Rubber composition for tire tread containing polyoctenamer and tire manufactured by using the same

A rubber composition for tire treads using natural rubber, solution-polymerized styrene-butadiene rubber, polyoctenamer, silica, and carbon black addresses the challenges of wear resistance, fuel efficiency, and processability, enhancing tire performance without compromising mechanical properties.

KR103047787B1Active Publication Date: 2026-11-11HANKOOK TIRE & TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230089309
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2026-11-11
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

Existing tire tread compounds face challenges in achieving improved wear resistance, fuel efficiency, and processability without compromising other physical properties, particularly when using high amounts of silica or adhesives.

Method used

A rubber composition for tire treads comprising natural rubber, solution-polymerized styrene-butadiene rubber, polyoctenamer, silica, and carbon black, with specific ratios and properties to enhance processability and fuel efficiency while maintaining reinforcing properties.

Benefits of technology

The composition improves processability and fuel efficiency while maintaining reinforcing properties, as demonstrated by increased fluidity, reduced hysteresis loss, and improved wear performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023075770702-PAT00001_ABST
    Figure 112023075770702-PAT00001_ABST
Patent Text Reader

Abstract

The present invention relates to a rubber composition for tire treads. By utilizing polyoctenamer as an organic filler and applying it to a rubber composition for tire treads, the invention contributes to the improvement of additional mechanical properties of the rubber composition and the resulting enhancement of tire performance by leveraging the advantages of improved rubber processability and good compatibility with conventionally used fillers and adhesives.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a rubber composition for a tire tread and a tire manufactured using the same, specifically a rubber composition for a tire tread comprising an organic filler that can be used to improve the wear performance and fuel efficiency of a tread compound utilized in tire development, and a tire manufactured using the same. Background Technology

[0002] For the rubber tread materials used in tires, grip and braking performance are essential for driver safety. Research on fillers is crucial to extend the service life by improving wear resistance while responding to various driving environments.

[0003] The key performance characteristics of a tire—wear, friction, and fuel efficiency—form a "magic triangle" and complement each other. Since the fuel efficiency of the tread compound is determined by road surface conditions, tire usage, and temperature, it possesses the viscoelastic properties that can lead to performance variations. To achieve maximum performance improvement with minimal sacrifice, it is common practice to use new polymers and incorporate large amounts of silica or adhesives. However, due to limitations such as poor processability and relatively low mechanical properties, this approach actually entails the problem of reduced wear performance and fuel efficiency.

[0004] If recipes are formulated to use low Tg. polymers or liquid polymers and add large amounts of silica or adhesives, as is the recent development trend, this also has the limitation of resulting in relatively poor mechanical properties.

[0005] Therefore, a new filler is needed that can improve performance without causing significant adverse effects on other physical properties, such as fuel efficiency or wear resistance. The problem to be solved

[0006] The objective of the present invention is to improve the performance and application of organic fillers introduced to enhance properties such as processability and low fuel consumption without altering the basic properties of the tread compound.

[0007] Another objective of the present invention is to provide a tire manufactured using a rubber composition for a tire tread comprising the organic filler. means of solving the problem

[0008] One embodiment of the present invention provides a rubber composition for a tire tread comprising 100 parts by weight of raw rubber comprising natural rubber and solution-polymerized styrene-butadiene rubber and polyoctenamer.

[0009] According to one embodiment of the present invention, the composition may include 5 to 30 parts by weight of the natural rubber and 70 to 95 parts by weight of the solution-polymerized styrene-butadiene rubber, based on 100 parts by weight of the raw rubber.

[0010] According to one embodiment of the present invention, the solution polymerized styrene-butadiene rubber comprises two types, and may comprise 40 to 70 parts by weight of a first solution polymerized styrene-butadiene rubber and 15 to 45 parts by weight of a second solution polymerized styrene-butadiene rubber per 100 parts by weight of raw rubber.

