Modified Minky Fabric Adapted for Quilting and Method of Manufacture
The modified minky fabric addresses quilting challenges by using warp knitting and specialized finishing processes to reduce slipperiness and seam width, improving cutting and sewing ease.
Patent Information
- Application Number
- US19/663972
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2025-05-06
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional minky fabric is challenging for quilting due to difficulties in cutting, uneven seams, wide seams, slippery nature, and time-consuming pinning, which affects the appearance and ease of use.
A modified minky fabric is produced through warp knitting with specific yarns and heat treatment, followed by specialized finishing processes to reduce slipperiness, improve seam sharpness, and eliminate the need for pinning, resulting in easier cutting and sewing.
The modified minky fabric is 75% less prone to 'cuddle dust', reduces seam width to ¼ inch, and eliminates the need for pinning, enhancing design creativity and sewing ease.
Smart Images

Figure US20260357489A1-D00000_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATION:
[0001] This application claims the benefit of U.S. Provisional Patent Application No. 63 / 801,051, filed on May 6, 2025.FIELD OF THE INVENTION
[0002] The present invention relates to fabrics used for quilting. More specifically, the production of a minky textured fabric suitable for quilting.BACKGROUND
[0003] Minky fabric is a type of fabric that is extremely popular for blankets and throws because of its extreme softness. Minky fabric is generally made using polyester filament yarn woven into fabric using tricot knitting. Conventional minky fabric is difficult to use for quilting for a variety of reasons. These reasons include the fact that minky fabric is difficult to cut by hand into quilting sections and produces what is called cuddle dust in the quilting industry. After the minky fabric sections are cut and sewn together, the resulting seams between the minky fabric sections in the finished quilt tend to be uneven, giving an undesired squiggly appearance.
[0004] Additionally, the corners formed among adjoining minky fabric sections are not sharp, which is visually disfavored among quilt makers and consumers. The seams in quilts made with minky fabric tend to be much wider than when traditional fabrics are used. In fact, a Minky quilt can have seams as large as ½ inch, which is considered visually undesirable in the quilting industry. Minky fabric is also difficult to us for quilting because it is slippery compared with traditional fabrics. To control its slipperiness, the minky fabric sections must be pinned together to stabilize the sections in place before they are sewn, which adds a time-consuming step to the process of making the quilt. In fact, the sewing process itself is more challenging when minky fabric is used compared to traditional fabrics used for quilting.
[0005] For these reasons it is an object of the present invention to create a minky fabric that retains much of the softness of minky fabric while substantially reducing the characteristics of minky fabric that make it challenging to use for quilting. These and other objects are more fully described in the following specification and drawings.SUMMARY
[0006] The present invention is a modified minky fabric that overcomes the many difficulties encountered when using convention minky fabric for quilting yet retains much of the softness that is the hallmark of minky fabric. The present invention is much easier to cut than traditional minky fabric and reduces the amount of cuddle dust by as much as 75% compared with traditional minky fabric. The present invention reduces the slipperiness of traditional minky fabric to the point that the need to pin the fabric sections together before sewing is eliminated. This not only dispenses with a time-consuming pinning step, but it also permits for much greater creativity in the design of the quilt.
[0007] The seams and corners among adjoining fabric sections using the present invention are also much sharper when traditional minky fabric is used. In fact, the ½ inch seam needed when traditional minky fabric is used is reduced to ¼ inch when the present invention is used. The sewing process in forming the quilt is much easier using the present invention when compared with conventional minky fabric. Hence, the present invention meets a long felt, but unfulfilled need in the quilting industry.
