superior piezoelectric properties, with enhanced electromechanical coupling and dielectric characteristics, reducing interlayer defects and ensuring structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025058660411-PAT00001_ABST
    Figure 112025058660411-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a lead-free piezoelectric ceramic having a 2DD crystal orientation structure and a method for manufacturing the same. More specifically, by cross-stacking a matrix piezoelectric ceramic sheet of the same composition and a template sheet including a plate-shaped NaNbO₃ template seed and then sintering, the crystal orientation and piezoelectric properties can be simultaneously improved. The matrix piezoelectric ceramic sheet is composed of a composition of 0.96(Na0.525K0.475)(Nb0.9325Sb0.675)-0.02BaZrO₃-0.02(Bi0.5Ag0.5)ZrO₃+ 0.5 mol% Fe₂O₃ (NKNS-BZ-BAZ), and the plate-shaped seed is composed of a NaNbO₃ micro-platelet. By stacking these two sheets alternately and sintering them at 1085°C, preferential growth of template particles and high orientation can be induced, and as a result, the sintered body exhibits a crystal orientation of 99% or more according to XRD analysis, and can achieve a maximum strain of 0.158% and an induced piezoelectric constant (d33*) of 886 pm / V when an electric field of 1 kV / mm is applied.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a 2DD TGG (two-dimensionally-dispersed template grain growth) manufacturing technique for improving the crystal orientation of lead-free piezoelectric ceramics.

[0002] Specifically, the present invention relates to a lead-free piezoelectric ceramic and a method for manufacturing the same, which can induce the growth of texture particles and improve piezoelectric properties during sintering by cross-stacking a template sheet containing a plate-shaped template seed and a matrix piezoelectric ceramic sheet to form a crystal grain orientation structure made by a 2DD process. Background Technology

[0004] Lead-free piezoelectric ceramics are being actively researched as alternative materials capable of exhibiting excellent piezoelectric properties without containing lead (Pb), which poses a high risk to the environment. To further enhance the performance of these lead-free ceramics, the Templated Grain Growth (TGG) method, which induces crystal orientation, is widely utilized.

[0005] In the conventional TGG process, a slurry is prepared by mixing plate-shaped template particles with matrix ceramic powder, ceramic sheets are formed through tape casting, and then laminated in single or multilayers and sintered to form a textured structure. However, this method has the following technical limitations.

[0006] First, because plate-shaped template particles are randomly dispersed within the slurry, during tape casting, the template particles often clump together to form clusters, or tilt or non-uniform orientation frequently occurs where the template particles are not parallel to the sheet surface. These tilted templates collide with adjacent particles during the sintering process or distort the direction of crystal growth, thereby hindering the overall crystal orientation.

[0007] Second, the non-uniform orientation of template particles reduces the crystal orientation of piezoelectric ceramics during the firing process, which leads to a degradation of electrical properties such as the piezoelectric constant, dielectric constant, and electromechanical coupling coefficient, making it difficult to manufacture reproducible piezoelectric materials.

[0008] Third, particularly when forming multilayer structures, the non-uniform orientation of template particles in each layer can accumulate, causing interlayer defects, deformation, or differences in sintering shrinkage, which can be a significant obstacle to the realization of high-performance piezoelectrics.

[0009] Therefore, in the manufacturing of lead-free piezoelectric ceramics, there is a need for a new structural approach and process development that arranges plate-shaped template particles in a more aligned form to induce preferential growth during sintering, thereby securing high crystal orientation and excellent piezoelectric properties. The problem to be solved

[0011] In conventional lead-free piezoelectric ceramics, the template crystal growth method (TGG) has generally been used to improve crystal orientation. In this process, plate-shaped template particles are mixed into a matrix ceramic slurry, and a sheet is manufactured by tape casting, followed by sintering to induce a textured structure. However, plate-shaped seeds dispersed within the slurry often become tilted or unevenly dispersed during the casting process. This causes deviations in the growth direction of the textured crystals during sintering, leading to a problem where the overall crystal orientation is degraded. In particular, such tilting or collisions between particles cause the textured crystals to be interfered with by surrounding particles in the growth direction, hindering the uniform growth of the textured particles and consequently causing a degradation of piezoelectric and dielectric properties.

[0012] Furthermore, if the template particles and the matrix ceramic have different compositions, interfacial instability caused by differences in shrinkage rates or interdiffusion may occur during the sintering process; in particular, when forming a multilayer stacked structure, there is a possibility of interlayer gaps or microcracks forming, which poses a problem in terms of reliability.

[0013] Accordingly, the present invention implements a structure capable of preferentially inducing the growth of texture particles and maximizing crystal orientation by separately manufacturing a matrix piezoelectric ceramic sheet of the same composition and a template sheet containing plate-shaped seeds, then stacking them alternately to form a laminate, and sintering it. In particular, by forming the template sheet thinner than the matrix sheet, texture growth is induced to proceed first in the layer where the template plate-shaped seeds are concentrated, and the structure is configured to allow crystals to grow without collision with the matrix sheet; consequently, high crystal orientation and excellent piezoelectric properties can be secured simultaneously. means of solving the problem

[0015] A method for manufacturing a stacked lead-free piezoelectric textured ceramic according to one embodiment of the present invention comprises: 1) preparing a matrix piezoelectric ceramic sheet; 2) preparing and placing a template sheet containing plate-shaped seeds on the matrix piezoelectric ceramic sheet; 3) placing the matrix piezoelectric ceramic sheet again on the template sheet; 4) repeating steps 2) and 3) one or more times; and 5) sintering the stacked laminate, wherein the matrix piezoelectric ceramic sheet and the template sheet containing plate-shaped seeds are made of the same lead-free piezoelectric ceramic composition.

