Preparation method for quantum chip, quantum chip, and quantum computer

In the preparation of quantum chips, positive photoresist is used to prepare metallized pads and air bridges, and negative photoresist is used to prepare metal pillar solder joints, and the glue is removed uniformly to solve the problem of air bridge bubbling and solder joint materials. Residual problems improve chip preparation efficiency and performance.

WO2024174406A9PCT designated stage expired Publication Date: 2024-10-03TENCENT TECHNOLOGY (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/097342
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-21
Filing Date
2023-05-31
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

In the process of preparing superconducting quantum chips, based on flip-chip soldering technology, the air bridge structure is prone to bubbling problems, leading to distortion and deformation, and residual metal wires affect chip performance, and cracks in the photoresist will cause solder joint material residues. Affect chip yield and performance.

Method used

Use positive photoresist to prepare metallized pads and air bridges, combine with negative photoresist to prepare metal pillar solder joints, and remove the glue uniformly to avoid air holes and solder joint material residues, improving preparation efficiency and chip performance.

Benefits of technology

By combining the method of positive and negative photoresists, one-time glue removal molding can be achieved to avoid bubbling problems, improve the performance of the air bridge, and protect the substrate through the cracking of the negative photoresist, reducing metal wire residues and improving quantum efficiency. Chip yield and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023097342_03102024_PF_FP_ABST
    Figure CN2023097342_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed are a preparation method for a quantum chip, a quantum chip, and a quantum computer, relating to the technical field of quantum chips. The method comprises: spin-coating a positive photoresist on a substrate, and preparing a metalized pad layer and an air bridge on the substrate spin-coated with the positive photoresist, so as to obtain a first substrate structure (701); spin-coating a negative photoresist on the first substrate structure, and preparing a metal column solder joint on the first substrate structure spin-coated with the negative photoresist, so as to obtain a second substrate structure (702); and removing the positive photoresist and the negative photoresist from the second substrate structure so as to obtain a quantum chip comprising the metalized pad layer, the air bridge, and the metal column solder joint (703). By using the method provided in embodiments, the preparation efficiency can be improved, and the chip performance can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Quantum chip preparation method, quantum chip and quantum computer

[0001] This application claims priority to Chinese patent application number 202310171588.6, filed on February 21, 2023, entitled “Method for preparing quantum chip and superconducting quantum chip”, the entire contents of which are incorporated herein by reference. Technical Field

[0002] The embodiments of the present application relate to the field of quantum chip technology, and in particular to a method for preparing a quantum chip, a quantum chip, and a quantum computer. Background Art

[0003] Microwave signals are transmitted through coplanar waveguides in superconducting quantum chips. When the lines on the quantum chip become more and more dense, signal crosstalk between the coplanar waveguides will occur. To alleviate the wiring problem, quantum chips based on flip-chip technology can be prepared.

[0004] In the prior art, the air bridge structure in a flip-chip quantum chip is typically prepared first, followed by the metal pillar solder joints. When the air bridge structure is prepared first, followed by the metal pillar solder joints, photoresist must be spin-coated. During this process, the air bridge below the bridge body is difficult to fill, resulting in unfilled air holes, which can subsequently cause bubbling and distortion of the air bridge. Furthermore, bubbling can cause cracking of the photoresist and, during the solder joint material evaporation process, can leave metal filaments, leading to changes in the chip circuitry.

[0005] It can be seen that the solutions in the related art will affect the yield of the air bridge, and the residual metal wire will also affect the performance of the chip.

[0006] Summary of the Invention

[0007] The embodiments of the present application provide a method for preparing a quantum chip, a quantum chip, and a quantum computer, which can improve the efficiency of preparing quantum chips based on flip-chip technology and improve chip performance. The technical solution is as follows:

[0008] In one aspect, an embodiment of the present application provides a method for preparing a quantum chip, the method being performed by a lithography apparatus, the method comprising:

[0009] Spin-coating a positive photoresist on a substrate, and preparing the metallized pad layer and the air bridge on the substrate based on the positive photoresist to obtain a first substrate structure;

[0010] Spin-coating a negative photoresist on the first substrate structure, and preparing the metal column solder joint based on the negative photoresist to obtain a second substrate structure;

[0011] The positive photoresist and the negative photoresist are removed from the second substrate structure to obtain the flip-chip quantum chip including the metallization pad, the air bridge and the metal column solder joint.

[0012] On the other hand, an embodiment of the present application provides a device for preparing a quantum chip, the device comprising:

[0013] A first preparation module is used to spin-coat a positive photoresist on a substrate, and prepare the metallization pad and the air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure, wherein the first substrate structure has the positive photoresist after photolithography;

[0014] a second preparation module, configured to spin-coat a negative photoresist on the first substrate structure, and prepare the metal column solder joints on the first substrate structure spin-coated with the negative photoresist, to obtain a second substrate structure;

[0015] The stripping module is used to remove the positive photoresist and the negative photoresist from the second substrate structure to obtain the quantum chip including the metallization pad, the air bridge and the metal column solder joint.

[0016] On the other hand, an embodiment of the present application provides a lithography device, which includes a lithography device, a processor and a memory, wherein the memory stores at least one instruction, and the at least one instruction is loaded by the processor and controls the lithography device to implement the method for preparing a quantum chip as described in the above aspect.

[0017] On the other hand, an embodiment of the present application provides a quantum chip, the chip structure of which includes a metallized pad, an air bridge, and a metal column solder joint; the quantum chip is prepared by the quantum chip preparation method provided by the above aspect.

[0018] On the other hand, an embodiment of the present application provides a quantum computer, which includes the quantum chip described in the above aspects.

[0019] In an embodiment of the present application, after preparing a metallization pad and air bridge using positive photoresist, and metal column solder joints using negative photoresist, a unified debonding process is performed to obtain a flip-chip quantum chip comprising the metallization pad, air bridge, and metal column solder joint structure. Specifically, by combining positive and negative photoresists, a single debonding process is achieved, which improves preparation efficiency. Furthermore, since the positive photoresist is not removed during the preparation of the metal column solder joints, i.e., positive photoresist is still present under the air bridge, air holes are not generated, thereby avoiding bubbling and improving the performance of the air bridge. Furthermore, if cracks occur in the negative photoresist during the preparation of the metal column solder joints, the remaining positive photoresist protects the substrate, preventing metal filaments from remaining on the substrate due to cracks, thereby helping to improve the yield and performance of the quantum chip. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] FIG1 shows a schematic structural diagram of a flip-chip quantum chip provided by an exemplary embodiment of the present application;

[0021] FIG2 shows a schematic structural diagram of an air bridge provided by an exemplary embodiment of the present application;

