Methods for manufacturing a first protective film wafer, a semiconductor device, and applications of the wafer.
Patent Information
- Application Number
- TW111147289
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-12
- Filing Date
- 2022-12-09
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-12-08
AI Technical Summary
Existing protective film-forming sheets struggle with high-speed attachment to semiconductor wafers, leading to difficulties in ensuring that the tops of bumps protrude from the film and preventing the film from remaining on the upper portion of the bumps, which is essential for flip-chip packaging.
A protective film-forming sheet with a specific elastic modulus ratio between the intermediate peeling layer and buffer layer, utilizing an ethylene-vinyl acetate copolymer with controlled elastic properties, allows for high-speed attachment and ensures that the bumps protrude from the film, minimizing film residue on the bumps.
The solution enables high-speed attachment of the protective film to semiconductor wafers while ensuring that the bumps protrude, thereby preventing film residue, making the semiconductor chips suitable for flip-chip packaging.
Smart Images

Figure TWG2TB001920082_001 
Figure TWG2TB001920082_002 
Figure TWG2TB001920082_003
Abstract
Description
Technical Field
[0001] This invention relates to a first protective film forming wafer, a method for manufacturing a semiconductor device, and the use of the wafer. This application claims priority based on Japanese Patent Application No. 2022-003124 filed in Japan on January 12, 2022, the contents of which are incorporated herein by reference. Prior Technology
[0002] Previously, when mounting multi-pin LSI (Large Scale Integration) packages used in MPUs (Micro Processor Units) or gate arrays on printed wiring boards, the following flip-chip mounting method was used: a semiconductor chip with convex electrodes (hereinafter referred to as "bumps" in this specification) formed on the bonding pads was used, and these bumps were brought into contact with corresponding terminals on the chip mounting substrate by a so-called face-down method, thereby performing fusion / diffusion bonding.
[0003] The semiconductor wafer used in this assembly method is obtained, for example, by grinding or dicing the side of a semiconductor wafer with bumps formed on the circuit surface (in other words, the bump forming surface) to monolithize it. During the process of obtaining this semiconductor wafer, for example, to protect the bump forming surface and the bumps of the semiconductor wafer, a hardening protective film is attached to the bump forming surface, and the film is hardened, thereby forming a protective film on the bump forming surface. In this specification, this protective film forming film and the protective film are sometimes referred to as "first protective film forming film" and "first protective film," respectively. At this time, the bumps on the bump forming surface must penetrate the protective film forming film (first protective film forming film), and the top of the bumps must protrude from the protective film forming film.
[0004] Figure 1 is a cross-sectional view schematically illustrating an example of a state where, contrary to this situation, a protective film formation film remains on the upper part of the bump. In the semiconductor wafer 9 shown here, a protective film formation film 82 is attached to the surface 9a of the bump 91 (bump forming surface), but the top 9101 of the bump 91 does not protrude from the protective film formation film 82, and the protective film formation film 82 remains on the upper part 910 of the bump 91. This shows an example where the entire surface 91a of the bump 91 is covered by the protective film formation film 82, but this example is an example of a residual state of the protective film formation film 82; for example, on the upper part 910 of the bump 91, there is also a situation where a portion of the surface 91a is not covered by the protective film formation film 82 and is exposed. Therefore, a semiconductor wafer with a protective film formation film remaining on the upper part of the bump in this state cannot be used for flip-chip packaging.
[0005] On the other hand, when attaching a protective film to the bump forming surface, a protective film forming sheet is sometimes used, which sequentially stacks a protective film forming film, an adhesive layer, and a substrate. In this specification, this protective film forming sheet is sometimes referred to as a "first protective film forming sheet". In this case, the adhesive layer and the substrate are removed from the protective film forming film after it is attached to the bump forming surface, and the protective film forming film is then hardened.
[0006] As a protective film forming sheet, a protective film forming sheet is disclosed, which sequentially comprises a substrate, an adhesive layer that can be cured by energy lines, a buffer layer, and a curable protective film forming film. The shear storage modulus of the protective film forming film before curing and the tensile storage modulus of the adhesive layer after energy line curing are set to specific ranges (see Patent Document 1). By using this protective film forming sheet (first protective film forming sheet), the adhesive layer and the substrate can be easily removed from the protective film forming film (first protective film forming film) attached to the bump forming surface, thereby enabling the formation of a good protective film (first protective film) on the bump forming surface. Furthermore, when the protective film forming film is attached to the bump forming surface, the buffer layer enhances the protective effect on the bump. [Previous Technical Documents] [Patent Literature]
[0007] [Patent Document 1] International Publication No. 2020 / 189447. Summary of the Invention
[0008] [The problem that the invention aims to solve]
[0009] On the other hand, in recent years, in order to efficiently form a protective film on the bump formation surface, research has been conducted on attaching the protective film forming film in the protective film forming wafer to the bump formation surface at a higher speed than before. However, when attaching the protective film forming film to the bump formation surface, not only is the attachment itself more difficult, but it is also difficult to make the top of the bump protrude from the protective film forming film. Even if it does protrude, the protective film forming film is easily left on the upper part of the bump, including the top. As a result, if the protective film forming film remains on the upper part of the bump, the protective film is directly attached to the upper part of the bump. In this state, the semiconductor wafer is not suitable for flip-chip packaging. In contrast, the protective film forming film in the protective film forming wafer disclosed in Patent Document 1 has excellent adhesion to the bump formation surface, but it is not designed for high-speed attachment.
[0010] The purpose of this invention is to provide a protective film forming sheet, which has a protective film forming film for forming a protective film on a bumped surface of a semiconductor wafer. Even when the protective film forming sheet is attached to the aforementioned surface of the semiconductor wafer at high speed by means of the protective film forming film, the top of the aforementioned bump can protrude from the protective film forming film, thereby suppressing the residual protective film forming film on the top of the bump. [Methods used to solve problems]
[0011] To address the aforementioned issues, the inventors of this invention conducted repeated and diligent research, and discovered that when the elastic modulus of the adhesive layer in the prior protective film forming sheet is approximately equal to that of the buffer layer, it exhibits the following characteristics: the lower the shear storage elastic modulus (Gx') of the intermediate release layer of the adhesive layer relative to the shear storage elastic modulus (GA') of the buffer layer, the more the residue of the first protective film forming film on the upper part of the bump is suppressed, and the easier it is for the top of the bump to protrude, thereby achieving the aforementioned objective.
[0012] That is, the present invention adopts the following structure. [1] A first protective film forming sheet is used to form a first protective film on a bumped surface of at least a semiconductor wafer. The first protective film forming sheet is formed by sequentially stacking a first substrate, a buffer layer, an intermediate release layer, and a first protective film forming film in the thickness direction of these layers. The ratio of the shear storage modulus (Gx') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer (Gx' / GA') is less than 0.6.
[0013] [2] The first protective film forming sheet as described in [1], wherein the aforementioned intermediate release layer contains an ethylene-vinyl acetate copolymer. [3] The first protective film forming sheet as described in [2], wherein in the aforementioned ethylene-vinyl acetate copolymer, the amount of constituent units derived from vinyl acetate is in the proportion of 16% to 40% by mass relative to the total amount of constituent units. [4] The first protective film forming sheet as described in [2] or [3], wherein the weight average molecular weight of the aforementioned ethylene-vinyl acetate copolymer is 200,000 or less. [5] The first protective film forming sheet as described in any of [1] to [4], wherein the shear storage elastic modulus (G x') of the aforementioned intermediate peeling layer is 10000 Pa or less.
[0014] [6] A method for manufacturing a semiconductor device, using a first protective film forming sheet as described in any one of [1] to [5], the manufacturing method comprising: an attachment step, attaching the first protective film forming film of the first protective film forming sheet to a bump-bearing surface of a semiconductor wafer, such that the top of the bump protrudes from the first protective film forming film, thereby setting the first protective film forming sheet on the semiconductor wafer; a first protective film forming step, after the attachment step, removing the layer other than the first protective film forming film from the first protective film forming film of the first protective film forming sheet, and further, when the first protective film forming film is hardenable, hardening the first protective film forming film to form a first protective film, and when the first protective film forming film is non-hardenable... In the case of hardening, the first protective film formed after removing the layers other than the first protective film is regarded as the first protective film, thereby forming the first protective film on the surface with the bumps; in the dicing step, after the first protective film formation step, the semiconductor wafer is diced to form a semiconductor wafer; in the cutting step, after the first protective film formation step, the first protective film is cut; and in the assembly step, the semiconductor wafer with the first protective film obtained after the dicing and cutting steps is flip-chip connected to a substrate with the top of the bumps, the semiconductor wafer with the first protective film having the semiconductor wafer and the first protective film provided on the surface with the bumps in the semiconductor wafer, and the top of the bumps protruding from the first protective film. [7] The semiconductor device manufacturing method described in [6] wherein, in the aforementioned attachment step, the aforementioned first protective film is attached to the surface of the semiconductor wafer having the aforementioned bumps at an attachment speed of 4 mm / s or more.
[0015] [8] Use of a sheet, wherein the sheet is used to form a first protective film on a bumped surface of at least a semiconductor wafer, the sheet being formed by sequentially depositing a first substrate, a buffer layer, an intermediate release layer and a first protective film forming film in the thickness direction of these layers, wherein the ratio (G x' / GA') of the shear storage modulus (G x') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer is less than 0.6. [Invention Benefits]
[0016] According to the present invention, a protective film forming sheet is provided, which includes a protective film forming film for forming a protective film on a bump-bearing surface of a semiconductor wafer. Even when the protective film forming sheet is attached to the aforementioned surface of the semiconductor wafer at high speed via the protective film forming film, the top of the bump can protrude from the protective film forming film, thereby suppressing the residual protective film forming film on the top of the bump. Simple Explanation of the Diagram
[0017] [Figure 1] is a cross-sectional view schematically showing an example of a protective film forming on the upper part of a bump. [Figure 2] is a cross-sectional view schematically showing an example of a first protective film forming sheet according to one embodiment of the present invention. [Figure 3A] is a cross-sectional view of a portion of an example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 3B] is a cross-sectional view of a portion of an example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 3C] is a cross-sectional view of a portion thereof used to schematically illustrate an example of a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 3D] is a cross-sectional view of a portion thereof used to schematically illustrate an example of a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 3E] is a cross-sectional view of a portion of an example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 4A] is a cross-sectional view of another example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 4B] is a cross-sectional view of another example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 4C] is a cross-sectional view of another example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. [Figure 4D] is a cross-sectional view of another example illustrating a method for manufacturing a semiconductor device using the first protective film forming sheet shown in Figure 2. Implementation
[0018] ◇ Sheet for forming the first protective film In one embodiment of the present invention, a first protective film forming sheet is used to form a first protective film on a bumped surface of at least a semiconductor wafer. The first protective film forming sheet is formed by sequentially depositing a first substrate, a buffer layer, an intermediate release layer, and a first protective film forming film in the thickness direction of these layers. The ratio (Gx' / GA') of the shear storage modulus (Gx') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer is less than 0.6. By having this configuration, the first protective film forming sheet of this embodiment can make the top of the bump protrude from the protective film forming film even when the protective film forming film is attached at high speed to the bump-bumped surface of the semiconductor wafer, thereby suppressing the residual protective film forming film on the top of the bump.
[0019] In this specification, the shear storage modulus (G x') of the intermediate release layer refers to the shear storage modulus (G x') [Pa] measured by a shear viscosity measuring device on a disc-shaped intermediate release layer specimen at a temperature of 90°C, a measuring frequency of 1Hz, and a shear strain of 1%.
[0020] In this specification, the shear storage modulus (GA') of the buffer layer refers to the shear storage modulus (GA') [Pa] measured by a shear viscosity measuring device on a circular plate-shaped buffer layer specimen at a temperature of 90°C, a measurement frequency of 1Hz, and a shear strain of 1%.
[0021] For example, the shear storage modulus of the intermediate release layer or buffer layer can be determined by stacking multiple layers of the intermediate release layer or buffer layer to form a circular plate with a diameter of 25 mm and a thickness of 400 μm. Using a shear viscosity measuring device (e.g., Anton-Paar MCR301), at a temperature of 90 °C and a measuring frequency of 1 Hz, the shear strain generated is gradually increased from 0.01% to 10%, and the shear storage modulus of the aforementioned plate is measured when the shear strain is 1%.
[0022] The ratio of the shear storage modulus (Gx') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer (Gx' / GA') is obtained by dividing the value of the shear storage modulus (Gx') [Pa] of the intermediate release layer specimen by the value of the shear storage modulus (GA') [Pa] of the buffer layer specimen.
[0023] In the first protective film forming sheet of this embodiment, the aforementioned ratio (G x' / GA') is less than 0.6, preferably 0.4 or less, more preferably 0.3 or less, further preferably 0.10 or less, and even more preferably 0.05 or less. By having the aforementioned ratio (G x' / GA') below the aforementioned upper limit value, the high-speed adhesion of the first protective film forming sheet and the penetration of the bumps in the first protective film forming film are both improved.
[0024] In the first protective film forming sheet of this embodiment, the aforementioned ratio (G x' / GA') may be 0.00001 or more.
[0025] In the first protective film forming sheet of this embodiment, the shear storage modulus (G x') of the intermediate release layer can be 50,000 Pa or less, preferably 10,000 Pa or less, more preferably 7,000 Pa or less, and even more preferably 1,000 or less, and most preferably 300 or less. By having the shear storage modulus (G x') of the intermediate release layer be below the aforementioned upper limit, it is easy to adjust the aforementioned ratio (G x' / GA') to less than 0.6, thereby improving the high-speed adhesion of the first protective film forming sheet and the penetration of the bumps in the first protective film forming film.
[0026] In the first protective film forming sheet of this embodiment, the shear storage modulus (G x') of the intermediate peel layer can be 1 Pa or more, or 5 Pa or more.
[0027] In the first protective film forming sheet of this embodiment, the shear storage modulus (GA') of the buffer layer is preferably from 10,000 Pa to 400,000 Pa, more preferably from 50,000 Pa to 300,000 Pa, and even more preferably from 100,000 Pa to 200,000 Pa. When the shear storage modulus (GA') of the buffer layer is above the aforementioned lower limit, the effect of the buffer layer becomes more pronounced. When the shear storage modulus (GA') of the buffer layer is below the aforementioned upper limit, the buffer layer can be prevented from becoming too stiff.
[0028] In this specification, the surface with bumps in either a semiconductor wafer or a semiconductor wafer is sometimes referred to as the "bump forming surface". Furthermore, the surface on the opposite side of the bump forming surface in a semiconductor wafer or semiconductor wafer is sometimes referred to as the "inner surface".
[0029] In this specification, the protective film disposed on the side opposite to the bump formation surface (i.e., the inner surface) of a semiconductor wafer or semiconductor chip is referred to as the "second protective film". To form a second protective film on the inner surface of a semiconductor wafer or semiconductor chip opposite to the bump formation surface, a second protective film forming sheet is used, which includes a second protective film forming film for forming the second protective film. Examples of the second protective film forming sheet include a sheet comprising a dicing die and the second protective film forming film disposed on the dicing die. When the dicing die has a substrate identical to the first substrate, this substrate is referred to as the "second substrate".
[0030] The first protective film forming sheet of this embodiment can form the first protective film not only on the bump forming surface of the semiconductor wafer, but also, as described later, on the side surface. That is, the first protective film forming sheet of this embodiment can be used as a sheet for forming the first protective film on at least the bump forming surface of the semiconductor wafer.
[0031] Figure 2 is a cross-sectional view schematically showing an example of a first protective film forming sheet of this embodiment. Furthermore, for ease of understanding of the features of the present invention, the figures used in the following description may sometimes be enlarged representations of the main parts, and the size ratios of the constituent elements may not be the same as the actual figures.
[0032] The first protective film forming sheet 1 shown here comprises a first substrate 11, a buffer layer 12 disposed on one side 11a of the first substrate 11, an intermediate release layer 13 disposed on the side 12a of the buffer layer 12 opposite to the side of the first substrate 11, and a first protective film forming film 14 disposed on the side 13a of the intermediate release layer 13 opposite to the side of the buffer layer 12 (sometimes referred to as the "first side" in this specification). That is, the first protective film forming sheet 1 is formed by sequentially laminating the first substrate 11, the buffer layer 12, the intermediate release layer 13, and the first protective film forming film 14 in the thickness direction of these layers. The first protective film forming sheet 1 further includes a release film 15 disposed on the side (sometimes referred to as "first side") 14a of the first protective film forming film 14 opposite to the side of the intermediate release layer 13.
[0033] In the first protective film forming sheet 1, the intermediate release layer 13 preferably contains an ethylene-vinyl acetate copolymer (sometimes referred to as "EVA" in this specification).
[0034] The release film 15 is not particularly limited and can be any known release film. In the first protective film forming sheet 1, the release film 15 can be of any configuration, and the first protective film forming sheet 1 may also not have a release film 15.
[0035] The first protective film forming sheet of this embodiment is not limited to the first protective film forming sheet shown in FIG2. It can also be modified, deleted or added to the first protective film forming sheet shown in FIG2 without impairing the effect of the present invention. For example, the first protective film forming sheet of this embodiment may further include other layers that do not conform to any of the first substrate, buffer layer, intermediate release layer, first protective film forming film, and release film. However, in the first protective film forming sheet without a release film, it is preferable that the first protective film forming film is the outermost layer on one side, that is, the outermost layer disposed in the lamination direction of each layer. In addition, in the first protective film forming sheet of this embodiment, it is preferable that the first substrate and the buffer layer are in direct contact, the buffer layer and the intermediate release layer are in direct contact, and the intermediate release layer and the first protective film forming film are in direct contact. Next, the layers of the first protective film forming sheet constituting this embodiment will be described.
[0036] ◎ First protective film formation film The aforementioned first protective film can be hardened or non-hardened. For example, the aforementioned first protective film can function as the first protective film by hardening, or it can function as the first protective film in an unhardened state. The first protective film forming the curable material can be either thermosetting or energy-curable, or it can have both thermosetting and energy-curable properties.
[0037] In terms of forming a first protective film with higher protective capabilities, the first protective film forming film is preferably hardened.
[0038] In this specification, the term "energy beam" refers to a beam of electromagnetic waves or charged particles that possess energy quanta. Examples of energy beams include ultraviolet light, radiation, and electron beams. Ultraviolet light can be emitted by using high-pressure mercury lamps, fusion lamps, xenon lamps, black lights, or LED (Light Emitting Diode) lamps as ultraviolet light sources. Electron beams can be emitted by irradiating electron beams generated by electron beam accelerators, etc. In this specification, "energy line hardening property" means the property of hardening by irradiation with energy lines, and "non-energy line hardening property" means the property of not hardening even when irradiated with energy lines. The term "non-hardening" refers to the property of not hardening by any method, such as heating or irradiating with energy lines.
[0039] The first protective film forming film contains resin components, and may or may not contain components other than resin components.
[0040] The first protective film is formed of a soft material, exhibiting high conformability to the bump formation surface and other uneven surfaces of the semiconductor wafer. As a result, the first protective film and the first protective film exhibit high adhesion to the bump formation surface and other uneven surfaces of the semiconductor wafer, and the first protective film exhibits high adhesion to the bump formation surface and other uneven surfaces of the semiconductor wafer.
[0041] When the first protective film forming film of this embodiment is heated and attached to the bump forming surface of a semiconductor wafer, the bumps on the bump forming surface penetrate the first protective film forming film, and the top of the bumps protrudes from the first protective film forming film. Furthermore, the softened first protective film forming film expands between the bumps in a manner that covers the bumps, closely contacting the bump forming surface, and covering the surface of the bumps, especially the surface near the bump forming surface, thereby embedding the base of the bumps. In this state, the residue of the first protective film forming film on the upper part of the bumps is suppressed. When the first protective film forming film is hardened, the first protective film forming film in this state (the state in which the base of the bumps is embedded) is subsequently hardened to finally form the first protective film. When the first protective film forming film is not hardened, the first protective film forming film in this state (the state in which the base of the bumps is embedded) functions as the first protective film. Furthermore, adhesion of the first protective film to the upper part of the bump is naturally suppressed. In particular, when using the first protective film forming sheet of this embodiment, even if the first protective film forming film in the first protective film forming sheet is attached to the bump forming surface of the semiconductor wafer at high speed, the top of the bump protrudes from the first protective film forming film, and the residue of the first protective film forming film and the adhesion of the first protective film to the upper part of the bump are suppressed. The reason why the first protective film forming sheet of this embodiment has such excellent characteristics is that the first protective film forming sheet is composed of a first substrate, a buffer layer, an intermediate release layer, and a first protective film forming film sequentially stacked, and the ratio (G x' / GA') of the shear storage elastic modulus (G x') of the aforementioned intermediate release layer to the shear storage elastic modulus (GA') of the aforementioned buffer layer does not reach 0.6.
[0042] Regarding whether there is a residual first protective film on the upper part of the bump forming surface and whether the first protective film is attached, this can be confirmed, for example, by obtaining scanning electron microscope (SEM) images of the upper part of the bump.
[0043] Regardless of whether the aforementioned first protective film is curable or non-curable, and in the case of curable film, whether it is thermosetting or energy-curing, the first protective film can be composed of one layer (single layer) or multiple layers (two or more). When the first protective film is composed of multiple layers, these multiple layers can be the same or different from each other, and there is no particular limitation on the combination of these multiple layers.
[0044] In this specification, the situation is not limited to the formation of the first protective film mentioned above. The phrase "multilayers may be the same or different" means that "all layers may be the same, all layers may be different, or only some layers may be the same". Furthermore, the phrase "multilayers may be different" means that "at least one of the constituent materials and thicknesses of each layer is different".
[0045] Regardless of whether the aforementioned first protective film is curable or non-curable, and in the case of curable film, whether thermosetting or energy-line curing, the thickness of the aforementioned first protective film is preferably 1 μm to 200 μm, more preferably 10 μm to 150 μm, and even more preferably 20 μm to 130 μm. By having the thickness of the first protective film at or above the aforementioned lower limit, the effect of the first protective film becomes greater. For example, when using the first protective film to form a protective film, a protective film with higher protective capabilities can be formed. By having the thickness of the first protective film at or below the aforementioned upper limit, the thickness of the first protective film can be prevented from becoming excessively thick.
[0046] As described below, when the first protective film is formed not only on the bump forming surface of the semiconductor wafer but also on the side surface, the semiconductor wafer must be a semiconductor wafer with trenches on the bump forming surface. Therefore, when the first protective film is also formed on the side surface of the semiconductor wafer, in addition to the reasons described above, the thickness of the first protective film is preferably 2 μm to 200 μm, more preferably 30 μm to 150 μm, and even more preferably 30 μm to 130 μm, in order to ensure that the first protective film can adequately fill the aforementioned trenches. On the other hand, when a first protective film is formed on the bump formation surface of a semiconductor wafer, but no protective film is formed on the side surface, a semiconductor wafer without trenches on the bump formation surface can be used as the semiconductor wafer. In this case, for the same reason as above (the effect of the first protective film formation becomes more effective; the thickness of the first protective film can be prevented from becoming too thick), the thickness of the first protective film formation is preferably 1 μm to 100 μm, more preferably 20 μm to 75 μm, and even more preferably 35 μm to 55 μm.
[0047] In this specification, the term "thickness of the first protective film forming film" refers to the overall thickness of the first protective film forming film. For example, the term "thickness of the first protective film forming film composed of multiple layers" refers to the total thickness of all the layers constituting the first protective film forming film.