[0016] The above matrix piezoelectric ceramic sheet does not contain plate-shaped seeds.

[0017] The step of preparing the above matrix piezoelectric ceramic sheet is 0.96 (Na 0.525 K0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 The method includes the steps of: preparing a slurry containing 0.5 mol% Fe2O3 piezoelectric powder (NKNS-BZ-BAZ powder) and performing ball milling; and producing a piezoelectric sheet using the slurry through a tape casting process.

[0018] The above 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 )ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder is prepared by weighing the molecular weights of raw materials Na2CO3, K2CO3, Nb2O5, BaCO3, ZrO2, Bi2O3, Ag2O, and Fe2O3 according to the composition formula, and by calcining at a temperature of 750 to 850℃ for 4 to 8 hours.

[0019] The above calcined powder is further ball-milled for 24 hours and then dried in an oven to finally obtain the above NKNS-BZ-BAZ calcined powder.

[0020] The above slurry is a mixture of ethanol, toluene, dibutyl phthalate, a binder, a dispersant, and the above NKNS-BZ-BAZ calcined powder according to the composition ratio.

[0021] The composition ratio is 41 wt% for the NKNS-BZ-BAZ calcined powder and 59 wt% for the remainder.

[0022] The above matrix piezoelectric ceramic sheet is an NKNS-BZ-BAZ green sheet with a thickness of about 30 μm.

[0023] The step of preparing a template sheet including the above plate-shaped seed is 0.96 (Na 0.525 K 0.475)(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 A step of preparing a slurry containing 0.5 mol% Fe2O3 piezoelectric powder (NKNS-BZ-BAZ powder) and performing ball milling;

[0024] The method includes the step of adding plate-shaped seeds to the slurry and mixing them; and the step of producing a template sheet using the slurry through a tape casting process.

[0025] The above 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 )ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder is prepared by weighing the molecular weights of raw materials Na2CO3, K2CO3, Nb2O5, BaCO3, ZrO2, Bi2O3, Ag2O, and Fe2O3 according to the composition formula, and by calcining at a temperature of 750 to 850℃ for 4 to 8 hours.

[0026] The above calcined powder is further ball-milled for 24 hours and then dried in an oven to finally obtain the above NKNS-BZ-BAZ calcined powder.

[0027] The above slurry is a mixture of ethanol, toluene, dibutyl phthalate, a binder, a dispersant, and the above NKNS-BZ-BAZ calcined powder according to the composition ratio.

[0028] The composition ratio is 41 wt% for the NKNS-BZ-BAZ calcined powder and 59 wt% for the remainder.

[0029] The above plate-shaped seed includes NaNbO3(NN) micro-platelets.

[0030] The above NN micro-platelets are included in an amount of 3.40g per 100g of slurry.

[0031] The above template sheet is an NKNS-BZ-BAZ + NN green sheet with a thickness of about 5 μm.

[0032] The step of sintering the stacked laminate is performed at a temperature of 1080 to 1090°C. It is preferable that the step of sintering the stacked laminate be performed at a temperature of 1085°C.

[0033] It is preferable that the thickness of the above template sheet be thinner than the thickness of the above matrix piezoelectric ceramic sheet.

[0034] After the above sintering step, a step of forming electrodes on both sides of the device may be additionally included, and after forming the electrodes, the electrodes are sintered by heat treatment. Effects of the invention

[0036] According to the present invention, by cross-stacking a matrix piezoelectric ceramic sheet having the same lead-free piezoelectric composition and a template sheet including a plate-shaped NaNbO₃ template seed and then sintering, a crystal orientation structure can be formed that prevents tilting or random orientation of template particles and induces preferential growth of texture particles.

[0037] In particular, the present invention sets the sintering temperature to 1080–1090°C and confirmed that the best crystal orientation and electrical properties can be secured when sintered at 1085°C. In fact, X-ray diffraction (XRD) analysis results of the 2DD sample sintered at 1085°C showed a crystal orientation of over 99% in all directions (f L It exhibited ), which is a significantly superior figure compared to a 3DD structure of the same composition. In addition, a maximum strain of 0.158% (S when an electric field of 1 kV / mm is applied) max ) and induced piezoelectric constant of 886 pm / V (d 33 *It represents ) which means a higher piezoelectric response characteristic compared to 0.136%, 424 pm / V shown by the 3DD structure under the same conditions.

