Lithium secondary battery comprising a separator

The lithium secondary battery design addresses the issue of silicon-based negative electrode expansion by using a separator with defined thickness, compressibility, and dielectric breakdown voltage, preventing micro shorts and maintaining battery performance.

KR103046740B1Active Publication Date: 2026-11-11LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
KR1020230009562
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-28
Filing Date
2023-01-25
Publication Date
2026-11-11
Estimated Expiration
2043-01-25

AI Technical Summary

Technical Problem

Silicon-based negative electrode materials in lithium-ion batteries experience rapid volume expansion during charging and discharging, leading to a rough surface that penetrates the separator and causes micro shorts, and existing solutions fail to address this issue effectively.

Method used

A lithium secondary battery design incorporating a silicon-based negative electrode with specific parameters: a separator thickness of 1 μm to 15 μm, compressibility of 1% to 14.5% defined by Equation 1, and a dielectric breakdown voltage of 400 V or more, ensuring the separator maintains rigidity and prevents damage during volume expansion.

Benefits of technology

The battery design prevents micro shorts and maintains performance by controlling the physical properties of the separator to withstand the expansion of the silicon-based negative electrode, ensuring stable operation and high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023008902345-PAT00001_ABST
    Figure 112023008902345-PAT00001_ABST
Patent Text Reader

Abstract

The present application relates to a separator for a lithium secondary battery and a lithium secondary battery including the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0012968 filed with the Korean Intellectual Property Office on January 28, 2022, the entire contents of which are incorporated herein.

[0002] The present application relates to a lithium secondary battery comprising a separator. Background Technology

[0003] Due to the rapid increase in the use of fossil fuels, there is a growing demand for alternative or clean energy. As part of this effort, the fields of power generation and energy storage utilizing electrochemical reactions are the most actively researched.

[0004] Currently, a representative example of an electrochemical device utilizing such electrochemical energy is the secondary battery, and its scope of application is steadily expanding.

[0005] With the increasing technological development and demand for mobile devices, the demand for secondary batteries as an energy source is rapidly rising. Among these secondary batteries, lithium-ion batteries, which possess high energy density and voltage, long cycle life, and low self-discharge rates, have been commercialized and are widely used. Furthermore, active research is being conducted on methods to manufacture high-density electrodes with higher energy density per unit volume for use in such high-capacity lithium-ion batteries.

[0006] Generally, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and extracts lithium ions from the positive electrode, and silicon-based particles with a large discharge capacity may be used as the negative electrode active material.

[0007] In particular, due to the recent demand for high-density energy batteries, research is actively being conducted on methods to increase capacity by using silicon-based compounds such as Si / C or SiOx, which have a capacity more than 10 times greater than that of graphite-based materials, as negative electrode active materials. However, silicon-based compounds, which are high-capacity materials, have a problem in that, although they have a large capacity compared to graphite used conventionally, they rapidly expand in volume during the charging process, which disrupts the conductive path and degrades battery characteristics.

[0008] In addition, silicon-based cathodes undergo a carbonization process, during which more than 50% of the cathode binder contained in the silicon-based cathode is lost, resulting in a problem where the surface becomes very rough. In other words, during the carbonization process of the silicon-based cathode, the surface of the silicon-based cathode becomes very rough, and as a result, there is a problem where it penetrates the separator and comes into contact with the anode, causing a micro short.

[0009] Accordingly, in order to resolve the problems associated with using silicon-based compounds as negative electrode active materials, methods such as adding a coating layer to the surface of the separator or changing the separator material are being researched as solutions; however, no suitable solution has been established at present.

[0010] Therefore, research is needed on separators capable of withstanding the pressure and roughness when the separator is compressed by expansion during charging and discharging of a silicon-based cathode with a rough surface. Prior art literature

[0011] Japanese Patent Publication No. 2009-080971 The problem to be solved

[0012] Research results regarding a separator capable of withstanding pressure and roughness when the separator is compressed by expansion during charging and discharging of a silicon-based anode having a rough surface confirmed through research that the above-mentioned problem can be solved by controlling the physical properties of the separator itself. Accordingly, this application relates to a lithium secondary battery comprising a separator under specific conditions. means of solving the problem

[0013] One embodiment of the present specification is a lithium secondary battery comprising: a silicon-based negative electrode; a positive electrode; a separator located between the negative electrode and the positive electrode; and an electrolyte; wherein the silicon-based negative electrode comprises: a negative electrode current collector layer; and a negative electrode active material layer comprising a negative electrode active material layer composition provided on one or both sides of the negative electrode current collector layer; and wherein the negative electrode active material layer composition comprises one or more selected from the group consisting of a silicon-based active material; a negative electrode conductive material; and a negative electrode binder, and wherein the silicon-based active material comprises SiOx (x=0) and SiOx (0 <x<2) 로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함하며, 상기 분리막은 1μm 이상 15 μm 이하 두께를 만족하고, 하기 식 1로 정의되는 내압축성이 1% 이상 14.5% 이하이고, 절연파괴전압이 400V 이상인 것인 리튬 이차 전지를 제공한다.

