Electrocatalyst including chiral plasmonics / single-atom and water splitting system including the same

A chiral plasmonic nanoparticle-based electrocatalyst with metal single atoms enhances oxygen and hydrogen evolution reactions, addressing the limitations of precious metals in water splitting systems by improving efficiency and stability.

KR103046986B1Active Publication Date: 2026-11-11EWHA UNIV IND COLLABORATION FOUND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020240035098
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2026-11-11
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

The high cost and scarcity of precious metals like platinum, ruthenium, and iridium limit the commercialization of water splitting systems, necessitating the development of more efficient and cost-effective electrocatalysts for hydrogen and oxygen evolution reactions.

Method used

An electrocatalyst comprising chiral plasmonic nanoparticles with spike-shaped projections and metal single atoms, such as iridium, is used to enhance the oxygen evolution reaction through localized surface plasmon resonance and improve catalytic efficiency.

Benefits of technology

The electrocatalyst increases the rate of oxygen evolution reaction and hydrogen evolution reaction, demonstrating stability under light irradiation for over 500 hours and efficient operation under acidic conditions, outperforming conventional catalysts in terms of activity and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure R1020240035098_ABST
    Figure R1020240035098_ABST
Patent Text Reader

Abstract

The present invention relates to an electrocatalyst comprising chiral plasmonic nanoparticles and a water splitting system using an electrode comprising the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an electrocatalyst comprising chiral plasmonic nanoparticles and single atoms, and a water splitting system using an electrode comprising the same. Background Technology

[0002] Water electrolysis is a technology that splits water into hydrogen and oxygen by supplying power to an electrolyte used for water ionization. Depending on the electrolyte used, representative types include alkaline electrolysis cells (AEC), proton exchange membrane electrolysis cells (PEMEC), and solid oxide electrolysis cells (SOEC). Hydrogen production through water splitting is attracting attention as a promising energy source. The hydrogen evolution reaction (HER) occurs at the cathode of the water splitting device, while the oxygen evolution reaction (OER) occurs at the anode. Research is underway to maximize the activity and stability of platinum (Pt), ruthenium (Ru), or iridium (Ir)-based precious metal catalysts that exhibit high activity in the hydrogen and oxygen evolution reactions. However, because the high cost and scarcity of precious metals make commercialization difficult, subsequent research and development on catalysts is essential. Prior art literature

[0003] Korean Registered Patent Publication No. 10-2471909. The problem to be solved

[0004] The present invention aims to provide a water splitting system using an electrocatalyst comprising chiral plasmonic nanoparticles and a single atom, and an electrode comprising the same.

[0005] However, the problems that this invention seeks to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by a person skilled in the art from the description below. means of solving the problem

[0006] A first aspect of the present invention provides an electrocatalyst comprising: a support; a chiral plasmonic nanoparticle located on the support and having a spike-shaped projection; and a metal single atom located on the chiral plasmonic nanoparticle.

[0007] A second aspect of the present invention provides a water splitting system using an electrode comprising an electrocatalyst according to a first aspect. Effects of the invention

[0008] The electrocatalyst according to the embodiments of the present invention comprises a single metal atom and may have increased catalytic efficiency compared to conventional electrocatalysts.

[0009] The electrocatalyst according to the embodiments of the present invention can increase the rate of the oxygen evolution reaction through hot carriers due to the localized surface plasmon resonance (LSPR) effect.

[0010] The electrocatalyst according to the embodiments of the present invention can be used in an oxygen evolution reaction and / or a hydrogen evolution reaction.

[0011] An electrode comprising an electrocatalyst according to embodiments of the present invention can be operated for about 500 hours under light irradiation.