[0038] These results are attributed to the realization of an optimal structure in which textured crystal grains can complete growth without colliding with adjacent grains by embedding plate-shaped template seeds in a thin template sheet and cross-stacking them with a matrix sheet. In addition, the template sheet and the matrix sheet are identical NKNS-BZ-BAZ (0.96(Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 Because it has a composition of )ZrO3+ 0.5 mol% Fe2O3), differences in physical properties or non-uniform shrinkage at the interface during sintering do not occur, thereby ensuring the structural stability and reliability of the entire laminate, and consequently, a high-performance lead-free piezoelectric ceramic device can be realized. Brief explanation of the drawing

[0041] FIG. 1 illustrates a flowchart of a method for manufacturing a stacked lead-free piezoelectric textured ceramic according to one embodiment of the present invention. FIG. 2 illustrates a schematic diagram of a ceramic laminate according to one embodiment of the present invention. FIG. 3 illustrates an NKNS-BZ-BAZ slurry batching table according to an embodiment of the present invention. Figure 4 shows the strain and induced piezoelectric coefficient (d) according to the electric field of a stacked piezoelectric texture ceramic according to the 3DD method. 33 * Graphs and tables showing the changes in ) are illustrated. FIG. 5 shows the strain and induced piezoelectric coefficient (d) according to the electric field of a stacked piezoelectric texture ceramic according to the 2DD method of the present invention. 33 * Graphs and tables showing the changes in ) are illustrated. Figure 6 is a graph showing the XRD diffraction pattern according to the sintering temperature of a stacked piezoelectric texture ceramic manufactured by the 3DD method. Figure 7 is a graph showing the XRD diffraction pattern according to the sintering temperature of a stacked piezoelectric texture ceramic manufactured using a 2DD structure method according to the present invention. FIG. 8 shows a graph comparing the physical properties of a stacked piezoelectric texture ceramic with a 3DD structure and a 2DD structure according to the present invention, evaluated under sintering temperature conditions from 1070°C to 1100°C. Figure 9 is an image showing the results of observing the microstructure of a stacked lead-free piezoelectric ceramic according to a conventional 3DD TGG process at a sintering temperature (1070℃~1100℃) using a scanning electron microscope (SEM). Figure 10 is an image showing the results of observing the microstructure of a stacked lead-free piezoelectric ceramic manufactured by the 2DD TGG process according to the present invention as a function of sintering temperature (1070℃~1100℃) using a scanning electron microscope (SEM). FIG. 11 is a comparison diagram of a manufacturing process according to a conventional 3DD RTGG process and a manufacturing process according to a 2DD RTGG process according to the present invention. Figure 12 shows a comparison of FE-SEM images of lead-free piezoelectric ceramics manufactured according to the 3DD RTGG process and the 2DD RTGG process. Various embodiments are now described with reference to the drawings, and throughout the drawings, similar reference numerals are used to denote similar elements. For illustrative purposes, various descriptions are provided in this specification to facilitate an understanding of the invention. However, it is evident that these embodiments can be practiced without such specific descriptions. In other examples, known structures and devices are presented in the form of block diagrams to facilitate the description of the embodiments. Specific details for implementing the invention

[0042] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. As the present invention is susceptible to various modifications and may take various forms, specific embodiments are illustrated in the drawings and described in detail in the text. However, this is not intended to limit the present invention to the specific disclosed forms, and it should be understood that the invention includes all modifications, equivalents, and substitutions that fall within the spirit and scope of the invention. Similar reference numerals have been used for similar components in the description of each drawing.

[0043] The terms used in this application are used merely to describe specific embodiments and are not intended to limit the invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this application, terms such as "comprising" or "having" are intended to indicate the presence of the features, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the existence or addition of one or more other features, steps, actions, components, parts, or combinations thereof.

[0044] The present invention relates to a lead-free piezoelectric ceramic having a 2DD crystal orientation structure and a method for manufacturing the same. More specifically, by cross-stacking a matrix piezoelectric ceramic sheet of the same composition and a template sheet including a plate-shaped NaNbO₃ template seed and then sintering, the crystal orientation and piezoelectric properties can be improved simultaneously.

[0045] In conventional lead-based TGG processes, plate-shaped BaTiO₃ (BT) templates remain within the matrix even after sintering, forming a structure where the textured crystals remain intact. However, in the present invention, the NaNbO₃ template undergoes a chemical reaction with a lead-free matrix of the same series during sintering and disappears, ultimately forming a homogeneous phase. This feature clearly distinguishes the process from conventional TGG processes in that the template particles perform only the function of inducing the direction of crystal growth during the initial sintering stage, and subsequently react completely with the matrix. Therefore, in the process of the present invention, TGG can be defined as a Reactive Templated Grain Growth (RTGG) method, which corresponds to a novel lead-free texture process capable of simultaneously achieving texture induction and homogeneous phase formation.

[0046] FIG. 1 illustrates a flowchart of a method for manufacturing a stacked lead-free piezoelectric textured ceramic according to one embodiment of the present invention.

[0047] As illustrated in FIG. 1, a method for manufacturing a stacked lead-free piezoelectric textured ceramic according to one embodiment of the present invention comprises: 1) preparing a matrix piezoelectric ceramic sheet; 2) preparing and placing a template sheet including a plate-shaped seed on the matrix piezoelectric ceramic sheet; 3) placing the matrix piezoelectric ceramic sheet again on the template sheet; 4) repeating steps 2) and 3) one or more times; and 5) sintering the stacked laminate.

