Substrate processing method, semiconductor device manufacturing method, program and substrate processing apparatus
Patent Information
- Application Number
- TW114102316
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-09-26
- Filing Date
- 2025-01-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-01-19
AI Technical Summary
Existing substrate processing methods for semiconductor devices do not effectively improve the properties of membranes.
A method involving the sequential supply of first and second raw materials and reactants in specified quantities and durations to form multiple layers on a substrate, utilizing a controlled gas supply system and heating mechanism to enhance membrane properties.
The method improves the properties of membranes by ensuring uniform and controlled deposition of layers, enhancing the performance and quality of semiconductor devices.
Smart Images

Figure TWG2TB001920431_001 
Figure TWG2TB001920431_002 
Figure TWG2TB001920431_003
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a program, and a substrate processing apparatus. [Previous Technology]
[0002] As a step in the manufacturing process of a semiconductor device, there is a process of forming a film on a substrate (see, for example, Patent Document 1). Prior Art Documents Patent Documents
[0003] Patent Document 1: Japanese Patent Application Publication No. 2008-124184 [Summary of the Invention]
[0004] Problem to be Solved by the Invention This invention discloses a technique that can improve the properties of membranes. Technical Means for Solving the Problem
[0005] According to one aspect of this disclosure, a technique is provided comprising: a) a step of supplying a first raw material to a substrate; b) a step of supplying a first reactant to the substrate in a first amount; c) a step of supplying a second reactant to the substrate in a second amount; d) a) and b) being performed a) and b) a predetermined number of times to form a first layer on the substrate; e) a) and c) being performed a) and c) a predetermined number of times to form a second layer on the substrate. Effects of the Invention
[0006] According to this disclosure, the properties of the membrane can be improved.
Implementation Method
[0008] <One Example of This Disclosure> The following description mainly refers to Figures 1 to 5 to illustrate one example of this disclosure. Furthermore, the figures used in the following description are all modeled objects, and the dimensional relationships and ratios of the elements shown in the figures may not be consistent with the actual objects. Moreover, the dimensional relationships and ratios of the elements may not be consistent between multiple figures.
[0009] (1) Configuration of the substrate processing apparatus The substrate processing apparatus 10 includes a processing furnace 202 equipped with a heater 207 as a heating means (heating mechanism, heating system). The heater 207 is cylindrical in shape and is supported by a heater base (not shown) as a holding plate, thereby being vertically mounted.
[0010] Inside the heater 207, an outer tube 203 constituting a processing container is arranged concentrically with the heater 207. The outer tube 203 is made of a heat-resistant material such as quartz or silicon carbide (SiC) and is formed into a cylindrical shape with a closed upper end and an open lower end. Below the outer tube 203, a manifold 209 (hereinafter referred to as MF209) is arranged concentrically with the outer tube 203. The MF209 is made of a metal such as stainless steel and is formed into a cylindrical shape with open upper and lower ends. An O-ring 220a as a sealing member is provided between the upper end of the MF209 and the outer tube 203. The MF209 is supported by the heater base, and thus the outer tube 203 is used to vertically support it.
[0011] An inner tube 204 constituting a processing container is disposed inside the outer tube 203. The inner tube 204 is made of a heat-resistant material such as quartz or SiC, and is formed into a cylindrical shape with a closed upper end and an open lower end. The processing container is mainly constituted by the outer tube 203, the inner tube 204, and MF209. A processing chamber 201 is formed in the hollow part of the processing container (inside the inner tube 204).
[0012] The processing chamber 201 is configured to accommodate multiple segments of the wafer 200, which serves as a substrate, arranged in a horizontal orientation in a vertical direction via the crystal boat 217 described later.
[0013] Inside the processing chamber 201, nozzles 410, 420, 430, and 440 are arranged to penetrate the side wall of MF209 and the inner tube 204. Gas supply pipes 310, 320, 330, and 340 are connected to each of the nozzles 410, 420, 430, and 440. However, the processing furnace 202 in this embodiment is not limited to the above-described configuration.
[0014] Flow controllers (flow control units), namely mass flow controllers (MFCs) 312, 322, 332, and 342, are sequentially provided from the upstream side of gas supply pipes 310, 320, 330, and 340. Furthermore, on / off valves, namely valves 314, 324, 334, and 344, are provided on the gas supply pipes 310, 320, 330, and 340, respectively. Downstream of valves 314, 324, 334, and 344 in the gas supply pipes 310, 320, 330, and 340, gas supply pipes 510, 520, 530, and 540 for supplying inactive gases are respectively connected. Gas supply pipes 510, 520, 530, and 540 are respectively equipped with flow controllers (flow control units) MFC512, 522, 532, and 542 and on / off valves 514, 524, 534, and 544 from the upstream side.
[0015] Nozzles 410, 420, 430, and 440 are respectively connected to the tip ends of gas supply pipes 310, 320, 330, and 340. Nozzles 410, 420, 430, and 440 are configured as L-shaped nozzles, with their horizontal portions penetrating the side wall of MF209 and the inner tube 204. The vertical portions of nozzles 410, 420, 430, and 440 protrude outward in the radial direction of the inner tube 204 and are disposed inside a groove-shaped preparation chamber 201a that extends vertically, and are disposed upward along the inner wall of the inner tube 204 (above the arrangement direction of the wafer 200) within the preparation chamber 201a.
[0016] Nozzles 410, 420, 430, and 440 are configured to extend from the lower region of the processing chamber 201 to the upper region of the processing chamber 201, and each has a plurality of gas supply holes 410a, 420a, 430a, and 440a at a position facing the wafer 200. Herein, processing gas is supplied to the wafer 200 from the gas supply holes 410a, 420a, 430a, and 440a of the nozzles 410, 420, 430, and 440. A plurality of these gas supply holes 410a, 420a, 430a, and 440a are provided from the lower part of the inner tube 204 across the upper part, each having the same opening area and the same opening pitch. However, the gas supply holes 410a, 420a, 430a, and 440a are not limited to the above-described configuration. For example, the opening area can be gradually increased from the lower part to the upper part of the inner tube 204. In this way, the flow rate of gas supplied from the gas supply holes 410a, 420a, 430a, and 440a can be made more uniform.
[0017] Gas supply holes 410a, 420a, 430a, and 440a of nozzles 410, 420, 430, and 440 are provided at a height from the lower part to the upper part of the crystal boat 217 (described later). Therefore, the processing gas supplied to the processing chamber 201 from the gas supply holes 410a, 420a, 430a, and 440 of nozzles 410, 420, 430a, and 440a will supply the entire area of the wafer 200 housed in the crystal boat 217 from the lower part to the upper part. Nozzles 410, 420, 430, and 440 can be provided to extend from the lower region to the upper region of the processing chamber 201, but it is preferable to extend them to the vicinity of the top plate of the crystal boat 217.
