Structure having a substrate-through-via and a method for forming the same
The method addresses non-uniformity in TSV formation by selective etching, dielectric deposition, and CMP to achieve uniform TSV lengths and stability, enhancing yield and enabling direct bonding for semiconductor devices.
Patent Information
- Application Number
- KR1020237025992
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-29
- Filing Date
- 2021-12-27
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2041-12-27
AI Technical Summary
Conventional methods for forming through-substrate vias (TSVs) in semiconductor devices face issues such as non-uniform etching, non-uniform via lengths, and non-uniform dielectric layer deposition, leading to reduced yield and difficulty in achieving flatness suitable for direct bonding, especially in thin dies.
A method involving selective etching, deposition of dielectric layers, and chemical-mechanical polishing (CMP) to uniformize TSV lengths, combined with controlled annealing and electroplating to stabilize copper plugs, ensuring uniformity and stability for direct hybrid bonding.
Improves device yield by achieving uniform TSV lengths and flatness, enabling reliable direct bonding without adhesives, suitable for mass production and multi-die stacking.
Smart Images

Figure 112023083533483-PCT00017_ABST
Abstract
Description
Technology Field
[0001] Cross-reference regarding related applications
[0002] This application claims priority to U.S. Provisional Application No. 63 / 216,389, filed June 29, 2021, with the title "STRUCTURES WITH THROUGH-SUBSTRATE VIAS AND METHODS FOR FORMING THE SAME," and U.S. Provisional Application No. 63 / 131,263, filed December 28, 2020, with the title "STRUCTURES WITH THROUGH-SUBSTRATE VIAS AND METHODS FOR FORMING THE SAME," the full contents of each of these documents being incorporated by reference in this specification. Background Technology
[0003] The field of the present invention relates to a structure having a substrate-through-via and a method for forming the same.
[0004] A semiconductor device, such as an integrated device die or chip, may be mounted or stacked on another device. For example, the semiconductor device may be mounted on a carrier, such as a package substrate, an interposer, a reconfigured wafer or element, or another semiconductor device. As another example, the semiconductor device may be stacked on another semiconductor device, for example, a first integrated device die may be stacked on a second integrated device die. In some configurations, through-substrate vias (TSVs) may extend vertically through the thickness of the semiconductor device to transmit electrical signals through the semiconductor device, for example, from a first surface of the semiconductor device to a second surface on the opposite side of the semiconductor device. There has been a continuing need for improved methods for forming TSVs. Brief explanation of the drawing
[0005] Specific implementation forms will now be described with reference to the following drawings, which are provided for illustrative purposes only and are not limiting. FIGS. 1a to 1f show conventional processing steps for forming TSVs within a device. Figure 2 shows the etching depth map of the processed wafer. Figures 3a and 3b are exemplary wafer maps of an etched wafer. FIGS. 4a to 4i illustrate a method for forming a microelectronic structure according to various embodiments. FIGS. 5a to 5i illustrate a method for forming a microelectronic structure according to various embodiments. FIGS. 6a to 6h illustrate a method for forming a microelectronic structure according to various embodiments. Specific details for implementing the invention
[0006] FIGS. 1a through 1f illustrate various conventional processing steps for forming TSVs within microelectronic structures. Conventionally, forming TSVs can be performed using via-middle or front-side via-last processing methods. Both of these methods are mass manufacturing processes for different dies, for example, including 40 μm thick dies. Both of these processes involve etching through the TSVs into bulk silicon after integrated circuit fabrication. The technical difficulties of these processes increase as the die thickness decreases. These difficulties may include TSV etching uniformity, die thickness uniformity, and the overall quality of the back-side dielectric layer formed.
[0007] In FIG. 1a, the microelectronic structure comprises a portion of a semiconductor wafer (102). The illustrated via structure comprises a via-intermediate structure, wherein the active circuit portion (106) (e.g.) EnterA transistor or other active circuit element) may be formed on or within the active surface of the bulk semiconductor portion (102), one or more insulating layers (112 and 113) may be formed on the active circuit portion (106), and an opening (104) for a through-substrate via (TSV) may be formed through one or more insulating layers (112 and 113) and a portion of the bulk semiconductor portion (102). In some configurations, a metal cladding layer (110) (e.g., a back-end-of-line (BEOL) or redistribution layer (RDL)) may be provided on or within one or more insulating layers.
[0008] A via structure (108) may be provided in FIG. 1b. The via structure (108) may extend into an opening and across insulating layers (112 and 113). In FIG. 1c, a conductive pad (114) may be provided on one or more of the insulating layers and may be electrically connected to the metal coating layer (110). The conductive overburden from electroplating the via structure (108) of FIG. 1b may be removed in FIG. 1c (e.g. Enter (..., polished away). As illustrated in FIG. 1d, a conductive pad (117) is provided on one or more insulating layers (112 and 113) and can be electrically connected to a via structure (108). Additionally, the conductive pad (117) can be configured to be electrically connected to other elements. In some configurations, the conductive pad (117) may be part of a BEOL or RDL.
[0009] As illustrated in FIG. 1e, the front side of the microelectronic structure (114) may be attached to a carrier (120) using an adhesive (118). The carrier (120) may include a temporary handle wafer used to support the microelectronic structure (114) during processing. In some embodiments, the adhesive (118) may include an organic adhesive and may be sensitive to high temperatures. Therefore, using the adhesive (118) to attach the carrier (120) to the microelectronic structure (114) may limit the temperature that can be applied during processing. However, in other embodiments, the carrier (120) may be directly bonded to the front side of the microelectronic structure (114) without the adhesive (118). Although the front side (114) is attached to the carrier (120), the back side of the semiconductor portion (124) may be ground or polished to expose the via (108). As illustrated in FIG. 1f, a dielectric layer (122) may be deposited on the back surface of a semiconductor (124). A back metal coating layer (116), for example, a line-backend (BEOL) or redistribution layer (RDL), may be provided on the dielectric layer (122) and configured to be electrically connected to a via structure (108).
[0010] Conventional via formation processes have several problems that result in non-uniform via lengths. For example, the etching process used to form openings for vias is non-uniform, particularly in the case of high aspect ratio openings used for vias, which leads to via openings with different depths. This non-uniformity present in the produced vias results in yield loss during the TSV reveal process. Furthermore, dielectric deposition, which is part of the TSV reveal process, can be limited by the temporary bonding material used to attach the die to the carrier. The adhesive limits the back-side dielectric deposition temperature and can cause complex issues during various processing steps. Moreover, non-uniformity in the thickness of the temporary bonding layer can be added to the thickness uniformity of the thin silicon wafer. In fact, as shown in FIG. 2, for a 12-inch wafer, the etching process used to form via openings can have a non-uniformity of about 7 microns. In some areas of the wafer, the etching depth (202) may be deeper, but some areas of the wafer will have a lower etching depth (206), and other areas of the wafer will have an etching depth (204) between the lower etching depth (206) and the higher etching depth (202). The varying depth of the etched via opening results in different via structure lengths when a conductive material, for example copper, is filled within the opening.
[0011] As illustrated in FIG. 3a, different via lengths can result in significant losses in yield. For example, if this loss in thickness is combined with wafer thickness variations caused by temporary processes, the TSV yield can be further reduced. For example, dies with TSVs (304) that are too short to be effective, or dies with TSVs (302) that are too long to be effective, cannot be used. For example, some dies in the wafer may have TSVs that are too long (302) and break during grinding or polishing. Other vias are too short (304) and are embedded within the semiconductor portion of the device. Additionally, in some processes, non-uniform TSVs may result in incomplete or non-uniform plating procedures. For example, in such processes, via openings may be uniformly etched, but the plating process passing through high aspect ratio openings may not uniformly fill the via openings. These process variations reduce the number of effective dies (306). Accordingly, non-uniform TSV lengths may result from various different processing methods.
[0012] Figure 3b illustrates thickness variations on an 8" wafer that can be measured after TSV planarization. As can be seen, the wafer thickness can vary by 4 microns. While some areas of the wafer may have a thickness of up to 58.09 microns, other areas may have a thickness of 56.09 microns, and other areas may have a smaller thickness of about 54.67 microns. Additionally, wafer thickness variations can cause some TSVs to become ineffective and reduce the level of process control.
[0013] As previously mentioned, the length of a TSV can vary significantly across the wafer after the back surface of the semiconductor part is ground to expose the TSV, for example, due to die thickness non-uniformity and TSV aperture etching non-uniformity. Therefore, when the back surface of the bulk semiconductor part is ground or otherwise thinned, the exposed vias may protrude by a varying length from the back surface of the thinned semiconductor part, while some vias, as previously mentioned, may remain embedded within the semiconductor part without being exposed. To reduce the non-uniform length of the TSV while preventing damage to the protruding TSV, one or more back dielectric layers may be provided on the back surface of the semiconductor part and on the TSV. Although it may be possible to employ solder bumping despite a certain degree of TSV height variability, such variability results in a lack of flatness and makes stacking difficult. Some stacking techniques, such as direct hybrid bonding, are particularly sensitive to topographic variations.