[0048] In this specification, the term "thickness" is not limited to the case of the first protective film forming a film. Unless otherwise specified, it refers to the average thickness measured at five randomly selected locations on the object, which can be obtained using a constant pressure thickness measuring instrument according to JIS K7130.
[0049] [Composition for forming the first protective film] The aforementioned first protective film forming film can be formed using a first protective film forming composition containing the constituent materials of the film. For example, the first protective film forming film can be formed by applying the aforementioned first protective film forming composition to the surface to which the first protective film forming film is to be formed, and then drying it as needed. The ratio of the content of components in the first protective film forming composition that do not vaporize at room temperature is usually the same as the ratio of the content of the aforementioned components in the first protective film forming film. In this specification, "room temperature" means a temperature that is neither particularly cold nor particularly hot, that is, a normal temperature, such as a temperature of 15°C to 25°C.
[0050] The thermosetting first protective film can be formed using a thermosetting first protective film forming composition, the energy line curing first protective film can be formed using an energy line curing first protective film forming composition, and the non-curing first protective film can be formed using a non-curing first protective film forming composition. In this specification, when the first protective film forming film possesses both thermosetting and energy-line hardening properties, and the contribution of thermosetting to the formation of the first protective film is greater than the contribution of energy-line hardening during the formation of the first protective film, the first protective film forming film is considered a thermosetting first protective film forming film. Conversely, when the contribution of energy-line hardening to the formation of the first protective film is greater than the contribution of thermosetting during the formation of the first protective film, the first protective film forming film is considered an energy-line hardening first protective film forming film.
[0051] In the aforementioned first protective film forming film, the total content of one or more of the following ingredients in the first protective film forming film is no more than 100% by mass relative to the total mass of the first protective film forming film. Similarly, in the first protective film forming composition, the total content of one or more of the following ingredients in the first protective film forming composition is no more than 100% by mass relative to the total mass of the first protective film forming composition.
[0052] The first protective film can be formed by applying the composition using known methods, such as the following methods using various coating machines: air knife coating machine, doctor blade coating machine, bar coating machine, gravure coating machine, roller coating machine, roller knife coating machine, curtain coating machine, die coating machine, knife coating machine, screen coating machine, Mayer bar coating machine, and light-touch coating machine.
[0053] Regardless of whether the aforementioned first protective film forming film is curable or non-curable, and in the case of curable film, whether it is thermosetting or energy-line curable, the drying conditions of the first protective film forming composition are not particularly limited. However, when the first protective film forming composition contains the solvent described later, it is preferable to perform heat drying. Furthermore, the first protective film forming composition containing the solvent is preferably heat dried, for example, at 70°C to 130°C for 10 seconds to 5 minutes. However, the thermosetting first protective film forming composition is preferably heat dried in such a way that neither the composition itself nor the thermosetting first protective film forming film formed by the composition is thermosetting.
[0054] The following provides a more detailed explanation of thermosetting first protective film formation, energy line curing first protective film formation, and non-curing first protective film formation.
[0055] ○ Thermosetting first protective film formation film As a thermosetting first protective film forming film, for example, a film containing a polymer component (A), a thermosetting component (B), a curing accelerator (C), a filler material (D), and an additive (I) can be cited.
[0056] Regarding the curing conditions for forming the first protective film by curing the thermosetting first protective film, there are no particular limitations on the degree of curing as long as the first protective film is cured to the extent that it fully performs its function. It can be appropriately selected according to the type of thermosetting first protective film. For example, the heating temperature for heat curing the thermosetting first protective film is preferably between 100°C and 200°C, such as any one of 110°C to 170°C and 120°C to 150°C. The heating time for the aforementioned heat curing is preferably between 0.5 hours and 5 hours, such as any one of 0.5 hours to 4 hours and 1 hour to 3 hours.
[0057] [Composition for forming a thermosetting first protective film] Examples of compositions for forming a thermosetting first protective film include a composition (III) containing a polymer component (A), a thermosetting component (B), a curing accelerator (C), a filler material (D), and an additive (I) (sometimes referred to simply as "composition (III)" in this specification).
[0058] [Polymer component (A)] Polymer component (A) is a polymer compound used to impart film-forming properties or flexibility to the thermosetting first protective film. Furthermore, in this specification, the polymer compound also includes products of polycondensation reactions.
[0059] The polymer component (A) contained in the composition (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these polymer components (A) can be arbitrarily selected.
[0060] Examples of polymer components (A) include: polyvinyl acetal, acrylic resin, urethane resin, phenoxy resin, silicone resin, saturated polyester resin, etc. Of these polymer components (A), polyvinyl acetal is preferred.
[0061] As a polymer component (A), the aforementioned polyvinyl acetal can be exemplified by well-known polyvinyl acetals. Among them, polyvinyl acetal is preferred, for example, polyvinyl formal and polyvinyl butyral, with polyvinyl butyral being more preferred. Polyvinyl butyral can be exemplified as having constituent units represented by the following formulas (i)-1, (i)-2 and (i)-3.
[0062] [Chemistry 1] (In the formula, l, m, and n are each an independent integer greater than or equal to 1.)
[0063] The weight-average molecular weight (Mw) of polyvinyl acetal is preferably between 5,000 and 200,000, and more preferably between 8,000 and 100,000. With the weight-average molecular weight of polyvinyl acetal in this range, the effect of suppressing the residue of the thermosetting first protective film on the upper part of the bump is improved when the thermosetting first protective film is attached to the aforementioned bump forming surface.
[0064] In this specification, the term "weight average molecular weight" refers to the converted value of polystyrene determined by gel permeation chromatography (GPC) unless otherwise specified.
[0065] The glass transition temperature (Tg) of polyvinyl acetal is preferably 40°C to 80°C, and more preferably 50°C to 70°C. With the Tg of polyvinyl acetal in this range, the effect of suppressing the residue of the thermosetting first protective film on the upper part of the bump is improved when the thermosetting first protective film is attached to the aforementioned bump forming surface.
[0066] The ratio of the three or more monomers constituting polyvinyl acetal can be arbitrarily selected.
[0067] As for the aforementioned acrylic resin in polymer component (A), well-known acrylic polymers can be cited as examples. The weight-average molecular weight (Mw) of the acrylic resin is preferably between 5,000 and 1,000,000, and more preferably between 8,000 and 800,000. With the weight-average molecular weight of the acrylic resin in this range, the effect of suppressing the residue of the thermosetting first protective film on the upper part of the bump is improved when the thermosetting first protective film is attached to the aforementioned bump forming surface.
[0068] The glass transition temperature (Tg) of the acrylic resin is preferably -50°C to 70°C, and more preferably -30°C to 60°C. By using this range of Tg for the acrylic resin, the effect of suppressing the thermosetting first protective film from remaining on the upper part of the bump is improved when the thermosetting first protective film is attached to the aforementioned bump forming surface.
[0069] When an acrylic resin has two or more constituent units, its glass transition temperature (Tg) can be calculated using the Fox formula. The Tg of the monomer from which the aforementioned constituent units are derived can be the value recorded in a polymer datasheet or adhesive manual.
[0070] The monomers constituting acrylic resin can be only one type or two or more types. When there are two or more types, the combination and ratio of these monomers can be arbitrarily selected.
[0071] Examples of acrylic resins include: polymers of one or more meth)acrylates; copolymers of two or more monomers selected from (meth)acrylate, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-hydroxymethylacrylamide; and copolymers of one or more meth)acrylates with one or more monomers selected from (meth)acrylate, itaconic acid, vinyl acetate, acrylonitrile, styrene, and N-hydroxymethylacrylamide.
[0072] In this specification, the concept of "(meth)acrylic acid" includes both "acrylic acid" and "methacrylic acid". The same applies to similar terms, such as "(meth)acrylate" which includes both "acrylate" and "methacrylate", and "(meth)acryl" which includes both "acryl" and "methacryl".
[0073] Examples of (meth)acrylates that constitute acrylic resins include, for example: methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, butyl tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (laurate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmitoyl (meth)acrylate), heptadecanyl (meth)acrylate, and so on. alkyl acrylates, such as octadecyl acrylate (stearyl methacrylate), in which the alkyl group has a chain structure with 1 to 18 carbon atoms; cycloalkyl acrylates, such as isoborneol acrylate and dicyclopentyl acrylate; aralkyl acrylates, such as benzyl acrylate; cycloalkyl acrylates, such as dicyclopentenyl acrylate; cycloalkyl acrylates, such as dicyclopentenyl acrylate; cycloalkyl acrylates, such as dicyclopentenyloxyethyl acrylate; and methacrylic acid acrylates. Imines; glycidyl acrylates containing glycidyl groups, such as glycidyl acrylate; hydroxyl-containing methacrylates such as methyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, and 4-hydroxybutyl methacrylate; and substituted amino acrylates such as N-methylaminoethyl methacrylate. Here, "substituted amino group" refers to a group whose structure has one or two hydrogen atoms of an amino group replaced by a group other than a hydrogen atom.
[0074] Acrylic resins may also possess functional groups such as vinyl, (meth)acrylic, amino, hydroxyl, carboxyl, and isocyanate groups, which can bond with other compounds. These functional groups of acrylic resins can bond with other compounds via a crosslinking agent (F) described later, or they can bond directly with other compounds without a crosslinking agent (F). By bonding acrylic resins with other compounds via the aforementioned functional groups, there is a tendency to improve the reliability of encapsulations obtained using a thermosetting first protective film.
[0075] In composition (III), regardless of the type of polymer component (A), the content of polymer component (A) relative to the total content of all components other than the solvent is preferably 5% to 25% by mass, and more preferably 5% to 15% by mass. This content is synonymous with the following: regardless of the type of polymer component (A), the content of polymer component (A) in the thermosetting first protective film forming film is preferably 5% to 25% by mass, and more preferably 5% to 15% by mass, relative to the total mass of the thermosetting first protective film forming film. This is based on the fact that during the process of forming a resin film by removing the solvent from a resin composition containing a solvent, the amount of components other than the solvent usually remains unchanged, and the content ratio of components other than the solvent is the same in both the resin composition and the resin film. Therefore, in this specification, the following is not limited to the case of forming a thermosetting first protective film; the content of components other than the solvent is only described in terms of the content of the resin film after removing the solvent from the resin composition.
[0076] Polymer component (A) sometimes also conforms to thermosetting component (B). In this embodiment, when composition (III) contains components that conform to both polymer component (A) and thermosetting component (B), composition (III) is considered to contain polymer component (A) and thermosetting component (B).
[0077] [Thermosetting component (B)] The thermosetting component (B) is a component that has thermosetting properties and is used to thermoset the thermosetting first protective film.
[0078] The thermosetting component (B) contained in the composition (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these thermosetting components (B) can be arbitrarily selected.
[0079] Examples of thermosetting components (B) include epoxy thermosetting resins, thermosetting polyimide resins, and unsaturated polyester resins, with epoxy thermosetting resins being preferred. In this specification, the term "thermosetting polyimide resin" refers to the general term for polyimide precursors that form polyimide resins through thermosetting and thermosetting polyimides.
[0080] [Epoxy thermosetting resin] Epoxy thermosetting resins are composed of epoxy resin (B1) and thermosetting agent (B2). The epoxy thermosetting resin contained in component (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these epoxy thermosetting resins can be arbitrarily selected.
[0081] ·Epoxy resin (B1) As for epoxy resin (B1), known epoxy resins can be cited, such as: multifunctional epoxy resins, biphenyl compounds, bisphenol A diglycidyl ether and its hydrides, o-cresol phenolic varnish epoxy resins, dicyclopentadiene type epoxy resins, biphenyl type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenyl skeleton type epoxy resins, and other epoxy compounds with two or more functions.
[0082] Epoxy resin (B1) can also be an epoxy resin with unsaturated hydrocarbon groups. Epoxy resins with unsaturated hydrocarbon groups have higher compatibility with acrylic resins compared to epoxy resins without unsaturated hydrocarbon groups. Therefore, by using epoxy resins with unsaturated hydrocarbon groups, there is a tendency to improve the reliability of encapsulations obtained by using thermosetting first protective film formation films.
[0083] Examples of epoxy resins containing unsaturated hydrocarbon groups include compounds with structures in which some of the epoxy groups of a multifunctional epoxy resin are transformed into groups containing unsaturated hydrocarbon groups. Such compounds are obtained, for example, by an addition reaction of (meth)acrylic acid or a derivative thereof onto the epoxy groups. Examples of epoxy resins containing unsaturated hydrocarbon groups include compounds with structures in which unsaturated hydrocarbon groups are directly bonded to the aromatic rings that constitute the epoxy resin. The unsaturated hydrocarbon group is an unsaturated group that has polymerizability. Specific examples of such unsaturated groups include: methine (vinyl), 2-propenyl (allyl), (meth)acrylyl, (meth)acrylamine, etc., with acrylyl being preferred.
[0084] The number of epoxy resins (B1) is not particularly limited in terms of average molecular weight, but in terms of the curability of the thermosetting first protective film and the strength and heat resistance of the cured product of the thermosetting first protective film (e.g., the first protective film), it is preferably 300 to 30,000, more preferably 400 to 10,000, and even more preferably 500 to 3,000. The epoxy equivalent of the epoxy resin (B1) is preferably from 100 g / eq to 1000 g / eq, and more preferably from 200 g / eq to 800 g / eq.
[0085] Epoxy resin (B1) can be used alone or in combination with two or more types. When two or more types are used together, the combination and ratio of these epoxy resins (B1) can be arbitrarily selected.
[0086] • Thermosetting agent (B2) Thermosetting agent (B2) functions as a curing agent for epoxy resin (B1). As a thermosetting agent (B2), examples include compounds having two or more functional groups in one molecule that can react with epoxy groups. Examples of the aforementioned functional groups include phenolic hydroxyl groups, alcoholic hydroxyl groups, amino groups, carboxyl groups, and groups formed by anhydride conversion of acid groups, with phenolic hydroxyl groups, amino groups, or groups formed by anhydride conversion of acid groups being more preferred, and phenolic hydroxyl groups or amino groups being even more preferred.
[0087] Among thermosetting agents (B2), examples of phenolic curing agents with phenolic hydroxyl groups include: polyfunctional phenolic resins, biphenol, phenolic varnish-type phenolic resins, dicyclopentadiene-type phenolic resins, and arylalkyl-type phenolic resins. Among thermosetting agents (B2), amine-based curing agents with amine groups can be exemplified by dicyandiamide (hereinafter sometimes simply referred to as "DICY").
[0088] Thermosetting agents (B2) may also have unsaturated hydrocarbon groups. Examples of thermosetting agents (B2) with unsaturated hydrocarbon groups include compounds with a structure in which some of the hydroxyl groups of a phenolic resin are replaced by groups with unsaturated hydrocarbon groups, and compounds with a structure in which groups with unsaturated hydrocarbon groups are directly bonded to the aromatic ring of a phenolic resin. The aforementioned unsaturated hydrocarbon group in the thermosetting agent (B2) is the same as the unsaturated hydrocarbon group in the epoxy resin having the aforementioned unsaturated hydrocarbon group.
[0089] In the thermosetting agent (B2), the average molecular weight of resin components such as polyfunctional phenolic resin, phenolic varnish-type phenolic resin, dicyclopentadiene-type phenolic resin, and aralkyl-type phenolic resin is preferably 300 to 30,000, more preferably 400 to 10,000, and even more preferably 500 to 3,000. In the thermosetting agent (B2), the molecular weight of non-resin components such as biphenol and dicyandiamide is not particularly limited, but is preferably 60 to 500.
[0090] The thermosetting agent (B2) can be used alone or in combination with two or more. When two or more are used together, the combination and ratio of these thermosetting agents (B2) can be arbitrarily selected.
[0091] The content of the thermosetting agent (B2) in the thermosetting first protective film forming film is preferably from 0.1 parts by weight to 500 parts by weight, more preferably from 1 part by weight to 200 parts by weight, relative to 100 parts by weight of epoxy resin (B1). For example, it can be any one of 5 parts by weight to 150 parts by weight, 10 parts by weight to 100 parts by weight, and 15 parts by weight to 75 parts by weight. By having the aforementioned content of the thermosetting agent (B2) at or above the aforementioned lower limit, the thermosetting first protective film forming film becomes easier to cure. By having the aforementioned content of the thermosetting agent (B2) at or below the aforementioned upper limit, the moisture absorption rate of the thermosetting first protective film forming film is reduced, for example, the reliability of the encapsulation obtained using the thermosetting first protective film forming film is further improved.
[0092] The content of the thermosetting component (B) in the thermosetting first protective film (e.g., the total content of epoxy resin (B1) and thermosetting agent (B2)) is preferably 600 to 1000 parts by mass relative to the content of polymer component (A). By using this range of content for the thermosetting component (B), the effect of suppressing the thermosetting first protective film from remaining on the upper part of the bump is improved when the thermosetting first protective film is attached to the aforementioned bump forming surface, and a hard first protective film can be formed. Furthermore, in order to achieve this effect more significantly, the content of the thermosetting component (B) can be appropriately adjusted according to the type of polymer component (A).
[0093] For example, when the polymer component (A) is the aforementioned polyvinyl acetal, the content of the thermosetting component (B) in the thermosetting first protective film forming film is 100 parts by mass, preferably 600 to 1000 parts by mass, more preferably 600 to 900 parts by mass, and even more preferably 600 to 800 parts by mass, relative to the content of the polymer component (A).
[0094] [Hardening Accelerator (C)] The curing accelerator (C) is a component used to adjust the curing speed of component (III). Examples of preferred curing accelerators (C) include: tertiary amines such as triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; imidazoles (imidazoles in which one or more hydrogen atoms are replaced by groups other than hydrogen atoms) such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; organophosphines (phosphines in which one or more hydrogen atoms are replaced by organic groups) such as tributylphosphine, diphenylphosphine, and triphenylphosphine; and tetraphenylboronic salts such as tetraphenylphosphonium tetraphenylboronic acid and triphenylphosphine tetraphenylboronic acid.
[0095] The curing accelerator (C) contained in component (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these curing accelerators (C) can be arbitrarily selected.
[0096] The content of the curing accelerator (C) in the thermosetting first protective film is preferably 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the thermosetting component (B). By having the aforementioned content of the curing accelerator (C) at or above the aforementioned lower limit, the effects of using the curing accelerator (C) can be obtained more significantly. By having the aforementioned content of the curing accelerator (C) at or below the aforementioned upper limit, for example, the effect of suppressing the segregation of highly polar curing accelerator (C) towards the bonding interface between the thermosetting first protective film and the substrate under high temperature and high humidity conditions is increased, and for example, the reliability of the encapsulation obtained using the thermosetting first protective film is further improved.
[0097] [Filling Material (D)] By adjusting the amount of component (III) and filler material (D) in the thermosetting first protective film, the effect of suppressing the thermosetting first protective film residue on the upper part of the bump can be adjusted when the thermosetting first protective film is attached to the aforementioned bump forming surface. Furthermore, the coefficient of thermal expansion of the cured material (e.g., the first protective film) of the thermosetting first protective film can be more easily adjusted. For example, by making the coefficient of thermal expansion of the first protective film most suitable for the object to which the first protective film is formed, the reliability of the package obtained using the thermosetting first protective film is further improved. Additionally, as described later, since the first protective film is formed not only on the bump forming surface of the semiconductor wafer but also on the side surface, the degree of filling can be adjusted when filling the trenches provided on the bump forming surface of the semiconductor wafer with the first protective film. In addition, by using a thermosetting first protective film forming film containing filler material (D), it is also possible to reduce the moisture absorption rate of the hardened material (e.g., the first protective film) of the thermosetting first protective film forming film or improve the heat dissipation.
[0098] The filler material (D) can be either an organic filler material or an inorganic filler material, preferably an inorganic filler material. Examples of preferred inorganic filler materials include: powders of silicon dioxide, alumina, talc, calcium carbonate, titanium dioxide, iron oxide, silicon carbide, boron nitride, etc.; beads formed by spherizing these inorganic fillers; surface-modified products of these inorganic fillers; single-crystal fibers of these inorganic fillers; glass fibers, etc. Among these inorganic filler materials, silicon dioxide or aluminum oxide are preferred.
[0099] The filler material (D) contained in the composition (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these filler materials (D) can be arbitrarily selected.
[0100] The content of filler material (D) in the thermosetting first protective film is preferably 5% to 45% by mass, more preferably 5% to 40% by mass, and even more preferably 5% to 30% by mass, relative to the total mass of the thermosetting first protective film. With this range of proportions, when the thermosetting first protective film is attached to the aforementioned bump forming surface, the effect of suppressing the thermosetting first protective film residue on the upper part of the bump is improved, and the coefficient of thermal expansion can be adjusted more easily. Furthermore, resin exudation outside the wafer during attachment can be suppressed.
[0101] [Additive (I)] By adjusting the type or amount of additive (I) in the composition (III) and the thermosetting first protective film forming film, when the thermosetting first protective film forming film is attached to the aforementioned bump forming surface, the effect of suppressing the thermosetting first protective film forming film residue on the upper part of the bump can be adjusted. Among these, in terms of improving the effect of inhibiting the formation of residual heat-curing first protective film, the preferred additives (I) include, for example, rheology control agents, surfactants, and silicone oils.
[0102] More specifically, examples of rheology control agents mentioned above include polyhydroxycarboxylic acid esters, polycarboxylic acids, and polyamide resins. Examples of surfactants mentioned above include modified siloxanes and acrylic polymers. Examples of silicone oils mentioned above include aralkyl-modified silicone oils and modified polydimethylsiloxanes. Examples of modifying groups include: aralkyl groups; polar groups such as hydroxyl groups; and groups with unsaturated bonds such as vinyl and phenyl groups.
[0103] Other additives besides those mentioned above in Additive (I) may include, for example, plasticizers, antistatic agents, antioxidants, gettering agents, UV absorbers, adhesive agents, and other general-purpose additives.
[0104] The additives (I) contained in the composition (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these additives (I) can be arbitrarily selected.
[0105] The content of additive (I) in composition (III) and thermosetting first protective film is not particularly limited, and can be appropriately adjusted according to the type or purpose of the aforementioned additive (I). For example, when the purpose is to adjust the above-mentioned effect of inhibiting the residue of the thermosetting first protective film, the content of additive (I) in the thermosetting first protective film is preferably 0.5% to 10% by mass, more preferably 0.5% to 7% by mass, and even more preferably 0.5% to 5% by mass relative to the total mass of the thermosetting first protective film.
[0106] [Coupling agent (E)] Component (III) and the thermosetting first protective film may also contain a coupling agent (E). By using a compound having a functional group that can react with inorganic or organic compounds as the coupling agent (E), the adhesion and bonding strength of the thermosetting first protective film to the substrate can be improved. In addition, by using the coupling agent (E), the water resistance of the cured product of the thermosetting first protective film (e.g., the first protective film) is improved without compromising its heat resistance.
[0107] The coupling agent (E) is preferably a compound having a functional group that can react with the functional groups of the polymer component (A), the thermosetting component (B), etc., and is more preferably a silane coupling agent. Preferred silane coupling agents include, for example, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxymethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, and 3-(2-aminoethylamino)propyltrimethoxysilane. Silane, 3-(2-aminoethylamino)propylmethyldiethoxysilane, 3-(phenylamino)propyltrimethoxysilane, 3-anilinepropyltrimethoxysilane, 3-ureopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfide, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, imidazole silane, etc.
[0108] The coupling agent (E) contained in the composition (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these coupling agents (E) can be arbitrarily selected.
