Method for manufacturing sintered ore
Patent Information
- Application Number
- TW114127733
- Authority / Receiving Office
- TW · TW
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2024-11-22
- Filing Date
- 2025-07-22
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-07-21
AI Technical Summary
The micronization of iron ore due to deterioration leads to variations in particle size, affecting the granulation properties of sintering raw materials, and the incorporation of concentrate worsens permeability and combustion rates, resulting in reduced productivity of sintered ore.
A method involving the blending of iron raw materials with concentrate and carbon materials, where palm shell charcoal (PKS char) with a smaller particle size than fossil fuel-derived charcoal is used to improve granulation properties, and the blending ratio of PKS char is optimized to enhance combustion and reduce carbon dioxide emissions.
The method improves granulation properties and combustion efficiency, leading to increased productivity and reduced carbon emissions in the sintering process.
Smart Images

Figure TWG2TB001920707_001 
Figure TWG2TB001920707_002 
Figure TWG2TB001920707_003
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing sintered ore. Prior Technology
[0002] The sintering process for producing sintered iron ore used in blast furnaces involves igniting the upper layer of the raw material in a sintering machine, drawing air from the lower layer, and causing the flame to spread from the upper to the lower layers, thus firing all layers of the raw material. The raw material is blended with iron, fluxing agents for composition adjustment, and solid carbon materials. Examples of iron raw materials include iron ore powder or return ore.
[0003] In the sintering process, large quantities of anthracite or coke powder (hereinafter referred to as coal) derived from fossil fuels are used as solid charcoal, and a portion of these are replaced with carbon-neutralizing materials (hereinafter referred to as biochar). This is to meet the requirement of reducing carbon dioxide emissions during the sintering process. Among carbon-neutralizing materials, palm kernel shell charcoal (hereinafter referred to as PKS charcoal) is relatively more readily available and is therefore used as charcoal in the sintering process. However, due to the large amount of coal used in the sintering process, supply issues prevent the complete replacement of all coal with PKS charcoal, thus only a portion of the coal is replaced with PKS charcoal.
[0004] Patent documents 1 and 2 disclose a method for manufacturing sintered ore, which improves the combustion rate of the sintering raw materials during the sintering process by partially replacing fossil fuel-derived charcoal with coarse-grained oil palm shell charcoal. This operation is believed to improve the productivity of sintered ore. Furthermore, oil palm shell charcoal and palm shell charcoal are the same, and are collectively referred to as PKS charcoal below.
[0005] On the other hand, the issue of iron ore deterioration remains. As a countermeasure to the decrease in iron content in iron ore, beneficiation is implemented. Beneficiation refers to crushing mined iron ore and separating high-iron-content iron ore from low-iron-content iron ore. The high-iron-content iron ore obtained through this separation (hereinafter referred to as concentrate ore) is then shipped. Concentrate ore contains less gangue. Therefore, it is incorporated into the sintering raw materials to dilute the gangue content of the sinter produced in the sintering process. [Previous Technical Documents] [Patent Literature]
[0006] Patent Document 1: Japanese Patent No. 6102484 Patent Document 2: Japanese Patent No. 5786795 Summary of the Invention
[0007] [The problem that the invention aims to solve] The micronization of iron ore due to its deterioration is increasing year by year. Compared to the past, the current micronization of iron ore results in variations in particle size, leading to differences in the granulation properties of sintering raw materials. Patent Documents 1 and 2 disclose methods for partially replacing fossil fuel-derived charcoal with PKS charcoal, but they do not specify the particle size of the iron ore incorporated into the sintering raw materials. Furthermore, as mentioned above, the current level of iron ore micronization exceeds that at the time the methods in Patent Documents 1 and 2 were invented. Therefore, the current method of manufacturing sintered ore based on Patent Documents 1 and 2, which involves partially replacing fossil fuel-derived charcoal with PKS charcoal, may become a cause of iron ore micronization, leading to a deterioration in the granulation properties of the sintering raw materials.
