Bale-molded article, block copolymer, resin composition, and method for producing block copolymer
A block copolymer with tailored aromatic vinyl monomer units and molecular weight distribution addresses the high hardness issue in styrene-based resin compositions, providing a bale molded body with enhanced handling and impact resistance.
Patent Information
- Application Number
- KR1020240038205
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-02-29
- Filing Date
- 2024-03-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-03-20
AI Technical Summary
Existing styrene-based resin compositions used in bale molded bodies suffer from high hardness, leading to issues such as slipping during transport and the need for spacing during crushing, despite the addition of low-viscosity aromatic vinyl-conjugated diene block copolymers to enhance impact resistance.
A block copolymer with specific compositions of aromatic vinyl monomer units, block aromatic vinyl portion, peak top molecular weight, and molecular weight distribution is used, along with a styrene-based resin, to achieve a bale molded body with appropriate hardness and improved handling properties.
The solution results in a bale molded body with controlled hardness, enabling easy handling, crushing, and improved impact resistance, while maintaining gloss and solubility in styrene-based resins.
Smart Images

Figure 112024031049490-PAT00001 
Figure 112024031049490-PAT00003 
Figure 112026032657588-PAT00005
Abstract
Description
Technology Field
[0001] The present invention relates to a bale molded body, a block copolymer, a resin composition, and a method for manufacturing a block copolymer. Background Technology
[0002] Styrene-based resins have excellent rigidity, transparency, gloss, and moldability, so they have been widely used for various applications for a long time. However, because their impact resistance is poor, rubbery polymers are added to styrene-based resins as modifiers.
[0003] Methods for adding a rubbery polymer to a styrene-based resin include, for example, mechanically blending the rubbery polymer into a polystyrene-based resin, bulk polymerizing a styrene solution of the rubbery polymer, or bulk suspension polymerization.
[0004] In particular, the method of adding a rubbery polymer to a styrene-based resin by various polymerization methods as described above is widely practiced industrially as an impact-resistant styrene-based resin composition because the physical properties of the resulting resin composition are excellent, and it is used as a material for household electrical products.
[0005] In addition, regarding the resin modification of acrylonitrile-styrene-based resin (ABS), a technique is known in which a 5 mass% styrene solution of a low-viscosity aromatic vinyl-conjugated diene block copolymer is used to quench the particles of the rubbery polymer used as a modifier.
[0006] For example, the following patent documents 1 and 2 disclose a technique for producing a styrene-based resin with good impact resistance by defining the peak top molecular weight of the block styrene portion in an aromatic vinyl-conjugated diene block copolymer, which is a modifier, to a predetermined value.
[0007] In addition, the following patent document 3 discloses a method for manufacturing a conjugated diene polymer with reduced Li content, and furthermore, a technique is disclosed in which the viscosity of a 5 mass% styrene solution of the conjugated diene polymer is set to 11 to 35 mPa·s and used for resin modification such as HIPS resin or ABS resin. Prior art literature
[0008] Japanese Patent No. 4029470, Japanese Patent No. 4029471, Japanese Patent No. 6646437 The problem to be solved
[0009] The aromatic vinyl-conjugated diene block copolymer as a modifier as described above provides good veil-forming properties by preparing the viscosity of the styrene solution to be low.
[0010] However, even with such low-viscosity aromatic vinyl-conjugated diene block copolymers, there are cases where the hardness of the molded bale is high. In such cases, when moving the bale by gripping it with the hook of a transport robot, there is a problem in that the hook does not penetrate sufficiently, causing the bale to slip out and fall. Additionally, if the bale is hard, a load is applied during crushing, so there is a problem in that it is necessary to have a feeding interval for the bale.
[0011] The hardness of the above bale molded body is influenced by the structure of the aromatic vinyl-conjugated diene block copolymer. Although Patent Document 2 describes bale moldability, Patent Documents 1 to 3 do not describe the hardness of the bale molded body or the crushability of the bale molded body at all.
[0012] In addition, "bale molded body" refers to a rectangular block unit weighing 25 to 35 kg made by press-molding synthetic rubber.
[0013] Therefore, the present invention aims to provide a bale molded body comprising a block copolymer having appropriate hardness, being easy to grind, and having excellent handling properties, and a resin composition comprising a block copolymer constituting the bale molded body and a polymer of the block copolymer and a styrene-based resin. means of solving the problem
[0014] As a result of careful consideration to solve the problems of the prior art described above, the inventors discovered that the problems of the prior art described above can be solved by specifying the content of aromatic vinyl monomer units, the ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units, the peak top molecular weight of the block aromatic vinyl portion, and the molecular weight distribution of the block aromatic vinyl portion, and thus completed the present invention.
[0015] That is, the present invention is as follows.
[0016] [1]
[0017] It is a veil-molded body of a block copolymer having aromatic vinyl monomer units and conjugated diene monomer units, and
[0018] The above block copolymer has a block aromatic vinyl portion, and
[0019] A veil-molded body satisfying the following <condition (a)> to <condition (d)>.
[0020] <condition (a)>
[0021] The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass%.
[0022] <Condition (b)>
[0023] The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass%.
[0024] <condition (c)>
[0025] The peak top molecular weight of the blocked aromatic vinyl portion is 10,000 to 30,000.
[0026] <condition (d)>
[0027] The ratio of the weight-average molecular weight Mw of the block aromatic vinyl portion to the number-average molecular weight Mn (Mw / Mn) is 1.15 to 1.40.
[0028] [2]
[0029] A veil molded body described in [1], wherein the viscosity of a styrene solution of 5 mass% of the block copolymer is 7 to 15 mPa·s under a temperature condition of 25°C.
[0030] [3]
[0031] A veil molded body described in [1] or [2], wherein the 1,2-vinyl bonding amount of the conjugated diene monomer unit of the block copolymer is 15 to 30 mol%.
[0032] [4]
[0033] A bale molded body described in any one of [1] to [3], having a hardness of 50 to 72 as measured by a hardness tester type E in accordance with JIS K6253.
[0034] [5]
[0035] It is a block copolymer having aromatic vinyl monomer units and conjugated diene monomer units, and
[0036] The above block copolymer has a block aromatic vinyl portion, and
[0037] A block copolymer satisfying the following <condition (a)> to <condition (d)>.
[0038] <condition (a)>
[0039] The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass%.
[0040] <Condition (b)>
[0041] The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass%.
[0042] <condition (c)>
[0043] The peak top molecular weight of the blocked aromatic vinyl portion is 10,000 to 30,000.
