A method for manufacturing a secondary battery
The CC-CV discharge process in lithium-sulfur battery activation addresses LiPS shuttling by converting inactive LiPS to Li2S, enhancing capacity and lifespan while reducing process time.
Patent Information
- Application Number
- KR1020230161212
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-18
- Filing Date
- 2023-11-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-11-20
AI Technical Summary
The lithium-sulfur battery activation process is hindered by lithium polysulfide (LiPS) shuttling, leading to anode degradation, capacity loss, and reduced cell performance due to non-uniform LiPS distribution and irreversible reactions.
A method involving a CC-CV discharge process for battery activation, where the preliminary battery is discharged in a constant current and constant voltage sequence, with specific voltage and current ranges, to convert remaining LiPS into Li2S, ensuring uniform distribution and reducing overvoltage effects.
This method enhances battery capacity, improves lifespan performance, and shortens the manufacturing process by converting inactive LiPS, thereby stabilizing the anode and improving overall electrochemical performance.
Smart Images

Figure 112023129159118-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for manufacturing a secondary battery, and more specifically, to a method for the initial discharge of the battery activation process.
[0002] This application is a priority claim application for Korean Patent Application No. 10-2022-0155730 filed on November 18, 2022, and all contents disclosed in the specification of said application are incorporated into this application by reference. Background Technology
[0004] Recently, interest in energy storage technology has been steadily increasing. As application fields expand to include energy for mobile phones, camcorders, laptop PCs, and even electric vehicles, efforts in the research and development of electrochemical devices, such as secondary batteries, are becoming increasingly concrete. Electrochemical devices are the most 주목받는 field in this regard, and among them, the development of rechargeable secondary batteries is the focus of attention. Recently, research and development in developing such batteries has been proceeding toward the design of new electrodes and batteries to improve capacity density and specific energy.
[0005] Among these secondary batteries, lithium-sulfur batteries are gaining attention as high-energy-density secondary batteries due to their high energy density, achieved through a lightweight lithium anode and a sulfur cathode with high discharge capacity.
[0006] In lithium-sulfur batteries, sulfur serves as the starting material for the reaction during discharge, with the cyclic structure of S8 acting as the initiator. As discharge progresses, the process involves the stages of lithium polysulfides (LiPS: Li2S8, Li2S6, Li2S5, Li2S4), which are linear structures of a continuous reduction reaction. These polysulfides, dissolved in the electrolyte, move from the anode to the cathode and are sequentially reduced to lower monomer polysulfides. These negatively charged polysulfides dissolve in the liquid organic solvent and migrate toward the cathode based on chemical potential and the concentration gradient between the anode and cathode. Ultimately, they produce the insoluble reduced substance Li2S (S8 + 16Li → 8Li2S). During charging, the oxidation reaction occurs in the reverse order of the above sequence, returning to the original substance S8, thereby triggering a "shuttle" mechanism. In lithium-sulfur batteries possessing these mechanistic characteristics, the activation process prior to the life cycle is a critical step that ensures sufficiently uniform distribution of LiPS within the electrolyte around the anode, thereby suppressing additional resistance variables during life evaluation operations. During this process, lithium polysulfide (LiPS) shuttlering affects overall cell performance degradation and can have a particularly severe impact on anode degradation. During the discharge process, sulfur is reduced to lithium polysulfides (Li2Sn, where 4 <n<8)가 되며, 이 중간 생성물이 전해질에 녹아나와 확산되면서 문제를 발생시킨다. 리튬폴리설파이드는 리튬금속인 음극 표면에서 셔틀효과로 인한 용량감소를 일으키고 일부는 부도체인 리튬설파이드(Li2S2, Li2S)로 환원되어 활물질 손실 및 리튬이온의 이동을 방해하여 율속 특성을 저하시킨다. 이러한 부반응은 쿨롱효율의 감소와 음극의 불안정으로 이어져 전반적인 전지의 성능을 저하시킨다. 이에 리튬-황 전지의 신규 활성화 공정을 확립하여 전지 제조시 적용할 필요가 있다. The problem to be solved
[0008] The present invention aims to provide a method for manufacturing a lithium-sulfur battery to solve the aforementioned problems, in particular a method for manufacturing a battery comprising a novel battery activation process. It will be readily apparent that other objects and advantages of the present invention can be realized by means or methods and combinations thereof as described in the claims. means of solving the problem
[0010] The first aspect of the present invention relates to a method for manufacturing a lithium-sulfur battery, wherein the method comprises the steps of: (S10) manufacturing a preliminary battery comprising an electrode assembly and an electrolyte; and
[0011] (S20) An activation step for activating the above-mentioned preliminary battery; comprising,
[0012] The electrode assembly comprises a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode comprises a positive active material containing sulfur, and
[0013] In the above (S10), the electrode assembly is impregnated with the electrolyte, and
[0014] The above step (S20) includes the step of discharging the reserve battery, wherein the discharge is performed in the order of constant current discharge and constant voltage discharge after the constant current discharge.
[0015] A second aspect of the present invention is that, in the first aspect, the constant current discharge in step (S20) is performed until a preset discharge termination voltage is reached, and the discharge termination voltage is set within the range of 1.3V to 1.8V.
[0016] A third aspect of the present invention is that, in the second aspect, the constant current discharge in step (S20) is performed at a rate set within the range of C rate 0.05 to 2 until a preset discharge termination voltage is reached.
[0017] The fourth aspect of the present invention is that, in any one of the second and third aspects, the constant voltage discharge is performed until the remaining current of the battery reaches 0 mAh at a preset discharge termination voltage.
[0018] A fifth aspect of the present invention is that, in any one of the first to fourth aspects, the reserve battery is not charged or discharged prior to the execution of step (S20), and discharge is applied for the first time to the reserve battery during charging and discharging in step (S20).
[0019] The sixth aspect of the present invention is that, in any one of the second to fifth aspects, the reserve battery is not charged or discharged before the step (S20) is performed, and the step (S20) consists only of discharging the reserve battery once.