[0018] A gas containing the first element is supplied to the processing chamber 201 through the gas supply pipe 310 via MFC 312, valve 314, and nozzle 410 as the first raw material (first processing gas).
[0019] A gas containing the second element is supplied to the processing chamber 201 through the gas supply pipe 320 via MFC 322, valve 324, and nozzle 420 as the second raw material (second processing gas).
[0020] The first reactant (the third processing gas) is supplied to the processing chamber 201 through the gas supply pipe 330 via MFC 332, valve 334, and nozzle 430.
[0021] The second reactant (the fourth processing gas) is supplied to the processing chamber 201 through the gas supply pipe 340 via MFC 342, valve 344, and nozzle 440.
[0022] Nitrogen (N2) gas, as an inactive gas, is supplied to the processing chamber 201 from gas supply pipes 510, 520, 530, and 540 through MFCs 512, 522, 532, and 542, valves 514, 524, 534, and 544, and nozzles 410, 420, 430, and 440, respectively. Hereinafter, an example of using N2 gas as an inactive gas will be described; however, in addition to N2 gas, rare gases such as Ar, He, Ne, and Xe gas can also be used as inactive gases.
[0023] The processing gas supply system is mainly composed of gas supply pipes 310, 320, 330, 340, MFCs 312, 322, 332, 342, valves 314, 324, 334, 344, and nozzles 410, 420, 430, 440. However, the nozzles 410, 420, 430, 440 can also be considered as the processing gas supply system. The processing gas supply system can also be simply referred to as the gas supply system. When the first raw material flows through the gas supply pipe 310, the first raw material supply system (also called the first supply system or first supply section) is mainly composed of the gas supply pipe 310, MFC 312, and valve 314. However, the nozzles 410 can also be considered as included in the first raw material supply system. Furthermore, when the second raw material flows through the gas supply pipe 320, the second raw material supply system (also referred to as the second supply system) is mainly constituted by the gas supply pipe 320, MFC 322, and valve 324. However, the nozzle 420 can also be considered as included in the second raw material supply system. When the first reactant flows through the gas supply pipe 330, the first reactant supply system (also referred to as the third supply system or second supply section) is mainly constituted by the gas supply pipe 330, MFC 332, and valve 334. However, the nozzle 430 can also be considered as included in the first reactant supply system. When the second reactant flows through the gas supply pipe 340, the second reactant supply system (also referred to as the fourth supply system or third supply section) is mainly constituted by the gas supply pipe 340, MFC 342, and valve 344. However, the nozzle 440 can also be considered as included in the second reactant supply system. In addition, the inactive gas supply system is mainly constituted by gas supply pipes 510, 520, 530, 540, MFC 512, 522, 532, 542 and valves 514, 524, 534, 544.
[0024] The gas supply method in this sample is to supply gas via nozzles 410, 420, 430, and 440, which are disposed within a preparation chamber 201a in an annular longitudinal space defined by the inner wall of the inner tube 204 and the ends of a plurality of wafers 200. Furthermore, gas is ejected into the inner tube 204 from a plurality of gas supply holes 410a, 420a, 430a, and 440 of the nozzles 410, 420, 430, and 440 located opposite the wafers.
[0025] The exhaust port (exhaust outlet) 204a is an opening formed on the side wall of the inner tube 204 and facing the nozzles 410, 420, 430, 440. The shape of the opening is, for example, a slit shape. Gas supplied from the gas supply holes 410a, 420a, 430a, 440a of the nozzles 410, 420, 430, 440 to the processing chamber 201 and flowing over the surface of the wafer 200 flows through the exhaust port 204a into the exhaust path 206 formed by the gap between the inner tube 204 and the outer tube 203. Then, the gas flowing into the exhaust path 206 flows into the exhaust pipe 231 and is discharged out of the processing furnace 202.
[0026] The vent 204a is disposed facing the plurality of wafers 200. Gas supplied from gas supply holes 410a, 420a, 430a, and 440a to the vicinity of the wafers 200 in the processing chamber 201 flows horizontally and then flows into the vent passage 206 through the vent 204a. The vent 204a is not limited to being configured as a slit-shaped through hole, but can also be configured as a plurality of holes.
[0027] An exhaust pipe 231 is provided in MF209 for venting the environment inside the processing chamber 201. From upstream, a pressure sensor 245 (a pressure detector, or pressure detection unit) is sequentially connected to the exhaust pipe 231, along with an APC (Auto Pressure Controller) valve 243 and a pump 246 (an exhaust device). The APC valve 243 opens and closes when the pump 246 is actuated, thereby enabling the venting and cessation of venting of the environment inside the processing chamber 201. Furthermore, by adjusting the valve opening while the pump 246 is actuated, the pressure inside the processing chamber 201 can be adjusted. The exhaust system is mainly composed of the exhaust port 204a, exhaust path 206, exhaust pipe 231, APC valve 243, and pressure sensor 245. The pump 246 can also be considered as being included within the exhaust system.
[0028] Below MF209, a sealing cap 219 (hereinafter referred to as SC219) serving as a furnace opening cover is provided, which can airtightly seal the lower opening of MF209. SC219 is configured to abut against the lower end of MF209 from the lower side in the vertical direction. SC219 is made of metal such as SUS and is formed in a disc shape. An O-ring 220b serving as a sealing member, abutting against the lower end of MF209, is provided on the upper side of SC219. On the side of SC219 opposite to the processing chamber 201, a rotation mechanism 267 is provided to rotate the crystal boat 217 containing the wafer 200. The rotation shaft 255 of the rotation mechanism 267 passes through SC219 and is connected to the crystal boat 217. The rotation mechanism 267 is configured to rotate the wafer 200 by rotating the crystal boat 217. SC219 is configured to move vertically upwards and downwards via a crystal boat lift 115 (hereinafter referred to as BE115), which is vertically mounted outside the outer tube 203 and serves as a lifting mechanism. BE115 is configured to move the crystal boat 217 in and out of the processing chamber 201 by raising and lowering SC219. BE115 is configured as a transport device (transport system) for transporting the crystal boat 217 and the wafers 200 contained within the crystal boat 217 in and out of the processing chamber 201.