[0022] FIG3 is a schematic diagram showing an air hole caused in the related art;

[0023] FIG4 shows a flow chart of a method for preparing a quantum chip provided by an exemplary embodiment of the present application;

[0024] FIG5 shows a schematic structural diagram of a metal column solder joint prepared based on a negative photoresist according to an exemplary embodiment of the present application;

[0025] FIG6 shows a flow chart of a method for preparing a quantum chip provided by another exemplary embodiment of the present application;

[0026] FIG7 is a schematic cross-sectional view showing a process for preparing a quantum chip according to an exemplary embodiment of the present application;

[0027] FIG8 shows a flow chart of a method for preparing a quantum chip provided by another exemplary embodiment of the present application;

[0028] FIG9 is a schematic cross-sectional view showing a process for preparing a quantum chip according to another exemplary embodiment of the present application;

[0029] FIG10 shows a flow chart of a method for preparing a quantum chip provided by another exemplary embodiment of the present application;

[0030] FIG11 is a block diagram of a quantum chip manufacturing apparatus according to an exemplary embodiment of the present application. DETAILED DESCRIPTION

[0031] In order to make the objectives, technical solutions and advantages of this application clearer, the implementation methods of this application will be further described in detail below with reference to the accompanying drawings.

[0032] In this document, "plurality" refers to two or more. "And / or" describes a relationship between associated objects, indicating that three possible relationships exist. For example, "A and / or B" can mean: A exists alone, A and B exist simultaneously, or B exists alone. The character " / " generally indicates an "or" relationship between the associated objects.

[0033] First, a brief introduction to the terms involved in the embodiments of this application is given:

[0034] A flip-chip quantum chip is made by bonding two chips, each with a metal post pad. The metal post pads on the top chip contact the metal post pads on the bottom chip, connecting the circuits on the two chips. As shown in Figure 1, the flip-chip quantum chip includes an air bridge 101, a metallized pad 102, and metal post pads 103.

[0035] Metal pillar solder joints: solder joint structures formed by superconducting elements, used to achieve circuit connections between different chips. As shown in Figure 1, metal pillar solder joints 103 are formed on both the top and bottom sheets.

[0036] Under Bump Metallization (UBM): placed between the superconducting metal film layer where the coplanar waveguide is located and the metal column solder joints, used to prevent the metal column solder joints from alloying with the superconducting metal film layer where the coplanar waveguide is located.

[0037] Coplanar waveguide, also known as a coplanar microstrip transmission line, consists of a central conductor (also known as the center strip) and two semi-infinite ground planes (also known as ground strips). As shown in Figure 1, a coplanar waveguide consisting of a center strip 104 and a ground strip 105 is formed on a substrate.

[0038] Air bridge: A three-dimensional bridge structure made of superconducting material, typically placed on a substrate, used to connect the infinite ground planes on either side of a coplanar waveguide, or to connect two separate coplanar waveguide center conductors. As shown in Figure 1, air bridge 101 connects ground straps 105 on either side. Air bridges can be categorized as discrete air bridges or fully enclosed air bridges. The difference between discrete and fully enclosed air bridges lies in whether the bridge body is continuous.

[0039] An air bridge consists of piers and a bridge body. During the air bridge fabrication process, the bridge support structure is first prepared. The air bridge, i.e., the piers and bridge body, are then fabricated based on the support structure. After the air bridge is fabricated, the support is released, completing the air bridge fabrication. Figure 2 shows a side view of an air bridge. First, a support 201 is fabricated. Then, a bridge body 202 and piers 203 are fabricated based on support 201 to form the air bridge structure. Finally, support 201 is released through a process to complete the air bridge.

[0040] Superconducting quantum chips transmit microwave signals through coplanar waveguides. As the computing power of quantum chips increases, the number of coplanar waveguides increases, and the number of lines on the quantum chip increases, which may cause signal crosstalk between coplanar waveguides. In related technologies, the chip wiring problem can be alleviated based on flip-chip packaging technology. As shown in Figure 1, the flip-chip quantum chip connects two different chips through metal column solder joints 103, so that the lines can be distributed on different chips, alleviating the problem of wiring congestion. At the same time, an air bridge is prepared on the coplanar waveguide to connect the ground planes on both sides of the coplanar waveguide, thereby reducing the signal crosstalk problem on different coplanar waveguides.

[0041] During the fabrication of superconducting quantum chips using flip-chip technology, because the metal pillar solder joints may form an alloy with the superconducting metal film layer corresponding to the coplanar waveguide on the substrate, a metallized pad is deposited between the metal pillar solder joints and the superconducting metal film layer to prevent alloying. Furthermore, the geometric height of the air bridge is typically lower than that of the metal pillar solder joints, and the corresponding photoresist height for the air bridge is also lower than that for the metal pillar solder joints. Therefore, to prevent patterns higher than the photoresist thickness from affecting the photoresist spread, the air bridge is usually deposited first, followed by the metal pillar solder joints.

[0042] In related technologies, the UBM layer, air bridges, and metal pillar solder joints are typically fabricated in separate steps. As shown in Figure 3, a UBM layer 301 is first formed on a substrate with a coplanar waveguide using photoresist. Air bridges 302 are then formed on the substrate. Finally, metal pillar solder joints are formed on the substrate containing the UBM layer 301 and air bridges 302. This process is complex, requiring multiple exposures and can easily damage the chip.

[0043] In addition, when preparing metal column solder joints, photoresist needs to be spin-coated. Due to the fluidity of the photoresist, it will flow under the air bridge. For a fully enclosed air bridge, due to the poor fluidity of the photoresist under the bridge, the photoresist will not be filled and air holes will appear. As shown in Figure 3, photoresist 303 is spin-coated on a substrate including a UBM layer 301 and an air bridge 302, and an air hole 304 appears under the bridge of the air bridge 302. When the air hole 304 exists, since the photoresist needs to be soft-baked at a high temperature, the gas remaining in the air hole will expand and contract due to heat and cold to form bubbles on the air bridge 302. In the subsequent metal evaporation process, the bubbles may further expand, causing squeezing of the air bridge 302, thereby affecting the yield of the air bridge.

[0044] In addition, when preparing metal column solder joints, the pressure from the external environment may cause the photoresist to crack. If the above-mentioned bubbling problem exists, stress will exist inside the photoresist, which will more easily cause the photoresist to crack. In the subsequent process of evaporating the solder joint material, the solder joint material will fill the cracks, leaving solder joint material at the corresponding position of the substrate, which may affect the circuit on the chip and affect the chip performance.

