Negative electrode active material for potassium secondary battery, method for preparing the same, negative electrode for potassium secondary battery and potassium secondary battery including the same
The use of nitrogen-doped carbon nanofibers with tin selenide nanoparticles in potassium-ion batteries addresses structural integrity issues, enhancing ion diffusion and conductivity to improve cycle characteristics and capacity retention.
Patent Information
- Application Number
- KR1020240163036
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-11-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-11-15
AI Technical Summary
Existing potassium-ion batteries face issues with structural integrity and lower energy density due to the large ionic radius of potassium, leading to reduced cycle characteristics and capacity retention rates.
A negative electrode active material comprising nitrogen-doped carbon nanofibers with tin selenide nanoparticles forms a continuous one-dimensional conductive network, enhancing potassium ion diffusion and storage through alloying/dealloying reactions, while maintaining structural stability.
The proposed material improves cycle characteristics and capacity retention rate by promoting potassium ion mobility and conductivity, resulting in enhanced performance of potassium secondary batteries.
Smart Images

Figure 112024125913089-PAT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a negative electrode active material for a potassium secondary battery, a method for manufacturing the same, a negative electrode for a potassium secondary battery comprising the same, and a potassium secondary battery. Background Technology
[0002] Rechargeable batteries are batteries capable of repeated charging and discharging, and with the advancement of the information and communication and display industries, they are widely applied as power sources for portable electronic communication devices such as camcorders, mobile phones, and laptop PCs. Furthermore, recently, battery packs containing rechargeable batteries are being developed and applied as power sources for eco-friendly vehicles, such as hybrid cars.
[0003] Examples of secondary batteries include sodium-ion batteries, potassium-ion batteries, lithium-ion batteries, nickel-cadmium batteries, and nickel-hydrogen batteries. For instance, lithium-ion secondary batteries capable of achieving high voltage and high energy density can be used as secondary batteries. However, lithium (Li) has limited reserves and is expensive, making it difficult to use in large-scale energy storage systems.
[0004] Sodium-ion batteries can be used as alternative batteries to lithium-ion batteries. However, sodium (Na) has a larger atomic weight than lithium, a higher standard electrode potential than lithium, and a lower cell voltage, which may result in a lower capacity for the secondary battery.
[0005] Potassium (K) is naturally abundant in the Earth's crust and oceans, possesses a low redox potential, and can provide high ion mobility. Therefore, potassium-ion batteries can be used as secondary batteries with high energy density and can be manufactured at a lower cost compared to lithium-ion batteries.
[0006] However, due to the large ionic radius of potassium, the structural integrity of the negative electrode active material in potassium-ion batteries can be weakened during the potassiumization / depotassiumization process, ultimately leading to lower energy density. Accordingly, there is a need for negative electrode active materials for potassium secondary batteries that possess higher non-specific capacity and enhanced stability. The problem to be solved
[0008] One objective of the present invention is to provide a negative electrode active material for a potassium secondary battery having improved cycle characteristics and capacity retention rate, and a method for manufacturing the same.
[0009] One objective of the present invention is to provide a negative electrode for a potassium secondary battery having improved cycle characteristics and capacity retention rate by including the negative electrode active material for a potassium secondary battery, and a potassium secondary battery including the same. means of solving the problem
[0011] One objective of the present invention is to provide a negative electrode active material for a potassium secondary battery and a method for manufacturing the same, which can improve cycle characteristics and capacity retention rate.
[0012] In addition, another objective of the present invention is to provide a negative electrode for a potassium secondary battery and a potassium secondary battery comprising the aforementioned negative electrode active material for a potassium secondary battery. Effects of the invention
[0014] The negative electrode active material for a potassium secondary battery according to the present invention comprises nitrogen (N)-doped carbon nanofibers, and the nitrogen (N)-doped carbon nanofibers can form a continuous one-dimensional conductive network by including tin selenide (SnSe) nanoparticles through electrospinning and heat treatment. Accordingly, the potassium secondary battery comprising the same can have improved cycle characteristics and capacity retention rate. Brief explanation of the drawing
[0016] Figure 1 is a transmission electron microscope image of a negative electrode active material for a potassium secondary battery prepared according to Example 1 of the present invention. FIG. 2 is a table showing the cycle performance of a negative electrode for a potassium secondary battery containing a negative electrode active material for a potassium secondary battery prepared according to Example 1 and Comparative Examples 1 to 3 of the present invention. Specific details for implementing the invention
[0017] The present invention will be described in more detail below.