[0020] The seventh aspect of the present invention is that in any one of the first to sixth aspects, the discharge is performed less than six times in step (S20).
[0021] The eighth aspect of the present invention is that, in any one of the first to seventh aspects, the constant current discharge in step (S20) is performed at a rate (C Rate) in the range of 0.05 to 2.00.
[0022] The ninth aspect of the present invention is that, in any one of the first to eighth aspects, the discharge in step (S20) is performed in a constant current manner up to a preset discharge termination voltage.
[0023] The tenth aspect of the present invention is that, in any one of the first to ninth aspects, the discharge in step (S20) is performed at a rate (C Rate) in the range of 0.50 to 1.00.
[0024] The eleventh aspect of the present invention is that in any one of the first to ten aspects, the step (S20) is performed in an environment where the preliminary battery is pressurized.
[0025] The 12th aspect of the present invention is that, in the 11th aspect, the pressure applied is greater than or equal to atmospheric pressure.
[0026] The 13th aspect of the present invention is that in any one of the 1st to 12th aspects, the step (S20) is performed at a temperature of 15°C to 40°C.
[0027] The 14th aspect of the present invention is that, in any one of the 1st to 13th aspects, an aging step is further performed in which the preliminary battery is maintained in an atmosphere of 15°C to 40°C after performing step (S10) and before performing step (S20).
[0028] The 15th aspect of the present invention is that, in any one of the 1st to 14th aspects, a charging process is performed between the discharge processes in step (S20), and the charging is performed in the order of constant current charging and constant voltage charging after the constant current charging. Effects of the invention
[0030] The battery manufacturing method according to the present invention can reduce the number of charge-discharge cycles during the battery activation process and shorten the time required for the battery manufacturing process by adding a CV section. In addition, the battery manufacturing method can improve the electrochemical performance of the battery, such as improving battery capacity, by converting the remaining LiPS that failed to undergo a complete phase change due to overvoltage into its final form as much as possible and reducing the overvoltage to uniformly distribute the LiPS around the anode. Brief explanation of the drawing
[0032] The drawings attached to this specification illustrate preferred embodiments of the present invention and serve to help to better understand the technical concept of the present invention together with the description of the invention above; therefore, the present invention is not to be interpreted as being limited only to the matters described in such drawings. Meanwhile, the shape, size, scale, or ratio of elements in the drawings included in this specification may be exaggerated to emphasize a clearer explanation. Figure 1 shows a comparison of the high-rate discharge characteristics of batteries according to the examples and comparative examples. Figure 2 shows a comparison of the Coulomb efficiency characteristics of batteries according to the examples and comparative examples. Figure 3 shows a comparison of the power density of batteries according to the SOC ranges in the examples and comparative examples. Specific details for implementing the invention
[0033] The present invention will be described in detail below. Terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept consistent with the technical spirit of the present invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention. Accordingly, the embodiments described in this specification and the configurations illustrated in the drawings are merely one preferred embodiment of the present invention and do not represent all of the technical spirit of the present invention; therefore, it should be understood that various equivalents and modifications capable of replacing them may exist at the time of filing this application.
[0035] Throughout this specification, when a part is described as 'include, comprise,' 'have,' or 'possess' a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0037] Additionally, terms such as “about,” “substantially,” as used throughout this specification, are used to mean at or near the stated value when inherent manufacturing and material tolerances are presented in the said sense, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute values are mentioned to aid in understanding this invention.
[0039] Throughout this specification, the description of 'A and / or B' means 'A or B or both'.
[0041] Specific terms used in the following detailed description are for convenience only and are not restrictive. The words 'right', 'left', 'top', and 'bottom' indicate directions in the referenced drawings. The words 'inward' and 'outward' indicate directions toward or away from the geometric center of the specified device, system, and its components, respectively. 'Forward', 'rear', 'upward', 'downward', and related words and phrases indicate positions and orientations in the referenced drawings and should not be restrictive. These terms include the words listed above, their derivatives, and words of similar meaning.
[0043] Method for manufacturing a secondary battery
[0044] The present invention relates to a method for manufacturing a secondary battery, specifically a method for manufacturing a lithium-sulfur secondary battery.
[0045] Specifically, the method for manufacturing a lithium-sulfur secondary battery according to the present invention comprises the steps of manufacturing a preliminary battery comprising an electrode assembly and an electrolyte, and activating the preliminary battery. The battery manufacturing method may include a degassing step for removing gas generated during the activation step. The electrode assembly comprises a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the positive electrode comprises a positive electrode active material containing sulfur, and the electrode assembly is prepared by impregnating it with the electrolyte prior to performing the activation step. Furthermore, in the present invention, the activation step of the battery manufacturing method comprises the step of discharging the preliminary battery, and the discharge is characterized by being performed in the order of constant current (CC) discharge and constant voltage (CV) discharge after the constant current discharge.
[0047] As described above, by performing a CC-CV discharge step during the activation process, the remaining LiPS that failed to undergo a complete phase change due to overvoltage can be converted into its final form as much as possible. Accordingly, capacity is increased compared to conventional lithium-sulfur batteries, and excellent lifespan performance can be secured. In addition, the process time can be shortened, and safety is improved.
[0049] Next, the method for manufacturing a lithium-sulfur battery according to the present invention will be described in detail for each process.
[0051] <S10 예비 전지의 제조>
[0052] First, a preliminary battery including an electrode assembly and an electrolyte is manufactured (S10).
[0054] In the present specification, the above-mentioned preliminary battery refers to a battery in a state where the formation process has not been completed. In the present invention, the above-mentioned formation process may refer to a battery shipment preparation process that includes activation and degassing processes after the electrolyte is injected.
[0056] The electrode assembly comprises a cathode, an anode, and a separator disposed between the cathode and the anode. Details regarding the cathode, anode, and separator will be described later.