[0008] Furthermore, when a portion of the iron raw material incorporated into the sintering feedstock is replaced with concentrate, the poor wettability of the concentrate may lead to a deterioration in the granulation properties of the sintering feedstock. When the granulation properties of the sintering feedstock deteriorate, the permeability during sintering in the sintering machine worsens, resulting in deteriorated operating conditions such as misfires or reduced combustion rates. Consequently, the productivity of sintered ore remains a concern.
[0009] The present invention was made to solve the above-mentioned problems. Its purpose is to provide a method for manufacturing sintered ore, which can improve the granulation properties of sintered ore even when PKS carbon is mixed into the sintering raw material in order to reduce carbon dioxide emissions and concentrate is mixed into the sintering raw material in order to increase the total Fe content. [Methods used to solve problems]
[0010] The methods used to solve the problem are as follows. [1] A method for manufacturing sintered ore, comprising a raw material blending step, a raw material layer forming step and a sintering step, wherein the raw material blending step involves blending iron raw material and solid carbon material and granulating them together to manufacture sintering raw material, wherein the iron raw material includes concentrate and iron ore powder, and the solid carbon material includes a first carbon material and a second carbon material with a combustion initiation temperature higher than the first carbon material, wherein the raw material layer forming step involves supplying the aforementioned sintering raw material to a pallet of a sintering machine to form a raw material layer, and wherein the sintering step involves igniting on the aforementioned raw material layer to sinter the aforementioned sintering raw material to manufacture sintered ore; wherein, in the aforementioned raw material blending step, palm shell carbon is blended as the aforementioned first carbon material, and carbon material derived from fossil fuels is blended as the aforementioned second carbon material, wherein the arithmetic mean particle size of the aforementioned palm shell carbon is smaller than the arithmetic mean particle size of the aforementioned second carbon material. [2] The method for manufacturing sintered ore as described in [1], wherein in the aforementioned raw material blending step, the blended arithmetic average particle size is less than 1.10 mm, as described above, palm shell charcoal. [3] The method for manufacturing sinter as described in [1] or [2], wherein in the aforementioned raw material blending step, the aforementioned iron raw material is blended with the aforementioned concentrate in such a way that the blending ratio of the aforementioned iron raw material to the aforementioned concentrate is 5.0 to 30.0% by mass. [4] The method for manufacturing sintered ore as described in any of [1] to [3], wherein in the aforementioned raw material blending step, the aforementioned palm shell char is blended into the aforementioned solid char in such a way that the blending ratio of the aforementioned palm shell char in the aforementioned solid char is 10.0 to 50.0% by mass. [Invention Effects]
[0011] According to the present invention, even when PKS carbon is mixed into the sintering raw material to reduce carbon dioxide emissions, or concentrate is mixed into the sintering raw material to increase the total Fe content, the granulation properties of the sintering raw material can still be improved. Simple Explanation of the Diagram
[0012] [Figure 1] A diagram illustrating the method of manufacturing sintered ore according to this embodiment. [Figure 2] shows an example of sinter manufacturing equipment applicable to the sinter manufacturing method of this embodiment. [Figure 3] A diagram illustrating the manufacturing process and particle size adjustment method of PKS charcoal. Implementation
[0013] Hereinafter, embodiments of the present invention (hereinafter referred to as "this embodiment") will be described with reference to the drawings. FIG1 is a diagram illustrating a method for manufacturing sintered ore according to this embodiment. In the example shown in FIG1, firstly, a plurality of raw materials are mixed in a specified proportion to manufacture sintering raw materials (stage S101, raw material blending step). FIG2 is a diagram showing an example of a sintering ore manufacturing equipment to which the method for manufacturing sintered ore according to this embodiment is applicable. As shown in FIG2, a plurality of hoppers 1 are provided on the sintering ore manufacturing equipment. Each of these hoppers 1 stores a different raw material.