[0011] According to one embodiment of the present invention, the first solution-polymerized styrene-butadiene rubber may have a styrene content of 20% to 30% by weight, a vinyl content of 15% to 25% by weight, and a glass transition temperature (Tg) of -60°C to -40°C, and the second solution-polymerized styrene-butadiene rubber may have a styrene content of 20% to 30% by weight, a vinyl content of 45% to 55% by weight, and a glass transition temperature (Tg) of -30°C to -20°C.

[0012] According to one embodiment of the present invention, the rubber composition may have a glass transition temperature (Tg) of -25 ℃ to -15 ℃.

[0013] According to one embodiment of the present invention, the polyoctenamer may comprise 5 to 20 parts by weight per 100 parts by weight of raw rubber.

[0014] According to one embodiment of the present invention, the polyoctenamer may have a weight average molecular weight of 110,000 g / mol to 170,000 g / mol and a glass transition temperature (Tg) of -75 ℃ to -55 ℃.

[0015] According to one embodiment of the present invention, the rubber composition further comprises a reinforcing organic filler, and the reinforcing organic filler may be silica and carbon black.

[0016] According to one embodiment of the present invention, the silica may comprise 100 to 150 parts by weight per 100 parts by weight of raw rubber.

[0017] According to one embodiment of the present invention, the carbon black may have an iodine adsorption amount of 135 mg / g to 145 mg / g and a DBP (Dibutylphthalate) oil absorption amount of 125 cc / 100g to 135 cc / 100g.

[0018] One embodiment of the present invention provides a tire manufactured using the rubber composition for the tire tread. Effects of the invention

[0019] A rubber composition for a tire tread according to one embodiment of the present invention includes polyoctenamer as an organic filler, and has the effect of improving processability and fuel efficiency while maintaining reinforcing properties.

[0020] A tire manufactured using a rubber composition for a tire tread according to one embodiment of the present invention includes polyoctenamer as an organic filler, thereby improving processability and fuel efficiency while maintaining reinforcing properties. Brief explanation of the drawing

[0021] Figure 1 shows a viscoelasticity (tanδ) graph according to one embodiment of the present invention. FIG. 2 shows a stress-strain curve graph according to one embodiment of the present invention. Specific details for implementing the invention

[0022] Hereinafter, each component of the present invention is described in more detail so that a person skilled in the art to which the present invention pertains can easily implement it; however, this is merely an example, and the scope of the rights of the present invention is not limited by the following.

[0023] The configuration of the present invention will be described in more detail below.

[0025] One embodiment of the present invention provides a rubber composition for a tire tread comprising 100 parts by weight of raw rubber including natural rubber and solution-polymerized styrene-butadiene rubber; and polyoctenamer.

[0026] A rubber composition for a tire tread according to one embodiment of the present invention includes polyoctenamer as an organic filler, and has the effect of improving processability and fuel efficiency while maintaining reinforcing properties.

[0027] According to one embodiment of the present invention, the raw rubber comprises natural rubber and solution polymerized styrene-butadiene rubber.

[0028] According to one embodiment of the present invention, the natural rubber (NR) is a general term for rubber that can be obtained from nature, and its place of origin is not limited. Both general natural rubber and modified natural rubber may be used. Although it mainly contains cis-1,4-polyisoprene, it is not necessarily limited thereto, and natural rubber containing trans-1,4-polyisoprene may also be used.

[0029] According to one embodiment of the present invention, the natural rubber may be included in an amount of 5 to 30 parts by weight per 100 parts by weight of raw rubber. If the amount is less than 5 parts by weight, there is a problem with reduced fuel efficiency and processability, and if the amount exceeds 30 parts by weight, there is a problem with reduced stiffness.

[0030] According to one embodiment of the present invention, the solution polymerized styrene-butadiene rubber may be included in an amount of 70 to 95 parts by weight per 100 parts by weight of raw rubber.

