Manufacturing method of valuable metals and chemical products from secondary battery wastewater using circular integrated process
A modular process with enhanced pretreatment, multi-stage bipolar electrodialysis, and pulse/reverse potential operation effectively addresses membrane fouling and scaling in secondary battery wastewater treatment, producing high-value chemicals and metals efficiently and stably.
Patent Information
- Application Number
- KR1020250092918
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-07-10
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-07-10
AI Technical Summary
Existing wastewater treatment methods for secondary battery manufacturing fail to effectively recover valuable resources like sodium sulfate and metals, suffer from membrane fouling and scaling issues, and have low energy efficiency, making them unsuitable for stable long-term operation.
A modular circular economy process that includes pretreatment to remove impurities, a multi-stage bipolar electrodialysis system with pulse/reverse potential operation, and metal recovery through solvent extraction and crystallization, addressing membrane fouling and scaling while enhancing energy efficiency.
Stably produces high-value sulfuric acid and caustic soda from secondary battery wastewater, recovers valuable metals, and maintains membrane performance over time, improving energy efficiency and scalability.
Smart Images

Figure 112025077966938-PAT00033_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing valuable metals and chemical products from secondary battery wastewater using a circular integrated process. More specifically, the present invention relates to a modular circular economy solution that produces high-value sulfuric acid and caustic soda using sodium sulfate in secondary battery wastewater and simultaneously recovers valuable metals in the wastewater. Background Technology
[0002] With the rapid growth of the electric vehicle market, the secondary battery industry is expanding rapidly, and consequently, the issue of wastewater treatment generated during the secondary battery manufacturing process is emerging as a significant environmental issue.
[0003] Wastewater discharged from the secondary battery manufacturing process contains a large amount of sodium sulfate (Na₂S). Since it contains SO₄ and valuable metals such as nickel, cobalt, and lithium, simply disposing of it not only causes environmental pollution but also results in a waste of resources.
[0004] Existing wastewater treatment methods primarily focus on removing pollutants through neutralization and sedimentation processes, failing to recover valuable resources from the wastewater. In particular, while sodium sulfate is discharged in large quantities, there is a lack of technology to effectively utilize it as a resource.
[0005] Bipolar Electrodialysis (BPED) technology is capable of decomposing salts into acids and bases and can be utilized to produce sulfuric acid and caustic soda from sodium sulfate. However, conventional BPED technology is difficult to operate stably for long periods due to membrane fouling and scaling issues, and performance degradation is a serious problem, particularly in solutions containing various impurities such as secondary battery wastewater.
[0006] In addition, existing BPED systems have limitations in producing high-concentration products due to single-stage operation and have low energy efficiency. Due to these problems, there is an urgent need to develop innovative technologies that can effectively utilize secondary battery wastewater. The problem to be solved
[0007] The present invention aims to provide a next-generation integrated process technology capable of stably and efficiently producing high-value sulfuric acid and caustic soda from sodium sulfate in secondary battery wastewater.
[0008] In addition, the present invention fundamentally solves the membrane fouling and scaling problems of the BPED system, thereby providing a system capable of stable operation for a long period of time.
[0009] In addition, the present invention provides a technology that can simultaneously improve high-concentration product production and energy efficiency through a multi-stage process configuration and a pulse / reverse potential operation method.
[0010] In addition, the present invention provides a modular circular economy solution that maximizes economic value by recovering even valuable metals from wastewater. means of solving the problem
[0011] A method for manufacturing valuable metals and chemical products from secondary battery wastewater using a circular integrated process according to the present invention comprises: a first removal step of adding caustic soda (NaOH) to secondary battery wastewater containing sodium sulfate (Na2SO₄) to precipitate and remove valuable metals including nickel and cobalt in the form of hydroxides; and a method for removing calcium ions (Ca₆) from the solution obtained after the first removal step. 2+ ) and magnesium ions (Mg 2+It includes: a secondary removal step for removing scaling-inducing ions, including ) to ppb units; an electrolysis step for producing sulfuric acid (H2SO₄) and caustic soda (NaOH) by feeding the ultra-purified sodium sulfate solution obtained from the secondary removal step into a multi-stage bipolar electrodialysis (BPED) stack; and a metal recovery step for recovering high-purity valuable metals through solvent extraction and crystallization after redissolving the valuable metal hydroxide sludge precipitated in the primary removal step with the sulfuric acid produced in the electrolysis step.
[0012] In addition, it can be performed in a pulse / reverse potential operation method that periodically repeats forward operation, which decomposes sodium sulfate into sulfuric acid and caustic soda by applying a forward voltage; and reverse operation, which cleans the membrane surface and relieves concentration polarization by applying a reverse voltage after the forward operation.