[0012] The water splitting system according to the embodiments of the present invention can be operated under acidic conditions. Brief explanation of the drawing

[0013] FIG. 1 is a schematic diagram of a method for manufacturing an Ir single atom (SA) / chiral Au nanoflower (NF) / Ti felt electrode according to one embodiment of the present invention. FIG. 2a and 2b are scanning electron microscopy (SEM) and transmission electron microscopy (TEM) images of an Ir SA / chiral Au NF / Ti felt electrode in one embodiment of the present invention. FIG. 3 is a powder X-ray diffraction (XRD) spectrum of an Ir SA / chiral Au NF / Ti felt electrode in one embodiment of the present invention. FIG. 4a and 4b are, in one embodiment of the present invention, a high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) image of Ir SA / L-Au NF and the corresponding fast Fourier transform (FFT) pattern and STEM-EDS (scanning transmission electron microscopy-energy dispersive X-ray spectroscopy) elemental mapping image of Ir SA / L-Au NF. FIG. 5 is an X-ray photoelectron spectroscopy (XPS) spectrum of Ir 4f Ir SA / L-Au NF and IrO2 reference samples in one embodiment of the present invention. FIG. 6 is a circular dichroism (CD) spectrum of Ir SA / D-Au NF; D-Au NF; DL-Au NF; L-Au NF; and Ir SA / L-Au NF in one embodiment of the present invention. FIG. 7 is a schematic diagram of a magnetic conductive probe atomic force microscopy (mc-AFM) in one embodiment of the present invention. FIG. 8a and 8b are power graphs (IV curves) of Ir SA / DL-cysteine ​​Au NF and Ir SA / L-cysteine ​​Au NF films according to a voltage in the range of -1.5 to +1.5 V in one embodiment of the present invention. FIG. 9 is a graph of the percentage of spin polarization (SP%) as a function of the bias applied to an Ir SA / L-cysteine ​​Au NF film in one embodiment of the present invention. FIG. 10a and b are linear sweep voltammetry (LSV) graphs of DL-Au NF, Ir SA / DL-Au NF, and Ir SA / L-Au NF for OER in one embodiment of the present invention; mass activity graphs of Ir SA / DL-Au NF, Ir SA / L-Au NF, and Ir O2; and FIG. 10c is a Tafel plot corresponding to FIG. 10a. FIGS. 11a to c are, in one embodiment of the present invention, 10 mA cm⁻¹ for OER -2 Overpotential graph at; turnover frequency (TOF) graph at 1.575V vs. RHE; and 10 mA cm⁻¹ of DL-Au NF, Ir SA / DL-Au NF, and Ir SA / L-Au NF -2 This is a graph of the stability test results in. FIG. 12a and b are linear sweep voltammetry (LSV) graphs of DL-Au NF, Ir SA / DL-Au NF, and Ir SA / L-Au NF for HER in one embodiment of the present invention; mass activity graphs of Ir SA / DL-Au NF, Ir SA / L-Au NF, and Pt / C; and FIG. 12c is a Tafel plot corresponding to FIG. 12a. FIG. 13a to c are, in one embodiment of the present invention, 10 mA cm for HER -2 and 100 mA cm -2 Overpotential graphs at; and 10 mA cm⁻¹ of DL-Au NF, Ir SA / DL-Au NF, and Ir SA / L-Au NF -2 This is a graph of the stability test results in. FIG. 14 is an image of a water splitting test performed in a three-electrode configuration using an Ag / AgCl reference electrode in one embodiment of the present invention. FIG. 15 is a polarization IV profile measured in 0.5 M H2SO4 in one embodiment of the present invention. FIG. 16 shows, in one embodiment of the present invention, 100 mA cm for 500 hours. -2 This is the time potential difference stability profile measured at. FIG. 17 is a graph comparing the stability of water electrolysis of an electrocatalyst according to one embodiment of the present invention and a conventional catalyst. Specific details for implementing the invention

[0014] Hereinafter, embodiments and examples of the present invention are described in detail with reference to the attached drawings so that those skilled in the art can easily implement the present invention. However, the present invention may be implemented in various different forms and is not limited to the embodiments and examples described herein. Furthermore, in order to clearly explain the present invention in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification have been given similar reference numerals.

[0015] Throughout this specification, when a part is described as being "connected" to another part, this includes not only cases where they are "directly connected," but also cases where they are "electrically connected" with other elements interposed between them.

[0016] Throughout this specification, when a component is described as being located "on" another component, this includes not only cases where a component is in contact with another component, but also cases where another component exists between the two components.

[0017] Throughout this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0018] Terms of degree used in this specification, such as “about,” “substantially,” etc., are used to mean at or near the stated value when inherent manufacturing and material tolerances are presented in the stated meaning, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute values ​​are mentioned to aid in understanding the invention.