[0109] When using a coupling agent (E), the content of the coupling agent (E) in the thermosetting first protective film is, for example, 0.03 to 20 parts by mass relative to 100 parts by mass of the total content of polymer component (A) and thermosetting component (B). By having the aforementioned content of the coupling agent (E) at or above the aforementioned lower limit, the following effects resulting from the use of the coupling agent (E) can be obtained more significantly: improved dispersibility of the filler material (D) in the resin, or improved adhesion between the thermosetting first protective film and the substrate. By having the aforementioned content of the coupling agent (E) at or below the aforementioned upper limit, the generation of outgassing can be further suppressed.
[0110] [Crosslinking agent (F)] When a compound having functional groups such as vinyl, (meth)acrylic, amino, hydroxyl, carboxyl, or isocyanate groups that can bond with other compounds is used as polymer component (A), component (III) and the thermosetting first protective film forming film may also contain a crosslinking agent (F). The crosslinking agent (F) is a component used to crosslink the aforementioned functional groups in polymer component (A) with other compounds. By crosslinking in this way, the initial adhesion and cohesion of the thermosetting first protective film forming film can be adjusted.
[0111] Examples of crosslinking agents (F) include: organic polyisocyanate compounds, organic polyimine compounds, metal chelate crosslinking agents (crosslinking agents with metal chelate structures), and aziridine crosslinking agents (crosslinking agents with aziridine groups).
[0112] Examples of the aforementioned organic polyisocyanate compounds include: aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, and alicyclic polyisocyanate compounds (hereinafter, these compounds are sometimes collectively referred to as "aromatic polyisocyanate compounds, etc."); trimers, isocyanurates, and adducts of the aforementioned aromatic polyisocyanate compounds, etc.; and terminal isocyanate carbamate prepolymers of the aforementioned aromatic polyisocyanate compounds and polyol compounds as reactants. The term "adduct" refers to the reaction product of the aforementioned aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, or alicyclic polyisocyanate compounds with ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, or castor oil, etc., containing low-molecular-weight active hydrogen compounds. Examples of the aforementioned adducts include the phenylenedimethyl diisocyanate adduct of trimethylolpropane, as described below. In this specification, the term "terminated isocyanate carbamate prepolymer" means a prepolymer having carbamate bonds and isocyanate groups at the ends of the molecules.
[0113] More specifically, examples of the aforementioned organic polyisocyanate compounds include: 2,4-toluene diisocyanate; 2,6-toluene diisocyanate; 1,3-phenylenedimethyl diisocyanate; 1,4-xylene diisocyanate; diphenylmethane-4,4'-diisocyanate; diphenylmethane-2,4'-diisocyanate; 3-methyldiphenylmethane diisocyanate; hexamethylene diisocyanate; isophorone diisocyanate; dicyclohexylmethane-4,4'-diisocyanate; dicyclohexylmethane-2,4'-diisocyanate; compounds formed by the addition of one or more of toluene diisocyanate, hexamethylene diisocyanate, and phenylenedimethyl diisocyanate to all or part of the hydroxyl groups of polyols such as trimethylolpropane; lysine diisocyanate, etc.
[0114] Examples of the aforementioned organic polyimide compounds include: N,N'-diphenylmethane-4,4'-bis(1-aziridinium methylamine), trimethylolpropane-tri-β-aziridinium propionate, tetramethylolmethane-tri-β-aziridinium propionate, and N,N'-toluene-2,4-bis(1-aziridinium methylamine)triethyl melamine.
[0115] When using an organic polyisocyanate compound as a crosslinking agent (F), it is preferable to use a hydroxyl-containing polymer as the polymer component (A). When the crosslinking agent (F) has isocyanate groups and the polymer component (A) has hydroxyl groups, the crosslinked structure can be easily introduced into the thermosetting first protective film by the reaction between the crosslinking agent (F) and the polymer component (A).
[0116] The crosslinking agent (F) contained in the composition (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these crosslinking agents (F) can be arbitrarily selected.
[0117] When a crosslinking agent (F) is used, the content of the crosslinking agent (F) in composition (III) relative to the content of polymer component (A) is, for example, 0.01 to 20 parts by mass. By ensuring that the content of the crosslinking agent (F) is above or below the aforementioned lower limit, the effects of using the crosslinking agent (F) can be obtained more significantly. By ensuring that the content of the crosslinking agent (F) is below the aforementioned upper limit, the excessive use of the crosslinking agent (F) is suppressed.
[0118] [Other ingredients] The composition (III) and the thermosetting first protective film may also contain other components that do not conform to the above-mentioned polymer component (A), thermosetting component (B), curing accelerator (C), filler material (D), additive (I), coupling agent (E) and crosslinking agent (F), to the extent that the effects of the present invention are not impaired. Other components mentioned above include, for example, energy-curing resins and photopolymerization initiators.
[0119] The other components contained in component (III) and the thermosetting first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these other components can be arbitrarily selected. The content of the aforementioned other components in composition (III) and the thermosetting first protective film is not particularly limited, and can be selected appropriately according to the purpose.
[0120] [solvent] Component (III) preferably contains a solvent. The operability of component (III) containing a solvent is improved. The aforementioned solvents are not particularly limited, but preferred solvents include, for example, hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutanol (2-methylpropane-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds with amide bonds) such as dimethylformamide and N-methylpyrrolidone. The solvent contained in component (III) may be only one type or two or more types. In the case of two or more types, the combination and ratio of these solvents may be arbitrarily selected.
[0121] As a better solvent for composition (III), for example, methyl ethyl ketone can be used to mix the components contained in composition (III) more evenly.
[0122] There is no particular limitation on the content of solvent in composition (III). For example, it can be appropriately selected according to the types of components other than solvent.
[0123] In terms of improving the target effect of the present invention (the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film, as an example of a preferred thermosetting first protective film forming film, the following thermosetting first protective film forming film can be cited: containing a polymer component (A), a thermosetting component (B), a curing accelerator (C), a filler material (D), and an additive (I), and the total content of the aforementioned polymer component (A), the aforementioned thermosetting component (B), the aforementioned curing accelerator (C), the aforementioned filler material (D), and the aforementioned additive (I) in the aforementioned thermosetting first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more, relative to the total mass of the aforementioned thermosetting first protective film forming film. In view of the above, as an example of a better thermosetting first protective film forming film, the following thermosetting first protective film forming film can be cited: containing a polymer component (A), a thermosetting component (B), a curing accelerator (C), a filler material (D), and an additive (I), wherein the aforementioned polymer component (A) is polyvinyl acetal, the aforementioned thermosetting component (B) is epoxy resin (B1) and a thermosetting agent (B2), and the aforementioned additive (I) is one or more selected from the group consisting of rheology control agents, surfactants, and silicone oils, wherein the total content of the aforementioned polymer component (A), the aforementioned thermosetting component (B), the aforementioned curing accelerator (C), the aforementioned filler material (D), and the aforementioned additive (I) in the aforementioned thermosetting first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. The thickness of these thermosetting first protective films is preferably 2 to 7 times, more preferably 3 to 6 times, relative to the thickness of the intermediate release layer.
[0124] [Method for manufacturing a composition for forming a thermosetting first protective film] The heat-curable first protective film forming composition (III) is obtained by blending the components used to form the composition. There is no particular restriction on the order in which the ingredients are added when preparing the formula, and more than two ingredients may be added at the same time. There are no particular limitations on the method of mixing the ingredients during preparation. You may choose an appropriate method from the following known methods: mixing by rotating a stir bar or stirring blade; mixing by using a mixer; mixing by applying ultrasound, etc. There are no particular restrictions on the temperature and time when adding and mixing the ingredients, as long as the ingredients are not deteriorated. Appropriate adjustments can be made, with the optimal temperature being 15°C to 30°C.
[0125] ○ Energy line hardening first protective film formation film As a first protective film for energy line hardening, an example of a film containing an energy line hardening component (a), a filler material, and an additive can be cited.
[0126] Regarding the hardening conditions for forming the first protective film by hardening the energy line hardening first protective film, there are no particular limitations as long as the first protective film becomes hardened to the extent that it fully performs its function. It can be appropriately selected according to the type of energy line hardening first protective film. For example, the illuminance of the energy line during the curing of the energy line hardening first protective film is preferably between 180 mW / cm² and 280 mW / cm². Furthermore, the light intensity of the energy line during the aforementioned curing is preferably between 450 mJ / cm² and 1000 mJ / cm².
[0127] [Composition for forming the first protective film with energy line hardening] Examples of compositions for forming a first protective film with energy line hardening properties include a composition (IV) containing an energy line hardening component (a), a filler material, and an additive (sometimes referred to simply as "composition (IV)" in this specification).
[0128] [Energy line hardening component (a)] The energy-line hardening component (a) is a component that is hardened by irradiation with energy lines. This component is used to impart film-forming properties or flexibility to the energy-line hardening first protective film. The energy line hardening component (a) is preferably unhardened, and more preferably adhesive, and even more preferably unhardened and adhesive.
[0129] Examples of energy line hardening components (a) include polymers (a1) having energy line hardening groups and a weight average molecular weight of 80,000 to 2,000,000, and compounds (a2) having energy line hardening groups and a molecular weight of 100 to 80,000. The aforementioned polymer (a1) may be at least partially cross-linked by a cross-linking agent, or it may not be cross-linked.
[0130] [Polymers with energy-line hardening groups and a weight-average molecular weight of 80,000 to 2,000,000 (a1)] As a polymer (a1) having an energy line hardening group and a weight average molecular weight of 80,000 to 2,000,000, an example is acrylic resin (a1-1), which has a structure formed by the polymerization of acrylic polymer (a11) and energy line hardening compound (a12). The acrylic polymer (a11) has functional groups that can react with groups of other compounds, and the energy line hardening compound (a12) has energy line hardening groups such as groups that react with the aforementioned functional groups and energy line hardening double bonds.
[0131] Examples of functional groups that can react with other compounds include hydroxyl, carboxyl, amino, substituted amino groups (groups with one or two hydrogen atoms of an amino group replaced by groups other than hydrogen atoms), and epoxy groups. However, for the purpose of preventing circuit corrosion of semiconductor wafers or semiconductor chips, the aforementioned functional groups are preferably groups other than carboxyl. Of these aforementioned functional groups, the hydroxyl group is preferred.
[0132] • Acrylic polymers with functional groups (a11) Examples of the aforementioned acrylic polymers with functional groups (a11) include polymers that are copolymerized from acrylic monomers having the aforementioned functional groups and acrylic monomers without the aforementioned functional groups, as well as polymers that are copolymerized from monomers other than these monomers (non-acrylic monomers). The aforementioned acrylic polymer (a11) can be a random copolymer or a block copolymer.
[0133] Examples of acrylic acid monomers having the aforementioned functional groups include: monomers containing hydroxyl groups, monomers containing carboxyl groups, monomers containing amino groups, monomers containing substituted amino groups, and monomers containing epoxy groups.
[0134] Examples of hydroxyl-containing monomers mentioned above include: hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl methacrylate, and other hydroxyalkyl methacrylates; and non-methacrylate unsaturated alcohols (unsaturated alcohols without a methacrylate backbone) such as vinyl alcohol and allyl alcohol.
[0135] Examples of the aforementioned carboxyl-containing monomers include: (meth)acrylic acid, butenoic acid, and other ethylene-unsaturated monocarboxylic acids (monocarboxylic acids with ethylene-unsaturated bonds); fumaric acid, iconic acid, maleic acid, citracic acid, and other ethylene-unsaturated dicarboxylic acids (dicarboxylic acids with ethylene-unsaturated bonds); anhydrides of the aforementioned ethylene-unsaturated dicarboxylic acids; and (meth)acrylic acid carboxylalkyl esters such as 2-carboxyethyl methacrylate.
[0136] Acrylic acid monomers having the aforementioned functional groups are preferably monomers containing hydroxyl groups, monomers containing carboxyl groups, and more preferably monomers containing hydroxyl groups.
[0137] The acrylic monomers having the aforementioned functional groups constituting the aforementioned acrylic polymer (a11) may be only one type or two or more types. In the case of two or more types, the combination and ratio of these acrylic monomers may be arbitrarily selected.
[0138] Examples of acrylic monomers that do not possess the aforementioned functional groups include: methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, and isononyl methacrylate. Alkyl esters, such as decyl methacrylate, undecyl methacrylate, dodecyl methacrylate (laurate methacrylate), tridecyl methacrylate, tetradecyl methacrylate (myristyl methacrylate), pentadecyl methacrylate, hexadecyl methacrylate (palmitoyl methacrylate), heptadecanyl methacrylate, and octadecyl methacrylate (stearyl methacrylate), are chain alkyl esters in which the alkyl group has a chain structure with 1 to 18 carbon atoms.
[0139] Examples of acrylic monomers that do not possess the aforementioned functional groups include: methoxymethyl methacrylate, methoxyethyl methacrylate, ethoxymethyl methacrylate, ethoxyethyl methacrylate, and other alkoxyalkyl-containing (meth)acrylates; aromatic (meth)acrylates including aryl (meth)acrylates such as phenyl (meth)acrylate; non-crosslinked (meth)acrylamide and its derivatives; and non-crosslinked tertiary amino (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate.
[0140] The acrylic monomers that do not have the aforementioned functional groups that constitute the aforementioned acrylic polymer (a11) may be only one type or two or more types. In the case of two or more types, the combination and ratio of these acrylic monomers may be arbitrarily selected.
[0141] Examples of non-acrylic acid monomers mentioned above include: olefins such as ethylene and norbornene; vinyl acetate; styrene, etc. The aforementioned non-acrylic monomers constituting the aforementioned acrylic polymer (a11) may be only one type or may be two or more types. In the case of two or more types, the combination and ratio of these non-acrylic monomers may be arbitrarily selected.
[0142] In the aforementioned acrylic polymer (a11), the proportion (content) of the constituent units derived from the acrylic monomer having the aforementioned functional groups relative to the total amount of the constituent units constituting the aforementioned acrylic polymer (a11) is preferably 0.1% to 50% by mass, more preferably 1% to 40% by mass, and even more preferably 3% to 30% by mass. By using the aforementioned proportion within this range, the content of the energy-curing groups in the aforementioned acrylic resin (a1-1) obtained by copolymerizing the aforementioned acrylic polymer (a11) and the aforementioned energy-curing compound (a12) allows the degree of curing of the cured material (e.g., the first protective film) of the energy-curing first protective film formation film to be easily adjusted to a preferred range.
[0143] The acrylic polymer (a11) that constitutes the aforementioned acrylic resin (a1-1) may be only one type or may be two or more types. In the case of two or more types, the combination and ratio of these acrylic polymers (a11) can be arbitrarily selected.
[0144] The content of acrylic resin (a1-1) in the energy line curing first protective film forming film is preferably 1% to 40% by mass, more preferably 2% to 30% by mass, and even more preferably 3% to 20% by mass relative to the total mass of the energy line curing first protective film forming film.
[0145] • Energy line hardening compound (a12) The aforementioned energy-line hardening compound (a12) preferably has one or more groups selected from the group consisting of isocyanate groups, epoxy groups, and carboxyl groups as functional groups that can react with the aforementioned acrylic polymer (a11), and more preferably has an isocyanate group as the aforementioned group. When the aforementioned energy-line hardening compound (a12) has an isocyanate group as the aforementioned group, the isocyanate group readily reacts with the hydroxyl group of the acrylic polymer (a11) having a hydroxyl group as the aforementioned functional group.
[0146] The aforementioned energy line hardening compound (a12) preferably has one to five aforementioned energy line hardening groups in one molecule, more preferably one to two.
[0147] Examples of the aforementioned energy line hardening compounds (a12) include: 2-methacryloxyethyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloxyisocyanate, allyl isocyanate, 1,1-(bisacryloxymethyl)ethyl isocyanate; acryloxymonoisocyanate compounds obtained by reacting diisocyanate compounds or polyisocyanate compounds with hydroxyethyl (meth)acrylate; and acryloxymonoisocyanate compounds obtained by reacting diisocyanate compounds or polyisocyanate compounds, polyol compounds, and hydroxyethyl (meth)acrylate. Among these aforementioned energy-hardening compounds (a12), 2-methylpropenyl ethyl isocyanate is preferred.
[0148] The energy-curing compound (a12) constituting the aforementioned acrylic resin (a1-1) may be only one type or may be two or more types. In the case of two or more types, the combination and ratio of these energy-curing compounds (a12) may be arbitrarily selected.
[0149] In the aforementioned acrylic resin (a1-1), the content of the energy-curing group derived from the aforementioned energy-curing compound (a12) relative to the content of the aforementioned functional groups derived from the aforementioned acrylic polymer (a11) is preferably 20 mol% to 120 mol%, more preferably 35 mol% to 100 mol%, and even more preferably 50 mol% to 100 mol%. By using the aforementioned content within this range, the adhesion of the cured material (e.g., the first protective film) of the energy-curing first protective film becomes stronger. Furthermore, when the aforementioned energy-curing compound (a12) is a single-functional compound (having one of the aforementioned groups in one molecule), the upper limit of the aforementioned content ratio is 100 mol%, but when the aforementioned energy-curing compound (a12) is a multifunctional compound (having two or more of the aforementioned groups in one molecule), the upper limit of the aforementioned content ratio sometimes exceeds 100 mol.
[0150] The weight average molecular weight (Mw) of the aforementioned polymer (a1) is preferably from 100,000 to 2,000,000, and more preferably from 300,000 to 1,500,000.
[0151] When at least a portion of the aforementioned polymer (a1) is crosslinked by a crosslinking agent, the aforementioned polymer (a1) may be formed by polymerizing monomers that do not conform to any of the monomers that constitute the aforementioned acrylic polymer (a11) as described above and have a group that reacts with the crosslinking agent, and crosslinking is carried out in the group that reacts with the aforementioned crosslinking agent, or it may be formed by crosslinking in the group that reacts with the aforementioned functional group derived from the aforementioned energy line hardening compound (a12).
[0152] The aforementioned polymer (a1) contained in the composition (IV) and the energy line hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these polymers (a1) can be arbitrarily selected.
[0153] [Compounds with energy-line hardening groups and molecular weights ranging from 100 to 80,000 (a2)] The aforementioned energy-line hardening group in a compound (a2) having an energy-line hardening group and a molecular weight of 100 to 80,000 can be exemplified by a group containing an energy-line hardening double bond, and preferably by (meth)acrylyl, vinyl, etc.
[0154] The aforementioned compound (a2) is not particularly limited as long as it meets the above conditions. Examples include: low molecular weight compounds with energy-line hardening groups, epoxy resins with energy-line hardening groups, and phenolic resins with energy-line hardening groups.
[0155] As a low molecular weight compound having an energy line hardening group in the aforementioned compound (a2), examples include multifunctional monomers or oligomers, and preferably acrylate compounds having a (meth)acrylic group. Examples of the aforementioned acrylate compounds include: 2-hydroxy-3-(meth)acryloxypropyl methacrylate, polyethylene glycol di(meth)acrylate, propoxylated and ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloxypolyethoxy)phenyl]propane, ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloxydiethoxy)phenyl]propane, 9,9-bis[4-(2-(meth)acryloxy)propane, and 2,2-bis[4-((meth)acryloxydiethoxy)phenyl]propane. [Ethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloxy)polypropoxy)phenyl]propane, tricyclodecanediethanol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate Diethyl esters, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 2,2-bis[4-((meth)propenyloxyethoxy)phenyl]propane, neopentyl glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, 2-hydroxy-1,3-di(meth)propenyloxypropane and other difunctional (meth)acrylates; tris(2-(meth)propenyloxyethyl) isocyanurate, ε-caprolactone-modified tris(2-(meth)propenyloxyethyl) isocyanurate Multifunctional (meth)acrylates such as methyl methacrylate, ethoxylated glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, di-trimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, dipentaerythritol hexa(meth)acrylate; and multifunctional (meth)acrylate oligomers such as (meth)acrylate aminocarbamate oligomers.
[0156] In the aforementioned compound (a2), the epoxy resin having a heat-curing group or the phenolic resin having a heat-curing group can be, for example, the resin described in paragraph 0043 of Japanese Patent Application Publication No. 2013-194102. Such a resin also conforms to the resin constituting the thermosetting component described later, but is regarded as the aforementioned compound (a2) in this embodiment.
[0157] The weight-average molecular weight of the aforementioned compound (a2) is preferably from 100 to 30,000, and more preferably from 300 to 10,000.
[0158] The aforementioned compound (a2) contained in the composition (IV) and the energy line hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these compounds (a2) can be arbitrarily selected.
[0159] [Polymers without energy-line hardening groups (b)] When the composition (IV) and the energy line hardening first protective film form contain the aforementioned compound (a2) as the aforementioned energy line hardening component (a), it is preferable that it also contains a polymer (b) that does not have an energy line hardening group. The aforementioned polymer (b) may be cross-linked at least in part by a cross-linking agent, or it may not be cross-linked.
[0160] Examples of polymers (b) that do not have energy-line hardening groups include: acrylic polymers, phenoxy resins, urethane resins, polyesters, rubber-based resins, urethane resins, etc. Of these aforementioned polymers (b), acrylic polymers are preferred (hereinafter, sometimes simply referred to as "acrylic polymer (b-1)").
[0161] The acrylic polymer (b-1) can be a known acrylic polymer, such as a homopolymer of one acrylic monomer, a copolymer of two or more acrylic monomers, or a copolymer of one or more acrylic monomers with one or more monomers other than acrylic monomers (non-acrylic monomers).
[0162] Examples of acrylic monomers that constitute the acrylic polymer (b-1) include: alkyl (meth)acrylates, (meth)acrylates having a cyclic backbone, (meth)acrylates containing glycidyl groups, (meth)acrylates containing hydroxyl groups, and (meth)acrylates containing substituted amino groups. Here, "substituted amino groups" are as explained above.
[0163] Examples of the aforementioned alkyl methacrylates include: alkyl methacrylates that are identical to the acrylic monomers (alkyl methacrylates, etc., in which the alkyl group constituting the acrylic polymer (a11) described above does not have the aforementioned functional group.
[0164] Examples of (meth)acrylates having a cyclic skeleton include: isocamphene methacrylate, dicyclopentyl methacrylate, and other cycloalkyl methacrylates; benzyl methacrylate and other aralkyl methacrylates; dicyclopentenyl methacrylate and other cycloalkyl methacrylates; dicyclopentenyl methacrylate and other cycloalkyl methacrylates; dicyclopentenyl methacrylate and other cycloalkyl methacrylates.
[0165] Examples of glycidyl acrylates containing glycidyl groups include glycidyl acrylate (meth)acrylate. Examples of hydroxyl-containing (meth)acrylates include: hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxybutyl methacrylate, 4-hydroxybutyl methacrylate, etc. Examples of (meth)acrylates containing substituted amino groups include N-methylaminoethyl (meth)acrylate.
[0166] Examples of non-acrylic monomers that constitute the acrylic polymer (b-1) include, for example, olefins such as ethylene and norbornene; vinyl acetate; styrene, etc.
[0167] As a polymer (b) that is at least partially cross-linked by a cross-linking agent and does not have the aforementioned energy line hardening groups, for example, a polymer formed by reacting the reactive functional groups of the aforementioned polymer (b) with a cross-linking agent. The aforementioned reactive functional groups can be appropriately selected based on the type of crosslinking agent, and there are no particular limitations. For example, when the crosslinking agent is a polyisocyanate compound, examples of the aforementioned reactive functional groups include hydroxyl, carboxyl, and amino groups. Among these reactive functional groups, hydroxyl groups, which have high reactivity with isocyanate groups, are preferred. Furthermore, when the crosslinking agent is an epoxy compound, examples of the aforementioned reactive functional groups include carboxyl, amino, and amide groups. Among these reactive functional groups, carboxyl groups, which have high reactivity with epoxy groups, are preferred. However, in terms of preventing circuit corrosion of semiconductor wafers or semiconductor chips, the aforementioned reactive functional groups are preferably groups other than carboxyl groups.
