Etchant composition for semiconductor substrate

TWI945197BActive Publication Date: 2026-11-11ENF TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
TW111114458
Authority / Receiving Office
TW · TW
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-22
Filing Date
2022-04-15
Publication Date
2026-11-11
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

Existing etching methods for semiconductor substrates cause surface damage, contamination, and poor etching rates, especially when dealing with high-concentration doped layers and low-concentration doped layers with small concentration differences, leading to issues like chip loss and substrate surface spots.

Method used

An etchant composition comprising specific compounds like hydrofluoric acid, nitric acid, acetic acid, phosphoric acid, and a balance of water, with additives such as diphenyl ether disulfonate, is used to achieve selective and stable etching, minimizing bubble formation and ensuring uniform etching across layers with varying doping concentrations.

Benefits of technology

The etchant composition provides high etching selectivity and stability, allowing for uniform etching of high-concentration doped layers with reduced bubble formation, enhancing the reliability and efficiency of semiconductor substrate processing.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention provides an etching solution composition for semiconductor substrates that selectively etches highly concentrated doped layers of extrinsic semiconductors. According to this invention, an etching solution composition for semiconductor substrates, an etching method using the same, and a method for manufacturing semiconductor devices are provided. When etching an extrinsic semiconductor substrate comprising doped layers with different doping concentrations, the etching solution composition can achieve a high selectivity for etching highly concentrated doped layers, suppress bubble formation during the etching process, and thereby achieve uniform and stable etching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to etchant compositions for semiconductor substrates, and more particularly, to etchant compositions for semiconductor substrates capable of stably etching extrinsic semiconductor substrates. Prior Technology

[0002] Recently, wafer thinning processes for semiconductor device manufacturing have been used for various purposes. For example, they can be used to manufacture outer semiconductor substrates for ultra-thin wafers, which can be a process that selectively removes highly doped layers while leaving less doped layers.

[0003] Specifically, the aforementioned exopolymer semiconductor substrate may have a structure in which a first layer and a second layer are sequentially stacked, the first layer having a high concentration of doped layer, and the second layer having a lower concentration of doped layer than the first layer. Furthermore, depending on the application, a coating layer selected from metal layers and insulating layers may be further formed on the second layer. Here, the selective etching process of the exopolymer semiconductor substrate may correspond to a process that removes the first layer while leaving the second layer.

[0004] Selective etching processes can be performed using plasma etching methods. However, this etching method may cause etching damage to the substrate surface and may introduce contamination from nickel or iron metals during the etching process. Furthermore, when the lower part of the patterned wafer is thinned, leakage current characteristics may deteriorate due to chip loss at the substrate edges, resulting in poor performance.

[0005] Alternatively, selective etching can be performed using a wet etching method. In this case, the wet etching solution composition may include a mixed solution of oxidants, reducing agents, and buffers, for example, a mixed solution of hydrofluoric acid (HF), nitric acid (HNO₃), and acetic acid (CH₃COOH). However, this etching method exhibits a rather low etching rate on silicon substrates with a resistivity of approximately 0.068 Ω·cm, resulting in spots on the substrate surface during the etching process. Therefore, it is undesirable as a secondary cleaning process is required to remove these spots.

[0006] Therefore, it is still necessary to study etching solution compositions for solving the above problems. Summary of the Invention

[0007] One embodiment of the present invention aims to provide an etching solution composition for stabilizing the etching of an external semiconductor substrate and its use.

[0008] Specifically, one embodiment of the present invention aims to provide an etchant composition, an etching method using the same, and a method for manufacturing a semiconductor device. The etchant composition can selectively etch a high-concentration doped layer in an external semiconductor substrate, the external semiconductor substrate comprising doped layers of non-metals at different concentrations.

[0009] Specifically, one embodiment of the present invention aims to provide an etching solution composition, an etching method using the same, and a method for manufacturing semiconductor devices. The etching solution composition can uniformly and stably etch objects even when there are small concentration differences between doped layers containing non-metals at different concentrations.

[0010] Specifically, one embodiment of the present invention aims to provide an etching method and a method for manufacturing semiconductor devices. The etching method can effectively suppress bubble formation during the etching process, thereby providing a uniform etching selectivity for the external semiconductor substrate.

[0011] In one general embodiment, an etchant composition for a semiconductor substrate comprises: a compound represented by the following chemical formula 1, hydrofluoric acid, nitric acid, acetic acid, phosphoric acid, and the balance being water. [Chemical Formula 1] [in, R1 and R2 are each independently a carboxylate, sulfonate, or sulfate group; R3 is an alkyl group from C1 to C10; L1 is a divalent linker group; a is an integer from 1 to 3; b is an integer from 0 to 3; and When a or b is an integer greater than 2, the substituents can be the same or different.

[0012] In an etchant composition for a semiconductor substrate according to one exemplary embodiment of the present invention, in the compound represented by chemical formula 1, L1 may be -O-, -S- or -NH-; and a and b may each be an integer of 1 or 2 independently.