[0031] According to one embodiment of the present invention, the solution polymerized styrene-butadiene rubber may be two or more types of solution polymerized styrene-butadiene rubber. Specifically, it may be a mixture of a first solution polymerized styrene-butadiene rubber and a second solution polymerized styrene-butadiene rubber.

[0032] According to one embodiment of the present invention, by using the first solution polymerized styrene-butadiene rubber having a low glass transition temperature (Tg), the Tg of the compound itself can be lowered, and if the Tg of the compound itself is lowered, the wear performance can be improved.

[0033] According to one embodiment of the present invention, the dispersion of the filler can be improved by using the second solution polymerized styrene-butadiene rubber with a high vinyl group content. This is because silica used as a filler can rapidly combine with the radicals of the vinyl group, and improving the dispersion of the filler can also improve mechanical properties and wear performance.

[0034] According to one embodiment of the present invention, by using two types of solution-polymerized styrene-butadiene rubbers with different glass transition temperatures (Tg), the wet performance can be improved as the heat generation increases.

[0035] According to one embodiment of the present invention, the first solution-polymerized styrene-butadiene rubber may be included in an amount of 40 to 70 parts by weight per 100 parts by weight of raw rubber. Specifically, the first solution-polymerized styrene-butadiene rubber may be in an amount of 45 to 65 parts by weight, 50 to 60 parts by weight, or 52 to 58 parts by weight per 100 parts by weight of raw rubber, and preferably 55 parts by weight. By adjusting the weight of the first solution-polymerized styrene-butadiene rubber within the above-described range and including it in a greater amount than the weight of the second solution-polymerized styrene-butadiene rubber, the glass transition temperature (Tg) can be lowered and mechanical properties and wear performance can be improved.

[0036] According to one embodiment of the present invention, the first solution-polymerized styrene-butadiene rubber may have a styrene content of 20% to 30% by weight. When the solution-polymerized styrene-butadiene rubber has a styrene content within the above range, the hysteresis of the rubber can be reduced to improve low fuel consumption performance.

[0037] According to one embodiment of the present invention, the first solution-polymerized styrene-butadiene rubber may have a vinyl content of 15% to 25% by weight. In the above vinyl content range, excellent braking performance may be achieved without a decrease in fuel efficiency and wear resistance.

[0038] According to one embodiment of the present invention, the first solution-polymerized styrene-butadiene rubber may have a glass transition temperature (Tg) of -60°C to -40°C. When having a glass transition temperature in the above range, the fluidity of the rubber at room temperature is increased, and wear performance and fuel efficiency performance may be improved by reducing hysteresis loss.

[0039] According to one embodiment of the present invention, the second solution polymerized styrene-butadiene rubber may comprise 15 to 45 parts by weight per 100 parts by weight of raw rubber.

[0040] According to one embodiment of the present invention, the second solution-polymerized styrene-butadiene rubber may have a styrene content of 20% to 30% by weight. If the styrene content exceeds the above range, it may be difficult to maximize the wear resistance performance of the tire, and if it is below the above range, a problem may arise regarding reduced processability when manufacturing the mixture.

[0041] According to one embodiment of the present invention, the second solution-polymerized styrene-butadiene rubber may have a vinyl content of 45% to 55% by weight. In the above vinyl content range, excellent braking performance may be achieved without a decrease in fuel efficiency and wear resistance.

[0042] According to one embodiment of the present invention, the second solution-polymerized styrene-butadiene rubber may have a glass transition temperature (Tg) of -30°C to -20°C. When having a glass transition temperature in the above range, the fluidity of the rubber at room temperature is increased, and wear performance and fuel efficiency performance may be improved by reducing hysteresis loss.