[0168] As for the polymer (b) having the aforementioned reactive functional group but not having a line-hardening group, examples include polymers obtained by polymerizing at least a monomer having the aforementioned reactive functional group. In the case of the acrylic polymer (b-1), any one or both of the acrylic monomers and non-acrylic monomers mentioned above that constitute the acrylic polymer (b-1) can be used, specifically a monomer having the aforementioned reactive functional group. As for the aforementioned polymer (b) having a hydroxyl group as a reactive functional group, examples include polymers obtained by polymerizing hydroxyl-containing (meth)acrylates. In addition, polymers obtained by polymerizing monomers having a structure in which one or more hydrogen atoms in the aforementioned acrylic monomers or non-acrylic monomers are replaced by the aforementioned reactive functional group can also be used.
[0169] In the aforementioned polymer (b) having reactive functional groups, the proportion (content) of the constituent units derived from the monomers having reactive functional groups relative to the total amount of constituent units constituting the aforementioned polymer (b) is preferably from 1% to 20% by mass, and more preferably from 2% to 10% by mass. With the aforementioned proportion within this range, the degree of crosslinking in the aforementioned polymer (b) becomes a more favorable range.
[0170] In terms of improving the film-forming properties of composition (IV), the weight average molecular weight (Mw) of the polymer (b) without energy line hardening groups is preferably 10,000 to 2,000,000, more preferably 100,000 to 1,500,000.
[0171] The polymer (b) contained in the composition (IV) and the energy line hardening first protective film forming film may be only one type or two or more types. In the case of two or more types, the combination and ratio of these polymers (b) may be arbitrarily selected.
[0172] As a composition (IV), examples include compositions containing either or both of the aforementioned polymer (a1) and compound (a2). Furthermore, when composition (IV) contains compound (a2), it is preferable that it also contains polymer (b) without a line-hardening group; in this case, it is also preferable that it contains (a1). Alternatively, composition (IV) may not contain compound (a2) and may contain both the aforementioned polymer (a1) and polymer (b) without a line-hardening group.
[0173] When composition (IV) contains the aforementioned polymer (a1), the aforementioned compound (a2), and a polymer (b) without a power line hardening group, the content of the aforementioned compound (a2) in composition (IV) relative to the total content of the aforementioned polymer (a1) and the polymer (b) without a power line hardening group is 10 parts by mass to 400 parts by mass, and more preferably 30 parts by mass to 350 parts by mass.
[0174] The total content of the aforementioned energy-curing component (a) and the polymer (b) without energy-curing groups in the energy-curing first protective film forming membrane is preferably 5% to 90% by mass, more preferably 10% to 80% by mass, and even more preferably 20% to 70% by mass, relative to the total mass of the energy-curing first protective film forming membrane. By using the aforementioned proportions within this range, the energy-curing properties of the energy-curing first protective film forming membrane are improved.
[0175] [Filling Material] By adjusting the amount of filler material in the composition (IV) and the energy line curing first protective film forming film, the effect of suppressing the energy line curing first protective film forming film residue on the upper part of the bump can be adjusted when the energy line curing first protective film forming film is attached to the aforementioned bump forming surface. Furthermore, the coefficient of thermal expansion of the cured material (e.g., the first protective film) of the energy line curing first protective film forming film can be more easily adjusted. For example, by making the coefficient of thermal expansion of the first protective film most suitable for the object to which the first protective film is formed, the reliability of the package obtained using the energy line curing first protective film forming film is further improved. Additionally, as described later, since the first protective film is formed not only on the bump forming surface of the semiconductor wafer but also on the side surface, the degree of filling can be adjusted when filling the trenches provided on the bump forming surface of the semiconductor wafer with the first protective film forming film. In addition, by using a first protective film with energy line hardening containing filler material to form a film, it is possible to reduce the moisture absorption rate of the hardened material (e.g., the first protective film) of the first protective film with energy line hardening or to improve heat dissipation.
[0176] The filler material contained in composition (IV) and the energy line curing first protective film forming film is the same as the filler material (D) contained in composition (III) and the thermosetting first protective film forming film described above.
[0177] The state in which composition (IV) and the energy line curing first protective film form containing filler material are the same as the state in which composition (III) and the thermosetting first protective film form containing filler material (D) are contained.
[0178] The filler material contained in the composition (IV) and the energy line hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these filler materials can be arbitrarily selected.
[0179] The proportion of filler material in the energy line curing first protective film relative to the total mass of the energy line curing first protective film can be, for example, 5% to 45% by mass. By using this range of proportions, when the energy line curing first protective film is attached to the aforementioned bump formation surface, the effect of suppressing the energy line curing first protective film residue on the upper part of the bump becomes more pronounced, and the aforementioned coefficient of thermal expansion can be more easily adjusted. Furthermore, as described later, since the first protective film is formed not only on the bump formation surface of the semiconductor wafer but also on the side surface, sufficient filling is possible when filling the trenches on the bump formation surface of the semiconductor wafer with the non-curing first protective film.
[0180] [additive] By adjusting the type or amount of additives in the composition (IV) and the energy line hardening first protective film forming film, when the energy line hardening first protective film forming film is attached to the aforementioned bump forming surface, the effect of suppressing the energy line hardening first protective film forming film residue on the upper part of the bump can be adjusted.
[0181] The additives contained in composition (IV) and the energy line curing first protective film forming film are the same as those contained in composition (III) and the thermosetting first protective film forming film described above. For example, in terms of making it easier to adjust the effect of inhibiting the formation of residual first protective film due to energy line hardening, rheology control agents, surfactants, silicone oils, etc., are good additives.
[0182] The state of the additives in composition (IV) and the energy-curing first protective film forming film may be the same as that of the additives (I) in composition (III) and the thermosetting first protective film forming film.
[0183] The additives contained in the composition (IV) and the energy line hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these additives can be arbitrarily selected.
[0184] The content of additives in composition (IV) and the energy line hardening first protective film forming film is not particularly limited, and can be appropriately adjusted according to the type or purpose of the aforementioned additives. For example, when the purpose is to adjust the effect of inhibiting the residual formation of the first protective film with energy line hardening, the ratio of the content of the additive in the first protective film with energy line hardening to the total mass of the first protective film with energy line hardening can be, for example, 0.5% by mass to 10% by mass.
[0185] [Other ingredients] The composition (IV) and the energy line hardening first protective film may also contain other components that do not conform to the energy line hardening component (a), the aforementioned filler material, the aforementioned additives, and the polymer (b) that does not have an energy line hardening group, to the extent that the effect of the present invention is not impaired. Other components mentioned above may include, for example, thermosetting components, photopolymerization initiators, coupling agents, and crosslinking agents. For instance, by using a composition (IV) containing the aforementioned energy-line curing component (a) and thermosetting component, the energy-line curing first protective film forming film exhibits increased adhesion to the substrate upon heating, and the strength of the cured product (e.g., the first protective film) of the energy-line curing first protective film forming film is also increased.
[0186] Examples of compounds that are the same as the thermosetting component (B), photopolymerization initiator, coupling agent and crosslinking agent in composition (III) as the aforementioned thermosetting component (B), photopolymerization initiator, coupling agent (E) and crosslinking agent (F) in composition (III).
[0187] The other components contained in the composition (IV) and the energy line hardening first protective film forming film may be only one type or two or more types. In the case of two or more types, the combination and ratio of these other components may be arbitrarily selected. The content of the aforementioned other components in composition (IV) and the energy line hardening first protective film is not particularly limited, and can be selected appropriately according to the purpose.
[0188] [solvent] Composition (IV) preferably contains a solvent. The operability of composition (IV) containing a solvent is improved. As a solvent contained in composition (IV), for example, a solvent that is the same as the solvent contained in composition (III) described above can be cited. The component (IV) may contain only one solvent or two or more solvents. In the case of two or more solvents, the combination and ratio of these solvents may be arbitrarily selected. There is no particular limitation on the amount of solvent in composition (IV), for example, it can be appropriately selected according to the types of components other than the solvent.
[0189] Regarding the improved objective effect of the present invention (high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film, as an example of a preferred energy line curing first protective film forming film, the following energy line curing first protective film forming film can be cited: containing an energy line curing component (a), a filler material, and an additive, wherein the total content of the aforementioned energy line curing component (a), the aforementioned filler material, and the aforementioned additive in the aforementioned energy line curing first protective film forming film relative to the total mass of the aforementioned energy line curing first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. In view of the above, as an example of a better energy line hardening first protective film forming film, the following energy line hardening first protective film forming film can be cited: containing an energy line hardening component (a), a polymer (b) without an energy line hardening group, a filler material, and an additive, wherein the aforementioned energy line hardening component (a) is either or both of a polymer (a1) having an energy line hardening group and a weight average molecular weight of 80,000 to 2,000,000, and a compound (a2) having an energy line hardening group and a molecular weight of 100 to 80,000, and the aforementioned polymer (b) without an energy line hardening group is selected from acrylic acid polymers. The additive is selected from one or more of the group consisting of phenoxy resin, urethane resin, polyester, rubber resin and acrylate urethane resin, and the additive is selected from one or more of the group consisting of rheology control agent, surfactant and silicone oil. The total content of the energy-line curing component (a), the polymer (b) without energy-line curing group, the filler material and the additive in the energy-line curing first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. The thickness of these energy-line hardening first protective films is preferably 2 to 7 times, more preferably 3 to 6 times, relative to the thickness of the intermediate release layer.
[0190] [Manufacturing method of composition for forming energy line hardening first protective film] The composition (IV) for forming an isoelectric line hardening first protective film is obtained by blending the components used to constitute the composition. The composition for forming the energy line curing first protective film can be manufactured using the same method as the composition for forming the thermosetting first protective film described above, except for the difference in the types of formulations.
[0191] ○ Non-hardening first protective film formation film As a non-curing first protective film forming film, examples include films containing thermoplastic resin, filler materials, and additives.
[0192] [Composition for forming a non-hardening first protective film (V)] Examples of compositions for forming a non-curing first protective film include compositions (V) containing thermoplastic resin, filler material, and additives (sometimes referred to as "composition (V)" in this specification).
[0193] [Thermoplastic resin] The aforementioned thermoplastic resins are not specifically limited. More specifically, examples of the aforementioned thermoplastic resins include resins that are the same as non-curing resins such as polyvinyl acetal, acrylic resin, urethane resin, phenoxy resin, silicone resin, and saturated polyester resin, which are included as components (III) above.
[0194] The thermoplastic resin contained in the composition (V) and the non-curing first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these thermoplastic resins can be arbitrarily selected.
[0195] The content of the aforementioned thermoplastic resin in the non-curing first protective film is preferably 25% to 75% by mass relative to the total mass of the non-curing first protective film.
[0196] [Filling Material] The non-curable first protective film forming film containing filler material has the same effect as the thermocurable first protective film forming film containing filler material (D).
[0197] As a filler material contained in composition (V) and the non-curable first protective film forming film, an example can be a filler material that is the same as that contained in composition (III) and the thermocurable first protective film forming film (D).
[0198] The filler material contained in the composition (V) and the non-hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these filler materials can be arbitrarily selected.
[0199] The content of the filler material in the non-curing first protective film forming film is preferably 15% to 70% by mass relative to the total mass of the non-curing first protective film forming film. With the aforementioned proportion in this range, similar to the case of using composition (III), when the non-curing first protective film forming film is attached to the aforementioned bump forming surface, the effect of suppressing the non-curing first protective film forming film residue on the upper part of the bump becomes higher, and it becomes easier to adjust the coefficient of thermal expansion of the non-curing first protective film forming film and the first protective film.
[0200] [additive] By adjusting the type or amount of additives in the composition (V) and the non-hardening first protective film forming film, when the non-hardening first protective film forming film is attached to the aforementioned bump forming surface, the effect of suppressing the non-hardening first protective film forming film residue on the upper part of the bump can be adjusted.
[0201] The additives contained in composition (V) and the non-curable first protective film forming film are the same as those contained in composition (III) and the thermocurable first protective film forming film described above. For example, in terms of making it easier to adjust the effect of inhibiting the formation of non-hardening first protective film residue, rheology control agents, surfactants, silicone oils, etc., are good additives.
[0202] The composition (V) and the additives in the non-curable first protective film forming film may be in the same manner as the composition (III) and the additives (I) in the thermocurable first protective film forming film.
[0203] The additives contained in the composition (V) and the non-hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these additives can be arbitrarily selected.
[0204] The content of additives in the composition (V) and the non-hardening first protective film is not particularly limited and can be appropriately adjusted according to the type or purpose of the aforementioned additives. For example, when the purpose is to adjust the effect of suppressing the residue of the non-hardening first protective film, the ratio of the content of the additive in the non-hardening first protective film to the total mass of the non-hardening first protective film can be, for example, 0.5% by mass to 10% by mass.
[0205] [Other ingredients] The composition (V) and the non-hardening first protective film may also contain other components that do not conform to any of the thermoplastic resin, filler material and additives, to the extent that the effect of the present invention is not impaired. The other ingredients mentioned above are not particularly limited and can be selected arbitrarily according to the purpose.
[0206] The other components contained in the composition (V) and the non-hardening first protective film can be only one type or two or more types. In the case of two or more types, the combination and ratio of these other components can be arbitrarily selected. The content of the aforementioned other components in the composition (V) and the non-hardening first protective film is not particularly limited, and can be appropriately selected according to the purpose.
[0207] [solvent] The composition (V) preferably contains a solvent. The operability of the composition (V) containing a solvent is improved. As a solvent contained in composition (V), for example, a solvent that is the same as the solvent contained in composition (III) described above can be cited. The component (V) may contain only one type of solvent or two or more types of solvents. In the case of two or more types of solvents, the combination and ratio of these solvents can be arbitrarily selected. There is no particular limitation on the content of solvent in composition (V), for example, it can be appropriately selected according to the types of components other than solvent.
[0208] In terms of improving the objective effects of the present invention (the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film, as a preferred example of a non-curing first protective film forming film, the following non-curing first protective film forming film can be cited: containing thermoplastic resin, filler material, and additives, and the total content of the aforementioned thermoplastic resin, the aforementioned filler material, and the aforementioned additives in the aforementioned non-curing first protective film forming film relative to the total mass of the aforementioned non-curing first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. In view of the above, as an example of a better non-curing first protective film forming film, the following non-curing first protective film forming film can be cited: containing a thermoplastic resin, a filler material, and an additive, wherein the aforementioned thermoplastic resin is one or more selected from the group consisting of polyvinyl acetal, acrylic resin, urethane resin, phenoxy resin, silicone resin, and saturated polyester resin, the aforementioned additive is one or more selected from the group consisting of rheology control agent, surfactant, and silicone oil, and the total content of the aforementioned thermoplastic resin, the aforementioned filler material, and the aforementioned additive in the aforementioned non-curing first protective film forming film relative to the total mass of the aforementioned non-curing first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. The thickness of these non-hardening first protective films is preferably 2 to 7 times, more preferably 3 to 6 times, relative to the thickness of the intermediate release layer.
[0209] [Method for manufacturing a composition for forming a non-hardening first protective film] The non-hardening first protective film forming composition (V) is obtained by blending the components used to form the composition. The composition for forming a non-curable first protective film can be manufactured using the same method as the composition for forming a thermocurable first protective film described above, except for the difference in the types of formulations.
[0210] ◎ Intermediate peeling layer Because the ratio (Gx' / GA') of the shear storage modulus of the intermediate release layer to the shear storage modulus of the buffer layer is less than 0.6, the embedding quality of the bumps in the first protective film is improved when the first protective film forming sheet is attached to the bump forming surface of the semiconductor wafer. This improves both the high-speed attachment of the first protective film forming sheet to the bump forming surface of the semiconductor wafer and the permeability of the bumps in the first protective film.
[0211] The aforementioned intermediate release layer preferably contains ethylene-vinyl acetate copolymer (EVA). By containing EVA, the embedding properties of the bumps of the first protective film are improved when the first protective film forming sheet is attached to the bump forming surface of the semiconductor wafer. This makes high-speed attachment of the first protective film forming sheet to the bump forming surface of the semiconductor wafer possible. In this specification, the characteristic that makes high-speed attachment of the first protective film forming sheet possible is sometimes referred to as "high-speed attachment capability". Furthermore, by containing EVA, the aforementioned intermediate release layer enables strong pressing of the first protective film formed by the buffer layer when the first protective film forming sheet is attached to the bump forming surface of the semiconductor wafer. This allows the top of the bump to protrude from the first protective film forming film even during high-speed attachment of the first protective film forming sheet, thereby further suppressing the residue of the first protective film forming film on the upper part of the bump. In this specification, the characteristic of suppressing the residue of the first protective film forming film on the upper part of the bump and easily allowing the top of the bump to protrude is sometimes referred to as "penetration." Because EVA has the property of softening moderately when heated, these effects, namely the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film, are particularly evident when the first protective film forming sheet is heated and applied simultaneously.
[0212] The first protective film forming sheet of this embodiment exhibits the aforementioned excellent effects by having an intermediate release layer, regardless of the type of the first protective film forming sheet.
[0213] The intermediate release layer preferably contains ethylene-vinyl acetate copolymer (EVA), but may also contain only ethylene-vinyl acetate copolymer (in other words, it may be a layer composed of ethylene-vinyl acetate copolymer), and may also contain ethylene-vinyl acetate copolymer and other components other than ethylene-vinyl acetate copolymer.
[0214] The intermediate peeling layer is in the form of sheets or films.
[0215] The intermediate peeling layer can be a single layer or multiple layers (two or more). In the case of multiple layers, these multiple layers can be the same or different from each other, and there are no particular restrictions on the combination of these multiple layers.
[0216] The thickness of the intermediate release layer is preferably 5 μm to 30 μm, more preferably 6 μm to 25 μm, and even more preferably 7 μm to 20 μm. Here, the term "thickness of the intermediate release layer" refers to the overall thickness of the intermediate release layer. For example, the thickness of an intermediate release layer composed of multiple layers refers to the total thickness of all the layers that make up the intermediate release layer.
[0217] [Composition for forming the intermediate release layer] The intermediate release layer can be formed using an intermediate release layer forming composition containing the constituent material of the intermediate release layer. For example, the intermediate release layer forming composition is applied to the surface to which the intermediate release layer is to be formed, and dried as needed, thereby forming the intermediate release layer. A more specific method for forming the intermediate release layer will be described in detail later along with methods for forming other layers. The ratio of the content of components in the intermediate release layer forming composition that do not vaporize at room temperature is generally the same as the ratio of the content of the aforementioned components in the intermediate release layer.
[0218] The composition of the aforementioned intermediate stripping layer is not limited as long as the aforementioned ratio (G x' / GA') can be adjusted to less than 0.6. In the intermediate stripping layer, the total content of one or more of the following ingredients in the intermediate stripping layer relative to the total mass of the intermediate stripping layer does not exceed 100% by mass. Similarly, in the composition for forming the intermediate release layer, the total content of one or more of the following ingredients in the composition for forming the intermediate release layer is not more than 100% by mass relative to the total mass of the composition for forming the intermediate release layer.
[0219] The composition for forming the intermediate release layer can be applied using the same method as the composition for forming the first protective film described above. There are no particular limitations on the drying conditions of the composition for forming the intermediate release layer. However, when the composition for forming the intermediate release layer contains the solvent described later, it is preferable to perform heat drying. Furthermore, the composition for forming the intermediate release layer containing the solvent is preferably heat dried at, for example, 70°C to 130°C for 10 seconds to 5 minutes.
[0220] [Composition for forming the intermediate peel layer (VII)] Examples of components for forming an intermediate release layer include: component (VII) containing ethylene-vinyl acetate copolymer (EVA) for forming an intermediate release layer (sometimes referred to as "component (VII)" in this specification). The aforementioned composition (VII) may also contain ethylene-vinyl acetate copolymer and other components besides ethylene-vinyl acetate copolymer.
[0221] In the ethylene-vinyl acetate copolymer, the ratio of the amount (parts by mass) of the constituent units derived from vinyl acetate to the total amount (parts by mass of all constituent units constituting the ethylene-vinyl acetate copolymer) ([Amount (parts by mass) of the constituent units derived from vinyl acetate constituting the ethylene-vinyl acetate copolymer] / [Total amount (parts by mass) of all constituent units constituting the ethylene-vinyl acetate copolymer] × 100) is preferably 40% by mass or less, more preferably 37% by mass or less, and even more preferably 34% by mass or less, for example, it can be any one of 30% by mass or less and 25% by mass or less. By setting the aforementioned ratio to the aforementioned upper limit value or less, the operability of the composition (VII) is further improved, the shear storage elastic modulus (G x') of the intermediate release layer can be adjusted to be smaller, the aforementioned ratio (G x' / GA') can be adjusted to be smaller, thereby improving the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film. In this specification, the ratio of the amount (parts by mass) of the constituent units derived from vinyl acetate in the ethylene-vinyl acetate copolymer to the total amount (parts by mass) of the constituent units is sometimes referred to as "VA content".
[0222] In the ethylene-vinyl acetate copolymer, the ratio (parts by mass) of the constituent units derived from vinyl acetate to the total amount (parts by mass) of the constituent units (VA content) is preferably 40% by mass or less, more preferably 37% by mass or less, and even more preferably 34% by mass or less, for example, it can be any one of 30% by mass or less and 25% by mass or less. By keeping the aforementioned ratio below the aforementioned upper limit, the operability of the composition (VII) is further improved, and it is easier to form the first protective film.
[0223] In ethylene-vinyl acetate copolymers, the ratio (parts by mass) of the constituent units derived from vinyl acetate to the total amount (parts by mass) of the constituent units (VA content) can be appropriately adjusted to a range set by any combination of the aforementioned lower limit and any of the aforementioned upper limit. For example, the aforementioned ratio is preferably 16% to 40% by mass, more preferably 17.5% to 37% by mass, and even more preferably 19% to 34% by mass, for example, it can be any of 25% to 34% by mass and 30% to 34% by mass, or any of 19% to 30% by mass and 19% to 25% by mass. However, these are just examples of the aforementioned ratios.
[0224] The weight-average molecular weight of the aforementioned ethylene-vinyl acetate copolymer is preferably 200,000 or less, more preferably 180,000 or less, and even more preferably 160,000 or less, for example, it can be any one of 100,000 or less and 60,000 or less. By having the aforementioned weight-average molecular weight below the aforementioned upper limit, the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film become higher.
[0225] There is no particular limitation on the lower limit of the weight average molecular weight of the aforementioned ethylene-vinyl acetate copolymer. For example, in terms of enabling good film-forming properties of composition (VII), the aforementioned weight average molecular weight may be 5000 or higher.
[0226] The weight-average molecular weight of the aforementioned ethylene-vinyl acetate copolymer may be, for example, any one of 5,000 to 200,000, 5,000 to 180,000, 5,000 to 160,000, 5,000 to 100,000, and 5,000 to 60,000. However, these are just examples of the aforementioned weight-average molecular weight.
[0227] Ethylene-vinyl acetate copolymer is preferably the main component of the intermediate release layer. This improves the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film. In particular, the ratio of the content of ethylene-vinyl acetate copolymer in the intermediate release layer to the total mass of the intermediate release layer ([content of ethylene-vinyl acetate copolymer in the intermediate release layer (parts by mass)] / [total mass of the intermediate release layer (parts by mass)]×100) is preferably 80% by mass or more, more preferably 90% by mass or more, for example, any one of 95% by mass or more, 97% by mass or more, and 99% by mass or more. By having the aforementioned ratio at or above the aforementioned lower limit value, the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film are further improved. The aforementioned percentage is below 100% by mass.