[0008] In one embodiment, a method of manufacturing a quilting minky fabric includes warp knitting an in-greige a three-bar tricot fabric using a first guide bar and a second guide bar to form a ground layer with polyester FDY yarns and using a third guide bar to form a pile layer with polyester DTY yarn. The in-greige fabric is heat-set preferably at a temperature between 180 °C and 220 °C to produce a reduced width fabric. The reduced width heat-set fabric is dyed for between 35 and 45 minutes with a temperature rise rate of approximately 2 °C per minute. Thereafter, a softener is applied to the dyed reduced width heat-set fabric and hot-air drying the fabric at a temperature between 170 °C and 180 °C, and the pile of the fabric is raised in a quilting cuddle raising machine using a flexible raising fillet followed by a hard raising fillet.
[0009] In various embodiments the ground layer may use polyester 50 / 24 FDY SD yarns and the pile layer uses polyester 65 / 204 DTY yarns. The first guide bar is preferably operated at a rack / mm ratio of 1540, the second guide bar L2 is operated at a rack / mm ratio of 1200, and the third guide bar is operated at a rack / mm ratio of 3150. Preferably the pile layer is formed to a height of approximately 1.5 mm. In various other embodiments, the raising step may be performed in two stages that are repeated between 4 and 8 times. The cuddle raising machine preferably comprises raising rolls having a thickness of 65 mm, a raising drum having a diameter of 730 mm, and a roll-to-roll distance of 30 mm.
[0010] The fabric is polished between heated rollers at a temperature between 120 °C and 130 °C after the raising step, and the polished fabric is air tumbled at a temperature between 130 °C and 140 °C. Preferably the in-greige fabric has a density of 27 fibers per centimeter and a weight of 340 grams per yard, and the finished fabric has a width of 44-46 inches. Additionally, the fabric may comprise of 100% polyethylene terephthalate (PET) with constituent ratios of approximately 23% for the ground warp yarns of guide bar L1, 17.6% for the ground warp yarns of guide bar L2, and 59.4% for the pile yarns of guide bar L3.
[0011] In an alternative embodiment, a cuddle raising apparatus is disclosed for raising the pile of a warp-knitted minky fabric for quilting. The apparatus includes a central raising drum and a plurality of raising rolls arranged around the periphery of the raising drum. The warp-knitted minky fabric is preferably a three-bar tricot fabric comprising a ground layer of polyester FDY yarns and a pile layer of polyester DTY yarn. The warp-knitted minky fabric is heat-set at a temperature between 180 °C and 220 °C to produce a reduced width fabric. Preferably, each raising roll has a thickness of no greater than 65 mm, the raising drum has a diameter of no greater than 730 mm, and the distance between each of the plurality of raising rolls is no greater than 30 mm.
[0012] The plurality of raising rolls may be configured to receive a flexible raising fillet in a first stage and a hard raising fillet in a second stage. The apparatus may repeat the raising process between 4 and 8 times on the same warp-knitted minky fabric, and may include a polishing station positioned downstream of the raising rolls. The polishing station preferably includes heated rollers maintained at a temperature between 120 °C and 130 °C, and an air tumbling station may be provided downstream of the raising rolls, wherein the air tumbling station is configured to operate at a temperature of between 130 °C and 140 °C.
[0013] In various embodiments, the apparatus is preferably configured to process a warp-knitted tricot fabric having a 1.5 mm pile height, configured to receive fabric that has been heat-set from an original in-greige width greater than that of the fabric, and is configured to produce a finished fabric having a width between 44 inches and 46 inches and a pile density of approximately 27 fibers per centimeter. The apparatus is preferably configured to raise the pile of a fabric comprising 100% PET with a majority of the yarns forming the pile layer.BRIEF DESCRIPTION OF THE FIGURES
[0014] FIG. 1 illustrates various percentage ranges of the yarns used in the preparation of a modified minky fabric adapted for quilting.
[0015] FIG. 2 illustrates the details of FIG. 1 including the cone quantity, wale, width, and weight of the quilting minky fabric.
[0016] FIG. 3 illustrates a side elevation view of various yarn layers forming the quilting minky fabric.
