Wooden structure load-bearing wall, construction method for wooden structure load-bearing wall, method for increasing wall magnification of wooden structure load-bearing wall, and gypsum-based load-bearing surface material

The use of a low-density gypsum-based load-bearing surface material with enhanced nail side resistance and specific nail fasteners addresses the challenge of increasing wall magnification in wooden load-bearing walls, improving shear strength and workability without additional reinforcing materials.

WO2024029210A9PCT designated stage expired Publication Date: 2024-10-24YOSHINO GYPSUM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/022235
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-30
Filing Date
2023-06-15
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing wooden load-bearing walls face challenges in increasing wall magnification without complicating the manufacturing process or deteriorating construction workability, particularly in reducing the effects of punching shear phenomenon and punch-out failure, especially when using conventional reinforcing materials like metal plates.

Method used

A low-density gypsum-based load-bearing surface material with increased nail side resistance and reduced surface density, combined with specific metal nail fasteners having a controlled area ratio, is used to enhance the wall magnification without the need for additional reinforcing materials, by increasing the compressive strength and initial stiffness of the load-bearing wall.

Benefits of technology

This approach effectively suppresses punching shear and punch-out failure, increasing the short-term standard shear strength and wall magnification while maintaining workability and reducing the self-weight and thickness of the load-bearing wall.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023022235_24102024_PF_FP_ABST
    Figure JP2023022235_24102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention increases the wall magnification of a wooden structure load-bearing wall without additionally attaching a reinforcing material or stiffener, and without increasing the specific gravity and / or sheet thickness of a gypsum-based surface material. A gypsum-based load-bearing surface material 10 for a wooden structure load-bearing wall is configured from: a main material or a core material comprising a plate-shaped gypsum cured body in which inorganic fibers and an organic-based strength-improving material are blended so as to exhibit a nail-side surface resistance of 500 N or greater; and a paper member covering at least front and back surfaces of the main material or core material. This load-bearing surface material: has a surface density that falls within a range of 6.5-8.9 kg / m2 and a compressive stiffness of 6.5 N / mm2 or greater; exhibits, in an in-plane shearing test of the load-bearing wall, an ultimate displacement (δu) greater than 20×10-3 rad and an initial stiffness (K) of 2.0 kN / 10-3 rad or greater; and raises a plasticity rate (μ) due to a reduction in yield point displacement (δv), not only the ultimate displacement. As a result, the wall magnification and short-term standard shear stiffness (P0) of the wooden structure load-bearing wall are effectively and efficiently increased.
Need to check novelty before this filing date? Find Prior Art

Description

Wooden structural shear wall, construction method for wooden structural shear wall, method for increasing the wall coefficient of wooden structural shear wall, and gypsum-based shear surface material

[0001] The present disclosure relates to a wooden shear wall, a construction method for a wooden shear wall, a method for increasing the wall factor of a wooden shear wall, and a gypsum-based shear face material. More specifically, the present disclosure relates to a wooden shear wall, a construction method for a wooden shear wall, a method for increasing the wall factor of a wooden shear wall, and a gypsum-based shear face material for a wooden shear wall, which increase nail lateral resistance and use a relatively low-density gypsum-based shear face material with a reduced surface density, and which can effectively reduce damage such as fracture or breakage of nailed portions without additionally attaching reinforcing or stiffening materials such as metal plates.

[0002] Generally, construction methods for wooden buildings are broadly divided into wooden frame construction and wooden frame wall construction. Due to the impact of recent large-scale earthquakes, research on the seismic resistance of wooden buildings has been attracting particular attention in Japan in recent years. As described in Patent Document 1 (International Publication WO 2019 / 203148 A1), in architectural design practice in Japan, the effective frame length of a shear wall (the length of the wall in the architectural plan) is generally used as an indicator of the strength of a wooden building against short-term horizontal loads (seismic force, wind pressure, etc.). A wall factor appropriate to the structure of the shear wall is used to calculate the frame length. The wall factor is an indicator of the seismic performance or strength performance of the shear wall, and the higher the value, the greater the seismic strength. A wall structure with a high wall factor is advantageous in improving the design flexibility and seismic resistance of the entire building.

[0003] The wall multipliers for general-purpose wooden shear walls, which have been used in Japan for many years, are specified in Article 46 of the Building Standards Act Enforcement Order, Ministry of Construction Notification No. 1100 (June 1, 1981), and Ministry of Land, Infrastructure, Transport and Tourism Notification No. 1541 (October 15, 2001). However, for many of the shear walls that do not fall under these general-purpose wall structures, the wall multiplier must be determined based on the certification of the Minister of Land, Infrastructure, Transport and Tourism as specified in Article 46, Paragraph 4, Table 1 (viii) of the Building Standards Act Enforcement Order. Therefore, the wall multipliers for the relatively large number of wooden shear walls constructed in recent years must be determined based on performance tests conducted by designated performance evaluation organizations. The test methods for these performance tests are described in detail in the "Wooden Shear Walls and Their Multipliers: Performance Testing and Evaluation Service Manual" published by each testing and inspection organization.

[0004] Patent Document 1 describes a panel reinforcement method for increasing the ultimate displacement and wall ratio of a shear wall by arranging reinforcing materials or stiffeners, such as metal plates, in nailed sections to prevent damage or fracture of the nailed sections. Wooden shear walls using such reinforcing materials or stiffeners are thought to be able to build wooden shear walls with relatively high wall ratios by increasing the ultimate displacement and other properties through improved toughness and deformation compliance of the shear wall, without relying on increasing the maximum load the shear wall can withstand. However, shear wall structures using such reinforcing materials or stiffeners to increase the ultimate displacement and other properties require an additional step of attaching the reinforcing materials or stiffeners to the surface of the shear wall during the shear wall construction process. This step can complicate the manufacturing process of gypsum-based shear walls or reduce the workability of construction work.

[0005] On the other hand, "structural gypsum board" is known as a gypsum-based surface material that can be suitably used as a bearing surface material for wooden structural shear walls. "Structural gypsum board" is a gypsum-based surface material that enhances the lateral nail resistance of "reinforced gypsum board" based on the applicant's technology described in Patent Publication No. 5642948 (Patent Document 2). The lateral nail resistance is the shear strength or shear strength of the nailed portion of the surface material measured by the lateral nail resistance test specified in JIS A 6901. Since the lateral nail resistance is described in relatively detail in Patent Publication No. 7012405 (Patent Document 3) filed by the applicant, further detailed description will be omitted. However, the lateral nail resistance is a physical property proposed by the applicant in Patent Publication No. 2 as a strength evaluation factor for gypsum-based bearing surface materials, and is one of the strength factors that the applicant has particularly focused on in recent years.

[0006] Structural gypsum board (GB-St) is a gypsum-based surface material that has improved overall strength as a bearing surface material compared to (ordinary) gypsum board (GB-R) and improved lateral nail resistance compared to reinforced gypsum board (GB-F). Currently, structural gypsum board is specified in JIS A 6901 as a gypsum-based surface material with a lateral nail resistance of 750 N or more (Type A) or 500 N or more (Type B). Wood-frame shear walls using structural gypsum board as a bearing surface material exhibit a relatively high wall ratio compared to wood-frame shear walls using (ordinary) gypsum board or reinforced gypsum board as a bearing surface material. On the other hand, like reinforced gypsum board, structural gypsum board requires a thickness of 12.5 mm or more and a specific gravity of 0.75 or more. Therefore, wood-frame shear walls to which structural gypsum board is fixed have a strength of at least approximately 9.4 kg / m. 2 The surface density or surface weight (mass of load-bearing surface material per unit area of ​​wall surface (hereinafter referred to as "surface density")) is required.

[0007] Patent Document 3 (Patent Publication No. 7012405) describes a gypsum-based bearing surface material that provides a bearing wall with a short-term standard shear strength (P0) equivalent to that of structural gypsum board, but has a lower surface density than structural gypsum board. The gypsum-based surface material described in Patent Document 3 is composed of a main or core material made of a plate-shaped gypsum hardened body that is blended with inorganic fiber and an organic strength-improving material so as to exhibit a nail lateral resistance of 500 N or more, and a paper member that covers at least the front and back surfaces of the main or core material, and has a strength of 6.5 to 8.9 kg / m 2 The gypsum-based facing material of Patent Document 3 has an areal density within the range of 0.01 mm. The gypsum-based facing material of Patent Document 3 can provide a relatively high wall factor to a shear wall even when the board thickness is less than 12 mm. This gypsum-based facing material (hereinafter referred to as a "low-density gypsum-based shear wall material") was developed with the intention of reducing the surface density and weight of the facing material compared to conventional gypsum-based shear wall materials such as structural gypsum boards, while suppressing a decrease in yield strength through relatively high nail lateral resistance. This low-density gypsum-based shear wall material increases the ultimate displacement of the shear wall, thereby increasing the shear wall's plasticity factor, and thereby increasing the shear wall's wall factor. Therefore, it is possible to provide a gypsum-based shear wall material that is extremely practically advantageous from the viewpoint of achieving the desired strength of a wooden shear wall while also being lightweight and easy to install.

[0008] In this specification, the term "gypsum-based load-bearing surface material" is used to include not only (ordinary) gypsum board, reinforced gypsum board, and structural gypsum board as defined in JIS A 6901 ("gypsum board products"), but also gypsum-based surface materials in which the outer surface or outer layer of a gypsum core portion (core material portion) made primarily of gypsum is covered with a paper member such as gypsum board base paper, such as the above-mentioned low-density gypsum-based load-bearing surface material (Patent Document 3) and the gypsum-based load-bearing surface material described in Patent Publication No. 6412431 (Patent Document 4).

[0009] International Publication WO2019 / 203148A1 Patent No. 5642948 Publication Patent No. 7012405 Publication Patent No. 6412431 Publication

[0010] Allowable Stress Design of Wooden Frame Construction Houses [1] (2017 Edition), pages 63 and 300

[0011] The inventors of the present invention have repeatedly conducted the above-mentioned performance tests to further increase the wall factor for a shear wall using the low-density gypsum-based shear face material proposed in Patent Document 3, and as a result have recognized that it is possible to further increase the wall factor by preventing phenomena such as punching-out failure and edge breakage due to the punching shear phenomenon. It is believed that destruction or breakage of the nailed portion, such as punching-out failure, can be prevented by arranging a reinforcing material or stiffening material, such as a metal plate, in the nailed portion, as in the face material reinforcing method described in Patent Document 1, for example.

[0012] However, as mentioned above, if a process for additionally attaching such reinforcing or stiffening materials to the surface of the load-bearing panel is added to the panel manufacturing process, or if such a process is additionally performed during the construction of a wooden load-bearing wall, it is expected that the manufacturing process for gypsum-based panel materials will become more complicated or that the workability of construction work will deteriorate.

[0013] The present disclosure has been made in consideration of the above circumstances, and its purpose is to provide a wooden structural shear wall and its construction method, a method for increasing the wall multiplier of a wooden structural shear wall, and a gypsum-based shear surface material that uses a low-density gypsum-based shear surface material with increased nail lateral resistance and reduced surface density, which suppresses the punching shear phenomenon or reduces the effect of punching-out destruction without the need to additionally attach reinforcing or stiffening materials such as metal plates, thereby suppressing or reducing the effect of destruction or breakage in the nailed parts and further increasing the wall multiplier.

[0014] In order to achieve the above object, the present disclosure provides a wooden structural shear wall having a structure in which a gypsum-based shear face material is fastened to a wooden structural wall substrate of a wooden frame construction method or a wooden frame wall construction method with fasteners, wherein the shear face material is composed of a main material or core material made of a plate-shaped gypsum hardened body and paper members covering at least the front and back surfaces of the main material or core material, and the shear face material has an areal density or surface weight of 6.5 to 8.9 kg / m, which is specified as the mass per unit area of ​​the wall surface. 2 and having an areal density or areal weight within the range of 500 N or more and a nail lateral resistance of at least 6.5 N / mm 2The fastener is made of a metal nail having a head and a body, and the area ratio of the head area to the cross-sectional area of ​​the body is set to a value within the range of 6 to 13, and the ultimate displacement of the bearing wall measured by an in-plane shear test using a bearing wall specimen with a wall length of 1.82 m is 20 x 10 -3 The present invention provides a wood structural shear wall characterized by having an ultimate displacement (δu) greater than rad.