[0043] According to one embodiment of the present invention, the solution-polymerized styrene-butadiene rubber may further comprise 20 to 50 parts by weight of TDAE (treated distillate aromatic extract) oil per 100 parts by weight of raw rubber. When the solution-polymerized styrene-butadiene rubber further comprises 20 to 50 parts by weight of TDAE oil per 100 parts by weight of raw rubber, an increase in the flexibility of the styrene-butadiene rubber, which is reduced due to the influence of styrene, can be expected, and processability can also be improved.

[0044] According to one embodiment of the present invention, the glass transition temperature (Tg) of the rubber composition may be -25 ℃ to -15 ℃. When the glass transition temperature is within the above range, the fluidity of the rubber at room temperature is increased, and wear performance and fuel efficiency performance may be improved by reducing hysteresis loss.

[0046] [Polyoctenamer]

[0047] One embodiment of the present invention comprises a rubber composition for a tire tread that further includes polyoctenamer.

[0048] According to one embodiment of the present invention, the polyoctenamer is a material composed of a macrocyclic polymer and an open-chain polymer in a ratio of about 30:70 by Ring-Opening-Metathesis-Polymerization (ROMP) of an octagonal carbon ring.

[0049] According to one embodiment of the present invention, the polyoctenamer can impart stiffness to a rubber composition due to its structural characteristics having a crystalline region of about 35%. In addition, it is not tangled, and since the melting point of the raw material is about 55°C as a result of DSC measurement, the crystalline structure is released during mixing and can act as a slight processing aid, and stiffness can be imparted due to the crystalline region when the temperature is reduced again after mixing.

[0050] According to one embodiment of the present invention, the polyoctenamer possesses the characteristics of both a processing aid and an organic filler; however, considering its role within the compound, it can be considered an organic filler because it exhibits improved stiffness, such as an increase in low elongation modulus and an increase in tanδ on the DMA phase, while other physical properties remain unchanged. These characteristics of the polyoctenamer can be used to further enhance the performance of rubber compositions for tire treads by utilizing the advantages of good compatibility with conventionally used fillers and adhesives.

[0051] According to one embodiment of the present invention, the polyoctenamer may comprise 5 to 20 parts by weight per 100 parts by weight of raw rubber. If the content deviates from the above, the effect of improving physical properties such as processability and low fuel consumption performance may not be significant.

[0052] According to one embodiment of the present invention, the polyoctenamer may have a weight-average molecular weight of 110,000 g / mol to 170,000 g / mol and a glass transition temperature (Tg) of -75 °C to -55 °C, most preferably -67 °C. By controlling the weight-average molecular weight and glass transition temperature (Tg) of the polyoctenamer within the above-described range, additional performance of the rubber composition for tire treads can be improved.

[0054] [Reinforcing Filler]

[0055] According to one embodiment of the present invention, the rubber composition further comprises a reinforcing filler, and the reinforcing filler may comprise an organic filler.

[0056] According to one embodiment of the present invention, the organic filler may include silica and carbon black. Additionally, the polyoctenamer may serve as an organic filler.

[0057] According to one embodiment of the present invention, silica, which is typically used as a reinforcing filler in rubber compositions for tire treads, has excellent reinforcing performance but may reduce the wear resistance performance of the rubber composition for tire treads. In response to this, by mixing in carbon black, which has no risk of reducing wear resistance and is superior to silica in terms of reinforcing performance, it is possible to improve durability performance in a balanced manner along with rolling resistance performance and fuel efficiency performance without reducing wear resistance performance, which is in a trade-off relationship.

[0058] According to one embodiment of the present invention, the silica may comprise 100 to 150 parts by weight per 100 parts by weight of raw rubber. Specifically, if the silica is less than 100 parts by weight, a problem may arise in which the reinforcing properties of the rubber composition are reduced, and if it exceeds 150 parts by weight, a problem may arise in which the mixability of the rubber composition is reduced.

[0059] According to one embodiment of the present invention, the carbon black is a spherical fine particle having a diameter of 10 nm to 500 nm, high rigidity (microcrystalline particles arranged parallel to the surface), and pores, and generally, the smaller the diameter of the particle, the greater the reinforcing effect.

