Rubber composition for tire innerliner and tire manufactured by using same
A rubber composition for tire inner liners using recycled butyl rubber, natural rubber, and carbon black addresses the challenge of maintaining air permeability and crack resistance, achieving comparable performance to conventional materials while promoting sustainability.
Patent Information
- Application Number
- KR1020230105067
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-08-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-10
AI Technical Summary
Existing tire inner liners face challenges in maintaining air permeability and crack resistance while transitioning to sustainable materials, particularly due to the limitations of conventional fillers that improve air permeability but degrade crack resistance, and the need for sustainable materials in response to environmental regulations.
A rubber composition for tire inner liners using recycled butyl rubber, natural rubber, liquid rubber, and carbon black, with specific molecular weight and viscosity ranges, to enhance air permeability and crack resistance, incorporating recycled materials to improve durability.
The composition improves air permeability and crack resistance, enhancing tire durability while utilizing recycled materials, achieving performance comparable to conventional compositions.
Abstract
Description
Technology Field
[0001] The present invention relates to a rubber composition for a tire inner liner utilizing recycled waste tire components and a tire manufactured using the same. Background Technology
[0002] Pneumatic tires, which have undergone steady technological development since the 1800s, are mounted on vehicles and play important roles such as supporting loads, absorbing and mitigating road shocks, driving the engine and transmitting braking power, and changing and maintaining direction.
[0003] In the case of pneumatic tires, since air leakage to the outside can lead to a decrease in driving stability, such as handling and cornering, as well as rolling resistance performance, the tire structure consists of an elastic air container, and maintaining constant tire pressure is closely related to tire durability.
[0004] The air permeability of these tires is closely related to the performance of the inner liner. The inner liner is an air-sealing rubber layer made of butyl rubber or polyisoprene-based rubber that improves durability by blocking air entry into the carcass and belt areas, thereby preventing corrosion of the tire's internal cords.
[0005] In addition, since the air permeability of a tire is closely related to its durability, it is designed to have low air permeability by creating barriers or obstacles in the passage through which air escapes. Methods to improve such air permeability performance include using butyl rubber or isoprene-based rubber, which can form a dense packed structure with few double bonds, and using plate-type fillers or high-performance carbon black fillers that have developed a structure to prevent air from escaping easily.
[0006] However, the aforementioned fillers have limitations in their application because, while adding more improves air permeability performance, it has the disadvantage of degrading the crack resistance of the compound. In particular, since tires continuously repeat expansion and contraction movements during vehicle operation, making them prone to cracks caused by fatigue, fatigue resistance is also one of the important required properties of the inner liner. Therefore, in conventional technology, only new butyl and carbon were used to satisfy the air permeability and fatigue resistance performance of the inner liner.
[0007] However, due to the recently adopted Paris Climate Agreement, the international community is strengthening regulations to reduce greenhouse gases across various industries to prevent global warming, and demands for carbon neutrality are intensifying, particularly centered on the automotive industry. In response to these changes, the tire industry is also making significant efforts to transition to sustainable materials used in manufacturing and is working to develop sustainable tires and compounds using natural and recycled raw materials. The problem to be solved
[0008] The objective of the present invention is to provide a rubber composition for a tire inner liner that improves air permeability performance while using recycled butyl rubber extracted from waste tires, and simultaneously improves crack resistance performance, thereby enhancing the durability of the tire even when using recycled raw materials.
[0009] Another objective of the present invention is to provide a tire manufactured using the rubber composition for a tire inner liner. means of solving the problem
[0010] A rubber composition for a tire inner liner according to one embodiment comprises natural rubber, butyl rubber, and liquid rubber.
[0011] A rubber composition for a tire inner liner may comprise, with respect to 100 parts by weight of raw rubber containing a rubber component among natural rubber and butyl rubber, 5 to 25 parts by weight of natural rubber, 30 to 80 parts by weight of butyl rubber, and 5 to 20 parts by weight of liquid rubber.
[0012] The rubber composition for tire inner liners may further include recycled butyl rubber.
[0013] A rubber composition for a tire inner liner may contain 20 to 90 parts by weight of recycled butyl rubber per 100 parts by weight of raw rubber containing a rubber component among natural rubber, butyl rubber, and recycled butyl rubber.
[0014] Recycled butyl rubber may comprise 40% to 60% by weight of a rubber component, 20% to 40% by weight of a carbon component, and 1% to 10% by weight of an ash component, based on the total weight of the recycled butyl rubber.