[0015] The present disclosure also provides a construction method for wooden structural bearing walls in which a gypsum-based bearing surface material is fixed to a wooden structural wall substrate of a wooden frame construction method or a wooden frame wall construction method, the method comprising: a gypsum-based bearing surface material comprising a main material or core material made of a plate-shaped gypsum hardened body and a paper member covering at least the front and back surfaces of the main material or core material, and a surface density or surface weight specified as the mass per unit area of ​​the wall surface of 6.5 to 8.9 kg / m 2 and having an areal density or areal weight within the range of 500 N or more and a nail lateral resistance of at least 6.5 N / mm 2 A gypsum-based bearing surface material having a compressive strength of 1.82 m or more is fastened to the wooden structural wall substrate with fasteners, and as the fasteners, metal nails are used in which the area ratio of the head area to the cross-sectional area of ​​the body is set to a value within the range of 6 to 13. The ultimate displacement (δu) of the bearing wall measured by an in-plane shear test using a bearing wall specimen having a wall length of 1.82 m is 20 x 10 -3 The present invention provides a construction method for wooden structural shear walls, characterized by constructing wooden structural shear walls that exhibit an ultimate displacement greater than rad.

[0016] Preferably, the nail has a head diameter within the range of 6.0 to 10.0 mm and a trunk diameter within the range of 2.0 to 5.0 mm. More preferably, the nail has a head diameter within the range of 6.8 to 9.0 mm and a trunk diameter within the range of 2.2 to 4.2 mm, and the area ratio of the head area to the cross-sectional area of ​​the trunk (hereinafter referred to as the "area ratio of the head area to the cross-sectional area of ​​the trunk") is set to a value within the range of 7 to 11. Preferably, the trunk of the nail is a straight, smooth trunk having a uniform circular cross-section and is equipped with a spire-shaped tip, and the head of the nail is a flat or mesh-shaped head having a circular contour in top view, and has an annular, flat seating surface that seats on the outer surface of the load-bearing face material by nailing, and a flat top surface that is constructed so as to be located after nailing in substantially the same plane as the wall surface formed by the outer surface of the load-bearing face material.

[0017] Preferably, the gypsum-based bearing surface material is made by mixing inorganic fibers and organic strength improving materials into the main material or core material to ensure the minimum physical properties required for a gypsum-based bearing surface material (nail side resistance: 500 N or more), while the surface density of the surface material is rather reduced to a relatively low value (6.5 to 8.9 kg / m 2 ) is set. For example, the amount of inorganic fiber to be blended is 0.3 to 5 parts by weight, preferably 2 to 4 parts by weight, per 100 parts by weight of calcined gypsum. Examples of inorganic fibers to be blended include glass fiber and carbon fiber. When glass fiber is used, glass fiber having a diameter of 5 to 25 μm and a length of 2 to 25 mm can be suitably used. Furthermore, the amount of organic strength-improving material to be blended is 0.3 to 15 parts by weight, preferably 1 to 13 parts by weight, per 100 parts by weight of calcined gypsum. Suitable examples of organic strength-improving materials include starch, polyvinyl acetate, polyvinyl alcohol, and polyacrylic. Both unmodified starch and modified starch can be used as the starch. Examples of modified starch include starch that has been subjected to physical, chemical, or enzymatic treatment. Suitable examples of physically treated starch include pregelatinized starch. Suitable chemically treated starches include oxidized starch, phosphated starch, urea phosphated starch, hydroxypropylated phosphate cross-linked starch, hydroxyethylated starch, hydroxypropylated starch, cationized starch, and acetylated starch.

[0018] In the following description of this specification, "minimum physical properties required for a gypsum-based load-bearing facing material" refers to a nail lateral resistance of 500 N or more. Factors known to vary the compressive strength of a gypsum-based load-bearing facing material include the mixing state of the gypsum slurry (mixing time, mixing temperature, etc.), the type and amount of impurities contained in the gypsum raw material, the cross-sectional properties, density, uniformity, etc. of the gypsum core, the amount, size, and dispersion state of air bubbles contained in the gypsum core, the water content or moisture content of the gypsum core, and the specific gravity of the gypsum core. While these factors may be used as control factors to increase or decrease compressive strength, they are not only closely related to the manufacturing conditions (type of gypsum raw material, type and amount of additives such as foaming agent, temperature of the mixing water, air temperature, humidity, etc.), but also relate to the overall quality of the gypsum core, and are often associated with a relatively low areal density (6.5 to 8.9 kg / m). 2 At a surface density within the range of 6.5 N / mm 2 The organic strength-enhancing agent is not a controlling factor of a property that can be used specifically for a specific application, that is, to provide a gypsum-based load-bearing facing with a desired compressive strength (a compressive strength of 500 N or more) and, moreover, to provide a gypsum-based load-bearing facing with a desired nail lateral resistance (a nail lateral resistance of 500 N or more) in cooperation with inorganic fibers. On the other hand, the organic strength-enhancing agent can be used specifically for such an application, and can be added to the gypsum slurry during the manufacturing process, providing a practical and effective means for increasing the compressive strength of the gypsum core.

[0019] The surface density value of the gypsum-based load-bearing surface material according to the present disclosure (6.5 to 8.9 kg / m 2 ) is the surface density of conventional gypsum-based load-bearing surface materials such as structural gypsum boards (approximately 9.4 kg / m 2) is a value significantly smaller than the above. Such an areal density allows the specific gravity and / or thickness of the gypsum-based load-bearing surface material to be reduced, thereby reducing the weight of the load-bearing wall or reducing the wall thickness. On the other hand, such a reduction in areal density is contrary to the conventional wall factor increase method that increases the short-term standard shear strength (P0) and wall factor of the load-bearing wall (i.e., the conventional wall factor increase method that increases the maximum strength (Pmax) by increasing the specific gravity and / or thickness, thereby increasing the short-term standard shear strength (P0)). However, as described in Patent Document 3, if the surface density is reduced while maintaining the minimum physical properties (nail lateral resistance: 500 N or more) of a gypsum-based load-bearing surface material, the toughness and deformation compliance inherent in the gypsum-based load-bearing surface material become apparent in the plastic region, and as a result, the ultimate displacement (δu) and plasticity factor (μ) of the load-bearing wall actually increase, which increases the ultimate strength (corrected value) (Pu') of the load-bearing wall.This can increase the short-term standard shear strength (P0) and wall factor without necessarily increasing the maximum strength (Pmax).

[0020] Furthermore, the inventors have found through many experiments that the initial stiffness (K) of a bearing wall increases as the compressive strength of a gypsum-based bearing surface material increases. Based on this finding, and as a result of extensive research, they have found that the compressive strength of a gypsum-based bearing surface material increases to 6.5 N / mm 2 It was realized that increasing the initial stiffness (K) of the shear wall to the above value would increase its yield point displacement (δv) without significantly decreasing the ultimate displacement (δu) of the shear wall, and as a result, the ductility factor (μ) could be increased relatively significantly.

[0021] That is, according to the present disclosure, the compressive strength of the gypsum-based bearing surface material is 6.5 N / mm 2 The initial stiffness (K) of the bearing wall is increased to the value above (preferably) 2.0 kN / 10 -3 rad or more, thereby increasing the value of the yield point displacement (δv) to, for example, 7.2 × 10 -3 rad or less, coupled with a relatively high value of ultimate displacement (δu), the value of the plasticity factor (μ) can be relatively greatly increased, and as a result, a value of, for example, 7.7 kN or more can be relatively easily secured as the ultimate proof stress correction value (Pu').

[0022] Incidentally, in the case of a bearing wall using a low-density gypsum-based bearing surface material in Patent Document 3, the initial stiffness (K) is 2.0 kN / 10 -3 rad (e.g., 1.9 kN / 10 -3 rad). The structural gypsum board described above is a gypsum-based bearing surface material that was developed to increase the lateral nail resistance as desired, focusing on a strength factor known as lateral nail resistance, in order to suppress tearing failure of the gypsum-based bearing surface material due to changes in the relative position between the gypsum-based bearing surface material and fasteners that may occur during vibration. The low-density gypsum-based bearing surface material of Patent Document 3 is intended to increase the ductility factor (μ) and ultimate strength (corrected value) (Pu') by reducing the surface density while maintaining the desired lateral nail resistance, thereby demonstrating the toughness and deformation followability of the gypsum-based bearing surface material in the plastic region. However, neither of these documents focuses on or considers the compressive strength of the gypsum-based bearing surface material or the initial stiffness generated in the elastic region as strength-improving factors, nor does it examine or study the structural relationship between the initial stiffness of a bearing wall and the compressive strength of the gypsum-based bearing surface material.

[0023] On the other hand, according to experiments by the present inventors, although increasing the areal density can increase the compressive strength as desired, increasing the areal density not only increases the weight of the face material but also tends to reduce the ultimate displacement, so it is desirable to increase the compressive strength to an appropriate value mainly by utilizing the compressive strength-increasing effect of organic strength-improving materials, etc. In other words, in the present disclosure, the compressive strength is set as desired mainly by setting an appropriate areal density and the compressive strength-increasing effect of blending an organic strength-improving material, etc.

[0024] Preferably, the yield point displacement (δv) of the bearing wall measured by an in-plane shear test is 7.2 × 10 -3 rad or less, or the initial stiffness (K) is set to 2.2 kN / 10 -3 rad or more and the yield point displacement (δv) is 7.2 × 10 -3 rad or less, 7.5N / mm 2 For example, in the gypsum-based bearing surface material according to the present disclosure, the yield point displacement (δv) is 6.0 × 10 -3rad, initial stiffness (K) = 2.5kN / 10 -3 rad, ultimate strength Pu = 15.0 kN, ultimate displacement (δu) = 30 × 10 -3 rad, plasticity factor (μ) = 5.0, and variation coefficient β = 1.0, the ultimate strength (corrected value) (Pu') is 9.0 kN. On the other hand, if the initial stiffness (K) is 1.9 kN / 10, as in the case of the low-density gypsum-based bearing surface material (Patent Document 3), -3 rad (<2.0kN / 10 -3 rad), the ultimate strength Pu = 15.0, the ultimate displacement (δu) = 30 × 10 -3 rad, and even if the variation coefficient β is 1.0, the yield point displacement (δv) is 7.8 × 10 -3 rad, ductility factor (μ) = 3.8, and the ultimate strength (corrected value) (Pu') is only about 7.7 kN. In other words, by increasing the compressive strength of the bearing face material and increasing the initial stiffness (K), the ultimate strength (corrected value) (Pu') increases relatively significantly, and the short-term standard shear strength (P0) and wall factor can also be increased relatively significantly.

[0025] In the present disclosure, the compressive strength is preferably 7.5 to 13.0 N / mm 2 More preferably, a value in the range of 8.0 N / mm 2 In the present disclosure, the initial stiffness is preferably set to a value equal to or greater than 2.2 kN / 10 -3 rad~4.0kN / 10 -3 rad, more preferably 2.4 kN / 10 -3 Further, according to the present disclosure, the yield displacement (δv) may be set to a value equal to or greater than 3.5×10 -3 rad ~ 7.2 x 10 -3 rad, more preferably 6.5 x 10 -3 It can be set to a value equal to or less than rad.

[0026] According to a preferred embodiment of the present disclosure, a bearing wall equipped with a gypsum-based bearing surface material has a plasticity factor (μ) of 4.2 or more and 10.0 or less, preferably 4.3 or more, measured by an in-plane shear test, and a yield strength (Py) of 7.7 kN or more, which is greater than the corrected ultimate strength (Pu'), preferably 8.0 kN or more, measured by an in-plane shear test. Furthermore, according to experiments conducted by the present inventors, as the initial stiffness (K) increases, the yield strength (Py) also tends to increase. Therefore, as with the low-density gypsum-based bearing surface material (Patent Document 3), the yield strength (Py) is generally greater than the corrected ultimate strength (Pu').