[0044] <condition (d)>
[0045] The ratio of the weight-average molecular weight Mw of the block aromatic vinyl portion to the number-average molecular weight Mn (Mw / Mn) is 1.15 to 1.40.
[0046] [6]
[0047] The block copolymer described in [5], wherein the viscosity of a styrene solution of 5 mass% of the block copolymer is 7 to 15 mPa·s under a temperature condition of 25°C.
[0048] [7]
[0049] A block copolymer described in [5] or [6], wherein the 1,2-vinyl bond content of the conjugated diene monomer unit of the block copolymer is 15 to 30 mol%.
[0050] [8]
[0051] 3 to 20 parts by mass of a block copolymer constituting a veil molded body as described in any one of [1] to [4] above, and
[0052] 97 to 80 parts by mass of styrene-based resin
[0053] A resin composition that is a polymer of
[0054] [9]
[0055] The resin composition described in [8] above, wherein the above styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile.
[0056]
[10]
[0057] A method for manufacturing a block copolymer constituting a veil molded body as described in any one of [1] to [4] above, and
[0058] A process of supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound such that the peak temperature is 91 to 100°C, and
[0059] A process having to polymerize an aromatic vinyl compound by supplying it to the reactor at a temperature of 90 to 100°C.
[0060] Method for manufacturing block copolymers.
[0061]
[11]
[0062] 3 to 20 parts by mass of the block copolymer described in any one of [5] to [7] above, and
[0063] 97 to 80 parts by mass of styrene-based resin
[0064] A resin composition that is a polymer of
[0065]
[12]
[0066] The resin composition described in
[11] above, wherein the above styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile.
[0067]
[13]
[0068] A method for manufacturing a block copolymer as described in any one of [5] to [7] above, and
[0069] A process of supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound such that the peak temperature is 91 to 100°C, and
[0070] A process having to polymerize an aromatic vinyl compound by supplying it to the reactor at a temperature of 90 to 100°C.
[0071] Method for manufacturing block copolymers. Effects of the invention
[0072] According to the present invention, a bale molded body comprising an aromatic vinyl-conjugated diene block copolymer having a suitable hardness, being easy to grind, and having excellent handling properties, and a resin composition comprising a block copolymer constituting the bale molded body and a polymer of the block copolymer and a styrene-based resin having excellent gloss and impact resistance can be provided. Specific details for implementing the invention
[0073] Hereinafter, an embodiment for carrying out the present invention (hereinafter referred to as "the present embodiment") will be described in detail.
[0074] Furthermore, the following embodiments are examples for explaining the present invention, and the present invention is not limited to the forms shown below. The present invention may be implemented with various modifications within the scope of its gist.
[0075] [Veil molded body and block copolymer]
[0076] The bale molded body of the present embodiment is a block copolymer bale molded body of the present embodiment having a conjugated diene monomer unit and an aromatic vinyl monomer unit.
[0077] Additionally, in this specification, a monomer that has become a component of a block copolymer is referred to as a “monomer unit,” and a monomer prior to being introduced into a polymer is referred to as a “compound.”
[0078] The block copolymer of the present embodiment constituting the veil molded body of the present embodiment has a block aromatic vinyl portion and also satisfies the following <condition (a)> to <condition (d)>.
[0079] <condition (a)>
[0080] The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass%.
[0081] <Condition (b)>
[0082] The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass%.
[0083] <condition (c)>
[0084] The peak top molecular weight of the blocked aromatic vinyl portion is 10,000 to 30,000.
[0085] <condition (d)>
[0086] The ratio of the weight-average molecular weight Mw of the block aromatic vinyl portion to the number-average molecular weight Mn (Mw / Mn) is 1.15 to 1.40.
[0087] By having the above composition of the bale molded body and block copolymer of the present embodiment, a bale molded body having appropriate hardness, easy to crush, and excellent handling properties is obtained.
[0088] In this specification, monomers used in the manufacture of polymers are referred to as "compounds," and polymer components are referred to as "monomer units."
[0089] Conjugated diene compounds forming conjugated diene monomer units in a block copolymer are not limited to the following, but examples include 1,3-butadiene, 2-methyl-1,3-butadiene (i.e., isoprene), 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, etc. Among these, 1,3-butadiene or 2-methyl-1,3-butadiene is preferred, and 1,3-butadiene is particularly preferred. Each of these conjugated diene compounds may be used individually or in combination of two or more types.
[0090] As aromatic vinyl compounds forming aromatic vinyl monomer units in a block copolymer, examples include, but are not limited to, styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, monochlorostyrene, dichlorostyrene, monofluorostyrene, etc. Among these, styrene is preferred. Each of these aromatic vinyl compounds may be used individually or in combination of two or more types.
[0091] (<Condition (a)> Content of aromatic vinyl monomer units in the block copolymer)
[0092] The block copolymer constituting the veil molded body of the present embodiment, and the content of aromatic vinyl monomer units in the block copolymer of the present embodiment are 10 to 30 mass%, preferably 14 to 26 mass%, and more preferably 17 to 23 mass%.
[0093] In addition, the content of conjugated diene monomer units in the block copolymer is 70 to 90 mass%, preferably 74 to 86 mass%, and more preferably 77 to 83 mass%.
[0094] If the content of aromatic vinyl monomer units in the block copolymer is 10 mass% or more, the required hardness of the bale molded body is ensured, and it tends to be difficult to deform under load. In addition, when used as a toughening agent for aromatic vinyl resins, an improvement in hardness is obtained. If the content of aromatic vinyl monomer units is 30 mass% or less, the hardness of the bale molded body does not become too high, good crushability and solubility of the bale molded body are obtained, and impact resistance can be secured when used as a toughening agent for aromatic vinyl resins.
[0095] In addition, in this specification, "hardness of bale molded article" refers to the hardness of a bale molded article formed without adding oil to a block copolymer. In this embodiment, by controlling the hardness of the bale molded article in a so-called non-genetic state through the structure of the block copolymer, the handling properties of the bale molded article are improved, and the case of unintended oil inclusion in the application in which the bale molded article is used is eliminated, and effects such as improved design freedom of the resin composition are also obtained.
[0096] The content of aromatic vinyl monomer units in the block copolymer can be controlled to the above-mentioned numerical range by adjusting the amount of aromatic vinyl compound added and the polymerization time during the polymerization process.