[0017] FIG. 4 illustrates a cross-section of a raising drum surrounded by several raising rolls for raising the quilting minky fabric.DESCRIPTION
[0018] The present invention is described more fully hereinafter, but not all embodiments are shown. While the invention has been described with reference to exemplary embodiments, it will be understood by those skilled in the art that various changes may be made, and equivalents may be substituted for elements thereof without departing from the scope of the disclosure. In addition, many modifications may be made to adapt a particular structure or material to the teachings of the disclosure without departing from the essential scope thereof.
[0019] The drawings accompanying the application are for illustrative purposes only. They are not intended to limit the embodiments of the present application. Additionally, the drawings are not drawn to scale. Common elements between different figures may retain the same numerical designation.
[0020] The present invention is a quilting minky fabric having a 1.50 MM thickness. It is made in widths of 63 inches in-greige and 44 / 45″ finished fabric. It has a density of 27.0 fibers per centimeter and an in-greige weight of 340 grams per yard. It will be understood by one skilled in the art that these thicknesses, weights, and densities can vary within reasonable ranges and remain within the spirit of the invention.
[0021] Referring to FIG. 1, The chemical composition of one embodiment of the quilting minky fabric is shown. The chemical composition consists of 100% PET (polyethylene terephthalate), with the constituent ratio for each structure distributed as follows: 23% for item #1, 17.6% for item #2, and 59.4% for item #3.
[0022] Regarding items #1 and #2, FDY refers to fully drawn yarn, which is produced by spinning a polyester polymer (e.g., PET) at high speeds, followed by integrated stretching, orientation, and heat-setting crystallization. Unlike Partially Oriented Yarn (POY), which requires further drawing, or Draw Textured Yarn (DTY), which adds crimp for bulk and stretch, FDY is ready for direct use in weaving or knitting.
[0023] The 50 / 30 ratio refers to 50 denier and 30 filaments. Denier measures the linear mass density of the yarn (for example, the weight in grams of 9,000 meters of yarn). A 50 denier yarn means 9,000 meters weighs 50 grams, indicating relatively fine yarn, since a higher denier is a thicker, heavier yarn, while a lower denier is finer and lighter, as is commonly used in lightweight apparel, linings, or sheer fabrics. Having thirty filaments indicates the yarn consists of 30 individual continuous filaments twisted or bundled together. More filaments for a given denier generally produce a softer, silkier hand feel because each filament is finer (i.e., having a lower denier per filament, or DPF count). In this instance, the DPF of 50 / 30 is approximately 1.67, which is quite fine and contributes to smoothness by affecting drape, softness, and coverage.
[0024] The SD indicator refers to semi-dull, which refers to a yarn's luster or shine. Semi-dull polyester contains a small amount of titanium dioxide (TiO2, typically about 0.1-0.3%) as a delustrant. It reduces the natural gloss of bright yarn to a soft, natural sheen, similar to silk or cotton, without making it fully matte. Semi-dull contrasts with bright (BR) which lacks or has minimal delustrant for a high shine, often with circular or trilobal cross-sections, and full-dull (FD), having a higher amount of TiO2 (typically about 2-2.5%) for a very matte appearance. Semi-dull is popular due to its balanced look, good dyeability, and versatility in apparel and home textiles.
[0025] The P65 / 204 DTY is a polyester draw textured yarn (DTY) which is produced by taking a partially oriented yarn and simultaneously stretching and texturing it on a high-speed texturing machine using heat, twisting, and de-twisting. This process introduces permanent crimps, curls, loops and coils into the filaments, which gives the yarn bulkiness and volume for a fluffy appearance, good elasticity and stretch with recovery, a soft, cotton-like or woolly hand feel, and better cover and warmth compared to flat yarns.
[0026] The ratio of 65 / 204 refers to the denier and filament count. In this instance, 65 denier is a relatively fine yarn, which is lighter and thinner than common 150D DTY but thicker than ultra-fine options like 50D, and is suitable for lightweight, soft fabrics. A 204 filament count indicates the yarn consists of 204 individual continuous filaments. This high filament count relative to the denier results in very fine individual filaments, having a DPF of approximately 0.32, and producing an exceptionally soft, silky, and smooth touch with excellent drape and fabric coverage. Higher filament counts generally enhance softness and reduce the “plastic” feel of the yarn. The chain pattern is the particular manufacturer machine configuration and pattern settings for the particular yarn.