[0027] Thus, the gypsum-based shear surface material of the present disclosure not only ensures the minimum physical properties required for a gypsum-based shear surface material, but also increases the ultimate strength (corrected value) (Pu') by improving the toughness and deformation compliance of the gypsum-based shear surface material in the plastic region due to the reduced surface density, and further increases the ultimate strength (corrected value) (Pu') by increasing the initial stiffness (K) and decreasing the yield point displacement (δv).As a result, it is possible to relatively significantly increase the short-term standard shear strength (P0) and wall factor of a wooden structural shear wall without attaching additional reinforcing or stiffening materials such as metal plates, and without increasing the surface density of the gypsum-based shear surface material. According to the present disclosure, metal nails with a head area / body area ratio set to a value within a range of 6 to 13 are used as fasteners to fasten such gypsum-based shear panels to wooden structural wall substrates. This effectively suppresses or reduces punch-out failure without the need for additional reinforcing or stiffening materials such as metal plates. This, combined with the above-described effects of the gypsum-based shear panel, further effectively and efficiently increases the short-term standard shear strength (P0) and wall ratio of the wooden structural shear wall. Furthermore, similar to structural gypsum boards and the aforementioned low-density gypsum-based shear panel (Patent Document 3), the shear panel has at least the front and back surfaces of the main or core material covered with paper components, allowing it to be easily manufactured on conventional gypsum board production lines. Preferably, the gypsum-based shear panel of the present disclosure has a laminated structure in which the surface or surface layer of the core material is covered with gypsum board base paper. The "front and back surfaces" refer to the front and back surfaces of the face material excluding the end faces or side surfaces of the end edges and side edges (i.e., the four outer edges) of the face material.

[0028] Preferably, the thickness of the gypsum-based bearing surface material is set to a value of 7.5 mm or more and less than 12 mm (more preferably, a value of 8.5 mm or more and 10 mm or less), for example, 9.5 mm or 9.0 mm. Gypsum-based bearing surface materials with such a thickness are advantageous in terms of reducing the wall thickness of wooden structural bearing walls, compared to structural gypsum boards that require a thickness of 12 mm or more. Optionally, the gypsum hardened body has a nail lateral resistance of 980 N or less.

[0029] Preferably, the gypsum-based bearing surface material has an ultimate displacement (δu) of the bearing wall measured by an in-plane shear test using a bearing wall specimen having a wall length of 1.82 m of 24 x 10 -3 rad or more (preferably 26 x 10 -3 rad or more) in the shear wall. The value of the ultimate displacement (δu) set to a relatively high value, coupled with the increase in the initial stiffness (K) of the shear wall and the decrease in the yield displacement (δv), results in a relatively large increase in the value of the plasticity factor (μ), and is therefore extremely advantageous in increasing the short-term standard shear strength (P0) and wall magnification factor. The ultimate displacement (δu) of a shear wall is an index showing the ductility and deformation followability of the shear wall in the plastic range. According to the "Wooden Shear Walls and Their Magnification Factors Performance Testing and Evaluation Procedure Manual," if the load does not decrease and the ultimate displacement value cannot be obtained even when the in-plane shear test exceeds 1 / 15 rad, the ultimate displacement (δu) is set to 1 / 15 rad. Therefore, the maximum value of the ultimate displacement (δu) is 1 / 15 rad (66.7 x 10 -3 rad).

[0030] Preferably, the specific gravity of the gypsum-based bearing surface material is set to a value within the range of 0.65 to 0.96, preferably a value within the range of 0.7 to 0.9 (more preferably a value within the range of 0.7 to 0.8). A gypsum-based bearing surface material with such a specific gravity has a board thickness of less than 12 mm but a specific gravity of 1.0 or more, and therefore can be made lighter than the gypsum-based bearing surface material of Patent Document 4, which has a relatively large weight (for example, "EX Board" (product name) manufactured by Yoshino Gypsum Co., Ltd.). This is advantageous for reducing the weight of wooden bearing walls or improving the workability of wooden bearing walls or the workability of their construction.

[0031] In a preferred embodiment of the present disclosure, the core material (gypsum core portion) of the gypsum-based load-bearing facing material contains an organopolysiloxane compound as a load-bearing deterioration inhibitor that mainly prevents load-bearing deterioration. This load-bearing facing material, like the gypsum-based load-bearing facing material described in Patent Document 4, can be applied to the exterior wall surface of a wooden exterior wall.

[0032] From another perspective, the present disclosure provides a method for increasing the wall coefficient of a wooden structural shear wall, which is constructed by fastening a gypsum-based shear face material to a wooden structural wall substrate of a wooden frame construction method or a wooden wall frame construction method with fasteners, comprising: forming the shear face material from a main material or core material made of a plate-shaped gypsum hardened body and paper members covering at least the front and back surfaces of the main material or core material; and increasing the surface density or surface weight of the shear face material, specified as the mass per unit area of ​​the wall surface, to 6.5 to 8.9 kg / m 2 and the bearing surface material has a nail side resistance of 500 N or more and a nail side resistance of 6.5 N / mm 2 The composition of the gypsum hardened body of the main material or the core material is set so as to exhibit a compressive strength of 20×10 or more, and as the fasteners, metal nails are used in which the area ratio of the head area to the cross-sectional area of ​​the body is set to a value within a range of 6 to 13, thereby suppressing the punching shear phenomenon or reducing the effect of punching-out destruction, and the ultimate displacement (δu) of the bearing wall measured by an in-plane shear test using a bearing wall specimen with a wall length of 1.82 m is 20×10 -3 The present invention provides a method for increasing the wall load-bearing factor of a wooden structural wall, characterized by obtaining an ultimate displacement greater than rad.

[0033] This method of increasing the wall factor reduces the areal density of the gypsum-based shear wall by reducing its specific gravity and / or thickness, thereby reducing the weight of the shear wall or its wall thickness. Furthermore, as described above, this method not only improves the toughness and deformation compliance (in the plastic region) of the gypsum-based shear wall by reducing its density, thereby increasing the ultimate displacement (δu). Furthermore, the increased compressive strength of the gypsum-based shear wall increases the initial stiffness (K) of the shear wall, thereby reducing the yield point displacement (δv). As a result, the synergistic effect of the relatively small yield point displacement (δv) and the relatively large ultimate displacement (δu) significantly increases the plasticity factor (μ = δu / δv). This allows the ultimate strength (corrected value) (Pu') of a wooden shear wall to be relatively easily achieved.

[0034] The present disclosure further provides a gypsum-based load-bearing surface material for wooden structural bearing walls, which is used in the above-mentioned construction method or the above-mentioned wall coefficient increasing method and is fastened to a wooden structural wall substrate of a wooden frame construction method or a wooden frame wall construction method by the above-mentioned fastener, and which exhibits a nail lateral resistance of 500 N or more and has a nail lateral resistance of at least 6.5 N / mm 2 It has a compressive strength of 6.5 to 8.9 kg / m 2 and in cooperation with the fasteners, the ultimate displacement (δu) of the bearing wall measured by an in-plane shear test using a bearing wall specimen having a wall length of 1.82 m is 20 x 10 -3 rad.

[0035] The gypsum-based shear facing material disclosed herein improves the toughness and deformation compliance of shear walls by using a low-density gypsum-based shear facing material with reduced areal density. For shear walls constructed by fastening the shear facing material to a wooden wall substrate with fasteners, the initial stiffness (K) is increased, reducing the yield point displacement (δv), thereby increasing the plasticity factor (μ = δu / δv) and increasing the short-term shear strength (P0) and wall ratio. The gypsum-based shear facing material disclosed herein can be effectively used as a shear facing material to further increase the short-term shear strength (P0) and wall ratio without increasing the wall thickness or weight, particularly for shear walls in which the ultimate displacement (δu) is difficult to increase easily or that are already experiencing an ultimate displacement (δu) close to its upper limit. Furthermore, since the gypsum-based load-bearing surface material of the present disclosure has at least the front and back surfaces of the main material or core material covered with paper members, it can be easily manufactured on a conventional gypsum board manufacturing line.

[0036] According to the disclosed wooden structural shear wall and construction method equipped with such a gypsum-based shear surface material, and further, the method for increasing the wall factor of a wooden structural shear wall, which is configured by fastening such a gypsum-based shear surface material to the wooden structural wall base of a wooden post-and-beam construction method or a wooden frame wall construction method with fasteners, by using metal nails having specific dimensions and shapes (head diameter D, body diameter d, and head area / body cross-sectional area ratio η) as fasteners, punching-out failure of the gypsum-based shear surface material can be effectively suppressed or its effect can be mitigated, thereby making it possible to relatively significantly improve the short-term allowable shear strength (Pa) and the wall factor. That is, according to the present disclosure, in a wooden structural shear wall and a construction method thereof, and further in a method for increasing the wall factor of a wooden structural shear wall, it is possible to further increase the short-term standard shear strength (P0) and wall factor of the shear wall without additionally attaching reinforcing or stiffening materials such as metal plates, without increasing the areal density (specific gravity and / or plate thickness) of the gypsum-based surface material (thus without increasing the weight and / or wall thickness of the shear wall), and without further increasing the value of the ultimate displacement (δu).

[0037] Furthermore, according to the shear wall structure of a wooden structure building or its construction method, or the shear wall construction method of the present disclosure, by using such gypsum-based shear face material as a shear face material in a wooden structure shear wall, the surface density of the gypsum-based shear face material can be reduced without reducing (or effectively increasing) the short-term standard shear strength (P0) and wall factor, thereby reducing the weight of the shear wall or reducing the wall thickness, or improving the workability of the shear wall.

[0038] Furthermore, according to the load-bearing wall structure of a wooden building or its construction method, or the method for increasing the wall factor according to the present disclosure, the initial stiffness (K) is increased to reduce the yield point displacement (δv), thereby increasing the ultimate strength (corrected value) (Pu') and increasing the short-term standard shear strength (P0) and wall factor. Therefore, it becomes possible to increase the wall factor without relying on reinforcement or stiffening using reinforcing or stiffening materials such as metal plates added to the gypsum-based surface material, without relying on an increase in the specific gravity and / or plate thickness of the gypsum-based surface material, and without relying heavily on an increase in the value of the ultimate displacement (δu).

[0039] 1 is a front view schematically illustrating an embodiment of a shear wall of a wooden building according to the present disclosure. It is a partial cross-sectional view and a partially cutaway perspective view of a shear wall showing, on a partially enlarged scale, a portion where a gypsum-based shear panel is fixed to a wooden framework by a nail. It is a front view, a cross-sectional view, and a side view showing the configuration of a shear wall specimen used in an in-plane shear test of the shear wall structure shown in FIG. 1. It is a diagram showing, for reference, the envelope of the load-deformation angle curve (shown by a solid line) obtained by an in-plane shear test of an arbitrary wooden framework shear wall, and a linear graph in which the envelope of the load-deformation angle curve is converted into the load-deformation angle characteristics of a perfectly elastic-plastic model, shown by a dashed-dotted line. It is a table showing the head diameter, body diameter, and head area / body cross-sectional area ratio for nails constituting a shear wall according to an embodiment of the present disclosure and two types of nails that have traditionally been used to fasten gypsum-based shear panel to the framework or framing of a wooden structure. 5A and 5B are diagrams and graphs comparing the results of in-plane shear tests on wooden structural shear walls using two types of conventional nails (Comparative Examples 1 and 2) shown in FIG. 5A and 5B are diagrams and graphs comparing the results of in-plane shear tests on wooden structural shear walls using the conventional nails (Comparative Example 3) shown in FIG. 5A and 5B are diagrams and graphs comparing the results of in-plane shear tests on wooden structural shear walls using the nails of this embodiment shown in FIG. 5A and 5B are diagrams showing the physical properties, composition, and strength test results of gypsum-based shear face materials constituting the present disclosure as Reference Examples 1 to 4, and the physical properties, composition, and strength test results of gypsum-based shear face material according to Comparative Example 4A and 5B are diagrams showing the test results of in-plane shear tests on shear wall structures as load-deformation angle characteristics of a perfectly elastic-plastic model for Reference Examples 1 to 4 and ... gypsum-based shear face materials according to Comparative Example 4A and

[0040] Hereinafter, the configuration of a wooden structural shear wall according to a preferred embodiment of the present disclosure will be described in detail with reference to the accompanying drawings.

[0041] [Overall Configuration of Wooden Structure Shear Wall] Fig. 1 is a front view showing a schematic configuration of a shear wall of a wooden structure building according to a preferred embodiment of the present disclosure. Fig. 2A and Fig. 2B are a partial cross-sectional view and a partially cutaway perspective view, respectively, of the shear wall shown in Fig. 1 , showing an enlarged portion of the shear wall in which a gypsum-based shear face material is fixed to a wooden framework with nails.