[0013] In addition, 8 minutes of forward operation and 2 minutes of reverse operation can be repeated as one cycle.
[0014] In addition, the product concentration can be gradually increased by including a 1-stage stack producing a low-concentration product, a 2-stage stack producing a medium-concentration product, and a 3-stage stack producing a high-concentration product.
[0015] In addition, calcium ions and magnesium ions can be removed to 1 ppb or less by using at least one of an ion exchange resin, a chelating agent, or a selective precipitating agent.
[0016] In addition, a bipolar membrane (BPM), a cation exchange membrane (CEM), and an anion exchange membrane (AEM) may be arranged sequentially to form an acid cell, a salt cell, and a base cell, and may have a structure.
[0017] In addition, it may be at least one of nickel sulfate (NiSO4), cobalt sulfate (CoSO4), lithium sulfate (Li2SO4), and manganese sulfate (MnSO4).
[0018] In addition, the concentration of sulfuric acid produced in the above electrolysis step may be 10 to 30 wt%, and the concentration of caustic soda may be 8 to 25 wt%.
[0019] In addition, the caustic soda produced in-house during the above electrolysis step can be reused.
[0020] In addition, the above secondary battery wastewater is wastewater discharged from the lithium-ion secondary battery manufacturing process, and may have a sodium sulfate concentration of 50 to 200 g / L. Effects of the invention
[0021] According to the method for manufacturing valuable metals and chemical products from secondary battery wastewater using a circular integrated process according to the present invention, high-value sulfuric acid and caustic soda can be produced stably and efficiently from sodium sulfate in secondary battery wastewater, and at the same time, valuable metals in the wastewater can be recovered to maximize economic value.
[0022] In addition, the present invention enables long-term stable operation by fundamentally solving membrane fouling and scaling problems of the BPED system through a triple defense system of enhanced pretreatment, multi-stage process, and pulse / reverse potential operation.
[0023] In addition, the present invention can simultaneously improve high-concentration product production and energy efficiency through a multi-stage stack configuration, and can maintain membrane performance in an optimal state through pulse / reverse potential operation.
[0024] In addition, the present invention provides practicality and scalability by being flexibly applicable to secondary battery wastewater treatment of various scales and conditions through a modular configuration. Brief explanation of the drawing
[0025] FIG. 1 is an overall process flow diagram of a method for manufacturing valuable metals and chemical products from secondary battery wastewater using a circular integrated process according to the present invention. FIG. 2 is a schematic diagram of pulse / reverse potential operation, which is a core technology of the present invention, and is a graph showing the voltage change pattern over time and the cycles of forward operation and reverse operation. FIG. 3 is a conceptual diagram of the triple defense structure of the BPED system of the present invention, showing the structure in which the first defense layer, enhanced pretreatment, the second defense layer, multi-stage process, and the third defense layer, pulse / reverse potential operation, each protect the system from threats such as scaling ions, concentration polarization, and membrane fouling, centered around the central BPED system, as well as the functions and interactions of each defense layer. Specific details for implementing the invention
[0026] Embodiments of the present invention will be described below with reference to the attached drawings. Unless otherwise specifically defined or mentioned, terms indicating direction used in this description are based on the state shown in the drawings. Additionally, throughout each embodiment, the same reference numeral indicates the same component. Meanwhile, the thickness or dimensions of each component shown in the drawings may be exaggerated for convenience of explanation and do not imply that it must actually be constructed according to the corresponding dimensions or ratios between components.
[0028] Referring to FIG. 1, an overview of the entire process according to one embodiment will be described.
[0029] The method for manufacturing valuable metals and chemical products from secondary battery wastewater using a circular integrated process according to the present invention relates to sodium sulfate (Na₂S) discharged from the secondary battery manufacturing process. High-value sulfuric acid (H₂) using SO₄-containing wastewater as a raw material It is a modular circular economy solution that produces SO₄), caustic soda (NaOH), and battery-grade valuable metals.
[0030] As illustrated in FIG. 1, the overall process of the present invention is largely composed of an impurity removal process in Module 1, a next-generation BPED (Bipolar Electrodialysis) system which is the main process, and a valuable metal recovery process in Module 2. Secondary battery wastewater is generated during the cleaning process, electrolyte purification process, and electrode plate formation process of the lithium-ion secondary battery manufacturing process, and generally exhibits acidity with a sodium sulfate concentration of 50 to 200 g / L and a pH in the range of 2 to 4.
[0032] Explain the components and characteristics of secondary battery wastewater.