[0014] Examples of raw materials for sintering include iron raw materials, by-products, and solid carbon materials (hereinafter referred to as carbon materials). Examples of iron raw materials include iron ore powder, recycled ore, and concentrate. Concentrate refers to iron ore with a high iron content, separated from mined iron ore through beneficiation. Concentrate has a lower gangue content compared to the iron ore before beneficiation. Therefore, in this embodiment, in order to dilute the gangue content in the sinter produced using iron ore undergoing deterioration and increase the total Fe content, it is incorporated into the iron raw materials. The proportion of concentrate in the iron raw materials is preferably 5.0 to 30.0% by mass. This is because if the proportion of concentrate is less than 5.0% by mass, the gangue content cannot be diluted. If the proportion of concentrate exceeds 30.0% by mass, it becomes difficult to form the granulated particles described later. Furthermore, concentrates have the characteristic that moisture is not easily retained on their surface, and therefore they are not easily agglomerated. In order to facilitate the agglomeration of concentrates, PKS char with a particle size smaller than coke powder is added to the sintering raw materials, as described later. Also, in the following description, "mass %" will be recorded as "%".
[0015] Examples of by-products include limestone, dolomite, and quicklime.
[0016] Examples of charcoal materials include coke powder or anthracite derived from fossil fuels, and palm shell charcoal derived from biomass (hereinafter referred to as PKS charcoal). In this embodiment, PKS charcoal is blended into fossil fuel-derived charcoal to reduce carbon dioxide emissions generated during the production of sinter. The arithmetic mean particle size (hereinafter referred to as average particle size) of the PKS charcoal is preferably smaller than that of coke powder. This is to improve granulation properties. Furthermore, the surface of PKS charcoal is smooth and has few pores, making it less likely to retain moisture compared to coke powder. Therefore, by pulverizing the PKS charcoal to reduce its particle size, the specific surface area is increased, thereby enabling moisture to be retained on the surface of the PKS charcoal. Specifically, since the average particle size of coke powder is around 1.20 mm, it is preferable to pulverize the PKS charcoal to make its average particle size smaller than 1.10 mm or less, which is even smaller than the average particle size of coke powder. This is because if the average particle size of PKS char exceeds 1.10 mm, the mass ratio of iron raw material in the granulated particles will become excessively low. Furthermore, the surface of PKS char cannot retain moisture, thus making it difficult to form granulated particles.
[0017] Furthermore, the proportion of PKS char in the solid char material is preferably between 10.0% and 50.0%. This is because, as will be explained later, if the proportion of PKS char is less than 10.0%, it will be difficult for the concentrate to agglomerate in the case of iron raw materials containing concentrate. If the proportion of PKS char exceeds 50.0%, the high combustibility of PKS char may lead to an excessively reduced yield of sinter. Moreover, the PKS char in the above-mentioned char material should be the first char material of this embodiment, and coke powder or anthracite should be the second char material of this embodiment. The details regarding PKS char will be explained later.
[0018] In the example shown in Figure 2, each raw material is supplied in a predetermined proportion from a hopper 1 containing various raw materials on a conveyor belt (not shown), and then transported to a drum mixer 2 by the conveyor belt.
[0019] In the rotary mixer 2, the raw materials are mixed and water is added to the mixture to humidify it, thereby producing a sintering raw material containing granulated particles (in some cases, quasi-particles) with a predetermined average particle size. The sintering raw material is then transported by conveyor belt to a surge hopper 3 for temporary storage. The steps of producing the sintering raw material by performing the operations described above constitute the raw material blending step of this embodiment.
[0020] Referring back to the explanation in Figure 1. After the raw material blending step in stage S101, the process proceeds to the raw material layer formation step in stage S102. In the raw material layer formation step, sintering raw materials are loaded onto the pallet 10 of the sintering machine 9, and a raw material layer 7 is formed on the pallet 10. That is, the sintering raw materials stored in the temporary storage hopper 3 shown in Figure 2 are fed in by a drum feeder 4 and loaded onto the ore layer 6 via a chute 5. This forms the raw material layer 7.