[0027] FIG. 2 illustrates the details of the warped knitting used to create the quilting minky fabric. Warp knitting is a machine-based textile production method in which multiple parallel yarns fed from warp beams run lengthwise in the warp direction and simultaneously form interlocking loops to create fabric. Unlike weft knitting, in which a single yarn travels horizontally forming one row at a time, warp knitting produces fabric with vertical loops interlocking in a chain-like pattern. This results in fabrics that are generally more dimensionally stable, holding their shape better after stretching or washing, and less prone to unraveling or running if a thread within the fabric breaks. Warped knitting also produces stronger and more durable fabric at high speeds in flat, wide sheets.
[0028] In the warp knitting process, numerous yarns are wound onto one or more warp beams, fed parallel to each other. Each yarn passes through a guide eye on a guide bar capable of moving along both an x and y axis in a precise, controlled lapping pattern. A row of needles across the machine width simultaneously forms loops from the yarns, wherein each needle typically works with an individual yarn. The x and y axis swinging movement creates overlaps around a particular needle and underlaps connecting to adjacent wales. The “chain pattern” referred to in FIG. 1 refers to these lapping patterns, or a mechanical chain of links or pattern drum controlling the guide bar movements on a knitting machine.
[0029] The measurement mm / 480c referred to in FIG. 2 refers to the number of courses, or horizontal rows of loops. A rack in warp knitting is a standard unit equal to 480 courses. Mm / 480c, or mm per rack, measures the warp run-in, which is the exact length of yarn fed from the beam for every 480 courses. This is a critical machine setting controlling fabric weight, density, tightness, and other properties. For example, higher than mm / 480c means more yarn is used, leading to a heavier and looser fabric.
[0030] Regarding the cones and beams referred to in FIG. 2, there are two main ways yarns engage the warp knitting machine, warp beams and cones. Warp beams provide continuous high-volume feeding with uniform tension across numerous ends. Multiple yarns are wound in parallel sheets onto flanged warp beams. Preparation involves transferring yarns from smaller supply packages onto the beam using a warping machine. A light oil or finish may be applied for better knitting performance. The beams are mounted on the knitting machine, and several beams may be used to cover the full width and simplify handling.
[0031] Cones are tapered, wound yarn packages, typically comprising plastic or paper cones, on which the FDY and DTY filament yarns are delivered from the manufacturer. During the warping process, hundreds of cones are placed on a large frame with pegs or holders, known as a “creel,” and yarns are drawn from these cones under controlled tension, passed through guides / combs, and wound parallel onto the warp beam. In smaller setups, yarns can feed directly from cones on a creel to the knitting machine, but as shown in in FIG. 2, beam feeding is far more common for efficiency in production. The total cone quantity refers to the total number of individual yarn cones required for a specific warp setup. It equals the total number of warp ends needed across all beams / guide bars.
[0032] Fine FDY, such as the 50 / 30 yarn as disclosed, is usually warped from cones onto beams for a smoother, stable feeding in warp knitting of linings, meshes, or base fabrics. Consistent cone quality ensures defect-free beams and high knitting efficiency.
[0033] Referring to FIG. 3, a side view of the minky fabric 10 is shown. The backing layer 12, comprising the FDY 50 / 36 SD yarns is the foundational woven structural base of the fabric. It consists of interlaced warp and weft yarns forming a stable base. Although a simple plain-weave is shown in the illustrated example, any structurally suitable base weave is contemplated. The backing layer 12 provides overall strength, dimensional stability, and a structural foundation for the rest of the fabric.
