Cured product, cured product-containing carbon material, negative electrode, and nonaqueous secondary battery

By bonding modifying elements to carbon materials and using a cured product with polyoxyalkylene and siloxane structures, the challenges of elution and swelling in lithium ion secondary batteries are addressed, resulting in improved durability and efficiency for lithium ion secondary batteries.

WO2024190840A1PCT designated stage expired Publication Date: 2024-09-19MITSUBISHI CHEM CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009866
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-14
Filing Date
2024-03-13
Publication Date
2024-09-19

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face issues with the durability of carbon materials used as negative electrode active materials due to high elution rates and swelling rates with respect to water and organic solvents, leading to reduced charging/discharging efficiency and battery durability.

Method used

A carbon material with modifying components like boron, aluminum, silicon, phosphorus, or germanium is bonded to the carbon material, and a cured product containing a polyoxyalkylene structure and crosslinkable siloxane with Q units is used to reduce elution and swelling rates, promoting stable negative electrode operation and improved battery performance.

Benefits of technology

The solution enables stable negative electrode operation, maintains initial discharge capacity, and reduces elution and swelling rates, enhancing the durability and efficiency of lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention pertains to a cured product that contains a three-dimensional siloxane structure having a polyoxyalkylene structure and a Q unit, and that has a swelling rate to ethyl methyl carbonate of 70 mass % or less.
Need to check novelty before this filing date? Find Prior Art

Description

Cured product, carbon material containing cured product, negative electrode and non-aqueous secondary battery

[0001] The present invention relates to a cured product, a cured-product-containing carbon material containing the cured product, a negative electrode, and a nonaqueous secondary battery.

[0002] The present invention also relates to a composition, a cured product, a method for producing a cured product, a carbon material containing the cured product, a method for producing a carbon material containing the cured product, a method for producing a negative electrode, and a method for producing a secondary battery.

[0003] In recent years, the miniaturization of electronic devices has led to an increasing demand for high-capacity secondary batteries. In particular, secondary batteries, especially lithium-ion secondary batteries, have attracted attention because they have higher energy density and superior charge / discharge characteristics than nickel-cadmium batteries and nickel-metal hydride batteries.

[0004] As a lithium-ion secondary battery, a positive electrode and a negative electrode capable of absorbing and releasing lithium ions, and LiPF 6 and LiBF 4 Non-aqueous lithium secondary batteries, which consist of a non-aqueous electrolyte solution in which lithium salts such as lithium ions are dissolved, have been developed and put to practical use. Lithium ion secondary batteries are made up of positive and negative electrodes that can absorb and release lithium ions, and LiPF 6 and LiBF 4 Non-aqueous lithium secondary batteries using a non-aqueous electrolyte solution in which lithium salts such as those mentioned above are dissolved have been developed and put to practical use.

[0005] Initially, lithium metal was used as the negative electrode active material for lithium-ion secondary batteries. However, it was discovered that repeated charge and discharge cycles could cause dendrite-like lithium to precipitate, penetrate the separator, and reach the positive electrode, potentially causing a short circuit. Therefore, carbon materials, which allow lithium ions to enter and exit the interlayer during the charge and discharge process and prevent lithium metal from precipitation, are now attracting attention as negative electrode active materials.

[0006] For example, Patent Document 1 discloses a negative electrode material for a lithium secondary battery, characterized in that two or more different polymer materials are attached to particles (A) selected from the group consisting of carbon material particles, metal particles, and metal oxide particles, at different positions on the particles. This material can be produced by a simple process, and is said to be capable of realizing a lithium secondary battery that is excellent in a balanced range of battery properties, such as electrode plate strength, immersion resistance, initial irreversible capacity, high current density charge / discharge characteristics, and cycle retention rate.

[0007] Furthermore, Patent Document 2 discloses a carbon material coated with a compound in which a water-soluble polymer is crosslinked with a silane coupling agent.

[0008] Japanese Unexamined Patent Publication No. 2007-042285 Japanese Unexamined Patent Publication No. 9-161848

[0009] When a carbon material such as graphite is used as a negative electrode active material in a lithium ion secondary battery, it is believed that lithium ions intercalate from the edge portions of the graphene structure of the carbon material.

[0010] However, lithium ions are solvated in the electrolyte, and if they intercalate into the carbon material while still in the solvated state, the interlayer space between the graphene layers will be destroyed, resulting in a decrease in their function as a negative electrode active material and a shortened lifespan of the lithium-ion secondary battery.

[0011] To address this issue, a compound that forms a coating on the edges of the graphene structure during charging can be added to the electrolyte as an additive, which promotes desolvation of lithium ions when they intercalate, improving the durability of the negative electrode active material.

[0012] However, the addition of additives to the electrolyte solution has trade-offs, such as an effect on the positive electrode and a decrease in the lithium ion conductivity in the electrolyte solution, and the amount and type of compounds that can be added are limited.

[0013] Therefore, in the above-mentioned Patent Document 1, two or more different polymer materials are attached to carbon material particles to improve the durability as a negative electrode active material. However, the polymer materials have difficulty in covering the edge portions of the graphene structure of the carbon material, and there is room for improvement in terms of durability, i.e., stable negative electrode operation.

[0014] Therefore, a first object of the present invention is to provide a carbon material that enables stable negative electrode operation when used as a negative electrode active material in a lithium ion secondary battery. Another object of the present invention is to provide a method for producing such a carbon material, and a method for producing a negative electrode and a secondary battery using the carbon material.

[0015] Furthermore, as in Patent Document 2, when a carbon material coated with a compound containing a three-dimensional siloxane structure without Q units is used in the negative electrode of a secondary battery, there is a problem that the elution rate and swelling rate in water or organic solvents cannot be sufficiently reduced. If the elution rate in water is high, when the coated carbon material is used to prepare a slurry in an aqueous system, components derived from the water-soluble polymer are significantly eluted from the coating layer, resulting in the coating layer being peeled off or damaged by mechanical processing such as kneading. If the elution rate in organic solvents is high, components derived from the water-soluble polymer are eluted inside the secondary battery, resulting in defects and resulting in poor charge / discharge efficiency and durability of the secondary battery. Furthermore, if the swelling rate in water or organic solvents is high, a lot of energy and time are required to remove water or organic solvent from the negative electrode when coating the carbon material or manufacturing the secondary battery, resulting in poor productivity. Furthermore, the water or organic solvent that is not completely removed remains in the secondary battery during manufacturing, resulting in poor charge / discharge efficiency and durability of the secondary battery. Even if the elution rate in water or organic solvents is low, if the swelling rate in water or organic solvents is high, the electrolyte will come into contact with the surface of the carbon material, making it impossible to suppress the decomposition reaction of the electrolyte, resulting in a problem of poor durability of the secondary battery.