[0014] [Equation 1]

[0015] (T1-T2) / T1 X 100

[0016] In the above Equation 1,

[0017] T1 refers to the initial thickness of the state in which three layers of the above-mentioned separator are stacked, and

[0018] T2 refers to the thickness after stacking three sheets of the above-mentioned separator and pressing them in a hot press (Q-mesys QM-940A Grade) at 2000 kgf, 70°C, for 10 seconds, and

[0019] The above dielectric breakdown voltage refers to the voltage at which the insulation breaks down while stepping up the monocell containing the above separator from 0V to 6000V at a rate of 100V / s using Chroma’s Hipot tester (AC / DC / IR Tester). Effects of the invention

[0020] A lithium secondary battery according to one embodiment of the present invention uses a silicon-based negative electrode, and is characterized by satisfying all three parameters: a thickness of 1 μm to 15 μm so that the separator can maintain a rigid shape even when the rough negative electrode surface, which is the volume expansion of the silicon-based negative electrode during charging and discharging, comes into contact with the separator; a compressibility defined by Equation 1 of 1% or more and 14.5% or less; and an dielectric breakdown voltage of 400 V or more.

[0021] That is, in the case of the lithium secondary battery in this application, the three parameters defined as the thickness range of the separator, dielectric breakdown voltage, and compressibility are set to a suitable range, thereby having the feature of being able to solve the existing problems that occur in lithium secondary batteries using silicon-based negative electrodes. Brief explanation of the drawing

[0022] FIG. 1 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present application. Specific details for implementing the invention

[0023] Before describing the present invention, we will first define some terms.

[0024] In this specification, when a part is described as "comprising" a certain component, it means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0025] In this specification, 'p to q' means a range of 'p or more and q or less'.

[0026] In this specification, "specific surface area" is measured by the BET method, specifically calculated from the amount of nitrogen gas adsorbed at a liquid nitrogen temperature (77K) using BELSORP-mino II of BEL Japan. That is, in this application, the BET specific surface area may refer to the specific surface area measured by the above measurement method.

[0027] In this specification, "Dn" refers to the particle size distribution and represents the particle size at the n% point of the cumulative distribution of the number of particles according to particle size. That is, D50 is the particle size (center particle size, average particle size) at the 50% point of the cumulative distribution of the number of particles according to particle size, D90 is the particle size at the 90% point of the cumulative distribution of the number of particles according to particle size, and D10 is the particle size at the 10% point of the cumulative distribution of the number of particles according to particle size. Meanwhile, the particle size distribution can be measured using the laser diffraction method. Specifically, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500) and the difference in diffraction patterns according to particle size is measured as the particles pass through the laser beam to calculate the particle size distribution.

[0028] In this specification, the meaning that a polymer contains a monomer in monomer units means that the monomer participates in a polymerization reaction and is included as a repeating unit within the polymer. In this specification, when it is stated that a polymer contains a monomer, this is interpreted as the same as the polymer containing the monomer in monomer units.

[0029] In this specification, the term "polymer" is understood to be used in a broad sense including copolymers unless specified as "homopolymer."

[0030] In this specification, the weight-average molecular weight (Mw) and the number-average molecular weight (Mn) are polystyrene equivalent molecular weights measured by gel permeation chromatography (GPC), using commercially available monodisperse polystyrene polymers of various degrees of polymerization (standard samples) for molecular weight measurement as standard materials. In this specification, the term "molecular weight" means weight-average molecular weight unless otherwise specified.

[0031] Hereinafter, the present invention will be described in detail with reference to the drawings so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in various different forms and is not limited to the description below.

[0032] One embodiment of the present specification is a lithium secondary battery comprising: a silicon-based negative electrode; a positive electrode; a separator located between the negative electrode and the positive electrode; and an electrolyte; wherein the silicon-based negative electrode comprises: a negative electrode current collector layer; and a negative electrode active material layer comprising a negative electrode active material layer composition provided on one or both sides of the negative electrode current collector layer; and wherein the negative electrode active material layer composition comprises one or more selected from the group consisting of a silicon-based active material; a negative electrode conductive material; and a negative electrode binder, and wherein the silicon-based active material comprises SiOx (x=0) and SiOx (0 <x<2) 로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함하며, 상기 분리막은 1μm 이상 15 μm 이하 두께를 만족하고, 하기 식 1로 정의되는 내압축성이 1% 이상 14.5% 이하이고, 절연파괴전압이 400V 이상인 것인 리튬 이차 전지를 제공한다.

[0033] [Equation 1]

[0034] (T1-T2) / T1 X 100

[0035] In the above Equation 1,

[0036] T1 refers to the initial thickness of the state in which three layers of the above-mentioned separator are stacked, and

[0037] T2 refers to the thickness after stacking three sheets of the above-mentioned separator and pressing them in a hot press (Q-mesys QM-940A Grade) at 2000 kgf, 70°C, for 10 seconds, and

[0038] The above dielectric breakdown voltage refers to the voltage at which the insulation breaks down while stepping up the monocell containing the above separator from 0V to 6000V at a rate of 100V / s using Chroma’s Hipot tester (AC / DC / IR Tester).

[0039] In the case of a separator according to one embodiment of the present invention, it satisfies all three parameters, such as a thickness of 1 μm to 15 μm, a compression resistance defined by Equation 1 of 1% or more and 14.5% or less, and an dielectric breakdown voltage of 400 V or more, and is characterized in that the separator can maintain a rigid form even when a rough cathode surface due to volume expansion during charging and discharging of a silicon-based cathode comes into contact with the separator.

[0040] FIG. 1 is a diagram showing a stacked structure of a lithium secondary battery according to one embodiment of the present application. Specifically, a negative electrode (100) for a lithium secondary battery including a negative active material layer (20) on one surface of a negative current collector layer (10) can be seen, and a positive electrode (200) for a lithium secondary battery including a positive active material layer (40) on one surface of a positive current collector layer (50) can be seen, and the structure is formed such that the negative electrode (100) for a lithium secondary battery and the positive electrode (200) for a lithium secondary battery are stacked with a separator (30) in between.