[0015] Liquid rubber may contain liquid polyisobutene.
[0016] The liquid polyisobutene may have a number average molecular weight (Mn) of 500 g / mol to 3000 g / mol, a pour point of -50 ℃ to 30 ℃, and a viscosity of 80 cSt to 13000 cSt.
[0017] Butyl rubber can be butyl halogenated rubber.
[0018] A rubber composition for a tire inner liner may contain 5 to 35 parts by weight of recycled carbon black per 100 parts by weight of raw rubber.
[0019] Regenerated carbon black has an iodine adsorption capacity of 70 mg / g to 160 mg / g and an N2 adsorption capacity of 60 m 2 / g to 90 m 2 / g, and the sieve residue (325 mesh) may be 0 ppm to 40 ppm.
[0020] A rubber composition for a tire inner liner may contain 40 to 60 parts by weight of carbon black per 100 parts by weight of raw rubber.
[0021] Carbon black has an iodine adsorption capacity of 30 mg / g to 50 mg / g and an N2 adsorption capacity of 25 m 2 / g to 45 m 2 / g, and the DBP oil absorption amount may be 65 cc / g to 95 cc / g.
[0022] A tire according to another embodiment is manufactured using a rubber composition for a tire inner liner.
[0023] The tire can be a passenger car tire. Effects of the invention
[0024] A rubber composition for a tire inner liner according to one embodiment uses recycled butyl rubber extracted from waste tires, and at the same time improves air permeability performance and crack resistance performance, thereby improving the durability of the tire even when using recycled raw materials. Specific details for implementing the invention
[0025] The advantages and features of the technology described below, and the methods for achieving them, will become clear by referring to the embodiments described below in detail together with the accompanying drawings. However, the forms of implementation are not limited to the embodiments disclosed below. Unless otherwise defined, all terms used in this specification (including technical and scientific terms) may be used in a meaning that is commonly understood by those skilled in the art. Furthermore, terms defined in commonly used dictionaries are not to be interpreted ideally or excessively unless explicitly and specifically defined otherwise.
[0026] Throughout this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components. Furthermore, the singular form includes the plural form unless specifically stated otherwise in the text.
[0027] A rubber composition for a tire inner liner according to one embodiment comprises natural rubber, butyl rubber, and liquid rubber. Optionally, the rubber composition for a tire inner liner may further comprise recycled butyl rubber.
[0028] A rubber composition for a tire inner liner according to one embodiment is a sustainable rubber composition for a tire inner liner utilizing recycled butyl rubber. By including polyisobutene together with recycled butyl rubber, the modulus, heat generation performance, crack resistance performance, and air permeability performance of the compound are similar to or better than those of conventional rubber compositions for tire inner liners.
[0029] Natural rubber possessing excellent tensile strength and friction resistance may be used without special restrictions as long as it is commonly used in tire rubber compositions. Specifically, the natural rubber may be ordinary natural rubber or modified natural rubber.
[0030] Any natural rubber known as natural rubber can be used, and its country of origin is not limited. Natural rubber contains cis-1,4-polyisoprene as the main component, but may also contain trans-1,4-polyisoprene depending on the required characteristics. Therefore, in addition to natural rubber containing cis-1,4-polyisoprene as the main component, natural rubber may also include natural rubber containing trans-1,4-isoprene as the main component, such as balata, a type of rubber from the Sapotaceae family in South America.
[0031] Modified natural rubber refers to ordinary natural rubber that has been modified or refined. Examples of modified natural rubber include epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), and hydrogenated natural rubber.
[0032] Natural rubber may be included in an amount of 5 to 25 parts by weight per 100 parts by weight of raw rubber. In this specification, raw rubber refers to all rubber components included in the rubber composition, and is a concept that includes, for example, rubber components included in natural rubber, butyl rubber, and recycled butyl rubber. In addition, the weight of natural rubber per 100 parts by weight of raw rubber is the weight ratio of natural rubber when the sum of the weight of natural rubber, the weight of butyl rubber, and the weight of rubber components included in recycled butyl rubber is converted to 100, for example. If the content of natural rubber is less than 5 parts by weight per 100 parts by weight of raw rubber, processability may be reduced and adhesion to tire structures using other diene-based rubbers may be reduced, and if it exceeds 25 parts by weight, air permeability and crack resistance may be reduced.