[0033] In the present invention, the secondary battery wastewater to be treated contains, in addition to sodium sulfate which is the main component, nickel (Ni 2+ ), Cobalt(Co 2+ ), lithium (Li + ), manganese (Mn 2+ Valuable metal ions such as ) and calcium (Ca 2+ ), magnesium (Mg 2+ ), Iron (Fe 3+ ), Aluminum (Al 3+ It contains impurity ions such as ). The concentration of valuable metal ions is generally in the range of nickel 500 to 2,000 ppm, cobalt 200 to 800 ppm, lithium 100 to 500 ppm, and manganese 300 to 1,200 ppm.
[0034] Calcium and magnesium ions are of particular concern, with calcium ions present in concentrations of approximately 5 to 50 ppm and magnesium ions in concentrations of approximately 3 to 30 ppm. These calcium and magnesium ions form scales in the form of calcium sulfate (CaSO4) and magnesium sulfate (MgSO4) during the subsequent BPED process, which are the primary causes of rapid degradation in membrane performance. Scale formation generates insoluble precipitates on the membrane surface, hindering ion transport, increasing electrical resistance to reduce energy efficiency, and, in severe cases, can even lead to membrane failure.
[0036] The impurity removal process of Module 1 is described. The impurity removal process of Module 1 is a key pretreatment step for the stable operation of the subsequent BPED system and consists of a primary removal step and a secondary removal step.
[0037] The metal precipitation process of the first removal step is as follows.
[0038] In the first removal step, caustic soda (NaOH) is added to the secondary battery wastewater to precipitate valuable metals in the form of hydroxides. The amount of caustic soda added is determined to adjust the pH of the wastewater to a range of 8.5 to 11.0, and generally, 30 to 80 g of caustic soda is required per liter of wastewater.
[0039] During the pH adjustment process, nickel ions precipitate in the form of nickel hydroxide (Ni(OH)2); the pH at which precipitation begins is approximately 7.2, and the pH at which complete precipitation occurs is 9.5 or higher. Cobalt ions precipitate in the form of cobalt hydroxide (Co(OH)2); the pH at which precipitation begins is approximately 7.8, and the pH at which complete precipitation occurs is 10.0 or higher. Lithium ions precipitate in the form of lithium hydroxide (LiOH); however, due to their high solubility, they do not precipitate completely even at pH 12 or higher, requiring a separate recovery process. Manganese ions precipitate as manganese hydroxide (Mn(OH) 2 It precipitates in the form of ), with a precipitation start pH of about 8.5 and a complete precipitation pH of 11.0 or higher.
[0040] The precipitation reaction is carried out for 10 to 30 minutes at 300 to 500 rpm using a high-speed stirrer, and a polyacrylamide (PAM)-based coagulant may be added at a concentration of 0.1 to 1.0 ppm to promote the aggregation of the precipitate. The precipitated metal hydroxide is separated by gravity sedimentation or centrifugation, and a plate sedimentation tank or an inclined plate sedimentation tank may be used to increase the solid-liquid separation efficiency.
[0042] The precision removal of scaling ions in the second removal step is explained.
[0043] The second removal step is one of the core technologies of the present invention and is an enhanced pretreatment process that precisely removes calcium and magnesium ions from the solution obtained from the first removal step down to the ppb (parts per billion) level. Calcium and magnesium ions react with sulfuric acid in the BPED system to form calcium sulfate, which has low solubility (solubility 0.24 g / 100 mL at 20 Magnesium persulfate (solubility 35.1 g / 100mL at 20 It forms and becomes a major cause of membrane fouling.
[0044] As a method for removing scaling ions, at least one of an ion exchange resin, a chelating agent, or a selective precipitating agent is used. When an ion exchange resin is used, a strong acidic cation exchange resin (e.g., Amberlite IR-120, Dowex 50WX8) is used to replace calcium ions and magnesium ions with sodium ions. The exchange capacity of the resin is generally 1.8 to 2.2 eq / L, the contact time is 30 to 120 minutes, and the system is operated at a linear flow rate of 5 to 15 BV / h.
[0045] When using a chelating agent, calcium ions and magnesium ions are removed in the form of chelating complexes using EDTA (Ethylenediaminetetraacetic acid), DTPA (Diethylenetriaminepentaacetic acid), NTA (Nitrilotriacetic acid), etc. In the case of EDTA, it exhibits high selectivity with a complexing constant (log K) with calcium ions of 10.96 and a complexing constant with magnesium ions of 8.69. The amount of chelating agent injected is determined at a molar ratio of 1.2 to 2.0 times the concentration of the ions to be removed.