[0228] [Other ingredients] The other components contained in composition (VII) and the intermediate release layer are not particularly limited and may be selected appropriately according to the purpose.
[0229] The other components contained in composition (VII) and the intermediate release layer may be only one type or two or more types. In the case of two or more types, the combination and ratio of these other components may be arbitrarily selected.
[0230] Other components contained in composition (VII) and the intermediate release layer include, for example, non-polar resins such as vinyl polymers. The aforementioned ethylene-based polymer system comprises polymers having at least ethylene-derived constituent units, which may be homopolymers of ethylene or copolymers of ethylene with other monomers.
[0231] Examples of homopolymers of the aforementioned ethylene (i.e., polyethylene) include: low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), metallocene linear low-density polyethylene (mLLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE).
[0232] The aforementioned ethylene-based polymers and other non-polar resins can be oily components such as paraffin oil and solid paraffin.
[0233] Other components mentioned above that are included in composition (VII) include solvents. Composition (VII) containing solvents has excellent operability.
[0234] Examples of solvents contained in composition (VII) include: hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutanol (2-methylpropane-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds containing amide bonds) such as dimethylformamide and N-methylpyrrolidone. The component (VII) may contain only one type of solvent or two or more types of solvents. In the case of two or more types of solvents, the combination and ratio of these solvents may be arbitrarily selected.
[0235] The content of the aforementioned other components in composition (VII) and the intermediate stripping layer may be appropriately adjusted according to the types of the aforementioned other components.
[0236] When the aforementioned other components are components other than the solvent, the ratio of the content of the aforementioned other components (components other than the solvent) in the intermediate release layer to the total mass of the intermediate release layer ([content of the aforementioned other components other than the solvent in the intermediate release layer (parts by mass)] / [total mass of the intermediate release layer (parts by mass)]×100) is preferably 20% by mass or less, more preferably 10% by mass or less, for example, it can be any one of 5% by mass or less, 3% by mass or less, and 1% by mass or less. By setting the aforementioned ratio to the aforementioned upper limit value, the high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film are further improved. When the aforementioned other components are components other than solvents, the aforementioned proportion is 0% by mass or more.
[0237] When the aforementioned other components are solvents, the ratio of the content of the aforementioned other components (solvents) in composition (VII) to the total mass of composition (VII) ([content of solvent in composition (VII) (parts by mass)] / [total mass of composition (VII) (parts by mass)]×100) is preferably 5% to 50% by mass, for example, it can be any one of 5% to 35% by mass and 5% to 20% by mass. By setting the aforementioned ratio to the aforementioned lower limit or above, the operability of composition (VII) is further improved. By setting the aforementioned ratio to the aforementioned upper limit or below, the first protective film can be formed more efficiently.
[0238] [Example of a modified intermediate peel layer] Up to this point, the intermediate release layer has been described in relation to an intermediate release layer formed using a composition for forming an intermediate release layer containing ethylene-vinyl acetate copolymer (EVA). However, in this embodiment, the intermediate release layer may also be a layer formed using a composition for forming an intermediate release layer containing other resin components such as acrylic resin instead of ethylene-vinyl acetate copolymer (EVA). Examples of acrylic resins include: the acrylic resin described in the above-described composition for forming a thermosetting first protective film, and the acrylic resin (a1-1) described in the above-described composition for forming a line-curable first protective film.
[0239] Regarding the improved objective effects of the present invention (high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film), as an example of a preferred intermediate release layer, the following intermediate release layer can be cited: containing an ethylene-vinyl acetate copolymer, wherein the content of the aforementioned ethylene-vinyl acetate copolymer in the aforementioned intermediate release layer is 80% by mass or more, preferably 90% by mass or more, relative to the total mass of the aforementioned intermediate release layer; in the aforementioned ethylene-vinyl acetate copolymer, the amount of constituent units derived from vinyl acetate is 16% by mass to 40% by mass relative to the total amount of constituent units; and the weight average molecular weight of the aforementioned ethylene-vinyl acetate copolymer is 200,000 or less.
[0240] [Manufacturing method of components for forming intermediate release layer] The intermediate release layer forming composition (VII) is obtained by blending the components used to form the composition. The composition for forming the intermediate release layer, for example, can be manufactured using the same method as the composition for forming the thermosetting first protective film described above, except for the difference in the types of ingredients.
[0241] ◎ Buffer layer The aforementioned buffer layer has a buffering effect on the forces applied to the buffer layer and the layers adjacent to the buffer layer. Here, the "layers adjacent to the buffer layer" include the intermediate peeling layer, the first protective film forming film, and the first protective film.
[0242] There are no particular limitations on the material of the buffer layer, but resin is preferred.
[0243] As a preferred buffer layer, for example, a layer formed by a buffer layer forming composition containing amino carbamate (meth) acrylate can be used.
[0244] The buffer layer can be a single layer or multiple layers, including two or more. In the case of multiple layers, these layers can be the same or different from each other, and there are no particular restrictions on the combination of these multiple layers.
[0245] The thickness of the buffer layer is preferably from 150 μm to 1000 μm, more preferably from 150 μm to 800 μm, even more preferably from 200 μm to 600 μm, and especially preferably from 250 μm to 500 μm. Here, the term "thickness of the buffer layer" refers to the overall thickness of the buffer layer. For example, the thickness of a buffer layer composed of multiple layers refers to the total thickness of all the layers that make up the buffer layer.
[0246] [Components for forming a buffer layer] The buffer layer can be formed using a buffer layer forming composition containing the material used to form the buffer layer. For example, the buffer layer forming composition is applied to the surface to which the buffer layer is to be formed, and then dried as needed, thereby forming the buffer layer. When the buffer layer forming composition has energy line hardening properties as described later, it is preferable to further harden the applied buffer layer forming composition using energy lines. A more specific method for forming the buffer layer will be described in detail later along with methods for forming other layers.
[0247] In the composition for forming a buffer layer, the total content of one or more of the following ingredients in the composition for forming a buffer layer is not more than 100% by mass relative to the total mass of the composition for forming a buffer layer.
[0248] The composition for forming the buffer layer can be applied using the same method as the composition for forming the first protective film described above. There are no particular limitations on the drying conditions of the composition for forming the buffer layer; for example, they can be the same as those for the composition for forming the intermediate release layer.
[0249] When the composition for forming the energy-line hardening buffer layer is subjected to energy-line hardening, the illuminance of the energy line is preferably from 100 mW / cm² to 350 mW / cm², and the light intensity of the energy line is preferably from 200 mJ / cm² to 1400 mJ / cm². The energy-line hardening of the composition for forming the energy-line hardening buffer layer can be performed in one step or in multiple steps (via semi-hardening). When the energy-line hardening is performed in multiple steps, it is preferable that the light intensity of the energy line is from 200 mJ / cm² to 1400 mJ / cm² in all steps, and preferably that the total light intensity in all steps is from 200 mJ / cm² to 1400 mJ / cm².
[0250] [Components for forming a buffer layer (VI)] Examples of components for forming a buffer layer include a buffer layer forming component (VI) containing urethane (meth)acrylate (X) (which is sometimes simply referred to as "component (VI)" in this specification).
[0251] [Aminocarbamate (meth)acrylate (X)] The urethane (meth)acrylate (X) contained in composition (VI) is a compound having at least a (meth)acrylic group and an urethane bond, and has the property of being polymerized by energy line irradiation. That is, composition (VI) has energy line hardening properties. The number of (meth)acrylic groups in the aforementioned urethane (meth)acrylate (X) can be any one, two, or more than three (that is, urethane (meth)acrylate (X) can be monofunctional, difunctional, or trifunctional or more), but is preferably monofunctional urethane (meth)acrylate (X). Monofunctional urethane (meth)acrylate (X) does not participate in the formation of a three-dimensional network structure in the polymerization structure, and therefore it is not easy for the buffer layer to form a three-dimensional network structure. In this case, the first protective film forming sheet becomes easier to follow the bump forming surface of the semiconductor wafer.
[0252] The composition (VI) may contain only one type of carbamate (meth)acrylate (X) or two or more types. In the case of two or more types, the combination and ratio of these carbamate (meth)acrylates (X) can be arbitrarily selected.
[0253] Examples of the aforementioned urethane (meth)acrylate (X) include: a terminal isocyanate urethane prepolymer as a reactant of a polyol compound (x1) and a polyisocyanate compound (x2), and a reactant of a compound (x3) having a (meth)acrylic group. Here, "terminated isocyanate urethane prepolymer" is as explained above.
[0254] There are no particular limitations on the aforementioned polyol compound (x1) as long as it is a compound having two or more hydroxyl groups in one molecule. Examples of polyol compounds (x1) include: alkyl glycols, polyether polyols, polyester polyols, polycarbonate polyols, etc. Among these polyol compounds (x1), polyether polyols are preferred.
[0255] The polyol compound (x1) may be any of a diol with two functions, a triol with three functions, or a polyol with four or more functions. However, from the viewpoints of ease of acquisition, versatility, and reactivity, a diol with two functions is preferred, and a polyether diol is even more preferred. Examples of polyether-type diols mentioned above include polyethylene glycol, polypropylene glycol, and polybutane glycol.
[0256] The aforementioned polyester-type polyols are obtained by polycondensation reaction of polyol components and polyacid components. Examples of the aforementioned polyol components include: various alkyl diols such as ethylene glycol, diethylene glycol, and butanediol (preferably alkyl diols with 2 to 10 carbon atoms), and various diols. As for the aforementioned polybasic acid components, examples include those known as polybasic acid components of general polyesters. More specifically, examples of polybasic acid components include: aliphatic dibasic acids with 4 to 20 carbon atoms, such as adipic acid and sebacic acid; aromatic dibasic acids, such as terephthalic acid; aromatic polybasic acids, such as trimellitic acid; anhydrides of these dibasic acids or polybasic acids; derivatives of these dibasic acids or polybasic acids, dimer acids, and hydrogenated dimer acids, etc.
[0257] The aforementioned polycarbonate-type polyols are not particularly limited. Examples of such polycarbonate-type polyols include reactants of diols and alkyl carbonates.
[0258] Examples of the aforementioned polyisocyanate compounds (x2) include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, etc.
[0259] As for the aforementioned compound (x3) having a (meth)acrylic group, examples include (meth)acrylates having hydroxyl groups, and examples include compounds that are the same as the hydroxyl-containing (meth)acrylates listed above as compounds constituting acrylic resins (polymer component (A) containing components of component (III)). Among them, the aforementioned (meth)acrylate with hydroxyl groups is preferably a (meth)acrylate hydroxyalkyl ester.
[0260] The weight-average molecular weight of the aforementioned urethane (meth)acrylate (X) is preferably from 1,000 to 100,000, more preferably from 3,000 to 80,000, and even more preferably from 5,000 to 65,000. If the aforementioned weight-average molecular weight is 1,000 or higher, the polymer of the urethane (meth)acrylate (X) and the polymerizable monomer (Z) described later imparts appropriate hardness to the buffer layer.
[0261] The ratio of the content of urethane (meth)acrylate (X) in composition (VI) to the total content of components other than the solvent ([content of urethane (meth)acrylate (X) in composition (VI) (parts by mass)] / [total content of components other than the solvent in composition (VI) (parts by mass)] × 100) is preferably 10% to 70% by mass, more preferably 20% to 70% by mass, further preferably 25% to 60% by mass, and even more preferably 30% to 50% by mass. With the aforementioned ratio within this range, the effect of having a buffer layer in the first protective film forming sheet is enhanced without compromising other effects.
[0262] [Other ingredients] Composition (VI) may also contain urethane (meth)acrylate (X) and other components that do not conform to urethane (meth)acrylate (X). Other components mentioned above in composition (VI) may include, for example, compounds (Y) containing thiol groups and polymerizable monomers (Z).
[0263] The other components (VI) may contain only one or more of the aforementioned components. In the case of two or more components, the combination and ratio of these other components may be arbitrarily selected. The composition (VI) may contain only one of the thiol-containing compound (Y) and the polymerizable monomer (Z), but it is preferred to contain both the thiol-containing compound (Y) and the polymerizable monomer (Z).
[0264] [Compound containing thiol group (Y)] There are no particular limitations on the aforementioned thiol-containing compound (Y), as long as it has one or more thiol groups (-SH) in one molecule.
[0265] Examples of compounds (Y) containing a thiol group include: nonylthiol, 1-dodecylthiol, 1,2-ethanedithiol, 1,3-propanedithiol, triazine thiol, triazine dithiol, triazine trithiol, 1,2,3-propanetrithiol, tetraethylene glycol-bis(3-mercaptopropionate), trimethylolpropane tri(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetramercaptoacetate, dipentaerythritol hexa(3-mercaptopropionate), tris[(3-mercaptopropoxy)-ethyl] isocyanurate, 1,4-bis(3-mercaptobutoxy)butane, pentaerythritol tetra(3-mercaptobutyrate), 1,3,5-tris(3-mercaptobutoxyethyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, etc.
[0266] The thiol-containing compound (Y) is preferably a polyfunctional thiol-containing compound (a compound having two or more thiol groups in one molecule), and more preferably a tetrafunctional thiol-containing compound (a compound having four thiol groups in one molecule).
[0267] The composition (VI) may contain only one type of thiol-containing compound (Y) or two or more types. In the case of two or more types, the combination and ratio of these thiol-containing compounds (Y) can be arbitrarily selected.
[0268] The content of the mercaptan-containing compound (Y) in composition (VI) is preferably 1 to 4.9 parts by mass relative to the total content of urethane (meth)acrylate (X) and polymerizable monomer (Z) ([content of mercaptan-containing compound (Y) in composition (VI) (parts by mass)] / [total content of urethane (meth)acrylate (X) and polymerizable monomer (Z) in composition (VI) (parts by mass)] × 100). More preferably, it is 1.5 to 4.8 parts by mass.
[0269] [Polymerizable monomer (Z)] From the perspective of improving the film-forming properties of the buffer layer, composition (VI) preferably contains a polymerizable monomer (Z). The aforementioned polymerizable monomer (Z) is a polymerizable compound other than urethane (meth)acrylate (X), and is a compound that can be polymerized by irradiation with an energy beam. However, the polymerizable monomer (Z) does not contain a resin component. Here, "resin component" refers to an oligomer or polymer with a repeating structure, meaning a compound with a weight average molecular weight of 1000 or higher.
[0270] The aforementioned polymerizable monomer (Z) is preferably a compound having one or more (meth)acrylic groups. Examples of such polymerizable monomers (Z) include: alkyl (meth)acrylates in which the alkyl group constituting the alkyl ester is a chain structure having 1 to 18 carbon atoms; (meth)acrylates having functional groups such as hydroxyl, amide, amino, or epoxy groups; (meth)acrylates having an alicyclic structure, such as cycloalkyl (meth)acrylates; (meth)acrylates having an aromatic structure; (meth)acrylates having a heterocyclic structure; and other vinyl compounds.
[0271] As one of the aforementioned functionalized (meth)acrylates, the aforementioned (meth)acrylates containing hydroxyl groups can be exemplified by compounds that are the same as the hydroxyl-containing (meth)acrylates exemplified above as compounds constituting acrylic resins (polymer component (A) as a component of composition (III)). Examples of (meth)acrylates having an alicyclic structure include: isocamphene (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentyl (meth)acrylate, dicyclopentenoxy (meth)acrylate, cyclohexyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, etc. Examples of (meth)acrylates having an aromatic structure include: phenyl hydroxypropyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate. Examples of (meth)acrylates with heterocyclic structures include tetrahydrofurfuryl (meth)acrylate and 2-morpholinoethyl (meth)acrylate.
[0272] The composition (VI) may contain only one type of polymerizable monomer (Z) or two or more types. In the case of two or more types, the combination and ratio of these polymerizable monomers (Z) can be arbitrarily selected.
[0273] In the composition (VI), the polymerizable monomer (Z) preferably contains at least a (meth)acrylate having an alicyclic structure, more preferably a (meth)acrylate having an alicyclic structure and a (meth)acrylate having a functional group, and even more preferably isocamphene methacrylate and hydroxyalkyl methacrylate.
[0274] The ratio of the content of polymerizable monomer (Z) in composition (VI) to the total content of components other than the solvent ([content of polymerizable monomer (Z) in composition (VI) (parts by mass)] / [total content of components other than the solvent in composition (VI) (parts by mass)] × 100) is preferably 20% to 80% by mass, more preferably 30% to 80% by mass, further preferably 40% to 75% by mass, and even more preferably 50% to 70% by mass. With the aforementioned content within this range, the mobility of the portion of the buffer layer having the structure formed by the polymerization of polymerizable monomer (Z) becomes higher, thus tending to make the buffer layer more flexible, thereby making it easier for the first protective film forming sheet to follow the bump formation surface of the semiconductor wafer.
[0275] The ratio of the content of alicyclic (meth)acrylate in composition (VI) to the total content of polymerizable monomers (Z) ([content of alicyclic (meth)acrylate in composition (VI) (parts by mass)] / [total content of polymerizable monomers (Z) in composition (VI) (parts by mass)] × 100) is preferably 52% to 87% by mass, more preferably 55% to 85% by mass, and even more preferably 60% to 80% by mass. With the aforementioned content within this range, the first protective film forming sheet becomes easier to follow the bump formation surface of the semiconductor wafer.
[0276] The mass ratio of [the content (parts by mass) of urethane (meth)acrylate (X) in composition (VI)] to [the content (parts by mass) of polymerizable monomer (Z) in composition (VI)] is preferably 20 / 80 to 60 / 40, more preferably 30 / 70 to 50 / 50, and even more preferably 35 / 65 to 45 / 55. With the aforementioned mass ratio within this range, the first protective film forming sheet becomes easier to follow the bump formation surface of the semiconductor wafer.
[0277] [Photopolymerization initiator] Composition (VI) preferably further includes a photopolymerization initiator. Composition (VI) containing a photopolymerization initiator is more easily cured by irradiation with an energy beam.
[0278] Examples of photopolymerization initiators contained in composition (VI) include, for example: acetophenone, 2,2-diethoxybenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, milchnerone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, benzoin dimethyl ketal, dibenzoin, diacetyl, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-ethylanthraquinone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1- Low molecular weight polymerization initiators such as hydroxycyclohexylphenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, diethylthioxanone, isopropylthioxanone, and 2,4,6-trimethylbenzyldiphenylphosphine oxide; oligomerization polymerization initiators such as oligomeric {2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, etc.
[0279] The composition (VI) may contain only one type of photopolymerization initiator or two or more types. In the case of two or more types, the combination and ratio of these photopolymerization initiators can be arbitrarily selected.
[0280] The content of the photopolymerization initiator in composition (VI) is preferably 0.05 to 15 parts by mass relative to the total content of urethane (meth)acrylate (X) and polymerizable monomer (Z) ([content of photopolymerization initiator in composition (VI) (parts by mass)] / [total content of urethane (meth)acrylate (X) and polymerizable monomer (Z) in composition (VI) (parts by mass)] × 100). More preferably, it is 0.1 to 10 parts by mass, and even more preferably, it is 0.3 to 5 parts by mass.
[0281] [Other Additives] In composition (VI), other additives that do not conform to the components described so far may also be included, without impairing the effects of the present invention. Other additives mentioned above include: crosslinking agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc.
[0282] When composition (VI) contains the aforementioned other additives, the content of the aforementioned other additives in composition (VI) is preferably 0.01 to 6 parts by mass relative to the total content of urethane (meth)acrylate (X) and polymerizable monomer (Z) ([content of other additives in composition (VI) (parts by mass)] / [total content of urethane (meth)acrylate (X) and polymerizable monomer (Z) in composition (VI) (parts by mass)] × 100). More preferably, it is 0.1 to 3 parts by mass.
[0283] [Other resin components] In composition (VI), other resin components that do not conform to urethane (meth) acrylate (X) may also be included, to the extent that the effects of the present invention are not impaired.
[0284] [Example of a variation of a buffer layer] Up to this point, a buffer layer has been described using a buffer layer forming composition containing urethane (meth)acrylate (X). However, in this embodiment, the buffer layer may also be a layer formed using a buffer layer forming composition containing other resin components such as olefin resin instead of urethane (meth)acrylate (X).
[0285] Regarding the improved objective effects of the present invention (high-speed adhesion of the first protective film forming sheet and the permeability of the first protective film forming film), as an example of a preferred buffer layer, the following buffer layer can be cited: it is obtained by using a buffer layer forming composition (composition (VI)) containing urethane (meth)acrylate (X), a mercaptan-containing compound (Y), a polymerizable monomer (Z), a photopolymerization initiator, and a crosslinking agent, and the total content of the aforementioned urethane (meth)acrylate (X), the aforementioned mercaptan-containing compound (Y), the aforementioned polymerizable monomer (Z), the aforementioned photopolymerization initiator, and the aforementioned crosslinking agent in the aforementioned buffer layer forming composition is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. In light of the above, as an example of a better buffer layer, the following buffer layer can be cited: it is obtained using a buffer layer forming composition (composition (VI)) containing urethane (meth)acrylate (X), a thiol-containing compound (Y), a polymerizable monomer (Z), a photopolymerization initiator, and a crosslinking agent, wherein the aforementioned urethane (meth)acrylate (X) is a terminal isocyanate urethane prepolymer that is a reactant of a polyol compound (x1) and a polyisocyanate compound (x2), and a reactant of a compound having a (meth)acrylic group (x3), wherein the aforementioned thiol-containing compound... The compound (Y) is a multifunctional compound containing thiol groups having two or more thiol groups in one molecule. The aforementioned polymerizable monomer (Z) is a (meth)acrylate having an alicyclic structure and a (meth)acrylate having a functional group. The total content of the aforementioned urethane (meth)acrylate (X), the aforementioned compound containing thiol groups (Y), the aforementioned polymerizable monomer (Z), the aforementioned photopolymerization initiator, and the aforementioned crosslinking agent in the aforementioned buffer layer forming composition is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more, relative to the total content of components other than the solvent. These buffer layers are preferably obtained by heat-line hardening of the aforementioned buffer layer with the composition. The thickness of these buffer layers is preferably 10 to 70 times, and more preferably 30 to 50 times, relative to the thickness of the intermediate release layer.
[0286] [Manufacturing method of components for forming a buffer layer] The buffer layer forming composition (VI) is obtained by blending the components used to form the composition. The composition for forming the buffer layer, except for the different types of ingredients, can be manufactured using the same method as the composition for forming the thermosetting first protective film described above.
[0287] ◎ First substrate The aforementioned first substrate is in sheet or film form, and various resins can be cited as examples of the constituent materials of the aforementioned first substrate. Examples of the aforementioned resins include: polyethylene such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resins; ethylene-based copolymers such as ethylene-vinyl acetate copolymers, ethylene-(meth)acrylate copolymers, ethylene-(meth)acrylate copolymers, and ethylene-norbornene copolymers (copolymers obtained using ethylene as a monomer); and vinyl chloride-based resins such as polyvinyl chloride and vinyl chloride copolymers. (Resins obtained using vinyl chloride as a monomer); polystyrene; polycyclic olefins; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polyethylene terephthalate, polyethylene isophthalate, polyethylene 2,6-naphthalenedicarboxylate, and fully aromatic polyesters whose constituent units all have aromatic cyclic groups; copolymers of two or more of the aforementioned polyesters; poly(meth)acrylates; polyurethane; polyurethane acrylates; polyimide; polyamide; polycarbonate; fluoropolymers; polyacetal; modified polyphenylene ether; polyphenylene sulfide; polyurethane; polyetherketone, etc. Examples of the aforementioned resins include polymer alloys such as mixtures of the aforementioned polyester and resins other than the aforementioned polyester. Preferably, in polymer alloys of the aforementioned polyester and resins other than the aforementioned polyester, the amount of the resin other than the polyester is relatively small. Examples of the aforementioned resins include, for example, cross-linked resins formed by cross-linking one or more of the resins described above; and modified resins such as ionomers used in one or more of the resins described above.