[0021] In the example shown in Figure 2, a sintering ore hopper 8 is provided upstream of the temporary storage hopper 3 in the conveying direction of the sintering raw materials in the sintering machine 9. The sintering ore is stored in the sintering ore hopper 8. The sintering ore is fed out from the cylindrical feeder of the sintering ore hopper 8 and loaded onto the pallet 10 of the sintering machine 9 via a chute, thereby forming the sintering ore layer 6.
[0022] A shut-off gate 11 is provided downstream of the temporary storage hopper 3 in the direction of raw material transport for sintering, to level the surface of the raw material layer 7 on the pallet 10 and make the thickness of the raw material layer 7 uniform. By passing through the shut-off gate 11, a raw material layer 7 of predetermined thickness is formed. The step of loading the raw material onto the pallet 10 to form a raw material layer 7 of predetermined thickness is the raw material layer forming step of this embodiment.
[0023] Returning to the explanation in Figure 1. After the raw material layer formation step in stage S102, the process proceeds to the sintering step in stage S103. In the sintering step, the raw material layer 7 formed on the pallet 10 of the sintering machine 9 is ignited to sinter the raw material. As shown in Figure 2, an ignition furnace 12 is provided in the conveying direction and downstream of the stop gate 11. The charcoal material existing on the surface (top) of the raw material layer 7 is ignited by the ignition furnace 12. Furthermore, a plurality of bellows 13 are provided in the vertical direction of the sintering machine 9 and under the pallet 10. Each bellows 13 is connected to a sintering blower 15 via an exhaust pipe 14. The sintering blower 15 draws air from the bellows 13. This operation causes air to flow from the top to the bottom in the thickness direction of the raw material layer 7. This allows the charcoal material in the sintering raw material to burn from the top to the bottom of the raw material layer 7. The sintering raw material is heated by the heat of combustion of charcoal, and at least a portion of the iron raw material melts and bonds together, sintering the raw material from the upper side to the lower side of the raw material layer 7. This forms a sintered raw material layer (sometimes called a sintered cake) on the pallet 10 of the sintering machine 9. The step of sintering the raw material in this manner is equivalent to the sintering step described above.
[0024] In the example shown in Figure 2, a dust collector 16 is installed upstream of the sintering blower 15 in the direction of airflow to collect dust in the air or microparticles in the sintering raw materials. A chimney 17 is installed downstream of the sintering blower 15 in the direction of airflow. The air drawn in by the sintering blower 15 is discharged to the outside through the chimney 17.
[0025] The sinter cake formed on the pallet 10 of the sintering machine 9 is discharged to the outside of the sintering machine 9 in the conveying direction and from the discharge section on the downstream side of the sintering machine 9. Subsequently, the sinter cake is crushed by the crusher 18 and then subjected to particle separation. The sinter with a predetermined particle size is recycled as the finished sinter.
[0026] (PKS Charcoal) This section explains PKS charcoal. PKS charcoal is a type of charcoal produced by the dry distillation of palm shells (hereinafter referred to as PKS). During the growth process of PKS, the raw material for PKS charcoal absorbs carbon dioxide. Therefore, from a carbon neutrality perspective, the amount of carbon dioxide emitted into the environment can be considered negligible when PKS charcoal produced by dry distillation is burned. Therefore, from a carbon neutrality perspective, if PKS charcoal is blended with biomass carbon as a sintering raw material, the amount of carbon dioxide emitted can be reduced accordingly.
[0027] Characteristics of PKS include a higher proportion of volatile matter and a lower combustion onset temperature compared to coke powder or anthracite. PKS has a volatile matter content of 70-80%. PKS char is produced by dry distillation of PKS, with a volatile matter content of 3-5%. The combustion onset temperature of PKS char is 420°C, lower than the 624°C combustion onset temperature of coke powder. Furthermore, as mentioned above, PKS char has a smooth surface with few pores, making it difficult to retain moisture on its surface. Therefore, in this embodiment, the specific surface area is increased by pulverizing PKS char, thereby enabling its surface to retain moisture. This operation facilitates the agglomeration of the concentrate when it is blended with the sintering raw material, thus improving the granulation properties of the sintering raw material.