[0014] For example, in some processes, after the silicon relative to the liner of the TSV is selectively removed by initial back-side silicon grinding and wet or dry etching methods, about 6 to 7 microns of the TSV protrude from the back side of the semiconductor portion. A barrier layer, for example, a dielectric barrier layer, such as silicon nitride, silicon oxynitride, silicon carbonitride, diamond carbon, or any other suitable dielectric barrier material layer, may be deposited on the back side of the semiconductor portion, on the sidewall of the exposed TSV, and on the exposed end face of the exposed TSV. A second dielectric layer, for example, silicon oxide or any other suitable dielectric, may be deposited on the dielectric barrier layer, including on the upper surface of the barrier layer, on a portion of the barrier layer extending along the sidewall of the exposed TSV, and on a portion of the barrier layer disposed along the end face of the exposed TSV. After depositing the back dielectric layer(s), portions of the vias and dielectric layer(s) can be polished or otherwise removed to flatten the vias and reduce non-uniformity.
[0015] In other processes, thinner layers of the first dielectric barrier layer and / or the second dielectric barrier layer may be deposited on thinned semiconductor parts and vias. For example, in other processes, the dielectric layer(s) may be only 1 or 2 microns thick, and may be much thinner than, for example, the length of the protrusion of the via. When the via and dielectric layer(s) are polished, some of the vias will break, causing the ends of the vias to be embedded within the semiconductor part and sunken relative to the back surface of the semiconductor part. Broken TSVs can reduce device yield.
[0016] In some of these processes, the selected metal within the TSV can significantly alter TSV performance. For example, in some processes, copper (Cu) can be an effective deposition metal. When used within a TSV, copper is an alloy metal that can alter the expansion and polishing characteristics of the TSV. Copper located at the bottom of etched vias is typically confined and may not be annealed at the same rate or temperature as free copper. These differing properties can result in Cu TSVs that lack stabilized crystallographic properties before the TSV is exposed during the deposition process. Furthermore, the TSV metal cladding may contain metallic or organic impurities that are unsuitable for reliable direct bonding, for example, by the Direct Bond Interconnect® process. Moreover, it has been found that shrinkage of the TSV during storage or heat treatment leads to topographical problems, such as the formation of rims or trenches within the isolating oxide surrounding the TSV.
[0017] Some of the major problems that reduce the yield of conventional TSV formation processes include non-uniformity of TSV etching depth and TSV failure during polishing. TSVs can have a typical depth variation of 2 to 4 µm out of a total depth of 55 µm on a 300 mm wafer. Such depth variation can make it difficult to achieve uniform surface bonding. Furthermore, non-uniform TSVs can cause failure during processing, leading to lower yields. Silicon wafers can be planarized using chemical mechanical polishing (CMP). Some TSVs may fail during CMP planarization. This failure can be partially caused by excessive TSV exposure, which is often caused by TSV depth variation.
[0018] Conventionally, back-side TSV processing has not been used for direct bonding during mass production. Conventional procedures for flattening TSVs on the back side of a wafer may also rely on patterning copper pads and adding solder bumps to the wafer. Furthermore, conventional back-side processing does not protect the TSVs from breakage and may not achieve a flatness suitable for direct bonding. Due to the length of the polishing time, the number of polishing cycles (which can range from 4 to 6 cycles and take 2 hours of machine time), the amount of material deposited (5 μm), the amount of material removed (2-4 μm depending on the deposited oxide), and the total annealing time used between polishes (3 to 5 one-hour annealing cycles), this process may not be suitable for mass production.
[0019] The various embodiments disclosed herein can improve device yield by ensuring that the TSV length is uniform across the entire thinned wafer. Some embodiments may use wet etching to lower the copper TSV surface to a few microns below the silicon surface. In some embodiments, the surrounding silicon bulk helps to confine and stabilize the copper within the TSV. In some embodiments, a barrier layer is deposited before the deposition of the copper seed layer. In some embodiments, an electroplating technique is used to fill vias. In some embodiments, some TSVs may be deeper than others, and an electroplating process may be used to accommodate additional depth of broken TSVs.
[0020] In some embodiments, the annealing process stabilizes the copper plug material to provide chemical and structural properties similar to the device-side copper used for bonding to the copper plug material. In some embodiments, the annealing process stabilizes the copper plug material to have the same impurity and texturing properties as the device-side bonding copper. In some embodiments, plated copper may be annealed as a direct bonding interface. Such annealing can stabilize the copper plug material and cause this plug material to chemically and physically resemble the device-side direct bonding interface copper pad.
[0021] In some embodiments, the CMP used on the copper layer may include a standard direct bonding interface CMP slurry and process. In some embodiments, the CMP for the TSV may be identical to the device-side CMP in terms of slurry usage and machine time. In some embodiments, the CMP parameters may be identical or similar to the device-side CMP parameters. In some embodiments, this CMP uniformity may be achieved with or without additional photolithography steps. In some embodiments, the only photolithography step used during the CMP process may be a blanked backside treatment.
[0022] FIGS. 4a through 4i illustrate a method for forming a microelectronic structure according to one embodiment. As illustrated in FIG. 4a and as previously described, the TSV structure (410) may be provided at least partially through the thickness of a substrate comprising a bulk semiconductor portion (404). In some embodiments, the bulk semiconductor portion (404) may comprise silicon, germanium, silicon carbide, or any other suitable semiconductor material. One or more lining layers (412) may be provided within an opening from the front surface (406) of the substrate. In some embodiments, one or more lining layers (412) may comprise a dielectric liner (415). The dielectric liner (415) of one or more lining layers (412) may comprise silicon nitride, silicon oxynitride, silicon carbonitride, diamond-like carbon, and any other suitable dielectric material. In some embodiments, one or more lining layers (412) may additionally or alternatively include a first lining barrier layer (413). Although FIG. 4a schematically illustrates the layer (412) as a single layer, it should be understood that the layer (412) may include a drainage layer or, for example, a sub-layer including a dielectric liner (415) and a lining barrier layer (413). A first conductive via (402) may be provided within an opening on the lining layer(s) (412). In various embodiments, the first conductive via (402) may include copper, but other suitable metals may also be used. The first conductive via portion (402) may be provided from the front surface of the substrate (406). The first lining barrier layer (413) may include a conductive barrier to reduce the diffusion of the conductive via material. The first lining barrier layer (413) may be a material different from the conductive material of the first (402) and second (424) conductive vias.The first lining barrier layer (413) may be configured to reduce the diffusion of the conductive material of the first (402) and / or second (424) conductive via portions into the surrounding dielectric and / or semiconductor material. Examples of materials used for the first lining barrier layer (413) include metal and metal nitride materials, such as titanium nitride, tantalum nitride, and any other suitable metal and metal nitride materials. The first conductive via portion (402) may be electroplated over a seed layer within the opening. The front or side of the wafer, for example, the first side (406), may include the active side of the semiconductor portion having an active integrated circuit portion, such as a transistor formed in or on the active side. The front or first side (406) of the wafer may be mounted on a carrier (414). In some embodiments, the carrier (414) may serve as a temporary handle wafer. In other embodiments, the microelectronic structure may be attached to the carrier (414) using an adhesive. In other embodiments, the microelectronic structure may be directly attached to the carrier (414) without an interposed adhesive, using a direct bonding technique described in more detail below. As illustrated in FIGS. 4a through 4c, the TSV (410) may have a variable height across the entire substrate due to variable etching through a significant depth through the bulk semiconductor.
[0023] In FIG. 4b, the second surface (408), which is the rear surface of the semiconductor portion (which is also the rear surface of the substrate in this stage), can be thinned by dry etching or otherwise removed to expose the TSV (410). As illustrated, the TSV (410) may protrude beyond the rear surface of the semiconductor portion (408). As previously mentioned, the length of the TSV (410) may be non-uniform across the wafer, causing the TSV (410) to protrude by varying lengths over the semiconductor portion (416). The etching process may leave the via structure (410) in a non-contacted state, thereby maintaining a state in which one or more lining layer(s) (412), including a dielectric liner (415) and a first lining barrier layer (413), are positioned on and along the sidewall (411) of the first conductive via portion. In FIG. 4c, one or more dielectric layers (418) may be provided, i.e., deposited along the sidewall (411) of the via structure (410) and on the end surface of the via structure (410) on the upper surface (408) of the bulk semiconductor portion (416) to form the back surface of the substrate (408). Although FIG. 4c schematically illustrates the layer (418) as a single layer, it should be understood that the layer (418) may include multiple layers or sub-layers. In various embodiments, the dielectric layer(s) (418) may be a first dielectric barrier layer (419) provided on the bulk semiconductor portion (416) and on the via structure (410). The dielectric layer(s) (418) may further include a second dielectric layer (421) on the first dielectric barrier layer (419). In various embodiments, the first dielectric barrier layer (419) may comprise a material for reducing copper migration, such as silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, diamond carbon (DLC), or any other suitable dielectric barrier layer material.The second dielectric layer (421) may comprise a dielectric material with a lower k, and may be an inorganic dielectric, such as silicon oxide. As illustrated in FIG. 4c, the TSV (410) may protrude beyond the semiconductor portion (408) by a distance ranging from about 0 to 10 microns, 1 to 7 microns, or 5 to 6 microns. As further described herein, the TSV (410) may be broken as seen in the TSV (420) and may be sunken into the semiconductor portion (416) and / or dielectric layer(s) (418) by a distance ranging from 0 to 10 microns, 1 to 7 microns, or 2 to 6 microns. The thickness of the dielectric layer(s) (418) may be in the range of about 2 to 7 microns, in the range of about 3 to 7 microns, in the range of 4 to 6 microns, or in one embodiment, about 5 microns.