[0060] According to one embodiment of the present invention, the carbon black may be included in an amount greater than 0 parts by weight and less than or equal to 20 parts by weight, preferably 5 to 15 parts by weight, per 100 parts by weight of raw rubber. If the carbon black is included in an amount less than 5 parts by weight, the reinforcing effect is negligible, and if it exceeds 15 parts by weight, processability may be reduced due to an increase in rotational resistance and excessive reinforcing.

[0061] According to one embodiment of the present invention, the carbon black may have an iodine adsorption amount of 135 mg / g to 145 mg / g. If the iodine adsorption amount of the carbon black exceeds 145 mg / g, the processability of the rubber composition may be reduced, whereas if the iodine adsorption amount is less than 135 mg / g, there is a risk that the reinforcing performance by the carbon black filler may be reduced.

[0062] According to one embodiment of the present invention, the carbon black may have a DBP oil absorption capacity of 125 cc / 100g to 135 cc / 100g. If the DBP oil absorption capacity of the carbon black exceeds 135 cc / 100g, the processability of the rubber composition may be reduced, and if it is less than 125 cc / 100g, the reinforcing performance by the carbon black filler may be disadvantageous. The DBP oil absorption capacity serves as an indicator of the degree of structural development, that is, the degree of structural complexity.

[0064] [Other Additives]

[0065] According to one embodiment of the present invention, the rubber composition for a tire tread may optionally further include one or more additives selected from additional coupling agents, adhesives, vulcanizing agents, vulcanization accelerators, vulcanization accelerating aids, oils, or processing aids. Any additive commonly used in the field to which the present invention belongs may be used, and their content is not particularly limited, as it follows the formulation ratio used in conventional rubber compositions for tires.

[0066] According to one embodiment of the present invention, a coupling agent may be additionally included to further improve the dispersibility of the silica used as the reinforcing filler.

[0067] In typical rubber compositions, carbon black is lipophilic, so it has the characteristic of being easily dispersed within the rubber when mixed by applying physical force during the mixing process. However, silica is hydrophilic, so there are limitations to dispersing it by physical force alone, and a coupling agent is required to chemically bond the rubber and silica. When silica and rubber are chemically bonded in this way, the movement of silica within the rubber is restricted, which lowers hysteresis, and as a result, the heat generation and rotational resistance of the rubber composition are reduced.

[0068] According to one embodiment of the present invention, the coupling agent may be any one selected from the group consisting of sulfide-based silane compounds, mercapto-based silane compounds, vinyl-based silane compounds, amino-based silane compounds, glycidoxy-based silane compounds, nitro-based silane compounds, chloro-based silane compounds, methacrylic-based silane compounds, and combinations thereof, and preferably, a sulfide-based silane compound may be used.

[0069] According to one embodiment of the present invention, 5 to 15 parts by weight may be additionally included with respect to 100 parts by weight of the raw rubber. If less than 5 parts by weight, the surface modification effect on silica is negligible, which may reduce the dispersibility of silica and reduce the reinforcement of the tire, and if more than 15 parts by weight is used, the wear resistance and fuel efficiency of the tire may be reduced due to excessive use.

[0070] According to one embodiment of the present invention, the processing aid is an amphiphilic material containing both a hydrophilic group of a metal ion and a hydrophobic group of a fatty acid. By reacting with the silanol group of the metal ion on the silica surface, it reduces the intermolecular surface energy of silica aggregates that are strongly bonded to each other by hydrogen bonds or dipole bonds, thereby inducing deagglomeration during the mixing process. As a result, it lowers the viscosity of the rubber composition for tires, thereby increasing flowability and improving scorch stability, durability, and wear resistance. Furthermore, the hydrocarbon group of the fatty acid acts as a plasticizer that weakens the rubber chains due to its excellent compatibility with the rubber chains, thereby improving processability.