[0028] (Methods for manufacturing and adjusting particle size of PKS charcoal) Figure 3 illustrates the manufacturing and particle size adjustment methods of PKS char. In Figure 3, for example, the PKS is first pyrolyzed at 1000°C for 1 hour (stage S201). The PKS pyrolyzing method is not limited; a batch pyrolyzer (not shown) can be used. Alternatively, a kiln-type continuous pyrolyzer can be used instead of a batch pyrolyzer. Furthermore, by pyrolyzing the PKS, the volatile matter content of the PKS char is reduced to less than 5%. This is to suppress problems such as smoke generation during exhaust gas treatment in the sintering process. Moreover, while unpyrolyzed PKS is difficult to pulverize, pyrolyzed PKS exhibits improved pulverability compared to before pyrolyzation. To ensure the pulverability of PKS char, a Hardgrove Grindability Index (HGI) of 25 or higher is preferred, with an HGI of 30 or higher, similar to that of coke powder, being even better. The HGI can be measured using the method described in JIS M 8801:2008. Furthermore, the HGI can be adjusted by changing the distillation time.
[0029] Following stage S201, PKS char is pulverized to make its particle size smaller than that of fossil fuel-derived charcoal (stage S202). This is to increase the specific surface area of the PKS char, making its surface easier to retain moisture. Furthermore, this is to improve the granulation properties of the sintering raw materials when PKS char is blended with concentrate, making the concentrate easier to agglomerate. There are no limitations on the pulverization method for PKS char; for example, it can be pulverized using a jaw crusher or a disc mill. Furthermore, examples of fossil fuel-derived charcoal include coke powder.
[0030] Next, the pulverized PKS char is sieved using a sieve with the same mesh size as the coke powder, separating PKS char that is larger than the average particle size of the coke powder and PKS char that is smaller than the average particle size of the coke powder (stage S203). Since the average particle size of the coke powder is around 1.20 mm, it is preferable to use a sieve with a mesh size of 1.10 mm for sieving the pulverized PKS char. PKS char that is larger than the average particle size of the coke powder (No in stage S203) is returned to stage S202 and pulverized again. PKS char that is smaller than the average particle size of the coke powder (Yes in stage S203) is recycled as charcoal material to be incorporated into the sintering raw materials (stage S204).
[0031] (Functions and Effects) In this embodiment, PKS char is pulverized, resulting in a smaller particle size and an increased specific surface area, making it easier to retain moisture on its surface. Therefore, even if the concentrate is difficult to retain moisture and agglomerate, the moisture retained by the PKS char can help agglomerate the concentrate, thereby improving the granulation properties of the sintering raw material. Furthermore, because the PKS char is pulverized, its smaller particle size makes it easier to burn compared to before pulverization. Therefore, during the firing of the sintering raw material, the amount of unburned char remaining on the pallet 10 can be suppressed. That is, the combustibility of the sintering raw material on the pallet 10 can be improved, thereby increasing the overall production yield of the sinter. Also, in this embodiment, by replacing a portion of the char with PKS char, the amount of carbon dioxide emitted during the sintering process can be reduced. Example 1
[0032] Example 1 describes the verification of the effectiveness of this embodiment. First, PKS was divided into small portions and placed in small containers, all of which were placed in a batch dry distillation furnace (hereinafter referred to as the dry distillation furnace). In the dry distillation furnace, the PKS was dry distilled at 1000°C under nitrogen for 6 hours to produce PKS char. Next, the PKS char was pulverized using a jaw crusher and a disc mill to produce three types of PKS char, A, B, and C, with different average particle sizes. Furthermore, coke powder was prepared as a char material derived from fossil fuels. The particle size distribution of the coke powder and each type of PKS char, A, B, and C, is presented in Table 1. In the following description, "mass %" will be referred to as "%".