[0045] To address the above-mentioned issues, the present invention proposes a method for preparing a quantum chip in an embodiment. This method simplifies the flip-chip fabrication process and avoids air bridge bubbling and solder material residue, thereby improving chip performance. The following describes an exemplary method of the method provided in the embodiment of the present invention.

[0046] Please refer to Figure 4, which shows a flow chart of a method for preparing a quantum chip provided by an exemplary embodiment of the present application. This embodiment uses the method for a lithography device as an example to illustrate the method, and the method includes the following steps:

[0047] Step 401 : spin-coating a positive photoresist on a substrate, and preparing a metallized pad layer and an air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure.

[0048] The method provided in the embodiments of the present application is used to prepare a quantum chip based on flip-chip technology, wherein the chip structure of the quantum chip includes a UBM layer, an air bridge, and a metal column solder joint.

[0049] The quantum chip fabrication process relies on photoresist fabrication. Photoresists can be divided into positive and negative photoresists based on whether the exposed areas are removed or retained during the development process. With positive photoresists, the exposed areas undergo a chemical reaction and dissolve in the developer, while the unexposed areas do not. The resulting photoresist pattern is identical to the mask. With negative photoresists, the exposed areas become insoluble in the developer due to crosslinking and curing, while the unexposed areas do. The resulting photoresist pattern is the opposite of the mask.

[0050] In one possible embodiment, a photolithography device may use positive photoresist to form a UBM layer and an air bridge on a substrate with a coplanar waveguide. The UBM layer and the air bridge may be formed simultaneously or in steps.

[0051] Optionally, the positive photoresist may be SPR220 or 6350A photoresist.

[0052] In some embodiments, after the UBM layer and the air bridge are prepared, a first substrate structure including the UBM layer and the air bridge is obtained. Since the resist has not been removed at this time, positive photoresist after photolithography still exists on the first substrate structure.

[0053] Step 402 : Spin-coat a negative photoresist on the first substrate structure, and prepare metal column solder joints on the first substrate structure spin-coated with the negative photoresist to obtain a second substrate structure.

[0054] After completing the preparation of the UMB layer and air bridge, the photolithography equipment can continue to prepare metal column solder joints based on the unremoved first substrate structure. After exposure and development, the negative photoresist forms an inverted trapezoidal undercut structure, which is conducive to the subsequent removal of the photoresist and the formation of metal columns with good morphology. Therefore, metal column solder joints can be prepared based on negative photoresist. Metal columns prepared based on negative photoresist are not easily adhered to the photoresist and are easy to remove. They also form metal column solder joints with a positive trapezoidal shape, which can facilitate subsequent pressure welding connections. As shown in Figure 5, a positive trapezoidal metal column solder joint 501 can be prepared based on negative photoresist.

[0055] Optionally, the negative photoresist may be E3510 photoresist.

[0056] In a possible implementation, a metal column solder joint can be prepared on the first substrate structure by spin-coating a negative photoresist on the first substrate structure, and then performing exposure, development, and evaporation of the solder joint material.

[0057] During the process of evaporating the solder joint material, since there is positive photoresist on the first base structure, that is, there is still positive photoresist under the air bridge body, there will be no air hole problem under the bridge body due to the flow of negative photoresist, thereby avoiding the bubbling problem.

[0058] Moreover, when the spin-coated negative photoresist has cracks, the positive photoresist can protect the substrate, preventing the solder joint material from remaining on the substrate through the cracks, which helps to improve the chip quality.

[0059] Step 403 : removing the positive photoresist and the negative photoresist from the second substrate structure to obtain a quantum chip including a metallized pad layer, an air bridge, and metal column solder joints.

[0060] Once the UBM layer, air bridge, and metal pillar solder joint structures are complete, a single stripping process removes the remaining positive and negative photoresists, completing the quantum chip fabrication process. After fabrication, a flip-chip quantum chip can be obtained through a pressure bonding process.

[0061] Optionally, the photolithography equipment can remove the photoresist using at least one of a dry process and a wet process. The dry process involves removing the photoresist using ashing. For example, the photoresist can be removed using the dry process alone, the wet process alone, or the dry process first and then the wet process.

[0062] In one possible embodiment, the photolithography equipment can be stripped by immersing the stripping solution. During the stripping process, the positive photoresist and the negative photoresist are dissolved in the stripping solution, resulting in a quantum chip containing only the UBM layer, air bridges, and metal pillar solder joints.

[0063] In summary, in the embodiments of the present application, after preparing the metallization pad and air bridge using positive photoresist, and preparing the metal column solder joints using negative photoresist, the photoresist is then removed uniformly to obtain a flip-chip quantum chip comprising the metallization pad, air bridge, and metal column solder joint structure. That is, by combining the positive and negative photoresist methods, a one-step photoresist removal process is achieved, which improves preparation efficiency. Furthermore, since the positive photoresist has not yet been removed when preparing the metal column solder joints, i.e., positive photoresist is still present under the air bridge, air holes are not generated, thereby avoiding bubbling problems and improving the performance of the air bridge. Furthermore, when preparing the metal column solder joints based on the negative photoresist, if the negative photoresist cracks, the unremoved positive photoresist also protects the substrate, preventing the problem of metal filaments remaining on the substrate due to cracks, thereby helping to improve the yield rate and chip performance of the quantum chip.

[0064] In the process of preparing the UBM layer and the air bridge, the UBM layer and the air bridge can be prepared simultaneously based on a positive photoresist, that is, the UBM layer and the air bridge can be prepared by a single exposure, simplifying the process flow.

[0065] Please refer to Figure 6, which shows a flow chart of a method for preparing a quantum chip provided by another exemplary embodiment of the present application. The method includes the following steps:

[0066] Step 601 , spin-coating a positive photoresist on a substrate, and using a grayscale exposure method, photolithography the photoresist area corresponding to the metallized pad layer and the air bridge in the positive photoresist to obtain a first layer of photoresist.

[0067] In one possible implementation, the lithography apparatus may first spin-coat a positive photoresist on the substrate with the coplanar waveguide. Optionally, the thickness of the positive photoresist may be determined according to the height of the air bridge, wherein the thickness of the positive photoresist is greater than the height of the air bridge.

[0068] Schematically, a positive photoresist with a thickness greater than 3 μm can be spin-coated. As shown in FIG7 , a positive photoresist 701 can be spin-coated on a substrate.