[0097] (<Condition (b)> Ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units in the block copolymer)
[0098] The ratio of the block aromatic vinyl portion to the total content of the aromatic vinyl monomer units in the block copolymer constituting the veil molded body of the present embodiment is 90 to 100 mass%, preferably 93 to 100 mass%, and more preferably 95 to 99.9 mass%.
[0099] Here, "block aromatic vinyl portion" refers to a block portion in which 10 or more aromatic vinyl monomer units are linked together.
[0100] Since the ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units in the block copolymer is 90 mass% or more, the solubility in styrene, styrene / acrylonitrile, styrene / methacrylic acid ester, etc., after crushing the bale molded body tends to be good, and when used as a toughening agent for aromatic vinyl resins, the impact resistance also tends to be improved.
[0101] The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units in the block copolymer can be controlled to the above numerical range by adjusting the timing of the addition of the aromatic vinyl compound during the polymerization process.
[0102] (<Condition (c)> Peak top molecular weight of the blocked aromatic vinyl portion)
[0103] The block copolymer constituting the veil molded body of the present embodiment and the block copolymer of the present embodiment has a peak top molecular weight of 10,000 to 30,000 for the block aromatic vinyl portion constituting the block copolymer.
[0104] Specifically, the block copolymer is ozone-decomposed, and the peak top molecular weight in the molecular weight distribution curve of the block aromatic vinyl portion is a value equivalent to standard monodisperse polystyrene measured by gel permeation chromatography (hereinafter also referred to as "GPC"), ranging from 10,000 to 30,000, preferably from 11,000 to 27,000, and more preferably from 12,000 to 25,000.
[0105] Since the peak top molecular weight of the block aromatic vinyl part is 10,000 or more, the bale molded body of the present embodiment has the required hardness, and when the bale molded body is stacked, deformation of the bale molded body due to load tends to occur. Since the peak top molecular weight of the molecular weight distribution curve of the block aromatic vinyl part is 30,000 or less, the hardness of the bale molded body of the present embodiment does not become too high, handling properties are good, and an increase in load during crushing tends to be prevented. In addition, if the peak top molecular weight of the block aromatic vinyl part is in the range of 10,000 to 30,000, when used as a toughening agent for aromatic vinyl resins, the balance of impact resistance and gloss tends to be good.
[0106] The peak top molecular weight of the aromatic vinyl part can be controlled to the above numerical range by adjusting the amount of polymerization initiator added and the amount of aromatic vinyl compound added in the polymerization process.
[0107] (<Condition (d)> Ratio of the weight-average molecular weight Mw and the number-average molecular weight Mn of the blocked aromatic vinyl portion)
[0108] The ratio of the weight-average molecular weight to the number-average molecular weight (Mw / Mn) of the block copolymer constituting the veil molded body of the present embodiment (hereinafter referred to as the molecular weight distribution) is 1.15 to 1.40.
[0109] Specifically, when the block copolymer is ozone decomposed and the molecular weight of the block aromatic vinyl portion is measured, the molecular weight distribution (Mw / Mn) is in the range of 1.15 to 1.40. In terms of adjusting the hardness of the veil molded body of the present embodiment, it is preferably in the range of 1.15 to 1.35, more preferably in the range of 1.15 to 1.30, even more preferably in the range of 1.15 to 1.25, even more preferably in the range of 1.18 to 1.35, even more preferably in the range of 1.18 to 1.30, and particularly preferably in the range of 1.20 to 1.30.
[0110] By setting the molecular weight distribution of the block aromatic vinyl portion to the above range, the hardness of the bale molded body can be controlled to a value that is practically good. Here, the hardness of the bale molded body refers to the hardness measured by a durometer type E in accordance with JIS K 6253, and specifically, it can be measured by the method described in the examples to be described later.
[0111] If the molecular weight distribution (Mw / Mn) of the block aromatic vinyl part is 1.15 or higher, it is easy to adjust the hardness of the bale molded body to 72 or lower, and when the bale molded body is moved by hooking it with a robot or the like, the hook tends to dig in and prevent the bale molded body from falling. If the molecular weight distribution (Mw / Mn) of the block aromatic vinyl part is 1.40 or lower, the hardness of the bale molded body tends to be 50 or higher, and when the bale molded body is stacked, it tends to prevent deformation of the bale molded body due to load.
[0112] The molecular weight distribution of the block aromatic vinyl part can be controlled to the above numerical range by adjusting the temperature inside the reactor when the aromatic vinyl compound is added during the polymerization process.
[0113] The hardness of the block copolymer bale molded body of the above-described embodiment, that is, the hardness measured by a durometer type E in accordance with JIS K 6253, is preferably in the range of 50 to 72, more preferably 53 to 70, and even more preferably 55 to 68. Since the hardness of the bale molded body is 50 or higher, it tends to prevent the lower bale molded body from being deformed by the load when multiple bale molded bodies are stacked. Since the hardness of the bale molded body is 72 or lower, handling of the bale molded body by a robot arm can be ensured, and also, the load does not increase during the crushing of the bale molded body, and the bale molded body can be continuously fed into the crusher without spacing, so good crushing efficiency can be ensured.
[0114] The hardness of the veil-molded body of the block copolymer can be controlled to the above numerical range by adjusting the molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion constituting the block copolymer. Specifically, by adjusting the molecular weight distribution (Mw / Mn) to 1.15 or higher, the hardness of the veil-molded body can be controlled to 72 or lower, and by adjusting the molecular weight distribution (Mw / Mn) to 1.40 or lower, the hardness of the veil-molded body can be controlled to 50 or higher.
[0115] The molecular weight distribution of the block aromatic vinyl part can be controlled to the above numerical range by adjusting the temperature inside the reactor when the aromatic vinyl compound is added during the polymerization process.
[0116] In the block copolymer constituting the bale molded body of the present embodiment, and in the block copolymer of the present embodiment, it is preferable that a block aromatic vinyl portion be disposed at the end of the block copolymer. By doing so, when used to dissolve styrene, styrene / acrylonitrile, styrene / methacrylic acid ester, etc. after crushing the bale molded body, the solubility in these substances tends to be good.
[0117] In addition, regarding the block copolymer constituting the veil molded body of the present embodiment and the block copolymer of the present embodiment, it is preferable that the viscosity of the styrene solution of 5 mass% of the block copolymer is 7 to 15 mPa·s under a temperature condition of 25°C, more preferably 8 to 13 mPa·s, and even more preferably 9 to 12 mPa·s.
[0118] Since the viscosity of the styrene solution of 5 mass% of the block copolymer is 7 mPa·s or higher, it tends to improve impact resistance when used as a toughening agent for aromatic vinyl resins.