[0029] The crystal boat 217, which serves as a substrate support, is configured to arrange multiple wafers 200, for example 10 to 200, at vertical intervals in a horizontal orientation. The crystal boat 217 is made of a heat-resistant material such as quartz or SiC. A heat-insulating cylinder 218, made of a heat-resistant material such as quartz or SiC, is provided at the lower part of the crystal boat 217. By this configuration, heat from the heater 207 is less likely to be transferred to the SC219 side. However, this configuration is not limited to the above configuration. For example, the heat-insulating cylinder 218 may not be provided at the lower part of the crystal boat 217, and instead, a heat-insulating plate made of a heat-resistant material such as quartz or SiC may be horizontally supported in multiple sections at the lower part of the crystal boat 217.
[0030] As shown in Figure 2, a temperature sensor 263, which serves as a temperature detector, is installed inside the inner tube 204. The power supply to the heater 207 is adjusted based on the temperature information detected by the temperature sensor 263, thereby achieving the desired temperature distribution within the processing chamber 201. The temperature sensor 263, like the nozzles 410, 420, 430, and 440, is configured in an L-shape and installed along the inner wall of the inner tube 204.
[0031] As shown in Figure 3, the control unit (control means), i.e., the controller 121, is configured as a computer equipped with a CPU (Central Processing Unit) 121a, RAM (Random Access Memory) 121b, a memory device 121c, and an I / O port 121d. The RAM 121b, memory device 121c, and I / O port 121d are configured to exchange data with the CPU 121a through an internal bus. An input / output device 122, configured as a touch panel, is connected to the controller 121.
[0032] The memory device 121c is constructed, for example, by flash memory, HDD (Hard Disk Drive). Within the memory device 121c, a control program for controlling the operation of the board processing device, or a process recipe describing the procedures or conditions of the semiconductor device manufacturing method described later, is readablely stored. The process recipe is a program that is combined to cause the controller 121 to execute each process (step) in the semiconductor device manufacturing method described later, so as to obtain a specified result, and its function is recorded on a computer-readable recording medium. Hereinafter, the process recipe, control program, etc., are collectively referred to as a program. When the term "program" is used in this specification, it may include only a single processing recipe, only a single control program, or a combination of a processing recipe and a control program. RAM 121b constitutes a memory area for temporarily storing programs or data read by the CPU 121a.
[0033] I / O port 121d is connected to the above-mentioned MFC312, 322, 332, 342, 512, 522, 532, 542, valves 314, 324, 334, 344, 514, 524, 534, 544, pressure sensor 245, APC valve 243, pump 246, heater 207, temperature sensor 263, rotating mechanism 267, BE115, etc.
[0034] CPU 121a is configured to read the control program from memory device 121c and execute it, and to read the recipe from memory device 121c according to the input of operation instructions from input / output device 122. CPU121a is configured to control, according to the read recipe, various gas flow adjustment actions performed by MFC312, 322, 332, 342, 512, 522, 532, and 542; opening and closing actions of valves 314, 324, 334, 344, 514, 524, 534, and 544; opening and closing actions of APC valve 243; pressure adjustment actions performed by APC valve 243 based on pressure sensor 245; temperature adjustment actions of heater 207 based on temperature sensor 263; starting and stopping pump 246; rotation and rotation speed adjustment actions of crystal boat 217 performed by rotating mechanism 267; lifting and lowering actions of crystal boat 217 performed by BE115; and receiving actions of wafer 200 into crystal boat 217.
[0035] The controller 121 is configured to install the aforementioned program stored in an external memory device (such as a magnetic disk like a hard drive, an optical disc like a CD or DVD, or a semiconductor memory like flash memory) 123 onto a computer. The memory device 121c or the external memory device 123 is configured as a computer-readable recording medium containing the program. Hereinafter, they are collectively referred to as recording media. The recording media in this specification may include only the memory device 121c, only the external memory device 123, or both. The provision of the computer program (program product) may also be carried out using communication means such as the Internet or dedicated lines, without using the external memory device 123.
[0036] (2) Substrate processing step (substrate processing method) As a process in the manufacturing of semiconductor devices (components), an example of the process of forming a film on a wafer 200 will be described using FIG4. This process is performed using the processing furnace 202 of the substrate processing apparatus 10 described above. In the following description, the operation of each part constituting the substrate processing apparatus 10 is controlled by the controller 121.
[0037] The substrate processing step (component manufacturing step) according to this embodiment includes: a) a step of supplying a first raw material to the wafer 200; b) a step of supplying a first reactant to the wafer 200 in a first amount; c) a step of supplying a second reactant to the wafer 200 in a second amount; d) a step of forming a first layer on the wafer 200 by performing a) and b) a predetermined number of times; e) a step of forming a second layer on the wafer 200 by performing a) and c) a predetermined number of times.
[0038] In this specification, when the term "wafer" is used, it is intended to refer to "the wafer itself" or "a laminate of a wafer and a specified layer or film formed on its surface." When the term "surface of a wafer" is used in this specification, it is intended to refer to "the surface of the wafer itself" or "the surface of a specified layer or film formed on the wafer." When the term "substrate" is used in this specification, it is synonymous with the use of the term "wafer."
[0039] (Wafer loading) Once a plurality of wafers 200 are placed in a crystal boat 217, as shown in FIG1, the crystal boat 217 supporting the plurality of wafers 200 is lifted by BE115 and loaded into the processing chamber 201 of the processing container, and is housed in the processing container.
[0040] (Pressure and Temperature Adjustment) The space within the processing chamber 201, i.e., where the wafer 200 is located, is vented by pump 246 to achieve the desired pressure. At this time, the pressure within the processing chamber 201 is measured by pressure sensor 245, and the APC valve 243 is controlled by feedback based on this measured pressure information (pressure adjustment). Pump 246 remains continuously operational at least until the processing of the wafer 200 is completed. Furthermore, the processing chamber 201 is heated by heater 207 to achieve the desired temperature. At this time, the current supplied to heater 207 is controlled by feedback based on temperature information detected by temperature sensor 263 to achieve the desired temperature distribution within the processing chamber 201 (temperature adjustment). Heating of the processing chamber 201 by heater 207 continues at least until the processing of the wafer 200 is completed. During the film formation process on the wafer 200, the temperature of the wafer 200 is controlled to be maintained between 150 and 400°C. Furthermore, the notation of numerical ranges such as "150~400℃" in this specification means that the lower and upper limits are included within the range. Therefore, for example, "150~400℃" means "above 150℃ and below 400℃". The same applies to other numerical ranges.
[0041] (Membrane Formation Process) Next, the membrane formation process is performed. In the membrane formation process, as shown in Figure 4, the first, second, and third processes are performed. Note that the third process, indicated by the dashed line, may or may not be performed.
[0042] (First Process) The first process includes a process of forming a layer containing a first element and a process of forming a layer containing a second element.