[0069] Afterwards, the lithography equipment can use grayscale exposure to expose the UBM layer and the photoresist areas corresponding to the air bridges in the positive photoresist. Grayscale exposure refers to the use of different exposure light intensities for different locations of the photoresist. By controlling the exposure light intensity, the depth of the positive photoresist is controlled to obtain the desired pattern. In one possible embodiment, the lithography equipment uses grayscale exposure to expose the photoresist areas corresponding to the metallization pad layer and the air bridges in the positive photoresist, which may include steps 601a-601c (not shown):

[0070] Step 601a: determining the exposure light intensity of the photoresist region corresponding to the air bridge based on the bridge support structure of the air bridge, wherein the exposure light intensity is positively correlated with the distance from the bridge body in the bridge support structure to the positive photoresist surface.

[0071] In one possible implementation, the relationship between the light intensity at a depth x from the photoresist surface (i.e., at a position x from the photoresist surface) and the initial light intensity is as follows: I(x) = I0exp(-x / ξ)

[0072] Here, I0 refers to the initial light intensity (referring to the exposure light intensity), and ξ is a constant.

[0073] In one possible embodiment, the photolithography equipment can determine the distance between each position of the air bridge body and the surface of the positive photoresist based on the required bridge support structure of the air bridge, and determine the initial light intensity I0 corresponding to each position based on the light intensity that can expose the photoresist at depth x, so that the bridge support after photolithography has an arch structure of the required size.

[0074] Step 601b: performing grayscale exposure processing on the air bridge in the positive photoresist and the photoresist area corresponding to the metallization pad layer based on the exposure light intensity corresponding to different positions.

[0075] After determining the exposure light intensity corresponding to each position, the photolithography equipment can perform grayscale exposure processing on the photoresist area corresponding to the air bridge according to the exposure light intensity corresponding to different positions, so that the photoresist above the air bridge body is exposed through and dissolved after development to form an arched bridge support.

[0076] For the photoresist areas corresponding to the UBM layer, the lithography equipment can use the same exposure light intensity to expose all the photoresist above the UBM layer. As shown in Figure 7, grayscale exposure is performed on the photoresist area 702 corresponding to the air bridge and the photoresist area 703 corresponding to the UBM layer (where the length of the arrow represents the intensity of the exposure light).

[0077] By adopting the grayscale exposure method, only the photoresist area corresponding to the air bridge and the photoresist area corresponding to the UBM layer need to be exposed once, which helps to shorten the process flow and help reduce the probability of chip damage.

[0078] In a possible implementation, during the exposure process, the photolithography equipment may cover the positive photoresist except the exposure area with a mask, and then apply light to perform the exposure process.

[0079] Step 601c: developing the positive photoresist after the exposure process to obtain a first layer of photoresist.

[0080] After the exposure process, a development process is required to dissolve the exposed photoresist and complete the photolithography process of the photoresist area corresponding to the air bridge and the UBM layer. The positive photoresist that has not been photolithographically processed is the first layer of photoresist.

[0081] Schematically, as shown in FIG. 7 , after the development process, a first layer of photoresist 704 that has not been photolithographically processed is obtained.

[0082] In step 602 , ion milling is performed on the coplanar waveguide exposed on the substrate after photolithography. During the ion milling process, a denatured photoresist is formed on the surface of the first layer of photoresist, and the denatured photoresist is steep.

[0083] Since there is a natural oxide layer on the superconducting metal film layer where the coplanar waveguide is located, in order to form a good superconducting contact, the lithography equipment needs to perform ion milling on the coplanar waveguide exposed on the substrate after lithography to remove the natural oxide layer and prevent the natural oxide layer from affecting the superconducting contact.

[0084] In a possible implementation, the photolithography equipment may bombard the superconducting metal film layer where the coplanar waveguide is located with 7 sccm of Ar ions for 5 minutes in a 1E-4 torr vacuum environment.

[0085] During ion milling, the entire substrate is bombarded with ions, including the first layer of photoresist. This results in a layer of denatured photoresist on the surface. However, due to the use of grayscale exposure, the photoresist is steep, with steep sidewalls at the edges of the air bridges. Therefore, during the subsequent stripping process, the denatured photoresist is removed along with the undenatured layer below, without affecting the stripping process or chip quality.

[0086] Schematically, as shown in FIG7 , the photolithography equipment performs ion milling on the coplanar waveguide exposed on the substrate after photolithography to remove the natural oxide layer 705 and simultaneously form a denatured photoresist 706 on the surface of the first photoresist layer.

[0087] Step 603: vapor-deposit a superconducting material on the first layer of photoresist to obtain a first substrate structure.

[0088] After ion milling, the superconducting material can be evaporated. In one possible embodiment, the lithography equipment uses in-situ evaporation of the superconducting material. In-situ refers to a multi-step process performed within a single vacuum chamber or multiple interconnected vacuum chambers. In this embodiment, the lithography equipment performs the ion milling process and the superconducting material evaporation process within a vacuum chamber to avoid the formation of a natural oxide layer on the surface of the superconducting metal film layer due to exposure to air before evaporating the superconducting material.

[0089] During the superconducting material evaporation process, the photolithography equipment evaporates a layer of superconducting material on the areas corresponding to the UBM layer and the areas corresponding to the air bridges, thereby forming a UBM layer structure and an air bridge structure. In other words, the evaporated superconducting material forms both the air bridge and the UBM layer. Optionally, the superconducting material can be titanium nitride (TiN), niobium (Nb), etc. This embodiment of the application is not limited to a specific superconducting material.

[0090] Since the UBM layer is used to prevent alloying between the metal column solder joints and the superconducting metal film layer where the coplanar waveguide is located, the superconducting material used to prepare the UBM layer must not form an alloy with the superconducting metal film layer corresponding to the coplanar waveguide, nor with the solder joint material corresponding to the metal column solder joints. That is, the selection of superconducting material is determined based on the materials of the superconducting metal film layer and the metal solder joints.

[0091] For example, when the superconducting metal film layer where the coplanar waveguide is located is aluminum (Al), and the solder joint material used for the metal pillar solder joint is indium (In), the superconducting material can be Nb. The lithography equipment can in-situ evaporate a layer of superconducting material Nb greater than 300 nm thick on the first layer of photoresist.

[0092] In one possible embodiment, after evaporating a superconducting material onto the first layer of photoresist, a UBM layer and an air bridge structure are formed, resulting in a first substrate structure comprising the UBM layer and the air bridges. As shown in FIG7 , after evaporating the superconducting material, a UBM layer 707 and air bridges 708 are formed, resulting in a first substrate structure comprising the UBM layer, the air bridges, and the unremoved positive photoresist.

[0093] Step 604 , spin-coating a negative photoresist on the first substrate structure, and photolithography the area of ​​the negative photoresist except for the metal column welding point to obtain a second layer of photoresist.