[0016] A second object of the present invention is to provide a cured product that can sufficiently reduce the elution rate and swelling rate in water or organic solvents, and a composition for obtaining such a cured product.

[0017] As a result of intensive research into solving the above problems, the inventors have found that, with regard to the first object, if a structure that promotes desolvation of the electrolyte can be introduced into the edge portion of the graphene structure of the carbon material, stable negative electrode operation becomes possible without adding an additive to the electrolyte, and have completed the present invention.

[0018] That is, the first gist of the present invention is as follows: Aspect A and Aspect B.

[0019] <<Aspect A>> [A1] A carbon material in which a modifying component is bonded to a carbon material raw material, wherein the modifying component contains at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium, and the total atomic concentration of the element in the carbon material is x (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g), x / y (atomic % g / m 2 ) is 0.05 to 1 atom % g / m 2 [A2] A carbon material in which the integrated area of ​​pores with a diameter of 1 nm or less, as determined by pore distribution analysis using the Grand Canonical Monte Carlo (GCMC) method of the molecular simulation method, is 0.01 m 2 [A3] The carbon material according to [A1] above, wherein the total content of the modifying components in the carbon material is 1% by volume or less. [A4] The carbon material according to any one of [A1] to [A3] above, wherein the molecular weight of the modifying components is 500 or less. [A5] The carbon material according to any one of [A1] to [A3] above, wherein the x / y (atomic % g / m 2 ) is 0.07 to 0.8 atomic % g / m 2 [A6] The carbon material according to any one of [A1] to [A4], wherein the raw carbon material contains at least one of artificial graphite and natural graphite. [A7] The carbon material according to [A6], wherein the raw carbon material contains natural graphite. [A8] The carbon material according to any one of [A1] to [A7], wherein the modifying component contains silicon as the element, and wherein x(Si), which is the atomic concentration of silicon in the carbon material, is 0.1 to 15 atomic %. [A9] The carbon material according to any one of [A1] to [A7], wherein y, which is the specific surface area of ​​the carbon material, is 1 to 15 m2 [A10] The carbon material according to any one of [A1] to [A9], having a Raman R value represented by the following formula of 0.01 to 0.7: Raman R value = (1360 cm in Raman spectrum analysis) -1 Nearby Peak P B Intensity I B ) / (1580 cm in Raman spectroscopy -1 Nearby Peak P A Intensity I A [A11] A method for producing a negative electrode, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [A1] to [A10] above, to obtain a negative electrode. [A12] A method for producing a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [A1] to [A10] above, to obtain the negative electrode.

[0020] <<Aspect B>> [B1] A method for producing a carbon material containing a carbon material raw material and silicon atoms as constituent elements, wherein the atomic concentration of the silicon atoms in the carbon material is x (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g), x / y (atomic % g / m 2 ) is 0.05 to 1 atom % g / m 2 [B2] The method for producing a carbon material according to [B1], further comprising a step of heating the mixture obtained in the mixing step.

[0021] As a result of intensive research conducted by the present inventors to solve the above problems, they discovered that, with regard to the second object, a cured product containing a polyoxyalkylene structure and a three-dimensional siloxane structure containing Q units can sufficiently reduce the elution rate and swelling rate in water or organic solvents, and thus arrived at the present invention.

[0022] That is, the second gist of the present invention is as follows: Aspects C, D, and E.

[0023] <Aspect C> [C1] A composition comprising a compound (A) having a polyoxyalkylene structure and a crosslinkable siloxane compound (B) having Q units, wherein the compound (A) has at least two crosslinkable silicon units per molecule. [C2] The composition according to [C1] above, wherein the content of the polyoxyalkylene structure in the composition is 10% by mass to 60% by mass. [C3] The composition according to [C1] or [C2] above, wherein the total content of the Q units in the composition is 10% by mass to 50% by mass. [C4] The composition according to any one of [C1] to [C3] above, wherein the compound (A) contains a crosslinkable silicon unit. [C5] The composition according to any one of [C1] to [C4] above, further comprising a solvent. [C6] The composition according to any one of [C1] to [C5] above, further comprising a boron-containing compound (C). [C7] The composition according to any one of [C1] to [C6], wherein the composition is a thermosetting composition.

[0024] <Aspect D> [D1] A cured product comprising a polyoxyalkylene structure and a three-dimensional siloxane structure having Q units, and having a swelling ratio in ethyl methyl carbonate of 70% by mass or less. [D2] The cured product according to [D1] above, wherein the content of the polyoxyalkylene structure in the cured product is 20% by mass to 80% by mass. [D3] The cured product according to [D1] or [D2] above, wherein the content of silicon atoms in the cured product is 10% by mass to 40% by mass. [D4] The cured product according to any one of [D1] to [D3] above, wherein the total content of Q units in the cured product is 20% by mass to 60% by mass. [D5] The cured product according to any one of [D1] to [D4] above, wherein after hydrolysis of the cured product, the cured product contains a polyoxyalkylene structure and a fragment having at least two silicon atoms per molecule. [D6] A cured product-containing carbon material comprising the cured product according to any one of [D1] to [D5] above and a carbon material. [D7] The carbon material comprises a carbon material raw material to which a modifying component is bonded, and the modifying component comprises at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium. [D8] The cured product-containing carbon material according to [D7] above, wherein the modifying component has a bonding site capable of bonding to the carbon material. [D9] The cured product-containing carbon material according to [D7] or [D8] above, wherein the molecular weight of the modifying component is 500 or less. [D10] The cured product-containing carbon material according to any one of [D7] to [D9] above, wherein the modifying component is represented by the following general formula (1): (Z) n-L-W (1) (In general formula (1), Z is a group capable of chemically bonding to a carbon material, W is a group containing at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur and germanium, L is a linker, and n is 1 or 2.) [D11] The cured product-containing carbon material according to [D10] above, wherein W is a group containing silicon in general formula (1). [D12] The cured product-containing carbon material according to [D10] or [D11] above, wherein Z in general formula (1) contains a structure capable of addition by a Diels-Alder reaction. [D13] The cured product-containing carbon material according to any one of [D10] to [D12] above, wherein Z in general formula (1) is a group containing an unsaturated bond at a terminal. [D14] The cured product-containing carbon material according to any one of [D10] to [D13] above, wherein Z in general formula (1) is a vinyl group. [D15] The cured product-containing carbon material according to any one of [D6] to [D14], wherein the surface of the carbon material contains a carbon-carbon unsaturated bond and a carbon radical structure. [D16] A negative electrode comprising the cured product-containing carbon material according to any one of [D6] to [D15]. [D17] A non-aqueous secondary battery comprising a positive electrode and a negative electrode capable of absorbing and desorbing lithium ions, and an electrolyte, wherein the negative electrode comprises the cured product-containing carbon material according to any one of [D6] to [D15].