[0034] The pile layer 14, comprising individual P65204 DTY yarns, preferably has a 1.5 mm pile height. Between the backing layer 12 and the pile layer 14, a connection layer 16 of loops and anchors is provided. The connection layer 16 is an intermediate zone where the pile layer 14 yarns are mechanically locked into the backing layer 12. The connection layer 16 comprises portions of the pile yarns that pass through or around the backing weave, forming loops and anchors that secure the pile layer 14 to the backing layer 12 and prevent the pile from pulling out. The pile layer 14 comprises raised, upright pile tufts, giving the minky fabric 10 its characteristic height, texture, softness, and appearance. In one embodiment, each tuft may have a clean cut end at the top, to form a visible and tactile pile surface.
[0035] Once quilted fabric of the present invention is woven it must undergo a finishing process involving the following specialized steps: dyeing, softening, and raising. Initially, the in-greige or raw fabric, which is typically wider and less stable, is heat set. The fabric is passed through a hot oven or stenter at high temperature while its width is mechanically controlled by pins or clips on the edges. The temperature range is typically 180-220 °C. In one preferred embodiment 215 degrees Celsius is used. The heat setting process relaxes internal stresses in the polyester fibers, stabilizes the fabric's dimensions so it won't shrink or distort significantly during later washing, dyeing, or use, and sets the final shape, to improve crease resistance and enhance overall stability.
[0036] Preferably, the in-greige fabric is heat-set from 63 inches to 46 inches and polished to achieve a final width of 44-46 inches. Polishing refers to a mechanical finishing process which may be a calendaring or a light shearing step. The fabric is passed between heated or polished rollers under pressure, which smooths the fabric surface, increases sheen, and compacts the structure slightly to give it a softer, more luxurious hand feel. For pile fabrics, polishing helps align or lightly brush the pile, as further discussed below.
[0037] In the first specialized finishing step, the fabric is dyed to achieve a desired color. The dyeing process is run at a temperature of approximately 130±5 °C for 35 to 45 minutes at a rate of 2C / min temperature increase. In the second step, after the dyeing process is completed, the softener is treated with a softener concentration of between 2.0% and 5.0% under a temperature of between 170 °C and 180 °C for hot air drying. The softener is applied to enhance the fabric's feel.
[0038] The next specialized process is a raising process which lifts the fibers of the pile to create a denser, softer, and bulkier surface. The raising process causes the piles rise up from the high density short 1.5 mm piles after the above heat treatment. Due to the difficulty inherent in the raising process, the raising process occurs in two stages. the first stage uses a flexible raising fillet, and the secondary process uses a hard raising fillet. These stages are preferably repeated 4-8 times, and the final cutting is done by raising the pile rather than just one time raising fillet process of the regular minky fabrics. This way has the advantage of forming a dense and soft-touch.
[0039] The primary difference between the quilting cuddle raising machine of the present disclosure and a regular minky raising machine lies in the thickness of the raising roll, the diameter of the raising drum, and the distance roll to roll. In a regular minky raising machine the thickness of the raising roll is typically between 70 mm and 80 mm. The diameter of the raising drum is typically between 800 mm and 900 mm, and the distance, roll to roll, is approximately 44 mm. In contrast, the quilting cuddle raising machine has a raising roll thickness of 65 mm, a raising drum diameter of 730 mm, and a distance, roll to roll, of 30 mm.
[0040] Referring to FIG. 4, a cross section of several raising rolls 18 surrounding a raising drum 20 is shown according to the quilting cuddle raising machine. The raising rolls 18 are thinner and the gap between each roll is narrower than that of the general raising machine as specified above. This makes the piles very fine and dense when forming the pile during the pile removal process. After the raising process, polishing is done at a temperature range of 120-130 °C and add air tumbling process to form voluminous piles with the temperature in the range of 130-140 °C and includes a shearing process followed by a stenter process. The fillet is a crucial component of the raising rollers. It consists of specialized coverings that contain fine, hooked wires or abrasive surfaces responsible for effectively lifting the fibers of the pile.