[0024] In FIG. 4d, the via structure (410) and the dielectric layer(s) (418) may be planarized using a chemical-mechanical polishing (CMP) process applied, for example, to the back surface of the substrate (408). As described herein, the planarization process may break one or more of the TSVs (410), for example, intermediate TSVs (420). In FIG. 4d, for example, an intermediate TSV (420) is broken so that the TSV (420) becomes embedded within or sunken beneath the dielectric layer(s) (418) and / or semiconductor part (416). As previously mentioned, a broken TSV, such as an intermediate TSV (420), can reduce the device yield for the wafer. Depending on the selected chemical for the CMP slurry, some or all of the other TSVs (410) may also be sunken beneath the dielectric layer(s) and / or semiconductor part.
[0025] In FIG. 4e, the first conductive via portion (402) may be optionally etched to be recessed below the back surface of the substrate (408), for example, below the dielectric layer(s) (418) and / or semiconductor portion (408). Because the intermediate TSV (420) is broken, the depth of etching for the intermediate via structure (420) is deeper than the etching for the other via structure (410). In various embodiments, optional copper wet etching may be performed to etch only a portion of the first conductive via portion (402). Preferably, in the illustrated embodiment, all of the TSVs (410) throughout the substrate (416) are recessed to some extent below the upper surface of at least the added dielectric layer(s) (418). In other embodiments, the recessing of the TSV (410) may be achieved during the CMP described for FIG. 4d. In another embodiment, not all TSVs (410) are recessed, and only some TSVs (410) are recessed depending on whether a separate recessing process is employed. For example, in some embodiments, a conventional CMP process is employed in which some TSVs (410) are substantially recessed below the surface (408), for example, due to breakage.
[0026] As illustrated in FIG. 4f, in order to improve yield and provide a flattened, high-quality bonding surface, a second barrier layer (422) may be provided over the exposed end surface of the first conductive via portion (402) and along the lining barrier layer (412). A seed layer (not shown) may be provided over the second barrier layer (422), and a second conductive via portion (424) may be provided over the second barrier layer (422) from the back surface of the substrate (416), for example, by electroplating. The microelectronic structure may be annealed, which preferably promotes grain growth to improve direct bonding. Preferably, as opposed to the plating process selected to improve filling of deep vias with a high aspect ratio, which was originally used to fill the TSV (410) vias, both a deposition process, e.g., electroplating, and an annealing process can be selected to prepare for direct hybrid bonding.
[0027] In various embodiments, an alloy additive may be provided to the conductive material of the TSV (410). The alloy additive may be provided to control thermal expansion and / or improve the corrosion resistance of the conductor. In some embodiments, the conductor is copper, silver, gold, or any other suitable conductive material. The alloy additive material(s) may include metallic elements, e.g., beryllium, indium, gallium, nickel, and manganese, and typically represent less than 5 atomic % and more specifically less than 2 atomic % of the TSV (410). The alloy additive may be provided as part of the seed layer or the second barrier layer (422) and may diffuse from it. These alloy elements may be present in different amounts to affect the hardness, corrosion resistance, and / or pin grain formation during subsequent annealing of the TSV (410). Because larger grains are preferred within the second conductive portion to aid in interdiffusion in the direct metal-metal bonding process, the first conductive portion (402) may contain a smaller percentage of alloying elements compared to the second conductive portion (424). For example, in some embodiments, the second conductive via portion (424) may contain at least less than 5%, at least less than 10%, at least less than 15%, or at least less than 20% of alloying elements compared to the first conductive via portion.
[0028] Additionally, one or more organic additives, such as a leveler, a suppressor, and an accelerator, may be provided to the plating bath during the formation of the TSV (410) to improve filling. In various embodiments, different additives and / or different ratios of additives may be provided when plating the second conductive via (424) compared to the type or amount of additive used when plating the first conductive via (402) that fills the opening. For example, in some embodiments, the additive may be used when plating both the first (402) and the second (424) conductive vias, but the amount of additive used for the first conductive via (402) may differ significantly from the amount used for the second conductive via (424). In some embodiments, more additives may be used when plating the first conductive via (402) than when plating the second conductive via (424). In some embodiments, additives, such as organic additives, may be provided during plating the first conductive via (402), for example, to improve filling, but different proportions or different types of organic additives may be provided during electroplating of the second conductive via (424). In various embodiments, the plating bath for the first conductive via (402) may contain a higher percentage of organic additives compared to the plating bath for forming the second conductive via (424). Thus, the first conductive via (402) may have a higher percentage of impurities such as sulfur, oxygen, nitrogen, and / or carbon compared to the second conductive via (424).In various embodiments, the first conductive via (402) may be formed in a plating bath having a higher concentration of leveler, e.g., Janus Green, which introduces more impurities such as nitrogen, carbon, and / or oxygen compared to the second conductive via (424). In parts of both (402 and 424), impurities from the additive may be measured in ppm (parts per million).
[0029] After electroplating, impurities from the plating additive, such as carbon, nitrogen, sulfur, and oxygen among other impurities, may be contained in the first (402) and / or second (424) conductive vias. In some embodiments, the amount of impurities present in the first conductive via (402) may be greater than the amount of impurities present in the second conductive via (424). In some embodiments, only a trace amount of impurities may be present in the second conductive via (424). Furthermore, the impurities present in the second conductive via (424) may have a different composition and / or concentration compared to the first conductive via (402). This composition may be selected to affect the grain size, the orientation of interconnections that may be formed by the second conductive portion, or thermal stability. The impurities may include other material elements present in the conductive via at a concentration lower than 2 atm%, for example, less than 100 ppm or less than 50 ppm. In one embodiment, the impurities in the second conductive via (424) may be less than the impurities in the first conductive via (402). For example, in some embodiments, the second conductive via (424) contains at least 5% less, at least 10% less, or at least 20% less non-copper elements (e.g., Enter It may contain metallic alloy elements, or impurities from plating bath additives.
[0030] In FIG. 4g, portions of the second conductive via (424) and the second barrier layer (422) located on the dielectric layer (418) can be removed, for example, using a CMP process applied to the back surface of the substrate. The polishing process can expose and flatten the dielectric layer(s) (418) and can serve as a preparatory step for direct bonding, that is, a very high degree of polishing achieves sufficient planarity for direct bonding. Preferably, the intermediate damaged TSV (420) is repaired, the metal recess is provided to an appropriate depth, and the polished dielectric layer(s) (418) and the second conductive via (424) can be used in the direct bonding process. For example, the plating and annealing process may form grains, e.g., copper, gold, or silver grains, or a metal texture, e.g., copper, oriented along a 111 crystal plane that is nearly perpendicular to the bonding plane, which can enhance metal diffusion and bonding during the direct bonding process. In various embodiments, the metal texture may be oriented to have geometric components that are schematically perpendicular to the bonding plane. In some embodiments, the second conductive via portion (424) may have a first proportion of the 111 plane oriented within 30° of the vertical axis, e.g., within 30° of the vertical axis extending along the longitudinal dimension of the via structure, within 20° of the vertical axis, or within 10° of the vertical axis. The second conductive via (424) may have a second ratio of a 111 plane oriented within 30° of the vertical axis, for example, within 30° of the vertical axis extending along the longitudinal dimension of the via structure, within 20° of the vertical axis, or within 10° of the vertical axis. In some embodiments, the second ratio may be greater than the first ratio.In the illustrated embodiment, where either CMP selection (see FIG. 4d and corresponding description) or subsequent recessing (see FIG. 4e and corresponding description) is selected to ensure some degree of recessing across the substrate, each TSV (410) may include both the first (402) and second (424) conductive vias. In other embodiments, not all TSVs (410) are recessed across the entire substrate in the stage of FIG. 4e, and only some TSVs (410) include the second conductive vias (424). In any case, the CMP process selected to obtain the structure of FIG. 4g may be selected to facilitate subsequent direct hybrid bonding. Accordingly, each TSV (410) may be sunken below the upper surface of the dielectric layer(s) (418) by, for example, less than 40 nm, less than 30 nm, less than 20 nm, less than 15 nm, or less than 10 nm, but more than about 5 nm, for example more than about 2 nm.
[0031] As illustrated in FIG. 4h, the aforementioned microelectronic device can be utilized in a multi-die or multi-device stack. For example, the first stacked die (434) can be directly bonded to the base wafer (432) without adhesive. In some embodiments, the front active surface can be bonded to the base wafer. As described below, the contact pad (426) of the first die can be directly bonded to the contact pad (426) of the wafer without adhesive, and the non-conductive region can be directly bonded to the corresponding non-conductive region of the wafer without adhesive (430). Additional devices can be stacked and directly bonded to the back surface of the microelectronic structure. For example, as illustrated, the contact pad (426) of the second device or die (436) can be directly bonded to the exposed TSV structure (410) of the first device (434) without adhesive. The non-conductive region of the second element or die (436) may be directly bonded to the dielectric layer(s) (418) without an adhesive. Additional elements may be directly bonded to the second element or die and stacked to form any number of elements within the directly bonded structure. In some other applications, wafers processed by the method described herein may be assembled or stacked and directly bonded to each other without an interposed adhesive layer.