[0119] In addition, since the viscosity of the styrene solution of 5 mass% of the block copolymer is 15 mPa·s or less, when used as a toughening agent for aromatic vinyl resins, it is easy to sufficiently quench-harden the rubber particles of the aromatic vinyl resin and tends to be easy to achieve a good balance of impact resistance, gloss, and stiffness.
[0120] The viscosity of a styrene solution of 5 mass% of a block copolymer can be controlled to the above numerical range by adjusting the peak top molecular weight of the block copolymer.
[0121] The block copolymer constituting the bale molded body of the present embodiment and the block copolymer of the present embodiment preferably have a 1,2-vinyl bonding amount of conjugated diene monomer units of 15 to 30 mol%, more preferably 16 to 28%, and even more preferably 17 to 25%. By having a 1,2-vinyl bonding amount of 30 mol% or less, when the bale molded body of the present embodiment and the block copolymer of the present embodiment are used as toughening agents for impact-resistant aromatic vinyl resins, it is easy to control the graft amount within an appropriate range and the particle size is also easy to control so that the shape of the rubber particles in the impact-resistant aromatic vinyl resin becomes salami particles. In addition, if the 1,2-vinyl bonding amount is 15 mol% or more, when the bale molded body of the present embodiment and the block copolymer of the present embodiment are used as toughening agents for impact-resistant aromatic vinyl resins, the rubber particles in the acrylonitrile-styrene resin (ABS) tend to become finer, and the impact resistance of the resin composition, which is a polymer of the impact-resistant aromatic vinyl resin and the block copolymer of the present embodiment, tends to be improved.
[0122] The 1,2-vinyl bond content of the block copolymer can be controlled to the above numerical range by adjusting the amount of polar material added and the polymerization reaction temperature in the polymerization process.
[0123] The block copolymer constituting the veil molded body of the present embodiment, and the block copolymer of the present embodiment, have an aromatic vinyl monomer unit content of 10 to 30 mass% in the block copolymer, a block aromatic vinyl portion ratio to the total content of aromatic vinyl monomer units of 90 to 100 mass%, a peak top molecular weight of the block aromatic vinyl portion of 10,000 to 30,000, and a molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion of 1.15 to 1.40.
[0124] A block copolymer having this structure is obtained by a method in which, in addition to adjusting the amount of catalyst added, a conjugated diene compound is supplied to a reactor and polymerized so that the peak temperature is 91 to 100°C, and then an aromatic vinyl compound is supplied and polymerized at a temperature of 90 to 100°C inside the reactor.
[0125] Preferably, an aromatic vinyl compound is supplied at a temperature of 91 to 99°C in the reactor, and more preferably, an aromatic vinyl compound is supplied at a temperature of 92 to 98°C in the reactor to polymerize it.
[0126] When the temperature inside the reactor is below 90°C, the molecular weight distribution (Mw / Mn) of the blocked aromatic vinyl portion tends to be lower than 1.15. When the temperature inside the reactor exceeds 100°C, the molecular weight distribution of the blocked aromatic vinyl portion widens, and there is a tendency for the molecular weight distribution (Mw / Mn) to fluctuate, even if it becomes diacid.
[0127] (Method for manufacturing block copolymers)
[0128] The block copolymer constituting the veil molded body of the present embodiment has an aromatic vinyl monomer unit and a conjugated diene monomer unit, and further has a block aromatic vinyl portion.
[0129] The above block copolymer can be prepared, for example, by polymerizing in a hydrocarbon solvent using an organic lithium compound as a polymerization initiator.
[0130] Examples of organic lithium compounds include, but are not particularly limited, compounds in which one or more lithium atoms are bonded in the molecule. Examples include, but are not limited to, ethyl lithium, n-propyl lithium, isopropyl lithium, n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexamethylene lithium, butadienyl dilithium, isoprenyl dilithium, etc. These may be used individually or in combination of two or more types.
[0131] Hydrocarbon solvents used in the manufacture of block copolymers may include, but are not limited to the following, aliphatic hydrocarbons such as butane, pentane, hexane, isopentane, heptane, octane, and isooctane; alicyclic hydrocarbons such as cyclopentane, methylcyclopentane, cyclohexane, methylcyclohexane, and ethylcyclohexane; or aromatic hydrocarbons such as benzene, toluene, ethylbenzene, and xylene.
[0132] These may be used as a single type or in combination with two or more types.
[0133] As a method for adjusting the 1,2-vinyl bonding amount of conjugated diene monomer units of a block copolymer, for example, a method of adding polar substances such as dimethyl ether, diethyl ether, diphenyl ether, tetrahydrofuran, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, trimethylamine, triethylamine, tetramethylethylenediamine, triphenylphosphine, and hexamethylphosphoramide to a polymerization system containing an organolithium compound as a polymerization initiator.
[0134] These may be used as a single type or in combination with two or more types.
[0135] Specifically, in a polymerization system containing an organic lithium compound and a polar material, it is preferable to supply a conjugated diene compound to a reactor and polymerize the conjugated diene compound until the peak temperature reaches 91 to 100°C, and then supply an aromatic vinyl compound at a temperature of 90 to 100°C inside the reactor to polymerize it.
[0136] In addition, although the polymerization time is prolonged, by applying a method of extending the addition time of the aromatic vinyl compound or a method of adding the aromatic vinyl compound in segments, the molecular weight distribution (Mw / Mn) of the block aromatic vinyl portion can be controlled to a range of 1.15 to 1.40.
[0137] More preferably, a method is used to obtain a block copolymer by supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound until the peak temperature reaches 91 to 100°C, and then supplying an aromatic vinyl compound at a temperature of 90 to 100°C inside the reactor and polymerizing it. This method is efficient as it has the best polymerization rate.
[0138] In addition, it is desirable to use an inert gas atmosphere, such as nitrogen gas, for the atmosphere of the polymerization system.
[0139] The polymerization pressure should be within a range sufficient to maintain the monomer and solvent in a liquid state within the polymerization temperature range, and is not particularly limited.
[0140] (Additives)
[0141] In the block copolymer of the above-described embodiment, after stopping the solution of the block copolymer with water, alcohol, organic acid, etc., various stabilizers such as phenolic stabilizers, phosphorus stabilizers, sulfur stabilizers, amine stabilizers, or other known additives may be added.