[0043] (Including the formation process of the first element layer) (First raw material supply process) Open valve 314 to allow the first raw material to flow into gas supply pipe 310. The first raw material, whose flow rate is adjusted by MFC 312, is supplied from gas supply hole 410a of nozzle 410 into processing chamber 201 and is exhausted from exhaust pipe 231.
[0044] At this time, adjust the supply rate of the first raw material by adjusting APC valve 243 or MFC312. Example processing conditions for the supply of the first raw material: First raw material supply flow rate (excluding dilution gas): 0.1~10 g / min, more preferably 0.5~5 g / min; Inactive gas (dilution gas) supply flow rate: 100~100000 sccm, more preferably 1000~50000 sccm; First raw material supply time: 10~600 seconds, more preferably 30~300 seconds; Inactive gas supply flow rate (per gas supply tube): 0~50000 sccm, more preferably 5000~15000 sccm.
[0045] At this time, the first material is supplied to the wafer 200. By supplying the first material to the wafer 200, the material containing the first element will be adsorbed onto the substrate film on the surface of the wafer 200.
[0046] As the first raw material, a gas containing the following molecules can be used, wherein the molecule has a first element and a ligand bonded to the first element. Examples of the first element include metallic elements, preferably transition metal elements, and more preferably group 4 elements such as zirconium (Zr), hafnium (Hf), and titanium (Ti). Furthermore, examples of the ligand bonded to the first element include organic ligands, preferably alkyl groups such as methyl, ethyl, propyl, and butyl, amino groups (at least NH-), alkylamino groups, and hydrocarbon groups including at least one selected from the group consisting of cyclopentadienyl, cyclohexadienyl, and cycloheptadienyl. Even more preferably, it comprises the first element, an amino group, and other groups.
[0047] As a first raw material containing Zr as the first element, a gas containing at least one of the following can be used: tetraethylmethylaminozirconium (Zr[N(CH3)C2H5]4), tetradiethylaminozirconium (Zr[N(C2H5)2]4), tetradimethylaminozirconium (Zr[N(CH3)2]4), Zr(MMP)4, Zr(O-tBu)4, and tridimethylaminocyclopentadienezirconium ((C5H5)Zr[N(CH3)2]3). One or more of these can be used as the first raw material.
[0048] Furthermore, as a first raw material containing Hf as the first element, a gas containing at least one of the following can be used: tetraethylmethylaminohafnium (Hf[N(CH3)C2H5]4), tetradiethylaminohafnium (Hf[N(C2H5)2]4), tetradimethylaminohafnium (Hf[N(CH3)2]4), Hf(O-tBu)4, Hf(MMP)4, and tridimethylaminocyclopentadienehafnium ((C5H5)Hf[N(CH3)2]3). One or more of these can be used as the first raw material.
[0049] Furthermore, as a first raw material containing Ti as the first element, a gas containing at least one of the following can be used: tetraethylmethylaminotitanium (Ti[N(CH3)C2H5]4), tetradiethylaminotitanium (Ti[N(C2H5)2]4), tetradimethylaminotitanium (Ti[N(CH3)2]4), Ti(O-tBu)4, Ti(MMP)4, and tridimethylaminocyclopentadienetitanium ((C5H5)Ti[N(CH3)2]3). One or more of these can be used as the first raw material.
[0050] (Inactive Gas Supply (Purge) Process) After a predetermined time has elapsed since the start of the supply of the first raw material, valve 314 is closed to stop the supply of the first raw material. At this time, valves 514, 524, 534, and 544 are opened to allow inactive gas to circulate (purge) through gas supply pipes 510, 520, 530, and 540. That is, inactive gas is supplied to the processing chamber 201.
[0051] At this time, adjust the APC valve 243 to set the pressure of the processing chamber 201 to a range of, for example, 1 to 3990 Pa. The supply flow rate of the inactive gas controlled by MFCs 512, 522, 532, and 542 is set to a range of, for example, 0.1 to 30 slm.
[0052] (Vacuuming (Purge) Process) After a predetermined time has elapsed since the start of the inactive gas supply, valves 514, 524, 534, and 544 are closed to stop the supply of inactive gas. At this time, the APC valve 243 of the exhaust pipe 231 is opened, and the vacuum in the processing chamber 201 is vented by pump 246. Therefore, residual gas is removed from the wafer 200, and residual gas or reaction byproducts in the processing chamber 201 are removed from the processing chamber 201. In this way, residual gas can be removed from the wafer 200, thereby reducing the amount of the first raw material or decomposition products remaining in the processing chamber 201. The vacuum venting time in the processing chamber 201 is set to, for example, within the range of 0.1 to 30 seconds.
[0053] In addition, the purification process includes at least one of the following: a process for supplying inactive gas and a process for venting gas.
[0054] (First reactant supply process) Next, valve 334 is opened to allow the first reactant to flow into the gas supply pipe 330. The first reactant is regulated by MFC 332 and supplied from the gas supply port 430a of nozzle 430 into the processing chamber 201, and is exhausted from the exhaust pipe 231.
[0055] At this time, adjust APC valve 243 and MFC 332 to adjust the supply rate of the first reactant to the first quantity. As for the processing conditions during the supply of the first reactant, the example first reactant supply flow rate is: 100~100000 sccm, more preferably 1000~10000 sccm. Alternatively, it can be set to 0.1~10 g / min, more preferably 0.2~5 g / min. Supply time: 10~600 seconds, more preferably 30~300 seconds. Inactive gas supply flow rate (per gas supply tube): 0~50000 sccm, more preferably 5000~15000 sccm.
[0056] At this time, a first reactant is supplied to wafer 200. Here, an oxidant (oxidizing gas) can be used as the first reactant, for example. As an oxidant, an oxygen-containing (O) gas and a gas containing O and hydrogen (H) can be used, for example. As a gas containing O and H, water vapor (H2O gas), hydrogen peroxide (H2O2) gas, hydrogen (H2) gas + oxygen (O2) gas, H2 gas + ozone (O3) gas, etc. can be used, for example. As a gas containing O, O2 gas, O3 gas, etc. can be used. One or more of these can be used as the oxidant. In addition, the description of "H2 gas + O2 gas" as two gases in this disclosure means a mixture of H2 gas and O2 gas. When supplying a mixed gas, the system can be designed to mix the two gases in the supply pipe (premix) before supplying them to the processing chamber 201, or it can be designed to supply the two gases separately to the processing chamber 201 through different supply pipes, and then mix them in the processing chamber 201 (postmix). O3 can be generated from O2 gas, for example, using an ozone generator. Therefore, the nozzle from the ozone generator will release gas containing O2 and O3. The O3 generated in this way is supplied to the processing container and wafer 200. Specifically, the oxidant supply nozzle provides O2 gas + O3 gas. In addition, other nozzles can provide inert gases, and the supply of inert gases prevents O3 gas from entering the nozzle. When neither oxidant nor inert gas is supplied, the oxidant supply nozzle and other nozzles supply O3, O2, and inert gases to the processing container and wafer 200. Furthermore, the term "agent" as used in this disclosure includes at least one of gaseous and liquid substances. Liquid substances include mist substances. That is, film-forming agents, modifiers, and etchants may include gaseous substances, liquid substances such as mist substances, or both.