[0094] In the embodiment of the present application, after the UBM layer and the air bridge are prepared using positive photoresist, the photolithography equipment directly prepares the metal column solder joints based on the substrate without removing the resist, and removes the resist uniformly after the preparation of the metal column solder joints is completed.

[0095] In one possible embodiment, a photolithography apparatus uses a negative photoresist to prepare metal post solder joints. The photolithography apparatus first spin-coats a layer of negative photoresist onto a first substrate structure. The thickness of the negative photoresist can be determined based on the desired height of the metal post solder joints, and the thickness of the negative photoresist is greater than the height of the metal post solder joints. Optionally, if the height of the metal post solder joints is 10 μm, the thickness of the negative photoresist is greater than 10 μm. Illustratively, a 16 μm thick layer of E3510 negative photoresist can be spin-coated onto the first substrate structure. As shown in FIG. 7 , negative photoresist 709 is spin-coated onto the first substrate structure.

[0096] After spin coating the negative photoresist, photolithography can be performed. Since negative photoresist is used, the area other than the metal column welding point in the negative photoresist can be photolithographically processed, so that the area other than the metal column welding point is retained and the photoresist in the area corresponding to the metal column welding point is removed.

[0097] The photolithography process may include steps 604a-604b (not shown in the figure):

[0098] Step 604a, performing exposure processing on the photoresist area except the metal pillar welding point in the negative photoresist.

[0099] In contrast to the photolithography process of positive photoresist, the photolithography equipment performs exposure processing on the photoresist area except the metal pillar welding point. Optionally, the photolithography equipment can use ultraviolet light for exposure processing.

[0100] Step 604b: developing the negative photoresist after the exposure process to obtain a second layer of photoresist.

[0101] The photolithography equipment performs a development process after the exposure process, so that the negative photoresist in the area corresponding to the unexposed metal column welding point is dissolved to form an undercut structure, and the remaining undissolved negative photoresist forms a second layer of photoresist.

[0102] Schematically, as shown in FIG. 7 , a photolithography device performs exposure processing on the area of ​​the negative photoresist 709 except for the metal column welding point, and then performs development processing with a developer to form an undercut structure 710 .

[0103] Step 605 , vapor-depositing solder joint material on the second layer of photoresist to obtain a second substrate structure.

[0104] After photolithography is complete, solder material can be evaporated to create metal pillar solder joints. Because the substrate leaves the vacuum environment during spin-coating of the negative photoresist, a natural oxide layer forms on the surface of the UBM layer. As shown in Figure 7, a natural oxide layer 711 forms on the UBM layer. (Superconducting material evaporated elsewhere will also be oxidized; only the natural oxide layer on the UBM layer is shown in the figure.) Therefore, to form a good superconducting contact, the photolithography equipment must first perform ion milling to remove the natural oxide layer on the UBM layer before evaporating the solder material.

[0105] In one possible embodiment, after ion milling, in order to avoid the formation of a natural oxide layer again, the photolithography equipment evaporates the solder joint material in situ. Since the photoresist in the area corresponding to the metal column solder joint is removed, the photolithography equipment can evaporate a layer of solder joint material on the UBM layer to form a metal column solder joint.

[0106] Alternatively, the solder joint material can be indium, and an indium pillar solder joint can be fabricated on the UBM layer. For example, 10 μm of indium can be evaporated to form the indium pillar solder joint. As shown in Figure 7, the lithography equipment first performs ion milling to remove the native oxide layer 711 on the UBM layer. Then, a layer of solder joint material is in-situ evaporated to form a metal pillar solder joint 712.

[0107] During the ion milling process, the negative photoresist may crack due to ion bombardment, and solder material may fill these cracks during the evaporation process. However, because the first layer of photoresist (positive photoresist) below is less prone to cracking (thicker than the negative photoresist), it blocks the solder material and prevents solder material residue. As shown in Figure 7, when the negative photoresist 709 cracks, cracks 713 are formed. The positive photoresist below provides protection, preventing solder material from remaining on the coplanar waveguide substrate.

[0108] After evaporating the solder joint material, a second substrate structure including metal column solder joints can be obtained.

[0109] Step 606 , removing the positive photoresist and the negative photoresist from the second substrate structure to obtain a quantum chip including a metallized pad layer, an air bridge, and metal pillar solder joints.

[0110] After the metal column solder joints are prepared, the photolithography equipment can perform stripping to remove both the positive photoresist and the negative photoresist to complete the chip preparation.

[0111] Schematically, as shown in FIG7 , after peeling and debonding, a quantum chip including a UBM layer, an air bridge, and metal column solder joints is obtained.

[0112] In this embodiment, the UBM layer and air bridge are formed through a single exposure process, which simplifies the process flow and reduces the probability of chip damage during exposure. Furthermore, compared to positive photoresist, metal pillar solder joints prepared using negative photoresist are less likely to cause adhesion issues and can produce metal pillar solder joints with better morphology.

[0113] In the above embodiment, the air bridge body is prepared by grayscale exposure to form an arched bridge support structure. In another possible embodiment, the air bridge body can also be prepared by reflow. The following will be described using an exemplary embodiment.

[0114] Please refer to Figure 8, which shows a flow chart of a method for preparing a quantum chip provided by another exemplary embodiment of the present application. The method includes the following steps:

[0115] Step 801 , spin-coating a positive photoresist on a substrate, and performing exposure and development processing on the photoresist region corresponding to the metallized pad layer in the positive photoresist to obtain a first layer of positive photoresist.

[0116] In one possible embodiment, the UBM layer and air bridge can be prepared in a step-by-step process. When preparing the UBM layer, the lithography equipment first spin-coats a positive photoresist onto the substrate. Then, the photoresist region corresponding to the UBM layer is photolithographically exposed and developed, resulting in a first positive photoresist layer. This first positive photoresist layer is the positive photoresist remaining after removing the photoresist region corresponding to the UBM layer.

[0117] Step 802 : vapor-depositing a first layer of superconducting material on the first layer of positive photoresist, and stripping the first layer of positive photoresist to obtain a substrate with a metallized pad layer.

[0118] The photolithography equipment deposits the first layer of superconducting material onto the first layer of positive photoresist to form the UBM layer. Prior to deposition, ion milling can be performed to remove the natural oxide layer on the UBM region of the coplanar waveguide, ensuring that the deposited UBM layer forms a good superconducting contact with the superconducting metal film layer where the coplanar waveguide resides.

[0119] Optionally, the first layer of superconducting material may be TiN, Nb, etc.

[0120] After the preparation is completed, the photolithography equipment can strip off the first layer of positive photoresist to obtain a substrate with a metallized pad layer.

[0121] Step 803 , spin-coating a positive photoresist on the substrate having the metallized pad layer, and performing exposure and development processing on the area corresponding to the air bridge in the positive photoresist to obtain a second layer of positive photoresist.