[0032] FIG. 4i illustrates a via structure (410) formed using various disclosed embodiments. As illustrated, the microelectronic structure may include a bulk semiconductor portion (404) having a first / front side (406) and a second side / back side opposite to the first side (408). In some embodiments, the second side (408) may include an active side having an active circuit formed in or on the second side. Additionally or alternatively, in some embodiments, the first side (406) may include an active side having an active circuit formed in or on the second side. In other embodiments, the first side (406) may include a non-active side without an active circuit. The via structure (410) may be disposed within an opening while extending along a direction not parallel to the first side through at least partially, for example, completely through the bulk semiconductor portion (404). The via structure may include a first conductive via portion (402), a second conductive via portion (424), and a second barrier layer (422). The second barrier layer (422) includes a first portion (440) disposed between the first conductive via portion (402) and the second conductive via portion (424). The second barrier layer (422) may further include a second portion (442) disposed along the sidewall (411) of the second conductive portion (402). The second conductive via portion (424) may extend from the second barrier layer (440) to at least the surface of the substrate (408). As mentioned above, the second conductive via portion (424) may have a different composition from the first conductive via portion (402).
[0033] Both the first (402) and second (424) conductive vias may be formed of, for example, copper, but have different types and / or concentrations of alloying elements and impurities and / or different grain sizes and / or orientations derived from, for example, the type of leveler, inhibitor, accelerator, and plating current density used in the electroplating process. For example, the first (402) and / or second (424) conductive vias may have different proportions of non-copper elements, such as metallic alloying elements, or impurities from plating bath additives. The first via (402) may have more non-copper elements than the second (424) via. In some embodiments, the first via (402) may have alloying elements, such as Be, Mn, Ni, included from the barrier layer (412) or through diffusion through the seed layer. The second via (424) may not have these non-copper elements, or may have only trace levels of impurities. The second via (424) may have these non-copper elements, but in smaller amounts compared to the first via. During plating, alloy material(s) included through the barrier layer(s) (412) and / or seed layer may be provided to the pin granules of the first via (402) in some configurations. Additionally, one or more organic additives may be provided during plating of the first via (402) to improve filling, and the additives may not be used in the second (424) conductive via. In other embodiments, an organic or other additive may be provided for both the first (402) and second (424) via sections, but the first via section (402) may have a higher concentration of impurities left by the additive after plating. As described herein, impurities such as sulfur, oxygen, carbon, or nitrogen may be present in a higher concentration in the first via section (402) compared to the second via section (424) of the TSV (410).In some embodiments, the composition of non-copper elements in the first conductive via (402), including impurities from alloy elements and additives, is higher than that in the second conductive via (424). For example, in some embodiments, the second conductive via (424) may have at least less than 5%, at least less than 10%, at least less than 15%, or at least less than 20% of non-copper elements compared to the first conductive via (402). The composition and grain structure of the first conductive portion (402) may be the result of a treatment selected to optimize filling of deep high aspect ratio vias, and the composition and grain structure of the second conductive portion (424) may be selected to optimize subsequent direct hybrid bonding.
[0034] As illustrated in FIG. 4i, the dielectric layer (418) may be disposed on the bulk semiconductor portion (404), and the second (424) conductive via portion extends through the dielectric layer (418) so that the end of the second conductive via portion (424) is at the same height as the upper surface (418) of the dielectric layer, or is slightly recessed relative to the upper surface (418) of the dielectric layer, for example, by less than about 40 nm, less than about 30 nm, less than about 20 nm, less than about 10 nm, or less than about 5 nm. The dielectric layer (418) may include a flattened dielectric coupling layer configured for direct coupling to another device. The dielectric layer (418) may further include a dielectric barrier layer on the bulk semiconductor portion (404), and the flattened dielectric coupling layer is disposed on the dielectric barrier layer. The first lining barrier layer (412) may extend along the sidewall (411) of the first (402) and second (424) conductive portions. As illustrated, the second barrier layer (440) may include a second portion (442) extending along the first barrier layer (412) between the first barrier layer (412) and the second conductive via portion (424). Thus, the total barrier thickness is greater between the second conductive portion (424) and the bulk substrate (404) compared to the thickness between the first conductive portion (402) and the bulk substrate (404), and may include two identifiable barrier layers, which may or may not have different compositions.
[0035] FIGS. 5a through 5i illustrate a method for forming a microelectronic structure according to other embodiments. Unless otherwise indicated, the embodiments of FIGS. 5a through 5i may be identical or approximately similar to similar components of FIGS. 4a through 4i. For example, the steps of FIGS. 5a through 5e may be the same as the steps described above in conjunction with FIGS. 4a through 4e. However, in the example of FIG. 5f, a barrier layer provided over the first conductive via portion (410) may not exist. Rather, the second conductive via portion (424) may be directly plated on the first conductive via portion (410), or only on the interposed seed layer, without a barrier layer interposed in the bulk semiconductor portion (416). As previously described, the structure of FIG. 5f may be annealed, which can promote copper grain growth beneficial for direct bonding.
[0036] In various embodiments, the embedded conductive material of the first conductive via (402) may be more constrained than the upper portion of the conductive material of the second conductive via (424). During annealing, the first (402) and second (424) conductive vias may form different metal textures and / or have different concentrations of impurities from non-copper elements, such as alloy elements and / or plating additives. For example, the first metal texture of the first conductive via (402) may be different from the second metal texture of the second conductive via (424). In various embodiments including the embodiments disclosed in FIGS. 4a through 4i and FIGS. 5a through 5i, the crystal structure of the second conductive via (424) may have grains oriented perpendicularly along a crystal plane that is non-parallel to the bonding interface, for example, generally perpendicular, to enhance metal diffusion during direct bonding, for example, copper diffusion. The grains may have geometric components that are approximately perpendicular to the bonding interface. In some embodiments, the first (402) and second (424) conductive vias may comprise different metals or different alloys. For example, in some embodiments, the first conductive via (402) may comprise a copper alloy, and the second conductive via (424) may comprise substantially pure copper.
[0037] FIGS. 5g and 5h may be schematically similar to the steps presented in FIGS. 4g and 4h. FIG. 5i illustrates a microelectronic structure without the interposed barrier layer of FIG. 4i. As shown in FIG. 5i, the second conductive via (424) may be formed after and separately from the first conductive via (402). Unlike in FIG. 4i, there is no interposed barrier layer (440) between the first conductive via (402) and the second conductive via (424).
[0038] FIGS. 6a through 6h illustrate other embodiments that enable the formation of conductive vias (606) having a schematically uniform length while avoiding degradation of the vias (606), e.g., copper vias or other suitable conductive metals, and / or contamination of the semiconductor portion (604), e.g., silicon or other suitable semiconductors. Unless otherwise indicated, the components of FIGS. 6a through 6h may be schematically similar to the components of FIGS. 4a through 5i. For example, as previously described and as illustrated in FIG. 6a, a semiconductor device (604), e.g., a semiconductor wafer, may have a plurality of conductive vias (606) formed within the semiconductor portion (604), e.g., silicon bulk or device portion. The front side of the bulk semiconductor (610) is depicted facing upward, and the rear side opposite the bulk semiconductor (612) is depicted facing downward. In various embodiments, the front side (610) may include the active side of the semiconductor device so that an active circuit may be formed on or near the front side (610). A dielectric liner and / or barrier layer (608) may line an opening in which a via (606) is disposed. One or more front-side dielectric layer(s) (602) may be provided on the front side of the semiconductor part (610). Although FIG. 6a schematically illustrates the layer (602) as a single layer, it should be understood that the layer (602) may include multiple layers or sub-layers. The front-side dielectric layer(s) (602) may include any suitable type of dielectric material(s), such as silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide nitride, diamond carbon (DLC), and any other suitable dielectric material.
[0039] As described above, the depth of the opening into which the conductive via (606) material is deposited, for example, by electroplating, can vary, which may result in the formation of vias having non-uniform lengths. If uniformity is lacking, it may be difficult to expose the vias from the back surface of the semiconductor device (612). In fact, the etching variation of the via opening (606) can be about 2-3 microns or more, so that a variation of more than 50% in the TSV height may exist. In the process of FIGS. 4b and FIGS. 5b, the semiconductor portion (604) is dry-etched to expose the vias (606), which may protrude at different heights above the semiconductor material (604). However, if a semiconductor material (604), such as silicon, is dry-etched using an etchant such as SF6, the copper via material may be severely worn away, particularly if the dielectric liner and / or lining barrier layer (608) is etched before the via (606) is properly exposed. Furthermore, the conductive via (606) roll, for example If processed by CMP, grinding, and other processing methods, some of the conductive material of the via, e.g., copper material, may contaminate the semiconductor part (604), e.g., silicon.