[0057] (Inactive Gas Supply Process) After a predetermined time has elapsed since the start of the supply of the first reactant, valve 334 is closed to stop the supply of the first reactant. At this time, valves 514, 524, 534, and 544 are opened to allow inactive gas to flow into gas supply pipes 510, 520, 530, and 540. That is, inactive gas is supplied to the processing chamber 201.
[0058] At this time, adjust APC valve 243 to set the pressure of processing chamber 201 to a range of, for example, 1 to 3990 Pa. The supply flow rate of the inactive gas controlled by MFCs 512, 522, 532, and 542 is set to a flow rate in a range of, for example, 0.1 to 30 slm. The time for supplying the inactive gas to wafer 200 is set to a time in a range of, for example, 0.1 to 30 seconds.
[0059] At this time, an inactive gas is supplied to the processing chamber 201. This reduces the amount of unreacted or first reactants or reaction byproducts remaining in the processing chamber 201 after membrane formation.
[0060] (Exhaust Process) After a predetermined time has elapsed since the start of the inactive gas supply, valves 514, 524, 534, and 544 are closed to stop the supply of inactive gas. At this time, the APC valve 243 of the exhaust pipe 231 is opened, and the processing chamber 201 is vented by pump 246. This removes residual gas from the wafer 200, and unreacted substances, first reactants, or reaction byproducts remaining in the processing chamber 201 are eliminated from the processing chamber 201. The venting time in the processing chamber 201 is set to, for example, within the range of 0.1 to 30 seconds.
[0061] (Specified number of times 1) The first raw material supply process to the exhaust process described above are performed sequentially a specified number of times (A times, where A is an integer of 1 or 2 or more), thereby forming a first layer containing the first element of a specified thickness on the wafer 200.
[0062] (Forming process of the second element layer) (Second raw material supply process) Open valve 324 to allow the second raw material to flow into gas supply pipe 320. The second raw material, whose flow rate is adjusted by MFC 322, is supplied from gas supply hole 420a of nozzle 420 into processing chamber 201 and is exhausted from exhaust pipe 231.
[0063] At this time, adjust the supply rate of the second raw material by adjusting APC valve 243 or MFC322. Example processing conditions for the supply of the second raw material: Second raw material supply flow rate (excluding dilution gas): 0.1~10 g / min, more preferably 0.5~5 g / min; Inactive gas (dilution gas) supply flow rate: 100~100000 sccm, more preferably 1000~50000 sccm; Second raw material supply time: 10~600 seconds, more preferably 30~300 seconds; Inactive gas supply flow rate (per gas supply tube): 0~50000 sccm, more preferably 5000~15000 sccm.
[0064] At this time, a second material is supplied to wafer 200. By supplying the second material to wafer 200, the material containing the second element will be adsorbed onto the substrate film on the surface of wafer 200.
[0065] As the second raw material, a gas containing molecules having a second element and a ligand bonded to the second element can be used. The second element and the first element can be the same or different elements. It is preferable that they are different elements. The specific material of the second raw material can be the material described as the first raw material above.
[0066] (Inactive Gas Supply Process) After a predetermined time has elapsed since the start of the supply of the second raw material, valve 324 is closed to stop the supply of the second raw material. At this time, valves 514, 524, 534, and 544 are opened to allow inactive gas to flow through gas supply pipes 510, 520, 530, and 540 (to be purged). That is, inactive gas is supplied to the processing chamber 201.
[0067] At this time, adjust APC valve 243 to set the pressure of processing chamber 201 to a range of, for example, 1 to 3990 Pa. The supply flow rate of inactive gas controlled by MFC512, 522, 532, and 542 is set to a range of, for example, 0.1 to 30 slm.
[0068] (Exhaust Process) After a predetermined time has elapsed since the start of the supply of inactive gas, valves 514, 524, 534, and 544 are closed to stop the supply of inactive gas. At this time, the APC valve 243 of the exhaust pipe 231 is opened, and the vacuum exhaust from the processing chamber 201 is performed by pump 246. Therefore, residual gas is removed from the wafer 200, and residual gas or reaction byproducts in the processing chamber 201 are removed from the processing chamber 201. In this way, residual gas can be removed from the wafer 200, thereby reducing the amount of the second raw material or decomposition products remaining in the processing chamber 201. The vacuum exhaust time in the processing chamber 201 is set to, for example, within the range of 0.1 to 30 seconds.
[0069] (First Reactant Supply Step) Next, the first reactant supply step is performed as described above. The supply conditions for the first reactant in the formation step containing the second element layer can also be set in the same way as the supply conditions for the first reactant in the formation step containing the first element layer.
[0070] (Inactive gas supply process) After a predetermined time has elapsed since the start of the supply of the first reactant, the inactive gas supply process is carried out as described above.
[0071] (Exhaust process) After a specified time has elapsed since the start of the supply of inactive gas, the exhaust process shall be carried out as described above.
[0072] (Specified number of times 2) The above-mentioned second raw material supply process to exhaust process are performed sequentially a specified number of times (B times, where B is an integer of 1 or 2 or more) to form a first layer containing the second element of a specified thickness on the wafer 200.
[0073] (Specified number of times 3) The above-described process for forming a layer containing the first element (formation of the first layer containing the first element) and the process for forming a layer containing the second element (formation of the first layer containing the second element) are sequentially performed a specified number of times (C times, where C is an integer of 1 or 2 or more), thereby depositing the first layer containing the first element and the first layer containing the second element on the wafer 200. This layered structure is referred to as the first layer. The first layer is a layer that can be crystallized by the modification process described later.
[0074] (Second Processing) Next, the second processing is performed. As shown in Figure 4, the second processing is the same as the first processing, except that the first reactant supply step is replaced by the second reactant supply step. The following describes in detail the reactant supply step (second reactant supply step) that is different from the first processing, while detailed descriptions of the same steps are omitted.
[0075] (Forming process containing the first element layer) The forming process containing the first element layer in the second process is performed by replacing the supply process of the first reactant in the forming process containing the first element layer in the first process with the supply process of the second reactant.