[0025] <Aspect E> [E1] A method for producing a cured product, comprising heating the composition described in any one of [C1] to [C7] above. [E2] A method for producing a cured product-containing carbon material, comprising heating the composition described in any one of [C1] to [C7] above in the presence of a carbon material. [E3] A method for producing a cured product-containing carbon material described in [E2] above, wherein the cured product-containing carbon material is used as a negative electrode active material. [E4] A method for producing a negative electrode, comprising the step of forming a negative electrode active material layer on a current collector using the cured product-containing carbon material obtained by the production method described in [E3] above, to obtain a negative electrode. [E5] A method for producing a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, comprising the step of forming a negative electrode active material layer on a current collector using the cured product-containing carbon material obtained by the production method described in [E3] above, to obtain the negative electrode.

[0026] Furthermore, in relation to the first and second objects of the present invention, the third gist of the present invention, Aspect F, is as follows.

[0027] <Aspect F> [F1] A method for modifying a carbon material, comprising a step of bonding a modifying component to a carbon material. [F2] The method according to [F1], wherein the modifying component contains at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, and germanium. [F3] The method according to [F1] or [F2], wherein the modifying component has a binding site capable of binding to a carbon material. [F4] The method according to any one of [F1] to [F3], wherein the molecular weight of the modifying component is 500 or less. [F5] The method according to any one of [F1] to [F4], wherein the modifying component is represented by the following general formula (1): (Z) n-L-W (1) (In general formula (1), Z is a group capable of chemically bonding to a carbon material, W is a group containing at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur and germanium, L is a linker, and n is 1 or 2.) [F6] The modification method according to [F5] above, wherein in general formula (1), W is a group containing silicon. [F7] The modification method according to [F5] or [F6] above, wherein Z in general formula (1) contains a structure capable of addition by a Diels-Alder reaction. [F8] The modification method according to any one of [F5] to [F7] above, wherein Z in general formula (1) is a group containing an unsaturated bond at a terminal. [F9] The modification method according to any one of [F5] to [F8] above, wherein Z in general formula (1) is a vinyl group. [F10] The modification method according to any one of [F1] to [F9], wherein the surface of the carbon material contains a carbon-carbon unsaturated bond and a carbon radical structure. [F11] The modification method according to any one of [F1] to [F10], wherein the step of bonding a modifying component to the carbon material comprises physically contacting the carbon material with the modifying component. [F12] The modification method according to any one of [F1] to [F11], further comprising heating at 120°C or higher. [F13] The modification method according to any one of [F1] to [F12], further comprising, after the step of bonding a modifying component to the carbon material, contacting the resulting carbon material with a polymer containing at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium. [F14] The modification method according to [F13], further comprising heating at 120°C or higher. [F15] A modification method comprising contacting a carbon material having a modifying component bound thereto with a polymer containing at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium. [F16] The modification method according to [F15], further comprising heating at 120°C or higher.

[0028] To achieve the first object, when the carbon material according to the present invention is used as a negative electrode active material in a lithium ion secondary battery, stable negative electrode operation is possible, and high initial efficiency can be achieved while maintaining a good initial discharge capacity. Furthermore, the method for producing a carbon material according to the present invention can obtain such an excellent carbon material. Furthermore, the method for producing a negative electrode and the method for producing a secondary battery according to the present invention can obtain an excellent negative electrode and a secondary battery containing the excellent carbon material as a negative electrode active material.

[0029] With respect to the second object, the cured product of the present invention can sufficiently reduce the elution rate and swelling rate in water and organic solvents. Also, the composition of the present invention can provide a cured product that can sufficiently reduce the elution rate and swelling rate in water and organic solvents.

[0030] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be practiced with various modifications within the scope of the gist. In this specification, when the expression "to" is used, it is used as an expression including the numerical value or physical property value before and after it. Furthermore, mass % and weight %, and parts by mass and parts by weight have the same meaning.

[0031] <<Carbon Material>> In order to achieve the first object, the carbon material according to this embodiment preferably has a modifying component bonded to the raw material of the carbon material. The modifying component contains at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium (hereinafter, sometimes referred to as "constituent element of the modifying component"). The total atomic concentration of the constituent elements of the modifying component in the carbon material is defined as x (atomic %), and the specific surface area of ​​the carbon material is defined as y (m 2 / g), x / y (atomic % g / m 2 ) is between 0.05 and 1 atomic % g / m 2 is preferred.

[0032] When the modifying component in this embodiment contains silicon, the carbon material according to this embodiment contains a carbon material raw material and silicon atoms as constituent elements. (Si) (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g), x(Si) / y(atomic%・g / m 2 ) is between 0.05 and 1 atomic % g / m 2 is preferably 0.07 to 0.8 atomic % g / m 2 More preferably, 0.3 to 1 atomic % g / m 2 is more preferable.