[0013] In an etchant composition for a semiconductor substrate according to one exemplary embodiment of the present invention, in the compound represented by chemical formula 1, R1 and R2 may be sulfonates; and R3 may be an alkyl group from C6 to C10.

[0014] According to one exemplary embodiment of the present invention, an etchant composition for a semiconductor substrate may contain, relative to the total weight of the etchant composition for a semiconductor substrate, 0.001 to 1% by weight of a compound represented by Formula 1, 4 to 20% by weight of hydrofluoric acid, 4 to 20% by weight of nitric acid, 20 to 60% by weight of acetic acid, 1 to 20% by weight of phosphoric acid, and the balance being water.

[0015] According to one exemplary embodiment of the present invention, an etching solution composition for a semiconductor substrate may contain two or more compounds represented by chemical formula 1 that are different from each other.

[0016] The etching solution composition for a semiconductor substrate according to one exemplary embodiment of the present invention may further contain diphenyl oxide disulfonate.

[0017] In an etchant composition for a semiconductor substrate according to one exemplary embodiment of the present invention, the semiconductor substrate may be an exogenous semiconductor substrate comprising a first doped layer and a second doped layer, wherein the first doped layer is doped with a nonmetal at a first concentration and the second doped layer is doped with a nonmetal at a second concentration lower than the first concentration.

[0018] According to one exemplary embodiment of the present invention, an etchant composition for a semiconductor substrate can satisfy the following relationship 1. [Relation 1] E Sub / E Epi ≥ 30 [in, Esub is the etch rate for the first doped layer; and EEp represents the etch rate for the second doped layer.

[0019] According to one exemplary embodiment of the present invention, the etchant composition for a semiconductor substrate can satisfy the above-mentioned formula 1, and can also satisfy the etching rate of 5 to 30 micrometers / minute for the first doped layer and the etching rate of 0 to 0.5 micrometers / minute for the second doped layer.

[0020] According to one exemplary embodiment of the present invention, the etchant composition for a semiconductor substrate satisfies the above-described relation 1, and also satisfies that the contact angle (γsub) for the first doped layer is 44˚ or less. Furthermore, the difference between the contact angles for the first doped layer and the second doped layer (γepi - γsub) can be 3˚ or more.

[0021] In another general embodiment, an etching method includes contacting the aforementioned etchant composition for a semiconductor substrate with an external semiconductor substrate, the external semiconductor substrate comprising a first doped layer doped with a nonmetal at a first concentration and a second doped layer doped with a nonmetal at a second concentration lower than the first concentration.

[0022] In yet another general embodiment, a method for manufacturing a semiconductor element includes the etching method described above.

[0023] The etchant composition according to the invention provides high selectivity when etching an exopolymer semiconductor substrate comprising doped layers with varying doping concentrations compared to etching a high-concentration doped layer. Furthermore, this etching is performed uniformly and stably, minimizing bubble formation during etching. Therefore, it is commercially advantageous for providing highly reliable exopolymer semiconductor substrates.

[0024] In particular, the etchant composition according to the invention can uniformly etch the object to be etched even when there are small concentration differences between doped layers containing nonmetals at different concentrations. Therefore, it has recently become advantageous for etching processes to provide exopolymer semiconductor substrates for the needs of miniaturized and high-resolution semiconductor devices.

[0025] Furthermore, it has the advantages of maintaining stable etching characteristics over a long period of time and increasing the number of wafers processed. Moreover, the etching solution composition according to the present invention exhibits excellent storage stability, and the number of wafers processed remains stable without decreasing even during long-term use or storage. Simple Explanation of the Diagram

[0026] :none Implementation

[0027] The advantages and features of the present invention, as well as the methods for implementing them, become clear from the detailed description of the following exemplary embodiments. However, the present invention is not limited to the exemplary embodiments disclosed below, but will be implemented in various forms. The exemplary embodiments of the present invention are provided to make the disclosure of the invention complete and to enable those skilled in the art to readily understand the scope of the invention. Therefore, the present invention will be defined by the scope of the appended claims. Hereinafter, the etching solution composition according to the present invention will be described in detail.

[0028] In this specification, the term "extrinsic semiconductor substrate" refers to a semiconductor substrate doped (implanted) with a non-metal. The non-metal can be one or more non-metallic elements, and the non-metallic elements can be elements other than metallic elements. Furthermore, depending on the non-metallic element used for doping, p-type or n-type semiconductor substrates can be obtained.

[0029] Furthermore, the term "first doped layer" used in this specification refers to a layer with a relatively high concentration of doped non-metallic material. It can also have the same meaning as the "high-concentration doped layer" in this specification, and refers to the object to be etched using the etching solution composition according to the present invention.

[0030] Furthermore, the term "second doped layer" used in this specification refers to a layer with a relatively low concentration of doped nonmetallic material. It can also have the same meaning as "low-concentration doped layer" in this specification.