[0046] When using a selective precipitating agent, sodium phosphate (Na PO₄), sodium carbonate (Na₂O₄) Calcium and magnesium ions are precipitated in the form of insoluble salts using CO₃, sodium hydroxide (NaOH), etc. When sodium phosphate is used, calcium phosphate (Ca (PO₄)₂, solubility 0.002 g / 100mL) and magnesium phosphate (Mg It can be precipitated in the form of (PO₄)₂, solubility 0.0002 g / 100mL).
[0047] The goal of the second removal step is to lower the concentrations of calcium and magnesium ions to 1 ppb or less, thereby fundamentally preventing scaling in the subsequent BPED process. Real-time concentration measurements are performed using Inductively Coupled Plasma-Mass Spectrometry (ICP-MS) or Atomic Absorption Spectrometry (AAS) to monitor removal efficiency.
[0049] The configuration and principle of a BPED system according to one embodiment of the present invention will be described. As shown in FIG. 3, the BPED system according to this embodiment is an innovative system that combines a multi-stage stack configuration with a pulse / reverse potential operation method. Bipolar Electrodialysis (BPED) is an electrochemical separation technology that uses a bipolar membrane (BPM) to decompose salts into corresponding acids and bases.
[0051] The membrane configuration and arrangement of the BPED stack are described.
[0052] A BPED stack is configured by arranging a bipolar membrane (BPM), a cation exchange membrane (CEM), and an anion exchange membrane (AEM) in a specific order. In the present invention, the membranes are arranged in the order of BPM-CEM-AEM-CEM-BPM to form an acid compartment, a salt compartment, a base compartment, and a salt compartment.
[0053] A bipolar membrane (BPM) is a composite membrane in which a cation exchange layer and an anion exchange layer are bonded, and a water splitting reaction (H2O → H + OH) occurs at the interface. A cation exchange membrane (CEM) consists of sulfonic acid groups (-SO 3- It has negatively charged fixed ions such as ) or carboxylic acid groups (-COO), allowing only cations to pass through. Anion exchange membranes (AEMs) have positively charged fixed ions such as quaternary ammonium groups (-N(CH₃)₃) or tertiary amine groups (-NH(CH₃)₂), allowing only anions to pass through.
[0054] The physical properties of the membranes include a thickness of 200 to 300 μm for the anode membrane and thicknesses of 150 to 250 μm for the cation exchange membrane and anion exchange membrane, respectively. The ion exchange capacity of the membranes is in the range of 1.5 to 2.5 meq / g for the cation exchange membrane and 1.2 to 2.0 meq / g for the anion exchange membrane. The electrical resistance of the membranes is in the range of 15 to 35 Ω·cm² for the anode membrane, 3 to 8 Ω·cm² for the cation exchange membrane, and 4 to 10 Ω·cm² for the anion exchange membrane.
[0056] The principle and effect of a multi-stage stack configuration according to one embodiment will be explained.
[0057] The multi-stage stack configuration of the present invention consists of a 1st stage stack producing a low-concentration product, a 2nd stage stack producing a medium-concentration product, and a 3rd stage stack producing a high-concentration product, thereby progressively increasing the product concentration. The core principle of the multi-stage configuration is to apply appropriate current density and flow rate at each stage to stably produce a high-concentration product while optimizing energy efficiency.
[0058] In the single-stage stack, 3 to 8 wt% sulfuric acid and 2 to 6 wt% caustic soda are produced using the ultra-purified sodium sulfate solution (concentration 50 to 100 g / L) processed in Module 1 as a raw material. The operating conditions of the single-stage stack are a current density of 200 to 400 A / m², a linear flow rate of 2 to 5 cm / s, and a temperature of 25 to 35 am.
[0059] In the two-stage stack, 8 to 18 wt% sulfuric acid and 6 to 15 wt% caustic soda are produced using the intermediate concentration product produced in the first-stage stack as a raw material. The operating conditions of the two-stage stack are a current density of 300 to 600 A / m², a linear flow velocity of 1.5 to 4 cm / s, and a temperature of 30 to 40 am.
[0060] In the 3-stage stack, the product produced in the 2-stage stack is used as a raw material to produce sulfuric acid at a final target concentration of 15 to 30 wt% and caustic soda at 12 to 25 wt%. The operating conditions of the 3-stage stack are a current density of 400 to 800 A / m², a linear flow velocity of 1 to 3 cm / s, and a temperature of 35 to 45 am.