[0288] The resin constituting the first substrate may be only one type or two or more types. In the case of two or more types, the combination and ratio of these resins can be arbitrarily selected.
[0289] The first substrate can be a single layer or multiple layers (two or more). In the case of multiple layers, these multiple layers can be the same or different from each other, and there are no particular restrictions on the combination of these multiple layers.
[0290] The thickness of the first substrate is preferably from 5 μm to 1000 μm, more preferably from 10 μm to 500 μm, even more preferably from 15 μm to 300 μm, and particularly preferably from 20 μm to 150 μm. Here, the term "thickness of the first substrate" refers to the overall thickness of the first substrate. For example, the thickness of a first substrate composed of multiple layers refers to the total thickness of all the layers that make up the first substrate.
[0291] The first substrate is preferably a substrate with high thickness accuracy, that is, preferably a substrate in which thickness deviation is suppressed regardless of the location. Examples of materials that can be used to form such a first substrate with high thickness accuracy include: polyethylene, polyolefins other than polyethylene, polyethylene terephthalate, ethylene-vinyl acetate copolymer, etc.
[0292] In addition to the aforementioned main constituent materials such as resin, the first substrate may also contain various known additives such as fillers, colorants, antistatic agents, antioxidants, organic lubricants, catalysts, and softeners (plasticizers).
[0293] The first substrate can be transparent or opaque, and can also be colored according to the purpose, and other layers can be vapor-deposited. When the aforementioned first protective film is an energy line hardening film, the first substrate is preferably a substrate that allows energy lines to pass through.
[0294] The first substrate can be manufactured using known methods. For example, the first substrate containing resin can be manufactured by molding a resin composition containing the aforementioned resin.
[0295] The first protective film forming sheet of this embodiment has the following characteristics. "1" A first protective film forming sheet for forming a first protective film on a bumped surface of at least a semiconductor wafer; the first protective film forming sheet is formed by sequentially depositing a first substrate, a buffer layer, an intermediate release layer, and a first protective film forming film in the thickness direction of these layers; the intermediate release layer contains an ethylene-vinyl acetate copolymer, and the content of the ethylene-vinyl acetate copolymer in the intermediate release layer is 80% by mass or more relative to the total mass of the intermediate release layer; the ratio of the shear storage modulus (Gx') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer (Gx' / GA') is less than 0.6. "2" The first protective film forming sheet as described in "1", wherein in the aforementioned ethylene-vinyl acetate copolymer, the proportion of the amount of constituent units derived from vinyl acetate to the total amount of constituent units is 16% to 40% by mass, more preferably 17.5% to 37% by mass, more preferably 19% to 34% by mass, and even more preferably 25% to 34% by mass. "3" refers to the first protective film forming sheet as described in "1" or "2", wherein the weight average molecular weight of the aforementioned ethylene-vinyl acetate copolymer is 200,000 or less, preferably 180,000 or less, more preferably 160,000 or less, and even more preferably 100,000 or less.
[0296] "4" refers to the first protective film forming sheet described in any of "1" to "3", wherein the shear storage elastic modulus (G x') of the aforementioned intermediate peeling layer is 10000 Pa or less. "5" The first protective film forming sheet as described in any one of "1" to "4", wherein the shear storage modulus (GA') of the aforementioned buffer layer is from 10,000 Pa to 400,000 Pa, more preferably from 50,000 Pa to 300,000 Pa, and even more preferably from 100,000 Pa to 200,000 Pa. "6" refers to the first protective film forming sheet described in any one of "1" to "5", wherein the aforementioned first protective film forming film is a thermosetting first protective film forming film containing a polymer component (A), a thermosetting component (B), a curing accelerator (C), a filler material (D), and an additive (I).
[0297] "7" The first protective film forming sheet as described in "6" wherein the aforementioned polymer component (A) is polyvinyl acetal, the aforementioned thermosetting component (B) is epoxy resin (B1) and thermosetting agent (B2), and the aforementioned additive (I) is one or more selected from the group consisting of rheology control agent, surfactant and silicone oil. The total content of the aforementioned polymer component (A), the aforementioned thermosetting component (B), the aforementioned curing accelerator (C), the aforementioned filler material (D) and the aforementioned additive (I) in the aforementioned thermosetting first protective film forming film is 85% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more. "8" The first protective film forming sheet as described in any one of "1" to "7", wherein the aforementioned buffer layer is a buffer layer obtained by a buffer layer forming composition containing urethane (meth)acrylate (X), a mercaptan-containing compound (Y), a polymerizable monomer (Z), a photopolymerization initiator, and a crosslinking agent, and the total content of the aforementioned urethane (meth)acrylate (X), the aforementioned mercaptan-containing compound (Y), the aforementioned polymerizable monomer (Z), the aforementioned photopolymerization initiator, and the aforementioned crosslinking agent in the aforementioned buffer layer forming composition is at least 85% by mass, preferably at least 90% by mass, and more preferably at least 95% by mass.
[0298] "9" refers to the first protective film forming sheet described in any one of "1" to "8", wherein the aforementioned buffer layer is a buffer layer obtained by using a buffer layer forming composition containing urethane (meth)acrylate (X), a thiol-containing compound (Y), a polymerizable monomer (Z), a photopolymerization initiator, and a crosslinking agent, and the aforementioned urethane (meth)acrylate (X) is a terminal isocyanate urethane prepolymer that is a reactant of a polyol compound (x1) and a polyisocyanate compound (x2), and a compound (x3) having a (meth)acrylic group, the aforementioned thiol-containing compound (Y) is a multifunctional thiol-containing compound having two or more thiol groups in one molecule, and the aforementioned polymerizable monomer (Z) is a (meth)acrylate having an alicyclic structure and a (meth)acrylate having a functional group. "10" refers to the first protective film forming sheet as described in any of "1" to "9", wherein the thickness of the first protective film forming film is 2 to 7 times, more preferably 3 to 6 times, relative to the thickness of the intermediate release layer.
[0299] ◇ Method for manufacturing the first protective film forming sheet The aforementioned first protective film forming sheet can be manufactured by sequentially stacking the above layers in a corresponding positional relationship. The method for forming each layer is as described above.
[0300] For example, the first protective film forming sheet can be manufactured by the method shown below. That is, a buffer layer forming composition (such as the aforementioned composition (VI)) is applied to one side of the first substrate and dried as needed, thereby forming a buffer layer on the first substrate. If the buffer layer forming composition has energy line hardening properties, the applied buffer layer forming composition is then subjected to energy line hardening. This yields a first laminated sheet composed of the first substrate and the buffer layer. A release film may also be provided on the exposed side of the buffer layer in the first laminated sheet (the side opposite to the first substrate side) as needed. Alternatively, an intermediate release layer forming composition (such as the aforementioned composition (VII)) is applied to the release film and dried as needed, thereby forming an intermediate release layer on the release film. In this case, the intermediate release layer forming composition is preferably applied to the release treatment surface of the release film. Alternatively, a first protective film forming composition (such as the aforementioned composition (III), composition (IV), or composition (V)) is applied to the release film and dried as needed, thereby forming a first protective film forming film on the release film. In this case, the first protective film forming composition is preferably applied to the release treatment surface of the release film.
[0301] Then, the exposed surface of the buffer layer (the side opposite to the first substrate side) and the exposed surface of the intermediate release layer (the side opposite to the release film side) in the first laminated sheet are bonded together. In this way, a second laminated sheet is obtained, which is formed by sequentially laminating the first substrate, the buffer layer, the intermediate release layer, and the release film in the thickness direction of these layers.
[0302] Next, in the second laminated sheet, the release film is removed, so that the exposed surface of the intermediate release layer (the side opposite to the buffer layer side) and the exposed surface of the first protective film forming film (the side opposite to the release film side) are bonded together. This yields a first protective film forming sheet formed by sequentially laminating the first substrate, buffer layer, intermediate release layer, first protective film forming film, and release film in the thickness direction of these layers. The release film disposed on the first protective film forming film in the first protective film forming sheet can be removed at any stage from the manufacture of the first protective film forming sheet until its use.
[0303] A first protective film forming sheet having other layers besides the aforementioned layers can be manufactured by adding either or both of the aforementioned other layer forming steps and lamination steps appropriately in the aforementioned manufacturing method, such that the lamination positions of the aforementioned other layers are in appropriate positions.
[0304] ◇ Manufacturing method of semiconductor device (method of using the first protective film forming wafer) As explained above, using the first protective film forming sheet of this embodiment, the first protective film is attached to the bump formation surface of a semiconductor wafer. Then, the first protective film is hardened as needed, thereby enabling the fabrication of a semiconductor wafer having a semiconductor wafer and a first protective film attached to the bump formation surface of the semiconductor wafer. At this time, the first protective film forming sheet of this embodiment can attach to the bump formation surface of the semiconductor wafer at high speed. Furthermore, even during this high-speed attachment of the first protective film forming sheet, the top of the bump can protrude from the first protective film, preventing the first protective film from remaining on the upper part of the bump. Then, the semiconductor wafer with the first protective film attached is diced, thereby enabling the fabrication of a semiconductor wafer having a semiconductor chip and a first protective film attached to the bump formation surface of the semiconductor chip. At this time, the residue of the first protective film formed on the top of the bumps of the semiconductor wafer with the first protective film is suppressed, and therefore the adhesion of the first protective film on the top of the bumps of the obtained semiconductor wafer with the first protective film is also suppressed. Furthermore, the semiconductor wafer with the first protective film is flip-chip bonded to a substrate using the bumps therein, thereby enabling the manufacture of a semiconductor device. At this time, the adhesion of the first protective film on the top of the bumps of the semiconductor wafer with the first protective film is suppressed, thus not hindering the electrical connection between the semiconductor wafer and the substrate. That is, the first protective film forming wafer of this embodiment is suitable for manufacturing semiconductor devices. The following describes a method for manufacturing a semiconductor device using the aforementioned first protective film forming wafer.
[0305] A method for manufacturing a semiconductor device according to one embodiment of the present invention uses the method for manufacturing a semiconductor device with a first protective film forming wafer according to one embodiment of the present invention described above. The manufacturing method includes: an attachment step, in which the first protective film forming wafer is attached to a bump-bumped surface (bump forming surface) of a semiconductor wafer, such that the top of the bump protrudes from the first protective film forming wafer, thereby setting the first protective film forming wafer on the semiconductor wafer; and a first protective film forming step, after the attachment step, in which layers other than the first protective film forming wafer are removed from the first protective film forming wafer, and then, if the first protective film forming wafer is hardenable, the first protective film forming wafer is hardened to form a first protective film. When the protective film forming film is non-curable, the first protective film forming film after removing the layers other than the first protective film forming film is regarded as the first protective film, thereby forming the first protective film on the surface with the aforementioned bumps (bump forming surface); the dicing step, after the aforementioned first protective film forming step, dicing the aforementioned semiconductor wafer, thereby fabricating a semiconductor wafer; the cutting step, after the aforementioned first protective film forming step, cutting the aforementioned first protective film; and the assembly step, the semiconductor wafer with the first protective film obtained after the aforementioned dicing step and cutting step is flip-chip connected to a substrate with the top of the aforementioned bumps, the aforementioned semiconductor wafer with the first protective film includes the aforementioned semiconductor wafer and the aforementioned first protective film disposed in the aforementioned semiconductor wafer with the aforementioned bumps, and the top of the aforementioned bumps protrudes from the aforementioned first protective film.
[0306] The manufacturing method of the semiconductor device of this embodiment, when the first protective film is hardened (sometimes referred to as "manufacturing method (1)" in this specification), includes: an attachment step, in which the first protective film forming film of the aforementioned first protective film forming sheet is attached to a bump-bumped surface (bump forming surface) of a semiconductor wafer, such that the top of the bump protrudes from the aforementioned first protective film forming film, thereby setting the aforementioned first protective film forming sheet on the aforementioned semiconductor wafer; and a first protective film forming step, in which, after the aforementioned attachment step, the layers of the aforementioned first protective film forming sheet other than the aforementioned first protective film forming film are removed from the aforementioned first protective film forming film, thereby making the aforementioned first protective film forming film... The first protective film is formed by hardening, thereby forming the first protective film on the surface having the aforementioned bumps (bump forming surface); a dicing step, after the first protective film forming step, dicing the aforementioned semiconductor wafer, thereby fabricating a semiconductor wafer; a cutting step, after the first protective film forming step, cutting the aforementioned first protective film; and a mounting step, flip-chip bonding the semiconductor wafer with the first protective film obtained after the dicing and cutting steps to a substrate with the top of the aforementioned bumps, wherein the aforementioned semiconductor wafer with the first protective film has the aforementioned semiconductor wafer and the aforementioned first protective film disposed in the aforementioned semiconductor wafer on the surface having the aforementioned bumps, and the top of the aforementioned bumps protrudes from the aforementioned first protective film.
[0307] The manufacturing method of the semiconductor device of this embodiment, when the first protective film forming film is non-curable (sometimes referred to as "manufacturing method (2)" in this specification), includes: an attachment step, in which the first protective film forming film of the aforementioned first protective film forming sheet is attached to a bump-bumped surface (bump forming surface) of a semiconductor wafer, such that the top of the bump protrudes from the aforementioned first protective film forming film, thereby setting the aforementioned first protective film forming sheet on the aforementioned semiconductor wafer; and a first protective film forming step, in which, after the aforementioned attachment step, the layers other than the aforementioned first protective film forming film in the aforementioned first protective film forming sheet are removed from the aforementioned first protective film forming film, and then the layers other than the aforementioned first protective film forming film are removed from the sheet. The first protective film formed thereafter is regarded as the first protective film, thereby forming the first protective film on the surface having the aforementioned bumps (bump forming surface); the dicing step, after the first protective film forming step, dicing the aforementioned semiconductor wafer, thereby fabricating a semiconductor wafer; the cutting step, after the first protective film forming step, cutting the aforementioned first protective film; and the assembly step, flip-chip bonding the semiconductor wafer with the first protective film obtained after the dicing step and the cutting step to a substrate with the top of the aforementioned bumps, wherein the aforementioned semiconductor wafer with the first protective film has the aforementioned semiconductor wafer and the aforementioned first protective film disposed in the aforementioned semiconductor wafer on the surface having the aforementioned bumps, and the top of the aforementioned bumps protrudes from the aforementioned first protective film.
[0308] [Manufacturing Method (1)] The manufacturing method (1) described above will be explained below. Figures 3A to 3E are cross-sectional views illustrating an example of a manufacturing method (1) when using the first protective film forming sheet 1 shown in Figure 2. Furthermore, in the figures following Figure 3A, for components that are the same as those shown in the previously described figures, the same symbols are used as in the previously described figures, and the detailed description of the components is omitted.
[0309] [Attachment Steps] In the attachment step described in manufacturing method (1), as shown in Figures 3A to 3B, the first protective film forming film 14 of the first protective film forming sheet 1 is attached to the surface (bump forming surface) 9a of the semiconductor wafer 9 with bumps 91, so that the top 9101 of the bumps 91 protrudes from the first protective film forming film 14, thereby setting the first protective film forming sheet 1 on the semiconductor wafer 9.
[0310] In the aforementioned attachment step, for example, as shown in FIG3A, the first protective film forming sheet 1 is arranged such that the first protective film forming film 14 therein faces the bump forming surface 9a of the semiconductor wafer 9.
[0311] The height of the bump 91 is not particularly limited, but is preferably 120μm to 300μm, more preferably 150μm to 270μm, and even more preferably 180μm to 240μm. By having the height of the bump 91 above the aforementioned lower limit, the function of the bump 91 can be further improved. By having the height of the bump 91 below the aforementioned upper limit, the effect of suppressing the residue of the first protective film 14 on the upper part 910 of the bump 91 becomes more effective. In this specification, the term "bump height" refers to the height of the part of the bump that is located at the highest point of the bump forming surface.
[0312] The width of the bump 91 is not particularly limited, but is preferably 170μm to 350μm, more preferably 200μm to 320μm, and even more preferably 230μm to 290μm. By having the width of the bump 91 above the aforementioned lower limit, the function of the bump 91 can be further improved. By having the width of the bump 91 below the aforementioned upper limit, the effect of suppressing the residue of the first protective film 14 on the upper part 910 of the bump 91 becomes more effective. In this specification, the term "bump width" refers to the maximum length of the line segment obtained by connecting two different points on the surface of the bump with a straight line when looking down at the bump from a direction perpendicular to the bump forming surface.
[0313] The distance between adjacent bumps 91 is not particularly limited, but is preferably 250 μm to 800 μm, more preferably 300 μm to 600 μm, and even more preferably 350 μm to 500 μm. By setting the aforementioned distance above or below the aforementioned lower limit, the function of the bumps 91 can be further improved. By setting the aforementioned distance below the aforementioned upper limit, the effect of suppressing the residue of the first protective film 14 on the upper part 910 of the bumps 91 becomes more effective. In this specification, the term "distance between adjacent bumps" means the minimum distance between the surfaces of adjacent bumps.
[0314] Subsequently, in the aforementioned attachment step, the first protective film forming film 14 is brought into contact with the bumps 91 on the semiconductor wafer 9, and the first protective film forming sheet 1 is pressed against the semiconductor wafer 9. This causes the first surface 14a of the first protective film forming film 14 to be sequentially pressed onto the surface 91a of the bumps 91 and the bump forming surface 9a of the semiconductor wafer 9. At this time, the first protective film forming film 14 is heated, thereby softening it and allowing it to expand between the bumps 91 in a manner that covers them, closely adhering to the bump forming surface 9a, and covering the surface 91a of the bumps 91, especially the surface 91a near the bump forming surface 9a, thereby embedding the base of the bumps 91. Through the above steps, as shown in Figure 3B, the first protective film forming film 14 of the first protective film forming sheet 1 is attached to the bump forming surface 9a of the semiconductor wafer 9.
[0315] As described above, as a method for pressing (in other words, attaching) the sheet 1 for forming the first protective film onto the semiconductor wafer 9, known methods for attaching various sheets to an object can be applied, such as using a roller laminating machine.
[0316] The heating temperature of the first protective film forming sheet 1 (first protective film forming film 14) when pressed (attached) to the semiconductor wafer 9 is only required to be a temperature at which the curing of the thermosetting first protective film forming film 14 is completely not carried out or is not excessively carried out, for example, it can be 80°C to 100°C. However, in terms of further improving the effect of suppressing the formation of the first protective film 14 remaining on the upper part 910 of the bump 91, the aforementioned heating temperature is preferably 85°C to 95°C.
[0317] The pressure applied when the first protective film forming sheet 1 (first protective film forming film 14) is pressed (attached) to the semiconductor wafer 9 is not particularly limited, for example, it can be from 0.1 MPa to 1.5 MPa. However, in terms of further enhancing the effect of suppressing the formation of the first protective film 14 remaining on the upper part 910 of the bump 91, the aforementioned pressure is preferably 0.3 MPa to 1 MPa.
[0318] The speed at which the first protective film forming sheet 1 (first protective film forming film 14) is attached to the semiconductor wafer 9 (attachment speed) can be, for example, 3 mm / s or more, preferably 4 mm / s or more. That is, in the aforementioned attachment step, it is preferable to attach the first protective film forming film 14 to the bump forming surface 9a of the semiconductor wafer 9 at an attachment speed of 4 mm / s or more. By attaching the first protective film forming film 14 at a high speed of 4 mm / s or more, the effect of suppressing the residue of the first protective film forming film 14 on the upper part 910 of the bump 91 is more significantly manifested. On the other hand, by attaching at a speed of 20 mm / s or less, the effect of suppressing the residue of the first protective film forming film 14 on the upper part 910 of the bump 91 is more stably manifested.
[0319] As described above, when the first protective film forming sheet 1 is pressed (attached) to the semiconductor wafer 9, the first protective film forming film 14 and the intermediate release layer 13 in the first protective film forming sheet 1 are subjected to pressure from the bump 91 by pressing in through the buffer layer 12. Initially, the first surface 14a of the first protective film forming film 14 and the first surface 13a of the intermediate release layer 13 become concave. Furthermore, in this state, a rupture occurs in the first protective film forming film 14 under pressure from the bump 91. Finally, during the stage where the first surface 14a of the first protective film forming film 14 is pressed into the bump forming surface 9a of the semiconductor wafer 9, the upper portion 910 of the bump 91, including the top tip 9101, protrudes through the first protective film forming film 14. In addition, when the intermediate release layer 13 contains an olefin-based thermoplastic resin such as EVA, in this final stage, the upper portion 910 of the bump 91 does not penetrate the intermediate release layer 13.
[0320] As shown in Figure 3B, at the end of the aforementioned bonding step, the first protective film 14 is completely or almost completely absent on the upper part 910 of the bump 91, including the top 9101. The presence of the first protective film 14 on the upper part 910 of the bump 91 is suppressed. Furthermore, in this specification, the phrase "almost no first protective film 14 remains on the upper part of the bump" means, unless otherwise specified, that a slight amount of the first protective film 14 remains on the upper part of the bump. However, the amount of the first protective film 14 remaining is such that it does not impede the electrical connection between the semiconductor wafer and the substrate when the bumped semiconductor wafer is flip-chip bonded to the substrate.
[0321] After the attachment step described in manufacturing method (1), the inner surface 9b of the semiconductor wafer 9, which is opposite to the bump forming surface 9a, is ground as needed, and a second protective film forming sheet (illustration omitted) is attached to the inner surface 9b.
[0322] [Step 1: Formation of the protective film] Following the attachment step described in manufacturing method (1), in the aforementioned first protective film formation step, firstly, as shown in FIG3C, the layers other than the first protective film forming film 14 in the first protective film forming sheet 1 are removed from the first protective film forming film 14. In this specification, this step in the first protective film formation step is sometimes referred to as the "removal step". More specifically here, the removed layers are the first substrate 11, the buffer layer 12, and the intermediate release layer 13. Thereby, a semiconductor wafer 914 with the first protective film forming film attached is obtained, which is composed of a semiconductor wafer 9 and the first protective film forming film 14 disposed on the bump forming surface 9a of the semiconductor wafer 9. The layer other than the first protective film forming film 14 can be removed from the first protective film forming film 14 using known methods.
[0323] In the first protective film forming step described in manufacturing method (1), then, as shown in FIG3D, the first protective film forming film 14 is further hardened to form the first protective film 14', thereby forming the first protective film 14' on the bump forming surface 9a. In this specification, this step in the first protective film forming step is sometimes referred to as the "hardening step". Thereby, a semiconductor wafer 914' with the first protective film attached is obtained, which is composed of a semiconductor wafer 9 and the first protective film 14' disposed on the bump forming surface 9a of the semiconductor wafer 9. The first protective film forming film 14 is curable. In this step (the aforementioned curing step), if the first protective film forming film 14 is thermocurable, it is cured by heating; if the first protective film forming film 14 is energy line curable, it is cured by irradiating an energy line. The heating conditions and energy line irradiation conditions are as described above.