[0033] The carbon material contains silicon atoms as a constituent element, and thus the edge portions of the graphene structure in the carbon material raw material can have a structure that promotes desolvation of lithium ions solvated with the electrolyte in a lithium ion secondary battery.

[0034] Although the reason for this is unclear, silicon atoms can form covalent bonds with carbon atoms, which facilitates the formation of strong bonds at the edge portions of the graphene structure in the carbonaceous raw material. As a result of this bonding, the electrochemically active graphene structure at the edge surfaces is replaced with less reactive silicon oxide, which facilitates desolvation of lithium ions solvated with the electrolyte in lithium-ion secondary batteries at the edge portions while suppressing side reactions. As a result, we believe that side reactions on the carbonaceous material surface and destruction of the interlayer space within the graphene structure can be suppressed.

[0035] Furthermore, when the modifying component in this embodiment contains aluminum, the carbon material according to this embodiment contains a carbon material raw material and aluminum atoms as a constituent element. (Al) (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g), x (Al) / y(atomic%・g / m 2 ) is between 0.05 and 1 atomic % g / m 2 is preferred.

[0036] By including aluminum atoms as a constituent element, the carbon material can have a structure that promotes desolvation of lithium ions solvated with the electrolyte in a lithium ion secondary battery at the edge portions of the graphene structure in the carbon material raw material.

[0037] Although the reason for this is unclear, aluminum atoms have the property of sol-gelling halides and alkoxy compounds when acidified, and therefore easily bond to acidic functional groups originating from the edge portions of the graphene structure in the carbonaceous raw material. As a result of this bonding, the chemically stable aluminum suppresses the reactivity of the electrochemically active edge surface graphene structure, making it easier for lithium ions solvated with the electrolyte in lithium-ion secondary batteries to desolvate at the edge portions while suppressing side reactions with the electrolyte. As a result, it is believed that side reactions on the carbonaceous material surface and destruction of the interlayer space within the graphene structure can be suppressed.

[0038] In this embodiment, x / y (atomic % g / m 2 ) is the specific surface area y (m 2 / g), and this value is 0.05 atomic % g / m 2 By satisfying the above, the effect of reducing side reactions due to the modifying component can be preferably exhibited. 2 ) is 1 atomic % g / m 2 By satisfying the condition of not more than 100%, it is possible to suppress an increase in the resistance to lithium ion migration due to the modifying component.

[0039] In this specification, the atomic concentration x (atomic %) of the constituent element of the modifying component in the carbon material is a value measured by X-ray photoelectron spectroscopy (XPS), specifically, a value measured under the conditions described in the examples described later. 2 / g) is a value determined by the nitrogen adsorption BET single-point method from the results of nitrogen adsorption / desorption measurement by a gas flow method, and specifically, is a value measured under the conditions described in the examples described later.

[0040] In this embodiment, x / y (atomic % g / m 2 ) is between 0.05 and 1 atomic % g / m 2 is preferably 0.07 to 0.8 atomic % g / m 2 More preferably, 0.3 to 1 atomic % g / m 2From the viewpoint of the effect of reducing side reactions, the above value is more preferably 0.05 atomic % g / m 2 Preferably, 0.07 atomic % g / m or more 2 More preferably, 0.1 atomic % g / m or more 2 More preferably, 0.15 atomic % g / m or more 2 More preferably, 0.3 atomic % g / m or more 2 or more, 0.4 atomic % g / m 2 or more, 0.5 atomic % g / m 2 From the viewpoint of suppressing an increase in resistance, the above value may be 1 atomic % g / m 2 Preferably, 0.9 atomic % g / m or less 2 More preferably, 0.8 atomic % g / m or less 2 The following is even more preferred:

[0041] In this embodiment, x (Si) / y(atomic%・g / m 2 ) is between 0.05 and 1 atomic % g / m 2 is preferably 0.07 to 0.8 atomic % g / m 2 More preferably, 0.3 to 1 atomic % g / m 2 From the viewpoint of the effect of reducing side reactions, the above value is more preferably 0.05 atomic % g / m 2 Preferably, 0.07 atomic % g / m or more 2 More preferably, 0.3 atomic % g / m or more 2 More preferably, 0.4 atomic % g / m or more 2 More preferably, 0.5 atomic % g / m or more 2 From the viewpoint of suppressing an increase in resistance, the above value is more preferably 1 atomic % g / m 2 Preferably, 0.9 atomic % g / m or less 2 More preferably, 0.8 atomic % g / m or less 2 The following is even more preferred:

[0042] In this embodiment, x (Al) / y(atomic%・g / m 2 ) is between 0.05 and 1 atomic % g / m 2From the viewpoint of the effect of reducing side reactions, the above value is preferably 0.05 atomic % g / m 2 Preferably, 0.07 atomic % g / m or more 2 More preferably, 0.1 atomic % g / m or more 2 More preferably, 0.15 atomic % g / m or more 2 From the viewpoint of suppressing an increase in resistance, the above value is more preferably 1 atomic % g / m 2 Preferably, 0.9 atomic % g / m or less 2 More preferably, 0.8 atomic % g / m or less 2 The following is even more preferred:

[0043] The total atomic concentration x (atomic %) of the constituent elements of the modifying component in the carbon material according to this embodiment is preferably 0.1 to 15 atomic %, more preferably 0.2 to 10 atomic %, and even more preferably 0.3 to 5 atomic %. From the viewpoint of the effect of reducing side reactions, the atomic concentration x (atomic %) is preferably 0.1 atomic % or more, more preferably 0.2 atomic % or more, and even more preferably 0.3 atomic % or more. Furthermore, from the viewpoint of suppressing an increase in resistance, the atomic concentration x (atomic %) is preferably 15 atomic % or less, more preferably 10 atomic % or less, and even more preferably 5 atomic % or less.

[0044] In this embodiment, x / y (atomic % g / m 2 ) is between 0.05 and 1 atomic % g / m 2 and the atomic concentration x (atomic %) is more preferably 0.1 to 15 atomic %.