[0061] The main advantages of a multi-stage configuration are improved energy efficiency, enhanced product purity, and extended membrane life. Producing high-concentration products in a single stage requires a high current density, which leads to a sharp increase in energy consumption and accelerates membrane degradation. In contrast, with a multi-stage configuration, applying an appropriate current density at each stage can reduce overall energy consumption by 20 to 35%.
[0063] A pulse / reverse potential operation system according to one embodiment will be described with reference to FIG. 2. FIG. 2 is a schematic diagram of pulse / reverse potential operation, which is a core technology of the present invention, showing a voltage change pattern over time and cycles of forward operation and reverse operation, and specifically illustrating the product production effect during forward operation and the film cleaning and performance restoration effect during reverse operation along the time axis.
[0064] As illustrated in FIG. 2, the pulsed / reverse polarity operating system of the present invention is an innovative operating method that maintains membrane performance in an optimal state by periodically repeating forward operation and reverse operation.
[0065] In the forward operation phase, a DC voltage is applied from the anode to the cathode to decompose sodium sulfate into sulfuric acid and caustic soda. The forward operation time is 8 minutes, and the applied voltage is adjusted within the range of 10 to 25 V depending on the stack configuration. During forward operation, a water splitting reaction occurs at the interface of the anode membrane to generate hydrogen ions (H) and hydroxide ions (OH), sodium ions (Na) pass through the cation exchange membrane to move to the base chamber, and sulfate ions (SO*) pass through the anion exchange membrane to move to the acid chamber.
[0066] In the reverse operation stage, a voltage is applied in the opposite direction to the forward direction to remove contaminants accumulated on the membrane surface and resolve concentration polarization. The reverse operation time is 2 minutes, and the applied voltage is controlled within the range of 80 to 120% of the forward operation voltage. During reverse operation, the direction of ion movement is reversed, the concentration gradient on the membrane surface is alleviated, fine contaminants are desorbed, and membrane performance is restored.
[0067] The main effects of pulse / reverse potential operation are prevention of membrane fouling, alleviation of concentration polarization, and extension of membrane life. During continuous operation, concentration polarization intensifies at the membrane surface, and when the limiting current density is reached, the ion transfer efficiency decreases rapidly. By periodically relieving concentration polarization through reverse operation, the limiting current density can be improved by 20 to 40%.
[0069] The valuable metal recovery process of Module 2 is a value-added process that produces high-purity valuable metal products using the mixed hydroxide precipitate (MHP) precipitated in the primary removal stage of Module 1 as a raw material.
[0070] The valuable metal hydroxide sludge has a moisture content of 70 to 85% and contains 15 to 35% nickel, 8 to 25% cobalt, 10 to 30% manganese, and 2 to 8% lithium on a dry basis. The sludge re-dissolution is carried out using sulfuric acid produced in-house in the main process, thereby establishing a circular economy system.
[0071] The redissolution reaction is as follows:
[0072] · Ni(OH)2+ H2SO₄ → NiSO4+ 2H2O
[0073] · Co(OH)2+ H2SO₄ → CoSO4+ 2H2O
[0074] · Mn(OH)2+ H2SO₄ → MnSO4+ 2H2O
[0075] · 2LiOH + H2SO₄ → Li2SO4+ 2H2O
[0076] The redissolution conditions are a sulfuric acid concentration of 15 to 25 wt%, a temperature of 60 to 80°C, a stirring speed of 200 to 400 rpm, and a reaction time of 1 to 3 hours. The amount of sulfuric acid injected is calculated as an excess of 20 to 50% of the stoichiometric ratio with the metal hydroxide in the sludge. The redissolution rate is achieved at least 95% for nickel, at least 93% for cobalt, at least 90% for manganese, and at least 98% for lithium.
[0077] The solvent extraction separation process is explained. A solvent extraction process is applied to selectively separate each metal from a redissolved mixed metal solution. Solvent extraction is a technique that separates specific metals by utilizing a selective complexation reaction between an organic phase extractant and aqueous metal ions.
[0078] For nickel extraction, bis(2,4,4-trimethylpentyl)phosphinic acid (Cyanex 272) or 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester (PC-88A) is used. In the case of Cyanex 272, the partition coefficient for nickel is approximately 100 at pH 4.5, and the selectivity coefficient for cobalt is 5 to 15. The extraction conditions are an extractant concentration of 0.3 to 0.8 M, an osmotic ratio (O / A) of 1:1 to 2:1, a pH of 4.0 to 5.5, and a temperature of 25 to 35°C. am.