[0018] Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.
[0020] Negative electrode active material for potassium secondary batteries
[0021] The negative electrode active material for a potassium secondary battery according to the present invention comprises nitrogen (N)-doped carbon nanofibers, wherein the nitrogen (N)-doped carbon nanofibers comprise tin selenide (SnSe) nanoparticles, and the tin selenide (SnSe) nanoparticles are included in an amount of 12% to 27% by weight based on the total weight of the negative electrode active material for a potassium secondary battery.
[0022] In the above nitrogen (N)-doped carbon nanofibers, the doped nitrogen (N) possesses two lone electron pairs favorable for p-π resonance, which can further enhance the electronic environment of the adsorption layer and create vacancies and defect sites, thereby improving the diffusion and storage characteristics of potassium ions.
[0023] The tin selenide (SnSe) nanoparticles can form a continuous one-dimensional conductive network and actively carry out alloying / dealloying reactions to easily capture and release potassium ions, and since they have semiconducting properties themselves, when combined with the carbon nanofibers, the carbon nanofibers provide conductivity, and the tin selenide (SnSe) nanoparticles play a role in assisting the movement of electrons and ions, thereby promoting the diffusion of potassium ions.
[0024] In addition, the tin selenide (SnSe) nanoparticles are included in an amount of 12% to 27% by weight based on the total weight of the negative electrode active material for the potassium secondary battery. If included in an amount less than 12% by weight, the alloying / dealloying reaction is reduced, and the movement path of potassium ions is not easily formed, resulting in a problem of reduced capacity retention rate. If included in an amount greater than 27% by weight, the volume expansion of the tin selenide (SnSe) nanoparticles occurs significantly during the cycling process, resulting in a problem of reduced capacity retention rate at currents of 1000 mA / g or higher.
[0025] For example, the tin selenide (SnSe) nanoparticles may preferably be included in an amount of 13 wt% or more, 13 wt% or more, 13 wt% or more, 14 wt% or more, 15 wt% or more, 16 wt% or more, 17 wt% or more, or 18 wt% or more based on the total weight of the negative electrode active material for the potassium secondary battery, and preferably in an amount of 25 wt% or less, 24 wt% or less, 23 wt% or less, 22 wt% or less, 21 wt% or less, 20 wt% or less, or 19 wt% or less. When the above range is satisfied, the volume expansion of the tin selenide (SnSe) nanoparticles is reduced, and the alloy / dealloying reaction is actively carried out to form a movement path for potassium ions, thereby increasing electrical conductivity and improving the capacity retention rate.
[0026] The above tin selenide (SnSe) nanoparticles may have an average particle size of 10 nm to 40 nm, preferably 15 nm to 30 nm, and more preferably 20 nm to 25 nm. When the above range is satisfied, the tin selenide (SnSe) nanoparticles provide more active sites by providing a larger surface area, and can improve the capacity retention rate by shortening the diffusion path of potassium ions.
[0027] The above negative electrode active material for a potassium secondary battery may have a plane spacing (d201) in the (201) plane measured by TEM of 0.1 nm to 0.5 nm, preferably 0.2 nm to 0.5 nm, and more preferably 0.3 nm to 0.4 nm. Satisfying the above range means that tin selenide (SnSe) nanoparticles are uniformly dispersed within nitrogen (N)-doped carbon nanofibers, thereby suppressing volume expansion caused by repeated charging and discharging of potassium ions.
[0028] The above-mentioned negative electrode active material for the potassium secondary battery has a specific surface area of 13 m² as measured by the BET (Brunauer-Emmett-Teller) method. 2 / g to 56m 2 / g, preferably 13m 2 / g to 40m 2 / g, more preferably 20m 2 / g to 30m 2 It may be / g. If the above range is satisfied, the contact between the electrode and the electrolyte can be improved, and the volume expansion of tin selenide (SnSe) nanoparticles can be accommodated. Specifically, the above specific surface area can be calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using BELSORP-mini II from BEL Japan.