[0033] Butyl rubber is a copolymer of isobutylene and isoprene, and is also known as isobutylene-isoprene rubber.
[0034] Butyl rubber may be butyl rubber (IIR), brominated butyl rubber (Br-IIR), chlorinated butyl rubber (Cl-IIR), or halogenated butyl rubber.
[0035] Butyl rubber has low gas permeability and exhibits excellent crack resistance and adhesion, and in particular, its air permeability is superior to that of other rubbers. In this specification, butyl rubber may also be referred to as new butyl rubber to distinguish it from recycled butyl rubber.
[0036] Butyl rubber may be included in an amount of 30 to 80 parts by weight per 100 parts by weight of raw rubber. If the content of butyl rubber is less than 30 parts by weight per 100 parts by weight of raw rubber, the air permeability and crack resistance of the rubber composition may decrease, and if it exceeds 80 parts by weight, the tanδ properties and exothermic properties of the rubber composition may increase.
[0037] Recycled butyl rubber may be produced by heating and pressurizing crushed rubber products containing a large amount of butyl rubber, such as inner liners of waste tires or bladders used in tire manufacturing, or by cutting the cross-linking bonds of the rubber components contained therein (desulfurization treatment) to make them revulcanizable. For example, recycled butyl rubber can be produced by heating waste tire inner liners under pressurized conditions or by crushing bladders with an extruder.
[0038] For example, recycled butyl rubber may contain 40% to 60% by weight of a rubber component, 20% to 40% by weight of a carbon component, and 1% to 10% by weight of an ash component, based on the total weight. When the content of the rubber component in the recycled butyl rubber is within the above range, air permeability performance can be secured. In addition, when the content of the carbon component in the recycled butyl rubber is within the above range, cross-linked fine particles can bypass or prevent the propagation of cracks, thereby improving crack resistance performance. Furthermore, when the content of the ash component in the recycled butyl rubber is within the above range, processability can be improved by controlling the content of fine powder that may act as a foreign substance.
[0039] Recycled butyl rubber may be included in an amount of 20 to 90 parts by weight per 100 parts by weight of raw rubber. If the content of recycled butyl rubber is less than 20 parts by weight per 100 parts by weight of raw rubber, the benefits of using recycled butyl rubber may not be fully obtained, and if it exceeds 90 parts by weight, air permeability and crack resistance performance may be reduced due to the influence of carbon components contained in the recycled butyl rubber.
[0040] As such, the rubber composition for tire inner liners contains a large amount of butyl rubber with excellent air permeability to improve air permeability performance.
[0041] Butyl rubber is a copolymer of isoprene and isobutylene and has a smaller amount of double bonds compared to general diene rubber, so it has low resilience and can easily absorb vibrations. In addition, butyl rubber has a smaller double bond structure, so it can form a dense packing structure compared to styrene-butadiene rubber (SBR) or butadiene rubber (BR), which has the advantage of effectively blocking the penetration of ozone, moisture, and air.
[0042] Butyl rubber has the advantage of being easier to use as a recycled material compared to general diene rubber because it is difficult to form a cross-linked structure due to the small number of double bonds; however, since recycled butyl rubber has a reduced molecular weight due to heat during the regeneration process and contains cross-linked particles, carbon components, and ash components, its tensile strength, crack resistance, fatigue resistance, and air permeability can be significantly reduced compared to using fresh butyl rubber.
[0043] Accordingly, the rubber composition for a tire inner liner includes liquid rubber together with recycled butyl rubber. As an example, the liquid rubber may include polyisobutene (PIB).
[0044] Liquid polyisobutene increases the compatibility between recycled butyl rubber and new butyl rubber, and at the same time, allows for the formation of a denser structure than when using conventional processing aids, thereby improving the fatigue resistance, crack resistance, and air permeability performance of the rubber composition even when using recycled butyl rubber.
[0045] Liquid polyisobutene may be in a somewhat viscous liquid state at room temperature (20°C). For example, liquid polyisobutene may have a number average molecular weight (Mn) of 500 g / mol to 3000 g / mol, a pour point of -50°C to 30°C, and a viscosity of 80 cSt to 13000 cS. If the number average molecular weight, pour point, or viscosity of the liquid polyisobutene is below the above ranges, a sufficiently dense structure cannot be formed, so there may be no improvement in air permeability due to the application of liquid polyisobutene, and if it exceeds the above ranges, raw material handling and processability of the rubber composition may be reduced due to high viscosity.