[0040] Accordingly, unlike the processes of FIG. 4b and FIG. 5b, in FIG. 6b, the back surface of the semiconductor part (612) can be ground and polished, for example using CMP, to expose vias (606). The grinding and polishing process can expose the conductive vias (606) uniformly, which can accommodate uneven lengths of vias (606) prior to grinding and polishing. For example, the back surface of the semiconductor device (612) can be ground and polished until all vias (606) are exposed on the flattened, ground, and polished back surface of the semiconductor device (614). Thus, in the illustrated embodiment, the grinding and polishing process can be used to expose vias (606) having roughly uniform lengths. In other embodiments such as those described above in conjunction with FIGS. 4a to 5i, it may not be desirable to use CMP to expose the via (606) because exposing the via (606), which may contain copper among other materials, to CMP can contaminate the semiconductor part, e.g., silicon. In these embodiments, as described above, an etching process, e.g., SF6 etching, may be used to expose the via (606).
[0041] Returning to FIG. 6c, the conductive via (606) may be etched from the back surface (614) to form an etched recess within a conductive material that may contain copper. For example, the conductive material may be etched to a depth of about 1 micron in a range of 0.25 to 3 microns, a range of 0.5 to 3 microns, for example, in one embodiment. FIG. 6d, a first back dielectric layer (616) may be provided, for example, deposited on the ground and polished back surface of the semiconductor part (618) and into the etched recess formed within the via (620). As illustrated, the first back dielectric layer (616) may extend within the recess over the copper via and border a dielectric liner and / or barrier layer disposed within the opening (620). In some embodiments, the first back dielectric layer (616) may comprise a plurality of layers. For example, in the illustrated embodiment, the first back dielectric layer (616) may comprise a first dielectric layer (617), e.g., a low-temperature silicon nitride dielectric layer, disposed on the back surface of the semiconductor portion and on the via (606), and a second dielectric layer (619), e.g., a low-temperature silicon oxide dielectric layer, disposed on the first dielectric layer (617). For example, in various embodiments, the first (617) and / or second (619) dielectric layers may be formed using a low-temperature chemical vapor deposition (CVD) process. However, in other embodiments, the first back dielectric layer (616) may comprise only one dielectric layer or three or more dielectric layers.
[0042] Returning to FIG. 6e, the back surface of the semiconductor device (614) can be polished to remove a first portion of the first back dielectric layer (616) located on the semiconductor portion (604) in order to expose the semiconductor portion (604) (e.g., using CMP). A second portion of the first back dielectric layer (620) can remain in a state where it is placed over the conductive via (606) within a recess as shown in FIG. 6e. The remaining second portion of the first back dielectric layer (620) can serve to protect the conductive via material during the subsequent dry etching of the semiconductor portion (604) shown in FIG. 6f. Thus, the dry etching of FIG. 6f can uniformly expose the via (606), and the second portion of the first back dielectric layer (620) can serve to protect copper during the dry etching, for example using SF6. Furthermore, in the step of FIG. 6f, an etchant having high selectivity for silicon on the first back dielectric layer (620), such as SF6, may be used, which may include silicon oxide on the exposed surface. Therefore, as shown after the dry etching of FIG. 6f, the via (606), the first portion of the first back dielectric layer (620), and the dielectric liner / barrier layer (608) may protrude relative to the etched surface on the back of the semiconductor portion (604). In various embodiments, the via may protrude by an amount ranging from 3 microns to 4 microns.
[0043] Returning to FIG. 6g, the second back dielectric layer(s) (624) may be provided, for example, deposited on the etched surface (622) of the semiconductor part (604), along the sidewall of the exposed lining layer of the via (606), on the end of the lining layer (608), and on the second portion of the first back dielectric layer (620). In some embodiments, the second back dielectric layer (624) may comprise a plurality of layers. For example, in the illustrated embodiment, the second back dielectric layer may comprise a first dielectric layer (625), for example, a low-temperature silicon nitride dielectric layer, disposed on the etched surface of the semiconductor part (622) and on the second portion of the first back dielectric layer (620), and a second dielectric layer (627), for example, a low-temperature silicon oxide dielectric layer, on the first dielectric layer (625). However, in other embodiments, the second back dielectric layer (624) may comprise only one dielectric layer or three or more dielectric layers. The thickness of the second back dielectric layer (624) may be any suitable thickness within the range of 4 to 5 microns in various embodiments, for example. Preferably, the thickness of one or both of the first (625) and second (627) back dielectric layer(s) may be selected to provide suitable support or stress compensation, particularly for a thinned die.
[0044] As shown in FIG. 6h, the back surface of the semiconductor device is polished (for example Enter(e.g., CMP) the via (606) can be exposed. In particular, polishing can remove the portion of the second back dielectric layer (624) placed over the first back dielectric layer (616), i.e., the remaining second portion of the first back dielectric layer (620), and can thin the portion of the second back layer above the semiconductor part. Thus, in the structure of FIG. 6h, the second back dielectric layer (624) can be placed over the etched surface (622) of the semiconductor part (604) and can be around the via lining layer(s) (608), for example, the lining dielectric layer and / or the lining barrier layer. In various embodiments, to prepare the back of the semiconductor device for direct bonding, polishing can also serve to sink the conductive material within the via (606) relative to the second back dielectric layer (624). In various embodiments, polishing may cause the conductive material to be recessed by an amount within the range of 1 nm to 20 nm or within the range of 1 nm to 10 nm. As previously described, the semiconductor device may be directly bonded and / or stacked with other devices. The front-side dielectric layer(s) (602) may also be removed to expose vias (606) on the front side, and one or more additional devices may be stacked or directly bonded on the front side of the semiconductor device.
[0045] Examples of direct coupling and directly coupled structures
[0046] The various embodiments disclosed herein relate to a directly bonded structure in which two elements can be directly bonded to each other without an interposed adhesive. Two or more semiconductor elements (e.g., an integrated device die, a wafer, etc.) may be stacked on top of each other or bonded to form a bonded structure. A conductive contact pad of one element may be electrically connected to a corresponding conductive contact pad of another element. Any appropriate number of elements may be stacked within the bonded structure.
[0047] In some embodiments, the devices are directly bonded to each other without adhesive. In various embodiments, the non-conductive or dielectric material of the first device may be directly bonded to a corresponding non-conductive or dielectric field region of the bonding layer of the second element without adhesive. The non-conductive material may be referred to as the non-conductive bonding region or bonding layer of the first device. In some embodiments, the non-conductive material of the first device may be directly bonded to a corresponding non-conductive material of the second device using an insulator-insulator (e.g., dielectric-dielectric) bonding technique. For example, the dielectric-dielectric bond may be formed without adhesive using direct bonding techniques disclosed in at least U.S. Patent Nos. 9,564,414, 9,391,143 and 10,434,749, the entire contents of each of which are incorporated herein by reference in all respects.
[0048] In various embodiments, the hybrid direct bond may be formed without an interposed adhesive. For example, the dielectric bonding surface may be polished to a high degree of smoothness. The bonding surface may be cleaned and exposed to plasma and / or an etchant to activate the surface. In some embodiments, the surface may be terminated with species after or during activation (e.g., during the plasma and / or etching process). Theoretically, but not limited to, in some embodiments, the activation process may be performed to break chemical bonds at the bonding surface, and the termination process may provide additional chemical species to the bonding surface to improve bonding energy during direct bonding. In some embodiments, activation and termination are provided in the same step, for example by a plasma or wet etchant to activate and terminate the surface. In other embodiments, the bonding surface may be terminated in a separate process to provide additional species for direct bonding. In various embodiments, the terminating species may include nitrogen. Furthermore, in some embodiments, the bonding surface may be exposed to fluorine. For example, one or more fluorine peaks may be present near the layer and / or bonding interface. Thus, in a directly bonded structure, the bonding interface between the two dielectric materials may include a very smooth interface having a high nitrogen content and / or fluorine peaks. Additional examples of activation and / or termination treatments may be found in the entirety of U.S. Patent Nos. 9,564,414; 9,391,143; and 10,434,749, the entire contents of each of which are incorporated by reference in all respects herein.
[0049] In various embodiments, the conductive contact pad of the first element may be directly coupled to the corresponding conductive contact pad of the second element. For example, a hybrid coupling technique may be used to provide a conductor-conductor direct coupling along a coupling interface comprising directly covalently coupled dielectric-dielectric surfaces formed as described above. In various embodiments, the conductor-conductor (e.g., contact pad-contact pad) direct coupling and the dielectric-dielectric coupling may be formed using the direct hybrid coupling technique disclosed in at least U.S. Patent Nos. 9,716,033 and 9,852,988, the entire contents of each of which are incorporated herein in their whole and in all respects.
[0050] For example, as described above, dielectric bonding surfaces may be formed and directly bonded to each other without an interposed adhesive. Conductive contact pads (which may be surrounded by a non-conductive dielectric field region) may also be directly bonded to each other without an interposed adhesive. In some embodiments, each contact pad may be recessed below the outer surface (e.g., top surface) of the dielectric field or the non-conductive bonding region, for example, by less than 30 nm, less than 20 nm, less than 15 nm, or less than 10 nm, for example, within the range of 2 nm to 20 nm, or within the range of 4 nm to 10 nm. In some embodiments, the non-conductive bonding regions may be directly bonded to each other without an adhesive at room temperature, and then the bonded structure may be annealed. Upon annealing, the contact pads may expand and come into contact with each other to form a direct metal-to-metal bond. Usefully, by using hybrid bonding techniques such as direct bonding interconnects, commercially available from Xperi, San Jose, CA, or the DBI® technique, high-density pads having small or fine pitches for a regular array, for example, can be made possible through the direct bonding interface. In some embodiments, the pitch of the bonding pads, or the conductive traces embedded within the bonding surface of one of the bonded elements, may be less than 40 microns, less than 10 microns, or even less than 2 microns. For some applications, the ratio of the pitch of the bonding pad to one of the dimensions of the bonding pad is less than 5 or less than 3, and preferably sometimes less than 2. In other applications, the width of the conductive trace embedded within the bonding surface of one of the bonded elements may range from 0.3 to 3 microns. In various embodiments, the contact pads and / or traces may comprise copper, but other metals may also be suitable.