[0033]
[0034] Furthermore, the open pore volume of each unit mass of PKS carbon A, B, and C, and the open pore volume of each unit mass of coke powder were measured using mercury porosimetry. The open pore volume of each PKS carbon A, B, and C was 0.11 cm³ / g, and the open pore volume of each unit mass of coke powder was 0.67 cm³ / g. Therefore, the open pore volume of each unit mass of PKS carbon A, B, and C is smaller than the open pore volume of each unit mass of coke powder.
[0035] Iron raw materials, flux for composition adjustment, and carbon materials are mixed in a predetermined blending ratio, and small amounts of water are added to the mixture step by step while simultaneously forming granulated particles. Examples of iron raw materials include iron ore powder, recycled ore, and concentrate. In Example 1, a portion of the iron ore powder is replaced with concentrate. Examples of flux for composition adjustment include limestone. Examples of carbon materials include PKS carbons A, B, and C, and coke powder. In Example 1, any one of PKS carbons A, B, and C, along with coke powder, is used as the carbon material. That is, a portion of the coke powder is replaced with any one of PKS carbons A, B, and C. The blending ratios (mass %) of each raw material are presented in Table 2. As shown in Table 2, the proportion of concentrate in the iron raw material after removing recycled ore is 5.0%, 20.0%, or 30.0%. The proportion of PKS carbon in the carbon material is 10.0%, 25.0%, or 50.0%.
[0036]
[0037] Furthermore, the names, particle size distributions of the iron ore powder used in this embodiment and the particle size distribution of the concentrate are presented in Table 3.
[0038]
[0039] The particle size distribution of the dried granulated particles is presented in Table 4. Furthermore, the particle size, i.e., the harmonic mean diameter, of the granulated particles was calculated by sieving the dried granulated particles.
[0040]
[0041] (evaluate) Experimental Examples 1, 2, and Comparative Example 1 all involved 5.0% concentrate in the charcoal material, and the types of PKS charcoal, i.e., the particle sizes, varied. As shown in Table 4, Experimental Examples 1, 2, and Comparative Example 1 revealed that the average diameter of the granulated particles decreased with increasing PKS charcoal particle size. In Comparative Example 1, the average diameter of the granulated particles was less than 0.60 mm, and during filling, fine particles penetrated the air gaps. Therefore, due to the blockage of these gaps, it was believed that the permeability of the raw material layer on the sintering machine pallet deteriorated.
[0042] Examples 2-4 show examples where the blending ratio of concentrate was increased by 5.0%, 20.0%, and 30.0%, respectively, while the type and blending ratio of PKS char were kept constant. In Examples 2-4, the blended average diameter decreased with the increase in the blending ratio of concentrate. In Example 4, although the blended average diameter was above 0.60 mm, since the particle size of the granulated particles was the smallest in Examples 2-4 and close to the threshold (blended average diameter 0.60 mm), it was considered that the blending ratio of concentrate should be below 30.0% relative to iron ore powder.
[0043] Compared to Experimental Example 4, Comparative Example 2 was formed using the same procedures as Experimental Example 4, except for the increased particle size of the PKS carbon. The average diameter of the granulated particles in Comparative Example 2 was 0.57 mm, as shown in Table 4, and was smaller than that of the granulated particles in Experimental Example 4. This is believed to be due to the increased particle size of the PKS carbon. Furthermore, in Comparative Example 2, since the average diameter was less than 0.60 mm, it is believed that, similar to Comparative Example 1, a deterioration in the permeability of the raw material layer occurred on the sintering machine pallet.
[0044] Example 5 was prepared by the same procedure as Example 3, except that the PKS char blending ratio was set to 25.0%. Example 6 was prepared by the same procedure as Example 3, except that the PKS char blending ratio was set to 50.0%. As shown in Table 4, the average diameter of the granulated particles increased with the increase of the PKS char blending ratio in Examples 3, 5, and 6. Based on these results, it can be concluded that the granulation performance improves with the increase of the PKS char blending ratio.