[0046] Liquid polyisobutylene may or may not be functionalized. When liquid polyisobutylene is functionalized, it may be, for example, polyisobutylene succinic anhydride (PIBSA) or polyisobutylene succinimide (PIBSI).
[0047] Liquid polyisobutene may be included in an amount of 5 to 20 parts by weight per 100 parts by weight of raw rubber. If the content of liquid polyisobutene is less than 5 parts by weight per 100 parts by weight of raw rubber, the mixing of rubber and carbon black may not proceed smoothly, and if it exceeds 20 parts by weight, the adhesiveness may be too high, and processability may be reduced during kneading and rolling.
[0048] In this way, the rubber composition for tire inner liners can recover fatigue resistance, crack resistance, and air permeability performance, which are degraded by replacing a portion of the new butyl rubber with recycled butyl rubber, by applying liquid polyisobutene.
[0049] The rubber composition for tire inner liners may further include carbon black as a reinforcing filler.
[0050] Considering the effects of improving processability and air permeability as well as reinforcing properties, carbon black has an iodine adsorption capacity of 30 mg / g to 50 mg / g and an N2 adsorption capacity of 25 m 2 / g to 45 m 2 / g, and one with a DBP oil absorption capacity of 65 cc / g to 95 cc / g can be used.
[0051] If the iodine adsorption amount, N2 adsorption amount, and DBP oil absorption amount of carbon black are below the above range, the reinforcing performance by carbon black as a filler may be disadvantageous, and if they exceed the above range, the processability and air permeability of the rubber composition may be disadvantageous.
[0052] Carbon black may be included in an amount of 40 to 60 parts by weight per 100 parts by weight of raw rubber. If the carbon black content is less than 40 parts by weight, the reinforcing performance due to the carbon black filler may be reduced, and if it exceeds 60 parts by weight, the processability and air permeability of the rubber composition may be reduced.
[0053] The rubber composition for tire inner liners may further include recycled carbon black.
[0054] Regenerated carbon black has an iodine adsorption capacity of 70 mg / g to 160 mg / g and an N2 adsorption capacity of 60 m 2 / g to 90 m 2 / g, the sieve residue (325 mesh) may be 0 ppm to 40 ppm.
[0055] If the iodine adsorption amount and N2 adsorption amount of recycled carbon black are less than the above range, the reinforcing performance by recycled carbon black may be disadvantageous, and if they exceed the above range, the processability and air permeability of the rubber composition may be disadvantageous.
[0056] In addition, if the residue of the recycled carbon black exceeds 40 ppm, the residue may act as a foreign substance and degrade mechanical properties.
[0057] Recycled carbon black may be included in an amount of 5 to 35 parts by weight per 100 parts by weight of raw rubber. If the content of recycled carbon black is less than 5 parts by weight, the air permeability and heat generation performance may be reduced, and if it exceeds 35 parts by weight, the processability and mechanical properties of the rubber composition may be reduced.
[0058] The rubber composition for tire inner liners may optionally further include various additives such as vulcanizing agents, vulcanization accelerators, vulcanization accelerating aids, and adhesives in addition to the components described above. Any additive commonly used in the field to which the present invention belongs may be used, and their content is not particularly limited, as it follows the formulation ratio used in conventional rubber compositions for tire inner liners.
[0059] Sulfur-based vulcanizing agents may preferably be used as vulcanizing agents. Sulfur-based vulcanizing agents may include inorganic vulcanizing agents such as powdered sulfur (S), insoluble sulfur (S), precipitated sulfur (S), and colloidal sulfur, as well as organic vulcanizing agents such as tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide (TETD), and dithiodimorpholine. Specifically, elemental sulfur or vulcanizing agents that produce sulfur, such as amine disulfide and polymeric sulfur, may be used as sulfur-based vulcanizing agents.
[0060] When the vulcanizing agent is included in an amount of 2 parts by weight or less, or 0.3 to 1.7 parts by weight, per 100 parts by weight of raw rubber, it can make the raw rubber less sensitive to heat and chemically stable through an appropriate vulcanization effect.
[0061] In addition, a vulcanization accelerator refers to an accelerator / retarder that accelerates the vulcanization rate or promotes a retarding effect during the initial vulcanization stage.