[0029] The above negative electrode active material for a potassium secondary battery may have an average diameter of 100 nm to 300 nm, preferably 150 nm to 250 nm, and more preferably 170 nm to 200 nm. When the above range is satisfied, the movement path of potassium ions, which have a larger radius than lithium ions or sodium ions, is shortened, thereby improving electrical conductivity and thus improving capacity retention rate.
[0030] The above negative electrode active material for a potassium secondary battery may have an average pore diameter of 10 nm to 20 nm, preferably 12 nm to 17 nm, and more preferably 13 nm to 15 nm as measured by the BJH (Barrett-Joyner-Halenda) method. When the above range is satisfied, the diffusion of potassium ions is smooth, and electrical conductivity is improved, so an excellent capacity retention rate can be exhibited.
[0031] The above-mentioned negative electrode active material for the potassium secondary battery is I in the Raman spectrum D / I G The ratio may be 1.0 to 2.0, preferably 1.2 to 1.8, and more preferably 1.4 to 1.6. In the Raman spectrum, 1592 cm⁻¹ -1 The nearby G peak is carbon's sp. 2 E of the bond 2g It originates from the vibration mode, and 1347cm -1 The D peak in the vicinity is the carbon's sp 2 It appears when a defect is present in the bond. I in the Raman spectrum D / I G If the ratio satisfies the above range, it means that there are many defects within the carbon matrix and the degree of graphitization is low, which provides additional defect sites to enhance potassium ion mobility, thereby improving the capacity retention rate.
[0033] Method for manufacturing negative electrode active material for potassium secondary batteries
[0034] The method for manufacturing a negative electrode active material for a potassium secondary battery according to the present invention is,
[0035] The method comprises the steps of: preparing a precursor material by mixing a selenium (Se) raw material and a tin (Sn) raw material (S1); preparing a nitrogen (N)-doped carbon nanofiber (S2); preparing a first intermediate by electrospinning the precursor material onto the nitrogen (N)-doped carbon nanofiber (S3); preparing a second intermediate by heat-treating the first intermediate at a temperature of 200°C to 350°C (S4); and heat-treating the second intermediate at a temperature of 700°C to 900°C (S5).
[0037] Below, each step is explained in detail.
[0039] (1) (S1) Step
[0040] The method for manufacturing a negative electrode active material for a potassium secondary battery according to the present invention comprises the step (S1) of manufacturing a precursor material by mixing a selenium (Se) raw material and a tin (Sn) raw material, and the step (S2) of preparing a nitrogen (N)-doped carbon nanofiber.
[0041] In the above step (S1), the selenium (Se) raw material may include oxides, nitrides, halides, hydroxides, carbonates, nitrates, or combinations thereof containing selenium (Se), and may include, for example, pure Se powder, SeO₂, H₂Se, Cu₂Se, ZnSe, SeS₂, H₂SeO₃, or combinations thereof, but is not limited thereto.
[0042] In addition, the tin (Sn) raw material may include oxides, nitrides, halides, hydroxides, carbonates, nitrates, or combinations thereof containing tin (Sn), and may include, for example, SnCl2, SnCl4, SnO, SnO₂, or combinations thereof, but is not limited thereto.
[0043] The above step (S1) may involve mixing the selenium (Se) raw material and the tin (Sn) raw material in a weight ratio of 4:6 to 6:4. When mixed within this range, a compound in the form of tin selenide (SnSe) may be formed.
[0044] The above step (S1) may be prepared by mixing the selenium (Se) raw material and the tin (Sn) raw material in a solvent such as N,N-dimethylformamide (DMF) and then stirring, but is not limited thereto.
[0045] The above step (S1) may additionally mix an organic material such as polyacrylonitrile (PAN), but is not limited thereto.