[0031] Additionally, the term "alkyl" used in this specification may include both straight-chain and branched chains.

[0032] In addition, the term "carboxylate group" used in this specification refers to a substituent containing a monovalent anion derived from a carboxylic acid, and in this specification, it may contain *-COOH or its salts.

[0033] In addition, the term "sulfonate" in this specification refers to a substituent containing a monovalent anion derived from sulfonic acid, and in this specification, it may contain *-S(=O) 2-OH or its salt.

[0034] In addition, the term "sulfate" in this specification refers to a substituent containing a monovalent anion derived from sulfuric acid, and in this specification, it may contain *-OS(=O) 2-OH or its salts.

[0035] Additionally, the term "etch selectivity" used in this specification refers to the ratio of the etch rate of the external semiconductor substrate (E Sub / E Epi).

[0036] Recently, due to the requirements of semiconductor devices, the doping degree of high-concentration doped layers on external semiconductor substrates has been gradually reduced. Therefore, it is impossible to achieve the target etching rate using previously developed etchant compositions. Here, the reduction in the doping degree of high-concentration doped layers refers to a decrease in the difference in doping degree between high-concentration doped layers and low-concentration doped layers (i.e., the difference in doping concentration).

[0037] The inventors conducted in-depth research under the aforementioned technical background. As a result, the inventors discovered that after etching the first doped layer with a composition containing specific polyvalent anionic additives, a large amount of additives adsorbed onto the exposed second doped layer, thereby significantly reducing the etching rate. In particular, the etching solution composition according to the present invention is significant in that it can achieve a high etching rate for the target object not only in extrinsic semiconductor substrates (e.g., doping concentration difference: 7.0 × 10¹⁸ / cm³ or more), but also in extrinsic semiconductor substrates with significantly reduced doping concentration differences. Furthermore, since bubble formation is reduced during the etching process, it brings greater benefits to the etching characteristics, thus the composition also has advantages in terms of process technology. As described above, the etching solution composition according to the present invention can uniformly etch higher concentration doped layers with high selectivity in extrinsic semiconductor substrates containing doped layers with different doping concentrations without complicated processes. Moreover, recently, the etching solution composition according to the present invention has been significant in that it can exert advantageous effects on extrinsic semiconductor substrates with low doping concentration differences required for semiconductor devices.

[0038] The etching solution composition according to the present invention will be described below.

[0039] Specifically, an etchant composition according to one exemplary embodiment of the present invention may comprise a compound represented by the following chemical formula 1, hydrofluoric acid, nitric acid, acetic acid, phosphoric acid, and the balance being water. [Chemical Formula 1] [in, R1 and R2 are each independently a carboxylate, sulfonate, or sulfate group; R3 is an alkyl group from C1 to C10; L1 is a divalent linker group; a is an integer from 1 to 3; b is an integer between 0 and 3; When a or b is an integer greater than 2, the substituents can be the same or different.

[0040] An etchant composition according to one exemplary embodiment of the present invention is an etchant composition for a semiconductor substrate, wherein the semiconductor substrate may be an exocrystalline silicon semiconductor substrate. Specifically, the etchant composition according to the present invention may be an etchant composition for an exocrystalline semiconductor substrate including doped layers, wherein the doped layers are doped with nonmetals of different concentrations, and the object to be etched in the present invention may be a doped layer on the exocrystalline semiconductor substrate with a relatively high concentration of doping.

[0041] As a specific example of an etched object using an etchant composition according to one exemplary embodiment of the present invention, it can be a silicon substrate doped with non-metallic particles ranging from 1.0 × 10¹⁸ to 9.9 × 10¹⁸ / cm³. Furthermore, silicon substrates doped with non-metallic particles at lower concentrations can have a difference of 7.0 × 10¹⁸ / cm³ or more, or a difference of less than 7.0 × 10¹⁸ / cm³. In particular, according to recent requirements for semiconductor devices, a significantly reduced difference in doping degree, i.e., a difference of less than 1.0 × 10¹⁸ to 7.0 × 10¹⁸ / cm³, is possible.

[0042] In the etchant composition of an exemplary embodiment of the present invention, the exogenous silicon semiconductor substrate may be doped with one or more non-metallic elements selected from boron, arsenic, phosphorus, etc. Here, when doped with elements such as boron having 4 or fewer outermost electrons, the exogenous semiconductor substrate may be a p-type exogenous semiconductor substrate; and when doped with elements such as arsenic or phosphorus having more than 4 outermost electrons, the exogenous semiconductor substrate may be an n-type exogenous semiconductor substrate.

[0043] The etchant composition according to one exemplary embodiment of the present invention increases the affinity for Si in the chemical solution and provides the advantage of a driving force for the compound represented by Chemical Formula 1, used as an additive, to move to the surface of the semiconductor substrate. Furthermore, the chemical solution is uniformly adsorbed on the surface of the substrate to effectively form a passivation layer, thereby exhibiting improved etching characteristics.