[0042] The wooden structural shear wall 1 shown in Figure 1 is a wooden structural shear wall constructed by fixing a gypsum-based shear face panel 10 to a wooden framework on a reinforced concrete (RC) continuous footing F. The shear face panel 10 has dimensions of 9.5 mm thick, 910 mm wide, and about 2800 to 3030 mm high (e.g., about 2900 mm), and has a strength of 6.5 to 8.9 kg / m 2 Area density within the range of (for example, area density 7.5 kg / m 2 ). The areal density (also called areal weight) is the mass (weight) per unit area (visible area) of the wall surface when viewed from the front. As shown in Figure 2, the load-bearing surface material 10 is a gypsum-based load-bearing surface material composed of a flat gypsum core (gypsum core material) 11 mixed with a predetermined amount of inorganic fiber (glass fiber) and organic strength-enhancing material (starch), and gypsum board base paper (paper member) 12 covering both sides of the gypsum core.

[0043] The bearing wall 1 has a base 2 fixed to the top surface of a continuous footing F by anchor bolts B. The bearing wall 1 is generally composed of this base 2, columns 3, partition studs 4, and inter-joint columns 4' arranged vertically at predetermined intervals on the base 2, horizontal cross members (beams, girths, eaves beams, gable beams) 5 supported on the upper ends (or middle parts) of the columns 3, and the bearing surface material 10. The base 2, columns 3, partition studs 4, inter-joint columns 4', and cross members 5 that make up the framework are made of wood (square timber) with the cross section used in ordinary wooden buildings.

[0044] The load-bearing face panel 10 is fixed to the sill 2, columns 3, studs 4, inter-joint columns 4', and cross members 5 with nails 20 made of iron or stainless steel (iron in this example). The nails 20 are arranged at intervals S1 in the four peripheral zones of the load-bearing face panel 10, and at intervals S2 in the central zone of the load-bearing face panel 10 extending in the vertical direction. Preferably, the interval S1 is set to a dimension within the range of 50 mm to 200 mm (e.g., 75 mm), and the interval S2 is set to a dimension within the range of 50 mm to 300 mm (e.g., 150 mm).

[0045] 2, the nail 20 is an iron nail comprising a flat or mesh-shaped head 21 having a circular contour in top view, a straight, smooth body 22 having a uniform circular cross section, a neck 23 located at the base end of the body 22 and integrally connecting the body 22 and head 21, and a spire-shaped tip 24 located at the tip of the body 22. The underside of the head 21 forms an annular seating surface 21b that seats on the outer surface of the bearing face material 10. The outer periphery of the neck 23 is locally slightly tapered or conically enlarged in diameter and continues to the head 21, so the radial dimension of the seating surface 21b does not necessarily match the diameter difference between the head 21 and body 22, but is slightly smaller than the diameter difference, but is generally the same value.

[0046] In general, the nail 20 is specified by the diameter of the head 21 (head diameter D), the diameter of the body 22 (body diameter d), and the overall length (length L) of the nail 20, in addition to the material and shape of the head 21 and body 22. In this embodiment, the head diameter D, body diameter d, and length L are 7.07 mm, 2.45 mm, and approximately 50 mm, respectively, and the ratio η of the visible area of ​​the top surface 21a of the head 21 to the cross-sectional area of ​​the body 22 (i.e., head area / body cross-sectional area) is 8.32 (see FIG. 5 ). In this disclosure, the head diameter D is preferably set to a value within a range of 6.0 to 10.0 mm, more preferably within a range of 6.8 to 9.0 mm, and the body diameter d is preferably set to a value within a range of 2.0 to 5.0 mm, more preferably within a range of 2.2 to 4.2 mm. The head area / body cross-sectional area ratio η is preferably set to a value within a range of 6 to 13, more preferably within a range of 7 to 11.

[0047] The gypsum core 11 of the bearing surface material 10 contains a predetermined amount of inorganic fiber and organic strength-enhancing material and has a nail lateral resistance of 500 N or more. The amount of inorganic fiber is 0.3 to 5 parts by weight, preferably 2 to 4 parts by weight, per 100 parts by weight of calcined gypsum. Examples of inorganic fibers to be added include glass fiber and carbon fiber. When glass fiber is used, glass fiber with a diameter of 5 to 25 μm and a length of 2 to 25 mm can be preferably used. The amount of organic strength-enhancing material to be added is 0.3 to 15 parts by weight, preferably 1 to 13 parts by weight, per 100 parts by weight of calcined gypsum. Examples of organic strength-enhancing materials to be added include starch, polyvinyl acetate, polyvinyl alcohol, polyacrylic, etc. Note that both unmodified and modified starch can be used as the starch. Examples of modified starch include starch that has been subjected to physical, chemical, or enzymatic treatment. As the physically treated starch, pregelatinized starch can be suitably used. As the chemically treated starch, oxidized starch, phosphated starch, urea phosphated starch, hydroxypropylated phosphate cross-linked starch, hydroxyethylated starch, hydroxypropylated starch, cationized starch, and acetylated starch can be suitably used. The blending of the organic strength improving material is suitable for a relatively low areal density (6.5 to 8.9 kg / m 2 While ensuring the areal density within the range of 6.5 N / mm 2 This provides the load-bearing face material 10 with a compressive strength of 500 N or more, and is an effective means of achieving or ensuring the desired nail lateral resistance (nail lateral resistance of 500 N or more) of the load-bearing face material 10 in cooperation with the inorganic fibers. In addition, considering that the blending of the organic strength-enhancing material does not significantly affect the overall quality of the gypsum-based load-bearing face material, this is a simple and yet realistically or practically effective means of improving the nail lateral resistance of the load-bearing face material 10.

[0048] The composition and structure of the bearing surface material 10 are similar to those of the "structural gypsum board" specified in JIS A 6901. However, the surface density of the bearing surface material 10 is 6.5 to 8.9 kg / m 2 A value within the range (for example, 7.5 kg / m 2 ) Therefore, the bearing surface material 10 has a strength of 9.4 kg / m as described above. 2This is fundamentally different from the "structural gypsum board" of JIS A 6901, which requires an areal density of 9.4 kg / m or more. Also, "reinforced gypsum board" specified in JIS A 6901 is known, but "reinforced gypsum board" also has an areal density of 9.4 kg / m. 2 Since the load-bearing face material 10 requires an area density of 500 N or more, it is fundamentally different from "reinforced gypsum board." Furthermore, the load-bearing face material 10 is different from other "gypsum boards" in that it has a main or core material (gypsum core 11) that is blended with inorganic fibers and organic strength-enhancing materials to exhibit a nail lateral resistance of 500 N or more. In other words, the load-bearing face material 10 does not fall under any of the "gypsum boards" specified in the current JIS A 6901. In this sense, the load-bearing face material 10 will be specified or expressed as a "gypsum-based load-bearing face material" in this specification.

[0049] Generally, gypsum-based load-bearing surface materials (including "gypsum boards," "reinforced gypsum boards," and "structural gypsum boards") formed by covering the front and back surfaces of a plate-shaped main material or core material made of a gypsum hardened body with paper members are manufactured using a general-purpose gypsum board manufacturing apparatus. As described in International Publication WO 2019 / 058936, for example, the gypsum board manufacturing apparatus has a mixer that prepares a gypsum slurry by mixing raw materials such as calcined gypsum, an adhesive aid, a hardening accelerator, and foam (or foaming agent) with mixing water required to form a slurry of the calcined gypsum. The gypsum slurry is poured and spread onto gypsum board base paper (bottom paper) on a conveyor belt of the gypsum board manufacturing apparatus, and gypsum board base paper (top paper) is layered on the gypsum slurry. The strip-shaped continuous laminate with a three-layer structure thus formed is processed by various devices constituting a gypsum board manufacturing apparatus, such as a rough cutting device, a forced drying device, and a cutting device, to form a gypsum product of a predetermined size, i.e., a gypsum-based facing material in which both sides of a hardened gypsum slurry body (i.e., a gypsum core) are covered with gypsum board base paper. The specific gravity of the gypsum-based facing material is adjusted mainly by the amount of foam blended in the gypsum slurry.

[0050] Regarding wooden structural shear walls that use structural gypsum board, reinforced gypsum board, and (ordinary) gypsum board as the load-bearing surface material as specified in JIS A 6901, examples of wall coefficients for surface-material shear walls of large wooden frame structures as specified in the aforementioned Ministry of Construction Notification No. 1100 are as follows:

[0051] Structural gypsum board (Type A) 1.7 Structural gypsum board (Type B) 1.2 Reinforced gypsum board 0.9 (Normal) gypsum board 0.9

[0052] In addition, examples of wall coefficients for frame wall construction shear walls (shear walls with a vertical frame spacing of more than 50 cm) specified in the aforementioned Ministry of Land, Infrastructure, Transport and Tourism Notification No. 1541 are as follows:

[0053] Structural gypsum board (Type A) 1.7 Structural gypsum board (Type B) 1.5 Reinforced gypsum board 1.3 (Normal) gypsum board 1.0

[0054] The wall factor values ​​specified in the notices of the Ministry of Construction or the Ministry of Land, Infrastructure, Transport and Tourism are generally applicable without the need for individual performance tests. However, structural gypsum board, reinforced gypsum board, and (ordinary) gypsum board that are recognized as effective load-bearing surface materials are limited to those with a thickness of 12 mm or more. Therefore, when using surface materials made from new materials or compositions, or gypsum-based surface materials with a thickness of less than 12 mm as load-bearing surface materials, or when using a wall factor different from the above values, it is necessary to conduct the aforementioned performance tests and determine the wall factor value.

[0055] As mentioned above, the structural gypsum board and reinforced gypsum board specified in JIS A 6901 have an areal density of 9.4 kg / m 2 The surface density and specific gravity must be 0.75 or more. This has been considered an important condition for increasing the maximum load that the surface material can withstand and for ensuring a high short-term allowable shear strength (and therefore a high wall ratio) for wooden structural shear walls. In particular, for structural gypsum boards that must exhibit higher nail lateral resistance than reinforced gypsum boards, it has been thought that these surface density and specific gravity cannot be reduced. That is, a surface density of 9.4 kg / m 2As described above, ensuring a specific gravity of 0.75 or more was considered an essential condition for further increasing the wall strength of the shear wall specimen (wooden shear wall) obtained in the aforementioned in-plane shear test. However, recent experiments by the present inventors and others have shown that in gypsum-based facing materials that have been given properties (nail lateral resistance) comparable to those of structural gypsum board by adding inorganic fibers or organic strength improvers, reducing the thickness of the facing material or adjusting the foam content to reduce the specific gravity of the gypsum core, thereby reducing the areal density, reveals the toughness or deformation compliance inherent in the facing material itself, thereby effectively utilizing the ultimate strength of the bearing wall and increasing the shear wall's plasticity factor, thereby further improving the short-term allowable shear strength of the bearing wall. This point is described in detail in Patent Document 3, but below we will provide an overview of in-plane shear tests on wooden structural shear walls, as well as general information regarding the increase in the plasticity factor of the shear wall due to the increase in the ultimate strength of the shear wall, and the resulting improvement in the short-term allowable shear strength and wall factor of the shear wall, for reference.

[0056] [Regarding the specimen for the in-plane shear test of the wooden structural shear wall] Figure 3 is a front view, a cross-sectional view, and a side view showing the configuration of the shear wall specimen used in the in-plane shear test on the shear wall structure shown in Figure 1.

[0057] In FIG. 3, the same reference numerals are used to designate elements or components of the load-bearing wall specimen that correspond to or correspond to the elements or components shown in FIGS.

[0058] In accordance with the specimen specifications described in the "Wooden Bearing Walls and Their Magnification Factors Performance Testing and Evaluation Procedure Manual," the inventors fabricated a bearing wall specimen (hereinafter simply referred to as "specimen") having the bearing wall structure shown in Figure 3, with a wall width of 1,820 mm and a height of 2,730 mm, as a specimen for the bearing wall structure shown in Figure 1, and conducted an in-plane shear test using a non-loading type testing device.

[0059] The specimen shown in Figure 3 has a main structural section of a wooden frame consisting of a sill 2 and a column 3 made of cedar lumber with a cross section of 105 x 105 mm, and a cross member 5 made of Douglas fir lumber with a cross section of 180 x 105 mm supported by the column 3. A cedar inter-joint column 4' with a cross section of 45 x 105 mm is erected in the center between the columns 3, and a cedar stud 4 with a cross section of 27 x 105 mm is erected between the column 3 and the inter-joint column 4'. Cedar or Douglas fir ties 5' are installed between the column 3 and the stud 4 and between the stud 4 and the inter-joint column 4'. As a test jig, a pull-out hardware 40 is installed at the joint between the sill 2 and the column 3 and at the joint between the cross member 5 and the column 3. The base 2, columns 3, joint columns 4', studs 4, cross members 5 and junction ties 5' constitute the shaft members of the load-bearing wall structure, and these members (shaft members) form a rectangular framework.