[0041] The silicon-based cathode, which is one of the feature parts of the present invention, will be described below.

[0042] In one embodiment of the present application, the silicon-based cathode comprises: a cathode current collector layer; and a cathode active material layer comprising a cathode active material layer composition provided on one or both sides of the cathode current collector layer, wherein the cathode active material layer composition comprises one or more selected from the group consisting of a silicon-based active material; a cathode conductive material; and a cathode binder.

[0043] In one embodiment of the present application, the silicon-based active material is SiOx (x=0) and SiOx (0 <x<2) 로 이루어진 군에서 선택되는 1 이상을 포함하며, 상기 실리콘계 활물질 100 중량부 기준 상기 SiOx (x=0)를 70 중량부 이상 포함하는 것인 리튬 이차 전지를 제공한다.

[0044] In another embodiment, based on 100 parts by weight of the silicon-based active material, the SiOx (x=0) may be included in an amount of 70 parts by weight or more, preferably 80 parts by weight or more, more preferably 90 parts by weight or more, and 100 parts by weight or less, preferably 99 parts by weight or less, more preferably 95 parts by weight or less.

[0045] In one embodiment of the present application, the silicon-based active material may particularly use pure silicon (Si) as the silicon-based active material. Using pure silicon (Si) as the silicon-based active material means that, when the silicon-based active material is based on 100 parts by weight of the total as described above, pure Si particles (SiOx (x=0)) that are not bonded with other particles or elements are included in the above range.

[0046] Although attempts to apply silicon-based active materials are increasing due to their significantly higher capacity compared to conventionally used graphite-based active materials, their use is limited to cases where they are mixed in trace amounts with graphite-based active materials because of their high volume expansion rate during the charging and discharging process.

[0047] In addition, compared to carbon-based anodes, the active material included in the silicon-based anode has a very rough surface, which caused a problem where it penetrated the separator and came into contact with the anode, resulting in a micro short circuit. However, the lithium secondary battery according to the present application has the characteristic of preventing micro short circuits while having excellent capacity characteristics and energy density by controlling the physical properties of the separator described below, even when using an anode with a very rough surface as described above.

[0048] Meanwhile, the average particle size (D50) of the silicon-based active material of the present invention may be 5㎛ to 10㎛, specifically 5.5㎛ to 8㎛, and more specifically 6㎛ to 7㎛. When the average particle size falls within the above range, the specific surface area of ​​the particles is within a suitable range, and the viscosity of the cathode slurry is formed within an appropriate range. Accordingly, the dispersion of particles constituting the cathode slurry becomes smooth. In addition, since the size of the silicon-based active material has a value greater than or equal to the lower limit range, the contact area between the silicon particles and the conductive material is excellent due to the composite composed of the conductive material and the cathode binder within the cathode slurry, which increases the likelihood of the conductive network continuing and thus increases the capacity retention rate. Meanwhile, when the average particle size satisfies the above range, excessively large silicon particles are excluded, and the surface of the cathode is formed smoothly, thereby preventing current density non-uniformity during charging and discharging.

[0049] In one embodiment of the present application, the silicon-based active material generally has a characteristic BET surface area. The BET surface area of ​​the silicon-based active material is preferably 0.01 to 150.0 m² 2 / g, more preferably 0.1 to 100.0 m 2 / g, particularly preferably 0.2 to 80.0 m 2 / g, most preferably 0.2 to 18.0 m 2 / g. The BET surface area is measured according to DIN 66131 (using nitrogen).

[0050] In one embodiment of the present application, the silicon-based active material may exist in, for example, a crystalline or amorphous form and is preferably not porous. The silicon particles are preferably spherical or fragmentary particles. Alternatively, but less preferably, the silicon particles may also have a fibrous structure or exist in the form of a silicon-containing film or coating.

[0051] In one embodiment of the present application, the silicon-based active material may be 60 parts by weight or more based on 100 parts by weight of the negative electrode active material layer composition.

[0052] In another embodiment, the silicon-based active material may comprise at least 60 parts by weight, preferably at least 65 parts by weight, more preferably at least 70 parts by weight, based on 100 parts by weight of the negative electrode active material layer composition, and may comprise 95 parts by weight or less, preferably 90 parts by weight or less, more preferably 80 parts by weight or less.

[0053] The negative electrode active material layer composition according to the present application uses a specific conductive material and binder capable of controlling the volume expansion rate during the charging and discharging process even when using a silicon-based active material with significantly high capacity within the above range, thereby having the characteristic of not degrading the performance of the negative electrode even when including the above range and having excellent output characteristics during charging and discharging.

[0054] In one embodiment of the present application, the silicon-based active material may have a non-spherical shape, and the sphericity is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.

[0055] In the present application, the circularity is determined by the following formula A-1, where A is the area and P is the boundary line.

[0056] [Formula A-1]

[0057] 4πA / P 2

[0058] Conventionally, it was common practice to use only graphite-based compounds as negative electrode active materials; however, with the recent rise in demand for high-capacity batteries, there have been increasing attempts to mix in silicon-based compounds to increase capacity. Nevertheless, silicon-based compounds have a limitation in that their volume expands rapidly during the charging and discharging process, damaging the conductive pathways formed within the negative electrode active material layer and actually degrading battery performance.

[0059] Accordingly, in one embodiment of the present application, the cathode conductive material may include one or more selected from the group consisting of a point-type conductive material; a linear conductive material; and a planar conductive material.