[0044] Furthermore, when etching the exopolymer semiconductor substrate, the etchant composition according to the present invention is used to adsorb the compound of Formula 1 onto the surface of the semiconductor substrate, thereby controlling the Si etching rate. Therefore, when using the etchant composition according to the present invention, the etching rate of low-concentration doped layers is significantly reduced, while the etching rate of high-concentration doped layers is increased, thereby providing an improved etch selectivity.

[0045] In an etchant composition according to one exemplary embodiment of the present invention, in chemical formula 1, L1 may be -O-, -S- or -NH-; and a and b may each be an integer of 1 or 2 independently.

[0046] In an etchant composition according to one exemplary embodiment of the present invention, in chemical formula 1, R1 and R2 may be sulfonates; and R3 may be a C6 to C10 alkyl group. Here, the sulfonate may be *-S(=O)2-OH or a salt thereof, and the salt may be a salt of an alkali metal exemplified by Na or K.

[0047] In the chemical formula 1 of an exemplary embodiment of the present invention, L1 may be -O- or -S-; R1 and R2 may be sulfonates; R3 may be an alkyl group from C6 to C10; and a and b may each be an integer of 1 or 2 independently.

[0048] In order to selectively etch highly doped layers with a higher selectivity ratio, specifically, the compound of Formula 1 can be a C6 to C10 straight-chain alkyl diphenyl ether disulfonate, and preferably a compound represented by Formula 2. Here, as the number of carbon atoms in the compound of Formula 1 is smaller, the force moving towards the surface to be etched is reduced, which is beneficial to the etching rate, and is more conducive to suppressing bubble formation in the process. [Chemical Formula 2] [in, R3 is a straight-chain alkyl group from C6 to C10; and M can be any of the following: hydrogen, sodium, or kJ.

[0049] According to one exemplary embodiment of the present invention, an etchant composition for a semiconductor substrate may contain, relative to the total weight of the etchant composition for a semiconductor substrate, 0.001 to 1% by weight of a compound represented by Formula 1, 4 to 20% by weight of hydrofluoric acid, 4 to 20% by weight of nitric acid, 20 to 60% by weight of acetic acid, 1 to 20% by weight of phosphoric acid, and the balance being water.

[0050] Specifically, the etching solution composition for semiconductor substrates may contain 0.05 to 1% by weight of a compound represented by Formula 1, 5 to 20% by weight of hydrofluoric acid, 5 to 20% by weight of nitric acid, 20 to 50% by weight of acetic acid, 1 to 15% by weight of phosphoric acid, and the balance being water.

[0051] More specifically, the etching solution composition for semiconductor substrates may contain 0.01 to 1% by weight of a compound represented by Formula 1, 10 to 15% by weight of hydrofluoric acid, 10 to 20% by weight of nitric acid, 20 to 40% by weight of acetic acid, 5 to 15% by weight of phosphoric acid, and the balance being water.

[0052] Furthermore, according to one exemplary embodiment of the present invention, an etchant composition for a semiconductor substrate oxidizes the object to be etched using nitric acid to facilitate etching. Therefore, the etchant composition for a semiconductor substrate, based on 1 part by weight of nitric acid, may contain 0.3 to 1 part by weight of hydrofluoric acid, 0.3 to 1 part by weight of phosphoric acid, and 1 to 4 parts by weight of acetic acid; or 0.5 to 1 part by weight of hydrofluoric acid, 0.5 to 1 part by weight of phosphoric acid, and 1.5 to 3 parts by weight of acetic acid; or 0.6 to 1 part by weight of hydrofluoric acid, 0.6 to 1 part by weight of phosphoric acid, and 1.5 to 2.5 parts by weight of acetic acid. When the above weight ratios are satisfied, uniform and stable etching can be achieved, and it can also be applied at a suitable viscosity, thereby exhibiting further improved etching characteristics.

[0053] In the etchant composition according to one exemplary embodiment of the present invention, when the amount of phosphoric acid used exceeds a certain range, the etching rate decreases significantly due to viscosity; and when the amount of acetic acid used exceeds a certain range, the etching rate decreases significantly due to poor interaction with the surface of the etched object, which is undesirable. Furthermore, when the amount of nitric acid used exceeds a certain range, the etching rate for the first doped layer decreases, while the etching rate for the second doped layer increases, resulting in a significantly reduced etching selectivity, which is also undesirable. Moreover, in the etchant composition according to one exemplary embodiment of the present invention, when the amount of the compound of Formula 1 used exceeds a certain range, excessive bubbles are formed during the etching process, leading to residue problems and uneven etching of the high-concentration doped layer, which is also undesirable.

[0054] According to one exemplary embodiment of the present invention, the etching solution composition may contain at least two or more compounds of different chemical formula 1, thereby achieving a more significant etching selectivity.

[0055] Furthermore, the etching solution composition according to one exemplary embodiment of the present invention may also contain a diphenyl ether disulfonate that does not contain alkyl groups. In this case, the diphenyl ether disulfonate may be represented by the following chemical formula A. [Chemical Formula A] [Where, R1, R2, L1, a, and b are defined as in chemical formula 1 above.]