[0045] Comparative Example 3 was formed by the same procedure as Experimental Example 6, except that the particle size of the PKS char was increased. The average diameter of the granulated particles in Comparative Example 3 was 0.56 mm, as shown in Table 4, and was smaller than that of the granulated particles in Experimental Example 6. This is believed to be due to the increased particle size of the PKS char. Furthermore, since the average diameter of Comparative Example 3 was less than 0.60 mm, it is believed that, similar to Comparative Example 1, a deterioration in the permeability of the raw material layer occurred on the sintering machine pallet. Example 2
[0046] (Sintered ore manufacturing experiment) Example 2 is a sinter manufacturing test conducted based on the results of the granulation test in Example 1. Specifically, the granulated particles from Experimental Examples 1-6 and Comparative Examples 1-3 were loaded into an intermittent sintering pot test apparatus (hereinafter referred to as the apparatus) for sintering. This was used to manufacture sinters from Experimental Examples 1-6 and Comparative Examples 1-3, respectively. Furthermore, the raw material loading section of the apparatus had a diameter of 300 mm and a height of 400 mm, and was equipped with an ignition furnace and exhaust equipment such as a bellows or blower. Therefore, it was possible to conduct sinter manufacturing tests simulating an actual sintering machine.
[0047] After firing, the sinter was removed from the apparatus, and the yield and productivity were measured. Here, yield refers to the mass proportion of sinter with a particle size of 5.00 mm or larger in the total amount of sinter after it has been dropped from a height of 2 m onto the support surface four times for crushing. Productivity is the value obtained by dividing the amount of sinter with a particle size of 5.00 mm or larger by the time required to produce the sinter and the area of the raw material layer in the apparatus. A higher value indicates better productivity. The yield and productivity of the sinter from Experimental Examples 1-6 and Comparative Examples 1-3 are summarized in Table 5.
[0048]
[0049] Comparing Experimental Examples 1 and 2 with Comparative Example 1, it was found that the yield and productivity of Experimental Example 1 were greater than those of Experimental Example 2, and the yield and productivity of Experimental Example 2 were greater than those of Comparative Example 1. This is believed to be because the particle size of PKS char gradually increases in the order of Experimental Examples 1, 2, and Comparative Example 1, and the particle size of the granulated particles decreases accordingly, resulting in a sequential deterioration of the permeability of the raw material layer during sinter production. That is, it is believed that in Experimental Example 1 or Experimental Example 2, the improved permeability compared to Comparative Example 1 leads to more uniform sintering and an overall increase in yield. Furthermore, it is believed that because PKS char has better combustibility than coke powder, the proportion of unburned carbon is reduced, thus increasing the yield. Unburned carbon refers to the free carbon (Free-C) contained in sinter with a particle size of less than 5.00 mm after yield measurement. The sinter in Experimental Example 1 contained 0.13% unburned carbon, the sinter in Experimental Example 2 contained 0.14% unburned carbon, and the sinter in Comparative Example 1 contained 0.21% unburned carbon.
[0050] The rationale for the increased productivity was examined. This is because a smaller particle size of the PKS char leads to an increase in its specific surface area. This is believed to be due to an increased combustion rate of the PKS char. Furthermore, it was found that under conditions where the concentrate blending ratio was increased compared to Experimental Examples 1 or 2, i.e., Experimental Examples 3, 4, and Comparative Example 2, as shown in Table 5, reducing the particle size of the PKS char also improved the yield and productivity of the sinter.
[0051] Comparing Experiments 2, 3, and 4, it was found that the yield and productivity decreased with increasing concentrate blending ratio. This is because, as shown in Table 4, the average particle size of the granulated particles gradually decreased in the order of Experiments 2, 3, and 4, thus increasing the likelihood of uneven combustion during the firing of the raw material layer. In other words, it was expected that the permeability of the raw material layer would decrease in the order of Experiments 2, 3, and 4, making uniform firing impossible. Based on these results, it was concluded that a concentrate blending ratio of 30.0% or less is preferable.
[0052] Furthermore, when comparing Experimental Example 4 and Comparative Example 2, the yield and productivity of Comparative Example 2 decreased compared to Experimental Example 4. This is believed to be because the average diameter of the granulated particles in Comparative Example 2 is smaller than that in Experimental Example 4, thus reducing the permeability of the raw material layer.