[0041] Returning to the polishing step, heated rollers with grooves are used to impart shine to the pile, enhancing its appearance. Two processes during polishing include tumbling, which softens the fabric, enhances bulkiness, and creates a relaxed, slightly wrinkled texture, and tentering, a crucial mechanical finishing process that stretches and dries the fabric to a specific width while setting the fabric grain straight. To achieve a polished, voluminous, and soft quality with the short 1.5 mm pile, a volume-oriented softener is used after polishing.
[0042] A first polishing machine processing is done through a raising machine equipped with a flexible raising fillet wound on the raising roll. This initial step helps lift the fibers. A second polishing machine process is performed using a hard fillet wound on the polishing machine. This step adds bulkiness to the piles, raising them further. To achieve a polished, voluminous, and soft quality with the short 1.5 mm pile, a volume-oriented softener is used after polishing. After the secondary raising process, the fabric's piles are raised voluminously and then cut. The cutting process is essential for achieving the desired finish.
[0043] More detailed features of the above processing steps include the following: The present invention provides heat treatment, raising, dyeing, processing, and post-processing techniques for the lightweight, cost-effective and high quality 3-bar Tricot knitted quilting fabric and it relates to a method of a warp knitting process with a guide bar L1 and L2 forming a ground, and a guide bar L3 forming a pile.
[0044] The process of dyeing the warp knitted fabric at a temperature of 130 °C±5 °C for 35-45 minutes by raising the temperature at a rate of 1.5 C / min. Hot air treatment the occurs at a temperature of 160-170 with a softener at a concentration of 2-3% and brushed process after the heat treatment. Air Tumbling process after polishing to give the pile volume and softness. The Raising fillet used for the raising process has cross-used between the Flexible Type and Hard Type 4 times to 6 times to maximize the raising of the file by maximum.
[0045] The guide bar L1 forming the ground is made of polyester 50 / 24FDY, having a rack / mm ratio of 1540, and a chain pattern is 23-10 forming a total fabric ratio of 23%. The guide bar L2 uses polyester 50 / 24FDY, the rack / mm ratio is 1200 and the chain pattern is 10-12, with a ratio of 17.6%. Guide bar L3, which forms the pile, uses Polyester 65 / 204DTY, with a rack / mm ratio of 3150 and a chain pattern of 10-56 in a ratio of 59.4%.
[0046] The softener treatment is a 50:50 ratio with 2 percent softener that forms efficient pile raising and another 2% of a softener that imparts softness. The Ground organization is composed of polyester 50 / 24SD yarns, and the p is composed of polyester 65 / 204DTY yarns, having a courses per centimeter density in the range of 27±1, and a weight of 250 250±10 g / m2, and its shape stability is 1 ±0.5%.
[0047] The present invention is described above, but not all embodiments are shown. While the invention has been described with reference to exemplary embodiments, it will be understood by those skilled in the art that various changes may be made, and equivalents may be substituted for elements thereof without departing from the scope of the disclosure. In addition, many modifications may be made to adapt a particular structure or material to the teachings of the disclosure without departing from the essential scope thereof.
[0048] The descriptions of embodiments of the present invention have been presented only for purposes of illustration and description. They are not intended to be exhaustive or to limit the present invention to the forms disclosed. Accordingly, many modifications and variations will be apparent to practitioners skilled in the art. Additionally, the above disclosure is not intended to limit the present invention. The scope of the present invention is defined by the appended claim.
Claims
1. A method of manufacturing a minky fabric for quilting, comprising:warp knitting an in-greige a three-bar tricot fabric using a first guide bar and a second guide bar to form a ground layer with polyester fully drawn yarns (FDY) and using a third guide bar to form a pile layer with polyester draw textured yarn (DTY);heat-setting the in-greige fabric at a temperature between 180 C and 220 °C to produce a reduced width fabric;dyeing the reduced width heat-set fabric for between 35 and 45 minutes with a temperature rise rate of 2 °C per minute;applying a softener to the dyed reduced width heat-set fabric and hot-air drying the dyed reduced width heat-set fabric at a temperature between 170 C and 180 C; andraising the pile layer of the dyed reduced width heat-set fabric in a cuddle raising machine using a flexible raising fillet followed by a hard raising fillet.