[0047] (2) (S2) Step
[0048] Next, the method for manufacturing a negative electrode active material for a potassium secondary battery according to the present invention comprises the step of manufacturing a first intermediate by electrospinning the precursor material onto nitrogen (N)-doped carbon nanofibers.
[0049] The description of the nitrogen (N)-doped carbon nanofibers mentioned above is omitted as it has been described above.
[0050] When the above precursor material is electrospun onto the nitrogen (N)-doped carbon nanofiber, the nanofiber is manufactured in the form of a uniformly mixed tin selenide (SnSe) nanoparticle during the electrospinning process, which can provide uniform electrochemical performance and can be manufactured with a very thin diameter, thereby increasing the contact area with the electrolyte.
[0051] Additionally, between steps (S2) and (S3), a step (S2a) of vacuum drying the first intermediate at a temperature of 70°C to 90°C for 4 to 6 hours may be further included. When the vacuum drying step is performed, the residue of the first intermediate prepared in step (S2) can be removed.
[0053] (3) (S3) Step
[0054] Next, the method for manufacturing a negative electrode active material for a potassium secondary battery according to the present invention includes the step (S3) of heat-treating the first intermediate at a temperature of 200°C to 350°C to produce a second intermediate.
[0055] When the above first intermediate is heat-treated at a temperature of 200°C to 350°C, the structure of the nitrogen (N)-doped carbon nanofiber is stabilized, and tin selenide (SnSe) nanoparticles can be uniformly bonded.
[0056] The above step (S3) can be performed for 0.1 to 1 hour under an active atmosphere. In this case, the organic material introduced in the step of manufacturing the precursor material is oxidized during heat treatment, thereby promoting the carbonization process and ensuring structural stability.
[0058] (5) (S4) Step
[0059] Next, the method for manufacturing a negative electrode active material for a potassium secondary battery according to the present invention includes the step (S4) of heat-treating the second intermediate at a temperature of 700°C to 900°C.
[0060] When the above second intermediate is heat-treated at a temperature of 700°C to 900°C, the chemical bonding between selenium (Se) and tin (Sn) within the tin selenide (SnSe) nanoparticles can be well maintained, and the crystallinity of the negative electrode active material for a potassium secondary battery can be improved.
[0061] The above step (S4) can be performed for 1 to 3 hours under an inert atmosphere. In this case, contact with oxygen is blocked, which prevents the tin selenide (SnSe) nanoparticles from oxidizing at high temperatures and allows for the formation of a fine carbon structure.
[0063] Negative electrode for potassium secondary batteries
[0064] The negative electrode for a potassium secondary battery according to the present invention may include the negative electrode active material for the potassium secondary battery.
[0065] Specifically, a negative electrode for a potassium secondary battery may include a negative current collector and a negative active material layer formed on at least one surface of the negative current collector. According to exemplary embodiments, the negative active material layer may be formed on both sides (e.g., an upper surface and a lower surface) of the negative current collector. The negative active material layer may be coated on the upper surface and the lower surface of the negative current collector, respectively. For example, the negative active material layer may be in direct contact with the surface of the negative current collector.
[0066] The above-mentioned cathode current collector may include, for example, gold, stainless steel, nickel, aluminum, titanium, copper, or an alloy thereof, and preferably may include copper or a copper alloy.
[0067] The above-described negative electrode active material layer may include the negative electrode active material for a potassium secondary battery described above. For example, as a negative electrode active material, it may include a core containing antimony-containing nanoparticles and a metal-organic framework surrounding the core. Accordingly, the electrochemical properties of the negative electrode active material may be improved, and structural stability may be improved as the metal-organic framework can accommodate the volume expansion of the core that occurs during cycling. Therefore, electrical disconnection and detachment between the negative electrode current collector and the negative electrode active material for a potassium secondary battery can be prevented, thereby improving the reversible capacity and capacity retention rate of the potassium secondary battery.
[0068] According to one embodiment, the negative electrode active material for the potassium secondary battery may further include crystalline carbon, amorphous carbon, or a mixture thereof. For example, the crystalline carbon may include amorphous, plate-like, flake, spherical, or fibrous natural graphite or artificial graphite. For example, the amorphous carbon may include soft carbon, hard carbon, mesophase pitch carbide, or calcined coke.