[0056] In an etchant composition according to one exemplary embodiment of the present invention, R1 and R2 in chemical formula A may be sulfonates; and a and b may each be an integer of 1 or 2.

[0057] Based on 1 part by weight of the compound of Formula 1, the diphenyl ether disulfonate represented by Formula A may be used in amounts of 0.01 to 3 parts by weight, specifically 0.1 to 2 parts by weight, more specifically 0.5 to 1.5 parts by weight, but not limited thereto.

[0058] The water contained in the etching solution composition for semiconductor substrates according to one exemplary embodiment of the present invention is not particularly limited, but may specifically be deionized water, more specifically deionized water for semiconductor manufacturing processes, and the resistivity value may be 18 MΩ·cm or higher.

[0059] As described above, the etchant composition according to one exemplary embodiment of the present invention can be used to etch an external semiconductor substrate doped with non-metals at different concentrations. Specifically, the external semiconductor substrate may include a first doped layer doped with non-metals at a first concentration and a second doped layer doped with non-metals at a second concentration lower than the first concentration.

[0060] As an example, the first doped layer may be a silicon substrate doped with nonmetals ranging from 1.0 × 10¹⁸ to 9.9 × 10¹⁸ / cm³.

[0061] As an example, the second doped layer can have a difference of 7.0 × 10¹⁸ / cm³ or more relative to the first doped layer. Furthermore, the second doped layer can have a difference of less than 7.0 × 10¹⁸ / cm³ relative to the first doped layer. In particular, according to the present invention, although the difference is less than 1.0 × 10¹⁸ / cm³ to less than 7.0 × 10¹⁸ / cm³, the first doped layer can be selectively etched.

[0062] According to one exemplary embodiment of the present invention, the etchant composition can satisfy the following equation 1. In this case, equation 1 can represent the etch selectivity ratio between the first doped layer (a high-concentration doped layer) and the second doped layer (a low-concentration doped layer). [Relation 1] E Sub / E Epi ≥ 30 [in, ESub is the etch rate for the first doped layer; EEp represents the etch rate for the second doped layer.

[0063] As an example, the etch selectivity (E Sub / E Epi) of the etch composition can be greater than 30 and less than or equal to 150, or in the range of 31 to 95.

[0064] As an example, the etching rate of the etchant composition for the first doped layer can be 5 to 30 micrometers per minute, and the etching rate for the second doped layer can be 0 to 0.5 micrometers per minute.

[0065] As an example, the etching rate of the etchant composition for the first doped layer can be 8 to 25 micrometers per minute, and the etching rate for the second doped layer can be 0.1 to 0.45 micrometers per minute.

[0066] Furthermore, the etching solution composition according to one exemplary embodiment of the present invention satisfies the above-described relation 1, and the contact angle for the first doped layer is 44˚ or less. When the angle is greater than this value, the interaction between the chemical solution and the surface of the etched object is not smooth, and therefore the first doped layer is not oxidized and etched, which is undesirable.

[0067] Furthermore, according to one exemplary embodiment of the present invention, the contact angle (γ sub) of the etchant composition with respect to the first doped layer can be 40˚ or less, or 20 to 40˚, and the difference in contact angle (γ epi - γ sub) with the second doped layer can be 3 to 15˚, or 5 to 15˚. When the above values ​​are met, it can be evaluated that it has high etch selectivity.

[0068] Furthermore, the etching solution composition according to one exemplary embodiment of the present invention may not contain additives selected from p-toluenesulfonic acid, methanesulfonic acid, dodecylbenzenesulfonic acid, and their salts.

[0069] The use of the etching solution composition according to the present invention will be described below.

[0070] The first embodiment of the present invention may be a method of etching a semiconductor substrate using the above-described etching solution composition.

[0071] A second embodiment of the present invention may be a method for manufacturing semiconductor devices that includes an etching process performed by the above-described method of etching a semiconductor substrate.

[0072] The method for etching a semiconductor substrate according to an exemplary embodiment of the present invention can be used to etch an external semiconductor substrate, specifically, to etch an external semiconductor substrate comprising doped layers having different doping concentrations. In this case, the etched object of the etchant composition according to the present invention can be a high-concentration doped layer in the external semiconductor substrate having a high doping concentration. That is, the etchant composition according to the present invention can be used for selective etching of high-concentration doped layers.

[0073] The doped layer can be formed by doping with one or more elements selected from boron, arsenic, phosphorus, etc. Here, when doped with an element such as boron with 4 or fewer outermost electrons, the exogenous semiconductor substrate can be a semiconductor substrate doped with a p-type element; and when doped with an element such as arsenic or phosphorus with more than 4 outermost electrons, the exogenous semiconductor substrate can be a semiconductor substrate doped with an n-type element.