[0058] The method for manufacturing a secondary battery according to the present invention includes the step of impregnating the electrode assembly with an electrolyte. After the electrode assembly is impregnated with the electrolyte, it may be activated by a discharge as described below. The electrolyte may include an organic solvent and a lithium salt. Detailed information regarding the organic solvent and the lithium salt will be described later.
[0060] The above impregnation is intended to sufficiently wet the electrode assembly with the electrolyte and to enable smoother activation during charging and discharging of the electrode assembly. The impregnation with the electrolyte can be performed, for example, by housing the electrode assembly in a battery case, injecting the electrolyte into the battery case, and maintaining it at a predetermined temperature for a predetermined time. For example, it can be maintained for 12 to 100 hours, more preferably 24 to 75 hours, after injecting the electrolyte to allow the electrolyte to permeate into the interior of the electrode assembly. (Aging step)
[0062] The impregnation of the electrode assembly can be performed at 15°C to 30°C, more specifically at 20°C to 27°C. It is desirable that the impregnation of the electrode assembly can be improved within this range, and that concerns regarding the formation of dendrites in the cathode due to excessively high temperatures and the resulting low voltage generation can be prevented.
[0064] Meanwhile, in the present invention, the electrode assembly may be manufactured by conventional methods known in the art, and the shape of the electrode assembly is not particularly limited and may be, for example, a wound type, a stacked type, or a stacked / folded type.
[0066] The above-mentioned wound electrode assembly is manufactured by coating an electrode active material, etc., onto a current collector, drying and pressing it, cutting it into a band shape of a desired width and length, separating the negative and positive electrodes using a separator, and then winding it spirally.
[0068] The above-described stacked electrode assembly has a structure in which a plurality of positive and negative unit cells are sequentially stacked. While it has the advantage of being easy to obtain a rectangular shape, it has the disadvantages of a cumbersome manufacturing process and the electrodes shifting when subjected to impact, thereby causing a short circuit.
[0070] Accordingly, as an advanced electrode assembly having a mixed form of the aforementioned winding type and stacking type, it is an electrode assembly having a structure in which full cells or bi-cells of a certain unit size are folded using a long continuous separating film. An electrode assembly with such a structure is a composite structure of the existing folding type and stacking type, and is referred to as a 'stacked / folding type electrode assembly'.
[0071] The above 'full cell' is a unit cell composed of a unit structure of an anode, a separator, and a cathode, wherein the anode and the cathode are located on opposite sides of the cell. Examples of such full cells include the most basic structure of an anode / separator / cathode cell and an anode / separator / cathode / separator / anode / separator / cathode cell. To construct an electrochemical cell using such full cells, a plurality of full cells must be stacked so that the anode and the cathode face each other with a separator film interposed between them.
[0073] The above 'bicell' is a unit cell in which identical electrodes are located on both sides of the cell, such as a unit structure of anode / separator / cathode / separator / anode and a unit structure of cathode / separator / anode / separator / cathode. In order to form an electrochemical cell using such a bicell, a plurality of bicells must be stacked such that a bicell with an anode / separator / cathode / separator / anode structure (anode bicell) and a bicell with a cathode / separator / anode / separator / cathode structure (cathode bicell) face each other with a separator film interposed therein. In some cases, a greater number of stacked bicells is also possible.
[0075] Meanwhile, in one embodiment of the present invention, a degassing process to remove gas generated inside the battery after the electrolyte impregnation process and before performing the activation process may be performed.
[0077] <S20 예비 전지의 활성화>
[0078] An activation process is performed on the preliminary battery obtained above. Meanwhile, in this specification, the term "activation" refers to a process of supplying a predetermined amount of electricity to an electrode assembly or battery cell that does not possess electrical characteristics, thereby causing the positive and negative electrodes to acquire electrical characteristics. Through the activation process, reactions such as the formation of an SEI film, partial charging of the battery capacity, and, in the case of using a carbon-based negative electrode active material, lithiation of the negative electrode may occur.
[0080] Meanwhile, in the present invention, the pre-cell is in a state where charging and discharging have not been performed prior to the activation process after impregnation with an electrolyte. More preferably, in the present invention, the activation process involves applying the first discharge during charging and discharging to the pre-cell.
[0082] In the present invention, the activation process may be performed by discharging the pre-cell prepared in step (S10) only once.
[0084] Alternatively, the above activation process may repeat charging and discharging after the initial discharge process is applied, and in this case, it is preferable that the above activation process be performed with fewer than 6 discharges.
[0085] In a more preferred embodiment of the present invention, the discharge is performed in the order of a constant current (CC) discharge followed by a constant voltage (CV) discharge. If the discharge is performed two or more times in the activation process, at least one discharge is performed in the order of a constant current discharge followed by a constant voltage discharge. In this case, it is preferable that the first discharge be performed in the order of a constant current discharge followed by a constant voltage discharge. In another embodiment, all discharges performed in the activation step may be performed in the order of a constant current discharge followed by a constant voltage discharge.
[0086] If constant voltage discharge is performed first, instantaneous overcurrent occurs in the lithium-sulfur battery, causing damage to the cell and leaving a significant amount of unreacted active material, so in the present invention, it is preferable to perform constant voltage discharge after constant current discharge.
[0088] The above constant current discharge can be performed until a preset discharge termination voltage is reached, and the discharge termination voltage can be set within the range of 1.3V to 1.8V.
[0090] In the above step (S20), the constant current discharge may be performed at a rate set within the range of C rate 0.05 C to 2.00 C or 0.50 C to 1.00 C until a preset discharge termination voltage is reached.
[0092] The above constant voltage discharge can be performed from a preset discharge termination voltage until a charge termination current is reached. In a specific embodiment, the discharge may be terminated when the charge termination current reaches a point where the remaining current of the battery is 0 mAh.
[0094] In another embodiment, the constant voltage mode may be performed for at least about 20 minutes, at least about 1 hour, at least about 2 hours, or at least about 4 hours at a discharge termination voltage of 1.3V to 1.8V. Meanwhile, the time of the constant voltage discharge is preferably within a range that does not cause excessive over-discharge, and does not exceed 6 hours.