[0076] (Purge process) Perform at least one of the following procedures: supplying inactive gas and venting gas, as described above.
[0077] (Second reactant supply process) Open valve 344 to allow the second reactant to flow into gas supply pipe 340. The second reactant is adjusted by MFC 342 and supplied from gas supply port 440a of nozzle 440 into processing chamber 201, and is exhausted from exhaust pipe 231.
[0078] At this time, adjust APC valve 243 and MFC 342 to adjust the supply rate of the second reactant to the second quantity. As for the processing conditions during the supply of the second reactant, the example supply flow rate is 100~100000 sccm, more preferably 1000~10000 sccm. Alternatively, it can be set to 0.01~10 g / min, more preferably 0.1~2 g / min. Supply time: 10~600 seconds, more preferably 30~300 seconds. Inactive gas supply flow rate (per gas supply tube): 0~50000 sccm, more preferably 5000~15000 sccm.
[0079] Furthermore, the oxidizing power of the second reactant is preferably set to be different from that of the first reactant. That is, the supply conditions (supply amount, gas type) of the second reactant are preferably set such that the oxidizing power of the second reactant is smaller (weaker) than that of the first reactant.
[0080] For example, when the materials (gas types) of the first reactant and the second reactant are the same, the supply amount is set such that the supply amount of the second reactant (i.e., the second quantity) is different from the supply amount of the first reactant (i.e., the first quantity). Specifically, for example, the supply amount is set such that the supply amount of the second reactant (i.e., the second quantity) is less than the supply amount of the first reactant (i.e., the first quantity). Here, the supply amount is adjusted by controlling at least one of the supply flow rate and the supply time. Specifically, the supply flow rate of the second reactant is set to be smaller than the supply flow rate of the first reactant. In addition, the supply time of the second reactant is set to be shorter than the supply time of the first reactant. Alternatively, the partial pressure of the second reactant can also be set to be smaller than the partial pressure of the first reactant.
[0081] The oxidizing power can also be adjusted by making the materials of the first reactant and the second reactant different. For example, compared with the oxidant disclosed herein, the oxidizing power of a gas containing O3, H2O2, or the gas disclosed herein activated is relatively stronger than that of other gases disclosed herein. For example, by using at least one of the gases activated by O3, H2O2, or H2+O2 as the first reactant, and using at least one of O2, H2O, or H2+O2 as the second reactant, the oxidizing power of the second reactant can be set to be weaker than that of the first reactant.
[0082] Alternatively, adjustments to oxidizing power can be made by combining adjustments to the combination of materials with adjustments to the supply conditions.
[0083] (Purge process) At least one of the following procedures is performed: an inactive gas supply process and an exhaust process, as described above.
[0084] (Specified number of times 1) The process containing the above-mentioned second reactant supply process is performed sequentially a specified number of times (D times, where D is an integer of 1 or 2 or more) to form a second layer containing the first element of a specified thickness on the wafer 200.
[0085] (Forming process containing the second element layer) The forming process containing the second element layer in the second process is performed by replacing the supply process of the first reactant in the forming process containing the second element layer in the first process with the supply process of the second reactant described above.
[0086] (Specified number of times 2) The process containing the above-mentioned second reactant supply process is performed sequentially a specified number of times (E times, where E is an integer of 1 or 2 or more) to form a second layer containing the second element of a specified thickness on the wafer 200.
[0087] (Specified number of times 3) The formation process containing the first element layer (formation of the second layer containing the first element) and the formation process containing the second element layer (formation of the second layer containing the second element) in the second process are sequentially performed a specified number of times (F times, where F is an integer of 1 or 2 or more), thereby depositing the second layer containing the first element and the second layer containing the second element on the wafer 200. This layered structure is referred to as the second layer. Here, the second layer is formed by using the second reactant, thereby containing less oxygen than the first layer. The second layer is an amorphous layer that can be formed by the modification process described later.
[0088] (Third Processing) The third processing can then be performed. The process and conditions of the third processing are set to be different from those of the second processing. In addition, the process and conditions of the third processing can be the same as those of the first processing, or they can be appropriately made different.
[0089] In this manner, the process of forming the first and second layers of film on the wafer 200 is carried out.
[0090] As a preferred embodiment disclosed herein, a gas containing Hf can be used as the first raw material, for example. A gas containing Zr can be used as the second raw material, for example. By forming an oxide film containing Hf and Zr in this way, a ferroelectric material film with extremely high capacitance can be formed.
[0091] An oxide film containing Hf and Zr is formed by the first and second layers respectively. However, as mentioned above, due to the relationship between the oxidizing power of the first reactant and the oxidizing power of the second reactant, the second layer contains less oxygen than the first layer. Furthermore, the ratio of the first element to the second element in the first layer is close to that in the second layer. In other words, the ratio of the first element to the second element is approximately the same in both the first and second layers. Therefore, the second layer can also be called an oxygen-deficient layer relative to the first layer. Moreover, the second layer can also be called an even more oxygen-deficient layer than the first layer. Conversely, the first layer can also be called an oxygen-rich layer relative to the second layer. Furthermore, since the first layer has a composition close to stoichiometry, the second layer can also be called an oxygen-deficient layer in terms of stoichiometry.
[0092] Furthermore, the first process (third process) described above can be represented by the following sequence (A). Furthermore, the second process can be represented by the following sequence (B). The first process (third process) can also be modified as shown in (C) and (D) below. Furthermore, the second process can also be modified as shown in (E) and (F) below. Additionally, the following description omits the process of rinsing. Furthermore, the sequence can also be constructed by omitting the process of rinsing. (A) [(First raw material supply → First reactant supply) × A → (Second raw material supply → First reactant supply) × B] × C (B) [(First raw material supply → Second reactant supply) × D → (Second raw material supply → Second reactant supply) × E] × F (C) (First raw material supply → First reactant supply → Second raw material supply) × C (D) (First raw material supply → Second reactant supply → First reactant supply) × C (E) (First raw material supply → Second reactant supply → Second raw material supply) × F (F) (First raw material supply → Second reactant supply → Second raw material supply) × F
[0093] (Purge and Atmospheric Pressure Restoration) Inactive gas is supplied into processing chamber 201 from gas supply pipes 510-540, and exhaust is performed from exhaust pipe 231. The inactive gas acts as a purging gas, thereby purging processing chamber 201 and removing any residual gas or reaction byproducts from processing chamber 201. Subsequently, the environment within processing chamber 201 is replaced with inactive gas, and the pressure within processing chamber 201 is restored to atmospheric pressure.