[0074] According to the method for etching a semiconductor substrate according to an exemplary embodiment of the present invention, even when the concentration difference between the first doped layer and the second doped layer is less than 7.0 × 10¹⁸ / cm³, there is no disadvantage to the etching selectivity. This doping concentration difference is due to the recent demand for miniaturization and higher resolution of semiconductor devices, and the significance of the present invention is that although it is impossible to selectively etch an external semiconductor substrate with such a concentration difference using conventional etchant compositions, it is now possible to perform etching with high etching selectivity according to the present invention.

[0075] The method for etching a semiconductor substrate according to an exemplary embodiment of the present invention can be usefully applied to the manufacturing method of semiconductor devices that can achieve high quantum efficiency, thus providing semiconductor devices with good reliability.

[0076] Specifically, a method for etching a semiconductor substrate using an etchant composition according to an exemplary embodiment of the present invention may include the following steps: contacting the aforementioned etchant composition for the semiconductor substrate with an external semiconductor substrate comprising a first doped layer doped with a non-metal at a first concentration and a second doped layer doped with a non-metal at a second concentration lower than the first concentration. Here, the contact can be performed according to a general wet etching method, and of course, it can also be performed within the corresponding general temperature conditions and processing time range.

[0077] As an example, contact can be made by immersing the exogenous semiconductor substrate in an etchant composition. Alternatively, it can be made by spraying the etchant composition onto the exogenous semiconductor substrate.

[0078] As an example, the immersion method can be carried out at process temperatures below 100°C, specifically between 20 and 100°C, and more specifically between 20 and 40°C. In this case, the processing time can be between 5 and 30 minutes, and can of course be adjusted appropriately depending on the purpose.

[0079] By using an etchant composition according to an exemplary embodiment of the present invention to etch a semiconductor substrate, the first doped layer can be etched rapidly with high selectivity, thereby providing a uniform semiconductor substrate. As described above, excellent results can be achieved even when the doping concentration difference between the doped layers contained in the semiconductor substrate is low. Furthermore, bubble formation is effectively suppressed, which is also commercially advantageous.

[0080] Furthermore, this invention provides a method for manufacturing a semiconductor element, which includes an etching method for a semiconductor substrate. According to the above-described method for manufacturing a semiconductor element, the first doped layer can be selectively etched, and damage to the second doped layer, which has a lower doping concentration, can be effectively suppressed. Therefore, the stability, efficiency, and reliability of the semiconductor element manufacturing process can be significantly improved. In this invention, the type of semiconductor element is not particularly limited.

[0081] The first and second doped layers can be formed on an amorphous silicon wafer. Furthermore, on one surface selected from the first and second doped layers, other functional layers may or may not be included, depending on the purpose.

[0082] The functional layer can be selected from the insulating layer and the conductive layer. Non-limiting examples of insulating layers may include silicon nitride films such as SiN films, SiON films, and doped SiN layers; and silicon nitride films such as spin-on-dielectric (SOD) films, high-density plasma (HDP) films, thermal oxide films, borophosphate silicate glass (BPSG) films, phospho silicate glass (PSG) films, boro silicate glass (BSG) films, polysilazane (PSZ) films, fluorinated silicate glass (FSG) films, low-pressure tetraethyl orthosilicate (LP-TEOS) films, plasma-enhanced tetraethyl orthosilicate (PETEOS) films, and high-temperature oxide films. Temperature Oxide (HTO) films, medium temperature oxide (MTO) films, undoped silicate glass (USG) films, spin-on glass (SOG) films, advanced planarization layer (APL) films, atomic layer deposition (ALD) films, plasma-enhanced oxide (PE-oxide) films, and silicon oxide of O3-tetra ethyl orthosilicate (O3-TEOS). Furthermore, the conductive layer may contain one or more metals selected from Ag, Mg, Al, Pt, Pd, Au, Ni, Nd, Ir, Cr, Li, Ca, Mo, Ti, Sn, Zn, In, and W.

[0083] As described above, according to the present invention, when etching an external semiconductor substrate including a first doped layer and a second doped layer, the first doped layer can be etched with high selectivity, and the etching rate for the second doped layer is significantly reduced, thereby providing an external semiconductor substrate with excellent reliability. Furthermore, even when the external semiconductor substrate includes the aforementioned functional layer, stable etching can be achieved without adversely affecting the etching characteristics.

[0084] Therefore, according to the present invention, when processing various embodiments of exopolymer semiconductor substrates, it is possible to remove only the target high-concentration doped layer with excellent selectivity, and a uniform and highly reliable semiconductor substrate can be provided. Furthermore, despite the increase in processing time, the etch rate and etch selectivity can be maintained consistently. Therefore, according to the present invention, effects surpassing conventional etchant compositions are achieved, thereby providing highly reliable semiconductor devices required for miniaturized and high-resolution semiconductor devices. In particular, compared to conventional etchant compositions, the etchant composition of the present invention for etching exopolymer semiconductor substrates is expected to achieve significantly improved etching characteristics.