[0122] After the metallized pad layer is prepared, the air bridge can be prepared. In one possible embodiment, during the air bridge preparation process, the photolithography equipment can spin-coat a positive photoresist on the substrate, and then perform an exposure and development process on the bridge pier area corresponding to the air bridge to obtain a second layer of positive photoresist.

[0123] Step 804 , reflowing the second positive photoresist layer, and evaporating a second layer of superconducting material on the reflowed second positive photoresist layer.

[0124] After photolithography of the bridge pier area, the lithography equipment can reflow the second layer of positive photoresist. Reflow refers to the process of baking the photoresist to a certain temperature, causing the sidewall morphology of the photoresist to change. In one possible embodiment, the lithography equipment can use high-temperature reflow to circularize the sidewalls of the photoresist corresponding to the bridge pier area, resulting in an arched photoresist structure, which can be used to prepare the bridge support structure. Alternatively, the lithography equipment can reflow the positive photoresist by heating the substrate at high temperature.

[0125] After the reflow process, a second layer of superconducting material can be evaporated to form an air bridge. This process may include steps 804a-804b (not shown in the figure):

[0126] In step 804a, ion milling is performed on the coplanar waveguide exposed on the substrate after the reflow treatment, wherein during the ion milling process, a denatured photoresist is formed on the surface of the second positive photoresist layer, and the denatured photoresist is continuous.

[0127] Among them, there is a natural oxide layer above the coplanar waveguide exposed on the substrate (that is, the coplanar waveguide corresponding to the pier area). In order to form a good superconducting contact between the air bridge and the coplanar waveguide, ion milling treatment is required first.

[0128] However, during the ion milling process, denatured photoresist will form on the surface of the second positive photoresist layer. And because the denatured photoresist is continuous after the reflow process, a continuous denatured photoresist will form at the edge of the air bridge (adhering to the air bridge pier), so subsequent stripping treatment is required.

[0129] Step 804b: vapor-depositing a second layer of superconducting material on the second layer of positive photoresist after ion milling.

[0130] After the ion milling process, the lithography equipment can evaporate a second layer of superconducting material onto the second layer of positive photoresist to create an air bridge.

[0131] Step 805 : spin-coating a third layer of positive photoresist on the second layer of superconducting material, and etching the second layer of superconducting material based on the third layer of positive photoresist to obtain a first substrate structure.

[0132] Since the evaporated superconducting material will cover the entire sample, the superconducting material needs to be etched to obtain the bridge body and bridge piers of the air bridge. In one possible implementation, an etching solution can be used to remove the superconducting material outside the air bridge.

[0133] To protect the air bridge's body and piers from etching, they can be covered with photoresist for protection. During this process, the lithography equipment first spin-coats a third layer of positive photoresist onto the second layer of superconducting material. The photoresist is then exposed and developed in areas other than the air bridge body and piers, leaving only the positive photoresist on the air bridge body and piers. Etching is then performed to remove the superconducting material in other areas, creating the air bridge and the first substrate structure. This first substrate structure comprises the UBM layer, the air bridge, and the remaining positive photoresist.

[0134] Schematically, as shown in FIG9 , the first substrate structure includes a UBM layer 901 , an air bridge 902 , a second positive photoresist layer 903 and a third positive photoresist layer 904 .

[0135] Step 806: Clean the denatured photoresist using plasma.

[0136] During the above process, ion milling treatment is performed to produce denatured photoresist. Since the bridge structure is prepared by reflow treatment, the denatured photoresist is continuous and cannot be removed along with the undenatured positive photoresist below. Therefore, the photolithography equipment needs to use plasma to remove the denatured photoresist first.

[0137] Schematically, as shown in FIG9 , the photolithography equipment removes the denatured photoresist 905 on the second positive photoresist layer 903 by plasma cleaning.

[0138] In one possible implementation, oxygen plasma may be used to remove the denatured photoresist on the surface. For example, the photoresist may be cleaned for 2 minutes using a plasma of 5 sccm O2, 100 Pa, and 300 W to remove the denatured photoresist adhering to the air bridge piers.

[0139] Step 807 , performing a flood exposure process on the positive photoresist on the first substrate structure.

[0140] In this embodiment, the metal stud solder joints are prepared without removing the positive photoresist. During the aforementioned step-by-step preparation of the UBM layer and the air bridge, a second layer of positive photoresist remains on the UBM layer from the air bridge preparation process. Therefore, the second layer of positive photoresist must be removed to expose the UBM layer before the metal stud solder joints are prepared on the UBM layer. Therefore, the photolithography equipment first performs a flood exposure process on the positive photoresist on the first substrate structure. Flood exposure refers to exposing the entire positive photoresist layer without using a mask. Subsequently, during development, the positive photoresist on the UBM layer is dissolved.

[0141] For example, the lithography equipment can use 9mW / cm 2 UV flood exposure for 10 s.

[0142] Step 808 : Spin-coat a negative photoresist on the first substrate structure, and prepare metal column solder joints on the first substrate structure spin-coated with the negative photoresist to obtain a second substrate structure.

[0143] After the flood exposure process, a negative photoresist can be spin-coated on the first substrate structure to prepare the metal pillar solder joints based on the negative photoresist. During the preparation process, the photolithography equipment can first expose the negative photoresist in the area other than the metal pillar solder joints, and then perform a development process. During the development process, the unexposed negative photoresist is dissolved, that is, the negative photoresist in the area corresponding to the metal pillar solder joints is dissolved. At the same time, because the positive photoresist has been flood exposed in advance, the positive photoresist on the UBM layer is also dissolved.

[0144] Schematically, as shown in FIG9 , a negative photoresist 906 can be spin-coated on the first substrate structure, and then the negative photoresist in areas other than the metal column solder joints is exposed and then developed. During the development process, the positive photoresist 907 and the negative photoresist 906 on the UBM layer are both dissolved.

[0145] After the photoresist is photolithographically processed, ion milling can be performed to remove the natural oxide layer, and then solder joint material can be evaporated in situ to form metal column solder joints to obtain a second substrate structure.

[0146] As shown in FIG. 9 , after the ion milling process, the natural oxide layer 908 on the UBM layer is removed, and then the solder joint material is in-situ evaporated to prepare the metal column solder joint.

[0147] Step 809 , removing the positive photoresist and the negative photoresist from the second substrate structure to obtain a quantum chip including a metallized pad layer, an air bridge, and metal column solder joints.

[0148] The implementation of this step can refer to the above-mentioned step 606, which will not be described in detail in this embodiment.