[0071] According to one embodiment of the present invention, specifically, the processing aid may be zinc soap, and it may be preferable to include 1 to 10 parts by weight per 100 parts by weight of raw rubber. If the content of the processing aid is less than 1 part by weight, the dispersion effect of silica is insufficient, and if the content of the processing aid exceeds 10 parts by weight, the degree of improvement in effect relative to the amount of processing aid used is negligible.

[0072] According to one embodiment of the present invention, the vulcanizing agent used is a sulfur-based vulcanizing agent, and powdered sulfur (S), insoluble sulfur (S), precipitated sulfur (S), colloidal sulfur, etc., may be used. Specifically, elemental sulfur or vulcanizing agents that produce sulfur, such as amine disulfide and polymeric sulfur, may also be used.

[0073] According to one embodiment of the present invention, the vulcanization accelerator refers to an accelerator that accelerates the vulcanization speed or accelerates a delaying action during the initial vulcanization stage. As the vulcanization accelerator, any one selected from the group consisting of sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamate-based, aldehyde-amine-based, aldehyde-ammonia-based, imidazoline-based, xanthate-based, and combinations thereof may be used. The vulcanization accelerator may be included in an amount of 0.5 to 3 parts by weight per 100 parts by weight of the raw rubber to maximize productivity enhancement and rubber property enhancement through acceleration of the vulcanization speed.

[0074] According to one embodiment of the present invention, the vulcanization accelerator is a compounding agent used in combination with the vulcanization accelerator to fully enhance the accelerating effect, and any one selected from the group consisting of inorganic vulcanization accelerators, organic vulcanization accelerators, and combinations thereof may be used. As the inorganic vulcanization accelerator, any one selected from the group consisting of zinc oxide (ZnO), zinc carbonate, magnesium oxide (MgO), lead oxide, potassium hydroxide, and combinations thereof may be used. As the organic vulcanization accelerator, any one selected from the group consisting of stearic acid, zinc stearate, palmitic acid, linoleic acid, oleic acid, lauric acid, dibutyl ammonium oleate, derivatives thereof, and combinations thereof may be used. In particular, the zinc oxide and the stearic acid can be used together as the above vulcanization accelerator. In this case, the zinc oxide dissolves in the stearic acid to form an effective complex with the vulcanization accelerator, thereby producing favorable sulfur during the vulcanization reaction, which facilitates the crosslinking reaction of the rubber.

[0075] According to one embodiment of the present invention, when the zinc oxide and the stearic acid are used together, they can be used in an amount of 0.5 to 5 parts by weight and 1 to 3 parts by weight, respectively, per 100 parts by weight of raw rubber, to serve as appropriate vulcanization accelerators.

[0076] According to one embodiment of the present invention, the softening agent is an additive added to impart plasticity to the rubber to facilitate processing or to reduce the hardness of vulcanized rubber, and any one selected from the group consisting of process oil, vegetable oil, and combinations thereof may be used, but is not particularly limited to any one used in the relevant technical field.

[0077] According to one embodiment of the present invention, a softening agent having a softening point of 45°C to 55°C may be used.

[0078] According to one embodiment of the present invention, the softener may be included in an amount of 1 to 50 parts by weight per 100 parts by weight of raw rubber in order to improve the processability of the raw rubber.

[0080] [Manufacturing Method and Tire]

[0081] A tire according to another embodiment of the present invention is manufactured using the rubber composition for tires. Since any method conventionally used for manufacturing tires can be applied to the method of manufacturing a tire using the rubber composition for tires, a detailed description is omitted in this specification.

[0082] The above tire may be a passenger car tire, a racing tire, an airplane tire, an agricultural machinery tire, an off-road tire, a truck tire, or a bus tire, etc. Additionally, the above tire may be a radial tire or a bias tire.