[0079] Bis(2,4,4-trimethylpentyl)phosphinic acid (Cyanex 272) or tri-n-octylphosphine oxide (TOPO) is used for cobalt extraction. Since cobalt is extracted at a lower pH than nickel, selective separation is possible through pH adjustment. The extraction conditions are an extractant concentration of 0.2 to 0.6 M, an ion-to-alpha ratio (O / A) of 1:1 to 1.5:1, a pH of 3.5 to 4.5, and a temperature of 25 to 35°C. am.
[0080] Di(2-ethylhexyl)phosphoric acid (D2EHPA) or bis(2,4,4-trimethylpentyl)phosphinic acid (Cyanex 272) is used for manganese extraction. Manganese is easy to separate because its extraction pH is higher compared to other metals. The extraction conditions are an extractant concentration of 0.5 to 1.0 M, an oxy-oxygen (O / A) ratio of 1:1 to 2:1, a pH of 5.5 to 7.0, and a temperature of 30 to 40°C. am.
[0081] Since lithium is difficult to extract with general organic extractants, tributyl phosphate (TBP) or crown ether-based extractants are used. Alternatively, ion exchange or selective precipitation methods can be applied instead of solvent extraction.
[0083] Explains crystallization and product production.
[0084] Each metal separated by solvent extraction is recovered as a high-purity aqueous solution through a stripping process and then produced as a final product through a crystallization process.
[0085] The crystallization of nickel sulfate (NiSO₄·6H₂O) involves a nickel sulfate solution with a nickel concentration of 80 to 120 g / L, 60 to 80 After concentrating in 20 to 30 It is performed by cooling. The crystallization yield is 85 to 95%, and the product purity is 99.5% or higher.
[0086] The crystallization of cobalt sulfate (CoSO₄·7H₂O) involves a cobalt sulfate solution with a cobalt concentration of 60 to 100 g / L at a concentration of 55 to 75 After concentrating in 15 to 25 It is performed by cooling. The crystallization yield is 80 to 90%, and the product purity is 99.3% or higher.
[0087] Manganese sulfate (MnSO₄H₂O) crystallization is performed by using a manganese sulfate solution with a manganese concentration of 100 to 150 g / L at a rate of 70 to 90 After concentrating in 25 to 35 It is performed by cooling. The crystallization yield is 75 to 85%, and the product purity is 99.0% or higher.
[0088] Lithium sulfate (Li SO₄H₂O) crystallization is performed on a lithium sulfate solution with a lithium concentration of 20 to 40 g / L in 80 to 100 0 to 10 after concentration in The process is carried out by cooling. Since the solubility of lithium sulfate varies significantly with temperature, cooling crystallization is effective. The crystallization yield is 70 to 80%, and the product purity is 99.0% or higher.
[0090] Referring to FIG. 3, the synergistic effect of the triple defense system is explained. FIG. 3 is a conceptual diagram of the triple defense structure of the BPED system of the present invention, conceptually illustrating the structure in which the first defense layer, enhanced pretreatment, the second defense layer, multi-stage process, and the third defense layer, pulse / reverse potential operation, protect the system from threats such as scaling ions, concentration polarization, and membrane fouling, centered around the central BPED system, as well as the functions and interactions of each defense layer.
[0091] As shown in FIG. 3, the triple defense system of the present invention is an integrated solution that perfectly protects the BPED system by organically combining enhanced pretreatment (first defense), multi-stage process (second defense), and pulse / reverse potential operation (third defense).
[0092] The enhanced pretreatment, which serves as the primary defense barrier, prevents membrane fouling by removing calcium and magnesium ions, the root causes of scaling, down to the ppb level. While conventional technology considered removal down to the ppm level to be sufficient, the present invention applies ultra-precision pretreatment that removes down to the ppb level for long-term stable operation.
[0093] The multi-stage process, acting as a secondary defense layer, distributes the load applied to the film by applying an appropriate current density at each stage and mitigates the concentration gradient on the film surface through a gradual increase in concentration. The multi-stage configuration effectively resolves the extreme concentration polarization and high electrical resistance that occur when producing high-concentration products in a single stage.
[0094] Pulse / reverse potential operation, which serves as the third layer of defense, maintains membrane performance in an optimal state by resolving minute membrane fouling and concentration polarization that may occur during operation in real time. While the first and second layers of defense block most risk factors in advance, the third layer continuously manages minute membrane degradation that inevitably occurs during long-term operation.
[0095] The synergistic effect of the three defense mechanisms extends beyond simple summation. If enhanced pretreatment fundamentally eliminates the critical risk of scaling, the multi-stage process and pulse / reverse potential operation can operate much more stably and efficiently. Similarly, if the multi-stage process distributes the membrane load, the cleaning effect of the pulse / reverse potential operation is maximized. Through this mutually complementary relationship, the stability and efficiency of the entire system are improved exponentially.