[0070] Potassium secondary battery
[0071] The potassium secondary battery according to the present invention may include a negative electrode and a positive electrode for the potassium secondary battery, and an electrolyte interposed between the negative electrode and the positive electrode for the potassium secondary battery.
[0072] The above positive electrode may include a positive current collector and a positive active material layer formed on at least one surface of the positive current collector. According to exemplary embodiments, the positive active material layer may be formed on both sides (e.g., an upper surface and a lower surface) of the positive current collector. For example, the positive active material layer may be coated on the upper and lower surfaces of the positive current collector, respectively, and may be directly coated on the surface of the positive current collector.
[0073] The above positive current collector may include, for example, nickel, aluminum, copper, stainless steel, titanium, or an alloy thereof. Preferably, the positive current collector may include aluminum or an aluminum alloy.
[0074] The above positive active material layer may include a compound capable of reversibly intercalating and deintercalating potassium ions as a positive active material.
[0075] According to one embodiment, the cathode active material may include a potassium-containing compound. For example, as a potassium-containing compound, potassium iron composite oxide (NaFeO2), potassium cobalt composite oxide (KCoO2), potassium chromium composite oxide (KCrO2), potassium manganese composite oxide (KMnO2), potassium nickel composite oxide (KNiO2), and potassium nickel titanium composite oxide (KNi 1 / 2 Ti 1 / 2 O2), potassium nickel manganese complex oxide (KNi 1 / 2 Mn 1 / 2 O2), potassium iron manganese complex oxide (K 2 / 3 Fe 1 / 3 Mn 2 / 3 O2), potassium nickel cobalt manganese complex oxide (KNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), potassium manganese complex oxide (K 2 / 3 MnO2, KMn2O4), potassium nickel manganese complex oxide (K 2 / 3 Ni 1 / 3 Mn 2 / 3 O2, KNi 1 / 2 Mn 3 / 2 Potassium-containing metal oxides such as O2), potassium iron phosphate compound (KFePO4), potassium manganese phosphate compound (KMnPO4), potassium cobalt phosphate compound (KCoPO4), K2FePO4F, K2MnPO4F, and K2CoPO4F may be included.
[0076] According to one embodiment, as a potassium-containing compound, a polymeric radical compound such as a potassium-containing iron cyano complex (KFFCN) or a potassium-containing iron manganese complex may be included.
[0077] A slurry can be prepared by mixing and stirring the above-mentioned positive active material with a binder, conductive material and / or dispersant, etc., in a solvent. After coating the slurry onto a positive current collector, a positive active material layer can be formed by compressing and drying.
[0078] The above binder may include, for example, organic binders such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyvinylidenefluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, PPC-LiTFSI, or water-based binders such as styrene-butadiene rubber (SBR), and may be used together with a thickener such as carboxymethyl cellulose (CMC). For example, a PPC-LiTFSI series binder may be used as an anode binder.
[0079] The above conductive material may be included to promote electron transfer between active material particles. For example, the conductive material may include carbon-based conductive materials such as graphite, carbon black, Super-P, graphene, carbon nanotubes, etc., and / or metal-based conductive materials such as perovskite materials such as tin, tin oxide, titanium oxide, LaSrCoO3, LaSrMnO3, etc.
[0080] The above solvent may include, for example, N-methylpyrrolidone, acetone, or water.
[0082] A separator may be interposed between the negative electrode and the positive electrode for the potassium secondary battery. The separator may include a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer. The separator may also include a nonwoven fabric formed of high-melting-point glass fibers, polyethylene terephthalate fibers, etc.
[0083] According to one embodiment, an electrode cell is defined by a cathode, an anode, and a separator, and a plurality of electrode cells may be stacked to form, for example, an electrode assembly in the form of a jelly roll. For example, the electrode assembly may be formed through winding, lamination, folding, etc., of the separator.
[0085] A potassium secondary battery can be defined by housing the above electrode assembly together with an electrolyte within a case.
[0086] The electrolyte may include an organic solvent and a potassium salt. The potassium salt may be dissolved in the organic solvent.