[0051] Accordingly, in a direct bonding process, the first element can be directly bonded without an adhesive interposed in the second element. In some configurations, the first element may include an individualized element, such as an individualized integrated device die. In other configurations, the first element may include a carrier or substrate (e.g., a wafer) comprising a plurality of (e.g., tens, hundreds, or more) device regions that, when individualized, form a plurality of integrated device dies. The second element may include an individualized element, such as an individualized integrated device die. In other configurations, the second element may include a carrier or substrate (e.g., a wafer).
[0052] As described herein, the first and second elements can be directly bonded to each other without an adhesive, which is different from a deposition process. In one application, the width of the first element within the bonded structure is similar to the width of the second element. In some other embodiments, the width of the first element within the bonded structure is different from the width of the second element. Similarly, the width or area of the larger element within the bonded structure may be at least 10% larger than the width or area of the smaller element. Thus, the first and second elements may include undeposited elements. Furthermore, unlike deposited layers, the directly bonded structure may include defect regions along the bonding interface where nanovoids are present. Nanovoids may be formed due to activation of the bonding surface (e.g., exposure to plasma). As previously mentioned, the bonding interface may contain a concentration of materials resulting from activation and / or a final chemical treatment process. For example, in embodiments utilizing nitrogen plasma for activation, a nitrogen peak may be formed at the bonding interface. In embodiments utilizing oxygen plasma for activation, an oxygen peak may be formed at the bonding interface. In some embodiments, the bonding interface may comprise silicon oxynitride, silicon oxycarbonitrile (oxycarbonitride), or silicon carbonitride (carbonitride). As described herein, direct bonding may comprise covalent bonding, which is stronger than van der Waals bonding. The bonding layer may further comprise a polished surface flattened to a high degree of smoothness.
[0053] In some embodiments, a metal-metal bond is formed between the contact pads. In some embodiments, the contact pad comprises copper or a copper alloy. In various embodiments, the metal-metal bonds between the contact pads may be bonded such that copper grains grow into each other's interiors across the bonding interface. In some embodiments, the copper may have grains oriented along the 111 crystal plane for improved copper diffusion through the bonding interface. The bonding interface may extend substantially entirely toward at least a portion of the bonded contact pad so that there is no substantially gap between the non-conductive bonding zones on or near the bonded contact pad. In some embodiments, a barrier layer may be provided beneath the contact pad (e.g., may comprise copper). However, in other embodiments, a barrier layer may not exist beneath the contact pad, as described, for example, in US 2019 / 0096741, which is incorporated herein in its whole and in all respects.
[0054] In one embodiment, a microelectronic structure is disclosed. The microelectronic structure may include a bulk semiconductor portion having a first surface and a second surface opposite to the first surface; and a via structure disposed within an opening extending at least partially through the bulk semiconductor portion along a direction not parallel to the first surface, wherein the via structure comprises a first conductive via portion, a second conductive via portion, a first barrier layer extending along the sidewall of the first conductive via portion, and a second barrier layer comprising a first portion disposed between the first conductive via portion and the second conductive via portion, the second conductive via portion extending from the second barrier layer to the at least first surface.
[0055] In some embodiments, the microelectronic structure further comprises a dielectric layer on the bulk semiconductor portion, and the second conductive via extends through the dielectric layer such that the end of the second conductive via is at the same height as or recessed from the upper surface of the dielectric layer. In some embodiments, the dielectric layer comprises a flattened dielectric bonding layer configured for direct bonding to another element. In some embodiments, the dielectric layer further comprises a dielectric barrier layer on the bulk semiconductor portion, and the flattened dielectric bonding layer is disposed on the dielectric barrier layer. In some embodiments, the second barrier layer comprises a second portion extending along the first barrier layer between the first barrier layer and the second conductive via. In some embodiments, the first metal texture of the first conductive via differs from the second metal texture of the second conductive via. In some embodiments, the second metal texture has grains oriented along a 111 crystal plane that is non-parallel to the bonding interface. In some embodiments, the first and second conductive vias comprise copper, and the copper in the first conductive via has an impurity material therein. In some embodiments, the first conductive via has a higher impurity concentration than the second conductive via. In some embodiments, the first conductive via further comprises one or more alloy elements comprising one or more of beryllium (Be), indium (In), gallium (Ga), manganese (Mn), and nickel (Ni). In some embodiments, the impurity material comprises one or more of sulfur, oxygen, carbon, or nitrogen. In some embodiments, the first and second conductive vias comprise different metals or different alloys. In some embodiments, the second surface comprises an active surface comprising an active integrated circuit formed in or on the second surface.In some embodiments, the microelectronic structure is directly bonded to another element without an adhesive. In some embodiments, the end face of the second conductive via is directly bonded to the contact pad of the other element without an adhesive interposed therein. In some embodiments, the non-conductive bonding region of the microelectronic element and the other element is directly bonded without an interposed adhesive. In some embodiments, the microelectronic device may include a first conductive via, a second conductive via, a first barrier layer extending along the sidewall of the first conductive via, and a second via structure having a second barrier layer, wherein the second barrier layer comprises a first portion disposed between the first conductive via and the second conductive via, and the second conductive via of the via structure extends along a length different from the length of the second conductive via of the second via structure.
[0056] In another embodiment, a microelectronic structure is disclosed. The microelectronic structure may include a bulk semiconductor portion having a first surface and a second surface opposite to the first surface; and a via structure disposed within an opening extending at least partially through the bulk semiconductor portion through the first surface along a direction not parallel to the first surface, wherein the via structure comprises a first conductive via portion and a second conductive via portion disposed immediately above the first conductive via portion and in contact with the first conductive via portion without an interposed barrier layer, the second conductive via portion disposed between the first surface and the first conductive via portion, and the first conductive via portion has a different material composition from the second conductive via portion.
[0057] In some embodiments, the microelectronic structure includes a barrier layer extending along the sidewalls of the first and second conductive portions. In some embodiments, the microelectronic structure further includes a dielectric layer on the bulk semiconductor portion, and the second conductive via portion extends through the dielectric layer such that the end of the second conductive via portion is at the same height as or recessed below the upper surface of the dielectric layer. In some embodiments, the dielectric layer includes a flattened dielectric coupling layer configured for direct coupling to another element. In some embodiments, the dielectric layer further includes a dielectric barrier layer on the bulk semiconductor portion, and the flattened dielectric coupling layer is disposed on the dielectric barrier layer. In some embodiments, the first metal texture of the first conductive via portion is different from the second metal texture of the second conductive via portion. In some embodiments, the second metal texture has grains oriented along the 111 crystal plane. In some embodiments, the first and second conductive vias comprise copper, and the copper in the first conductive via has an impurity material therein. In some embodiments, the first conductive via comprises one or more alloy elements comprising one or more of beryllium (Be), indium (In), gallium (Ga), manganese (Mn), and nickel (Ni). In some embodiments, the impurity material comprises one or more of sulfur, oxygen, carbon, or nitrogen. In some embodiments, the first and second conductive vias comprise different metals or different alloys. In some embodiments, the microelectronic device is directly bonded to another element without an adhesive. In some embodiments, the end face of the second conductive via is directly bonded to the contact pad of the other element without an adhesive interposed therein. In some embodiments, the non-conductive bonding regions of the microelectronic element and the other element are directly bonded without an interposed adhesive.
[0058] In another embodiment, a microelectronic structure is disclosed. The microelectronic structure may include a bulk semiconductor portion having a first surface and a second surface opposite to the first surface; and a via structure disposed within an opening extending at least partially through the bulk semiconductor portion through the first surface along a direction not parallel to the first surface, wherein the via structure comprises a first conductive via portion and a second conductive via portion disposed immediately above the first conductive via portion and in contact with the first conductive via portion without an interposed barrier layer, wherein the second conductive via portion is disposed between the first surface and the first conductive via portion, and the first conductive via portion is formed before and separately from the second conductive via portion.
[0059] In some embodiments, the microelectronic structure comprises a barrier layer extending along the sidewalls of the first and second conductive portions. In some embodiments, the first metal texture of the first conductive via portion differs from the second metal texture of the second conductive via portion. In some embodiments, the second metal texture has grains oriented along 111 crystal planes. In some embodiments, the first metal texture has a first proportion of 111 planes oriented within 30° vertically, and the second metal texture has a second proportion of 111 planes oriented within 30° vertically, wherein the second proportion is greater than that of the first portion. In some embodiments, the first and second conductive via portions comprise copper, and the copper of the first conductive via portion contains impurity material therein. In some embodiments, the first conductive portion has a higher percentage of alloy elements compared to the second conductive via portion. In some embodiments, the microelectronic device is directly bonded to another element without an adhesive. In some embodiments, the end face of the second conductive via portion is directly bonded to the contact pad of the other element without an adhesive interposed therein. In some embodiments, the non-conductive bonding regions of the microelectronic device and the other element are directly bonded without an interposed adhesive.