[0096] In this way, when the battery activation process is initiated by discharge and the discharge is performed using the CC-CV method, the battery capacity can be increased by activating even the remaining inactive LiPS that failed to undergo a complete phase change due to overvoltage. Furthermore, since the activation process is simplified by the discharge method described above, the process time can be shortened compared to the conventional activation process that proceeds in the order of charge and discharge. In addition, lifespan characteristics similar to those of batteries manufactured by the conventional activation process can be secured.
[0098] Meanwhile, in one embodiment of the present invention, the step (S20) may be performed in an environment where the preliminary battery is pressurized. It is preferable that the pressurization be applied at a pressure greater than atmospheric pressure. The term 'atmospheric pressure' refers to pressure without applying separate pressurization or depressurization equipment. For example, it may refer to approximately 1 atm, which is a typical atmospheric condition. The pressurization is applied in terms of performing a safe process, and specifically, the impregnated electrode assembly may be fastened between two pressurization jigs or pressurization plates and the impregnated electrode assembly may be pressurized.
[0099] The above pressure range may be performed by applying pressure, for example, from 1 atm to 15 atm, more specifically from 4 atm to 10 atm. When applying pressure within the above pressure range, it is desirable to prevent volume expansion and deformation of the cathode, thereby allowing lithium to be inserted into the cathode stably and uniformly. Meanwhile, the above activation process may be performed at 15°C to 40°C, or 20°C to 30°C. Within this range, the mobility of lithium is improved, preventing localized insertion of lithium into the electrode and enabling uniform charging.
[0101] Meanwhile, in the present invention, a charging process may be performed between the discharge processes in (S20), and when the charging process is performed, the charging may be performed in the order of constant current charging and constant voltage charging after the constant current charging.
[0103] The above charging can be performed by charging the electrode assembly such that the state of charge (SOC) of the electrode assembly is 40% or more. Specifically, in order to prevent excessive volume expansion of the negative electrode active material (e.g., silicon-based active material) and deformation of the negative electrode during charging, and to prevent the formation of overvoltage of the negative electrode due to excessive charging and the resulting decrease in potential of the negative electrode, thereby preventing the reduction and precipitation of lithium, the above charging can be performed by charging the electrode assembly such that the state of charge of the electrode assembly is 60% to 90%, more preferably 70% to 85%.
[0105] <S30 탈기>
[0106] In one embodiment of the present invention, after performing the activation process, a degassing process can be performed to remove residual gas in the battery.
[0107] Gas may be generated as a byproduct due to the formation of an SEI layer or the generation of irreversible capacity after the activation of the above-mentioned battery. Accordingly, a process to remove the byproduct may be performed to use the activated secondary battery, and the secondary battery may be manufactured into a usable form through the gas removal process. The step of removing the gas may be performed using any method generally used in the field of secondary batteries without limitation. For example, the step of removing the gas may be performed by partially opening a case housing the electrode assembly to remove the gas and then sealing it.
[0109] Electrode Assembly
[0110] In one embodiment of the present invention, the electrode assembly may include a cathode, an anode, and a separator interposed between the cathode and the anode.
[0112] The electrode assembly is loaded into a battery case together with an electrolyte, and the case is sealed. In one embodiment of the present invention, the battery case is made of a metal material and may be a rectangular case or a cylindrical case.
[0114] The electrode assembly comprises a cathode, an anode, and a separator, and may have a stacked form with a separator interposed between the cathode and the anode. The method of manufacturing the electrode assembly is not particularly limited and may be performed according to known methods. Furthermore, the electrode assembly is not particularly limited as long as it has a structure comprising a cathode, an anode, and a separator interposed between the cathode and the anode, and may, for example, be a jelly-roll type, a stack type, or a stack / folding type structure.
[0116] <Cathode>
[0117] In a specific embodiment of the present invention, the cathode may include a current collector and a cathode active material layer formed on the surface of the current collector. According to a specific embodiment of the present invention, the cathode active material layer comprises a cathode active material and may further include a binder and a conductive material as needed.
[0118] In one embodiment of the present invention, the negative electrode active material is lithium metal; Li x Fe2O3(0≤x≤1), Li x WO2(0≤x≤1), Sn x Me 1-x Me y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, Group 1, 2, and 3 elements of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬과 이종 금속이 합금화된 리튬 합금; 규소계 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물; 리튬 티타늄 산화물; 탄소계 재료로 이루어진 군에서 선택된 1종 또는 이 중 2종 이상의 혼합물을 포함할 수 있다. 상기 리튬 합금에서 이종 금속은 Al, Mg 중 선택된 1종 이상을 포함할 수 있다. 한편, 상기 탄소계 재료는 결정질 인조 흑연, 결정질 천연 흑연, 비정질 하드 카본, 저결정질 소프트카본, 카본 블랙, 아세틸렌 블랙, 그래핀 및 섬유상 탄소로 이루어진 군으로부터 선택되는 하나 이상일 수 있다. 바람직하게는 본 발명에 있어서, 상기 음극 활물질은 리튬 금속 또는 리튬 합금일 수 있다.
[0120] In one embodiment of the present invention, the negative electrode active material may be lithium metal or an alloy of lithium and a heterogeneous metal, wherein the negative electrode active material layer may be prepared in the form of a thin film containing said metal and the negative electrode may be formed by laminating it with a current collector. The lamination may be performed by applying pressure, and the current collector and the thin film may be heated to a temperature above room temperature when pressure is applied. Additionally, the lamination may be performed by applying a roll press method.
[0122] In one embodiment of the present invention, the negative current collector may be any negative current collector commonly used in the art, such as copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy. The negative current collector may typically have a thickness of 3 to 500 μm, and, similar to the positive current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding force of the negative active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric. For example, when a current collector in the form of a metal thin film is used, the thickness of the current collector may be 1 μm to 20 μm.