[0060] In one embodiment of the present application, the point-shaped conductive material can be used to improve conductivity of the cathode and refers to a spherical or point-shaped conductive material having conductivity without causing chemical changes. Specifically, the point-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, Farnes black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably may include carbon black in terms of achieving high conductivity and excellent dispersibility.

[0061] In one embodiment of the present application, the point-shaped conductive material has a BET specific surface area of ​​40 m² 2 / g or more 70m 2 It may be less than / g, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2It may be less than / g.

[0062] In one embodiment of the present application, the point-shaped conductive material may satisfy a volatile matter content of 0.01% or more and 0.05% or less, preferably 0.01% or more and 0.04% or less, and more preferably 0.01% or more and 0.03% or less.

[0063] Specifically, as the dispersibility of the point-shaped conductive material is improved, the viscosity of the cathode slurry can be maintained at an appropriate level even when the content of the point-shaped conductive material is increased in a cathode slurry having the same solid content, so the uniformity of the cathode formed can be improved while maintaining a stable processability.

[0064] In one embodiment of the present application, the particle size of the dot-shaped conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 20 nm to 60 nm.

[0065] In one embodiment of the present application, the conductive material may include a planar conductive material.

[0066] The above-mentioned planar conductive material can be described as a plate-shaped conductive material or a bulk-shaped conductive material, as it can improve conductivity by increasing surface contact between silicon particles within the cathode and simultaneously suppress the interruption of conductive pathways due to volume expansion.

[0067] In one embodiment of the present application, the planar conductive material may comprise at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and preferably may be plate-shaped graphite.

[0068] In one embodiment of the present application, the average particle size (D50) of the planar conductive material may be 2 μm to 7 μm, specifically 3 μm to 6 μm, and more specifically 4 μm to 5 μm. When the above range is satisfied, dispersion is easy without causing an excessive increase in the viscosity of the cathode slurry due to the sufficient particle size. Therefore, when dispersion is performed using the same equipment and time, the dispersion effect is excellent.

[0069] In one embodiment of the present application, the planar conductive material provides a cathode composition in which D10 is 0.5 μm or more and 1.5 μm or less, D50 is 2.5 μm or more and 3.5 μm or less, and D90 is 7.0 μm or more and 15.0 μm or less.

[0070] In one embodiment of the present application, the planar conductive material may be a high specific surface area planar conductive material having a high BET specific surface area; or a low specific surface area planar conductive material.

[0071] In one embodiment of the present application, a planar conductive material with a high specific surface area or a planar conductive material with a low specific surface area may be used without limitation as the planar conductive material; however, since the planar conductive material according to the present application may be affected to some extent by dispersion in electrode performance, it may be particularly preferable to use a planar conductive material with a low specific surface area that does not cause problems with dispersion.

[0072] In one embodiment of the present application, the planar conductive material has a BET specific surface area of ​​5 m² 2 It can be more than / g.

[0073] In another embodiment, the planar conductive material has a BET specific surface area of ​​5m² 2 / g or more than 500m 2 It may be less than / g, preferably 5m 2 / g or more than 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2It may be less than / g.

[0074] In another embodiment, the planar conductive material is a high specific surface area planar conductive material, and has a BET specific surface area of ​​50 m² 2 / g or more than 500m 2 / g or less, preferably 80m 2 / g or more than 300m 2 / g or less, more preferably 100m 2 / g or more than 300m 2 It can satisfy a range of / g or less.

[0075] In another embodiment, the planar conductive material is a low specific surface area planar conductive material, and the BET specific surface area is 5m² 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 It can satisfy a range of / g or less.

[0076] Other conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundled carbon nanotubes. The bundled carbon nanotubes may comprise a plurality of carbon nanotube units. Specifically, "bundle type" here refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged in parallel or intertwined with the axes along the length direction of the carbon nanotube units in substantially the same orientation, unless otherwise noted. The carbon nanotube units have a graphite sheet having a cylindrical shape with a nano-sized diameter and an sp2 bonding structure. Depending on the angle and structure in which the graphite sheet is rolled, it may exhibit conductive or semiconductor properties. Compared to entangled type carbon nanotubes, the bundled carbon nanotubes described above can be uniformly dispersed during cathode manufacturing and smoothly form a conductive network within the cathode, thereby improving the conductivity of the cathode.

[0077] In one embodiment of the present application, the cathode conductive material comprises a linear conductive material, and the linear conductive material may be a carbon nanotube.

[0078] In one embodiment of the present application, the carbon nanotubes may be SWCNTs or / and MWCNTs. When the linear conductive agent is an SWCNT, the length of the SWCNT may be 0.5 μm to 100 μm, preferably 1 μm to 80 μm.

[0079] In one embodiment of the present application, the cathode conductive material may be 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the cathode active material layer composition.

[0080] In another embodiment, the cathode conductive material may comprise 10 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, based on 100 parts by weight of the cathode active material layer composition, and more preferably 10 parts by weight or more and 20 parts by weight or less.

[0081] The cathode conductive material according to the present application has a completely separate composition from the conductive material applied to the anode. That is, the cathode conductive material according to the present application serves to hold the contact points between silicon-based active materials, which undergo significant volume expansion of the electrodes due to charging and discharging, whereas the anode conductive material serves as a buffer during rolling and provides partial conductivity; thus, their composition and roles are completely different from those of the cathode conductive material of the present invention.