[0060] In the specimen shown in Figure 3, the vertical distance h1 between the base 2 and the cross member 5, the height h2 of the junction 5', and the relative height h3 of the cross member 5 relative to the junction 5' were set to h1 = 2625 mm, h2 = 1790 mm, and h3 = 835 mm, respectively. The distance w1 between the column 3 and the joint column 4' (column center distance) was set to w1 = 910 mm, and the wall length L was set to 1.82 m. The face panel 10 was divided into upper and lower sections by the junction 5'. The lower face panel 10a had dimensions of 910 mm wide and 1820 mm high, and the upper face panel 10b had dimensions of 910 mm wide and 865 mm high. The overlap dimensions h4 and h5 of the face panels 10a and 10b were set to 30 mm.

[0061] In the test specimen shown in Figure 3, nails 20 for fastening the face plates 10a, 10b to the sill 2, columns 3, joint columns 4', cross members 5, and junction ties 5' were arranged at equal intervals (interval S1 = 75 mm) around the entire periphery of the edge zones of the face plates 10a, 10b. Nails 20 for fastening the face plates 10a, 10b to the studs 4 were arranged at equal intervals (interval S2 = 150 mm) in the vertical center zones of the face plates 10a, 10b.

[0062] [Explanation of the short-term allowable shear strength and wall magnification factor of wooden shear walls (premise of the present disclosure)] Figure 4 is an explanatory diagram and graph showing, for reference, the test results of an in-plane shear test using any gypsum-based shear face material, and in Figure 4, the load-deformation angle curve generally obtained by the in-plane shear test is displayed as an envelope curve (shown by a solid line). With reference to Figure 4, the in-plane shear test of a wooden shear wall will be explained, and a method for determining the short-term allowable shear strength and wall magnification factor of a wooden shear wall will be explained.

[0063] In Figure 4, the dot-dash line shows a linear graph in which the envelope of the load-deformation curve is converted into the load-deformation characteristic of a perfectly elastoplastic model. The perfectly elastoplastic model is composed of a linear function line (Y = KX) in the linear elastic region that indicates the initial stiffness K, and a line (Y = Pu) in the plastic deformation region (plastic region) that extends parallel to the X-axis from the yield point σs. The yield point σs indicates the elastic limit. The initial stiffness K is a coefficient that indicates the slope of the linear function line (Y = KX) in the elastic region. The area on the diagram of the region enclosed by the envelope, the X-axis, and the line segments X = δu is equal to the area on the diagram of the region enclosed by the X-axis, the line segments Y = KX, Y = Pu, and X = δu. The method of converting the envelope into a fully elastic-plastic model is described in many documents, such as the "Wooden Shear Walls and Their Magnification Factors - Performance Testing and Evaluation Procedure Manual," and is also a well-known matter in the field of material mechanics, so further explanation will be omitted.

[0064] Figure 4 shows the maximum strength Pmax, the 0.8Pmax load drop region, the ultimate strength Pu, the yield strength Py, the ultimate displacement δu, the yield point displacement δv, and the yield displacement δy. The ultimate displacement δu and the yield point displacement δv are the deformation angle values ​​at the 0.8Pmax load drop region and the yield point σs, respectively. The yield displacement δy is the deformation angle value when the yield strength Py is reached. The ductility factor μ is the value (ratio) of the ultimate displacement δu / the yield point displacement δv. When the load (strength) drops to 0.8Pmax after reaching the maximum strength Pmax, the wall is considered to have substantially lost its strength, and the in-plane shear test is essentially completed at the 0.8Pmax load drop region.

[0065] As described in many technical documents, such as "Allowable Stress Design for Wooden Frame Construction Houses [1] (2017 Edition)" on pages 63 and 300 (Non-Patent Document 1), the wall factor is calculated by dividing the short-term allowable shear strength (Pa) by the predetermined strength (wall length L (m) × 1.96 (kN / m)) calculated based on the strengths Pmax, Pu, Py and displacements δu, δv, δy determined by the fully elasto-plastic model shown in Figure 4. In other words, the wall factor is an indexed value obtained by dividing the short-term allowable shear strength (Pa) by this reference value (1.96L).

[0066] To further explain this point, in calculating the wall factor, the smallest of the following four strength values ​​is generally identified as the short-term standard shear strength (P0), and this short-term standard shear strength (P0) is multiplied by a specified reduction coefficient (α) (a coefficient used to evaluate the factors behind the reduction in strength). Generally, for gypsum-based shear panels, the strength of (1) or (2) below, i.e., the yield strength (Py) or ultimate strength (corrected value) (Pu'), is the smallest. The short-term standard shear strength (P0) calculated from the following strength values ​​(Py, Pu, Pmax) is calculated by multiplying the following value by the variation coefficient (β):

[0067] (1) Yield strength (Py) (2) Value of ultimate strength (Pu) corrected based on the plasticity factor (μ) (hereinafter referred to as "ultimate strength (corrected value) (Pu')") (3) Value of 2 / 3 of maximum strength (Pmax) (4) Strength when shear deformation angle = 1 / 120 rad (for unloaded or loaded type)

[0068] Generally, the short-term standard shear strength (P0) of a bearing wall formed by fastening the aforementioned structural gypsum board (Patent Document 2) to a wooden wall substrate with fasteners is determined by the yield strength (Py) of the four types of strength values ​​(P0 = β × Py). As mentioned above, the wall factor is the short-term standard shear strength (P0) multiplied by the reduction coefficient (α) and divided by the predetermined strength (1.96L). Therefore, the wall factor of a bearing wall formed by fastening structural gypsum board to a wooden wall substrate with fasteners is proportional to the yield strength (Py).

[0069] On the other hand, the short-term standard shear strength (P0) of the gypsum-based face material described in Patent Document 3, i.e., a bearing wall formed by fastening the aforementioned low-density gypsum-based bearing face material to a wooden structural wall substrate with fasteners, usually exhibits the smallest ultimate strength (corrected value) (Pu') among the four types of strength values. Therefore, unlike structural gypsum board, the short-term standard shear strength (P0) and wall factor for calculating the wall magnification are proportional to the ultimate strength (corrected value) (Pu'). In the low-density gypsum-based bearing face material, the unexpected effect of its low density is that the toughness and deformation followability that the gypsum-based bearing face material potentially possesses become apparent due to the decrease in surface density, and as a result, the ultimate displacement (δu) of the bearing wall increases to 20 x 10 -3 As a result of obtaining an ultimate displacement (δu) greater than rad, a bearing wall formed by fixing the low-density gypsum-based bearing surface material of Patent Document 3 to a wooden structural wall substrate exhibits an ultimate strength (corrected value) (Pu') greater than 7.6 kN. Thus, as described above, the low-density gypsum-based bearing surface material exhibits a strength equivalent to that of structural gypsum board, despite having a reduced surface density compared to structural gypsum board.

[0070] The ultimate strength (corrected value) (Pu') is a value calculated using the formula below based on the ultimate strength (Pu) and the plasticity factor (μ), and the short-term standard shear strength (P0) is a value calculated using the formula below based on the ultimate strength (corrected value) (Pu') and the coefficient of variation (β) of its measurement value.

[0071] Pu'=Pu×0.2×(2μ-1)1 / 2 P0=β×Pu'

[0072] That is, in the gypsum-based bearing surface material of Patent Document 3 (i.e., low-density gypsum-based bearing surface material) in which the surface density is reduced to make the toughness or deformation followability inherent in the surface material itself apparent, the ultimate displacement (δu) of the bearing wall is 20 × 10 -3rad, resulting in an increase in the plasticity factor μ (=δu / δv) and an increase in the ultimate strength (corrected value) (Pu'), which in turn increases the short-term allowable shear strength (Pa) and the wall ratio. The inventors further studied the fastening structure of the face plate and the plasticity factor μ in order to further increase the short-term allowable shear strength (Pa) and the wall ratio, and found that by changing the dimensions and shape of the nails 20 and increasing the initial rigidity, the plasticity factor μ could be increased, leading to the present disclosure. This point will be explained below.

[0073] [Regarding the dimensions and shape of the nail 20] In conventional wooden shear walls in which gypsum-based shear panels are fixed to the framework or framing of a wooden structure, the gypsum-based shear panels are generally fixed to the framework or framing using NZ50 nails (plated iron round nails: JIS A 5508). NZ50 nails have dimensions (JIS A 5508) of 6.6 mm head diameter, 2.75 mm shaft diameter, and 50 mm nail length, with a head area / shaft cross-sectional area ratio η of 5.76. In an in-plane shear test using a wooden shear wall specimen in which low-density gypsum-based shear panels are fixed to the framework or framing of a wooden structure using such nails, the ultimate displacement (δu) increases, as described in Patent Document 3, resulting in increases in the ultimate strength (corrected value) (Pu'), short-term reference shear strength (P0), and wall magnification factor. However, in this in-plane shear test, repeated application of force to the test specimen caused the nail holes to break, resulting in a punching shear phenomenon. This resulted in punching-out failure of the gypsum-based shear panel, causing a rapid drop in the specimen's strength to Pu = 0.8Pmax, which terminated the in-plane shear test. Therefore, unless damage or fracture of the nailed sections and punching-out failure of the gypsum-based shear panel are suppressed, it is believed that further increases in the short-term allowable shear strength (Pa) and wall ratio are difficult. While it may be possible to suppress or reduce punching-out failure by providing reinforcing or stiffening materials such as metal plates in the nailed sections, as in the panel reinforcement method described in Patent Document 1, the addition or placement of such reinforcing or stiffening materials complicates the manufacturing process of the gypsum-based shear panel and reduces the workability of construction work, as mentioned above.

[0074] 5 is a comparative chart showing the head diameter D, trunk diameter d, length L, and head area / trunk cross-sectional area ratio η for nail 20 constituting a bearing wall according to an embodiment of the present disclosure and nails N1 and N2 constituting bearing walls according to a comparative example. The values ​​of head diameter D, trunk diameter d, length L, and head area / trunk cross-sectional area ratio η for nail 20 are as described above. Nail N1 is an iron nail distributed on the market as an NZ50 nail (JIS A 5508). The values ​​shown in FIG. 5 (head diameter D = 6.62 mm, trunk diameter d = 2.83 mm, head area / trunk cross-sectional area ratio η = 5.48) were obtained by measuring the dimensions of each part of 10 randomly selected NZ50 nails available on the market and averaging the measured values. These values ​​differ slightly from the values ​​specified in JIS A 5508. Nail N2 is an iron nail distributed on the market as a CN50 nail (JIS A 5508), and the values ​​shown in Figure 5 (head diameter D = 6.67 mm, body diameter d = 2.92 mm, head area / body cross-sectional area ratio η = 5.2) were also obtained by measuring the dimensions of each part of 10 randomly selected CN50 nails available on the market and averaging the measured values, and are slightly different from the values ​​specified in JIS A 5508. The length L of nails 20, N1, and N2 is all approximately 50 mm.

[0075] 6 is a diagram and chart for comparing the results of an in-plane shear test for a bearing wall using nail N1 (Comparative Example 1) and a bearing wall using nail N2 (Comparative Example 2). FIG. 7 is a diagram and chart for comparing the results of an in-plane shear test for a bearing wall using nail 20 (embodiment of the present disclosure) and a bearing wall using nail N1 (Comparative Example 3). The gypsum-based bearing surface materials 10 of the embodiment and Comparative Examples 1 to 3 are all low-density gypsum-based bearing surface materials described above, each composed of a flat gypsum core (gypsum core material) 11 containing a predetermined amount of inorganic fiber (glass fiber) and organic strength-enhancing material (starch), and gypsum board base paper (paper component) 12 covering both sides of the gypsum core. The low-density gypsum-based bearing surface materials have an areal density in the range of 6.5 to 8.9 kg / m², a compressive strength of 6.5 N / mm² or more, and a nail lateral resistance of 500 N or more.