2. The method of claim 1, wherein the ground layer uses polyester 50 / 24 FDY semi-dull yarns and the pile layer uses polyester 65 / 204 DTY yarns.
3. The method of claim 1, wherein the first guide bar is operated at a rack / mm ratio of 1540, the second guide bar is operated at a rack / mm ratio of 1200, and the third guide bar is operated at a rack / mm ratio of 3150.
4. The method of claim 1, wherein the pile layer is formed to a height of 1.5 mm.
5. The method of claim 1, wherein the raising step is performed in two stages that are repeated between 4 and 8 times.
6. The method of claim 1, wherein the cuddle raising machine comprises raising rolls having a thickness of 65 mm, a raising drum having a diameter of 730 mm, and a roll-to-roll distance of 30 mm.
7. The method of claim 1, further comprising polishing the dyed reduced width heat-set fabric between heated rollers at a temperature between 120 C and 130 °C after raising.
8. The method of claim 7, further comprising air tumbling the polished fabric at a temperature between 130 C and 140 °C.
9. The method of claim 1, wherein the in-greige fabric has a density of 27 fibers per centimeter and a weight of 340 grams per yard, and a finished fabric has a width of 44-46 inches.
10. The method of claim 1, wherein the in-greige fabric comprises 100% polyethylene terephthalate (PET) with constituent ratios of approximately 23% for ground warp yarns of a guide bar L1, 17.6% for ground warp yarns of a guide bar L2, and 59.4% for pile yarns of a guide bar L3.
11. A cuddle raising apparatus for raising a pile of a warp-knitted minky fabric for quilting, comprising:a central raising drum; anda plurality of raising rolls arranged around a periphery of the raising drum;wherein the warp-knitted minky fabric comprises is a three-bar tricot fabric comprising a ground layer of polyester fully drawn yarns (FDY) and a pile layer of polyester draw textured yarn (DTY);wherein the warp-knitted minky fabric is heat-set at a temperature between 180 C and 220 C to produce a reduced width fabric; andwherein each roll of the plurality of raising rolls has a thickness of no greater than 65 mm, the raising drum has a diameter of no greater than 730 mm, and a distance between each of the plurality of raising rolls is no greater than 30 mm.
12. The apparatus of claim 11, wherein the plurality of raising rolls is configured to receive a flexible raising fillet in a first stage and a hard raising fillet in a second stage.
13. The apparatus of claim 11, configured to repeat a raising process between 4 and 8 times on the warp-knitted minky fabric.
14. The apparatus of claim 11, further comprising a polishing station positioned downstream of the plurality of raising rolls.
15. The apparatus of claim 14, wherein the polishing station comprises heated rollers maintained at a temperature between 120 °C and 130 °C.
16. The apparatus of claim 11, further comprising an air tumbling station downstream of the plurality of raising rolls, the air tumbling station configured to operate at a temperature of between 130 °C and 140 °C.
17. The apparatus of claim 11, wherein the apparatus is configured to process a warp-knitted tricot fabric having a 1.5 mm pile height.
18. The apparatus of claim 11, wherein the apparatus is configured to receive a heat-set fabric that has been reduced from an original in-greige width greater than that of the heat-set fabric.
19. The apparatus of claim 11, wherein the apparatus is configured to produce a finished fabric having a width between 44 inches and 46 inches and a pile density of approximately 27 fibers per centimeter.
20. The apparatus of claim 11, wherein the apparatus is configured to raise the pile of a warp-knitted minky fabric comprising 100% polyethylene terephthalate (PET) with a majority of the yarns forming the pile layer.