[0149] In this embodiment, the air bridge can be formed by reflow. During this process, the denatured photoresist is removed by plasma. By adding a flood exposure method, the metal pillar solder joints can be formed using a negative photoresist without removing the positive photoresist. This allows the UBM layer, air bridge, and metal pillar solder joints to be formed in a single stripping process, simplifying the process. Furthermore, the positive photoresist protects the air bridge structure and the base, helping to improve the quality of the air bridge and chip performance.

[0150] In one possible embodiment, the metal column solder joints may be indium column solder joints. Please refer to FIG10 , which shows a flow chart of the complete preparation process of a quantum chip provided by an exemplary embodiment of the present application, using grayscale exposure as an example. The process includes:

[0151] Step 1001: spin-coat a first layer of positive photoresist on a substrate.

[0152] Optionally, the photolithography equipment can spin-coat a first layer of positive photoresist with a thickness greater than 3 μm on the substrate with the coplanar waveguide. The positive photoresist can be SPR220, 6350A, etc.

[0153] Step 1002 : Photolithography of air bridge and UBM regions.

[0154] Optionally, the photolithography equipment may expose the air bridge and the UBM area using a grayscale exposure method, and then perform a development process after exposure to complete the photolithography.

[0155] Step 1003: evaporating superconducting metal.

[0156] Optionally, the superconducting metal can be Nb. The lithography equipment first bombards the superconducting metal film layer where the coplanar waveguide resides with 7 sccm of Ar ions for 5 minutes in a 1E-4 torr vacuum environment. Then, a layer of superconducting metal thicker than 300 nm is in situ evaporated. As shown in Figure 10, after the superconducting metal is evaporated, the substrate contains a positive photoresist, air bridges, and a UBM layer.

[0157] Step 1004 , spin-coating a second layer of negative photoresist.

[0158] Optionally, the photolithography equipment can spin-coat E3510 negative photoresist with a thickness of 16 μm.

[0159] Step 1005 , photolithography the area outside the indium column solder joint.

[0160] The photolithography equipment can perform exposure and development processing on the area outside the indium column solder joint to remove the negative photoresist in the area corresponding to the indium column solder joint.

[0161] Step 1006: Indium plating.

[0162] Before indium vapor deposition, the lithography equipment first needs to remove the native oxide layer on the UBM layer through ion milling. After ion milling, vapor deposition is performed to obtain the indium pillar solder joint.

[0163] Step 1007, peeling and removing the glue.

[0164] Optionally, the photolithography equipment performs stripping and debonding using a debonding solution to remove the first layer of positive photoresist and the second layer of negative photoresist.

[0165] Please refer to Figure 11, which shows a block diagram of a device for preparing a quantum chip according to an exemplary embodiment of the present application. The device includes:

[0166] A first preparation module 1101 is configured to spin-coat a positive photoresist on a substrate, and prepare a metallized pad and an air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure;

[0167] A second preparation module 1102 is configured to spin-coat a negative photoresist on the first substrate structure, and prepare metal column solder joints on the first substrate structure spin-coated with the negative photoresist to obtain a second substrate structure;

[0168] The stripping module 1103 is used to remove the positive photoresist and the negative photoresist from the second substrate structure to obtain the quantum chip including the metallization pad, the air bridge and the metal column solder joints.

[0169] Optionally, the first preparation module 1101 is used to:

[0170] Using a grayscale exposure method, photolithography is performed on the photoresist region corresponding to the metallized pad layer and the air bridge in the positive photoresist to obtain a first layer of photoresist;

[0171] A superconducting material is evaporated on the first photoresist layer to obtain the first substrate structure.

[0172] Optionally, the first preparation module 1101 is used to:

[0173] Determining, based on the bridge support structure of the air bridge, the exposure light intensity of the photoresist region corresponding to the air bridge, wherein the exposure light intensity is positively correlated with the distance from the bridge body in the bridge support structure to the surface of the positive photoresist;

[0174] Based on the exposure light intensity corresponding to different positions, grayscale exposure processing is performed on the air bridge in the positive photoresist and the photoresist area corresponding to the metallization pad layer;

[0175] The positive photoresist after the exposure process is developed to obtain the first layer of photoresist.

[0176] Optional, ion milling module for:

[0177] The coplanar waveguide exposed on the substrate after photolithography is subjected to ion milling treatment, wherein during the ion milling treatment, a denatured photoresist is formed on the surface of the first photoresist layer, and the denatured photoresist is steep.

[0178] Optionally, the first preparation module 1101 is used to:

[0179] performing exposure and development processing on the photoresist region corresponding to the metallized pad layer in the positive photoresist to obtain a first layer of positive photoresist;

[0180] Vapor-depositing a first layer of superconducting material on the first layer of positive photoresist, and stripping the first layer of positive photoresist to obtain a substrate having the metallized pad layer;

[0181] Spin coating the positive photoresist on the substrate having the metallized pad layer, and performing exposure and development treatment on the area corresponding to the air bridge in the positive photoresist to obtain a second layer of positive photoresist;

[0182] performing a reflow process on the second positive photoresist layer, and evaporating a second layer of superconducting material on the reflowed second positive photoresist layer;

[0183] A third layer of positive photoresist is spin-coated on the second layer of superconducting material, and the second layer of superconducting material is etched based on the third layer of positive photoresist to obtain the first substrate structure.

[0184] Optionally, the first preparation module 1101 is used to:

[0185] performing ion milling on the coplanar waveguide exposed on the substrate after the reflow treatment, wherein during the ion milling process, a denatured photoresist is formed on the surface of the second positive photoresist layer, and the denatured photoresist is continuous;

[0186] vapor-depositing the second layer of superconducting material on the second layer of positive photoresist after ion milling;

[0187] The stripping module is also used to clean the denatured photoresist using plasma.

[0188] Optionally, the device further includes:

[0189] The flood exposure module is used to perform flood exposure processing on the positive photoresist on the first substrate structure.

[0190] Optionally, the second preparation module 1102 is used to:

[0191] Photolithography of the negative photoresist except for the metal column welding point to obtain a second layer of photoresist;

[0192] A solder joint material is evaporated on the second layer of photoresist to obtain the second substrate structure.

[0193] Optionally, the second preparation module 1102 is used to:

[0194] performing an exposure process on the photoresist region in the negative photoresist except the metal column welding point;

[0195] The negative photoresist after the exposure process is developed to obtain the second layer of photoresist.

[0196] Optionally, the superconducting material used in the metallized pad does not form an alloy with the superconducting metal film layer corresponding to the coplanar waveguide, and does not form an alloy with the solder joint material corresponding to the metal column solder joint.