[0087] Organic solvents may include, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolan, 4-methyldioxolan, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0088] Electrode tabs may be formed from the positive current collector and the negative current collector belonging to each electrode cell, respectively, and may extend to one side of the case. The electrode tabs may be fused together with the one side of the case to form an electrode lead that extends or is exposed to the outside of the case.
[0089] Potassium secondary batteries can be manufactured in various forms, such as cylindrical, prismatic, pouch, or coin types using cans, for example.
[0091] Hereinafter, preferred embodiments are presented to aid in understanding the present invention; however, these embodiments are merely illustrative of the invention and are not intended to limit the appended claims. It is obvious to those skilled in the art that various changes and modifications to the embodiments are possible within the scope and spirit of the invention, and that such variations and modifications fall within the scope of the appended claims.
[0093] <Examples and Comparative Examples>
[0094] Example 1: Preparation of negative electrode active material for potassium secondary batteries
[0095] 0.276 g of selenium (Se) powder was dispersed in 10 mL of N,N-dimethylformamide (DMF), stirred for 30 minutes, and then sonicated for 1 hour to obtain a uniform black suspension. Subsequently, 0.821 g of polyacrylonitrile (PAN, Mw=150,000) was mixed into the suspension, and 0.221 g of tin chloride (SnCl2) was added and stirred at 60°C for 12 hours to obtain a precursor material.
[0096] After loading the above precursor material into a plastic syringe, the first intermediate was prepared by electrospinning it onto nitrogen (N)-doped carbon nanofibers while maintaining a distance of 15 cm between the needle and the rotary drum collector. The device used was the NanoNC ESR200R2D, and the electrospinning was performed at room temperature and humidity of 30% or less at a voltage of 5 kV and a flow rate of 0.8 mL.
[0097] Subsequently, the collected spun fibers were vacuum dried at 80°C for 5 hours and subjected to a first heat treatment at 280°C for 30 minutes under an atmospheric atmosphere to obtain a second intermediate, and the intermediate was subjected to a second heat treatment at 800°C for 2 hours under an argon atmosphere to obtain nitrogen (N)-doped carbon nanofibers containing tin selenide (SnSe) nanoparticles.
[0099] Comparative Example 1: Preparation of negative electrode active material for potassium secondary batteries
[0100] Nitrogen (N)-doped carbon nanofibers were used as the negative electrode active material for a potassium secondary battery without adding separate selenium (Se) powder and tin chloride (SnCl2).
[0102] Comparative Example 2: Preparation of negative electrode active material for potassium secondary batteries
[0103] Nitrogen (N)-doped carbon nanofibers containing tin selenide (SnSe) nanoparticles were prepared in the same manner as in Example 1, except that 0.197 g of selenium (Se) powder and 0.158 g of tin chloride (SnCl2) were added.
[0105] Comparative Example 3: Preparation of negative electrode active material for potassium secondary batteries
[0106] Nitrogen (N)-doped carbon nanofibers containing tin selenide (SnSe) nanoparticles were prepared in the same manner as in Example 1, except that 0.355 g of selenium (Se) powder and 0.284 g of tin chloride (SnCl2) were added.
[0108] Table 1 below shows the weight% of tin selenide (SnSe) nanoparticles in the negative electrode active material for potassium secondary batteries according to Example 1 and Comparative Examples 1 to 3.
[0110]
[0112] Experimental Example: Evaluation of Cycle Characteristics
[0113] (1) Manufacturing of cathode and battery
[0114] Carbon nanofibers, which are negative electrodes for potassium secondary batteries, were prepared according to the methods of Example 1 and Comparative Examples 1 to 3 above.
[0115] Subsequently, a half-cell was fabricated using potassium metal (Sigma-Aldrich) as the counter electrode. A glass fiber microfilter (Whatman, GF / C) was immersed in EC / DMC (1:1 vol%) solvent of 1M KFSI as a separator and inserted between the negative electrode and the counter electrode.