[0142] In addition, the block copolymer of the present embodiment can be separated from the solution by removing catalyst residue as necessary, for example, as described in Japanese Patent No. 6646437. Separation from the solvent can be performed by introducing the block copolymer solution into a hot water bath under stirring and removing the solvent by steam stripping. After a desolvation process such as steam stripping, the block copolymer in the form of a clam obtained by extrusion molding with an extruder and then hot air drying or vacuum drying can be formed into a bale molded body by molding with a bale molding machine.
[0143] The bale-molded body of the present embodiment manufactured as described above can be adjusted to a hardness with excellent handling properties, has excellent handling and grindability by a robot, and enables the quenching and hardening of rubber particles within an aromatic vinyl resin such as ABS, thereby obtaining a resin composition with excellent gloss and impact resistance. That is, the block copolymer of the present embodiment can be used as a resin modifier (toughening agent) capable of improving gloss and impact resistance.
[0144] [Resin Composition]
[0145] The resin composition of the present embodiment is a polymer of 3 to 20 parts by mass of the block copolymer or the block copolymer of the present embodiment constituting the bale molded body of the present embodiment described above, and 97 to 80 parts by mass of a styrene-based resin.
[0146] As a styrene-based resin, a styrene-based compound used in the manufacture of a resin composition may be used. In addition, the styrene-based compound may include any of the states of a polymer, a monomer, and an oligomer.
[0147] As styrene-based compounds, at least one type among styrene and its derivatives, such as styrene, α-methylstyrene, vinyltoluene, and chlorostyrene, may be cited, although not limited to the following. Among these, styrene is preferred.
[0148] These styrene-based compounds can each be used individually or in combination of two or more types.
[0149] The above styrene-based compound may be a homopolymer of the above compound, or a copolymer of styrene and other copolymerizable compounds.
[0150] Examples of compounds copolymerizable with styrene-based compounds include vinyl monomers such as unsaturated nitrile compounds like acrylonitrile and methacrylonitrile, acrylic acid esters such as methyl acrylate, and methacrylic acid esters such as methyl methacrylate, and acrylonitrile is particularly preferred.
[0151] In the resin composition of the present embodiment, the block copolymer content of the present embodiment is preferably 5 to 18 parts by mass, and more preferably 8 to 15 parts by mass.
[0152] In addition, the content of the styrene-based resin is preferably 95 to 82 parts by mass, and more preferably 92 to 85 parts by mass.
[0153] The resin composition of the present embodiment can be prepared by polymerizing a styrene-based resin and a block copolymer, or by mixing a monomer of the styrene-based resin and a block copolymer and polymerizing them. Specifically, it can be prepared by the method described in the examples to be described later.
[0154] [Example]
[0155] The present embodiment will be described in more detail below with reference to specific examples and comparative examples, but the present invention is not limited by the following examples and comparative examples.
[0156] The measurement of physical properties and evaluation of characteristics in the examples and comparative examples were performed as follows.
[0157] ((1) Content of aromatic vinyl monomer units in the block copolymer)
[0158] The content of aromatic vinyl monomer units in the block copolymer was obtained by using the block copolymer as a sample, preparing the sample as a chloroform solution, and measuring the content of aromatic vinyl monomer units (mass%) by the absorption of UV 254 nm by the phenyl group of the aromatic vinyl using a measuring instrument (JASCO V-550).
[0159] ((2) Ratio of the content of the block aromatic vinyl portion to the total content of the aromatic vinyl monomer units in the block copolymer)
[0160] The content of the block aromatic vinyl part relative to the total content of aromatic vinyl monomer units in the block copolymer was measured according to the osmotic acid decomposition method described in LM Kolthoff, et al., J. Polym. Sci., 1, 429 (1948).
[0161] Specifically, 0.05 g of block copolymer was dissolved in 10 mL of chloroform, 16 mL of a 69% aqueous solution of tert-butyl hydroperoxide and 4 mL of a 0.05% chloroform solution of osmium tetraoxide were added, and an oxidative decomposition reaction was carried out by refluxing in a 90°C bath for 12 minutes. After the reaction was finished, the reaction solution was cooled, and 200 mL of methanol was added to the reaction solution under stirring to precipitate the block aromatic vinyl part component. This was then filtered and separated using a 5 μm glass filter, and the content of the block aromatic vinyl part in the block copolymer was measured. Subsequently, the ratio of the block aromatic vinyl part to the total content of aromatic vinyl monomer units in the block copolymer, which is the value measured by (1) above, was calculated.
[0162] ((3) Peak top molecular weight of block copolymer)
[0163] The peak top molecular weight of the block copolymer was measured by gel permeation chromatography (hereinafter also referred to as "GPC").
[0164] The chromatograph of the GPC (the device was a Dosoh HLC-8320GPC EcoSEC, three PL Gel Column MiniMIX-C 4.6mmΦ×300mm columns were used, and tetrahydrofuran was used as the solvent. The measurement conditions were a column temperature of 40℃, a flow rate of 0.4mL / min, a sample concentration of 0.1 mass%, and an injection volume of 50μL) was measured.
[0165] The peak top molecular weight was determined from the obtained GPC chromatogram using a calibration curve prepared with commercially available standard monodisperse polystyrene of known molecular weight.
[0166] GPC; HLC-8320GPC EcoSEC (Dososaje)
[0167] Detector; RI
[0168] Column; PL Gel Column 5㎛ MiniMIX-C 4.6mmΦ×300mm 3 pieces
[0169] Solvent; Tetrahydrofuran
[0170] Flow rate; 0.4 mL / min
[0171] Concentration; 0.1 mass%
[0172] Column temperature; 40℃
[0173] Injection volume: 50μL
[0174] ((4) Peak top molecular weight of the block aromatic vinyl portion in the block copolymer, and molecular weight distribution (Mw / Mn))
[0175] 0.1 g of block copolymer was dissolved in 100 mL of dichloromethane, and oxygen with an ozone concentration of 1.5% was passed through the solution at a rate of 150 mL / min to oxidatively decompose it, and the obtained ozonide was reduced by adding dropwise to diethyl ether mixed with lithium aluminum hydride.
[0176] Subsequently, pure water was added dropwise to hydrolyze, and potassium carbonate was added to perform salting out and filtration, thereby obtaining the components of the blocked aromatic vinyl part. This blocked aromatic vinyl part was measured by GPC.
[0177] The chromatograph of the GPC (the device was a Dosoh HLC-8320GPC EcoSEC, two Shodex KF-803L and KF-801 columns were used, tetrahydrofuran was used as the solvent, and the measurement conditions were a column temperature of 40℃, a flow rate of 0.8 mL / min, a sample concentration of 0.1 mass%, and an injection volume of 50 μL) was measured to obtain the peak top molecular weight.