[0045] The atomic concentration x of silicon atoms in the carbon material according to this embodiment (Si) (atomic %) is preferably 0.1 to 15 atomic %, more preferably 0.2 to 10 atomic %, and even more preferably 0.3 to 5 atomic %. Here, from the viewpoint of the effect of reducing side reactions, the atomic concentration x (Si) (atomic %) is preferably 0.1 atomic % or more, more preferably 0.2 atomic % or more, and even more preferably 0.3 atomic % or more. (Si) (atomic %) is preferably 15 atomic % or less, more preferably 10 atomic % or less, and even more preferably 5 atomic % or less.

[0046] The atomic concentration x of aluminum atoms in the carbon material according to this embodiment (Al) (atomic %) is preferably 0.1 to 15 atomic %, more preferably 0.2 to 10 atomic %, and even more preferably 0.3 to 5 atomic %. Here, from the viewpoint of the effect of reducing side reactions, the atomic concentration x (Al) The atomic concentration x (atomic %) is preferably 0.1 atomic % or more, more preferably 0.2 atomic % or more, and even more preferably 0.3 atomic % or more. From the viewpoint of suppressing an increase in resistance, the atomic concentration x (atomic %) is preferably 15 atomic % or less, more preferably 10 atomic % or less, and even more preferably 5 atomic % or less.

[0047] The specific surface area y (m 2 / g) is 1 to 15 m 2 / g is preferred, and 1.2 to 10m 2 / g is more preferable, and 1.4 to 5m 2 Here, from the viewpoint of ensuring sufficient sites for lithium ion intercalation / deintercalation and obtaining good high-speed charge / discharge characteristics and output characteristics, the specific surface area y (m 2 / g) is 1m 2 / g or more is preferable, and 1.2m 2 / g or more is more preferable, and 1.4m 2 / g or more is more preferable. In addition, from the viewpoint of appropriately suppressing the activity of the negative electrode active material in the electrolyte, suppressing an increase in the initial irreversible capacity, and realizing a high capacity, the specific surface area y (m 2 / g) is 15m 2 / g or less is preferable, and 10m 2 / g or less is more preferable, and 5m 2 / g or less is more preferable.

[0048] In this embodiment, x / y (atomic % g / m 2 ) is between 0.05 and 1 atomic % g / m 2 and the specific surface area y (m 2 / g) is 1 to 15 m 2 / g. It is more preferable that the atomic concentration x (atomic %) is 0.1 to 15 atomic % and the specific surface area y (m 2 / g) is 1 to 15 m2 It is more preferable that x / y (atomic % g / m 2 ) is between 0.05 and 1 atomic % g / m 2 The atomic concentration x (atomic %) is 0.1 to 15 atomic %, and the specific surface area y (m 2 / g) is 1 to 15 m 2 It is more preferable that the SiO2 content is 1 / g.

[0049] The carbon material according to this embodiment preferably contains phosphorus atoms as a modifying component, more preferably contains phosphorus atoms in addition to aluminum atoms, and more preferably has an atomic concentration of phosphorus atoms in the carbon material of 0.1 to 1 when the atomic concentration of aluminum atoms in the carbon material is 1. This makes it possible to achieve higher initial efficiency when the carbon material according to this embodiment is used as a negative electrode active material for a lithium ion secondary battery.

[0050] Although it is unclear why the initial efficiency is higher when phosphorus atoms are included in addition to aluminum atoms as constituent elements, the reason is thought to be as follows: It is thought that aluminum phosphate is partially produced by the reaction between phosphoric acid and aluminum, and that the high chemical stability and the micropores that are formed allow for more stable desolvation.

[0051] When the atomic concentration of aluminum atoms in the carbon material is taken as 1, the atomic concentration of phosphorus atoms in the carbon material, i.e., the atomic concentration ratio of phosphorus atoms, is preferably 0.1 to 1, more preferably 0.15 to 0.95, and even more preferably 0.2 to 0.9. Here, from the viewpoint of preferably obtaining the effect of including phosphorus atoms, the atomic concentration ratio of phosphorus atoms is preferably 0.1 or more, more preferably 0.15 or more, and even more preferably 0.2 or more. Furthermore, from the viewpoint of suppressing an increase in battery resistance, the atomic concentration ratio of phosphorus atoms is preferably 1 or less, more preferably 0.95 or less, and even more preferably 0.9 or less.

[0052] Furthermore, the preferred range of the atomic concentration of phosphorus atoms in the carbon material varies depending on the atomic concentration of aluminum atoms in the carbon material, but is, for example, preferably 0.01 to 15 atomic %, more preferably 0.02 to 10 atomic %, and even more preferably 0.03 to 5 atomic %. Here, from the viewpoint of optimally obtaining the effects of containing phosphorus atoms, the atomic concentration of the phosphorus atoms is preferably 0.01 atomic % or more, more preferably 0.02 atomic % or more, and even more preferably 0.03 atomic % or more. From the viewpoint of potential capacity, the atomic concentration of the phosphorus atoms is preferably 15 atomic % or less, more preferably 10 atomic % or less, and even more preferably 5 atomic % or less.

[0053] The carbon material according to this embodiment has an integrated area of ​​pores with a diameter of 1 nm or less, determined by pore distribution analysis using the Grand Canonical Monte Carlo (GCMC) method, a molecular simulation method. 2 / g or less is preferable.

[0054] Here, the adsorption simulation using the GCMC molecular simulation method is a technique for simulating the amount of adsorption at a certain pressure for a certain pore diameter. Specifically, interaction parameters such as pore diameter and shape, adsorbed molecules, and adsorbent surface atoms are determined, and adsorbed molecules are actually placed into the virtual space of the pore, and the adsorbed molecules are allowed to move, be created, and disappear. Then, if the energy of the system becomes negative (stable), they are accepted, and if the opposite occurs, they are returned to their original state. This process is repeated to determine the amount of adsorption described above.

[0055] By selecting the pore structure (slit, cylinder, cage) and determining the parameters of the adsorbate and adsorbent, theoretical adsorption isotherms for various pore sizes can be derived using GCMC. By fitting an isotherm obtained by integrating this theoretical adsorption isotherm with the measured isotherm and calculating the pore distribution curve that minimizes the error in the amount of adsorption, it is possible to analyze the pore distribution in all regions from micropores to mesopores. 2 Intermolecular interactions and graphite / N 2As the intermolecular interaction parameters, for example, the parameters determined by Sweatman, M. B. et al., "J. Phys. Chem., 105, 1403 (2001)" can be used.