[0082] Furthermore, the cathode conductive material according to the present application is applied to silicon-based active materials and has a completely different composition from that of a conductive material applied to graphite-based active materials. That is, a conductive material used in an electrode having a graphite-based active material simply has particles smaller than the active material, thereby providing improved output characteristics and some conductivity; thus, its composition and role are completely different from that of a cathode conductive material applied together with a silicon-based active material as in the present invention.

[0083] In one embodiment of the present application, the plate-shaped conductive material used as the aforementioned negative electrode conductive material has a structure and function different from that of a carbon-based active material generally used as a negative electrode active material. Specifically, the carbon-based active material used as a negative electrode active material may be artificial graphite or natural graphite, and refers to a material processed into a spherical or dot shape to facilitate the storage and release of lithium ions.

[0084] On the other hand, planar (plate-shaped) conductive materials used as cathode conductive materials are substances having a planar or plate-like form, which can be described as plate-shaped graphite. In other words, they refer to materials included to maintain conductive pathways within the cathode active material layer; rather than serving the role of lithium storage and release, they refer to materials intended to secure conductive pathways in a planar form within the cathode active material layer.

[0085] In other words, in the present application, the fact that planar (plate-shaped) graphite is used as a conductive material means that it is processed into a planar or plate-shaped form and used as a material that secures a conductive pathway rather than serving the role of storing or releasing lithium. At this time, the negative electrode active material included together has high capacity characteristics for lithium storage and release and plays a role in storing and releasing all lithium ions delivered from the positive electrode.

[0086] On the other hand, in the present application, the fact that a carbon-based active material is used as an active material means that it is processed into a point or spherical shape and used as a material that serves the role of storing or releasing lithium.

[0087] That is, in one embodiment of the present application, the carbon-based active material, artificial graphite or natural graphite, is in a point-like form, with a BET specific surface area of ​​0.1 m² 2 / g or more than 4.5 m 2 It can satisfy a range of / g or less. In addition, plate-shaped graphite, a planar conductive material, has a planar form with a BET specific surface area of ​​5m² 2 It can be more than / g.

[0088] In one embodiment of the present application, the cathode binder may comprise at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and materials in which hydrogens thereof are substituted with Li, Na, or Ca, etc., and may also comprise various copolymers thereof.

[0089] The cathode binder according to one embodiment of the present application serves to hold the active material and the conductive material to prevent distortion and structural deformation of the cathode structure during volume expansion and relaxation of the silicon-based active material. Any general binder that satisfies the above role can be applied, specifically a water-based binder can be used, and more specifically, a PAM-based binder can be used.

[0090] In one embodiment of the present application, the cathode binder may be included in an amount of 30 parts by weight or less, preferably 25 parts by weight or less, more preferably 20 parts by weight or less, based on 100 parts by weight of the cathode active material layer composition, and may be included in an amount of 5 parts by weight or more, or 10 parts by weight or more.

[0091] In one embodiment of the present application, the negative electrode current collector layer generally has a thickness of 1 μm to 100 μm. Such a negative electrode current collector layer is not particularly limited as long as it possesses high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy may be used. In addition, fine irregularities may be formed on the surface to strengthen the bonding strength of the negative electrode active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In one embodiment of the present application, a lithium secondary battery is provided in which the surface roughness (Ra) of the surface of the negative electrode active material layer in contact with the separator is 3 μm or more and 10 μm or less.

[0092] In one embodiment of the present application, a lithium secondary battery is provided in which the thickness of the negative electrode current collector layer is 1 μm or more and 100 μm or less, and the thickness of the negative electrode active material layer is 10 μm or more and 100 μm or less.

[0093] In one embodiment of the present application, a lithium secondary battery is provided in which the thickness of the negative electrode active material layer is 10 μm or more and 100 μm or less.

[0094] However, the thickness may vary depending on the type and application of the cathode used, and is not limited thereto.

[0095] In one embodiment of the present application, the porosity of the negative electrode active material layer may satisfy a range of 10% or more and 60% or less.

[0096] In another embodiment, the porosity of the negative electrode active material layer may satisfy a range of 10% or more and 60% or less, preferably 20% or more and 50% or less, and more preferably 30% or more and 45% or less.

[0097] The above porosity varies according to the composition and content of the silicon-based active material, conductive material, and binder included in the negative electrode active material layer, and in particular, the range of the above porosity is satisfied by including the silicon-based active material and conductive material according to the present application in a specific composition and content, and accordingly, the electrical conductivity and resistance of the electrode have an appropriate range.

[0098] The separator according to the present application satisfies all three of the above conditions, and each condition is described below.

[0099] A separator according to one embodiment of the present specification satisfies a thickness of 1 μm or more and 15 μm or less.

[0100] According to another embodiment, the separator may satisfy a thickness of 1 μm or more and 15 μm or less, preferably 3 μm or more and 15 μm or less, more preferably 6 μm or more and 15 μm or less, and 10 μm or more and 15 μm or less.

[0101] The thickness of the above-mentioned separator may refer to the thickness of one sheet when one sheet is used, and a total thickness range including two or more sheets when two or more sheets are used.

[0102] If the thickness of the separator satisfies the above range, damage to the separator can be minimized even if contact occurs when the rough-surfaced silicon-based negative electrode expands; if it is less than the above range, even if the compressibility and dielectric breakdown voltage described later are satisfied, the separator may be perforated by the expansion of the negative electrode, and if it exceeds the above range, the exchange of lithium ions between the positive and negative electrodes is not smooth, which may result in defects in the lithium secondary battery.

[0103] A separator according to one embodiment of the present application may satisfy a compression resistance defined by Formula 1 below in the range of 1% or more and 14.5% or less.