[0048] In step 1), a matrix piezoelectric ceramic sheet is prepared. The matrix piezoelectric ceramic sheet does not contain plate-shaped seeds.

[0049] The step of preparing the matrix piezoelectric ceramic sheet is 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675)-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 The method includes the steps of: preparing a slurry containing 0.5 mol% Fe2O3 piezoelectric powder (NKNS-BZ-BAZ powder) and performing ball milling; and producing a piezoelectric sheet using the slurry through a tape casting process.

[0050] In this case, the above 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 The )ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder is prepared by weighing the molecular weights of raw materials Na2CO3, K2CO3, Nb2O5, BaCO3, ZrO2, Bi2O3, Ag2O, and Fe2O3 according to the compositional formula, and is used after calcination at a temperature of 750 to 850°C for 4 to 8 hours. Preferably, calcination can be carried out at a temperature of 800°C for 6 hours. The powder after calcination is further ball-milled for 24 hours and then dried in an oven to finally obtain the NKNS-BZ-BAZ calcined powder.

[0051] The above slurry is prepared by mixing ethanol, toluene, dibutyl phthalate, a binder, a dispersant, and the NKNS-BZ-BAZ calcined powder according to the compositional ratio. Preferably, the compositional ratio is such that the NKNS-BZ-BAZ calcined powder is 41 wt% and the remainder is 59 wt%, and the matrix piezoelectric ceramic sheet produced with this composition is an NKNS-BZ-BAZ green sheet with a thickness of approximately 30 μm. Further details will be explained in the examples described later.

[0052] 2) In step 2), a template sheet containing plate-shaped seeds is prepared and placed on a matrix piezoelectric ceramic sheet.

[0053] In this case, the thickness of the template sheet is thinner than the thickness of the matrix piezoelectric ceramic sheet. By forming the template sheet thinner than the matrix sheet, texture growth is induced to proceed first in the layer where the template plate-shaped seeds are concentrated, and the crystals are configured to grow without collision with the matrix sheet, thereby enabling high crystal orientation and excellent piezoelectric properties to be secured simultaneously.

[0054] The step of preparing a template sheet including the above plate-shaped seed is 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 The method includes the steps of: preparing a slurry containing 0.5 mol% Fe2O3 piezoelectric powder (NKNS-BZ-BAZ powder) and performing ball milling; adding plate-shaped seeds to the slurry and mixing; and producing a template sheet using a tape casting process with the slurry.

[0055] In this case, the above 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 The )ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder is prepared by weighing the molecular weights of raw materials Na2CO3, K2CO3, Nb2O5, BaCO3, ZrO2, Bi2O3, Ag2O, and Fe2O3 according to the compositional formula, and is used after calcination at a temperature of 750 to 850°C for 4 to 8 hours. Preferably, calcination can be carried out at a temperature of 800°C for 6 hours. The powder after calcination is further ball-milled for 24 hours and then dried in an oven to finally obtain the NKNS-BZ-BAZ calcined powder.

[0056] The plate-shaped seeds contain NaNbO3(NN) micro-platelets. It is preferable to include 3.40 g of these NN micro-platelets per 100 g of slurry.

[0057] In this invention, the NaNbO₃ template reacts with the matrix during the sintering process to induce only the directionality of crystal growth in the initial texturing stage, and subsequently disappears completely to form a homogeneous phase. Accordingly, the matrix composition is designed with a certain reduction in the content of Na and Nb as the template disappears, and is designed to ultimately form a Morphological Boundary (MPB) when the template composition and the matrix composition are combined.

[0058] The above slurry is prepared by mixing ethanol, toluene, dibutyl phthalate, a binder, a dispersant, and the NKNS-BZ-BAZ calcined powder according to the compositional ratio. Preferably, the compositional ratio is such that the NKNS-BZ-BAZ calcined powder is 41 wt% and the remainder is 59 wt%, and the template sheet produced with this composition is an NKNS-BZ-BAZ + NN green sheet with a thickness of approximately 5 μm. Further details will be explained in the examples described later.

[0059] A method for manufacturing a stacked lead-free piezoelectric textured ceramic according to one embodiment of the present invention can be configured such that a matrix piezoelectric ceramic sheet and a template sheet including a plate-shaped seed are alternately arranged in a plurality of layers by repeating steps 2) and 3) one or more times. FIG. 2 illustrates a schematic diagram of a ceramic stack according to one embodiment of the present invention.

[0060] The step of sintering the stacked laminate can be performed in an oxygen atmosphere at a temperature of 1070 to 1100°C, preferably 1080 to 1090°C, most preferably 1085°C, for 4 to 8 hours, preferably 5 to 7 hours, most preferably 6 hours.

[0061] In the case of the stacked lead-free piezoelectric textured ceramic produced in this way, the matrix piezoelectric ceramic sheet and the template sheet including plate-shaped seeds are made of the same lead-free piezoelectric ceramic composition.

[0062] After the sintering step, a step of forming electrodes on both sides of the device may be additionally included, and after forming the electrodes, the electrodes are sintered by heat treatment. Afterward, dry or wet polarization (air poling or wet poling) may be performed using an electric field.