[0324] [Segmentation step, cutting step] After the first protective film formation step described in manufacturing method (1), the semiconductor wafer 9 is divided in the aforementioned dicing step to fabricate a semiconductor wafer 90, and the first protective film 14' is cut in the aforementioned dicing step. Here, the cut first protective film 14' is relabeled with the symbol 140'. By performing the aforementioned slitting and cutting steps, as shown in FIG3E, a semiconductor wafer 9140' with a first protective film attached is obtained, which includes a semiconductor wafer 90 and a first protective film (sometimes referred to as "first protective film" in this specification) 140' after cutting, which is provided on the bump forming surface (the surface with bumps) 90a of the semiconductor wafer 90.
[0325] The aforementioned segmentation and cutting steps can be performed using known methods.
[0326] There is no particular limitation on the order of the aforementioned dicing and cutting steps, but it is preferable to perform the dicing and cutting steps simultaneously, or in the order of the dicing and cutting steps. When the dicing and cutting steps are performed sequentially, for example, the dicing step can be performed by a known cutting method, and then the cutting step can be performed immediately and consecutively. The cutting can be performed by setting a cutting disc (not shown) on the inner surface (or the ground inner surface) 9b of the semiconductor wafer 9. In the aforementioned cutting step, the first protective film 14' is cut along the predetermined or divided portion of the semiconductor wafer 9 (in other words, the outer periphery of the semiconductor wafer 90).
[0327] In the semiconductor wafer 9140' with the first protective film, the top tip 9101 of the bump 91 protrudes from the first protective film 140', and the first protective film is completely or almost not attached to the upper part 910 of the bump 91 including the top tip 9101, thus suppressing the attachment of the first protective film to the upper part 910 of the bump 91. Furthermore, in this specification, the phrase "almost not attached to the upper part of the bump" means, unless otherwise specified, that the first protective film is slightly attached to the upper part of the bump, but the amount of the first protective film attached is the amount to which the semiconductor wafer with the bump is flip-chip bonded to the substrate without hindering the electrical connection between the semiconductor wafer and the substrate.
[0328] [Assembly Steps] In the assembly step described in manufacturing method (1), a semiconductor wafer 9140' with the first protective film attached, whose top tip 9101 of the bump 91 obtained after the aforementioned dividing and cutting steps protrudes from the first protective film 140', is flip-chip connected to a substrate (illustration omitted) with the top tip 9101 of the bump 91. At this time, the semiconductor wafer 9140' with the first protective film is connected to the circuit formation surface of the substrate. The upper part 910 of the bump 91 in the semiconductor wafer 9140' with the first protective film is suppressed due to the attachment of the first protective film 140', so the electrical connection between the semiconductor wafer 90 and the substrate is high in this step.
[0329] When using the aforementioned second protective film forming wafer, the semiconductor wafer 9140' with the first protective film attached is picked up from the dicing die (not shown) in the second protective film forming wafer before flip-chip bonding. The semiconductor wafer 9140' with the first protective film can be picked up using known methods. When a second protective film is used to form a wafer, the semiconductor wafer 90 of the semiconductor wafer 9140' with the first protective film has a cut second protective film on its inner surface 90b (illustration omitted).
[0330] When the second protective film forming film in the second protective film forming sheet is curable, the second protective film forming film is cured at an appropriate time point according to its type, thereby becoming the second protective film. Furthermore, the second protective film is cut at an appropriate time point according to its type.
[0331] The second protective film can be hardened using the same method as the first protective film 14. It can be hardened simultaneously with the first protective film 14, or it can be hardened separately from the first protective film 14.
[0332] The second protective film can be cut using the same method as the first protective film. There is no particular limitation on the order of performing the aforementioned segmentation step and cutting the second protective film. It is preferable to perform the segmentation step and cutting the second protective film simultaneously, or to cut the second protective film after the segmentation step. When the segmentation step and cutting the second protective film are performed sequentially, for example, the segmentation step can be performed by a known cutting method, and then the cutting of the second protective film can be performed immediately and continuously. The second protective film is cut along the predetermined or divided portion of the semiconductor wafer 9 (in other words, the outer periphery of the semiconductor wafer 90).
[0333] The following describes how a semiconductor package is fabricated using a circuit board containing a semiconductor chip 90 obtained in this manner, according to a known method. By using the semiconductor package, a target semiconductor device can be manufactured (illustrations omitted).
[0334] [Manufacturing Method (2)] Next, the aforementioned manufacturing method (2) will be explained. Figures 4A to 4D are cross-sectional views illustrating an example of a manufacturing method (2) when using the first protective film forming sheet 1 shown in Figure 2.
[0335] In the attachment step described in manufacturing method (2), as shown in Figures 4A to 4B, the first protective film forming film 14 of the first protective film forming sheet 1 is attached to the surface (bump forming surface) 9a of the semiconductor wafer 9 with bumps 91, so that the top 9101 of the bumps 91 protrudes from the first protective film forming film 14, thereby setting the first protective film forming sheet 1 on the semiconductor wafer 9. The attachment step in manufacturing method (2) is the same as the attachment step described above in manufacturing method (1), except that the first protective film forming film 14 in the first protective film forming sheet 1 is non-curable instead of curable. Therefore, further detailed description of the attachment step in manufacturing method (2) is omitted.
[0336] In manufacturing method (2), the first protective film forming film 14 is attached to the bump forming surface 9a of the semiconductor wafer 9 at high speed, as shown in FIG4B. At the end of the aforementioned attachment step, the first protective film forming film 14 is completely or almost completely absent from the upper part 910 of the bump 91, including the top 9101 of the bump. The residue of the first protective film forming film 14 is suppressed in the upper part 910 of the bump 91.
[0337] After the attachment step described in manufacturing method (2), the inner surface 9b of the semiconductor wafer 9, which is opposite to the bump forming surface 9a, is ground as needed, and a second protective film forming sheet (illustration omitted) is attached to the inner surface 9b.
[0338] [Step 1: Formation of the protective film] Following the attachment step described in manufacturing method (2), in the aforementioned first protective film forming step, the layer other than the first protective film forming film 14 in the first protective film forming sheet 1 is removed from the first protective film forming film 14. In this specification, similar to the case of manufacturing method (1), this step in the first protective film forming step is sometimes referred to as the "removal step". This step (the aforementioned removal step) is the same as the aforementioned removal step in manufacturing method (1) except that the first protective film forming film 14 in the first protective film forming sheet 1 is non-curable instead of curable, and can be performed in the same manner as the removal step in manufacturing method (1). Therefore, further detailed description of the removal step in manufacturing method (2) is omitted.
[0339] In the first protective film forming step described in manufacturing method (2), the non-hardened first protective film forming film 14 after the layers other than the first protective film forming film 14 are removed is regarded as the first protective film. Thereby, as shown in FIG4C, the first protective film 14' is formed on the bump forming surface 9a. The non-hardening first protective film 14 also functions directly as a protective film in this state. Therefore, in this embodiment, the non-hardening first protective film 14 is regarded as the first protective film 14' after the intermediate peeling layer 13 is removed during use. In this way, similar to the case after the hardening step described in manufacturing method (1), a semiconductor wafer 914' with a first protective film is obtained.
[0340] In manufacturing method (2), in semiconductor wafer 9140' with first protective film attached, the top 9101 of bump 91 protrudes from the first protective film 140', and the first protective film is completely or almost not attached to the upper part 910 of bump 91 including the top 9101, and the attachment of the first protective film to the upper part 910 of bump 91 is suppressed.
[0341] [Segmentation step, cutting step] After the first protective film formation step described in manufacturing method (1), the semiconductor wafer 9 is divided in the aforementioned dicing step to produce a semiconductor wafer 90, and the first protective film 14' is cut in the aforementioned cutting step. By performing the aforementioned segmentation and cutting steps, as shown in Figure 4D, a semiconductor wafer 9140' with a first protective film is obtained.
[0342] The slitting and cutting steps of manufacturing method (2) are the same as those of manufacturing method (1) except that the first protective film 14' is not a hardened product of the first protective film forming film 14. They can be performed in the same manner as those of manufacturing method (1). Therefore, further detailed descriptions of the slitting and cutting steps of manufacturing method (2) are omitted.
[0343] [Assembly Steps] In the assembly step described earlier in manufacturing method (2), a semiconductor wafer 9140' with the first protective film attached, whose top tip 9101 of the bump 91 obtained after the aforementioned dividing and cutting steps protrudes from the first protective film 140', is flip-chip connected to a substrate (illustration omitted) with the top tip 9101 of the bump 91. At this time, the semiconductor wafer 9140' with the first protective film attached is connected to the circuit formation surface of the substrate. The upper part 910 of the bump 91 in the semiconductor wafer 9140' with the first protective film is suppressed due to the attachment of the first protective film 140', so the electrical connection between the semiconductor wafer 90 and the substrate is high in this step.
[0344] The assembly steps of manufacturing method (2) are the same as those of manufacturing method (1) except that the first protective film 140' is not a hardened form of the first protective film forming film 14. Therefore, further detailed descriptions of the assembly steps of manufacturing method (2) are omitted.
[0345] In manufacturing method (2), a semiconductor package is made using a circuit board with a semiconductor wafer 90 already mounted on it, using the same method as in manufacturing method (1). By using the semiconductor package, a target semiconductor device can be manufactured (illustrations omitted).
[0346] In either of the manufacturing methods (1) and (2), the case of using the first protective film forming sheet 1 shown in FIG2 has been described here. However, when using the first protective film forming sheet of other embodiments, the first protective film forming sheet also performs the same effect as when using the first protective film forming sheet 1.
[0347] [A variation of the semiconductor device manufacturing method (method of using the first protective film forming wafer)] In the semiconductor device manufacturing method of this embodiment, a semiconductor wafer with trenches formed on its bump forming surface can be used as the semiconductor wafer. These trenches serve as the dicing points for the semiconductor wafer when it is sliced and monolithically assembled into a semiconductor chip. By using this type of semiconductor wafer, a semiconductor chip can be manufactured that has a first protective film not only on its bump forming surface but also on its side surfaces. Here, "side surface" refers to the outer periphery of the semiconductor chip continuous with the bump forming surface; a rectangular semiconductor chip has four side surfaces. Furthermore, the first protective film is provided on the bump forming surface and the four side surfaces of the rectangular semiconductor chip. Regardless of the planar shape of the semiconductor chip, a semiconductor chip whose side surfaces are also protected can achieve a higher level of protection provided by the first protective film.
[0348] As a method for manufacturing a semiconductor device in this embodiment, for example, the following method can be used: A first protective film forming sheet according to one embodiment of the present invention is used; and the manufacturing method includes: an attachment step, using a semiconductor wafer having grooves forming on a bumped surface (bump forming surface) as the semiconductor wafer, and attaching the first protective film forming sheet to the bumped surface (bump forming surface) of the semiconductor wafer as the semiconductor wafer, and attaching the first protective film forming sheet to the bumped surface (bump forming surface) of the semiconductor wafer. The first protective film is formed by forming a surface, such that the top of the aforementioned bump protrudes from the aforementioned first protective film forming film, and filling the aforementioned first protective film forming film in the aforementioned groove, thereby setting the aforementioned first protective film forming sheet on the aforementioned semiconductor wafer; the first protective film forming step, after the aforementioned attachment step, removes the layer of the aforementioned first protective film forming sheet other than the aforementioned first protective film forming film from the aforementioned first protective film forming film, and then, if the aforementioned first protective film forming film is hardenable, hardens the aforementioned first protective film forming film to form the first protective film, thereby setting the aforementioned first protective film forming sheet on the aforementioned semiconductor wafer; When the film-forming film is non-hardening, the first protective film formed after removing the layers other than the first protective film formed is regarded as the first protective film, thereby forming the first protective film on the surface with the aforementioned bumps (bump forming surface); in the dicing step, after the first protective film forming step, the surface (inner surface) of the semiconductor wafer opposite to the surface with the aforementioned bumps (bump forming surface) is ground until the ground surface reaches the trench filled with the protective film (so that the aforementioned trench appears on the aforementioned opposite surface), and the semiconductor wafer is diced. This process involves creating a semiconductor wafer assembly by means of a first protective film filled into the trench; a cutting step, after the aforementioned dicing step, cutting the aforementioned first protective film; and a mounting step, flip-chip bonding the semiconductor wafer with the first protective film obtained after the aforementioned dicing and cutting steps to a substrate using the top of the aforementioned bumps, wherein the aforementioned semiconductor wafer with the first protective film includes the aforementioned semiconductor wafer, and the aforementioned first protective film disposed in the aforementioned semiconductor wafer with the aforementioned bumps on the surface and side surfaces, and the top of the aforementioned bumps protrudes from the aforementioned first protective film.
[0349] In a variation of the manufacturing method of the semiconductor device of this embodiment, the manufacturing method when the first protective film forming film is hardened (sometimes referred to as "manufacturing method (3)" in this specification) includes: an attachment step, using a semiconductor wafer with bumps (bump forming surface) on which trenches are formed to form the dividing portions of the aforementioned semiconductor wafer as the semiconductor wafer, attaching the aforementioned first protective film forming film from the first protective film forming sheet to the bump forming surface (bump forming surface) of the aforementioned semiconductor wafer, such that the top of the bumps protrudes from the aforementioned first protective film forming film, and the aforementioned first protective film forming film fills the aforementioned trenches, thereby setting the aforementioned first protective film forming sheet on the aforementioned semiconductor wafer; a first protective film forming step, after the aforementioned attachment step, removing the layer other than the aforementioned first protective film forming film from the aforementioned first protective film forming film in the aforementioned first protective film forming sheet, and then hardening the aforementioned first protective film forming film to form The first protective film is formed on the surface with the aforementioned bumps (bump forming surface); the dicing step, after the first protective film formation step, grinds the surface (inner surface) of the semiconductor wafer opposite to the surface with the aforementioned bumps (bump forming surface) so that the grinding surface reaches the trench filled with the aforementioned first protective film (so that the aforementioned trench appears on the aforementioned opposite surface), and dices the semiconductor wafer, thereby creating a semiconductor wafer group integrally formed by the first protective film filled in the trench; the cutting step, after the dicing step, cuts the aforementioned first protective film; and the assembly step, flip-chip connects the semiconductor wafer with the first protective film obtained after the dicing and cutting steps to a substrate with the top of the aforementioned bumps, wherein the semiconductor wafer with the first protective film has the aforementioned semiconductor wafer, and the aforementioned first protective film provided on the surface and side of the aforementioned semiconductor wafer with the aforementioned bumps, and the top of the aforementioned bumps protrudes from the aforementioned first protective film.
[0350] In a variation of the semiconductor device manufacturing method of this embodiment, the manufacturing method when the first protective film forming film is non-hardening (sometimes referred to as "manufacturing method (4)" in this specification) includes: an attachment step, using a semiconductor wafer with bumps (bump forming surface) on which trenches are formed to form the dividing portions of the aforementioned semiconductor wafer as the semiconductor wafer, attaching the aforementioned first protective film forming film of the first protective film forming sheet to the bump-faced surface (bump forming surface) of the aforementioned semiconductor wafer, such that the top of the bumps protrudes from the aforementioned first protective film forming film, and filling the aforementioned first protective film forming film in the aforementioned trenches, thereby setting the aforementioned first protective film forming sheet on the aforementioned semiconductor wafer; a first protective film forming step, after the aforementioned attachment step, removing the layers other than the aforementioned first protective film forming film from the aforementioned first protective film forming film, and removing the layers other than the aforementioned first protective film forming film from the aforementioned first protective film forming sheet. The protective film is considered as the first protective film, thereby forming the first protective film on the surface with the aforementioned bumps (bump forming surface); the dicing step, after the first protective film forming step, grinds the surface (inner surface) of the semiconductor wafer opposite to the surface with the aforementioned bumps (bump forming surface), so that the grinding surface reaches the trench filled with the aforementioned first protective film (so that the aforementioned trench appears on the aforementioned opposite surface), and dices the semiconductor wafer, thereby creating a semiconductor wafer group that is integrally formed by the first protective film filled in the trench; the cutting step, after the dicing step, cuts the aforementioned first protective film; and the assembly step, flip-chip connects the semiconductor wafer with the first protective film obtained after the dicing and cutting steps to a substrate with the top of the aforementioned bumps, the aforementioned semiconductor wafer with the first protective film having the aforementioned semiconductor wafer, and the aforementioned first protective film provided on the surface and side of the aforementioned semiconductor wafer with the aforementioned bumps, and the top of the aforementioned bumps protruding from the aforementioned first protective film.
[0351] The aforementioned modified examples (manufacturing method (3) and manufacturing method (4)) use the aforementioned attaching step on the bump forming surface to form the aforementioned trench as a semiconductor wafer. Apart from this, it can be performed in the same way as the aforementioned attaching step in the manufacturing method (manufacturing method (1) and manufacturing method (2)) using a semiconductor wafer without trench. The first protective film formation step described above in the modified examples (manufacturing method (3) and manufacturing method (4)) can be performed in the same way as the first protective film formation step described above in the manufacturing methods (manufacturing method (1) and manufacturing method (2)) using semiconductor wafers without trenches. Regarding the aforementioned dicing steps in the modified examples (manufacturing method (3) and manufacturing method (4)), the method of dicing the semiconductor wafer is limited to the specific method of grinding the inner surface of the semiconductor wafer. Apart from this, it can be performed in the same way as the aforementioned dicing steps in the manufacturing methods (manufacturing method (1) and manufacturing method (2)) using semiconductor wafers without trenches. In the aforementioned variations (manufacturing method (3) and manufacturing method (4)), the cutting step can be performed, for example, by attaching a cutting disc to the side (inner surface) of the semiconductor wafer opposite to the surface with the aforementioned bumps (bump forming surface), and then cutting the first protective film filled in the aforementioned trench along the side surface of the semiconductor wafer at a portion near the center in the width direction of the aforementioned trench. By performing this operation, the first protective film is cut between the side surfaces of adjacent semiconductor wafers, thereby obtaining a semiconductor wafer in which the first protective film is provided on these side surfaces. The cutting of the first protective film can be performed using known methods. The aforementioned mounting steps in the modified examples (manufacturing method (3) and manufacturing method (4)) can be performed in the same manner as the aforementioned mounting steps in the manufacturing methods (manufacturing method (1) and manufacturing method (2)) using semiconductor wafers without trenches.
[0352] The uses of the sheet in this embodiment are as follows. "101" is the use of a sheet for forming a first protective film on a bumped surface of at least a semiconductor wafer, and the sheet is a sheet for forming a first protective film as described in any of [1] to [5] or as described in any of "1" to "10". [Example]
[0353] The present invention will now be described in more detail with reference to specific embodiments. However, the present invention is not limited to the embodiments shown below.
[0354] [Raw materials for manufacturing the first protective film composition] The following lists the raw materials used to manufacture the components for forming the first protective film. [Polymer component (A)] (A)-1: Polyvinyl butyral ("S-LEC BL-10" manufactured by Sekisui Chemicals Co., Ltd., with a weight average molecular weight of 25,000 and a glass transition temperature of 59°C) having the constituent units represented by the following formulas (i)-1, (i)-2 and (i)-3.
[0355] [Chemistry 2] (In the formula, l1 is approximately 28, m1 is 1 to 3, and n1 is an integer from 68 to 74.)
[0356] [Epoxy Resin (B1)] (B1)-1: Liquid modified bisphenol A type epoxy resin ("Epiclon EXA-4850-150" manufactured by DIC Company, molecular weight 900, epoxy equivalent 450g / eq) (B1)-2: Dicyclopentadiene type epoxy resin ("Epiclon HP-7200HH" manufactured by DIC Company, epoxy equivalent 254g / eq to 264g / eq) [Thermosetting agent (B2)] (B2)-1: o-Cresol-type phenolic varnish resin ("Phenolite KA-1160" manufactured by DIC Company) [Hardening Accelerator (C)] (C)-1:2-Phenylon-4,5-Dihydroxymethylimidazol (Curezol 2PHZ-PW manufactured by Shikoku Chemical Industry Co., Ltd.) [Filling Material (D)] (D)-1: Epoxy-modified spherical silicon dioxide (Admanano YA050C-MKK manufactured by Admatechs, with an average particle size of 50 nm) [Additive (I)] (I)-1: Surfactant (acrylic polymer, BYK-361N manufactured by BYK Corporation) (I)-2: Silicone oil (arane-modified silicone oil, manufactured by Momentive Performance Materials Japan, "XF42-334")
[0357] [Example 1] [Manufacturing of the first protective film forming sheet] [Manufacturing of a composition for forming a thermosetting first protective film] Polymer component (A)-1 (100 parts by mass), epoxy resin (B1)-1 (290 parts by mass), epoxy resin (B1)-2 (220 parts by mass), (B2)-1 (160 parts by mass), curing accelerator (C)-1 (2 parts by mass), filler (D)-1 (200 parts by mass), additive (I)-1 (25 parts by mass), and additive (I)-2 (3 parts by mass) are dissolved or dispersed in methyl ethyl ketone and stirred at 23°C to obtain a composition (III) for forming a thermosetting first protective film, with a total concentration of all components other than the solvent of 45% by mass. Furthermore, the amounts of components other than the solvent shown here are all amounts of the target substance excluding the solvent.
[0358] [Manufacturing of the first protective film] A release film ("SP-PET381031", manufactured by Lintec Corporation, with a thickness of 38 μm) with one side treated by silicone using polyethylene terephthalate to form a release film, the aforementioned composition (III) was coated on the aforementioned release-treated side of the release film, and then heated and dried at 120°C for 2 minutes to form a first protective film with a thickness of 45 μm.
[0359] [Manufacturing of components for forming a buffer layer] Composition (VI) was prepared by blending monofunctional amino carbamate acrylate (40 parts by weight), isoborneol acrylate (45 parts by weight), 2-hydroxypropyl acrylate (15 parts by weight), pentaerythritol tetra(3-mercaptobutyrate) (Karenz MT (registered trademark) PE1 manufactured by Showa Denko Co., Ltd., a secondary 4-functional compound containing thiol groups, with a solid content concentration of 100% by weight), a crosslinking agent (1.8 parts by weight), and a photopolymerization initiator (2-hydroxy-2-methyl-1-phenyl-propane-1-one, Darocur (registered trademark) 1173 manufactured by BASF Co., Ltd., with a solid content concentration of 100% by weight).
[0360] [Formation of the buffer layer] Using a PET film (COSMOSHINE A4300, manufactured by Toyobo Co., Ltd., with a thickness of 75 μm) as the first substrate, the aforementioned composition (VI) was coated onto one side of the first substrate to form a coating film. Ultraviolet light was then irradiated onto the exposed side of the coating (opposite to the PET film side) to form a semi-cured portion of the coating film. At this time, a conveyor belt-type ultraviolet irradiation device (ECS-401GGX, manufactured by EYE GRAPHICS Co., Ltd.) was used as the ultraviolet irradiation device, and a high-pressure mercury lamp (H04-L41, manufactured by EYE GRAPHICS Co., Ltd.) was used as the ultraviolet source. Ultraviolet light with a wavelength of 365 nm was irradiated under conditions of 120 mW / cm² illuminance and 200 mJ / cm² luminous intensity. These irradiation conditions were specified using an ultraviolet cumulative illuminance meter (UVPF-A1, manufactured by EYE GRAPHICS Co., Ltd.). Subsequently, a laminate was formed by attaching the exposed surface of the aforementioned semi-cured material to the release treatment surface of the aforementioned release film ("SP-PET381031" manufactured by Lintec Corporation, with a thickness of 38 μm). Ultraviolet light was then irradiated onto this laminate from the outside of the release film side to completely cure the semi-cured material, thereby forming a buffer layer with a thickness of 400 μm. At this time, using the same ultraviolet irradiation device and ultraviolet source as described above, ultraviolet light with a wavelength of 365 nm was irradiated under conditions of illuminance of 330 mW / cm² and light intensity of 1200 mJ / cm². These irradiation conditions were specified using the same ultraviolet cumulative illuminance meter as described above. Through the above steps, a laminated sheet (equivalent to the aforementioned first laminated sheet) is obtained by sequentially stacking the first substrate, the buffer layer, and the release film in the thickness direction of these layers.