[0019] The terms “step of” or “step of” as used throughout this specification do not mean “step for”.

[0020] Throughout this specification, the term “combination(s) of these” included in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including one or more selected from the group consisting of said components.

[0021] Throughout this specification, the description "A and / or B" means "A or B, or A and B".

[0023] A first aspect of the present invention provides an electrocatalyst comprising: a support; a chiral plasmonic nanoparticle located on the support and having a spike-shaped projection; and a metal single atom located on the chiral plasmonic nanoparticle.

[0024] In one embodiment of the present invention, the chiral plasmonic nanoparticles may comprise one or more selected from Au, Ag, Pd, Cu, Al, and Mg. In one embodiment of the present invention, the chiral plasmonic nanoparticles may be Au.

[0025] In one embodiment of the present invention, the chiral derivative of the chiral plasmonic nanoparticle may be D / L-cysteine.

[0026] In one embodiment of the present invention, the chiral plasmonic nanoparticles may be flower-like.

[0027] In one embodiment of the present invention, the chiral plasmonic nanoparticles can be synthesized on the support using electroplating.

[0028] In one embodiment of the present invention, the metal included in the metal single atom may include one or more selected from Ir, Ru, Pd, Rh, and Pt. In one embodiment of the present invention, the metal included in the metal single atom may be Ir.

[0029] In one embodiment of the present invention, the metal single atom can be synthesized by electroplating on the chiral plasmonic nanoparticle.

[0030] In one embodiment of the present invention, the metal single atom may be present in an amount of about 1 part by weight to about 5 parts by weight per 100 parts by weight of the chiral plasmonic nanoparticle, but is not limited thereto. In one embodiment of the present invention, the metal single atom may be present in an amount of about 1 part by weight to about 5 parts by weight, about 1 part by weight to about 4 parts by weight, or about 1 part by weight to about 3 parts by weight per 100 parts by weight of the chiral plasmonic nanoparticle, but is not limited thereto. In one embodiment of the present invention, it may be most preferable for the metal single atom to be present in an amount of about 2 parts by weight per 100 parts by weight of the chiral plasmonic nanoparticle.

[0031] In one embodiment of the present invention, the diameter of the chiral plasmonic nanoparticle may be about 20 nm to about 200 nm, but is not limited thereto. In one embodiment of the present invention, the diameter of the chiral plasmonic nanoparticle is about 20 nm to about 200 nm, about 20 nm to about 180 nm, about 20 nm to about 160 nm, about 20 nm to about 140 nm, about 20 nm to about 120 nm, about 20 nm to about 100 nm, about 20 nm to about 80 nm, about 20 nm to about 60 nm, about 20 nm to about 40 nm, about 40 nm to about 200 nm, about 40 nm to about 180 nm, about 40 nm to about 160 nm, about 40 nm to about 140 nm, about 40 nm to about 120 nm, about 40 nm to about 100 nm, about 40 nm to about 80 nm, about 40 nm to about 60 nm, about 60 nm to about 200 nm, about 60 nm to about 180 nm, about 60 nm to about 160 nm, about 60 nm to about 140 nm, about 60 nm to about 120 nm, about 60 nm to about 100 nm, about 60 nm to about 80 nm, about 80 nm to about 200 nm, about 80 nm to about 180 nm, about 80 nm to about 160 nm, about 80 nm to about 140 nm, about 80 nm to about 120 nm, about 80 nm to about 100 nm, about 100 nm to about 200 nm, about 100 nm to about 180 nm, about 100 nm to about 160 nm, about 100 nm to about 140 nm, about 100 nm to about 120 nm, about 120 nm to about 200 nm, about 120 nm to about 180 nm, about 120 nm to about 160 nm, about 120 nm to about 140 nm, about 140 nm to about 200 nm, about 140 nm to about 180 nm,It may be about 140 nm to about 160 nm, about 160 nm to about 200 nm, about 160 nm to about 180 nm, or about 180 nm to about 200 nm, but may not be limited thereto.

[0032] In one embodiment of the present invention, the support may be in a form that includes a fluid movement passage.