[0062] Vulcanization accelerators may include sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamate-based, aldehyde-amine-based, aldehyde-ammonia-based, imidazoline-based, xanthate-based, or combinations thereof.
[0063] As a sulfenamide-based vulcanization accelerator, for example, sulfenamide-based compounds including N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazylsulfenamide (TBBS), N,N-dicyclohexyl-2-benzothiazylsulfenamide, N-oxydiethylene-2-benzothiazylsulfenamide, N,N-diisopropyl-2-benzothiazolsulfenamide, or combinations thereof may be used.
[0064] As a thiazole-based vulcanization accelerator, for example, thiazole compounds including 2-mercaptobenzothiazole (MBT), dibenzothiazyl disulfide (MBTS), sodium salt of 2-mercaptobenzothiazole, zinc salt of 2-mercaptobenzothiazole, copper salt of 2-mercaptobenzothiazole, cyclohexylamine salt of 2-mercaptobenzothiazole, 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl4-morpholinothio)benzothiazole, or a combination thereof may be used.
[0065] As a thiuram-based vulcanization accelerator, for example, a thiuram-based compound including tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide, tetramethylthiuram monosulfide, dipentamethylenethiuram disulfide, dipentamethylenethiuram monosulfide, dipentamethylenethiuram tetrasulfide, dipentamethylenethiuram hexasulfide, tetrabutylthiuram disulfide, pentamethylenethiuram tetrasulfide, or a combination thereof may be used.
[0066] As thiourea-based vulcanization accelerators, thiourea-based compounds including, for example, thicarbamide, diethylthiourea, dibutylthiourea, trimethylthiourea, diortotolylthiourea, or combinations thereof may be used.
[0067] As a guanidine-based vulcanization accelerator, for example, guanidine-based compounds including diphenylguanidine, diortotolylguanidine, triphenylguanidine, orthotolylbiguanidine, diphenylguanidine phthalate, or a combination thereof may be used.
[0068] As dithiocarbamate-based vulcanization accelerators, examples include: zinc ethylphenyl dithiocarbamate, zinc butylphenyl dithiocarbamate, sodium dimethyl dithiocarbamate, zinc dimethyl dithiocarbamate, zinc diethyl dithiocarbamate, zinc dibutyl dithiocarbamate, zinc diamyl dithiocarbamate, zinc dipropyl dithiocarbamate, a complex salt of zinc pentamethylene dithiocarbamate and piperidine, zinc hexadecyl isopropyl dithiocarbamate, zinc octadecyl isopropyl dithiocarbamate, zinc dibenzyl dithiocarbamate, sodium diethyl dithiocarbamate, piperidine pentamethylene dithiocarbamate, selenium dimethyl dithiocarbamate, tellurium diethyl dithiocarbamate, cadmium diamyl dithiocarbamate, or a combination thereof; dithiocarbamate-based Compounds can be used.
[0069] As an aldehyde-amine or aldehyde-ammonia vulcanization accelerator, for example, an aldehyde-amine or aldehyde-ammonia compound including an acetaldehyde-aniline reactant, a butylaldehyde-aniline condensate, hexamethylenetetramine, an acetaldehyde-ammonia reactant, or a combination thereof may be used.
[0070] As imidazoline-based vulcanization accelerators, imidazoline-based compounds such as 2-mercaptoimidazoline can be used, and as xanthate-based vulcanization accelerators, xanthate-based compounds such as zinc dibutylxantogenate can be used.
[0071] Among these, thiazole-based vulcanization accelerators can be used to maximize productivity and rubber properties by accelerating the vulcanization speed.
[0072] The vulcanization accelerator may be included in an amount of 0.5 to 2 parts by weight, for example, 0.8 to 0.5 parts by weight, per 100 parts by weight of raw rubber.
[0073] A vulcanization accelerator is a compounding agent used in combination with a vulcanization accelerator to fully enhance the accelerating effect, and may include an inorganic vulcanization accelerator, an organic vulcanization accelerator, or a combination thereof.
[0074] Inorganic vulcanization accelerators may include zinc oxide (ZnO), zinc carbonate, magnesium oxide (MgO), lead oxide, potassium hydroxide, or a combination thereof.
[0075] Organic vulcanization accelerators may include stearic acid, zinc stearate, palmitic acid, linoleic acid, oleic acid, lauric acid, dibutyl ammonium oleate, derivatives thereof, or combinations thereof.