[0361] [Manufacturing of components for forming the intermediate release layer] At room temperature, ethylene-vinyl acetate copolymer (EVA, weight average molecular weight 55000, VA content 20% by mass) was dissolved in toluene to prepare a toluene solution with a solid content concentration of 12% by mass. This solution was designated as composition (VII).
[0362] [Formation of the intermediate peeling layer] The aforementioned composition (VII) was applied to the release treatment surface of the aforementioned release film ("SP-PET381031" manufactured by Lintec Corporation, with a thickness of 38 μm), and then heated and dried at 100°C for 2 minutes to form an intermediate release layer with a thickness of 10 μm.
[0363] [Manufacturing of the first protective film forming sheet] In the aforementioned laminated sheet with a buffer layer (first laminated sheet), the release film is removed, and the exposed surface of the aforementioned intermediate release layer is bonded to the exposed surface of the buffer layer thereby creating the buffer layer, thereby obtaining a laminated sheet with an intermediate release layer (equivalent to the aforementioned second laminated sheet). Subsequently, the release film is removed from the bonded intermediate release layer (in the second laminated sheet), and the exposed surface of the aforementioned first protective film forming film is bonded to the exposed surface of the intermediate release layer thereby creating the intermediate release layer. Through the above steps, a first protective film forming sheet is obtained by sequentially depositing a first substrate (75 μm thick), a buffer layer (400 μm thick), an intermediate release layer (10 μm thick), and a first protective film forming film (45 μm thick) in the thickness direction of these layers.
[0364] [Evaluation of the first protective film forming sheet] [Determination of the shear storage elastic modulus (G x') of the intermediate exfoliated layer] The exposed surface of the first protective film forming sheet (the side opposite to the intermediate release layer side) of the first protective film forming sheet obtained above is pressed onto the mirror surface of an 8-inch diameter semiconductor mirror wafer, thereby attaching the first protective film forming sheet to the mirror surface of the semiconductor mirror wafer. At this time, the attachment of the first protective film forming sheet is performed using an attachment device (roller laminator, "RAD-3510 F / 12" manufactured by Lintec Corporation) under the conditions of a table temperature of 90°C, an attachment speed of 5 mm / s, an attachment pressure of 0.5 MPa, and a roller attachment height of -400 μm, while heating the first protective film forming sheet.
[0365] Next, the first protective film is formed and left on the semiconductor mirror wafer, and the first substrate, buffer layer and intermediate release layer are peeled off to obtain the constituent body 2 formed by the stacking of the first substrate, buffer layer and intermediate release layer.
[0366] Then, the intermediate release layer of component 2 is attached to the adhesive layer of the adhesive sheet (manufactured by Lindeco Corporation, Adwill (registered trademark) D-210) formed by laminating the adhesive layer and the substrate. Next, the first substrate and the buffer layer are peeled off to form the structure 3, and the intermediate release layer, the adhesive layer and the substrate are laminated to form the structure 4.
[0367] Furthermore, the adhesive layer and substrate of the peeling component 4 are peeled off, and multiple layers of the intermediate release layer are stacked to a thickness of 400 μm. Then, the layers are cut into circles with a diameter of 25 mm to obtain a test piece of the intermediate release layer in the shape of a circular plate with a diameter of 25 mm and a thickness of 400 μm.
[0368] The test piece placement area of the shear viscosity measuring device (manufactured by Anton-Paar: MCR301) is preheated to 90°C. The test piece with the intermediate peel layer obtained above is placed on the placement area, and the measuring fixture is pressed against the upper surface of the test piece to fix the test piece in the aforementioned placement area.
[0369] Subsequently, under the conditions of 90°C and 1Hz, the shear strain generated was gradually increased from 0.01% to 10%, and the shear storage modulus (G x') [Pa] of the aforementioned intermediate peel layer specimen was measured when the shear strain was 1%.
[0370] [Determination of the shear storage modulus (GA') of the buffer layer] The buffer layer of the aforementioned component 3 was cut into a circle with a diameter of 25 mm and peeled off from the first substrate to obtain a test piece of a buffer layer in the shape of a circular plate with a diameter of 25 mm and a thickness of 400 μm.
[0371] The test piece placement area of the shear viscosity measuring device (manufactured by Anton-Paar: MCR301) is preheated to 90°C. The test piece with the buffer layer obtained above is placed on the placement area, and the measuring fixture is pressed against the upper surface of the test piece to fix the test piece in the aforementioned placement area.
[0372] Subsequently, under the conditions of 90°C and 1Hz, the shear strain generated was gradually increased from 0.01% to 1000%, and the shear storage modulus (GA') [Pa] of the aforementioned buffer layer specimen at 1% shear strain was measured.
[0373] [Calculation of the ratio (Gx' / GA') of the shear storage modulus of the intermediate stripping layer to the shear storage modulus of the buffer layer] The shear storage modulus (G x') [Pa] of the aforementioned intermediate release layer specimen is divided by the shear storage modulus (GA') [Pa] of the aforementioned buffer layer specimen, thereby obtaining the ratio (G x' / GA') of the shear storage modulus (G x') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer.
[0374] [Evaluation of the permeability of the bumps forming the first protective film (confirmation of the thickness of the first protective film attachment on the upper part of the bumps)] The exposed surface of the first protective film forming sheet (the side opposite to the intermediate release layer side) of the first protective film forming sheet obtained above is pressed against the bump forming surface of an 8-inch diameter semiconductor wafer with bumps, thereby attaching the first protective film forming sheet to the bump forming surface of the semiconductor wafer. At this time, a semiconductor wafer with a bump height of 210 μm, a bump width of 250 μm, and a bump spacing of 400 μm is used. In addition, the attachment of the first protective film forming sheet is performed using an attachment device (roller laminator, "RAD-3510 F / 12" manufactured by Lintec Corporation) under the conditions of a table temperature of 90°C, an attachment speed of 5 mm / s, an attachment pressure of 0.5 MPa, and a roller attachment height of -400 μm, while heating the first protective film forming sheet.
[0375] Then, using a grinding device (Disco's "DFG8760"), the inner surface of the semiconductor wafer was ground to make the thickness of the semiconductor wafer 250μm. Subsequently, using a multi-wafer mounter (LINDECO's "RAD-2700 F / 12"), the first substrate, buffer layer, and intermediate release layer are removed from the first protective film forming film, exposing the first protective film forming film. The first protective film forming film is then heated at 130°C for 4 hours to form the first protective film.
[0376] Next, a dicing disc (Adwill D-686H dicing tape manufactured by Lintec Corporation) is attached to the inner surface (grinding surface) of the semiconductor wafer. Using a blade dicer (DFD6362 manufactured by Disco Corporation) and dicing blades (ZH05-SD2000-N1-90CC manufactured by Disco Corporation), the blade rotation speed is set to 30,000 rpm and the blade feed speed is set to 30 mm / s. The semiconductor wafer is then divided into semiconductor wafers with a size of 6 mm × 6 mm, and the first protective film is cut into the same size. Through the above steps, a semiconductor wafer group with a first protective film is obtained. The semiconductor wafer group with a first protective film is formed by arranging and holding a plurality of semiconductor wafers with a first protective film, which have semiconductor wafers and a first protective film disposed on the bump forming surface of the aforementioned semiconductor wafers, on a dicing wafer.
[0377] In the semiconductor wafer group with the first protective film obtained above, one part in the central part and four parts in the part near the outer periphery are selected at equal intervals. At this time, the direction connecting the two parts near the outer periphery and the one part in the central part is aligned with the attachment direction of the first protective film forming sheet. One of each of these five parts is taken out, for a total of five semiconductor wafers with the first protective film.
[0378] Subsequently, using a scanning electron microscope (SEM, Keyence VE-9700), the surfaces of the bumps on these semiconductor wafers with the first protective film were observed at a 60° angle relative to the direction perpendicular to the bump formation surface of the semiconductor wafer with the first protective film, to confirm whether the first protective film was attached to the top of the bumps. Furthermore, each of these five semiconductor wafers with the first protective film contained eight bumps, meaning a total of 40 bumps were observed. The reason for observing the surfaces of the bumps on the semiconductor wafers with the first protective film at the aforementioned 60° angle is that, in this way, the first protective film remaining on the top of the bumps becomes most easily identifiable.
[0379] Subsequently, each of the five semiconductor wafers with the first protective film was sealed with epoxy resin, and the sealant was polished with a grinding wheel until a cross-section of the central portion of the bump was visible. The aforementioned cross-section was observed using a field emission scanning electron microscope (FE-SEM, Hitachi High Technologies S-4700), and the thickness of the first protective film deposit on the upper part of the bump was measured. The maximum value was taken as the thickness of the deposit. The amount (thickness) of the first protective film deposit on the upper part of the bump reflects the amount of residue in the first protective film formation on the upper part of the bump, and therefore becomes an indicator for evaluating the permeability of the bump forming the first protective film. The results are shown in Table 1.
[0380] [Manufacturing and Evaluation of the First Protective Film Forming Sheet] [Example 2] In manufacturing the composition for forming the intermediate release layer (composition (VII)), ethylene-vinyl acetate copolymer (EVA, weight average molecular weight 65,000, VA content 28% by mass) was used instead of ethylene-vinyl acetate copolymer (EVA, weight average molecular weight 55,000, VA content 20% by mass). Except in this respect, the first protective film forming sheet was manufactured using the same method as in Example 1, and the results were evaluated. The results are shown in Table 1.
[0381] [Example 3] In manufacturing the composition for forming the intermediate release layer (composition (VII)), ethylene-vinyl acetate copolymer (EVA, weight average molecular weight 150,000, VA content 32% by mass) was used instead of ethylene-vinyl acetate copolymer (EVA, weight average molecular weight 55,000, VA content 20% by mass). Except in this respect, the first protective film forming sheet was manufactured using the same method as in Example 1, and the results were evaluated. The results are shown in Table 1.
[0382] [Manufacturing and Evaluation of the First Protective Film Forming Sheet] [Example 4] [Manufacturing of components for forming the intermediate release layer] An acrylic copolymer composed of n-butyl acrylate (52 parts by mass), methyl methacrylate (20 parts by mass), and 4-hydroxybutyl acrylate (28 parts by mass) was copolymerized. Then, 2-isocyanoethyl methacrylate ("Karenz MOI (registered trademark)" manufactured by Showa Denko Co., Ltd.) was added to the acrylic copolymer at an addition rate of 90 equivalents relative to the hydroxyl groups (100 equivalents) of the constituent units derived from 4-hydroxybutyl acrylate in the aforementioned acrylic copolymer, thereby obtaining an acrylic polymer with energy line hardening properties (weight average molecular weight 750,000).
[0383] Methyl ethyl ketone was added to the acrylic polymer to prepare a liquid with a concentration of 20% by mass of the aforementioned acrylic polymer. The liquid was stirred for 30 minutes to prepare a solution composition (VII).
[0384] [Formation of the intermediate peeling layer] Using the aforementioned release film ("SP-PET381031" manufactured by Lintec Corporation, with a thickness of 38 μm), the aforementioned composition (VII) was applied to the aforementioned release treatment surface of the aforementioned release film, and then heated and dried at 100°C for 2 minutes to form an intermediate release layer with a thickness of 10 μm.
[0385] [Manufacturing of the first protective film forming sheet] Except for the use of the aforementioned intermediate release layer, a first protective film forming sheet is manufactured using the same method as in Example 1.
[0386] [Manufacturing of the first protective film forming sheet] [Comparative Example 1] [Manufacturing of adhesive composition] An acrylic copolymer was obtained by copolymerizing 2-ethylhexyl acrylate (82 parts by mass) and 2-hydroxyethyl acrylate (18 parts by mass). The addition rate of the hydroxyl groups (100 equivalents) of the constituent units of 2-hydroxyethyl acrylate in the acrylic copolymer was 66 equivalents. 2-Isoethyl methacrylate (Karenz MOI (registered trademark) manufactured by Showa Denko Co., Ltd.) was added to the acrylic copolymer to obtain an acrylic polymer (weight average molecular weight 800,000).
[0387] In addition to the acrylic polymer (100 parts by weight), 3 parts by weight of 1-hydroxycyclohexylphenyl ketone (photopolymerization initiator, "Irgacure 184" manufactured by BASF) and 1.0 parts by weight of trimethylolpropane addition toluene diisocyanate (crosslinking agent, "Coronate L" manufactured by Tosoh Corporation) were added. A liquid was prepared using methyl ethyl ketone, and the liquid was stirred for 30 minutes to prepare a solution of adhesive composition with a solid content concentration of 20% by weight.
[0388] Using the aforementioned release film ("SP-PET381031" manufactured by Lintec Corporation, with a thickness of 38 μm), the adhesive composition obtained above was applied to the aforementioned release treatment surface of the aforementioned release film, and then heated and dried at 120°C for 2 minutes to form an adhesive layer with a thickness of 10 μm.
[0389] The first protective film forming sheet is manufactured by replacing the aforementioned intermediate release layer with the adhesive layer obtained above, except in this respect, using the same method as in Example 1.
[0390] [Comparative Example 2] [Manufacturing of adhesive composition] An acrylic copolymer was obtained by copolymerizing 2-ethylhexyl acrylate (80 parts by mass) and 2-hydroxyethyl acrylate (20 parts by mass). The addition rate of the hydroxyl groups (100 equivalents) of the constituent units of the acrylic copolymer derived from 2-hydroxyethyl acrylate was 80 equivalents. 2-Isoethyl methacrylate (Karenz MOI (registered trademark) manufactured by Showa Denko Co., Ltd.) was added to the acrylic copolymer to obtain an acrylic polymer (weight average molecular weight 800,000).
[0391] In addition to the acrylic polymer (100 parts by weight), 3 parts by weight of 1-hydroxycyclohexylphenyl ketone (photopolymerization initiator, "Irgacure 184" manufactured by BASF) and 1.5 parts by weight of trimethylolpropane addition toluene diisocyanate (crosslinking agent, "Coronate L" manufactured by Tosoh Corporation) were added. A liquid was prepared using methyl ethyl ketone, and the liquid was stirred for 30 minutes to prepare an adhesive composition with a solid content of 20% by weight.
[0392] Using the aforementioned release film ("SP-PET381031" manufactured by Lintec Corporation, with a thickness of 38 μm), the adhesive composition obtained above was applied to the aforementioned release treatment surface of the aforementioned release film, and then heated and dried at 100°C for 2 minutes to form an adhesive layer with a thickness of 10 μm.
[0393] The first protective film forming sheet is manufactured by replacing the aforementioned intermediate release layer with the adhesive layer obtained above, except in this respect, using the same method as in Example 1.
[0394] [Evaluation of the first protective film forming sheet] The first protective film forming sheets of Comparative Example 1 and Comparative Example 2 obtained above were evaluated using the same method as in Example 1. The results are shown in Table 1.
[0395] [Table 1] Example Comparative example 1 2 3 4 1 2 Intermediate release layer or adhesive layer Ingredient Name EVA EVA EVA acrylic polymer acrylic polymer acrylic polymer VA content (mass%) 20 28 32 0 0 0 Weight average molecular weight 55000 65000 150000 800000 800000 800000 Thickness of the intermediate exfoliating layer [μm] 10 10 10 10 10 10 Evaluation results Shear storage elastic modulus of the intermediate exfoliated layer (G x') [Pa] 11 200 7000 45000 140000 92000 Shear storage modulus of the buffer layer (GA') [Pa] 150000 150000 150000 150000 150000 150000 G x' / GA' 0.0001 0.0013 0.0467 0.30 0.9333 0.6133 The thickness [μm] of the first protective film adhering to the upper part of the bump. 0.1 0.25 0.4 0.7 1.5 1.3
[0396] As can be clearly seen from the above results, in Examples 1 to 4, the first protective film forming sheet can be normally attached to the bump forming surface of the semiconductor wafer at an attachment speed of 5 mm / s using the first protective film forming film, demonstrating high-speed attachment capability. Furthermore, even with such high-speed attachment, the thickness of the first protective film adhering to the upper part of the bump remains below 0.7 μm (0.1 μm to 0.7 μm), suppressing the adhesion of the first protective film to the upper part of the bump. That is, in Examples 1 to 4, even when the first protective film forming sheet is attached to the bump forming surface of the semiconductor wafer at high speed, the top of the bump can still protrude from the protective film forming film, thereby suppressing the residue of the first protective film forming film on the upper part of the bump. Thus, in Examples 1 to 4, both the high-speed attachment capability of the first protective film forming sheet and the bump penetration of the first protective film forming film are high.
[0397] The first protective film forming sheets of Examples 1 to 3 include an intermediate release layer containing an ethylene-vinyl acetate copolymer. Compared to the first protective film forming sheet of Example 4 containing an acrylic polymer, the first protective film forming sheets of Examples 1 to 3 have a smaller ratio (G x' / GA'), resulting in a thinner thickness of the first protective film attachment on the upper part of the bumps. Compared to the first protective film forming sheet of Example 4 containing an acrylic polymer, the first protective film forming sheets of Examples 1 to 3 have higher permeability of the bumps. Based on the results of Examples 1 to 3, the following trend can be confirmed: as the VA content of the ethylene-vinyl acetate copolymer decreases, and as the weight average molecular weight of the ethylene-vinyl acetate copolymer decreases, the permeability of the bumps of the first protective film forming film increases.
[0398] In contrast, when the first protective film forming sheet of Comparative Example 1 or Comparative Example 2 is attached at an attachment speed of 5 mm / s using the first protective film forming film, the thickness of the first protective film adhering to the upper part of the bump is 1.5 μm or 1.3 μm, which fails to suppress the adhesion of the first protective film to the upper part of the bump. That is, in Comparative Example 1 and Comparative Example 2, when the first protective film forming sheet is attached to the bump forming surface of the semiconductor wafer at an attachment speed of 5 mm / s, the residue of the first protective film forming film on the upper part of the bump cannot be suppressed. As a result, in Comparative Example 1 and Comparative Example 2, the first protective film forming sheet lacks high-speed attachment capability, and the penetration of the bumps of the first protective film forming film is also low. The first protective film forming sheet of Comparative Examples 1 and 2 does not have an intermediate release layer containing ethylene-vinyl acetate copolymer, but has an adhesive layer containing acrylic polymer. [Industry Availability]
[0399] The present invention can be used to manufacture semiconductor wafers, etc. The aforementioned semiconductor wafers are used in flip-chip interconnection methods and have bumps, with a protective film on the bump forming surface.
[0400] 1: Sheet for forming the first protective film 9: Semiconductor wafers 9a: Bump formation surface of a semiconductor wafer (the bumped surface of a semiconductor wafer) 9b: Inner surface of a semiconductor wafer 11: First substrate 11a: One side of the first substrate 12: Buffer layer 12a: One side of the buffer layer 13: Intermediate peel layer 13a: First surface of the intermediate peeling layer 14: First protective film formation 14a: The first protective film forms the first surface of the film. 14': First protective film 15: Peel-off membrane 82: Previous protective film formation film 90: Semiconductor wafers 90a: Bump formation surface of a semiconductor wafer (the bumped surface of a semiconductor wafer) 90b: Inner surface of a semiconductor wafer 91: Bump 91a: Surface of the bump 140': First protective film after cutting 910: Upper part of the bump 914: Semiconductor wafer with first protective film forming film 914': Semiconductor wafer with first protective film 9101: Head of the bump 9140': Semiconductor wafer with first protective film
Claims
1. A first protective film forming sheet for forming a first protective film on a bumped surface of at least a semiconductor wafer; the first protective film forming sheet is formed by sequentially depositing a first substrate, a buffer layer, an intermediate release layer, and a first protective film forming film in the thickness direction of these layers; the intermediate release layer contains an ethylene-vinyl acetate copolymer; the content of the ethylene-vinyl acetate copolymer in the intermediate release layer is 80% by mass or more relative to the total mass of the intermediate release layer; the buffer layer is formed using a buffer layer forming composition containing urethane (meth)acrylate; the content of the urethane (meth)acrylate in the buffer layer forming composition is 10% by mass to 70% by mass relative to the total content of components other than the solvent; the ratio (Gx' / GA') of the shear storage modulus (Gx') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer is less than 0.
6.
2. The first protective film forming sheet as described in claim 1, wherein in the aforementioned ethylene-vinyl acetate copolymer, the amount of the constituent units derived from vinyl acetate is in the proportion of 16% to 40% by mass relative to the total amount of the constituent units.
3. The first protective film forming sheet as described in claim 1 or 2, wherein the weight average molecular weight of the aforementioned ethylene-vinyl acetate copolymer is 200,000 or less.
4. The sheet for forming the first protective film as described in claim 1 or 2, wherein the shear storage modulus (Gx') of the aforementioned intermediate release layer is 10000 Pa or less.
5. The sheet for forming the first protective film as described in claim 3, wherein the shear storage modulus (Gx') of the aforementioned intermediate release layer is 10000 Pa or less.
6. A method for manufacturing a semiconductor device, using a first protective film forming wafer as described in any one of claims 1 to 5; the aforementioned method for manufacturing the semiconductor device includes: In the attachment step, the first protective film forming sheet is attached to the bumped surface of the semiconductor wafer at an attachment speed of 4 mm / s or more, so that the top of the bump protrudes from the first protective film forming sheet, thereby setting the first protective film forming sheet on the semiconductor wafer; In the first protective film forming step, after the attachment step, the layers other than the first protective film forming film in the first protective film forming sheet are removed from the first protective film forming film. Then, if the first protective film forming film is hardened, it is hardened to form the first protective film. If the first protective film forming film is not hardened, the first protective film forming film after the removal of the layers other than the first protective film forming film is regarded as the first protective film, thereby forming the first protective film on the bumped surface; In the dicing step, after the first protective film forming step, the semiconductor wafer is diced to fabricate a semiconductor wafer. The cutting step involves cutting the first protective film after the first protective film formation step; and the assembly step involves flip-chip bonding the semiconductor wafer with the first protective film obtained after the slitting and cutting steps to a substrate with the top of the bumps. The semiconductor wafer with the first protective film includes the semiconductor wafer and the first protective film disposed on the surface of the semiconductor wafer with the bumps, and the top of the bumps protrudes from the first protective film.
7. Use of a sheet, wherein the sheet is used to form a first protective film on a bumped surface of at least a semiconductor wafer; the sheet is formed by sequentially depositing a first substrate, a buffer layer, an intermediate release layer, and a first protective film forming film in the thickness direction of these layers; the intermediate release layer contains an ethylene-vinyl acetate copolymer; the content of the ethylene-vinyl acetate copolymer in the intermediate release layer is 80% by mass or more relative to the total mass of the intermediate release layer; the buffer layer is formed using a buffer layer forming composition containing urethane (meth)acrylate; the content of the urethane (meth)acrylate in the buffer layer forming composition is 10% by mass to 70% by mass relative to the total content of components other than the solvent; and the ratio (Gx' / GA') of the shear storage modulus (Gx') of the intermediate release layer to the shear storage modulus (GA') of the buffer layer is less than 0.6.
Citation Information
Patent Citations
Polarizing plate, liquid crystal display and protective film
CN101460306A
Protection tape, and method for manufacturing semiconductor device by use thereof
JP2018098228A
Resin film, composite sheet and method for producing semiconductor chip with first protective film
TW202200373A