[0094] (Wafer Removal) Subsequently, SC219 is lowered via BE115, and the lower end of the outer tube 203 is opened. Then, the processed wafer 200, supported by the wafer boat 217, is removed from the lower end of the outer tube 203 to the outside of the outer tube 203. Subsequently, the processed wafer 200 is removed from the wafer boat 217.
[0095] (Modification Processing) As shown in Figure 5, the wafer 200 on which the first and second layers are formed can also undergo modification processing. Modification processing can also be performed in the same substrate processing apparatus 10, following the first, second, and (third) processing described above. Furthermore, after the wafer is removed, the wafer 200 can be transferred to a substrate processing apparatus 10 different from the one that performed the first, second, and (third) processing, and the modification process can be performed thereon.
[0096] In the modification process, for example, heat treatment of the wafer 200 or plasma treatment can be performed. When the film formed on the wafer 200 is a dielectric (especially a ferroelectric material), heat treatment (annealing) can be performed. Heat treatment involves heating the wafer 200 to a temperature higher than that of the film formation process. For example, the wafer 200 can be heated to 350°C to 800°C for heat treatment. Through the modification process, the first layer is crystallized, and the second layer is modified to contain an amorphous layer.
[0097] (3) Effects according to the present state sample According to the present state sample, one or more of the following effects can be obtained. (a) By setting the amount of oxygen contained in the second layer to be less than the amount of oxygen contained in the first layer, the first layer can be crystallized and the second layer can be made into a layer containing amorphous material when performing a modification treatment (e.g., heat treatment). (b) When the dielectric layer is crystallized, the permittivity of the dielectric can be increased. In particular, in ferroelectric materials, the properties of ferroelectric materials can be exhibited. On the other hand, there is a problem that leakage current may increase due to the grain boundaries of crystallization. In this disclosure, a structure is formed by laminating a crystallized first layer and a second layer containing amorphous material. The grain boundaries contained in such a second layer are less than those in the first layer. As a result, even if there are paths in the first layer that may generate leakage current, the paths that may generate leakage current can be blocked (intercepted) by the second layer. Therefore, leakage current can be suppressed.
[0098] (4) Other forms The forms disclosed herein have been specifically described above. However, this disclosure is not limited to the forms described above, and various changes may be made without departing from its purpose.
[0099] Furthermore, the above-described examples illustrate the use of an oxidizing agent as the first reactant and the second reactant; however, this disclosure is not limited to this. When a single-metal film, rather than an oxide film, is formed as a film system on wafer 200, a reducing agent can be used. Examples of reducing agents include hydrogen-containing gases such as H2 gas and deuterium (D2) gas. Additionally, a nitriding agent can also be used when forming a nitriding film. A nitrogen-containing gas can be used as the nitriding agent. Specifically, at least one of NH3 gas, N2H4 gas, and N2H2 gas can be used. Furthermore, for each of the nitriding agent, reducing agent, and oxidizing agent, a gas that activates at least one of the gases disclosed herein can be used.
[0100] The process formulas (programs containing processing procedures or conditions, etc.) used to form these various thin films are preferably prepared individually (in multiples) according to the content of the substrate processing (the type, composition ratio, film quality, film thickness, processing procedures, processing conditions, etc. of the thin film to be formed). Then, it is preferable that when the substrate processing begins, an appropriate process formula is selected from the multiple process formulas according to the content of the substrate processing. Specifically, it is preferable that the multiple process formulas (programmable products) prepared individually according to the content of the substrate processing are stored in advance (installed) in the memory device 121c of the substrate processing apparatus via an electrical communication line or a recording medium (external memory device 123) containing the process formulas. Then, it is preferable that when the substrate processing begins, the CPU 121a of the substrate processing apparatus selects an appropriate process formula from the multiple process formulas stored in the memory device 121c according to the content of the substrate processing. By configuring it in this way, a wide variety of thin films with different compositions, textures, and thicknesses can be formed with versatility and good reproducibility using a single substrate processing unit. In addition, it can reduce the operator's workload (input burden such as processing procedures or processing conditions), avoid operational errors, and enable rapid commencement of substrate processing.
[0101] Furthermore, this disclosure can also be implemented, for example, by changing the process formula of an existing substrate processing apparatus. When changing the process formula, the process formula disclosed herein can also be installed on an existing substrate processing apparatus via an electrical communication line or a recording medium recording the process formula, or the process formula itself can be changed to the process formula disclosed herein by operating the input / output device of an existing substrate processing apparatus.
[0102] Furthermore, this disclosure can be applied, for example, to the word line portion of NAND flash memory or DRAM with a three-dimensional structure.
[0103] Furthermore, the above-described embodiments and variations illustrate an example of forming a film using a batch-type substrate processing apparatus that processes multiple wafers 200 at a time. This disclosure is not limited to the above-described embodiments; for example, it is also well applicable when forming a film using a leaf-type substrate processing apparatus that processes one or more wafers 200 at a time. Furthermore, the above-described embodiments illustrate an example of forming a film using a substrate processing apparatus with a hot-wall type furnace. This disclosure is not limited to the above-described embodiments; it is also well applicable when forming a film using a substrate processing apparatus with a cold-wall type furnace.
[0104] Furthermore, the above-described configuration illustrates an example in which the above-described processing sequence is performed in the same processing chamber (in-situ) of the same processing device. This disclosure is not limited to the above-described configuration; for example, it may also be designed to perform one step of the above-described processing sequence and other steps separately in separate processing chambers (ex-situ) of different processing devices, or it may be designed to perform them separately in separate processing chambers of the same processing device.
[0105] Even when using these substrate processing apparatuses, each processing can be performed with the same processing procedures and processing conditions as the above-described state or modified example, and the same effect as the above-described state or modified example can be obtained.
[0106] The above-described states or variations can be used in combination. The processing procedures and conditions at this time can be set as those of the above-described states or variations. [Simplified Explanation of the Diagram]
[0007] [Figure 1] Figure 1 is a schematic longitudinal cross-sectional view of the substrate processing apparatus. [Figure 2] A schematic cross-sectional view along line A-A in Figure 2. [Figure 3] Figure 3 is a schematic configuration diagram of the controller of the substrate processing apparatus, which is a block diagram illustrating the control system of the controller. [Figure 4] Figure 4 is a flowchart including a series of substrate processing steps. [Figure 5] Figure 5 is a flowchart up to the first processing to the modification processing.