[0076] In particular, zinc oxide and stearic acid can be used together as vulcanization accelerators. In this case, zinc oxide dissolves in stearic acid to form an effective complex with the vulcanization accelerator, thereby facilitating the crosslinking reaction of rubber by producing favorable sulfur during the vulcanization reaction.
[0077] When zinc oxide and stearic acid are used together, they may each be used in an amount of 0.1 to 1.5 parts by weight per 100 parts by weight of raw rubber to serve as appropriate vulcanization accelerators. If the content of zinc oxide and stearic acid is below the above range, the vulcanization speed may be slow, which may reduce productivity, and if it exceeds the above range, scorching may occur, which may degrade physical properties.
[0078] A rubber composition for a tire inner liner may further include 0.3 to 1.7 parts by weight of a sulfur-based vulcanizing agent and 0.8 to 1.5 parts by weight of a thiazole-based vulcanizing accelerator per 100 parts by weight of raw rubber.
[0079] A rubber composition for a tire inner liner can be manufactured through a conventional two-stage continuous manufacturing process. That is, it can be manufactured in a suitable mixer using a first stage of thermomechanical treatment or kneading at a high temperature of up to 110°C to 190°C, for example, 130°C to 180°C, and a second stage of mechanical treatment at a low temperature of typically less than 110°C, for example, 40°C to 100°C, during a finishing stage in which a crosslinking system is mixed, but the present invention is not limited thereto.
[0080] The rubber composition for tire inner liners is not limited to the inner liner but may be included in various rubber components constituting the tire. Examples of rubber components include the tread, sidewall, sidewall insert, apex, chafer, or wire coat.
[0081] A tire according to another embodiment includes an inner liner manufactured using the rubber composition for a tire inner liner. Since any method conventionally used for manufacturing tires can be applied to the method of manufacturing a tire including the inner liner manufactured using the rubber composition for a tire inner liner, a detailed description is omitted in this specification.
[0082] Tires can be passenger car tires, racing tires, airplane tires, agricultural machinery tires, off-road tires, truck tires, or bus tires, and among these, they can be passenger car tires.
[0083] In addition, the tire may be a radial tire or a bias tire, and, for example, it may be a radial tire.
[0084] Specific embodiments of the invention are presented below. However, the embodiments described below are merely for the purpose of specifically illustrating or explaining the invention and should not limit the scope of the invention.
[0085] [Preparation Example: Preparation of a Rubber Composition]
[0086] A rubber composition is prepared by adding the composition shown in Table 1 below to a Banbury mixer and then vulcanizing it at 170°C for 15 minutes to prepare specimens according to the examples and comparative examples.
[0087] division Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 natural rubber 10 10 10 10 10 butyl rubber 90 80 90 80 50 recycled butyl rubber 0 18.8(10) 0 18.8(10) 75.2(50) Carbon Black 57.5 57.5 57.5 57.5 57.5 Recycled Carbon Black 11.5 11.5 11.5 11.5 11.5 Processing oil 8 8 0 0 0 Liquid polyisobutene 0 0 8 8 8 stearic acid 1 1 1 1 1 brimstone 0.5 0.5 0.5 0.5 0.5 accelerant 0.7 0.7 0.7 0.7 0.7
[0088] Unit) Parts by weight
[0089] 1) Butyl rubber: Chlorobutyl rubber
[0090] 2) Recycled butyl rubber: Contains approximately 53% by weight of rubber components, approximately 33% by weight of carbon components, and approximately 14% by weight of other ash components (the figures in parentheses in Table 1 indicate the weight portion of the rubber components of recycled butyl rubber within the raw rubber).
[0091] 3) Carbon Black: Iodine adsorption capacity 37 mg / g, N2 adsorption capacity 25 m2 / g, DBP oil absorption capacity 93 cc / g
[0092] 4) Regenerated Carbon Black: Iodine adsorption capacity 79 mg / g, N2 adsorption capacity 60 m 2 / g, Sieve residue (325 mesh) 0.6 ppm
[0093] 5) Liquid Polyisobutene: Number average molecular weight 1,300 g / mol, Pour point 3.0 ℃, ASTM D445 viscosity 640 cSt
[0094] [Experimental Example: Measurement of Physical Properties of Rubber Composition]
[0095] The physical properties of the rubber specimens prepared in the examples and comparative examples were measured, and the results are shown in Table 2 below.