[0033] In one embodiment of the present invention, the above material may be used without limitation as long as it is used as a substrate for electrodes in the relevant industry, and as non-limiting examples, it may be a carbon-based material; a metal including Ti, Ni, or Cu, etc.; an inorganic oxide including an oxide of Ti, Zr, Al, or Si, etc.; or a perovskite oxide or a zeolite.

[0034] In one embodiment of the present invention, the carbon-based material may comprise one or more selected from graphite, carbon fiber, carbon sheet, carbon black, carbon nanotube (CNT), carbon sphere, carbon ribbon, fullerene, active carbon, carbon nanowire, and graphene, but is not limited thereto.

[0035] In one embodiment of the present invention, the substrate may be in a form including a fluid movement passage, but is not limited thereto. Here, the fluid movement passage may be included in one or more of the substrate. In one embodiment of the present invention, the substrate may be in the form of a mesh structure, but is not limited thereto.

[0036] In one embodiment of the present invention, the above material may be formed of Ti fibers, Ni fibers, or Pt fibers in a network structure, but is not limited thereto.

[0037] In one embodiment of the present invention, the support may comprise a carbonaceous material; a metal comprising Ti, Ni, or Cu; an inorganic oxide comprising an oxide of Ti, Zr, Al, or Si; a perovskite oxide, or a zeolite.

[0038] In one embodiment of the present invention, the electrocatalyst may be used for an oxygen evolution reaction and / or a hydrogen evolution reaction.

[0040] A second aspect of the present invention provides a water splitting system using an electrode comprising an electrocatalyst according to a first aspect.

[0041] Detailed explanations have been omitted for parts that overlap with the first aspect of the present invention, but the content described in the first aspect of the present invention may be applied in the same way even if such explanations are omitted in the second aspect of the present invention.

[0042] In one embodiment of the present invention, the water splitting system may have a symmetric structure in which both the anode and the cathode of the water splitting system are composed of the electrodes.

[0043] In one embodiment of the present invention, the water splitting system may be operated under conditions of irradiating light.

[0044] In one embodiment of the present invention, the water splitting system may be operated under acidic conditions. This means that it is operated under acidic conditions as well as alkaline conditions, which are generally milder than acidic conditions, and does not mean that it is limited to being operated only under acidic conditions.

[0045] In one embodiment of the present invention, the electrode may be operated for about 250 hours or more.

[0047] The present invention will be explained in more detail below using examples, but the following examples are merely illustrative to aid in understanding the present invention, and the content of the present invention is not limited to the following examples.

[0049] [Example]

[0050] Flower-shaped gold nanoparticles were synthesized on a titanium felt substrate (Ti felt) using electroplating. During this process, D / L-cysteine ​​was used as a chiral derivative. Subsequently, chiral plasmonic nanostructures containing iridium single atoms (SA) were obtained by controlling the loading of iridium single atoms using precise electroplating cycles (see Fig. 1).

[0051] Gold nanoparticles (Au NPs) enhance the rate of the oxygen evolution reaction through hot carriers resulting from the localized surface plasmon resonance (LSPR) effect. Chiral structures using D / L-cysteine ​​suppress the generation of singlet oxygen while generating triplet oxygen through the polarization of electron spins due to chiral-induced spin selectivity. Iridium single atoms improve oxygen evolution reaction activity under acidic conditions.

[0052] <Ir 단일원자(single atom, SA) / 키랄 Au 나노플라워(nanoflower, NF) / Ti 전극의 특성 분석>

[0053] Referring to Figure 2, scanning electron microscopy (SEM) and transmission electron microscopy (TEM) analysis results showed uniform surface electroplating and lattice spacing indicating nanocrystalline properties of Au NF.

[0054] Ti 334.941 nm 197 Au [No gas] 193 Ir [No gas] (DL) 193 Ir [No gas] (L) Concentration [ppm] RSD Concentration [ppm] RSD Concentration [ppm] RSD Concentration [ppm] RSD 2686.038 0.567 2922.808 0.196 73.360 0.630 79.848 0.709

[0055] Referring to Figure 3 and Table 1 above, the crystal structure of Au NF was confirmed through X-ray diffraction (XRD) spectra, and inductively coupled plasma-mass spectrometry (ICP-MS) analysis confirmed that the amount of iridium was 1.4 wt%, which is a very low amount suitable for single atoms.