[0083] Hereinafter, embodiments of the present invention are described in detail so that those skilled in the art can easily implement the present invention; however, this is merely an example, and the scope of the present invention is not limited by the following.

[0085] [Manufacturing Example and Experimental Example]

[0086] Tire rubber compositions according to the examples and comparative examples were prepared using the compositions shown in Table 1 below.

[0087] Comparative example Example 1 Example 2 Example 3 NR 15 15 15 15 S-SBR (1) 55 55 55 55 S-SBR (2) 30 30 30 30 C / B 10 10 10 10 silica 130 130 130 130 Coupling Agent 10.4 10.4 10.4 10.4 zinc oxide 2 2 2 2 stearic acid 1 1 1 1 Anti-aging agent 5.9 5.9 5.9 5.9 Processing preparation 5 5 5 5 Polyoctenamer - 5 10 20 adhesive 40 40 40 40 oil 8 8 8 8 Imperial Emperor 0.7 0.7 0.7 0.7 accelerant 2.5 2.5 2.5 2.5

[0088] (Unit: parts by weight)

[0089] 1) S-SBR (1): Styrene-butadiene rubber (SBR) with Styrene / Vinyl content (in SBR, %) = 25 / 19 and containing TDAE Oil Extended (25 phr) / Trade name is HPR621

[0090] 2) S-SBR (2): Styrene-butadiene rubber (SBR) with Styrene / Vinyl content (in SBR, %) = 25 / 50 and containing TDAE Oil Extended (37.5 phr) / Trade name is SOL C6270L

[0091] 3) C / B: Carbon black with an iodine adsorption capacity of 135–145 mg / g and an oil absorption capacity of 125–135 cc / 100g / Product name is HP1107

[0092] 4) Processing aid: An amphiphilic processing aid composed mainly of zinc soap / Product name is EF44

[0093] 5) Adhesive: Softener with a softening point of 45–55 ℃ / Product name is Opera383

[0095] The physical properties of the rubber composition were analyzed in accordance with ASTM regulations.

[0096] Comparative example Example 1 Example 2 Example 3 Glass transition temperature (Tg, °C) -17.7 -17.9 -18.3 -18.6 10% Modulus 10 11 10 9 30% Modulus 83 79 80 81 60 ℃ tanδ(0.5%) 0.160 0.157 0.155 0.162 Rubber friction coefficient (μ) 1.619 1.625 1.732 1.691 Rubber Wear Amount (Index) 100 105 105 104

[0097] The modulus, viscoelasticity, wear characteristics, etc. of the obtained specimens were measured in accordance with ASTM relevant regulations, and the results are shown in Table 2 above.

[0098] - The glass transition temperature was measured using the tanδ phase peak (Dynamic Tg) of the viscoelasticity test results.

[0099] - The modulus was measured according to ISO 37 standards.

[0100] - Viscoelasticity was measured using an ARES meter at 3.5% strain from -60 ℃ to 100 ℃ at a frequency of 10 Hz.

[0101] - Friction and wear were measured using an RTMS measuring instrument at a speed of 30 km / h under a 70 N load at 40% deformation (slip ratio).

[0103] In Table 2 above, the modulus represents the strength of the rubber; the higher the value, the narrower the contact area with the road surface due to mechanical properties, thereby improving fuel efficiency. In particular, the low elongation modulus is a region heavily influenced by the filler.

[0104] 60 ℃ tanδ represents rolling resistance characteristics, and the lower the value, the better the fuel efficiency performance.

[0105] RTMS is an index value, and performance improves as the value increases.

[0107] According to Table 2 above, the modulus generally decreases overall when a softener is added, but the low-elongation modulus shows a slight increase, so it can be confirmed that polyoctenamer acted as an organic filler in the compound.

[0108] In addition, the decrease in high elongation modulus indicates that polyoctenamer acted as a processing aid. As a result, improved fuel efficiency performance can be expected.