[0056] Specifically, a Microtrack Bell BELSORP MINIII was used, and N 2 The adsorption isotherm is measured and analyzed using the analytical kinetics analyzer BEL Master T under the following conditions: Measurement: Microtrack Bell automatic specific surface area / pore distribution analyzer BELSORP MINIII Measurement temperature: 77 K Adsorbate: N 2 Pretreatment conditions: 100°C, 3 hours Analysis: BELMaster™ V6.3.00 Distribution function: No-assumption Pore size definition: Solid and Fluid def. Pore Size Model: GCMC Pore structure: Slit Adsorbent: C

[0057] The integrated area of ​​pores with diameters of 1 nm or less determined using the GCMC method is 0.01 m from the viewpoint of suppressing decomposition by the electrolyte. 2 / g or less is preferable, and 0m 2 In addition, the integrated area of ​​pores with diameters of 1.5 nm or less determined using the GCMC method is preferably 0.01 m / g from the viewpoint of suppressing decomposition by the electrolyte. 2 / g or less is preferable, and 0m 2 / g is more preferred.

[0058] The Raman R value of the carbon material according to this embodiment is preferably 0.01 to 0.7, more preferably 0.02 to 0.65, and even more preferably 0.03 to 0.6. Here, from the viewpoint of preventing deterioration of charge / discharge characteristics due to the difficulty of crystals being oriented in a plane when densified, the Raman R value is preferably 0.01 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. Furthermore, from the viewpoint of suppressing an increase in irreversible capacity as a negative electrode active material, obtaining good initial efficiency and long-term storage recovery rate, and suppressing excessive reaction with the electrolyte, preventing a decrease in charge / discharge efficiency and an increase in gas generation, the Raman R value is preferably 0.7 or less, preferably 0.65 or less, and more preferably 0.6 or less. The Raman R value of the carbon material can be adjusted by the content of amorphous carbon material in the carbon raw material, which will be described later, the heating temperature during production of the carbon raw material, and the like.

[0059] The Raman R value in this specification is a value expressed by the following formula: Raman R value = (1360 cm in Raman spectrum analysis) -1 Nearby Peak P B Intensity I B ) / (1580 cm in Raman spectroscopy -1 Nearby Peak P A Intensity I A ) In the above formula, "1580 cm -1 "Nearby" is 1580 cm -1 ~1620cm -1 It also refers to the range of 1360 cm. -1 "Nearby" is 1350 cm -1 ~1370cm -1 Refers to the range of.

[0060] Here, 1580 cm -1 Nearby Peak P A is a peak called the G band derived from the graphite structure, and is at 1360 cm -1 Nearby Peak P B The Raman R value, which uses these peaks, can be used to evaluate the crystalline purity and defect ratio of carbon materials.

[0061] The Raman spectrum is obtained by measurement using a Raman spectrometer. Specifically, the carbon material is filled into a measurement cell by gravity, and measurement is performed while irradiating the measurement cell with argon ion laser light and rotating the measurement cell in a plane perpendicular to the laser light. The measurement conditions are as follows: Wavelength of argon ion laser light: 514.5 nm Laser power on sample: 25 mW Resolution: 4 cm -1 Measurement range: 1100 cm -1 ~1730cm -1 Peak intensity measurement, peak half-width measurement: background processing, smoothing processing (simple average convolution 5 points)

[0062] As the amount of surface functional groups in the carbon material according to this embodiment, the O / C value, which indicates the surface oxygen concentration, is preferably 0.01% to 4%, more preferably 0.1 to 4%, even more preferably 0.3 to 3.6%, and even more preferably 0.5 to 3%. From the viewpoint of strengthening the interaction between the carbon material surface and the organic compound and preventing the organic compound from peeling off, the surface functional group amount O / C value is preferably 0.01% or more, more preferably 0.1% or more, even more preferably 0.3% or more, and particularly preferably 0.5% or more. Furthermore, from the viewpoint of facilitating adjustment of the O / C value by oxidation treatment or the like, improving productivity, and reducing costs, the surface functional group amount O / C value is preferably 4% or less, more preferably 3.6% or less, and even more preferably 3% or less.

[0063] The volume-based average particle size d50 of the carbon material according to this embodiment is preferably 1 to 50 μm, more preferably 4 to 30 μm, and even more preferably 6 to 25 μm. From the viewpoint of preventing the specific surface area from becoming too large and suppressing activity in the electrolyte, the average particle size d50 is typically 1 μm or more, preferably 4 μm or more, and more preferably 6 μm or more. Furthermore, from the viewpoint of suppressing process problems such as striating during electrode formation, the average particle size d50 is typically 50 μm or less, preferably 30 μm or less, and more preferably 25 μm or less. The volume-based average particle size d50 of the carbon material is the volume-based median diameter measured using a laser diffraction / scattering particle size distribution analyzer, and can be adjusted, for example, by pulverization, crushing, classification, or the like.

[0064] The aspect ratio of the carbon material according to this embodiment is preferably 1 to 10, more preferably 1.1 to 8, even more preferably 1.1 to 5, and even more preferably 1.2 to 3. Theoretically, the aspect ratio is 1 or more, and from the viewpoints of preventing striations when formed into an electrode plate, obtaining a uniform coating surface, and obtaining good high-current density charge / discharge characteristics, the aspect ratio is preferably 1.1 or more, more preferably 1.2 or more. From the same viewpoint, the aspect ratio is preferably 10 or less, more preferably 8 or less, even more preferably 5 or less, and particularly preferably 3 or less.

[0065] The pore volume of the carbon material according to this embodiment in the range of 10 nm to 1000 nm is preferably 0.05 to 0.3 mL / g, more preferably 0.07 to 0.28 mL / g, and even more preferably 0.1 to 0.25 mL / g. From the viewpoint of lithium metal deposition during rapid charging and electrode plate strength, the pore volume is preferably 0.05 mL / g or more, more preferably 0.07 mL / g or more, and even more preferably 0.1 mL / g or more. From the same viewpoint, the pore volume is preferably 0.3 mL / g or less, more preferably 0.28 mL / g or less, and even more preferably 0.25 mL / g or less. The pore volume in the range of 10 nm to 1000 nm is a value measured using mercury porosimetry by mercury intrusion porosimetry.