[0076] As is clear from the test results shown in Figure 6, the inventors confirmed that in the case of gypsum-based bearing face materials, thicker nails (Comparative Example 2, in which the trunk diameter d is larger than that of Comparative Example 1) are not necessarily effective in suppressing punch-out failure (and therefore are not necessarily advantageous in improving the short-term allowable shear strength (Pa) and wall factor). Furthermore, as is clear from the test results shown in Figure 7, the inventors confirmed that in the case of gypsum-based bearing face materials, punch-out failure of the gypsum-based bearing face materials can be suppressed or reduced, and the short-term allowable shear strength (Pa) and wall factor can be relatively significantly improved by appropriately setting the head diameter D, trunk diameter d, and head area / trunk cross-sectional area ratio η. This point will be explained below with reference to Figures 6 and 7.

[0077] Generally, the head diameter D and body diameter d of nail N2 (Comparative Example 2) are larger than those of nail N1 (Comparative Example 1), which is advantageous in suppressing or reducing punch-out failure and is generally recognized as superior in shear strength compared to nail N1 (thin nail) with its relatively small body diameter d. However, in the case of low-density gypsum-based bearing surface materials with increased compressive strength and nail lateral resistance, nail N2 was found to actually reduce the short-term allowable shear strength (Pa) (and therefore the wall ratio), as shown in Figure 6. This is because punching shear occurred relatively early in the in-plane shear test, and the wall's strength (load) was quickly reduced to Pu = 0.8Pmax (ultimate displacement δuB < δuA) due to fracture or breakage of the nailed portion due to punch-out failure, resulting in the wall essentially losing its strength.

[0078] On the other hand, when comparing the shear wall of this embodiment using nail 20 with the shear wall of Comparative Example 3 using nail N1, as shown in Figure 7, the barrel diameter d of nail 20 is smaller than the barrel diameter d of nail N1 (Comparative Example 3), and although nail 20 is a thin nail that is generally recognized to have inferior shear strength compared to nail N1, such conventional recognition or knowledge is not necessarily applicable in the case of low-density gypsum-based shear surface materials that have increased compressive strength and nail lateral resistance, and as shown in Figure 7, nail 20 increases the short-term allowable shear strength (Pa) compared to nail N1 (and therefore increases the wall coefficient). This is thought to be because the difference in the area ratio η of the head area to the cross-sectional area of ​​the trunk increases the difference in diameter between the trunk diameter d and the head diameter D of the nail 20, which delays the occurrence of the punching shear phenomenon, delays the time of the reduction in strength (load) (Pu = 0.8Pmax) caused by the destruction or breakage of the nailed part due to punching-out failure, and results in an increase in ultimate displacement (δuE > δuC).

[0079] Therefore, by setting the head diameter D and the body diameter d to 7.07 mm and 2.45 mm, respectively, and setting the head area / body cross-sectional area to 8.32, thereby increasing the diameter difference between the head 21 and the body 22 and ensuring a sufficient annular and flat seating surface 21b (see Figure 2) that seats on the surface of the low-density gypsum-based bearing face material, it is possible to effectively increase the short-term allowable shear strength (Pa) of the bearing wall 1 using a low-density gypsum-based bearing face material with increased compressive strength and nail lateral resistance (and therefore effectively increase the wall factor). However, in addition to increasing the diameter difference between the head 21 and the body 22, it is thought that the following conditions also need to be considered.

[0080] (1) In order to prevent the face material 10 from cracking due to the penetration of the nail during nailing, and taking into consideration the head diameter D of the nail suitable for use with a nail gun, the head diameter D is set to 10 mm or less, preferably 9 mm or less. (2) In order to prevent the punching shear phenomenon and reduce the effect of punching-out destruction, the head diameter D is set to 6 mm or more, preferably 6.8 mm or more. (3) In order to prevent the face material 10 from cracking due to the penetration of the nail during nailing, and to prevent the edge of the face material from breaking during an in-plane shear test, the trunk diameter d is set to 5 mm or less, preferably 4.2 mm or less. (4) In order to prevent excessive bending deformation of the nail during an in-plane shear test, the trunk diameter d is set to 2 mm or more, preferably 2.2 mm or more. (5) In order to prevent an extreme decrease in the strength of the neck portion 23, the head area / trunk cross-sectional area ratio η is set to 13 or less, preferably 11 or less. (6) In order to ensure the effect of suppressing the punching shear phenomenon, the ratio η of the head area to the cross-sectional area of ​​the body is set to 6 or more, preferably 7 or more.

[0081] Thus, in a bearing wall 1 using a low-density gypsum-based bearing surface material with increased compressive strength and nail lateral resistance, the head diameter D, the trunk diameter d, and the ratio η of head area / trunk cross-sectional area are set to values ​​within appropriate numerical ranges, thereby preventing the head 21 (nail head) from sinking into the surface material 10, suppressing or reducing the punching shear phenomenon, and suppressing cracks in the surface material 10 that may occur when nailing, thereby effectively increasing the short-term allowable shear strength (Pa) of the bearing wall 1 (and therefore effectively increasing the wall multiplier). In particular, in the case of gypsum-based load-bearing surface materials 10, nailing is required so that the head 21 is flush with the surface of the surface material and so that the covering material (plasterboard base paper) 12 of the surface material 10 is not broken or damaged. However, if the head 21 has an excessively large head diameter D, the surface material 10 is likely to crack when the top surface 21a of the head 21 is made flush with the surface of the surface material 10 (see (1) above), and therefore the above settings for the head diameter D, body diameter d, and head area / body cross-sectional area ratio η are important in order to avoid such a phenomenon.

[0082] [Regarding the increase in initial stiffness due to increased compressive strength, and the increase in short-term allowable shear strength Pa and wall ratio] The inventors recognized that the short-term allowable shear strength Pa and wall ratio of the shear wall 1 can be increased by fixing the low-density shear face panel 10, which has increased compressive strength and nail lateral resistance, to the framework or frame of a wooden structure using the nails 20 having the specific dimensions and shape as described above. However, the inventors further recognized that the short-term allowable shear strength Pa and wall ratio of the shear wall 1 can be further increased by increasing the initial stiffness of the face panel as the compressive strength increases. That is, by using the nails 20 having the specific dimensions and shape and the low-density shear face panel 10, which has increased compressive strength and nail lateral resistance, not only can the punching shear phenomenon be suppressed or reduced, but the initial stiffness of the face panel can be increased, thereby increasing the plasticity modulus μ. The combined effect of these two factors can effectively or efficiently increase the short-term allowable shear strength Pa and wall ratio. The effect of the increase in initial rigidity of the bearing face material 10 due to the increase in compressive strength and the resulting increase in short-term allowable shear strength Pa and wall ratio will be explained below.

[0083] As mentioned above, the compressive strength and nail lateral resistance of the gypsum-based bearing surface material 10 can be increased by supplying an organic strength-improving material such as starch, polyvinyl acetate, polyvinyl alcohol, or polyacrylic together with inorganic fibers to a gypsum slurry kneading mixer to incorporate appropriate amounts of the organic strength-improving material and inorganic fibers into the gypsum slurry. The blending of the organic strength-improving material into the gypsum slurry is carried out at a relatively low areal density (6.5 to 8.9 kg / m 2 While ensuring the areal density within the range of 6.5 N / mm 2 This is an effective means for imparting a compressive strength of 500 N or more to the gypsum-based load-bearing surface material 10, and furthermore, working in conjunction with the inorganic fibers, for imparting the desired nail lateral resistance (a nail lateral resistance of 500 N or more) to the gypsum-based load-bearing surface material 10. In addition, considering that the blending of the organic strength-enhancing material does not significantly affect the overall quality of the gypsum-based load-bearing surface material, this is a simple and yet realistically or practically effective means.

[0084] Furthermore, recent experiments by the present inventors have revealed that an increase in the compressive strength of the bearing face material 10 contributes to an increase in the initial stiffness K of the bearing wall 1, thereby reducing the yield point displacement δv without significantly reducing the ultimate displacement δu of the bearing wall, resulting in a relatively large increase in the plasticity factor μ of the bearing wall 1, and thus increasing the short-term allowable shear strength Pa and the wall factor, as will be explained below.

[0085] The inventors fabricated gypsum-based bearing surface materials according to Reference Examples 1 to 4 and Comparative Example 4 shown in the table of Fig. 8 as test specimens, and conducted in-plane shear tests using a non-loading testing device. The blending amounts of inorganic fiber and organic strength improver shown in Fig. 8 are shown in parts by weight per 100 parts by weight of calcined gypsum. As mentioned above, the gypsum-based bearing surface material of Comparative Example 4 is a surface material composed of a flat gypsum core (gypsum core material) mixed with a predetermined amount of inorganic fiber (glass fiber) and organic strength improver (starch), and gypsum board base paper (paper component) covering both sides of the gypsum core. Each of them has a shear strength of about 7.4 to about 8.7 kg / m 2 The gypsum-based shear face material has an areal density within the range of 0.01 mm, and compared to conventional gypsum-based shear face material (Patent Document 4), it has the performance of increasing the ultimate displacement δu and plasticity factor μ of the wooden structural shear wall, and increasing the short-term allowable shear strength Pa and wall factor. However, the gypsum-based shear face materials of Reference Examples 1 to 4 and Comparative Example 4 were fastened to the sill 2, columns 3, partition 4, joint columns 4', cross members 5, and truss 5' (wooden framework shown in Figure 3) with conventional nails N1 (NZ50 nails) rather than the nails 20 of the present disclosure. This is to eliminate the effect or influence of the use of nails 20 and evaluate only the increase in initial stiffness K of the shear wall 1 (and therefore the increase in the plasticity factor μ of the shear wall 1) due to the increased compressive strength of the shear face material 10, and the resulting increase in short-term allowable shear strength Pa and wall factor. The shear walls whose performance is shown in Figures 8 and 9 do not have a structure in which the shear face panels 10 are fastened to a wooden frame using the nails 20 according to the present disclosure, and are therefore shown in Figures 8 and 9 as Reference Examples 1 to 4.

[0086] Referring to the test results shown in FIGS. 8 and 9, the test results for each specimen of Reference Examples 1 to 4 and Comparative Example 4 show that the deformation angle was approximately 20×10 -3After reaching the maximum load (maximum strength) Pmax (Fig. 3), the specimen does not break immediately, but instead reaches the deformation angle in the 0.8Pmax load drop region, i.e., the ultimate displacements δu1 to δu5 (Fig. 9), due to the subsequent repeated loading. The ultimate displacements δu1 to δu5 are approximately 30 × 10 -3 rad. This means that after the test specimens in Reference Examples 1 to 4 and Comparative Example 4 reached the maximum load (maximum strength) Pmax, plastic deformation continued due to subsequent repeated application of force until a deformation angle of approximately 1.5 times the deformation angle at the maximum load Pmax occurred. As mentioned above, this continuity of plastic deformation is thought to be due to the fact that the surface density was reduced while maintaining the minimum physical properties (nail lateral resistance: 500 N or more) required for a gypsum-based load-bearing surface material, and the toughness or deformation compliance inherent in the gypsum board itself was made apparent.

[0087] On the other hand, when comparing the compressive strengths of Reference Examples 1 to 4 and Comparative Example 4, the compressive strength of the gypsum-based bearing surface material of Comparative Example 4 was 6.0 N / mm 2 The compressive strength of the gypsum-based bearing surface materials of Reference Examples 1 to 4 (6.5 N / mm 2 The gypsum-based load-bearing surface material of Comparative Example 4 has a relatively lower short-term allowable shear strength Pa and wall factor than the gypsum-based load-bearing surface materials of Reference Examples 1 to 4.

[0088] [Measurement of Compressive Strength of Bearing Face Material] FIG. 10 shows a schematic diagram of a method for measuring the compressive strength of a gypsum-based bearing face material.

[0089] When measuring the compressive strength of the gypsum-based bearing surface materials, the inventors cut the gypsum-based bearing surface materials according to the Examples, Reference Examples, and Comparative Examples into flat plates measuring 4 cm x 4 cm, as shown in Figure 10. For each of the Examples, Reference Examples, and Comparative Examples, multiple test pieces 101 were produced. A test piece stack 100, consisting of four identical test pieces 101 stacked together without bonding, was inserted between upper and lower loading plates 102 and 103 of the measuring device. A vertical compressive load Fv (and reaction force Rv) was then applied to the test piece stack 100 by upper and lower loading rods 104, destroying the main or core material (i.e., the gypsum core portion of the test piece 101) made of a gypsum hardened body, and the compressive load Fv at the time of destruction was measured. A precision universal testing machine (Shimadzu Corporation's "Autograph," model AG-10NKI) was used as the measuring device. The inventors measured the compressive load Fv at the time when any of the test pieces 101 constituting the test piece stack 100 was compressed and fractured, and multiplied this measurement value by the area (16 cm 2 ) was determined as the compressive strength of each gypsum-based load-bearing surface material.