[0063] In this invention, after final fabrication, the NaNbO₃ template undergoes a chemical reaction with a linkage-free matrix of the same series during sintering and disappears, ultimately forming a homogeneous phase. That is, the template particles perform only the function of inducing the directionality of crystal growth during the initial sintering stage, and are subsequently completely absorbed into the matrix.

[0064] Ceramic properties (e.g., d) for a stacked lead-free piezoelectric texture ceramic according to one embodiment of the present invention manufactured in this manner 33 Characteristics, etc. were measured, and such piezoelectric structures can be used as actuators, transducers, sensors, and energy harvesters.

[0065] Below, the contents of the present invention will be further explained along with specific embodiments.

[0067] In the examples, ceramic properties were tested after manufacturing each of the 3DD manufacturing method and the 2DD manufacturing method to compare them.

[0068] 3DD stands for Three Dimensionally Dispersed. According to conventional technology, plate-shaped seeds randomly dispersed within a ceramic slurry often tilt and become inverted within a piezoelectric ceramic sheet produced by a tape casting method. This reduces crystal orientation during the sintering process, making it difficult to expect excellent piezoelectric properties.

[0069] 2DD stands for Two Dimensionally Dispersed. It is a laminated structure consisting of a matrix piezoelectric ceramic sheet / template sheet / matrix piezoelectric ceramic sheet / template sheet / matrix piezoelectric ceramic sheet. By preventing tilting through this 2DD process, the quality and orientation of the texture grain can be significantly improved, and ultimate piezoelectric properties can be obtained.

[0071] 1) 0.96(Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 Synthesis of )ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder

[0072] 0.96(Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5)ZrO3+ 0.5 mol% Fe2O3(NKNS-BZ-BAZ) piezoelectric powder was prepared via a general solid-state synthesis method. The raw materials used were Na2CO3 (Kojundo Chemical, 99%, Japan), K2CO3 (Kojundo Chemical, 99%, Japan), Nb2O5 (Kojundo Chemical, 99.9%, Japan), BaCO3 (Kojundo Chemical, 99.95%, Japan), ZrO2 (Kojundo Chemical, 98%, Japan), Bi2O3 (Kojundo Chemical, 99.9%, Japan), Ag2O (Sigma-Aldrich, 99%, USA), and Fe2O3 (Kojundo Chemical, 99.9%, Japan). Since Na2CO3, K2CO3, and BaCO3 have a potential for water content, they were dried in a 120°C oven for at least 5 hours and removed immediately for weighing. After weighing the raw powders according to the compositional formula of NKNS-BZ-BAZ, they were placed in a polyethylene bottle along with zirconia balls (ф= 1 mm, 3 mm, 5 mm, 10 mm), and ball milled for 24 hours after adding an equal amount of ethanol. The milled mixture was dried in a 90°C oven. The dried powder was placed in an alumina crucible, heated to 800°C at a heating rate of 5°C per minute, and calcined for 6 hours. The calcined powder was again placed in a polyethylene bottle along with ethanol and zirconia balls (ф= 1 mm, 3 mm, 5 mm, 10 mm), ball milled for 24 hours, and then dried in a 90°C oven to obtain calcined NKNS-BZ-BAZ powder.

[0074] 2) Manufacture of NKNS-BZ-BAZ piezoelectric ceramic matrix sheets

[0075] Ethanol (99.9%, Daejeong Chemical, Korea), toluene (99.9%, Daejeong Chemical, Korea), dibutyl phthalate (99%, Daejeong Chemical, Korea), polyvinyl butyral (BM-SZ, Sekisui, Japan), dispersant (BYK-111, BYK-Chemie GmbH, Germany), and NKNS-BZ-BAZ calcined powder were mixed in various proportions according to the composition ratios in Table 1. The mixture was placed in a polyethylene bottle along with zirconia balls (ф= 3 mm, 5 mm, 10 mm) and mixed and ground for 24 hours to prepare a slurry. The prepared slurry was sieved using a mesh cloth, and a degassing process was performed for 10 minutes using a vacuum degassing machine to remove residual bubbles remaining in the slurry. Subsequently, an aging process was carried out for 2 hours at 15 rpm to stabilize the slurry. The stabilized slurry was subjected to a tape casting process under conditions of a blade gap of 100 μm and a casting speed of 1 m / min, and green sheets were successfully manufactured for all compositions from #1 to #5 as shown in Fig. 3. Among them, an optimized NKNS-BZ-BAZ green sheet with a thickness of approximately 30 μm was obtained from composition #4. Fig. 3 shows an NKNS-BZ-BAZ slurry batch table according to an embodiment of the present invention.