[0178] Using a calibration curve prepared with commercially available standard monodisperse polystyrene of known molecular weight, the weight-average molecular weight Mw and number-average molecular weight Mn were determined from the obtained GPC chromatogram, and the molecular weight distribution (Mw / Mn) was calculated.
[0179] GPC; HLC-8320GPC EcoSEC (Dososaje)
[0180] Detector; UV
[0181] Column; Shodex K-803L, K801, K8013 pieces
[0182] Solvent; Tetrahydrofuran
[0183] Flow rate; 0.8 mL / min
[0184] Concentration; 0.1 mass%
[0185] Column temperature; 40℃
[0186] Injection volume: 50μL
[0187] ((5) Amount of 1,2-vinyl bonds in conjugated diene monomer units in block copolymers)
[0188] The 1,2-vinyl binding amount of conjugated diene monomer units was determined by infrared spectroscopic analysis “Hampton, Anal, Chem, 21, 923(1941)”.
[0189] ((6) Viscosity of styrene solution of 5 mass% of block copolymer under temperature conditions of 25℃)
[0190] The viscosity of a styrene solution of 5 mass% of block copolymer under temperature conditions of 25℃ was measured by dissolving 5g of block copolymer in 95g of styrene and using a Canon-Penske type viscometer (manufactured by Kusano Kagaku Kiki Se Asakusho, product name: Canon-Penske No. 200) at a measurement temperature of 25℃.
[0191] ((7) Hardness of the veil-molded body of the block copolymer)
[0192] 35 kg of block copolymer clamps are inserted into a bale forming mold (length 70 cm, width 35 cm), and the compression pressure is 200 kg / cm². 2 A bale was formed under conditions of compression time: 50 seconds, compression temperature: 60°C, and the hardness of the obtained bale was recorded using an Asuka "JIS K 6253 durometer type E" when the durometer was pressed on a smooth part.
[0193] The bale molded body was turned over, and five smooth points were measured, with the average value taken as the hardness of the bale molded body.
[0194] ((8) Peak current during grinding of the block copolymer bale molded body)
[0195] 35 kg of a bale of block copolymer was fed longitudinally into a Ritz cutter (Hosokawa Micron Co., Ltd. Ritz Rubber Chopper Model PB15H), and then the power to the Ritz cutter was turned on to rotate the screw. The peak current value was measured when the entire bale of the bale was cut longitudinally into the rotating screw inside the Ritz cutter, and this was used as an indicator of the load during the crushing of the bale.
[0196] In addition, there are cases where the current value momentarily exceeds the upper limit and goes outside the scale when bail digging begins after the Litz cutter power is turned on; however, since this occurs only for a brief moment, it was decided not to treat this as the peak current value.
[0197] ((9) Grinding time of the veil-molded body of the block copolymer)
[0198] 35 kg of bale molded body was fed vertically into the above-mentioned Ritz cutter, and the bale molded body was sheared between a screw-type hammer and a fixed blade, and the crushed product extruded from the orifice plate by the movement of the screw was further cut by a cut-off knife. The time from the start of feeding the bale molded body at this time until the current value returns to the level before feeding the next bale molded body, when no crushed product comes out of the orifice plate, was defined as the crushing time per bale.
[0199] The Ritz cutter current value when not feeding the bale-formed body was 19 amperes.
[0200] [Polymerization of Block Copolymers and Fabrication of Veil Molds]
[0201] [Example 1]
[0202] (Polymerization and Veil Forming of Block Copolymer (SBR1))
[0203] Using a polymerization vessel with a capacity of 100 liters and equipped with a rotary stirring blade and a jacket, 79 parts by mass of 1,3-butadiene containing 100 ppm of 1,2-butadiene and 600 parts by mass of a cyclohexane solution containing 150 ppm of tetrahydrofuran (THF) were introduced into the polymerization vessel; 0.016 parts by mass of tetramethylethylenediamine (TMEDA) was added as a regulator of the 1,2-vinyl binding amount; and 0.095 parts by mass of a polymerization initiator, n-butyllithium, was added at a polymerization initiation temperature of 43.2°C, and polymerization was carried out under stirring. The reaction peak temperature of 1,3-butadiene was 96.1°C. 21 parts by mass of styrene were added 1 minute after reaching the reaction peak temperature. The temperature inside the reactor at the time of styrene addition was 95.2°C.
[0204] Next, 5 minutes after reaching the reaction peak temperature of styrene, methanol was added to inactivate the polymerization initiator n-butyllithium at a ratio of 0.8 molar to the polymerization initiator, and the polymerization reaction of the block copolymer (SBR1) was completed.
[0205] Afterwards, 2,4-bis(octylthiomethyl)-o-cresol was added as a stabilizer at a concentration of 0.15 mass% relative to the mass of the block copolymer.
[0206] Likewise, polymerization was performed four times, and after inactivation with methanol, a stabilizer was added and four blocks of copolymer rubber solution were blended.
[0207] In addition, the obtained block copolymer rubber solution was immersed in a stirring hot water bath, and after removing the solvent by steam stripping using pure water, vacuum drying was performed to obtain a clam-shaped block copolymer.
[0208] 35 kg of the obtained clamp was fed into a bale forming machine (bale forming mold: length 70 cm, width 35 cm) to produce a bale formed body of block copolymer (SBR1).
[0209] Table 1 shows the polymerization content of the block copolymer (SBR1), the physical properties of the block copolymer, the results of hardness adjustment of the bale molded body, and the pulverization properties of the bale molded body.
[0210] [Examples 2, 3 and Comparative Examples 1, 2, 3]
[0211] A veil-molded body of a block copolymer (SBR2, SBR3, SBR13, SBR14, SBR15) was obtained by the conditions of the polymerization contents described in Tables 1 and 3, except that the polymerization initiation temperature was changed in the same manner as in Example 1, and the reaction peak temperature of 1,3-butadiene and the temperature inside the reactor at the time of styrene addition were changed.
[0212] The polymerization content of the block copolymers (SBR2, SBR3 and SBR13, SBR14, SBR15) of Examples 2 and 3 and Comparative Examples 1, 2, and 3, the physical properties of the block copolymers, the results of hardness adjustment of the bale molded body, and the pulverization properties of the bale molded body are shown in Tables 1 and 3.