[0090] The compressive strengths of the gypsum-based bearing surface materials of Reference Examples 1 to 4 and Comparative Example 4 thus identified are shown in Figure 8. As shown in Figure 8, the initial stiffness K of the gypsum-based bearing surface materials of Reference Examples 1 to 4 and Comparative Example 4 changes roughly in response to increases or decreases in compressive strength, and the value of initial stiffness K can be increased by increasing the compressive strength. Also, as shown in Figure 8, the plasticity factor μ can be changed by increasing or decreasing the initial stiffness K, and the values ​​of the ultimate strength (corrected value) Pu' and short-term allowable shear strength Pa can be changed. According to the physical properties of Reference Examples 1 to 4, the compressive strength of the gypsum-based bearing surface material was 6.5 N / mm 2 By increasing the value to the above, as shown in FIG. 8, an ultimate strength (corrected value) Pu' (short-term allowable shear strength Pa of 5.85 kN or more) of 7.8 kN or more can be obtained.

[0091] That is, the gypsum-based load-bearing surface materials of Reference Examples 1 to 4 have a strength of 6.5 N / mm 2The specimens have a compressive strength of 1.64 to 2.50, and the resulting increase in initial rigidity K and decrease in yield point displacement δv result in a relatively high plasticity coefficient μ. As a result, the ultimate strength (corrected value) Pu' and short-term allowable shear strength Pa of the specimens of Reference Examples 1 to 4 are Pu' = 7.8 to 11.9 kN and Pa = 5.85 to 8.92, respectively. These values ​​are significantly increased compared to the ultimate strength (corrected value) (= 7.62 kN) and short-term allowable shear strength Pa (= 5.72 kN) of the specimen of Comparative Example 4. Also, assuming a reduction coefficient α = 0.75 and a variation coefficient β = 1.0, the wall factor of the specimens of Reference Examples 1 to 4 is 1.64 to 2.50, which is significantly increased compared to the wall factor (1.60) of the specimen of Comparative Example 4. In other words, the increase in the compressive strength of the shear panel 10 increases the initial stiffness K of the shear wall 1, and as a result, the yield point displacement δv decreases without a significant decrease in the ultimate displacement δu of the shear wall. As a result, the plasticity factor μ (= δu / δv) of the shear wall 1 increases relatively significantly, and thus the short-term allowable shear strength Pa and wall factor increase.

[0092] [Regarding the Increase in the Ductility Factor μ with Increased Initial Stiffness K] As mentioned above, the ultimate strength (corrected value) Pu' is the ultimate strength Pu corrected based on the ductility factor μ. The short-term allowable shear strength Pa is the ultimate strength (corrected value) Pu' multiplied by a predetermined reduction factor α and a dispersion factor β. The wall factor is the short-term allowable shear strength Pa divided by a predetermined reference strength value (L × 1.96). Therefore, the wall factor and short-term allowable shear strength Pa are proportional to the ultimate strength Pu and increase with an increase in the ductility factor μ. The ductility factor μ is proportional to the ultimate displacement δu and inversely proportional to the yield point displacement δv. Therefore, the wall factor and short-term allowable shear strength Pa can be increased by increasing the ultimate displacement δu or decreasing the yield point displacement δv.

[0093] 9 shows the test results of each specimen of Reference Examples 1 to 4 and Comparative Example 4 as a linear graph of the load-deformation angle characteristics of the completely elastic-plastic model. -3The linear function line Y=KX in the linear elastic region set at 100 kN / 10 rad is shown by a two-dot chain line as the reference line for the initial stiffness K in the present disclosure. Furthermore, Fig. 9 shows the linear function lines Y=K1X to Y=K5X in the linear elastic region, the ultimate strengths Pu1 to Pu5, and the yield points σs1 to σs5 for each of the test specimens of Reference Examples 1 to 4 and Comparative Example 4. As shown in Fig. 8, the initial stiffness of each of the test specimens of Reference Examples 1 to 4 was K4=2.04 kN / 10 at the minimum. -3 rad, and at the maximum value, K3 = 2.91 kN / 10 -3 On the other hand, the initial rigidity of the specimen of Comparative Example 4 is K5 = 1.94 kN / 10 -3 rad. The initial stiffness K appears in FIG. 9 as the gradient of the linear function line of Y = KX. -3 In the specimens of Reference Examples 1 to 4 showing values ​​of rad or more, the linear function lines of Y = K1-4X show the initial stiffness K = 2.0 kN / 10 -3 9 as a straight line steeper than the reference line of 1.0 kN / 10 rad. -3 In Comparative Example 4, which shows a value less than rad, the linear function line of Y = K5X is -3 9 as a straight line with a gentler gradient than the reference line of 1.0 kN / 10 rad. That is, in each of the specimens of Reference Examples 1 to 4 in which the compressive strength was increased, the initial stiffness K1-4 was 2.0 kN / 10 -3 rad or more, resulting in relatively small yield point displacements δv1 to δv4, which, combined with the relatively large ultimate displacements δu1 to δu4 and ultimate strengths Pu1 to Pu4, result in relatively large ultimate strengths (corrected values) Pu', short-term allowable shear strength Pa, and wall factor as shown in Figure 8, compared to Comparative Example 4.

[0094] As shown in Figures 8 and 9, the initial stiffness K of each test specimen in Reference Examples 1 to 4 was 2.0 kN / 10 -3 rad, and the initial rigidity K of the specimen of Comparative Example 4 was 2.0 kN / 10 -3rad, and the yield point displacements δv1 to δv4 of the specimens of Reference Examples 1 to 4 are significantly smaller than the yield point displacement δv5 of the specimen of Comparative Example 4. As shown in Figure 8, the wall factor and short-term allowable shear strength Pa obtained by the specimens of Reference Examples 1 to 4 are significantly larger than the wall factor and short-term allowable shear strength Pa obtained by the specimen of Comparative Example 4. This is thought to be the result of the increase in plasticity factor μ accompanying the decrease in yield point displacement δv making a relatively large contribution to the increase in the wall factor and short-term allowable shear strength Pa.

[0095] As described above, the bearing wall 1 according to this embodiment has the following features: (1) The bearing face material 10 exhibits a nail lateral resistance of 500 N or more and a nail lateral resistance of 6.5 N / mm 2 The wall is constructed of a main or core material made of a plate-shaped gypsum hardened body containing inorganic fibers and organic strength-improving materials to maintain the above compressive strength, and a paper member covering at least the front and back surfaces of the main or core material. The surface density of the bearing surface material 10, specified as the mass per unit area of ​​the wall surface, is 6.5 to 8.9 kg / m 2 In the bearing wall 1 using the low-density gypsum-based bearing surface material 10 with increased compressive strength and nail lateral resistance, the head diameter D is set to a value within the range of 6.0 to 10.0 mm, the trunk diameter d is set to a value within the range of 2.0 to 5.0 mm, and the head area / trunk cross-sectional area ratio η is set to a value within the range of 6 to 13. This prevents the head 21 from penetrating into the surface material 10, suppresses or reduces the punching shear phenomenon, and suppresses cracks in the surface material 10 that may occur during nail driving. Furthermore, the short-term allowable shear strength Pa of the bearing wall 1 can be effectively increased (therefore, the wall factor can be effectively increased). (2) In the bearing wall 1 using the low-density gypsum-based bearing surface material 10 with increased compressive strength and nail lateral resistance as described above, the ultimate displacement δu can be, for example, 28.09 x 10 -3 ~34.98 x 10 -3 rad, and therefore, the ultimate displacement δu of the bearing wall using a conventional gypsum-based bearing surface material (for example, the gypsum-based bearing surface material described in Patent Document 4) increases by 20 × 10 -3rad, the ultimate displacement δu of the bearing wall 1 increases significantly. (3) In the bearing wall 1 using the low-density gypsum-based bearing surface material 10 with increased compressive strength and nail lateral resistance as described above, as explained as the yield point displacements δv1 to δv4 of the bearing walls 1 according to Reference Examples 1 to 4 (FIGS. 8 and 9), the increase in initial stiffness K is accompanied by an increase in the ultimate displacement δu of 6.04×10 -3 ~6.80 x 10 -3 rad, and this value is the yield point displacement δv5 of the bearing wall according to Comparative Example 4 = 7.26 × 10 -3 rad. That is, the bearing face materials 10 described above as Reference Examples 1 to 4 not only increase the ultimate displacements δu1 to δu4 of the bearing wall 1 to increase the plasticity factor μ, but also increase the plasticity factor μ by reducing the yield point displacements δv1 to δv4 of the bearing wall 1, thereby enabling a relatively large increase in the wall ratio and short-term allowable shear strength Pa.

[0096] The above describes in detail preferred embodiments and examples of the present disclosure, but it goes without saying that the present disclosure is not limited to the above embodiments and examples, and various modifications and changes are possible within the scope of the present disclosure described in the claims.

[0097] For example, although the above embodiments and examples relate to a bearing wall at the first floor level of a wooden building, the present disclosure can be similarly applied to a bearing wall at the second or third floor level. In the case of a bearing wall at the second or third floor level, the lower end of the bearing face material is fastened to a cross member or the like at the second or third floor level.

[0098] Furthermore, although the above embodiments and examples relate to a wooden frame construction and large wall construction load-bearing wall structure, the present disclosure may also be applied to a wooden frame construction and a load-bearing wall structure with a solid wall construction or a floor-first (floor-first) and large wall construction. As a modified example, the present disclosure may also be applied to a wooden frame construction and load-bearing wall structure, in which case the load-bearing face material is fastened to the vertical frame, lower frame, upper frame, etc. instead of the foundation, columns, and cross members.

[0099] Furthermore, although the specimen shown in Figure 3 is constructed by dividing the gypsum board into upper and lower halves and arranging a tether at the midpoint in the height direction, it is also possible to conduct an in-plane shear test using gypsum boards with a height dimension substantially equal to the total height of the wooden framework. In the latter case, it is believed that the short-term standard shear strength can be further increased.

[0100] The present disclosure is applied to a wooden structural shear wall of a wooden structure building and a construction method thereof. In particular, the present disclosure is applied to a shear wall of a wooden structure building and a construction method thereof. 2 The present disclosure is applicable to a wooden structural shear wall and a construction method thereof, in which a low-density gypsum-based shear face material is fastened to a wooden structural wall substrate of a wooden frame construction method using metal nails, and the shear face material has an areal density within the range of 1000 N and is composed mainly or as a core of a plate-shaped gypsum hardened body mixed with inorganic fibers and organic strength-enhancing materials so as to exhibit a nail lateral resistance of 500 N or more. The present disclosure is also applicable to a method for increasing the wall factor of a wooden structural shear wall using such gypsum-based shear face material. The present disclosure further applies to such wooden structural shear walls, the method for increasing the wall factor, and the gypsum-based shear face material used in the construction method. According to the present disclosure, by fastening a load-bearing panel to a wooden structural wall substrate using metal nails having a specific shape and size, it is possible to increase the wall ratio of a wooden structural wall without additionally attaching reinforcing or stiffening materials, without increasing the specific gravity and / or thickness of the gypsum-based panel, and without further increasing the value of the ultimate displacement (δu), and therefore the practical value or effect thereof is remarkable.

[0101] This international application claims priority based on Japanese Patent Application No. 2022-122390, filed on July 30, 2022, the entire contents of which are incorporated herein by reference.