[0117] (2) Evaluation of capacity retention rate
[0118] For the battery manufactured above, charging and discharging were performed at a current of 500 mA / g and a potential range of 0.01 V to 3.0 V. After measuring the initial reversible capacity with charging and discharging as one cycle, the reversible capacity was measured after 1000 cycles.
[0119] Afterwards, the dose retention rate (%) was evaluated as the percentage of the value obtained by dividing the reversible dose by the initial reversible dose after 100 cycles.
[0120] The evaluation results are shown in Table 2 below.
[0122]
[0124] Referring to Table 2 above, it can be seen that the battery according to Example 1 has a higher reversible capacity after 1,000 cycles and a higher capacity retention rate compared to the batteries according to Comparative Examples 1 to 3.
Claims
Claim 1 A negative electrode active material for a potassium secondary battery comprising nitrogen (N)-doped carbon nanofibers; wherein the nitrogen (N)-doped carbon nanofibers comprise tin selenide (SnSe) nanoparticles, and the tin selenide (SnSe) nanoparticles are included in an amount of 12% to 27% by weight based on the total weight of the negative electrode active material for a potassium secondary battery, and wherein the negative electrode active material for a potassium secondary battery has a plane spacing (d201) in the (201) plane measured by TEM of 0.1nm to 0.5nm. Claim 2 Claim 1, wherein the tin selenide (SnSe) nanoparticles are a negative electrode active material for a potassium secondary battery having an average particle size of 10 nm to 40 nm. Claim 3 delete Claim 4 In claim 1, the negative electrode active material for the potassium secondary battery has a specific surface area of 13 m² as measured by the BET method. 2 / g to 56m 2 Negative active material for a potassium secondary battery with a phosphorus content of / g. Claim 5 In claim 1, the negative electrode active material for a potassium secondary battery is a negative electrode active material for a potassium secondary battery having an average diameter of 100 nm to 300 nm. Claim 6 In claim 1, the negative electrode active material for a potassium secondary battery is a negative electrode active material for a potassium secondary battery having an average pore diameter of 10 nm to 20 nm measured by the BJH method. Claim 7 In claim 1, the negative electrode active material for the potassium secondary battery is I in the Raman spectrum D / I G Negative active material for a potassium secondary battery having a ratio of 1.0 to 2.
0. Claim 8 A method for manufacturing a negative electrode active material for a potassium secondary battery, comprising: a step (S1) of manufacturing a precursor material by mixing a selenium (Se) raw material and a tin (Sn) raw material; a step (S2) of manufacturing a first intermediate by electrospinning the precursor material onto nitrogen (N)-doped carbon nanofibers; a step (S3) of manufacturing a second intermediate by heat treating the first intermediate at a temperature of 200°C to 350°C; and a step (S4) of heat treating the second intermediate at a temperature of 700°C to 900°C; wherein the negative electrode active material for a potassium secondary battery manufactured by the method is characterized in that the interplanar spacing (d201) in the (201) plane measured by TEM is 0.1 nm to 0.5 nm. Claim 9 A method for manufacturing a negative electrode active material for a potassium secondary battery according to claim 8, wherein step (S1) involves mixing the selenium (Se) raw material and the tin (Sn) raw material in a weight ratio of 4:6 to 6:
4. Claim 10 A method for manufacturing a negative electrode active material for a potassium secondary battery according to claim 8, further comprising the step (S2a) of vacuum drying the first intermediate at a temperature of 70°C to 90°C for 4 to 6 hours between the steps (S2) and (S3). Claim 11 A method for manufacturing a negative electrode active material for a potassium secondary battery according to claim 8, wherein step (S3) is performed for 0.1 to 1 hour under an active atmosphere. Claim 12 A method for manufacturing a negative electrode active material for a potassium secondary battery according to claim 8, wherein step (S4) is performed for 1 to 3 hours under an inert atmosphere. Claim 13 A negative electrode for a potassium secondary battery comprising a negative electrode active material for a potassium secondary battery according to any one of claims 1, 2 and 4 to 7. Claim 14 A potassium secondary battery comprising a negative electrode for a potassium secondary battery according to claim 13.
Citation Information
Patent Citations
High-surface-capacity potassium ion battery negative electrode material and preparation method thereof