[0056] Further structural analysis at the atomic level using high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) (Fig. 4a) revealed no noticeable Ir metal particles. Referring to Fig. 4b, a uniform distribution of Au and Ir single atoms was confirmed, and Ir single atoms were dispersed on the surface of Au NFs, confirming that the electrocatalyst was successfully prepared.

[0057] Referring to Fig. 5, the chemical state of the synthesized catalyst was determined using X-ray photoelectron spectroscopy (XPS). XPS analysis showed that the Ir 4f spectrum is split into two doublets, indicating electron transfer from iridium to gold.

[0058] <Ir SA / 키랄 Au NF / Ti 전극의 키롭틱(chiroptical) 특성 분석>

[0059] D-Cysteine:Au 3+ (D-Au NF) and L-cysteine:Au 3+ The circular dichroism (CD) spectra of these electrodes obtained from (L-Au NF) show approximate mirror symmetry, which reflects the opposite chirality of Au NF electrodes grown in solutions with different Au-cysteine ​​chirality (Fig. 6).

[0060] The spin-dependent current of the chiral Au NF was measured using magnetic conductive probe atomic force microscopy (mc-AFM) as shown in Fig. 7. For the Ir SA / DL-Au NF (a-chiral) electrode, no significant change in current was observed even with changes in tip magnetization (Fig. 8a). Spin polarization (SP) was calculated using a specific equation, and the average spin polarization for the Ir SA / L-Au NF electrode was found to be 81.4% (Fig. 9). For the Ir SA / L-Au NF (chiral) electrode, the current under tip-up conditions (north-magnetized ferromagnetic tip) showed a distinct current compared to tip-down conditions (south-magnetized ferromagnetic tip), indicating a preference for upward spin charge carriers (Fig. 8b).

[0061] <Electrochemical Performance Analysis 1 (Oxygen Evolution Reaction)>

[0062] The oxygen evolution reaction electrocatalytic activity of the Ir SA / chiral Au NF electrode was evaluated using a three-electrode system in a 0.5 M H2SO4 electrolyte. Referring to Fig. 10a, the OER activity analysis of the Ir SA / L-Au NF electrode and the comparative example using linear sweep voltammetry (LSV) showed that the Ir SA / L-Au NF electrode exhibited superior OER activity compared to the commercial IrO2 electrode, particularly under light irradiation.

[0063] Referring to Figure 10b, the mass activity analysis of Ir SA / L-Au NF showed a more efficient OER pathway compared to Ir O2.

[0064] Referring to Figure 10c, Tafel analysis provided a deeper understanding of the OER kinetics of Ir SA / L-Au NF. Ir SA / L-Au NF exhibited a low Tafel slope under light conditions, indicating a more efficient OER pathway stimulated by the combination of iridium single atoms, chirality, and plasmonic effects.

[0065] 10 mA cm -2 In terms of achieving the current density, Ir SA / L-Au NF under light irradiation required an overpotential (η) of 272.6 mV, which was lower than under dark conditions (313.8 mV) and Ir SA / DL-Au NF (340 mV) (Fig. 11a). Electrocatalytic system evaluation typically involves key parameters such as specific activity and time-of-flight (TOF). Referring to Fig. 11b, for the specific activity measured at 1.575 V vs RHE, Ir SA / L-Au NF under light irradiation exhibited the highest specific activity (60.2 mA cm⁻¹). -2 It showed ), which is Ir SA / L-Au NF (21.6 mA cm⁻¹) under dark conditions. -2 ) and Ir SA / DL-Au NF (8.85 mA cm -2 They were about 2.8 times and 6.8 times higher, respectively, than ).

[0066] Referring to Fig. 11c, Ir SA / L-Au NF also showed excellent stability in OER and exhibited only a slight increase in overpotential during a 10-hour test, demonstrating excellent durability as an OER electrocatalyst.

[0067] <Electrochemical Performance Analysis 2 (Hydrogen Evolution Reaction)>

[0068] Referring to Fig. 12a, linear scanning potentiometry (LSV) analysis results showed that the HER current density of the Ir SA / L-Au NF electrode and the comparative example gradually increased with or without light. This increase was observed due to doping of a single iridium atom (Ir SA / L-Au NF), application of chirality (Ir SA / L-Au NF), and induction of plasmonic effects under light irradiation (Ir SA / L-Au NF light).