[0213] It was found that SBR15 of Comparative Example 3 had slightly more of the crushed material adhering to the litz cutter after bale crushing compared to SBR2 and SBR3 of the Example and SBR13 and SBR14 of the Comparative Example.
[0214] [Example 4 and Comparative Example 4]
[0215] In the same manner as in Example 1, the amount of tetramethylethylenediamine (TMEDA), a 1,2-vinyl bonding modifier, was increased, and veil-molded bodies of block copolymers SBR4 and SBR16 were obtained.
[0216] The polymerization content of block copolymers SBR4 and SBR16 of Example 4 and Comparative Example 4, the physical properties of the block copolymers, the results of hardness adjustment of the bale molded body, and the pulverization properties of the bale molded body are shown in Tables 1 and 3.
[0217] [Examples 5, 6 and Comparative Example 5]
[0218] Under the conditions of the polymerization contents described in Tables 1 and 3, a block copolymer (SBR5) with an aromatic vinyl monomer unit content of 16.2 mass%, a block copolymer (SBR6) with an aromatic vinyl monomer unit content of 24.8 mass%, and a block copolymer (SBR17) with an aromatic vinyl monomer unit content of 34.8 mass% were obtained. As for Example 5, Example 6, and Comparative Example 5, the physical properties of the block copolymers, the results of hardness adjustment of the veil molded bodies, and the pulverization properties of the veil molded bodies are shown in Tables 1 and 3.
[0219] Comparative Example 5 (SBR17) was found to have a high load on the grinder, with a peak current of 47A during grinding, because the hardness of the bale molded body was 78.
[0220] [Examples 7, 8 and Comparative Example 6]
[0221] Polymerization was carried out under the conditions of the polymerization contents described in Tables 2 and 3, and styrene was added at a stage prior to the reaction peak, when the 1,3-butanediene reaction exceeded 90°C. For Example 7 (SBR7), styrene was added at 90.3°C, for Example 8 (SBR8) at 95.2°C, and for Comparative Example 6 (SBR18) at 92.0°C. As a result, the ratio of the content of the block aromatic vinyl part to the content of the aromatic vinyl monomer unit was 90.8 mass%, 90.5 mass%, and 91.4 mass%, respectively.
[0222] In addition, Comparative Example 6 (SBR18) reduced the amount of catalyst added to increase the molecular weight, and as the peak top molecular weight of the block aromatic vinyl part exceeded 30,000, the hardness of the bale molded body exceeded 80, and the load during grinding increased, resulting in poor grindability.
[0223] [Comparative Example 7]
[0224] Polymerization was carried out under the conditions of the polymerization contents listed in Table 3. Before the start of polymerization, 6.3 parts by mass of styrene were introduced into the polymerization vessel together with 79 parts by mass of 1,3-butadiene, and the remaining 14.7 parts by mass of styrene were added after the 1,3-butadiene reaction peak temperature. As a result, a block copolymer (SBR19) was obtained in which the ratio of the content of the block aromatic vinyl part to the content of the aromatic vinyl monomer unit was 73.1 mass%.
[0225] Although the bale hardness is low at 42 and the load during bale crushing is small, adhesion was confirmed inside the crusher due to heat generation during crushing, similar to Comparative Example 3 (SBR15). In addition, it was found that the bale molded body is prone to deformation when stacked because the hardness of the bale molded body is low.
[0226] [Example 9]
[0227] A veil-molded body of a block copolymer (SBR9) was obtained by increasing the amount of n-BuLi, a polymerization initiator, in the same manner as in Example 1.
[0228] By increasing the amount of polymerization initiator, the peak top molecular weight of the block copolymer was lower than in Example 1, and the hardness of the veil was 49.
[0229] Table 2 shows the polymerization content of the block copolymer (SBR9), the physical properties of the block copolymer, the results of hardness adjustment of the bale molded body, and the pulverization properties of the bale molded body.
[0230] [Example 10]
[0231] A veil-molded body of a block copolymer (SBR10) was obtained by reducing the amount of the polymerization initiator n-BuLi added in the same manner as in Example 1.
[0232] By reducing the polymerization initiator, the peak top molecular weight of the block copolymer was higher than in Example 1, and the hardness of the veil was 69.
[0233] The polymerization content of the block copolymer (SBR10), the physical properties of the block copolymer, the results of hardness adjustment of the bale molded body, and the pulverization properties of the bale molded body are shown in Table 2.
[0234] [Example 11]
[0235] In the same manner as in Example 1, tetramethylethylenediamine (TMEDA), which is a 1,2-vinyl bonding amount adjusting agent, was not added, and the amount of tetrahydrofuran (THF) was increased to obtain a bale-molded body of a block copolymer (SBR11) with a 1,2-vinyl bonding amount of 13.3 mass%. The polymerization details of the block copolymer (SBR11), the physical properties of the block copolymer, the results of hardness adjustment of the bale-molded body, and the pulverization properties of the bale-molded body are shown in Table 2.
[0236] [Example 12]
[0237] In the same manner as in Example 1, the amount of tetramethylethylenediamine (TMEDA), a 1,2-vinyl bonding amount adjusting agent, was increased to obtain a veil-molded body of a block copolymer (SBR12) with a 1,2-vinyl bonding amount of 31.2%.
[0238] The polymerization content of the block copolymer (SBR12), the characteristics of the block copolymer, the results of hardness adjustment of the bale molded body, and the pulverization properties of the bale molded body are shown in Table 2.
[0239]
[0240]
[0241]
[0242] From Tables 1 to 3, it was found that block copolymers SBR1 to 12 (Examples 1 to 12) are suitable for controlling the hardness of bale molded bodies, which is optimal for crushing bale molded bodies, and have a low load (current value) during crushing and can be continuously fed, resulting in a short crushing time per bale molded body.
[0243] [Characteristics of Impact-Resistant Aromatic Vinyl Resin Compositions]
[0244] As shown in [Examples 13 to 19] and [Comparative Examples 8 and 9] described below, impact-resistant aromatic vinyl resin compositions were prepared, and the following characteristic measurements and evaluations were performed.
[0245] <Average particle size of rubber particles>
[0246] An impact-resistant aromatic vinyl resin composition was dissolved in dimethylformamide, and only the polystyrene-based resin portion forming the matrix of the resin composition was dissolved. A portion of the solution was then dispersed into the solvent dimethylformamide solution in a measuring cell using a particle size distribution (laser diffraction / scattering) measuring device, LA-920, manufactured by Horiba Seisakusho, and the result was measured. The obtained volume-averaged particle size was defined as the rubber particle size.