[0124] <Polar>
[0125] The above lithium-ion secondary battery is a lithium-sulfur battery. The positive electrode according to the present invention comprises a current collector and a positive electrode active material layer disposed on at least one surface of the current collector.
[0126] The above current collector may be any material used in the relevant technical field that has electrical conductivity and serves as a current collection component. For example, the above positive current collector may be stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. The above positive current collector may typically have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the above positive current collector to increase the adhesion of the positive active material. The above positive current collector may be used in various forms, such as films, sheets, foils, nets, porous materials, foams, nonwoven materials, etc.
[0128] In one embodiment of the present invention, the positive active material layer comprises a positive active material, a conductive material, and a binder material. Based on the total weight of the positive active material, the conductive material, and the binder material, the positive active material may be included in a ratio of 80 to 97 wt%, the conductive material in a ratio of 2 to 10 wt%, and the binder in a ratio of 2 to 10 wt%.
[0130] In the present invention, the positive electrode active material comprises a sulfur-carbon composite. Preferably, the positive electrode active material may comprise 80 wt% or more, preferably 90 wt% or more, of the sulfur-carbon composite relative to 100 wt% of the positive electrode active material, and more preferably, the positive electrode active material may consist solely of the sulfur-carbon composite. Additionally, it is preferable that the sulfur content relative to 100 wt% of the sulfur-carbon composite be 70 wt% or more.
[0131] In one embodiment of the present invention, the sulfur-carbon composite may be formed by simply mixing the sulfur and the carbon material, or may have a core-shell structured coating or support form. The core-shell structured coating form is one in which either the sulfur or the carbon material is coated with another material; for example, the surface of the carbon material may be coated with sulfur or vice versa. The carbon material may have a porous structure having pores inside and on the surface of the body, and may be in a form in which sulfur is filled into the internal pores. The form of the sulfur-carbon composite may be any form that satisfies the content ratio of the sulfur-based compound and the carbon material described below, and is not limited in the present invention. Meanwhile, in the present invention, it is preferable that the sulfur content be 70% by weight or more relative to the total weight of the cathode active material.
[0132] Since the aforementioned sulfur alone does not conduct electricity, it is used in combination with carbon materials.
[0133] In one embodiment of the present invention, the sulfur is inorganic sulfur (S8), Li2S n (n≥1), disulfide compounds such as 2,5-dimercapto-1,3,4-thiadiazole, 1,3,5-trithiocyanuic acid, organic sulfur compounds, and carbon-sulfur polymers ((C2S x ) n It may be one or more selected from the group consisting of x=2.5 to 50, n≥2). Preferably, it may include inorganic sulfur (S8).
[0134] The above carbon material has a porous structure containing numerous irregular pores on the surface and within, and acts as a support providing a framework for uniformly and stably immobilizing sulfur, and compensates for the low electrical conductivity of sulfur to enable the electrochemical reaction to proceed smoothly. In particular, in a sulfur-carbon composite, the carbon material acting as a sulfur support has a large BET specific surface area and an appropriate particle size (D 50 When it has a size, the loading amount of sulfur is high, while the irreversible capacity is low and the energy density is increased, which can increase the utilization rate of sulfur during electrochemical reactions.
[0135] In one embodiment of the present invention, the BET specific surface area of the carbon material is at least 100 m² 2 It can be more than / g, up to 3000m 2 It may be / g. In conjunction with or independently thereof, the carbon material has a particle size (D) of the primary particles. 50 ) can be 1㎛ to 50㎛.
[0136] BET specific surface area and particle size (D) of the above carbon material 50 By satisfying the above range, sulfur can be uniformly dispersed on the inner and outer surfaces of the carbon material, while the irreversible capacity is lowered, thereby increasing the electrochemical reactivity of sulfur. In addition, the use of the carbon material improves the electrochemical reactivity, stability, and electrical conductivity of the sulfur-carbon composite, which not only improves the capacity and lifespan characteristics of the lithium-sulfur battery but also enables optimal charge-discharge performance even if sulfur loss or volume change occurs during charge-discharge.
[0137] The above primary particle diameter (D 50 If ) exceeds 50㎛, the movement of lithium ions into the interior of the particle is difficult due to restrictions on mass transfer, making it difficult to efficiently utilize the sulfur located at the carbon center. Primary particle diameter (D 50When the particle size is less than 1㎛, it is difficult to increase the solid content because a large amount of solvent is required during the electrode slurry preparation process, and there is a problem of reduced output because sufficient inter-particle pores are not secured.
[0138] In the sulfur-carbon composite of the present invention, the carbon material used as a sulfur carrier can generally be manufactured by carbonizing a precursor of various carbon materials.
[0139] Meanwhile, in one embodiment of the present invention, the pores of the carbon material may have a diameter ranging from 0.5 nm to 200 nm based on the longest diameter. The carbon material may be used without limitation as long as it is in a spherical, rod-shaped, needle-shaped, plate-shaped, tubular, or bulk shape, which are commonly used in lithium-sulfur secondary batteries.
[0140] The above carbon material may be any carbon-based material having porosity and conductivity that is commonly used in the industry. For example, it may include one or more selected from the group consisting of graphite; graphene; carbon black such as Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; carbon nanotubes (CNT) such as single-walled carbon nanotubes (SWCNT) and multi-walled carbon nanotubes (MWCNT); carbon fibers such as graphite nanofibers (GNF), carbon nanofibers (CNF), and activated carbon fibers (ACF); graphite such as natural graphite, artificial graphite, and expanded graphite; carbon nanoribbons; carbon nanobelts, carbon nanorods, and activated carbon.