[0069] Referring to Figure 12b, the mass activity analysis of Ir SA / L-Au NF showed an efficient HER pathway similar to Pt / C.

[0070] Referring to Figs. 12c and 13a, the Ir SA / L-Au NF electrode under light irradiation is 10 mA / cm² 2 At a current density of only 35.9 mV overvoltage and 45.2 mV dec -1 It showed a Tafel slope, exhibiting performance very similar to Pt / C.

[0071] Referring to Fig. 13b, under light irradiation, Ir SA / L-Au NF is 0.15 A mg at an overpotential of 100 mV. Ir -1 It exhibits mass activity, which is commercial Pt / C (0.30 A mg Pt -1 It is similar to the performance of ).

[0072] Referring to Fig. 13c, Ir SA / L-Au NF also showed excellent stability in HER and exhibited only a slight increase in overpotential during a 10-hour test, demonstrating excellent durability as an HER electrocatalyst.

[0073] <Overall Water Splitting Analysis>

[0074] An overall water splitting test was performed using a three-electrode configuration with an Ag / AgCl reference electrode in a 0.5 M H2SO4 acidic electrolyte (Fig. 14). Referring to Fig. 15, the cell potential (E through HER and OER) cell = E anode - E cathode Through this, it was confirmed that the water splitting efficiency of the Ir SA / L-Au NF electrode increased under light irradiation. In addition, the electrochemical stability and durability of the Ir SA / L-Au NF electrode were 100 mA cm⁻¹ -1 It was evaluated through chronopotentiometric experiments performed at current densities (Fig. 16). The Ir SA / L-Au NF electrode operated stably for over 250 hours with minimal performance change. Under light irradiation, this stability reached 500 hours, demonstrating excellent durability of the electrode in HER and OER.

[0075] Referring to FIG. 17, when the electrode used in this embodiment was compared with the performance of other conventional catalysts, the electrode of this embodiment showed excellent performance in overall water splitting stability despite challenging conditions such as high current density.

[0078] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical concept or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.

Claims

Claim 1 An electrocatalyst comprising: a support; a chiral plasmonic nanoparticle located on the support and having a spike-shaped projection; and a metal single atom located on the chiral plasmonic nanoparticle, wherein the chirality of the metal single atom is induced by the chiral plasmonic nanoparticle, and which is used in an oxygen evolution reaction and / or a hydrogen evolution reaction. Claim 2 The electrocatalyst of claim 1, wherein the chiral plasmonic nanoparticle comprises one or more selected from Au, Ag, Pd, Cu, Al, and Mg. Claim 3 An electrocatalyst according to claim 1, wherein the chiral plasmonic nanoparticles are flower-like. Claim 4 An electrocatalyst according to claim 1, wherein the metal included in the single metal atom comprises one or more selected from Ir, Ru, Pd, Rh, and Pt. Claim 5 An electrocatalyst according to claim 1, wherein the metal single atom is present in an amount of 1 to 5 parts by weight per 100 parts by weight of the chiral plasmonic nanoparticle. Claim 6 An electrocatalyst according to claim 1, wherein the diameter of the chiral plasmonic nanoparticles is 20 nm to 200 nm. Claim 7 An electrocatalyst according to claim 1, wherein the support is in a form including a fluid movement passage. Claim 8 An electrocatalyst according to claim 1, wherein the support comprises a carbonaceous material; a metal comprising Ti, Ni, or Cu; an inorganic oxide comprising an oxide of Ti, Zr, Al, or Si; a perovskite oxide, or a zeolite. Claim 9 delete Claim 10 A water splitting system using an electrode comprising an electrocatalyst according to claim 1. Claim 11 A water splitting system according to claim 10, wherein both the anode and the cathode of the water splitting system are composed of the electrodes. Claim 12 In claim 10, the water splitting system is a water splitting system that operates under conditions of irradiating light. Claim 13 In claim 10, the water splitting system is a water splitting system that operates under acidic conditions. Claim 14 A water splitting system according to claim 10, wherein the electrode is operated for 250 hours or more.