[0060] In another embodiment, a method for forming a microelectronic structure is disclosed. This method may include the steps of: forming an opening at least partially through a substrate having a front surface and a rear surface opposite the front surface—the opening extends through the front surface along a direction not parallel to the second surface—; providing a first conductive via portion from the front surface into the opening; exposing the first conductive via portion by removing material from the rear surface; and, after the step of exposing, providing a filling structure on the first conductive via portion from the rear surface into the opening.
[0061] In some embodiments, the step of providing the filling structure comprises providing a second conductive via portion on the first conductive via portion within the opening from the rear side. In some embodiments, the method comprises, after the step of exposing, the step of recessing the first conductive via portion from the rear side. In some embodiments, the method comprises the step of providing a second barrier layer on the first conductive via portion after the step of providing the first conductive via portion, but before the step of providing the second conductive via portion. In some embodiments, the method comprises the step of providing a first barrier layer along the sidewall of the first conductive via portion. In some embodiments, the method comprises the step of providing a first barrier layer before providing the first conductive via portion. In some embodiments, the step of providing the second barrier layer comprises providing the second barrier layer along the first barrier layer between the first barrier layer and the second conductive via portion. In some embodiments, the method comprises the step of providing a dielectric layer on the bulk semiconductor portion, wherein the dielectric layer forms at least partially the back surface of the substrate, and the second conductive via portion extends through the dielectric layer such that the end of the second conductive via portion is at the same height as or recessed from the back surface. In some embodiments, the method comprises the step of preparing the dielectric layer for direct coupling to another device. In some embodiments, the method comprises the step of providing a dielectric barrier layer on the bulk semiconductor portion, wherein the dielectric coupling layer is disposed on the dielectric barrier layer. In some embodiments, the method comprises the step of directly coupling the dielectric layer to another device without an adhesive interposed therein.In some embodiments, the method comprises the step of directly bonding the end face of the second conductive via portion without an adhesive interposed in the contact pad of the other element. In some embodiments, the step of providing the filling structure comprises providing a dielectric layer on the first conductive via portion within a recess. In some embodiments, the method may comprise the step of removing a portion of the substrate from the back surface so that the first conductive via portion protrudes from the back surface of the substrate, and removing the dielectric layer to expose the conductive via. In some embodiments, the step of removing a portion of the substrate comprises etching the back surface of the substrate. In some embodiments, the method may comprise the step of providing a second back surface dielectric layer on at least the etched back surface of the substrate and on the portion of the dielectric layer disposed within the recess. In some embodiments, the method may comprise the step of removing at least a portion of the second back surface dielectric layer on the portion of the dielectric layer disposed within the recess. In some embodiments, the method may include the step of flattening the second back dielectric layer and sinking the first conductive via relative to the second back dielectric layer.
[0062] In another embodiment, a method for forming a microelectronic structure is disclosed. This method may include the steps of: forming an opening through a substrate having a front surface and a rear surface opposite to a first surface, wherein the opening extends through the front surface along a direction not parallel to the front surface; filling the opening with a first conductive via portion; exposing the first conductive via portion by removing material from the rear surface; and refilling a portion of the opening using a filling structure after exposing the first conductive portion.
[0063] In some embodiments, the step of refilling a portion of the opening using a filling structure comprises providing a second conductive via portion on the first conductive via portion within the opening from the rear side. In some embodiments, the method comprises the step of recessing the first conductive portion after exposing and forming a portion of the opening. In some embodiments, the method comprises the step of depositing a second barrier layer on the first conductive via portion through the portion after the recessing step and before the refilling step. In some embodiments, the method comprises the step of depositing a first barrier layer to line the opening before filling. In some embodiments, the step of depositing the second barrier layer comprises depositing the second barrier layer on the first barrier layer within the portion of the opening. In some embodiments, the step of refilling a portion of the opening using the filling structure comprises providing a dielectric layer on the first conductive via portion within a recess through the portion. In some embodiments, the method may include the step of removing a portion of the substrate from the back surface so that the first conductive via portion protrudes from the back surface of the substrate, and removing the dielectric layer to expose the conductive via. In some embodiments, the step of removing the portion of the substrate includes etching the back surface of the substrate. In some embodiments, the method may include the step of providing a second back surface dielectric layer on at least the etched back surface of the substrate and on the portion of the dielectric layer disposed within the recess. In some embodiments, the method includes the step of removing at least a portion of the second back surface dielectric layer on the portion of the dielectric layer disposed within the recess.In some embodiments, the method may include the step of flattening the second back dielectric layer and sinking the first conductive via relative to the second back dielectric layer.
[0064] In another embodiment, a bonded structure is disclosed. The bonded structure may include a first element having a first bonding surface and a second element having a second bonding surface—the first element having a third surface opposite to the first bonding surface—; and a via structure disposed within an opening extending from the first bonding surface through the first element in a direction not parallel to the first bonding surface, wherein the via structure comprises a first conductive via portion and a second conductive via portion in contact with each other, the second conductive via portion being at least partially embedded in a bonding material at the bonding surface of the first element, and the bonding material and the second conductive via portion being directly bonded without an adhesive interposed at the bonding surface of the second element. In some embodiments, non-conductive bonding regions of the first and second elements are directly bonded without an interposed adhesive.
[0065] In another embodiment, a method for forming a microelectronic structure is disclosed. This method comprises the steps of: providing a substrate having an opening and a conductive via disposed within the opening, wherein the conductive via extends from a first surface of the substrate toward a second surface through the substrate in part; removing a portion of the substrate from the second surface to expose the conductive via; removing a portion of the conductive via from the second surface of the substrate to form a recess; providing a dielectric layer over the conductive via within the recess; further removing a portion of the substrate from the second surface so that the conductive via protrudes from the second surface of the substrate; and removing the dielectric layer to expose the conductive via.
[0066] In some embodiments, the step of removing a portion of the substrate comprises at least one of grinding and polishing the second surface. In some embodiments, at least one of grinding and polishing comprises planarizing the substrate and the conductive via. In some embodiments, the step of removing a portion of the conductive via comprises etching the conductive via. In some embodiments, the step of providing the dielectric layer comprises providing a first back dielectric layer on the back surface of the substrate and within the recess. In some embodiments, providing the first back dielectric layer comprises providing a plurality of dielectric layers. In some embodiments, providing the plurality of dielectric layers comprises providing a first silicon nitride layer on the back surface of the substrate and on the conductive via, and providing a second silicon oxide layer on the first silicon nitride layer. In some embodiments, the method may include the step of removing a portion of the first back dielectric layer disposed on the back surface of the substrate before further removing a portion of the substrate. In some embodiments, the method further comprises the step of removing a portion of the substrate by etching the back surface of the substrate. In some embodiments, the method may include the step of providing a second back dielectric layer over at least the etched back surface of the substrate and a portion of the first back dielectric layer disposed within the recess. In some embodiments, the method may include the step of removing at least a portion of the second back dielectric layer over the portion of the dielectric layer disposed within the recess. In some embodiments, the method may include the step of flattening the second back dielectric layer and recessing the conductive via relative to the second back dielectric layer.
[0067] Unless the context explicitly requires otherwise, throughout the detailed description and claims, terms such as “comprise,” “comprising,” “include,” and “including” shall be interpreted as including, but not limited to, as opposed to being exclusive or comprehensive. The word “coupled,” as used generally in this specification, refers to two or more elements that may be directly connected or connected via one or more intermediate elements. Similarly, the word “connected,” as used generally in this specification, refers to two or more elements that may be directly connected or connected via one or more intermediate elements. Additionally, the words “here,” “above,” “below,” and words of similar meaning, as used herein, refer to the entirety of the invention and not to any specific part of the invention. Furthermore, as used herein, when a first element is described as existing "on" or "over" a second element, the first element may exist directly on or over the second element so that the first and second elements are in direct contact, or the first element may exist indirectly on or over the second element so that one or more elements are interposed between the first and second elements. Where permitted by context, words in the above detailed description using singular or plural numbers may also include plural or singular numbers, respectively. The word "or" when referring to a list of two or more items covers all of the following interpretations of the word: any one of the items in the list, all of the items in the list, and any combination of the items in the list.
[0068] Furthermore, the conditional language used herein, among others, such as “can,” “could,” “might,” “may,” “for example,” “for instance,” etc., is broadly intended to convey the meaning that certain embodiments (although other embodiments are not) include certain features, elements, and / or states, unless specifically stated otherwise or understood differently from the context in which they are used. Accordingly, such conditional language is generally not intended to imply that features, elements, and / or states are required for one or more embodiments in any case.
[0069] Although specific embodiments have been described, these embodiments are provided merely by way of example and are not intended to limit the scope of the invention. In fact, the novel apparatus, method, and system described herein may be implemented in various other forms; furthermore, various omissions, substitutions, and modifications of the method and system described herein may be made without departing from the scope of the invention. For example, while blocks are presented in a given configuration, alternative embodiments may perform similar functionality using different components and / or circuit topologies, and some blocks may be deleted, moved, added, subdivided, combined, and / or modified. Each of these blocks may be implemented in various different ways. Any suitable combination of elements and operations of the various embodiments described above may be combined to provide additional embodiments. The appended claims and their equivalents are intended to encompass such forms or variations that fall within the scope and spirit of the invention.