[0247] Glossiness
[0248] Gloss was measured in accordance with JIS Z8742 (angle of incidence 60°).
[0249] Impact resistance
[0250] The Izod impact strength was measured according to JIS K7110 (with notch).
[0251] [Examples 13 to 19]
[0252] In a stirred polymerization vessel subjected to nitrogen substitution, 20 parts by weight of ethylbenzene and 12 parts by weight of a block copolymer (listed in Table 4) were dissolved with respect to 100 parts by weight of a monomer mixture containing 75% by weight of styrene and 25% by weight of acrylonitrile; additionally, 0.15 parts by weight of octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 200 ppm by weight of 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane with respect to 100 parts by weight of the monomer mixture, and 1500 ppm by weight of t-dodecyl mercaptan with respect to 100 parts by weight of the monomer mixture were added, stirred at 150 rpm at 100°C for 7 hours, and thereafter stirred at 15 rpm at 120°C for 1 hour. Polymerization was continued by sequentially increasing the temperature at 135°C for 2 hours, 150°C for 2 hours, and 170°C for 2 hours, and finally, heat treatment was performed at 230°C for 30 minutes. After that, the inside of the polymerization vessel was brought to atmospheric pressure, and the impact-resistant aromatic vinyl resin composition, which is the polymer at the time of heating, was taken out and cooled in pure water.
[0253] To remove unreacted styrene, acrylonitrile, and ethylbenzene, 1000 ml of dichloromethane was added per 100 g of the polymer after cooling and stirred to dissolve.
[0254] The solution was redeposited by adding dropwise to 10 times the amount of isopropyl alcohol relative to the solution.
[0255] The impact-resistant aromatic vinyl resin composition that was reprecipitated was vacuum dried to obtain an impact-resistant aromatic vinyl resin composition (ABS resin composition).
[0256] After heat-pressing this at 200℃ and cooling it, it was ground to a size of 5 mmφ, and the ground product was injection molded to measure the physical properties of the ABS resin composition.
[0257] The measurement results are shown in Table 4.
[0258] [Comparative Example 8, Comparative Example 9]
[0259] SBR14 and SBR15 were used as block copolymers, and test specimens of ABS were prepared in the same manner as in Example 13.
[0260] The results of the physical property measurements are shown in Table 4.
[0261]
[0262] From Table 4, it was found that when comparing the physical properties of ABS resin compositions using block copolymer SBRs with different molecular weight distributions (Mw / Mn) of the block aromatic vinyl portion of the block copolymer, the physical properties of the ABS resin compositions were equivalent and good for SBR1 of Example 13 with Mw / Mn=1.20 and SBR14 of Comparative Example 8 with Mw / Mn=1.07, but the impact resistance of the ABS was lower for SBR15 of Comparative Example 9 with Mw / Mn=1.41. Industrial applicability
[0263] The block copolymer bale molded body of the present embodiment has industrial applicability as a modifier for styrene-based resins.
Claims
Claim 1 A veil-molded article of a block copolymer having aromatic vinyl monomer units and conjugated diene monomer units, wherein the block copolymer has a block aromatic vinyl portion, the viscosity of a styrene solution of 5 mass% of the block copolymer is 7 to 15 mPa·s under a temperature condition of 25°C, and the veil-molded article satisfies the following <Condition (a)> to <Condition (d)>. <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass%; <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass%; <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000; <Condition (d)> The ratio (Mw / Mn) of the weight-average molecular weight Mw and the number-average molecular weight Mn of the block aromatic vinyl portion is 1.15 to 1.40 Claim 2 A veil-molded body according to claim 1, wherein the 1,2-vinyl bonding amount of the conjugated diene monomer unit of the block copolymer is 15 to 30 mol%. Claim 3 In claim 1, a bale molded body having a hardness of 50 to 72 as measured by a hardness tester type E in accordance with JIS K6253. Claim 4 A block copolymer having aromatic vinyl monomer units and conjugated diene monomer units, wherein the block copolymer has a block aromatic vinyl portion, the viscosity of a styrene solution of 5 mass% of the block copolymer is 7 to 15 mPa·s under a temperature condition of 25°C, and the block copolymer satisfies the following <Condition (a)> to <Condition (d)>. <Condition (a)> The content of aromatic vinyl monomer units in the block copolymer is 10 to 30 mass% <Condition (b)> The ratio of the block aromatic vinyl portion to the total content of aromatic vinyl monomer units is 90 to 100 mass% <Condition (c)> The peak top molecular weight of the block aromatic vinyl portion is 10,000 to 30,000 <Condition (d)> The ratio of the weight-average molecular weight Mw and the number-average molecular weight Mn of the block aromatic vinyl portion (Mw / Mn) is 1.15 to 1.40 Claim 5 In paragraph 4, the block copolymer having a 1,2-vinyl bond content of the conjugated diene monomer unit of the block copolymer of 15 to 30 mol%. Claim 6 A resin composition comprising 3 to 20 parts by mass of a block copolymer constituting a veil molded body as described in any one of claims 1 to 3, and 97 to 80 parts by mass of a styrene-based resin. Claim 7 A resin composition according to claim 6, wherein the styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile. Claim 8 A method for manufacturing a block copolymer constituting a bale molded body as described in any one of claims 1 to 3, comprising the steps of: supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound such that the peak temperature is 91 to 100°C; and supplying an aromatic vinyl compound to the reactor at a temperature of 90 to 100°C and polymerizing it. Claim 9 A resin composition comprising 3 to 20 parts by mass of the block copolymer described in claim 4 or 5 and 97 to 80 parts by mass of a styrene-based resin. Claim 10 In claim 9, the resin composition wherein the styrene-based resin is a copolymer of a styrene-based compound and acrylonitrile. Claim 11 A method for manufacturing a block copolymer as described in claim 4 or 5, comprising the steps of: supplying a conjugated diene compound to a reactor and polymerizing the conjugated diene compound such that the peak temperature is 91 to 100°C; and supplying an aromatic vinyl compound to the reactor at a temperature of 90 to 100°C and polymerizing it. Claim 12 delete Claim 13 delete
Citation Information
Patent Citations
Block copolymer and its production
JP1998265537A
Block copolymer rubber, resin modifier, resin composition and method for producing the same resin composition
JP2001240637A
Resin composition, adhesive agent, and compatibilizer
WO2022149574A1
Aromatic vinyl / conjugated diene block copolymer and its production
JP1998204136A
Block copolymer, composition for resin modification, and modified resin composition
WO2008001907A1