[0085] The present invention will now be described in more detail through embodiments. However, these embodiments are for the purpose of providing a more detailed explanation of the invention, and the scope of the invention is not limited to these embodiments. Of course, the embodiments can be appropriately modified and altered by those skilled in the art within the scope of the invention.

[0086] In addition, unless otherwise stated in this invention, the unit of temperature is °C, and the unit of the amount of the composition used is by weight.

[0087] (Evaluation Method)

[0088] 1. Etching rate measurement

[0089] Specifically, an external semiconductor substrate (with boron (B) concentration of the first doped layer to the second doped layer = 7.0 × 10¹⁸ / cm³: 3.0 × 10¹⁴ / cm³) was cut into 10 × 20 mm pieces to prepare evaluation substrates, and the thickness and weight of each substrate were measured. The etching solution compositions of the examples and comparative examples were added to a bath maintained at 25°C by a constant temperature bath, and the wafers were immersed in the bath for 15 minutes for etching. After etching, the substrates were rinsed with ultrapure water, and the remaining etching solution composition and moisture were completely dried using a drying device. The weight of the dried substrates was then measured, and the weight change before and after evaluation was calculated. The etching rate was determined using the following formula 1. [Formula 1] (Initial substrate thickness * weight reduction rate) / processing time = Etching rate

[0090] 2. Bubble formation determination

[0091] Prepare 200 ml of the etching solution compositions of the examples and comparative examples in 1 L graduated cylinders. After forming bubbles with N2 gas in each etching solution composition for 1 minute, the defoaming rate is measured. For bubble formation, a rate of 10 seconds or less (≤10 s) as measured by the above method is marked as 0, and a rate greater than 10 seconds (>10 s) is marked as ×.

[0092] 3. Contact angle measurement

[0093] In the exogenous semiconductor substrate, the surface was cleaned with dilute hydrofluoric acid (DHF) to remove the native oxide films of the first and second doped layers. Immediately afterward, 5 ml of the etching solution composition of each example and comparative example was dropped onto the layer to be evaluated, and the contact angle was measured using a CCD camera.

[0094] (Examples 1 to 11 and Comparative Examples 1 to 6)

[0095] The components listed in Table 1 below are mixed to prepare the etching solution compositions according to the embodiments and comparative examples of the present invention.

[0096] Table 1 distinguish Etching agent (weight %) Additives (by weight %) hydrofluoric acid Nitric acid Phosphoric acid acetic acid substance content Example 1 13 15 10 30 C1 0.1 Example 2 13 15 10 30 C1 0.3 Example 3 13 15 10 30 C1 0.5 Example 4 13 15 10 30 C1 1 Example 5 13 15 10 30 C2 0.1 Example 6 13 15 10 30 C2 0.32 Example 7 13 15 10 30 C3 0.1 Example 8 13 15 10 30 C1+C2 0.1+0.1 Example 9 13 15 10 30 C1 1.5 Example 10 13 15 10 30 C1+B1 0.1+0.1 Example 11 13 15 10 10 C1 0.1 Comparative Example 1 13 15 10 30 - - Comparative Example 2 13 15 10 30 C4 0.1 Comparative Example 3 4.5 20.9 5.5 50.8 - - Comparative Example 4 13 15 10 30 A1 0.15 Comparative Example 5 13 15 10 30 A2 0.28 Comparative Example 6 13 15 - 30 C1 0.1 C1: Sodium Diphenyl Oxide Disulfonate (C6) C2: Sodium Diphenyl Oxide Disulfonate (C8) C3: Sodium Diphenyl Oxide Disulfonate (C10) C4: Sodium Diphenyl Oxide Disulfonate (C16) B1: Diphenyl oxide disulfonic acid A1: p-Toluenesulfonic acid A2: Dodecylbenzenesulfonic acid Example 8: C1+C2 (1:1, weight: weight) Example 10: C1+B1 (1:1, weight: weight)

[0097] Table 2 distinguish Contact angle (°) Etching rate (micrometers per minute) Selection ratio Bubble formation γ sub γ epi-γ sub E Sub Epi E Sub / E Epi Example 1 38.9 8.3 12.36 0.32 38.6 × Example 2 31.4 9.1 10.83 0.14 77.4 × Example 3 30.4 8.7 9.97 0.11 90.6 × Example 4 29.1 9.4 9.42 0.10 94.2 × Example 5 39.4 7.5 13.1 0.40 35.7 × Example 6 31.2 8.5 11 0.20 71.7 × Example 7 39.8 6.7 13.74 0.42 32.7 × Example 8 36.6 9 12.1 0.20 50.4 × Example 9 19.3 5.6 15.47 0.43 36.0 × Example 10 36.2 9 12.1 0.22 55.1 × Actual example 11 41.4 4.4 1.87 0.10 18.7 × Comparative Example 1 43.7 5.9 14.39 0.84 17.1 × Comparative Example 2 40.3 6.3 13.81 0.46 30.0 〇 Comparative Example 3 30.4 5.2 2.99 0.23 13.0 × Comparative Example 4 29.4 4.3 15.42 0.88 17.5 × Comparative Example 5 27.4 4.1 16.13 0.90 17.9 × Comparative Example 6 35.2 4.2 2.15 0.10 21.5 ×