[0077] 3) Preparation of NKNS-BZ-BAZ + NaNbO3 micro-platelet green sheet

[0078] NKNS-BZ-BAZ powder, ethanol (99.9%, Daejeong Chemical, Korea), toluene (99.9%, Daejeong Chemical, Korea), dibutyl phthalate (99%, Daejeong Chemical, Korea), a dispersant (BYK-111, BYK-Chemie GmbH, Germany), and a binder, polyvinyl butyral (BM-SZ, Sekisui, Japan), were mixed according to the composition (#4) of Fig. 3. This mixture was placed in a polyethylene bottle along with zirconia balls (ф= 3 mm, 5 mm, 10 mm) and mixed using a stirrer at a speed of 2000 rpm for 1 hour to prepare a slurry. The prepared slurry was sieved using a mesh cloth, and then 3.40 g of NaNbO3(NN) micro-platelets and a small amount of ethanol were mixed per 100 g of slurry. This mixture was then placed in a vial and dispersed using a sonicator for 5 minutes. Subsequently, this mixture was combined with the existing slurry and thoroughly mixed. To remove residual bubbles contained in the slurry, a degassing process was performed for 10 minutes using a vacuum degassing machine, and an aging process was performed for 2 hours at 15 rpm to stabilize the slurry. Tape casting was performed on the stabilized slurry under conditions of a blade gap of 12 μm and a casting speed of 3 m / min, and as a result, an NKNS-BZ-BAZ + NN green sheet with a thickness of approximately 5 μm was obtained.

[0080] 4) Fabrication and firing of ceramic laminates

[0081] To fabricate a ceramic laminate, NKNS-BZ-BAZ green sheets and NKNS-BZ-BAZ + NN green sheets manufactured by a tape casting process were alternately laminated as shown in Fig. 2. Lamination was performed under conditions of 60°C and 10 MPa, ultimately forming a ceramic laminate with a thickness of approximately 1.2 mm. The fabricated laminate was further compressed through a warm isostatic pressing (WIP) process for 20 minutes under conditions of 65°C and 25 MPa. After the WIP was completed, the laminate was cut into 10 mm × 10 mm pieces using a blade cutter, and organic matter was removed (burn-out) by heating to 450°C at a heating rate of 1°C / min and maintaining the temperature for 5 hours. Subsequently, a cold isostatic pressing (CIP) process was performed for 2 minutes at a pressure of 200 MPa. The specimens, after the completion of the CIP process, were sintered for 6 hours under various temperature conditions ranging from 1070°C to 1100°C at a heating rate of 5°C / min. Electrodes were formed on both sides of the sintered ceramic device by screen printing Ag paste, and electrode firing was completed by heat treatment at 700°C for 10 minutes. To relieve residual stress that may occur at the electrode-ceramic interface during electrode firing, the specimens were heat-treated in silicone oil at 210°C for 2 hours. Finally, a poling process was performed for 20 minutes by applying an electric field of 3 kV / mm in silicone oil at 25°C, after which the piezoelectric and dielectric properties of the fabricated device were evaluated.

[0083] 5) Comparison of Physical Property Evaluations

[0084] Figure 4 shows the strain and induced piezoelectric coefficient (d) according to the electric field of a stacked piezoelectric texture ceramic according to the 3DD method. 33 *Graphs and tables showing the change of ) are presented. The sample consists of a composition of 0.96KNN-0.02BZ-0.02BAZ and is based on a 3DD structure sintered at 1085℃ for 6 hours. As the electric field increases, the strain increases up to a maximum of 0.136%, and (d 33 * The value was measured at 424 pm / V. This result represents the average response characteristics obtainable from conventional 3D texturing methods, and while it shows an excellent electrical response under specific conditions, it can be confirmed that there is a tendency for the growth direction of texture particles to be non-uniform or restricted.

[0085] FIG. 5 shows the strain and induced piezoelectric coefficient (d) according to the electric field of a stacked piezoelectric texture ceramic according to the 2DD method of the present invention. 33 * A graph and table showing the change of ) are presented. The corresponding sample was also sintered at 1085℃ for 6 hours. As a result of the measurement, the maximum strain was approximately 0.158%, and (d 33 * The value reached a maximum of 529 pm / V. This confirmed that it exhibits higher piezoelectric characteristics compared to the 3DD method of Fig. 4.

[0086] Figure 6 is a graph showing the XRD diffraction patterns of stacked piezoelectric textured ceramics fabricated by the 3DD method according to the sintering temperature. Based on the relative intensity ratio of the (001) and (002) diffraction peaks of each sample measured under various sintering temperature conditions from 1070°C to 1100°C, the crystal orientation (f L ) was calculated, and as a result, under the condition of 1070℃, f L This was relatively low at 94%, and was measured at 98% at 1080–1085°C and 97% at 1100°C. This suggests that while the degree of crystal orientation may be temporarily improved under specific temperature conditions in the 3D texturing method, the overall uniformity and consistency of orientation are somewhat limited.

[0087] Figure 7 is a graph showing the XRD diffraction patterns of a stacked piezoelectric textured ceramic manufactured using the 2DD structure method according to the present invention as a function of sintering temperature. Even under the same sintering temperature conditions ranging from 1070°C to 1100°C, f was consistently observed in all samples L This was maintained at 99%, which clearly demonstrates the characteristics of crystal orientation in which the growth path of texture crystal grains is stably secured by cross-stacking the template sheets at regular intervals. These results indicate that the 2DD structure according to the present invention can secure superior crystal orientation compared to the 3DD structure, and support the fact that it is a structure suitable for mass production processes due to its wide process window for temperature and excellent repeatability.