[0104] [Equation 1]

[0105] (T1-T2) / T1 X 100

[0106] In the above Equation 1,

[0107] T1 refers to the initial thickness of the state in which three layers of the above-mentioned separator are stacked, and

[0108] T2 refers to the thickness after stacking three layers of the above separator and pressing at 2000 kgf, 70°C, and 10 seconds in a hot press (Q-mesys QM-940A Grade).

[0109] In another embodiment, the compressibility defined by Equation 1 may satisfy the range of 1% or more and 14.5% or less, 5% or more and 14.5% or less, 10% or more and 14.5% or less, and 10.5% or more and 14.5% or less.

[0110] In one embodiment of the present application, the compressibility of Formula 1 may mean the ratio of the thickness of the separator after applying pressure to the separator under conditions within a certain range to the thickness when no pressure is applied, and low compressibility may mean that the separator is compressed less.

[0111] When the above compressibility satisfies the above range, the durability of the separator increases. If it is below the above range, the separator cannot flexibly respond to the rough surface of the cathode, causing breakage or puncture of the separator. If it exceeds the above range, the separator becomes excessively rigid, making it difficult for lithium ions to pass through, which may result in a problem of increased diffusion resistance.

[0112] In addition, separators made of only an inorganic layer without polymers such as PE or PP are evaluated to have very low compressibility. In this case, since they are almost uncompressed, the pores of the separator remain in their initial state, so the passage of lithium ions is smooth during charging and discharging, and the diffusion resistance does not increase further.

[0113] In one embodiment of the present application, the dielectric breakdown voltage of the separator may be 400V or higher.

[0114] In another embodiment, the dielectric breakdown voltage of the separator may satisfy a range of 400V or more, preferably 450V or more, 6000V or less, preferably 5000V or less, and 2000V or less.

[0115] The above dielectric breakdown voltage refers to the voltage at which the insulation breaks down while increasing the voltage from 0V to 6000V at a rate of 100V / s using Chroma’s Hipot tester (AC / DC / IR Tester) containing the above separator, and the higher the measured voltage, the more the separator can withstand the higher voltage.

[0116] When the above dielectric breakdown voltage satisfies the above range, the durability of the separator increases, and if it is below the above range, the separator may break or be punctured by a rough-surfaced cathode. The fact that the dielectric breakdown voltage is measured means that charge is flowing, and if it falls below the lower limit range as described above, it can be determined that a short circuit has occurred.

[0117] That is, the separator according to the present application must satisfy all three of the above conditions to enable the operation of a lithium secondary battery without damage to the separator even with volume expansion of a silicon-based negative electrode with a rough surface.

[0118] In one embodiment of the present application, the compressibility and dielectric breakdown voltage can satisfy the above range by controlling the molecular weight and internal pore distribution of the separator.

[0119] Specifically, the higher the molecular weight of the material constituting the separator, the stronger the compressibility and dielectric breakdown voltage. In this case, the separator according to the present application satisfies the above range by controlling the molecular weight and simultaneously controlling the thickness to satisfy the range of compressibility and dielectric breakdown voltage.

[0120] In addition, by controlling the pore distribution together, the compressibility and dielectric breakdown voltage ranges are satisfied. Generally, by uniformly distributing the pores of the separator membrane, which have a level of 10 nm or more, the compressibility and dielectric breakdown voltage ranges can be controlled to the above ranges.

[0121] That is, the separator according to the present application is characterized by satisfying the above compressibility and dielectric breakdown voltage by adjusting the molecular weight range, internal pore distribution, and thickness range to a suitable range.

[0122] In one embodiment of the present application, the weight-average molecular weight of the separation membrane may include a range of 1,000,000 g / mol or more and 10,000,000 g / mol or less.

[0123] In another embodiment, the weight-average molecular weight of the separation membrane may satisfy a range of 1,000,000 g / mol or more and 10,000,000 g / mol or less, preferably 1,000,000 g / mol or more and 9,000,000 g / mol or less, and more preferably 1,000,000 g / mol or more and 8,000,000 g / mol or less.

[0124] In addition, in one embodiment of the present application, the pore size of the separator may satisfy a range of 10 nm or more and 100 nm or less, specifically a range of 20 nm or more and 60 nm or less, and the compressibility and dielectric breakdown voltage may be controlled by appropriately adjusting the distribution according to the pore size.

[0125] As an example, in the case of a separator with 40 nm pores and a separator with 20 nm pores, if the pore distribution of the separator with 20 nm pores is made uniform, the compressibility and dielectric breakdown voltage can be increased.

[0126] In one embodiment of the present application, the separator is a wet separator; or a dry separator, thereby providing a separator for a lithium secondary battery.

[0127] The above wet membrane and dry membrane can be distinguished based on differences in the process itself.

[0128] Specifically, a wet separation membrane can be manufactured by mixing polyethylene and paraffin, extruding the mixture, and then passing the film through methylene chloride (MC) to melt the paraffin. Since polyethylene does not dissolve in MC, the pores formed in the places where the paraffin was melted can be used to manufacture the wet separation membrane.

[0129] The above dry separation membrane can be manufactured by extruding a polypropylene polymer into a film and then stretching it to create gaps between the polymer chains.

[0130] In one embodiment of the present application, the separator for a lithium secondary battery comprises one or more selected from the group consisting of a porous polymer film; a porous nonwoven fabric; and a ceramic component.