[0197] Optionally, the superconducting material used for the metallized pad and the air bridge is niobium, and the solder joint material used for the metal column solder joint is indium.

[0198] An embodiment of the present application also provides a lithography device, which includes a lithography device, a processor and a memory, wherein at least one instruction is stored in the memory, and the at least one instruction is loaded by the processor and controls the lithography device to implement the method for preparing a quantum chip as described in the above embodiment.

[0199] An embodiment of the present application further provides a quantum chip, wherein the chip structure of the quantum chip includes a metallized pad, an air bridge, and metal column solder joints; the quantum chip is prepared by the quantum chip preparation method described in the above embodiment.

[0200] An embodiment of the present application also provides a quantum computer, which includes the quantum chip described in the above embodiment.

[0201] The above description is merely an optional embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A method for preparing a quantum chip, the method being performed by a photolithography device, the method comprising: Spin-coating a positive photoresist on a substrate, and preparing a metallized pad layer and an air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure; Spin-coating a negative photoresist on the first substrate structure, and preparing a metal column welding point on the first substrate structure spin-coated with the negative photoresist to obtain a second substrate structure; The positive photoresist and the negative photoresist are removed from the second substrate structure to obtain the quantum chip including the metallization pad, the air bridge and the metal column solder joint.

2. The method according to claim 1, wherein: The step of preparing a metallized pad layer and an air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure comprises: Using a grayscale exposure method, photolithography is performed on the photoresist region corresponding to the metallization pad layer and the air bridge in the positive photoresist to obtain a first layer of photoresist; A superconducting material is evaporated on the first layer of photoresist to obtain the first substrate structure.

3. The method according to claim 2, wherein: The method of using a grayscale exposure method to photolithographically process the metallized pad layer and the area corresponding to the air bridge in the positive photoresist to obtain a first layer of photoresist includes: Based on the bridge support structure of the air bridge, determining the exposure light intensity of the photoresist region corresponding to the air bridge, wherein the exposure light intensity is positively correlated with the distance from the bridge body in the bridge support structure to the surface of the positive photoresist; Based on the exposure light intensity corresponding to different positions, grayscale exposure processing is performed on the air bridge in the positive photoresist and the photoresist area corresponding to the metallization pad layer; The positive photoresist after the exposure process is developed to obtain the first layer of photoresist.

4. The method according to claim 2 or 3, wherein: After the grayscale exposure method is adopted to photolithography the metallization pad layer and the area corresponding to the air bridge in the positive photoresist to obtain the first layer of photoresist, the method further comprises: The coplanar waveguide exposed on the substrate after photolithography is subjected to ion milling treatment, wherein during the ion milling treatment, a denatured photoresist is formed on the surface of the first layer of photoresist, and the denatured photoresist is steep.

5. The method according to claim 1, wherein: The step of preparing a metallized pad layer and an air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure comprises: Performing exposure and development processing on the photoresist region corresponding to the metallized pad layer in the positive photoresist to obtain a first layer of positive photoresist; Vapor-depositing a first layer of superconducting material on the first layer of positive photoresist, and removing the first layer of positive photoresist to obtain a substrate having the metallized pad layer; Spin coating the positive photoresist on the substrate having the metallized pad layer, and performing exposure and development treatment on the area corresponding to the air bridge in the positive photoresist to obtain a second layer of positive photoresist; performing a reflow treatment on the second layer of positive photoresist, and evaporating a second layer of superconducting material on the reflowed second layer of positive photoresist; A third layer of positive photoresist is spin-coated on the second layer of superconducting material, and the second layer of superconducting material is etched based on the third layer of positive photoresist to obtain the first substrate structure.

6. The method according to claim 5, wherein: The step of evaporating a second layer of superconducting material on the second layer of positive photoresist after the reflow treatment comprises: Performing ion milling on the coplanar waveguide exposed on the substrate after the reflow treatment, wherein during the ion milling process, a denatured photoresist is formed on the surface of the second layer of positive photoresist, and the denatured photoresist is continuous; Vapor depositing the second layer of superconducting material on the second layer of positive photoresist after ion milling; After the second layer of superconducting material is etched based on the third layer of positive photoresist to obtain the first substrate structure, the method further includes: The denatured photoresist is cleaned by plasma.

7. The method according to claim 5 or 6, wherein: After the second layer of superconducting material is etched based on the third layer of positive photoresist to obtain the first substrate structure, the method further includes: The positive photoresist on the first substrate structure is subjected to a flood exposure process.

8. The method according to any one of claims 1 to 7, wherein: The step of preparing metal column welding points on the first substrate structure spin-coated with the negative photoresist to obtain a second substrate structure comprises: Photolithography of the area except the metal column welding point in the negative photoresist to obtain a second layer of photoresist; A solder joint material is evaporated on the second layer of photoresist to obtain the second substrate structure.

9. The method according to claim 8, wherein: The photolithography of the area of ​​the negative photoresist except the metal column welding point to obtain a second layer of photoresist comprises: Performing exposure processing on the photoresist area except the metal column welding point in the negative photoresist; The negative photoresist after the exposure process is developed to obtain the second layer of photoresist.

10. The method according to any one of claims 1 to 7, wherein: The superconducting material used in the metallized pad does not form an alloy with the superconducting metal film layer corresponding to the coplanar waveguide, and does not form an alloy with the soldering point material corresponding to the metal column soldering point.

11. The method according to claim 10, wherein: The superconducting material used in the metallized pad and the air bridge is niobium, and the welding point material used in the metal column welding point is indium.

12. A device for preparing a quantum chip, the device comprising: The first preparation module is used to spin-coat a positive photoresist on a substrate, and to prepare the metallized pad layer and the air bridge on the substrate spin-coated with the positive photoresist to obtain a first substrate structure. The first substrate structure has a positive photoresist after photolithography; A second preparation module is used for spin-coating a negative photoresist on the first substrate structure, and preparing the metal column welding point on the first substrate structure spin-coated with the negative photoresist to obtain a second substrate structure; The stripping module is used to remove the positive photoresist and the negative photoresist from the second substrate structure to obtain the quantum chip including the metallization pad, the air bridge and the metal column welding point.

13. A lithography device, comprising a lithography device, a processor and a memory, wherein the memory stores at least one instruction, and the at least one instruction is loaded by the processor and controls the lithography device to implement the method for preparing a quantum chip as described in any one of claims 1 to 11.

14. A quantum chip, wherein the chip structure of the quantum chip comprises a metallized pad, an air bridge and a metal column solder joint; the quantum chip is prepared by the method for preparing a quantum chip according to any one of claims 1 to 11.

15. A quantum computer, comprising the quantum chip according to claim 14.