Claims
1. A substrate processing method comprising: a) a step of supplying a first raw material to a substrate; b) a step of supplying a first reactant to the substrate in a first amount; c) a step of supplying a second reactant to the substrate in a second amount; d) a step of forming a first layer on the substrate by performing a) and b) a predetermined number of times; e) a step of forming a second layer on the substrate by performing a) and c) a predetermined number of times; f) a step of supplying a second raw material to the substrate; wherein in d), a)b)f) are performed a predetermined number of times, and in e), a)c)f) are performed a predetermined number of times.
2. The substrate processing method as described in claim 1, wherein, The first quantity mentioned above and the second quantity mentioned above are different quantities.
3. The substrate processing method as described in claim 1, wherein, The second quantity mentioned above is a quantity that is less than the first quantity mentioned above.
4. The substrate processing method as described in claim 1, wherein, It also has the following features: performing d) and e) a specified number of times to stack the aforementioned first layer and the aforementioned second layer.
5. The substrate processing method as described in claim 1, wherein, The first raw material contains a first element, the second raw material contains a second element, and the ratio of the first element to the second element in the first layer is close to the ratio of the first element to the second element in the second layer.
6. The substrate processing method as described in claim 1, wherein, It also has: g) the process of modifying the aforementioned first layer and the aforementioned second layer.
7. A substrate processing method comprising: a) a step of supplying a first raw material to a substrate; b) a step of supplying a first reactant to the substrate in a first amount; c) a step of supplying a second reactant to the substrate in a second amount; d) a step of performing a) and b) a predetermined number of times to form a first layer on the substrate; e) a step of performing a) and c) a predetermined number of times to form a second layer on the substrate; g) a step of crystallizing the first layer and modifying the second layer into a layer containing an amorphous material.
8. The substrate processing method as described in claim 6 or 7, wherein, The first layer mentioned above is a layer that can be crystallized by modification, and the second layer mentioned above is a layer that can contain amorphous material by modification.
9. The substrate processing method as described in claim 6 or 7, wherein, The aforementioned modification was achieved through heat treatment.
10. The substrate processing method as described in claim 1, wherein, The oxidizing power of the first reactant mentioned above is different from that of the second reactant mentioned above.
11. The substrate processing method as described in claim 1, wherein, The oxidizing power of the second reactant is weaker than that of the first reactant.
12. The substrate processing method as described in claim 1, wherein, The supply amounts of the first reactant and the second reactant are different.
13. The substrate processing method as described in claim 1, wherein, The amount of the second reactant supplied is less than the amount of the first reactant supplied.
14. The substrate processing method as described in claim 1, wherein, The partial pressure of the second reactant is lower than that of the first reactant.
15. The substrate processing method as described in claim 1, wherein, The supply flow rate of the second reactant is less than that of the first reactant.
16. The substrate processing method as described in claim 1, wherein, The first reactant and the second reactant mentioned above are dissimilar materials.
17. A method for manufacturing a semiconductor device, comprising: a) a step of supplying a first raw material to a substrate; b) a step of supplying a first reactant to the substrate in a first amount; c) a step of supplying a second reactant to the substrate in a second amount; d) a step of forming a first layer on the substrate by performing a) and b) a predetermined number of times; e) a step of forming a second layer on the substrate by performing a) and c) a predetermined number of times; f) a step of supplying a second raw material to the substrate; wherein in d), a)b)f) are performed a predetermined number of times; and in e), a)c)f) are performed a predetermined number of times.
18. A program, by means of a computer, instructs a substrate processing apparatus to perform: a) supplying a first raw material to a substrate; b) supplying a first reactant to the substrate in a first amount; c) supplying a second reactant to the substrate in a second amount; d) performing a) and b) a predetermined number of times to form a first layer on the substrate; e) performing a) and c) a predetermined number of times to form a second layer on the substrate; f) supplying a second raw material to the substrate; wherein in d), a) b) and f) are performed a predetermined number of times; and in e), a) c) and f) are performed a predetermined number of times.
19. A substrate processing apparatus comprising: a first supply unit for supplying a first raw material to a substrate; a second supply unit for supplying a first reactant to the substrate; a third supply unit for supplying a second reactant to the substrate; a fourth supply unit for supplying a second raw material to the substrate; and a control unit configured to control the first, second, third, and fourth supply units to perform: a) a process of supplying the first raw material to the substrate; b) a process of supplying the first reactant to the substrate in a first amount; c) a process of supplying the second reactant to the substrate in a second amount; d) a process of forming a first layer on the substrate by performing a) and b) a predetermined number of times; e) a process of forming a second layer on the substrate by performing a) and c) a predetermined number of times; f) a process of supplying the second raw material to the substrate; wherein in d), a)b)f) are performed a predetermined number of times; and in e), a)c)f) are performed a predetermined number of times.
20. A method for manufacturing a semiconductor device, comprising: a) a step of supplying a first raw material to a substrate; b) a step of supplying a first reactant to the substrate in a first amount; c) a step of supplying a second reactant to the substrate in a second amount; d) a step of performing a) and b) a predetermined number of times to form a first layer on the substrate; e) a step of performing a) and c) a predetermined number of times to form a second layer on the substrate; g) a step of crystallizing the first layer and modifying the second layer into a layer containing an amorphous material.
21. A program, by means of a computer, instructs a substrate processing apparatus to perform: a) supplying a first raw material to a substrate; b) supplying a first reactant to the substrate in a first amount; c) supplying a second reactant to the substrate in a second amount; d) performing a) and b) a predetermined number of times to form a first layer on the substrate; e) performing a) and c) a predetermined number of times to form a second layer on the substrate; g) crystallizing the first layer and modifying the second layer into a layer containing an amorphous material.
22. A substrate processing apparatus comprising: a first supply unit for supplying a first raw material to a substrate; a second supply unit for supplying a first reactant to the substrate; a third supply unit for supplying a second reactant to the substrate; and a control unit configured to control the first, second, and third supply units to perform: a) a process of supplying the first raw material to the substrate; b) a process of supplying the first reactant to the substrate in a first amount; c) a process of supplying the second reactant to the substrate in a second amount; d) a process of forming a first layer on the substrate by performing a) and b) a predetermined number of times; e) a process of forming a second layer on the substrate by performing a) and c) a predetermined number of times; and g) a process of crystallizing the first layer and modifying the second layer into a layer containing an amorphous material.
Citation Information
Patent Citations
Film formation method and film formation apparatus
JP2021106217A
Semiconductor device manufacturing method, substrate processing method, substrate processing device, and program
TW202311558A
Method of processing substrate, method of manufacturing semiconductor device, substrate processing apparatus, and program
TW202329244A
Method of manufacturing semiconductor device, substrate processing apparatus, and recording medium
US20160071720A1
Film-forming method and film-forming apparatus
US20220396874A1