[0131] Specifically, the separator separates the negative and positive electrodes and provides a pathway for the movement of lithium ions. Any separator typically used in secondary batteries can be used without special restrictions, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte wettability. Specifically, a porous polymer film, such as a porous polymer film made from a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymer materials may be used to ensure heat resistance or mechanical strength, and it may optionally be used in a single-layer or multi-layer structure.

[0132] That is, the separator of the present application can be used without limitation in type as long as it falls within the range satisfying the three parameters above.

[0133] In one embodiment of the present application, the separator may comprise a single layer; or two or more layers.

[0134] In one embodiment of the present application, the positive electrode may include a positive electrode current collector layer and a positive electrode active material layer formed on the positive electrode current collector layer and comprising the positive electrode active material.

[0135] In the above-mentioned positive electrode, the positive electrode current collector layer is not particularly limited as long as it is conductive without causing chemical changes in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector layer may typically have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesion of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0136] The above-mentioned positive electrode active material may be a commonly used positive electrode active material. Specifically, the above-mentioned positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4 (0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2, etc.; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7, etc.; chemical formula LiNi 1-c2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, satisfying 0.01≤c2≤0.3); chemical formula LiMn 2-c3 M c3Examples include lithium manganese composite oxides represented by O2 (where M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, satisfying 0.01≤c3≤0.1) or Li2Mn3MO8 (where M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn); and LiMn2O4 in which a portion of the Li in the chemical formula is substituted with alkaline earth metal ions, but are not limited thereto. The anode may also be Li-metal.

[0137] In one embodiment of the present application, the anode is LiNi x Co y Mn z O2(x+y+z=1); LiNi a Co b Mn c Al d O2(a+b+c+d=1); LiMn2O4; LiNi 0.5 Mn 1.5 O2; and LiM x Fe y A lithium secondary battery comprising one or more selected from the group consisting of PO4 (M: Transition metal, x+y=1) is provided.

[0138] The above-described positive active material layer may include a positive conductive material and a positive binder together with the positive active material described above.

[0139] At this time, the positive electrode conductive material is used to impart conductivity to the electrode, and in the battery being constructed, any material that has electronic conductivity without causing chemical changes can be used without special limitations. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powder or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used.

[0140] In addition, the anode binder serves to improve adhesion between anode active material particles and adhesion between the anode active material and the anode current collector layer. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used.

[0141] Examples of the above electrolytes that can be used in the manufacture of lithium secondary batteries include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., but are not limited to these.

[0142] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0143] As the above-mentioned non-aqueous organic solvent, for example, aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyl lactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolone, formamide, dimethylformamide, dioxolone, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolone derivative, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivative, tetrahydrofuran derivative, ether, methyl propionate, ethyl propionate, etc. may be used.

[0144] In particular, among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants that effectively dissociate lithium salts, so they can be used preferably. Furthermore, if low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate are mixed with these cyclic carbonates in appropriate proportions, an electrolyte with high electrical conductivity can be produced, making it even more preferable to use.

[0145] The metal salt mentioned above may be a lithium salt, and the lithium salt is a substance that dissolves well in the non-aqueous electrolyte; for example, as the anion of the lithium salt, F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3- , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more types selected from the group consisting of can be used.

[0146] In addition to the components of the above electrolyte, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, a haloalkylene carbonate-based compound such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride.

[0147] One embodiment of the present invention provides a battery module including the secondary battery as a unit cell and a battery pack including the same. Since the battery module and the battery pack include the secondary battery having high capacity, high rate capability and cycle capability, they can be used as a power source for a medium-to-large device selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles and power storage systems.

[0148] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, the above embodiments are merely illustrative of the description, and it is obvious to those skilled in the art that various changes and modifications are possible within the scope and spirit of the description, and that such variations and modifications fall within the scope of the appended claims.

[0149] <Preparation Example>

[0150] <Manufacturing of the Cathode>

[0151] A Si slurry was prepared by mixing inorganic Si (Wacker), polyacrylamide (Aldrich), and a conductive material (Super-C, Immerys) in a ratio of 7:2:1 at a concentration of 34 wt% in DI Water.

[0152] This slurry was applied to both sides of an 8 μm thick Cu foil (SK Nexilis) and then rolled to produce a cathode with a total thickness of 53 μm.

[0153] Manufacturing of the anode

[0154] An anode slurry with a solid content of 75.5% was prepared by mixing NCMA cathode material (LG Chem HN803 Grade) and PVdF binder (Arkema KF9709) in an NMP solvent at a ratio of 97.74:2.26.

[0155] The above anode slurry was applied to both sides of a 12 μm thick Al foil (Samya Aluminum Co. A1100 grade) and then rolled to produce an anode with a final thickness of 142 μm.

[0156] A monocell was assembled in the order of anode / separator / cathode / separator with the anode and cathode prepared above and a separator satisfying the physical properties of Table 1 below.

[0157] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Fabric thickness (μm) 14.6 12.1 11.2 11.9 11.5 9.2 Compression resistance (%) 14.5 12.4 10.5 11.0 14.8 15.0 Dielectric breakdown voltage (V) 1526 484 495 452 325 198

[0158] In Table 1 above, the compressibility and dielectric breakdown voltage can be measured as follows.

[0159] - Compression resistance (%)

[0160] The thickness (T1) after stacking three separator membranes of Table 1 above was measured, and the thickness (T2) after pressing at 2000 kgf, 70°C, and 10 seconds in a hot press (Q-MESYS QM-940A Grade) was measured and calculated according to the aforementioned Equation 1.