[0097] The process operating conditions and control system are explained.
[0098] The circular integrated process of the present invention ensures stable and efficient operation through optimized operating conditions and a precise control system for each module.
[0099] pH control is the most important variable in the primary removal stage of Module 1. For pH measurement, a combination electrode resistant to high temperature and high concentration brine is used, and measurement accuracy is maintained within ±0.05 pH unit. pH control is automatically controlled within a range of ±0.1 pH unit of the set value using a PID (Proportional-Integral-Derivative) controller.
[0100] The amount of caustic soda injected is calculated in real time based on the acidity and metal ion concentration of the raw wastewater. A metering pump is used for the caustic soda injection, and the flow rate accuracy is within ±1%. The stirring intensity is controlled by the impeller rotation speed, and changes in viscosity are monitored through torque measurement.
[0101] To monitor sedimentation efficiency, a turbidimeter is installed to measure the turbidity of the supernatant in real time. Sedimentation is considered complete when the turbidity is 10 NTU or less, and additional coagulant is injected if necessary.
[0102] In the second removal step, an ion-selective electrode (ISE) or inductively coupled plasma mass spectrometer (ICP-MS) is used to monitor calcium and magnesium ion concentrations online. If the target concentration (1 ppb or less) is not reached, the treatment time is automatically extended or additional treatment agent is injected.
[0103] The key control variables of the BPED system are current density, voltage, flow rate, temperature, and concentration. Current density is controlled independently for each stack and can be operated in constant current or constant voltage modes. Generally, the constant current mode is used to ensure stable product production.
[0104] Changes in membrane resistance are detected in real time through voltage monitoring. If the membrane resistance increases by more than 150% of the initial value, it is determined that membrane fouling has occurred, and the reverse operation time is extended or chemical cleaning is performed. The membrane resistance is calculated from voltage and current measurements using Ohm's Law (V = IR).
[0105] Flow rate control is performed independently for each compartment using a mass flow meter with an accuracy of ±2%. Since the flow rates in the acidity and base chambers directly affect product concentration, they are controlled with particular precision.
[0106] Temperature control is performed using an external cooling / heating system utilizing heat exchangers and circulation pumps. Temperature sensors are installed at the inlet and outlet of each stack, with a temperature deviation of ±2 It is controlled so as not to exceed. While a rise in temperature is beneficial for improving film performance and reducing electrical resistance, excessive temperature accelerates film degradation, so the optimal point must be maintained.
[0107] Concentration monitoring is performed using conductivity meters and pH measurements. Sulfuric acid concentration is estimated using the correlation between conductivity and pH, and titration is performed periodically to ensure accurate concentration measurements. Similarly, caustic soda concentration is monitored through conductivity and pH measurements.
[0108] Pulse / reverse potential operation is operated by an automatic control system using a programmable logic controller (PLC). The basic cycle of 8 minutes for forward operation and 2 minutes for reverse operation can be adjusted according to operating conditions. If the rate of increase in film resistance is high, the reverse operation time can be extended to 3 to 5 minutes, and if film performance is good, the forward operation time can be extended to 10 to 12 minutes.
[0109] Voltage switching is completed within 1 second using an IGBT (Insulated Gate Bipolar Transistor) module capable of high-speed switching. Ramping control is applied to prevent transients that may occur during voltage switching.
[0110] To quantitatively evaluate the effect of reverse operation, film resistance and current efficiency are measured after each cycle. If the film resistance decreases to 95% or less compared to the previous cycle, it is determined that reverse operation has been performed effectively.
[0111] sulfuric acid (H₂) produced The concentration of SO₄ is in the range of 15 to 30 wt%, and the purity is targeted to be 98% or higher. The sulfuric acid concentration is measured using a combination of the specific gravity method and the titration method. The specific gravity method is monitored in real-time using an online densimeter, while the titration method measures the accurate concentration through acid-base titration using a standard sodium hydroxide solution.
[0112] Atomic absorption spectroscopy (AAS), inductively coupled plasma emission spectroscopy (ICP-OES), and ion chromatography (IC) are used for impurity analysis. Major impurities are controlled to be sodium (Na) 100 ppm or less, chlorine (Cl) 50 ppm or less, nitrogen compounds (NO) 20 ppm or less, and heavy metals (Fe, Cu, Ni, etc.) 10 ppm or less each.
[0113] To prevent microbial contamination of sulfuric acid, the inorganic and organic content are measured. The total organic carbon (TOC) content is maintained at 50 ppm or less, and organic matter is removed through activated carbon filtration or ozone treatment if necessary.