Claims
Claim 1 A microelectronic device comprising: a rear side and a front side opposite to the rear side; a bulk semiconductor portion having a rear side and a front side opposite to the rear side - the front side includes an active surface having an active integrated circuit portion formed on or above the front side -; A microelectronic device comprising a via structure disposed within an opening extending through the rear surface along a direction not parallel to the rear surface through at least partially the bulk semiconductor portion, wherein the via structure comprises a first conductive via portion, a second conductive via portion, a first barrier layer extending along the sidewall of the first conductive via portion, and a second barrier layer comprising a first portion disposed between the first conductive via portion and the second conductive via portion, wherein the second conductive via portion is positioned over the first conductive via portion and extends from the second barrier layer to at least the rear surface, and the end of the second conductive via portion forms a portion of the rear surface of the microelectronic device and serves as a contact pad configured for direct coupling to a corresponding conductive feature of another device. Claim 2 The microelectronic device according to claim 1 further comprises a dielectric layer on the rear surface of the bulk semiconductor portion, wherein the second conductive via portion extends through the dielectric layer such that the end of the second conductive via portion is at the same height as or recessed from the upper surface of the dielectric layer. Claim 3 A microelectronic device according to claim 2, wherein the dielectric layer comprises a flattened dielectric coupling layer configured for direct coupling to another element. Claim 4 A microelectronic device according to claim 3, wherein the dielectric layer further comprises a dielectric barrier layer on the bulk semiconductor portion, and the planarized dielectric bonding layer is disposed on the dielectric barrier layer. Claim 5 A microelectronic device according to claim 1, wherein the second barrier layer comprises a second portion extending along the first barrier layer between the first barrier layer and the second conductive via portion. Claim 6 A microelectronic device according to claim 1, wherein the first metal texture of the first conductive via portion is different from the second metal texture of the second conductive via portion. Claim 7 A microelectronic device according to claim 6, wherein the second metal texture has grains oriented along a 111 crystal plane non-parallel to the bonding interface. Claim 8 A microelectronic device according to claim 1, wherein the first and second conductive vias comprise copper, and the copper of the first conductive via has an impurity material therein. Claim 9 A microelectronic device according to claim 8, wherein the first conductive via has a higher impurity concentration than the second conductive via. Claim 10 A microelectronic device according to claim 8, wherein the first conductive via further comprises one or more alloy elements including one or more of beryllium (Be), indium (In), gallium (Ga), manganese (Mn), and nickel (Ni). Claim 11 A microelectronic device according to claim 8, wherein the impurity material comprises one or more of sulfur, oxygen, carbon, or nitrogen. Claim 12 A microelectronic device according to claim 1, wherein the first and second conductive vias comprise different metals or different alloys. Claim 13 delete Claim 14 A combined structure comprising a microelectronic device of claim 1, wherein the microelectronic device is directly combined without an adhesive interposed between other elements. Claim 15 delete Claim 16 In claim 14, the non-conductive bonding regions of the microelectronic device and the other element are directly bonded without an interposed adhesive, forming a bonded structure. Claim 17 delete Claim 18 A microelectronic device comprising: a rear side and a front side opposite to the rear side; a bulk semiconductor portion having a rear side and a front side opposite to the rear side - the front side includes an active surface having an active circuit portion formed therein or on top of it -; A microelectronic device comprising a via structure disposed within an opening extending along a direction not parallel to the rear surface through the rear surface through at least partially the bulk semiconductor portion, wherein the via structure comprises a first conductive via portion and a second conductive via portion disposed immediately above the first conductive via portion and in contact with the first conductive via portion without an interposed barrier layer, wherein the second conductive via portion is disposed between the rear surface and the first conductive via portion and is above the first conductive via portion, wherein the first conductive via portion has a different material composition from the second conductive via portion, and the end of the second conductive via portion forms a portion of the rear surface of the microelectronic device and serves as a contact pad configured for direct coupling to a corresponding conductive feature of another device. Claim 19 In claim 18, the microelectronic device further comprises a barrier layer extending along the sidewalls of the first and second conductive portions. Claim 20 In claim 18, the microelectronic device further comprises a dielectric layer on the rear surface of the bulk semiconductor portion, wherein the dielectric layer forms another portion on the rear side of the microelectronic device, and the second conductive via portion extends through the dielectric layer such that the end of the second conductive via portion is at the same height as or recessed below the upper surface of the dielectric layer. Claim 21 delete Claim 22 delete Claim 23 delete Claim 24 delete Claim 25 A microelectronic device according to claim 18, wherein the first and second conductive vias comprise copper, and the copper of the first conductive via has an impurity material therein. Claim 26 A microelectronic device according to claim 25, wherein the first conductive via comprises one or more alloy elements including one or more of beryllium (Be), indium (In), gallium (Ga), manganese (Mn), and nickel (Ni). Claim 27 In claim 25, the microelectronic device wherein the impurity material comprises one or more of sulfur, oxygen, carbon, or nitrogen. Claim 28 In claim 18, the first and second conductive vias comprise different metals or different alloys, in a microelectronic device. Claim 29 A combined structure comprising a microelectronic device of claim 18, wherein the rear side of the microelectronic device is directly bonded without an adhesive interposed between other elements. Claim 30 delete Claim 31 delete Claim 32 A microelectronic device comprising a bulk semiconductor portion having a rear surface and a front surface opposite to the rear surface—the front surface comprising an active surface having an active circuit portion formed therein or on top of it—; A microelectronic device comprising a via structure disposed within an opening extending along a direction not parallel to the rear surface through the rear surface through at least partially the bulk semiconductor portion, wherein the via structure comprises a first conductive via portion and a second conductive via portion disposed immediately above the first conductive via portion and in contact with the first conductive via portion without an interposed barrier layer, wherein the second conductive via portion is disposed between the rear surface and the first conductive via portion and is above the first conductive via portion, wherein the first conductive via portion is formed before and separately from the second conductive via portion, and the end surface of the second conductive via portion forms a portion of the rear side of the microelectronic device and serves as a contact pad configured for direct coupling to a corresponding conductive feature of another device. Claim 33 In claim 32, the microelectronic device further comprises a barrier layer extending along the sidewalls of the first and second conductive portions. Claim 34 In claim 32, a microelectronic device wherein the first metal texture of the first conductive via portion is different from the second metal texture of the second conductive via portion. Claim 35 In claim 34, the microelectronic device having a second metal texture having grains oriented along a 111 crystal plane. Claim 36 A microelectronic device according to claim 35, wherein the first metal texture has a first ratio of 111 planes oriented within 30° vertically, the second metal texture has a second ratio of 111 planes oriented within 30° vertically, and the second ratio is larger than the first ratio. Claim 37 A microelectronic device according to claim 32, wherein the first and second conductive vias comprise copper, and the copper of the first conductive via has an impurity material therein. Claim 38 A microelectronic device according to claim 32, wherein the first conductive portion has a higher percentage of alloying elements compared to the second conductive via portion. Claim 39 A combined structure comprising a microelectronic device according to claim 32, wherein the microelectronic device is directly combined without an adhesive interposed between other elements. Claim 40 In claim 39, the end surface of the second conductive via portion is directly bonded to the contact pad of the other element without an adhesive interposed therein, forming a bonded structure. Claim 41 In claim 39, the non-conductive bonding regions of the microelectronic device and the other element are directly bonded without an interposed adhesive, forming a bonded structure. Claim 42 delete Claim 43 delete Claim 44 delete Claim 45 delete Claim 46 delete Claim 47 delete Claim 48 delete Claim 49 delete Claim 50 delete Claim 51 delete Claim 52 delete Claim 53 delete Claim 54 delete Claim 55 delete Claim 56 delete Claim 57 delete Claim 58 delete Claim 59 delete Claim 60 delete Claim 61 delete Claim 62 delete Claim 63 delete Claim 64 delete Claim 65 delete Claim 66 delete Claim 67 delete Claim 68 delete Claim 69 delete Claim 70 delete Claim 71 delete Claim 72 A combined structure comprising: a first element having a first bonding surface and a second element having a second bonding surface—the first element having a third surface opposite to the first bonding surface—; and a via structure disposed within an opening extending from the first bonding surface along a direction not parallel to the first bonding surface through at least partially the first element, wherein the via structure comprises a first conductive via portion and a second conductive via portion in contact with each other, wherein the second conductive via portion is at least partially embedded in a bonding material at the bonding surface of the first element, and the bonding material and the second conductive via portion are directly bonded without an adhesive interposed at the bonding surface of the second element. Claim 73 In claim 72, the non-conductive adhesive regions of the first and second elements are directly bonded without an interposed adhesive, forming a bonded structure. Claim 74 delete Claim 75 delete Claim 76 delete Claim 77 delete Claim 78 delete Claim 79 delete Claim 80 delete Claim 81 delete Claim 82 delete Claim 83 delete Claim 84 delete Claim 85 delete
Citation Information
Patent Citations
Semiconductor device and its manufacturing method
JP2003068741A
Integrated circuit device having through silicon via structure
KR1020130053338A
Integrated circuit device having through silicon via structure and method of manufacturing the same
KR1020140011137A