[0161] - Dielectric breakdown voltage (V)

[0162] The dielectric breakdown voltage in Table 1 above was measured by increasing the voltage from 0V to 6000V at a rate of 100V / s for the monocells of Examples 1 to 4, Comparative Example 1, and Comparative Example 2 containing the separator, using a Chroma Hipot tester (AC / DC / IR Tester), and measuring the voltage at the point where the insulation breaks.

[0163] For the monocells of Examples 1 to 4 and Comparative Examples 1 and 2 manufactured as described above, the presence of a short circuit was observed using an AC resistance meter. Specifically, 20 monocells were manufactured for each example, and it was confirmed whether a short circuit occurred among them. If a short circuit occurred, it was marked as "Fail," and the results were as shown in Table 2 below.

[0164] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Fail / Test 0 / 20 0 / 20 1 / 20 2 / 20 8 / 20 18 / 20

[0165] As can be seen from Tables 1 and 2 above, in the case of the separator for the lithium secondary battery of Examples 1 to 4, it was confirmed through the experiment in Table 2 above that the separator maintains a rigid form even when the rough negative surface, which is due to volume expansion during charging and discharging of the silicon-based negative electrode, comes into contact with the separator, as the separator satisfies all three parameters: a thickness of 1 μm to 15 μm, a compression resistance defined by Equation 1 above of 1% or more and 14.5% or less, and an dielectric breakdown voltage of 400 V or more.

[0166] In the case of Comparative Examples 1 and 2 above, the compressibility was outside the range according to the present application. Since the separator was excessively rigid, it became difficult for lithium ions to pass through, resulting in an increase in diffusion resistance. It was confirmed that the short test was not as good as the example.

[0167] In addition, in the case of Comparative Example 2 above, the dielectric breakdown voltage falls outside the range according to the present application (below the lower limit range), and in the case of Comparative Example 2, the durability of the separator is poor, and the separator is broken or punctured by the cathode with a rough surface, and as a result, it was confirmed that there were the most cases of failure in the short-circuit evaluation. Explanation of the symbols

[0168] 10: Cathode current collector layer 20: Cathode active material layer 30: Separator 40: Positive active material layer 50: Positive current collector layer 100: Negative electrode for lithium secondary battery 200: Cathode for lithium secondary batteries

Claims

Claim 1 A lithium secondary battery comprising: a silicon-based negative electrode; a positive electrode; a separator located between the negative electrode and the positive electrode; and an electrolyte; wherein the silicon-based negative electrode comprises a negative electrode current collector layer; and a negative electrode active material layer comprising a negative electrode active material layer composition provided on one or both sides of the negative electrode current collector layer; and wherein the negative electrode active material layer composition comprises a silicon-based active material; a negative electrode conductive material; A lithium secondary battery comprising one or more selected from the group consisting of a silicon-based active material and a negative electrode binder, wherein the silicon-based active material comprises SiOx (x=0) and comprises 70 parts by weight or more of SiOx (x=0) based on 100 parts by weight of the silicon-based active material, wherein the separator satisfies a thickness of 1 μm or more and 15 μm or less, has a compressibility defined by the following Equation 1 of 1% or more and 14.5% or less, and has a dielectric breakdown voltage of 400 V or more: [Equation 1] (T1-T2) / T1 X 100 In the above Equation 1, T1 refers to the initial thickness of the separator in a state where three sheets are stacked, and T2 refers to the thickness after pressing three sheets of the separator at 2000 kgf, 70°C, and 10 seconds in a hot press (Q-mesys QM-940A Grade), and the dielectric breakdown voltage includes the separator It refers to the voltage at which insulation breaks down while stepping up the monocell from 0V to 6000V at a rate of 100V / s using Chroma’s Hipot tester (AC / DC / IR Tester), and the monocell is assembled by sequentially assembling an anode, a separator, a cathode, and a separator. Claim 2 A lithium secondary battery according to claim 1, wherein the separator is a wet separator or a dry separator. Claim 3 A lithium secondary battery according to claim 1, wherein the separator comprises one or more selected from the group consisting of a porous polymer film; a porous nonwoven fabric; and a ceramic component. Claim 4 A lithium secondary battery according to claim 1, wherein the separator comprises a single layer; or two or more layers. Claim 5 A lithium secondary battery according to claim 1, wherein the pore size of the separator is 10 nm or more and 100 nm or less. Claim 6 A lithium secondary battery according to claim 1, wherein the silicon-based active material comprises 60 parts by weight or more based on 100 parts by weight of the negative electrode active material layer composition. Claim 7 A lithium secondary battery according to claim 1, wherein the negative electrode conductive material comprises one or more selected from the group consisting of a point-type conductive material; a linear conductive material; and a planar conductive material. Claim 8 A lithium secondary battery according to claim 1, wherein the surface roughness (Ra) of the surface of the negative electrode active material layer in contact with the separator is 3 μm or more and 10 μm or less. Claim 9 A lithium secondary battery according to claim 1, wherein the thickness of the negative electrode active material layer is 10 μm or more and 100 μm or less. Claim 10 In claim 1, the anode is LiNi x Co y Mn z O2(x+y+z=1); LiNi a Co b Mn c Al d O2(a+b+c+d=1); LiMn2O4; LiNi 0.5 Mn 1.5 O2; and LiM x Fe y A lithium secondary battery comprising one or more selected from the group consisting of PO4 (M: Transition metal, x+y=1).

Citation Information

Patent Citations

  • Separator, method for preparing the same, and lithium battery comprising the same

    KR1020190105881A

  • high-strength separator

    KR1020200108476A

  • Secondary battery

    KR1020210143980A