[0088] FIG. 8 shows a graph comparing the physical properties of stacked piezoelectric texture ceramics of a 3DD structure and a 2DD structure according to the present invention, evaluated under sintering temperature conditions ranging from 1070°C to 1100°C. The items compared are the relative permittivity ratio, dielectric breakdown electric field (ε0), and electromechanical coupling coefficient (k p ), Machine quality factor (Q m ), and electromechanical conversion gain coefficient (g 33 ...and was measured under the same composition and the same heat treatment conditions.

[0089] The measurement results showed that, overall, the 2DD structure exhibited superior characteristics compared to the 3DD structure in all categories, and among them, the electromechanical coupling coefficient (k p ) and induced piezoelectric coefficient (d 33 ) showed the most significantly improved results in the 2DD structure. Under 1085℃ conditions k p The 2DD structure showed a significantly higher value of approximately 59.1% compared to 50% for the 3DD structure, and the induced piezoelectric coefficient d 33Furthermore, based on the proportional relationship of relative permittivity, the 2DD structure maintained a tendency to be higher than the 3DD structure under all temperature conditions in values ​​indirectly derived. This is attributed to the structural effect resulting from the aligned orientation of template particles and the consequently clearly controlled grain growth pathways; in particular, in the 2DD structure according to the present invention, the growth of texture crystals is effectively achieved, resulting in a high k p and d 33 It was possible to realize these characteristics. These characteristics are critical elements required for high-performance piezoelectric devices, demonstrating that the structure of the present invention is a highly advantageous technology in terms of practical applications.

[0090] Figure 9 is an image showing the results of observing the microstructure of a stacked lead-free piezoelectric ceramic manufactured according to a conventional 3DD TGG process as a function of sintering temperature (1070°C to 1100°C) using a scanning electron microscope (SEM). Figure 10 is an image showing the results of observing the microstructure of a stacked lead-free piezoelectric ceramic manufactured according to the 2DD TGG process according to the present invention as a function of sintering temperature (1070°C to 1100°C) using a scanning electron microscope (SEM). Compared to 3DD, the 2DD process was observed to have a structure in which the growth direction of textured particles is clearly aligned, particle boundaries are distinct, and overall density is maintained at a high level. In particular, the specimen sintered at 1085°C exhibited a very dense microstructure with almost no pores and a uniform particle size distribution, confirming that it is the most stable structure in terms of crystal growth and sintering density. The 2DD structure clearly demonstrates the excellence of the process, which exhibits excellent microstructural consistency with changes in sintering temperature overall and simultaneously improves crystal orientation and piezoelectric properties under optimal conditions.

[0091] FIG. 11 is a comparison diagram of a manufacturing process according to a conventional 3DD RTGG process and a manufacturing process according to a 2DD RTGG process according to the present invention.

[0092] When the 2DD RTGG process according to the present invention is applied to the crystal orientation of lead-free piezoelectric ceramics, an improvement in density was also confirmed. This is because NKN lead-free crystal particles have an angular structure, but using the 2DD RTGG process causes them to align parallel, thereby reducing micropores at the interface. Figure 12 illustrates a comparison of FE-SEM images of lead-free piezoelectric ceramics manufactured according to the 3DD RTGG process and the 2DD RTGG process. As shown in Figure 12, when comparing the microstructures, micropores were observed at the textured grain boundaries due to the misaligned NN template when the 3DD RTGG process was used, whereas when the 2DD RTGG process according to the present invention was used, it was confirmed that micropores were reduced due to parallel alignment. Through this, density can be increased, which contributes to the improvement of dielectric strength characteristics in lead-free piezoelectric materials.

[0094] Although the present invention has been described above with reference to preferred embodiments, those skilled in the art will understand that various modifications and changes can be made to the invention without departing from the spirit and scope of the invention as set forth in the following claims.