[0096] division Comparative Example 1 Comparative Example 2 Example 1 Example 2 Example 3 Mixed processability (ML1+4) 47 47 49 49 49 hardness 54 56 55 57 58 300% modulus 27 24 28 26 26 Endopathic performance index 100 91 101 99 92 Crack resistance performance index 100 90 102 95 91 Internal air permeability performance index 100 95 128 116 106
[0097] 1) Mixed processability: An indicator of processability measured at 100°C, and the smaller the number, the more favorable the processability.
[0098] 2) Tensile properties (hardness, 300% modulus): Unvulcanized rubber was vulcanized at a temperature of 170°C to produce dumbbell-shaped specimens, and the hardness and 300% modulus were measured.
[0099] 3) Fatigue resistance: A value expressed as an index representing the number of times a specimen breaks due to fatigue when a dumbbell-shaped specimen is subjected to repeated fatigue of a certain strain using a fatigue-failure test device; the higher the value, the more favorable the fatigue resistance performance.
[0100] 4) Crack resistance: A value representing the degree of crack growth in a specimen due to fatigue applied to the specimen when repeated fatigue with a constant strain is applied to a specimen aged at 100°C for one week using a DeMattia tester, and the higher the value, the more favorable the crack resistance performance.
[0101] 5) Air permeability performance: A value in which the degree of increase in permeable gas pressure of a test specimen due to the pressure difference is expressed as an index by using a gas permeability tester to create a vacuum on one side and apply a constant gas pressure to the other side, and the higher the value, the more favorable the air permeability performance.
[0102] As shown in the results of Table 2, Example 1, which uses liquid polyisobutene, exhibits superior fatigue resistance, crack resistance, and air permeability performance compared to Comparative Example 1 and Comparative Example 2.
[0103] In addition, in the case of Example 2, in which the amount of recycled butyl rubber was increased compared to Example 1, it can be confirmed that even if the new butyl rubber is replaced with recycled butyl rubber, results similar to Comparative Example 1 in terms of fatigue resistance, crack resistance, and excellent air permeability performance are obtained.
[0104] Although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims are also included within the scope of the present invention.
Claims
Claim 1 The composition comprises natural rubber, butyl rubber, and liquid rubber, recycled butyl rubber, recycled carbon black, and carbon black, wherein, with respect to 100 parts by weight of raw rubber containing a rubber component among the natural rubber, the butyl rubber, and the recycled butyl rubber, the composition comprises 5 to 25 parts by weight of the natural rubber, 30 to 80 parts by weight of the butyl rubber, 5 to 20 parts by weight of the liquid rubber, 40 to 90 parts by weight of the recycled butyl rubber, 5 to 35 parts by weight of the recycled carbon black, and 40 to 60 parts by weight of the carbon black, wherein the recycled butyl rubber comprises 40% to 60% by weight of the rubber component, 20% to 40% by weight of the carbon component, and 1% to 10% by weight of the ash component, based on the total weight of the recycled butyl rubber, and the liquid rubber is liquid It comprises polyisobutene, wherein the liquid polyisobutene has a number average molecular weight (Mn) of 500 g / mol to 3000 g / mol, a pour point of -50 ℃ to 30 ℃, and a viscosity of 80 cSt to 13000 cSt, and the regenerated carbon black has an iodine adsorption amount of 70 mg / g to 160 mg / g and an N2 adsorption amount of 60 m 2 / g to 90 m 2 / g, and the sieve residue (325 mesh) is 0 ppm to 40 ppm, and the carbon black has an iodine adsorption amount of 30 mg / g to 50 mg / g and an N2 adsorption amount of 25 m 2 / g to 45 m 2 A rubber composition for a tire inner liner, having a DBP oil absorption capacity of 65 cc / g to 95 cc / g. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 A rubber composition for a tire inner liner, wherein, in claim 1, the butyl rubber is a butyl rubber halogenated. Claim 7 delete Claim 8 delete Claim 9 delete Claim 10 delete Claim 11 A tire comprising an inner liner manufactured using a rubber composition for a tire inner liner according to claim 1. Claim 12 In paragraph 11, the above tire is a tire that is a passenger car tire.
Citation Information
Patent Citations
Rubber composition for inner liner
JP2005247969A
inner liner rubber composition including polybutadienefor tire
KR1020060101659A
Rubber composition for tire innerliner
KR1020090068400A
Tire inner liner rubber composition comprising liquid phase polybutene for improving anti-air permeability
KR1020120038235A