[0142] In the sulfur-carbon composite according to the present invention, the sulfur is located on at least one of the inner and outer surfaces of the pores of the carbon material, and may be present in an area of less than 100%, preferably 1 to 95%, and more preferably 60 to 90% of the entire inner and outer surfaces of the carbon material. When the sulfur is located within the above range on the surface of the carbon material, it can exhibit maximum effects in terms of electron transfer area and electrolyte wettability. Specifically, since the sulfur is thinly and evenly impregnated on the surface of the carbon material within the above range, the electron transfer contact area can be increased during the charging and discharging process. If the sulfur is located in an area of 100% of the entire surface of the carbon material, the carbon material is completely covered with sulfur, resulting in reduced electrolyte wettability and reduced contact with the conductive material contained in the electrode, which prevents electron transfer and thus prevents participation in the reaction.
[0144] <Manufacture of Sulfur-Carbon Composites>
[0145] In addition, in one embodiment of the present invention, the sulfur-carbon composite can be obtained by the following manufacturing method.
[0146] The method for manufacturing a sulfur-carbon composite according to the present invention is not particularly limited and is commonly known in the art, and can be manufactured by a composite method comprising the steps of (S1) mixing a carbon material and sulfur, and (S2) composite.
[0147] The mixing in step (S1) above is intended to increase the degree of mixing between sulfur and carbon materials and can be performed using a stirring device commonly used in the industry. At this time, the mixing time and speed can also be selectively adjusted according to the content and conditions of the raw materials.
[0148] The composite method of step (S2) above is not specifically limited in the present invention, and methods commonly used in the art may be used. For example, methods commonly used in the art, such as dry composite or wet composite such as spray coating, may be used. For example, a method may be used in which the mixture of sulfur and carbon materials obtained after mixing is heat-treated so that molten sulfur can be evenly coated on the inner and outer surfaces of the carbon material. Meanwhile, in one embodiment of the present invention, a process of grinding the mixture of sulfur and carbon materials by a method such as ball milling may be performed before the heat treatment. In one embodiment of the present invention, the heat treatment may be performed for about 20 minutes to 24 hours at a temperature of 120 to 160°C, and a heating device such as an oven may be applied.
[0149] The sulfur-carbon composite produced by the aforementioned manufacturing method has a structure that has a high specific surface area, a high sulfur loading, and an improved sulfur utilization rate. As a result, not only is the electrochemical reactivity of sulfur improved, but the accessibility and contact of the electrolyte are also enhanced, thereby improving the capacity and lifespan characteristics of the lithium-sulfur battery.
[0151] In one embodiment of the present invention, the positive electrode active material may be composed solely of the sulfur-carbon composite. In addition, in addition to the sulfur-carbon composite, it may further include one or more additives selected from transition metal elements, Group IIIA elements, Group IVA elements, sulfur compounds of these elements, and alloys of these elements and sulfur.
[0153] In a specific embodiment of the present invention, the positive electrode active material layer may comprise a lithium transition metal composite oxide represented by the following [Chemical Formula 1].
[0155] [Chemical Formula 1]
[0156] Li a Ni b Co c M1 d M 2 e O2
[0157] In the above chemical formula 1, M 1 It may be Mn, Al, or a combination thereof, and preferably may be Mn or Mn and Al.
[0158] The above M 2 is one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, preferably one or more selected from the group consisting of Zr, Y, Mg, and Ti, and more preferably Zr, Y, or a combination thereof. 2 Although the element is not necessarily included, if included in an appropriate amount, it can play a role in promoting grain growth during sintering or improving crystal structure stability.
[0160] Challenge
[0161] The above conductive material is used to impart conductivity to the negative electrode, and in the battery being constructed, it may be used without special limitations as long as it possesses electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, carbon nanotube; metal powder or metal fiber such as copper, nickel, aluminum, or silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. The above conductive material may typically be included in an amount of 1 to 30 wt%, preferably 1 to 20 wt%, and more preferably 1 to 10 wt% based on the total weight of the negative electrode active material layer.
[0163] Binder material
[0164] The above binder material serves to improve adhesion between positive active material particles and adhesion between the positive active material and the positive current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof. One of these alone or a mixture of two or more may be used.
[0166] Separator
[0167] The above separator is disposed within the electrode assembly in a manner interposed between the negative electrode and the positive electrode. The separator separates the negative electrode and the positive electrode and provides a pathway for the movement of lithium ions; any separator typically used as a separator in a lithium secondary battery can be used without any particular restrictions. Specifically, the separator may be a porous polymer film, such as a porous polymer film made of a polyolefin-based polymer like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof. Alternatively, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, to ensure heat resistance or mechanical strength, a separator coated with a coating layer containing a ceramic component or a polymer material may be used.
[0169] battery
[0170] Another aspect of the present invention relates to a secondary battery comprising the electrode assembly. The secondary battery comprises an electrode assembly and an electrolyte housed together in a battery case. The battery case may be selected without special limitations from any type commonly used in the field of technology, such as a pouch type or a metal can type. The shape of the battery is not particularly limited and can be of various shapes, such as cylindrical, stacked, or coin-shaped.
[0172] electrolytes
[0173] In the present invention, the electrolyte may include an organic solvent and a lithium salt.
[0175] Organic solvent
[0176] The above organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move. The above organic solvent may be any that is commonly used in lithium secondary battery electrolytes without limitation, and for example, ethers, esters, amides, chain carbonates, cyclic carbonates, etc., may be used alone or in combination of two or more. Among these, ether-based compounds may be included as a representative example.
[0177] The above ether-based compound may include acyclic ether or cyclic ether.
[0178] For example, the above-mentioned acyclic ether may be one or more selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, dimethoxyethane, diethoxyethane, ethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, and polyethylene glycol methyl ethyl ether.