[0066] The total pore volume of the carbon material according to this embodiment is preferably 0.1 to 10 mL / g, more preferably 0.2 to 5 mL / g, even more preferably 0.25 to 2 mL / g, and even more preferably 0.5 to 1 mL / g. From the viewpoint of the dispersion effect of the thickener and binder during electrode formation, the total pore volume is preferably 0.1 mL / g or more, more preferably 0.2 mL / g or more, even more preferably 0.25 mL / g or more, and even more preferably 0.5 mL / g or more. From the same viewpoint, the total pore volume is preferably 10 mL / g or less, more preferably 5 mL / g or less, even more preferably 2 mL / g or less, and even more preferably 1 mL / g or less. The total pore volume can be adjusted by heating the carbon material. The total pore volume in this specification is a value measured using a mercury porosimeter by mercury intrusion porosimetry.

[0067] The average pore diameter of the carbon material according to this embodiment is preferably 0.03 to 80 μm, more preferably 0.05 to 50 μm, even more preferably 0.1 to 50 μm, and even more preferably 0.5 to 20 μm. From the viewpoints of the amount of binder used in forming the electrode plate and the high current density charge / discharge characteristics of the battery, the average pore diameter is preferably 0.03 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and even more preferably 0.5 μm or more. From the same viewpoint, the average pore diameter is preferably 80 μm or less, more preferably 50 μm or less, and even more preferably 20 μm or less.

[0068] The tap density of the carbon material according to this embodiment is usually 0.1 to 1.3 g / cm 3 and 0.15 to 1.2 g / cm 3 is preferably 0.2 to 1.2 g / cm 3 More preferably, 0.3 to 1.1 g / cm 3 Here, from the viewpoint of obtaining good high-speed charge / discharge characteristics, the tap density is usually 0.1 g / cm 3 or more, and 0.15 g / cm 3 More than 0.2 g / cm 3 More preferably, 0.3 g / cm 3Furthermore, from the viewpoint of suppressing an increase in carbon density within the particles, suppressing a decrease in rollability, and obtaining a high-density negative electrode sheet, the tap density is usually 1.3 g / cm 3 or less, and 1.2 g / cm 3 Preferably, 1.1 g / cm or less 3 The tap density in this specification is measured using a powder density measuring instrument with a diameter of 1.6 cm and a volume capacity of 20 cm 3 The density is calculated from the volume and mass of the sample when a cylindrical tap cell is filled to the brim with the sample and then tapped 1,000 times with a stroke length of 10 mm.

[0069] <Carbonaceous Material> The carbonaceous material according to the present embodiment preferably has a modifying component bonded to the carbonaceous material raw material, and preferably contains the carbonaceous material raw material and at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium as a constituent element of the modifying component. Here, the constituent element of the modifying component more preferably contains silicon or aluminum, and when aluminum is contained, it is even more preferable that phosphorus is further contained. The carbonaceous material raw material in the present embodiment is not particularly limited, and carbonaceous material raw materials with various degrees of graphitization, from graphite to amorphous, can be used, and one type may be used alone, or two or more types may be mixed and used.

[0070] From the viewpoint of commercial availability, the carbonaceous raw material preferably contains at least one of graphite and a raw carbon material with a low degree of graphitization (amorphous carbon), and more preferably contains graphite. The graphite and amorphous carbon are also preferred from the viewpoint of charge-discharge characteristics at high current densities.

[0071] The content of graphite in the carbonaceous raw material of the present embodiment is preferably 90 to 100 mass%, more preferably 95 to 99 mass%, and the type and content of graphite in the carbonaceous raw material may be appropriately adjusted so that desired physical properties such as the d002 value of the carbonaceous material can be realized.

[0072] When the carbonaceous raw material in this embodiment contains graphite, the carbonaceous raw material preferably contains at least one of artificial graphite and natural graphite, and from the viewpoints of a large specific surface area and an effect of improving initial efficiency, it is more preferable to contain natural graphite, and from the viewpoint of cycle characteristics, it is more preferable to contain artificial graphite. Graphite with few impurities is preferred, and it may be used after being subjected to various purification treatments as necessary.

[0073] Examples of natural graphite include amorphous graphite, scaly graphite, and flake graphite. Among these, scaly graphite and scaly graphite are preferred, with scaly graphite being more preferred, from the viewpoint of a high degree of graphitization and a low content of impurities. Furthermore, spherical natural graphite may be used from the viewpoint of particle packing and charge / discharge load characteristics, which are achieved by forming suitable dense pores inside the carbon material.

[0074] Examples of artificial graphite include those obtained by heating organic materials such as coal tar pitch, coal-based heavy oil, atmospheric residual oil, petroleum-based heavy oil, aromatic hydrocarbons, nitrogen-containing cyclic compounds, sulfur-containing cyclic compounds, polyphenylene, polyvinyl chloride, polyvinyl alcohol, polyacrylonitrile, polyvinyl butyral, natural polymers, polyphenylene sulfide, polyphenylene oxide, furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin to 2500° C. or higher to graphitize them.

[0075] In this embodiment, it is preferable to use a carbonaceous raw material that satisfies the desired physical properties of the resulting carbonaceous material. For example, since the Raman R value of the carbonaceous raw material and the resulting carbonaceous material are the same, if a carbonaceous material with a Raman R value of 0.01 to 0.7 is desired, it is preferable to use a carbonaceous raw material with a Raman R value of 0.01 to 0.7. That is, the Raman R value of the carbonaceous raw material is preferably 0.01 to 0.7, more preferably 0.02 to 0.65, and even more preferably 0.03 to 0.6. Here, with regard to the resulting carbonaceous material, from the viewpoint of avoiding deterioration of charge / discharge characteristics due to the difficulty in orienting the crystals in a planar orientation when densified, the Raman R value is preferably 0.01 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. Furthermore, from the viewpoint of suppressing an increase in irreversible capacity as a negative electrode active material, obtaining good initial efficiency and long-term storage recovery rate, and from the viewpoint of suppressing excessive reaction with the electrolyte and preventing a decrease in charge / discharge efficiency and an increase in gas generation, the Raman R value of the obtained carbon material is preferably 0.7 or less, more preferably 0.65 or less, and more preferably 0.6 or less. The Raman R value of the carbon material raw material can be adjusted by the content of amorphous carbon material, the heating temperature during production of the carbon material raw material, etc.