[0115] Explain process optimization and scalability.
[0116] The circular integrated process of the present invention provides excellent scalability by adopting a modular design that can be applied to various scales and conditions.
[0117] Process optimization uses multi-objective optimization techniques to simultaneously consider product purity, energy efficiency, and economic feasibility. Key optimization variables include the current density, flow rate, temperature, and concentration of the BPED system, as well as the cycle time of pulse / reverse potential operation.
[0118] The influence of each variable is analyzed using Design of Experiments (DOE), and optimal operating conditions are derived by applying Response Surface Methodology (RSM). Through statistical analysis, significant variables at a 95% confidence level are selected, and a process model is constructed based on this.
[0119] A Model Predictive Control (MPC) system is introduced for real-time optimization. Based on the current state, MPC predicts future process behavior and calculates control inputs that optimize the set objective function. This ensures robustness against disturbances and maximizes operational efficiency.
[0121] Although preferred embodiments of the present invention have been described above, the technical concept of the present invention is not limited to the preferred embodiments described above and can be implemented in various ways within the scope that does not depart from the technical concept of the present invention as embodied in the claims. Explanation of the symbols
[0122] doesn't exist
Claims
Claim 1 A method for manufacturing valuable metals and chemical products from secondary battery wastewater containing sodium sulfate (Na2SO₄), comprising: a first removal step of adding caustic soda (NaOH) to the secondary battery wastewater to precipitate and remove valuable metals including nickel and cobalt in the form of hydroxides; and a solution obtained from the first removal step in which calcium ions (Ca 2+ ) and magnesium ions (Mg 2+ A secondary removal step for removing scaling-inducing ions, including ) to ppb levels; an electrolysis step for producing sulfuric acid (H2SO₄) and caustic soda (NaOH) by feeding the ultrapurified sodium sulfate solution obtained from the secondary removal step into a multi-stage bipolar electrodialysis (BPED) stack; A method for manufacturing valuable metals and chemical products from secondary battery wastewater using a circular integrated process comprising: a metal recovery step in which the valuable metal hydroxide sludge precipitated in the first removal step is redissolved with sulfuric acid produced in the electrolysis step, and then high-purity valuable metals are recovered through solvent extraction and crystallization; wherein the multi-stage bipolar electrodialysis (BPED) stack comprises a first-stage stack that produces a low-concentration product, a second-stage stack that produces a medium-concentration product, and a third-stage stack that produces a high-concentration product, thereby progressively increasing the product concentration, wherein the second-stage stack uses the product produced in the first-stage stack as a raw material and the third-stage stack uses the product produced in the second-stage stack as a raw material. Claim 2 A manufacturing method according to claim 1, performed by a pulse / reverse potential operation method that periodically repeats: a forward operation in which a forward voltage is applied to decompose sodium sulfate into sulfuric acid and caustic soda; and a reverse operation in which a reverse voltage is applied after the forward operation to clean the membrane surface and relieve concentration polarization. Claim 3 A manufacturing method according to paragraph 2, wherein 8 minutes of forward operation and 2 minutes of reverse operation are repeatedly performed as one cycle. Claim 4 delete Claim 5 A method for manufacturing, wherein, in claim 1, calcium ions and magnesium ions are removed to 1 ppb or less using at least one of an ion exchange resin, a chelating agent, or a selective precipitating agent. Claim 6 A manufacturing method according to claim 1, wherein a bipolar membrane (BPM), a cation exchange membrane (CEM), and an anion exchange membrane (AEM) are sequentially arranged to form an acid chamber, a salt chamber, and a base chamber. Claim 7 A method for manufacturing, wherein the high-purity valuable metal recovered in the metal recovery step is in the form of at least one sulfate crystal among nickel sulfate (NiSO4), cobalt sulfate (CoSO4), lithium sulfate (Li2SO4), and manganese sulfate (MnSO4). Claim 8 A method of manufacturing according to claim 1, wherein the concentration of sulfuric acid produced in the electrolysis step is 10 to 30 wt% and the concentration of caustic soda is 8 to 25 wt%. Claim 9 A manufacturing method according to claim 1, wherein the caustic soda produced in-house during the electrolysis step is circulated. Claim 10 A method for manufacturing, wherein the secondary battery wastewater is wastewater discharged from a lithium-ion secondary battery manufacturing process, and has a sodium sulfate concentration of 50 to 200 g / L.
Citation Information
Patent Citations
Electrochemical production of alkali metal hydroxides and sulfuric acid by battery manufacturing and waste stream recycling