[0179] For example, the cyclic ether is 1,3-dioxolane, 4,5-dimethyl-dioxolane, 4,5-diethyl-dioxolane, 4-methyl-1,3-dioxolane, 4-ethyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, 2,5-dimethoxytetrahydrofuran, 2-ethoxytetrahydrofuran, 2-methyl-1,3-dioxolane, 2-vinyl-1,3-dioxolane, 2,2-dimethyl-1,3-dioxolane, 2-methoxy-1,3-dioxolane, 2-ethyl-2-methyl-1,3-dioxolane, tetrahydropyran, 1,4-dioxane, 1,2-dimethoxybenzene, It may be one or more selected from the group consisting of 1,3-dimethoxybenzene, 1,4-dimethoxybenzene and isosorbid dimethyl ether, furan, 2-methyl furan, 3-methyl furan, 2-ethyl furan, 2-butyl furan, 2,3-dimethyl furan, 2,4-dimethyl furan, 2,5-dimethyl furan, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzoburane, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene, and 2,5-dimethylthiophene, but is not limited thereto.
[0180] Examples of the esters of the above organic solvents include, but are not limited to, any one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone and mixtures of two or more of these.
[0181] Specific examples of the above linear carbonate compounds include, but are not limited to, any one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethylmethyl carbonate (EMC), methylpropyl carbonate and ethylpropyl carbonate, or a mixture of two or more of these.
[0182] In addition, specific examples of the above-mentioned cyclic carbonate compounds may include ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, vinylethylene carbonate, and their halides, or mixtures of two or more of these. Examples of such halides include, but are not limited to, fluoroethylene carbonate (FEC).
[0184] lithium salt
[0185] The above lithium salt is a compound capable of providing lithium ions in the electrolyte. Such lithium salts include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3CO2, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiCH3SO3, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiC4BO8, LiCl, LiBr, LiB 10 Cl 10Li, LiI, or LiB(C2O4)2, etc., may be used. In the present invention, in order to increase the potential for sulfur utilization and to realize high-capacity and high-voltage batteries, it is preferable to include Li-TFSI as the lithium salt. More preferably, the lithium salt may include LiN(CF3SO2)2(Li-TFSI) at a content of 80 wt% or more, 90 wt% or more, or 100% relative to 100 wt% of the total lithium salt.
[0186] The concentration of the lithium salt is in the range of 0.1 to 2.0 M, preferably 0.5 to 1 M, and more preferably 0.5 to 0.75 M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance and allow lithium ions to move effectively. If the concentration of the lithium salt is below the above range, it may be difficult to secure ion conductivity suitable for battery operation, and if it exceeds the above range, the viscosity of the electrolyte increases, which may reduce the mobility of lithium ions, or the decomposition reaction of the lithium salt itself increases, which may degrade the performance of the battery.
[0188] In a specific embodiment of the present invention, in an electrolyte comprising a first solvent, a second solvent, and a lithium salt, the molar ratio of the lithium salt, the second solvent, and the first solvent may be 1:0.5 to 3:4.1 to 15. In addition, in an embodiment of the present invention, the molar ratio of the lithium salt, the second solvent, and the first solvent may be 1:2:4 to 13, 1:3:3 to 10, or 1:4:5 to 10, and so on. In the electrolyte included in the lithium-sulfur battery of the present invention, the first solvent comprising a fluorine-based ether compound may be included in a higher content ratio compared to the second solvent comprising a glycine-based compound.
[0190] Other additives
[0191] In addition to the electrolyte components, the above electrolyte may further include additives for the purpose of improving the lifespan characteristics of the battery, suppressing the reduction of battery capacity, and improving the discharge capacity of the battery. For example, the above additives may include nitrate compounds, nitrite compounds, haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexamethylphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, either alone or in combination. The above additives may be included in an amount of 0.1 to 10 wt%, preferably 0.1 to 5 wt%, based on the total weight of the electrolyte.
[0193] In a specific embodiment of the present invention, the electrolyte may include a nitric acid compound and / or a nitrite-based compound as an additive. Such nitric acid compound / nitrite-based compound forms a stable film on the lithium metal electrode serving as the negative electrode and has the effect of improving charge and discharge efficiency. Such nitric acid or nitrite-based compounds include inorganic nitric acid or nitrite compounds such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), and ammonium nitrite (NH4NO2); Organic nitric acid or nitrite compounds such as methyl nitrate, dialkyl imidazolium nitrate, guanidine nitrate, imidazolium nitrate, pyridinium nitrate, ethyl nitrite, propyl nitrite, butyl nitrite, pentyl nitrite, octyl nitrite, etc.; organic nitro compounds such as nitromethane, nitroprophane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, dinitrotoluene, etc., and combinations thereof may include one or more selected from the group consisting of these, but are not limited thereto. In a preferred embodiment of the present invention, the additive may include lithium nitrate.
[0195] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the invention. However, the embodiments according to the present invention may be modified in various different forms, and the scope of the present invention should not be interpreted as being limited to the embodiments described above. The embodiments of the present invention are provided to more completely explain the invention to those with average knowledge in the art.
[0197] <Example>
[0198] (Manufacturing of spare batteries)
[0199] Carbon nanotubes and sulfur were evenly mixed and placed in an oven at 155°C for 30 minutes to prepare a sulfur-carbon composite. The sulfur content of the 100 wt% sulfur-carbon composite was 75 wt%. A slurry for manufacturing the anode was prepared by mixing 90 wt% of the prepared sulfur-carbon composite, 5 wt% of Denka Black, and 5 wt% of a binder (styrene butadiene rubber / carboxymethylcellulose, 7:3 weight ratio). The solid content of the slurry was 25 wt%. The slurry was applied to both sides of a 20 µm thick aluminum current collector, dried at 50°C for 12 hours, and compressed using a roll press to manufacture the anode. The loading amount of the anode active material (relative to electrode area) was 2.5 to 2.7 mAh / cm². 2 And, the porosity was 70 to 83 vol%.
[0201] A lithium thin film with a thickness of 60 μm was prepared as the cathode.
[0203] As the electrolyte, a mixture of 1 M concentration lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1 wt% lithium nitrate (LiNO3) dissolved in an organic solvent composed of 1,3-dioxolane and dimethyl ether (DOL:DME=1:1 (volume ratio)) was used.