[0053] In comparing Experiments 3, 5, and 6, while productivity increased with increasing PKS char blending ratio, yield decreased. The reason for the increased productivity is examined. PKS char has higher combustibility than coke powder. Therefore, it is believed that increasing the PKS char blending ratio leads to an increased firing rate at the feedstock layer. Regarding the decreased yield, as mentioned above, PKS char has higher combustibility than coke powder. This means that PKS char has a higher combustion rate. On the other hand, a higher combustion rate may lead to increased incomplete combustion of PKS char, potentially resulting in insufficient combustion of the total amount of PKS char. Therefore, it is believed that insufficient heat for sintering leads to a decreased yield. Furthermore, based on these results, it is considered that a PKS char blending ratio of 50.0% or less in the char material is preferable.
[0054] In Comparative Example 3, misfire occurred during the firing of the raw material layer, making it impossible to complete the firing process. As a result, sintered ore could not be produced. This is believed to be due to the fact that the average diameter of the granulated particles in Comparative Example 3, as shown in Table 4, was the smallest among Experimental Examples 1-6 and Comparative Examples 1-3, thus resulting in poor permeability.
[0055] 1: Hopper 2: Rotary drum mixer 3: Temporary storage 4: Tube feeder 5: Slide 6: Ground-level mineral layer 7: Raw material layer 8: Ground-level ore hopper 9: Sintering machine 10: Pallet 11: Stop gate 12: Ignition Stove 13: Bellows 14: Exhaust duct 15: Sintering blower 16: Dust collector 17: Chimney 18: Crusher S1: Raw material blending steps S2: Raw material layer formation step S3: Sintering Step
Claims
1. A method for manufacturing sintered ore, comprising a raw material blending step, a raw material layer forming step, and a sintering step, wherein the raw material blending step involves blending iron raw materials and solid carbon materials and granulating them together to produce sintering raw materials, the iron raw materials comprising concentrate and iron ore powder, the solid carbon materials comprising a first carbon material and a second carbon material with a combustion initiation temperature higher than the first carbon material, the raw material layer forming step involves feeding the aforementioned sintering raw materials onto a pallet of a sintering machine to form a raw material layer, and the sintering step involves igniting on the aforementioned raw material layer to sinter the aforementioned sintering raw materials to produce sintered ore; wherein... In the aforementioned raw material blending step, palm shell charcoal is blended as the first charcoal material, and charcoal material derived from fossil fuels is blended as the second charcoal material. The arithmetic mean particle size of the palm shell charcoal is smaller than the arithmetic mean particle size of the second charcoal material.
2. The method for manufacturing sintered ore as claimed in claim 1, wherein in the aforementioned raw material blending step, the blended material with an arithmetic mean particle size of less than 1.10 mm is the aforementioned palm shell charcoal.
3. The method for manufacturing sinter as claimed in claim 1 or 2, wherein in the aforementioned raw material blending step, the aforementioned iron raw material is blended with the aforementioned concentrate in such a way that the blending ratio of the aforementioned iron raw material to the aforementioned concentrate is 5.0 to 30.0% by mass.
4. The method for manufacturing sintered ore as claimed in claim 1 or 2, wherein in the aforementioned raw material blending step, the aforementioned palm shell char is blended into the aforementioned solid char material in such a way that the blending ratio of the aforementioned palm shell char in the aforementioned solid char material is 10.0 to 50.0% by mass.
5. The method for manufacturing sintered ore as claimed in claim 3, wherein in the aforementioned raw material blending step, the aforementioned palm shell char is blended into the aforementioned solid char in such a way that the blending ratio of the aforementioned palm shell char in the aforementioned solid char is 10.0 to 50.0% by mass.
Citation Information
Patent Citations
Method for realizing ultralow-temperature ignition by utilizing biomass fuel in sintering process
CN116878022A
Green low-carbon sintering method based on biomass energy
CN118423991A
Sintered ore production method
TW202428890A