[0098] As shown in Table 2 above, it is confirmed that when using the etching solution composition according to the present invention, a first doped layer with a high doping concentration included in an external semiconductor substrate having two doped layers with different doping concentrations can be etched with a high selectivity. Furthermore, the etching solution composition according to the present invention suppresses bubble formation during etching, thereby enabling more efficient etching of the external semiconductor substrate. Moreover, it has been confirmed that when using two or more additives with different structures, the etching solution composition according to the present invention exhibits superior performance in terms of etching selectivity. Furthermore, when both the compound represented by the above-described chemical formula 1 and the diphenyl ether disulfonate are included, a synergistic effect is also observed in terms of etching selectivity.

[0099] Furthermore, the etching composition according to the present invention has a lower contact angle for an external semiconductor substrate with two doped layers having different doping concentrations, thus enabling a higher etching rate and rapid etching of doped layers with high doping concentrations with a high selectivity.

[0100] However, in comparative cases, selective etching of the first doped layer with a high doping concentration included in an external semiconductor substrate with two layers having different doping concentrations is not possible, or excessive bubbles are formed, resulting in unstable etching. Furthermore, it was confirmed that when using additives containing long-chain alkyl groups with more than 10 carbon atoms, bubbles formed during the etching process are difficult to break, leading to a decrease in etching efficiency and thus poor results.

[0101] Those skilled in the art will understand that this invention is not limited to the illustrative embodiments and drawings described above, and various substitutions, modifications, and alterations can be made without departing from the scope and spirit of the invention. .

[0102] none

Claims

1. An etching solution composition for a semiconductor substrate, comprising a compound represented by the following chemical formula 1, hydrofluoric acid, nitric acid, acetic acid, phosphoric acid, and the balance water: [Chemical Formula 1] wherein, R1 and R2 are each independently a carboxylate, sulfonate, or sulfate group; R3 is a C1 to C10 alkyl group; L1 is -O-, -S-, or -NH-; a is an integer from 1 to 3; b is an integer from 0 to 3; and when a or b is an integer of 2 or more, the substituents can be the same or different, and wherein, relative to the total weight of the etching solution composition for the semiconductor substrate, the etching solution composition for the semiconductor substrate comprises: 0.001 to 1 wt% of the compound represented by the chemical formula 1, 4 to 20 wt% of hydrofluoric acid, 4 to 20 wt% of nitric acid, 20 to 60 wt% of acetic acid, 1 to 20 wt% of phosphoric acid, and the balance being water, wherein the object etched by the etching solution composition for the semiconductor substrate is an exogenous semiconductor including a first doped layer and a second doped layer. A semiconductor substrate, wherein a first doped layer is doped with a non-metal at a first concentration, a second doped layer is doped with a non-metal at a second concentration lower than the first concentration, and wherein the etchant composition for the semiconductor substrate satisfies the following Equation 1: [Equation 1] ESub / EEpi ≥ 30 where ESub is the etch rate for the first doped layer; EEpi is the etch rate for the second doped layer.

2. The etching solution composition for a semiconductor substrate as described in claim 1, wherein, In this chemical formula 1, a and b are each an independent integer of 1 or 2.

3. The etching solution composition for a semiconductor substrate as described in claim 2, wherein, In this chemical formula 1, R1 and R2 are both sulfonates; and R3 is an alkyl group from C6 to C10.

4. The etching solution composition for a semiconductor substrate as described in claim 1, wherein, It contains two or more compounds represented by the chemical formula 1 that are different from each other.

5. The etching solution composition for a semiconductor substrate as described in claim 1, wherein, It also contains diphenyl oxide disulfonate.

6. The etching solution composition for a semiconductor substrate as described in claim 1, wherein, The etching rate for the first doped layer is 5 to 30 micrometers per minute, and the etching rate for the second doped layer is 0 to 0.5 micrometers per minute.

7. The etching solution composition for a semiconductor substrate as described in claim 1, wherein, The contact angle of the first doped layer is below 44˚.

8. The etching solution composition for a semiconductor substrate as described in claim 6, wherein, The difference in contact angle between the etchant composition for the semiconductor substrate and the first doped layer and the second doped layer is 3˚ or more.

9. An etching method comprising contacting an etchant composition selected from any one of claims 1 to 8 for a semiconductor substrate with an external semiconductor substrate, the external semiconductor substrate comprising a first doped layer doped with a nonmetal at a first concentration and a second doped layer doped with a nonmetal at a second concentration lower than the first concentration.

10. A method for manufacturing a semiconductor element, the method comprising the etching method described in claim 9.

Citation Information

Patent Citations

  • Etching solution composition and wet etching method using same

    CN104039925B

  • Wet etching patterning compositions and methods

    TW201510181A