[0205] A preliminary battery was manufactured by positioning the above-manufactured positive and negative electrodes facing each other, interposing a polyethylene porous film with a thickness of 16 μm and a porosity of 68% as a separator between them, loading them into a pouch, injecting the above-manufactured electrolyte, and sealing the pouch. In the battery, a total of 7 positive electrodes and a total of 8 negative electrodes were configured in a stacked and folded form with the separator interposed.
[0207] Examples
[0208] The pre-prepared battery was placed in a jig and a pressure of approximately 7 atm was applied. Next, it was discharged using a PNE-0506 charger / discharger (manufacturer: PNE solution) in CC-CV mode. Constant current discharge was performed at a rate of 0.5C, and the constant voltage mode was maintained for approximately 4 hours after reaching the discharge termination voltage of 1.8V until the discharge termination current reached 0mAh.
[0210] Comparative example
[0211] The pre-prepared battery prepared above was placed in a jig and a pressure of about 7 atm was applied. Next, using a PNE-0506 charger / discharger (manufacturer: PNE solution), it was discharged in a constant current manner at 0.5C to 1.7V, and then charged in a constant current manner at 0.3C to 2.5V, and this was repeated 6 times.
[0213] Lifespan characteristics evaluation
[0214] In each example and comparative example, the life characteristics of the battery manufactured after the activation process were evaluated using a PNE-0506 charge / discharger (manufacturer: PNE solution). For each battery, it was charged at 0.3C to 2.5V using a constant current method, discharged at 1C to 1.7V using a constant current method, and the charging and discharging were repeated until the capacity reached 80% relative to the discharge capacity of 100% of the first cycle.
[0216] Figure 1 shows a comparison of the specific capacity of each battery at 1C discharge, and Figure 2 shows the Coulomb efficiency characteristics. According to this, it was confirmed that the specific capacity of the example and the comparative example were similar at similar charge-discharge cycles, but the Coulomb efficiency of the example was found to be superior.
[0218] Meanwhile, Figure 3 shows the output density for each state of charge (SOC) range. The output density for each SOC range was measured by decreasing the SOC by 10% increments from 95% to 15%. When each specific SOC was reached at 95%, 85%, 75%, 65%, 55%, 45%, 35%, 25%, and 15%, a 5C pulse current was applied in the discharge direction for 10 seconds, and the output density (kW / kg) was calculated by converting this into a voltage value. This can serve as an indicator of the degree of overvoltage when a pulse current is applied to each battery. Subsequently, the measurement was performed by taking a rest period of 1 minute, charging to 100% SOC at 0.1C, applying a charging current of 0.3C for 10 seconds, and then repeating the process when the next specific SOC was reached relative to the initial discharge standard. The lithium-sulfur battery exhibits the lowest voltage at the SOC 75% range, and this is also the range with the highest overvoltage, making it a key range for verifying battery performance. According to Figure 3, the output density of the example and the comparative example is equivalent at the point of SOC 75%, and it can be seen that the example and the comparative example show almost identical levels in other ranges as well. Accordingly, the battery manufacturing method of the present invention secures an output density equivalent to that of the prior art while reducing the number of charge-discharge cycles during the activation process compared to the prior art, thereby shortening the time required for the battery manufacturing process and demonstrating excellent process efficiency.
Claims
Claim 1 (S10) a step of manufacturing a preliminary battery comprising an electrode assembly and an electrolyte; and (S20) an activation step of activating the preliminary battery; wherein the electrode assembly comprises a positive electrode, a negative electrode and a separator interposed between the positive electrode and the negative electrode, and the positive electrode comprises a positive active material comprising sulfur, and the step (S10) comprises the electrode assembly being impregnated with the electrolyte, and the step (S20) comprises a step of discharging the preliminary battery, wherein the discharge is performed in the order of a constant current discharge and a constant voltage discharge after the constant current discharge, and in the step (S20), the constant current discharge is performed until a preset discharge termination voltage is reached, and the discharge termination voltage is set within the range of 1.3V to 1.8V. Claim 2 delete Claim 3 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein in step (S20), the constant current discharge is performed at a rate limit set within the range of C rate 0.05 to 2 until a preset discharge termination voltage is reached. Claim 4 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the constant voltage discharge is performed until the residual current of the battery reaches 0 mAh at a preset discharge termination voltage. Claim 5 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the preliminary battery is not charged or discharged prior to the execution of step (S20), and the first discharge is applied to the preliminary battery during charging and discharging in step (S20). Claim 6 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the preliminary battery is not charged or discharged prior to the execution of step (S20), and the step (S20) consists only of discharging the preliminary battery once. Claim 7 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the discharge is performed less than 6 times in step (S20). Claim 8 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein in step (S20), the constant current discharge is performed in a range of C Rate of 0.05 to 2.
00. Claim 9 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein in step (S20), the discharge is performed in a constant current manner up to a preset discharge termination voltage. Claim 10 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the discharge in step (S20) is performed at a rate (C Rate) in the range of 0.50 to 1.
00. Claim 11 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the step (S20) is performed in an environment where the preliminary battery is pressurized. Claim 12 A method for manufacturing a lithium-sulfur battery according to claim 11, wherein the above-mentioned pressure is applied at a pressure greater than atmospheric pressure. Claim 13 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein the step (S20) is performed at a temperature of 15°C to 40°C. Claim 14 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein an aging step of maintaining the preliminary battery in an atmosphere of 15°C to 40°C is further performed after performing step (S10) and before performing step (S20). Claim 15 A method for manufacturing a lithium-sulfur battery according to claim 1, wherein, after applying an initial discharge process in step (S20), charging and discharging are repeated thereafter, and a charging process is performed between the discharge processes, and the charging is performed in the order of constant current charging and then constant voltage charging after the constant current charging.
Citation Information
Patent Citations
An in-situ preparation method for lithium-sulfur batteries based on graphite anodes
CN106785075B
Method of manufacturing lithium-sulfur battery and lithium-sulfur battery using the same
KR1020190088610A
Manufacturing methods for the secondary battery
KR1020200129518A