[0109] According to Figure 1 above, through the viscoelastic results of Examples 1 to 3 and the Comparative Example, it can be expected that the low fuel consumption characteristics of Examples 1 to 3 are improved compared to the Comparative Example.

[0110] Therefore, in the case of the newly introduced polyoctenamer in the present invention, it can be confirmed that when simply added, the change in the glass transition temperature (Tg) is not significant, while maintaining the reinforcement properties of the existing recipe and improving processability and fuel efficiency.

[0111] In terms of processability improvement, it can be confirmed that not only is the surface of the rubber sheet improved, but the adhesiveness is also significantly improved. According to Figure 1, it can also be confirmed that the peak height of the viscoelastic (tanδ) property increases slightly due to the improvement in processability.

[0112] Figure 2 shows the SS curve (Stress-strain curve) graphs of Examples 1 to 3 and the Comparative Example above.

[0113] According to Figure 2 above, it can be confirmed that the strength does not decrease depending on whether polyoctenamer is introduced.

[0114] Therefore, unlike commonly used fillers, it can be confirmed that with the introduction of polyoctenamer, the overall modulus does not decrease and the viscoelasticity (tanδ) graph does not change significantly, while stiffness increases.

[0115] Although preferred embodiments of the present invention have been described in detail above, the above-described embodiments are presented as specific examples of the present invention and are not intended to limit the present invention. Furthermore, various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the claims set forth below also fall within the scope of the present invention.

Claims

Claim 1 100 parts by weight of raw rubber comprising natural rubber and solution-polymerized styrene-butadiene rubber; and polyoctenamer; comprising 5 to 30 parts by weight of the natural rubber and 70 to 95 parts by weight of the solution-polymerized styrene-butadiene rubber per 100 parts by weight of the raw rubber, wherein the solution-polymerized styrene-butadiene rubber comprises 40 to 70 parts by weight of a first solution-polymerized styrene-butadiene rubber and 15 to 45 parts by weight of a second solution-polymerized styrene-butadiene rubber per 100 parts by weight of the raw rubber, wherein the first solution-polymerized styrene-butadiene rubber has a styrene content of 20% to 30% by weight, a vinyl content of 15% to 25% by weight, and a glass transition temperature (Tg) of -60°C to -40°C, and the second solution-polymerized styrene-butadiene rubber A rubber composition for a tire tread having a styrene content of 20% to 30% by weight, a vinyl content of 45% to 55% by weight, a glass transition temperature (Tg) of -30°C to -20°C, and the polyoctenamer having a weight average molecular weight of 110,000 g / mol to 170,000 g / mol, a glass transition temperature (Tg) of -75°C to -55°C, and a glass transition temperature (Tg) of -25°C to -15°C. Claim 2 delete Claim 3 delete Claim 4 delete Claim 5 delete Claim 6 A rubber composition for a tire tread according to claim 1, wherein the polyoctenamer comprises 5 to 20 parts by weight per 100 parts by weight of raw rubber. Claim 7 delete Claim 8 A rubber composition for a tire tread according to claim 1, wherein the rubber composition further comprises a reinforcing organic filler, and the reinforcing organic filler is silica and carbon black. Claim 9 A rubber composition for a tire tread according to claim 8, wherein the silica comprises 100 to 150 parts by weight per 100 parts by weight of raw rubber. Claim 10 A rubber composition for a tire tread according to claim 8, wherein the carbon black has an iodine adsorption amount of 135 mg / g to 145 mg / g and a DBP (Dibutylphthalate) oil absorption amount of 125 cc / 100g to 135 cc / 100g. Claim 11 A tire manufactured using a rubber composition for a tire tread according to any one of claims 1, 6, and 8 through 10.

Citation Information

Patent Citations

  • Rubber composition for tire tread and pneumatic tire

    JP2007009062A

  • Rubber compositions for tires and pneumatic tires

    JP5536539B2