Claims

Claim 1 delete Claim 2 delete Claim 3 1) a step of preparing a matrix piezoelectric ceramic sheet; 2) a step of preparing and placing a template sheet containing plate-shaped seeds on the matrix piezoelectric ceramic sheet; 3) a step of placing the matrix piezoelectric ceramic sheet again on the template sheet; 4) a step of repeating steps 2) and 3) one or more times; 5) a step of sintering the stacked laminate, wherein the matrix piezoelectric ceramic sheet and the template sheet containing plate-shaped seeds are made of the same lead-free piezoelectric ceramic composition, and the step of preparing the matrix piezoelectric ceramic sheet comprises 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, comprising the steps of: preparing a slurry containing 0.5 mol% Fe2O3 piezoelectric powder (NKNS-BZ-BAZ powder) and performing ball milling; and producing a piezoelectric sheet from the slurry using a tape casting process. Claim 4 In claim 3, the above 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein the ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder is prepared by weighing the molecular weights of Na2CO3, K2CO3, Nb2O5, BaCO3, ZrO2, Bi2O3, Ag2O, and Fe2O3 raw materials according to the compositional formula, and calcining is carried out at a temperature of 750 to 850°C for 4 to 8 hours. Claim 5 A method for manufacturing a stacked lead-free piezoelectric textured ceramic according to claim 4, wherein the calcined powder is further ball-milled for 24 hours and then dried in an oven to finally obtain the NKNS-BZ-BAZ calcined powder. Claim 6 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein, in claim 3, the slurry is a mixture of ethanol, toluene, dibutyl phthalate, a binder, a dispersant, and the NKNS-BZ-BAZ calcined powder according to a compositional ratio. Claim 7 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein, in claim 6, the composition ratio is 41 wt% for the NKNS-BZ-BAZ calcined powder and 59 wt% for the remainder. Claim 8 A method for manufacturing a laminated lead-free piezoelectric textured ceramic, wherein the matrix piezoelectric ceramic sheet is an NKNS-BZ-BAZ green sheet with a thickness of about 30 μm. Claim 9 1) a step of preparing a matrix piezoelectric ceramic sheet; 2) a step of preparing and placing a template sheet containing plate-shaped seeds on the matrix piezoelectric ceramic sheet; 3) a step of placing the matrix piezoelectric ceramic sheet again on the template sheet; 4) a step of repeating steps 2) and 3) one or more times; 5) a step of sintering the stacked laminate, wherein the matrix piezoelectric ceramic sheet and the template sheet containing plate-shaped seeds are made of the same lead-free piezoelectric ceramic composition, and the step of preparing the template sheet containing plate-shaped seeds is 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, comprising the steps of: preparing a slurry containing 0.5 mol% Fe2O3 piezoelectric powder (NKNS-BZ-BAZ powder) and performing ball milling; adding plate-shaped seeds to the slurry and mixing; and producing a template sheet using a tape casting process with the slurry. Claim 10 In claim 9, the above 0.96 (Na 0.525 K 0.475 )(Nb 0.9325 Sb 0.675 )-0.02BaZrO3-0.02(Bi 0.5 Ag 0.5 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein the ZrO3+ 0.5 mol% Fe2O3 piezoelectric powder is prepared by weighing the molecular weights of Na2CO3, K2CO3, Nb2O5, BaCO3, ZrO2, Bi2O3, Ag2O, and Fe2O3 raw materials according to the compositional formula, and calcining is carried out at a temperature of 750 to 850°C for 4 to 8 hours. Claim 11 A method for manufacturing a stacked lead-free piezoelectric textured ceramic according to claim 10, wherein the calcined powder is further ball-milled for 24 hours and then dried in an oven to finally obtain the NKNS-BZ-BAZ calcined powder. Claim 12 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein, in claim 9, the slurry is a mixture of ethanol, toluene, dibutyl phthalate, a binder, a dispersant, and the NKNS-BZ-BAZ calcined powder according to a compositional ratio. Claim 13 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein, in claim 12, the composition ratio is 41 wt% for the NKNS-BZ-BAZ calcined powder and 59 wt% for the remainder. Claim 14 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein the plate-shaped seed comprises a NaNbO3(NN) micro-platelet. Claim 15 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein the NN micro-platelets are included at a rate of 3.40 g per 100 g of slurry. Claim 16 A method for manufacturing a laminated lead-free piezoelectric textured ceramic, wherein the template sheet is an NKNS-BZ-BAZ + NN green sheet with a thickness of about 5 μm. Claim 17 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, comprising: 1) a step of preparing a matrix piezoelectric ceramic sheet; 2) a step of preparing and placing a template sheet containing plate-shaped seeds on the matrix piezoelectric ceramic sheet; 3) a step of placing the matrix piezoelectric ceramic sheet again on the template sheet; 4) a step of repeating steps 2) and 3) one or more times; and 5) a step of sintering the stacked laminate, wherein the matrix piezoelectric ceramic sheet and the template sheet containing plate-shaped seeds are made of the same lead-free piezoelectric ceramic composition, and the step of sintering the stacked laminate is performed at a temperature of 1080 to 1090°C. Claim 18 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, comprising: 1) a step of preparing a matrix piezoelectric ceramic sheet; 2) a step of preparing and placing a template sheet containing plate-shaped seeds on the matrix piezoelectric ceramic sheet; 3) a step of placing the matrix piezoelectric ceramic sheet again on the template sheet; 4) a step of repeating steps 2) and 3) one or more times; and 5) a step of sintering the stacked laminate, wherein the matrix piezoelectric ceramic sheet and the template sheet containing plate-shaped seeds are made of the same lead-free piezoelectric ceramic composition, and the step of sintering the stacked laminate is performed at a temperature of 1085°C. Claim 19 A method for manufacturing a laminated lead-free piezoelectric textured ceramic, wherein, in any one of claims 3 to 18, the thickness of the template sheet is thinner than the thickness of the matrix piezoelectric ceramic sheet. Claim 20 A method for manufacturing a stacked lead-free piezoelectric textured ceramic, wherein, in any one of claims 3 to 18, the step of forming electrodes on both sides of the element after the sintering step is further included. Claim 21 A method for manufacturing a stacked lead-free piezoelectric textured ceramic according to claim 20, wherein the electrode is fired by heat treatment after forming the electrode. Claim 22 delete

Citation Information

Patent Citations

  • Laminated Piezoelectric Texture Ceramic and Method for Manufacturing the Same

    KR102766868B1