[0102] DESCRIPTION OF SYMBOLS 1 Bearing wall 2 Sill 3 Column 4 Partition 4' Joint column 5 Cross member (beam, girth, eaves beam, gable beam) 5' Girth joint 10, 10a, 10b Gypsum-based bearing surface material 11 Flat gypsum core (gypsum core material) 12 Base paper for gypsum board (paper component) 20 Nail (fastener) 21 Head 21a Top surface 21b Seat surface 22 Body 23 Neck 24 Tip D Head diameter d Body diameter L Length η Area ratio of head area / body cross-sectional area

Claims

1. In a wooden structural wall having a structure in which a gypsum-based load-bearing surface material is fastened to the wooden structural wall base of a wooden frame construction method or a wooden frame wall construction method with fasteners, the load-bearing surface material is composed of a main material or core material made of a plate-shaped gypsum hardened body and a paper member covering at least the front and back surfaces of the main material or core material, and the surface density or surface weight of the load-bearing surface material, specified as the mass per unit area of ​​the wall surface, is 6.5 to 8.9 kg / m 2 and has an areal density or areal weight within the range of 500 N or more and a nail side resistance of at least 6.5 N / mm 2 The fastener is made of a metal nail having a head and a body, and the area ratio of the head area to the cross-sectional area of ​​the body is set to a value within the range of 6 to 13. The ultimate displacement of the bearing wall measured by an in-plane shear test using a bearing wall specimen having a wall length of 1.82 m is 20 x 10 -3 A wooden structural load-bearing wall having an ultimate displacement (δu) greater than rad.

2. A wooden structural load-bearing wall as described in claim 1, characterized in that the body of the nail is a straight, smooth body having a uniform circular cross section and a pointed tip, and the head of the nail is a flat head or a flat head with a mesh pattern having a circular contour in top view.

3. A wooden structural load-bearing wall as described in claim 1, characterized in that the nail has an annular and flat seating surface that seats on the outer surface of the load-bearing face material by the nailing operation, and a flat top surface that is constructed so as to be located after nailing in substantially the same plane as the wall surface formed by the outer surface of the load-bearing face material.

4. In the wooden structural bearing wall described in any one of claims 1 to 3, the bearing surface material has an initial stiffness (K) of the bearing wall measured by the in-plane shear test of 2.2 kN / 10 -3 rad or more, 7.5N / mm 2 A wooden structural load-bearing wall characterized by having the above compressive strength.

5. In the wooden structural bearing wall described in any one of claims 1 to 3, the physical properties of the bearing wall measured by the in-plane shear test are as follows: (1) 7.2 x 10 -3 rad or less, (2) a yield point displacement (δv) of 100 MPa or less, (3) a plasticity factor (μ) of 4.2 or more, (4) a corrected value (Pu') of the ultimate strength (Pu) of 7.7 kN or more, and (5) a yield strength (Py) of 7.7 kN or more that is greater than the corrected value (Pu') of the ultimate strength (Pu), wherein at least one of the physical properties is ensured by setting the areal density or areal weight and the nail lateral resistance, and by setting the head diameter, body diameter, and head area / body cross-sectional area ratio of the nails to suppress punching shear phenomenon or reduce the effect of punching-out destruction.

6. A wooden structural load-bearing wall according to any one of claims 1 to 3, characterized in that the load-bearing face material has a board thickness of less than 12 mm and / or a specific gravity of 0.96 or less.

7. A wooden structural load-bearing wall as described in claim 1, characterized in that the main material or the core material of the load-bearing surface material is blended with inorganic fibers and / or organic strength-enhancing materials.

8. A wooden structural load-bearing wall according to claim 1 or 7, characterized in that the main material or core material of the gypsum-based load-bearing surface material contains an organopolysiloxane compound.

9. In a construction method for wooden structural bearing walls in which a gypsum-based bearing surface material is fixed to the wooden structural wall base of a wooden frame construction method or a wooden frame wall construction method, the gypsum-based bearing surface material is composed of a main material or core material made of a plate-shaped gypsum hardened body and a paper material covering at least the front and back surfaces of the main material or core material, and the surface density or surface weight specified as the mass per unit area of ​​the wall surface is 6.5 to 8.9 kg / m 2 and having a surface density or surface weight within the range of 500 N or more and a nail side resistance of at least 6.5 N / mm 2A gypsum-based load-bearing surface material having a compressive strength of 1.82 m or more is fastened to the wooden structural wall base by a fastener, and a metal nail having a head area / body cross-sectional area ratio set to a value within the range of 6 to 13 is used as the fastener. The ultimate displacement (δu) of the load-bearing wall measured by an in-plane shear test using a load-bearing wall specimen having a wall length of 1.82 m is 20 x 10 -3 A construction method for a wooden structural load-bearing wall, comprising constructing a wooden structural load-bearing wall that exerts an ultimate displacement greater than rad.

10. A method for constructing a wooden structural load-bearing wall as described in claim 9, characterized in that the body of the nail is a straight, smooth body having a uniform circular cross-section and has a steeple-shaped tip, and the head of the nail is a flat head or a flat head with a mesh pattern having a circular contour in top view.

11. A construction method for wooden structural load-bearing walls as described in claim 9, characterized in that the nail has an annular and flat seating surface that seats on the outer surface of the load-bearing face material by the nailing operation, and a flat top surface that is constructed so as to be located after nailing in substantially the same plane as the wall surface formed by the outer surface of the load-bearing face material.

12. In the method for constructing a wooden structural bearing wall according to any one of claims 9 to 11, the initial stiffness (K) of the bearing wall measured by the in-plane shear test is 2.2 kN / 10 -3 rad or more, 7.5N / mm 2 A construction method for a wooden structural load-bearing wall, characterized in that the wall has the above compressive strength.

13. In the construction method for a wooden structural bearing wall according to any one of claims 9 to 11, the physical properties of the bearing wall measured by the in-plane shear test are as follows: (1) 7.2 x 10 -3rad or less, (2) a yield point displacement (δv) of 100 rad or less, (3) a plasticity factor (μ) of 4.2 or more, (4) a corrected value (Pu') of the ultimate strength (Pu) of 7.7 kN or more, and (5) a yield strength (Py) of 7.7 kN or more and greater than the corrected value (Pu') of the ultimate strength (Pu), wherein at least one of the physical properties is ensured by setting the areal density or areal weight and the nail lateral resistance, and by setting the head diameter, body diameter, and head area / body area ratio of the nails to suppress punching shear phenomenon or reduce the effect of punching-out destruction.

14. A construction method for a wooden structural load-bearing wall as claimed in any one of claims 9 to 11, characterized in that the load-bearing face material has a board thickness of less than 12 mm and / or a specific gravity of 0.96 or less.

15. A construction method for wooden structural load-bearing walls as described in claim 9, characterized in that the main material or the core material of the load-bearing surface material is blended with inorganic fibers and / or organic strength-enhancing materials.

16. A construction method for a wooden structural load-bearing wall as described in claim 9 or 15, characterized in that the main material or core material of the gypsum-based load-bearing surface material contains an organopolysiloxane compound.

17. A method for increasing the wall strength of a wooden structural wall, which is implemented by fastening a gypsum-based strength surface material to the wooden structural wall base of a wooden frame construction method or a wooden frame wall construction method with fasteners, comprising: forming the strength surface material from a main material or core material made of a plate-shaped gypsum hardened body and a paper member covering at least the front and back surfaces of the main material or core material; and setting the surface density or surface weight of the strength surface material, specified as the mass per unit area of ​​the wall surface, to 6.5 to 8.9 kg / m 2 and the load-bearing surface material has a nail side resistance of 500 N or more and a nail side resistance of 6.5 N / mm 2The composition of the gypsum hardened body of the main material or the core material is set so as to exhibit a compressive strength of 1000 mm or more, a metal nail having a head area / body cross-sectional area ratio set to a value within a range of 6 to 13 is used as the fastener to suppress the punching shear phenomenon or reduce the effect of punching out destruction, and the ultimate displacement (δu) of the bearing wall measured by an in-plane shear test using a bearing wall specimen having a wall length of 1.82 m is 20 x 10 -3 A method for increasing the wall factor of a wooden structural load-bearing wall, characterized in that an ultimate displacement greater than rad is obtained.

18. A method for increasing the wall factor of a wooden structural load-bearing wall as described in claim 17, characterized in that the shaft of the nail is a straight, smooth shaft having a uniform circular cross section and is provided with a steeple-shaped tip, and the head of the nail is a flat head or a flat head with a mesh pattern having a circular contour in top view.

19. A method for increasing the wall factor of a wooden structural load-bearing wall as described in claim 17, characterized in that the nail has an annular and flat seating surface that seats on the outer surface of the load-bearing face material by the nailing operation, and a flat top surface that is constructed so as to be located after nailing in substantially the same plane as the wall surface formed by the outer surface of the load-bearing face material.

20. In the method for increasing the wall ratio of a wooden structural load-bearing wall according to any one of claims 17 to 19, the initial stiffness (K) of the load-bearing wall measured by the in-plane shear test is 2.2 kN / 10 -3 rad or more, 7.5N / mm 2 A method for increasing the wall strength of a wooden structural wall, comprising: making the bearing surface material retain the above compressive strength.

21. In the method for increasing the wall factor of a wooden structural load-bearing wall according to any one of claims 17 to 19, the physical properties of the front load-bearing wall measured by the in-plane shear test are as follows: (1) 7.2 x 10 -3rad or less, (2) a yield point displacement (δv) of 100 MPa or less, (3) a plasticity factor (μ) of 4.2 or more, (4) a corrected value (Pu') of the ultimate strength (Pu) of 7.7 kN or more, and (5) a yield strength (Py) of 7.7 kN or more and greater than the corrected value (Pu') of the ultimate strength (Pu), wherein at least one of the physical properties is ensured by setting the areal density or areal weight and the nail lateral resistance, and by setting the head diameter, body diameter, and head area / body area ratio of the nail, which are set to suppress punching shear phenomenon or reduce the effect of punching-out destruction.

22. A method for increasing the wall factor of a wooden structural load-bearing wall as claimed in any one of claims 17 to 19, characterized in that the load-bearing face material has a board thickness of less than 12 mm and / or a specific gravity of 0.96 or less.

23. A method for increasing the wall strength factor of a wooden structural load-bearing wall as described in claim 17, characterized in that the main material or the core material of the load-bearing surface material is blended with inorganic fibers and / or organic strength-enhancing materials.

24. A method for increasing the wall factor of a wooden structural load-bearing wall as described in claim 17 or 23, characterized in that an organopolysiloxane compound is blended in the main material or core material of the gypsum-based load-bearing surface material.

25. A gypsum-based load-bearing surface material for wooden load-bearing walls, which is used in the construction method for wooden load-bearing walls described in claim 9 or in the method for increasing the wall factor of a wooden load-bearing wall described in claim 17 and is fastened to the wooden load-bearing wall base of a wooden frame construction method or a wooden frame wall construction method by the fastener, exhibits a nail side resistance of 500 N or more and has a nail side resistance of at least 6.5 N / mm 2 It has a compressive strength of 6.5 to 8.9 kg / m 2 and in cooperation with the fastener, the ultimate displacement (δu) of the bearing wall measured by an in-plane shear test using a bearing wall specimen having a wall length of 1.82 m is 20×10 -3A gypsum-based load-bearing surface material characterized in that the load-bearing strength is increased to a value greater than rad.

26. A gypsum-based load-bearing surface material as described in claim 25, characterized in that the load-bearing surface material has a plate thickness of less than 12 mm and / or a specific gravity of 0.96 or less.

27. In the gypsum-based load-bearing surface material described in claim 25 or 26, the initial stiffness (K) of the load-bearing wall measured by the in-plane shear test is 2.2 kN / 10 -3 rad or more, 7.5N / mm 2 A gypsum-based load-bearing surface material characterized by having the above compressive strength.

28. A gypsum-based load-bearing surface material according to claim 25 or 26, characterized in that at least one of the physical properties of the load-bearing wall measured by the in-plane shear test, consisting of: (1) a yield point displacement (δv) of 7.2 x 10-3 rad or less; (2) a plasticity factor (μ) of 4.2 or more; (3) a corrected value (Pu') of an ultimate strength (Pu) of 7.7 kN or more; and (4) a yield strength (Py) of 7.7 kN or more that is greater than the corrected value (Pu') of the ultimate strength (Pu). is ensured by setting the areal density or areal weight and the nail lateral resistance, and by setting the head diameter, body diameter, and area ratio of the nail (head area / body cross-sectional area) to suppress punching shear phenomenon or reduce punching-out failure.

29. A gypsum-based load-bearing surface material as claimed in claim 25 or 26, characterized in that said gypsum-based load-bearing surface material has a nail lateral resistance of 980N or less.

30. A gypsum-based load-bearing surface material as described in claim 25, characterized in that the main material or the core material of the load-bearing surface material is blended with inorganic fibers and / or organic strength-enhancing materials.

31. A gypsum-based load-bearing surface material as claimed in claim 25 or 30, characterized in that the main material or core material of said gypsum-based load-bearing surface material contains an organopolysiloxane compound.