[0076] <Modifying Component> The modifying component in this embodiment preferably contains at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium, and more preferably has a binding site capable of binding to a carbon material. In addition, in order to control the reactivity of the modifying component, a manufacturing method described below is usually used for the carbon material. The molecular weight of the modifying component is preferably 500 or less, and more preferably has a structure represented by the following formula (1): (Z) n -L-W (1) (In general formula (1), Z is a group capable of chemically bonding to a carbon material, W is a group containing at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium, L is a linker, and n is 1 or 2.) In addition, the total content of modifying components in the carbon material according to this embodiment is usually 1% by volume or less.

[0077] Moiety capable of chemically bonding to a carbon material Examples of the surface structure of a carbon material include a structure containing a carbon-carbon unsaturated bond and a carbon radical structure. Z in the general formula (1) is not particularly limited as long as it is a group that forms a bond with these, and known groups can be used. From the viewpoint of being able to form a bond with the carbon-carbon unsaturated bond-containing structure of the surface structure of the carbon material, Z in the general formula (1) preferably contains a structure that can be added by a Diels-Alder reaction, is more preferably a group having an unsaturated bond at its terminal, and is even more preferably a vinyl group.

[0078] Silicon atoms: Silicon atoms, which are constituent elements of the modifying component contained in the carbonaceous material according to the present embodiment, are introduced by reacting a silicon-containing compound with the carbonaceous raw material. By bonding silicon atoms to carbon atoms in the carbonaceous raw material, silicon atoms are present on the surface of the carbonaceous raw material and also at the edge portions of the graphene structure in the carbonaceous raw material. This allows solvated lithium ions attempting to intercalate from the edge portions of the graphene structure to be desolvated while suppressing side reactions.

[0079] The atomic concentration x of silicon atoms in the carbon material according to this embodiment (Si) (atomic %) is the x (Si) / y(atomic%・g / m 2 ) is 0.05 to 1 atom % g / m 2 It is preferable that the value is 0.07 to 0.8 atomic % g / m 2 It is more preferable that the atomic concentration x of silicon atoms is such that (Si) The content (atomic %) can be adjusted by adjusting the amount of silicon-containing compound added to the carbonaceous material.

[0080] Aluminum atoms: Aluminum atoms, which are constituent elements of the modifying component contained in the carbonaceous material according to the present embodiment, are introduced into the carbonaceous raw material by directly or indirectly reacting an aluminum-containing compound with the carbonaceous raw material. By bonding the aluminum atoms to the carbonaceous raw material carbon atoms, aluminum atoms are present on the surface of the carbonaceous raw material and also at the edge portions of the graphene structure in the carbonaceous raw material. This allows solvated lithium ions attempting to intercalate from the edge portions of the graphene structure to be desolvated while suppressing side reactions.

[0081] The atomic concentration x of aluminum atoms in the carbon material according to this embodiment (Al) (atomic %) is the x (Al) / y(atomic%・g / m 2 ) is 0.05 to 1 atom % g / m 2 If so, there is no particular limitation, but specifically, the atomic concentration x of aluminum atoms is preferably 0.1 to 15 atomic %. (Al) The content (atomic %) can be adjusted by adjusting the amount of aluminum-containing compound added to the carbonaceous material raw material.

[0082] Phosphorus Atom The phosphorus atom, which is a constituent element of the modifying component contained in the carbon material according to the present embodiment, is introduced by reacting a phosphorus-containing compound with the carbon raw material. When the phosphorus atom is bonded to a carbon atom of the carbon raw material, the phosphorus atom is also present on the surface of the carbon raw material and at the edge of the graphene structure in the carbon raw material. When aluminum and phosphorus are contained as constituent elements of the modifying component, aluminum selectively reacts with the phosphorus atom, thereby more suitably promoting desolvation of solvated lithium ions that attempt to intercalate from the edge of the graphene structure while suppressing side reactions.

[0083] When the modifying component contains aluminum and phosphorus as constituent elements, the atomic concentration of phosphorus atoms in the carbon material according to this embodiment is preferably adjusted to 0.1 to 1 when the atomic concentration of aluminum atoms in the carbon material is taken as 1, as described above, and specifically, although it differs depending on the atomic concentration of aluminum atoms, it is preferably 0.01 to 15 atomic %, for example. The atomic concentration of phosphorus atoms (atomic %) can be adjusted by increasing or decreasing the amount of phosphorus-containing compound added to the carbon raw material.

[0084] Boron, sulfur, germanium The boron atom as a constituent element of the modifier contained in the carbon material according to the present embodiment is introduced by reacting a boron-containing compound with the carbon raw material. The sulfur atom as a constituent element of the modifier contained in the carbon material according to the present embodiment is introduced by reacting a sulfur-containing compound with the carbon raw material. The germanium atom as a constituent element of the modifier contained in the carbon material according to the present embodiment is introduced by reacting a germanium-containing compound with the carbon raw material.

[0085] The molecular weight of the modifying component in this embodiment is preferably 500 or less, more preferably 100 to 500, and even more preferably 100 to 400. From the viewpoint of facilitating the modification, the molecular weight is preferably 500 or less, more preferably 400 or less, and even more preferably 300 or less.

[0086] In this embodiment, it is more preferable that the modifying component contains silicon or aluminum, and that the molecular weight of the modifying component is 500 or less. In this embodiment, it is more preferable that the modifying component contains silicon or aluminum, and that the total content of the modifying component in the carbon material is 1% by volume or less. Furthermore, it is even more preferable that the modifying component contains silicon or aluminum, that the total content of the modifying component in the carbon material is 1% by volume or less, and that the molecular weight of the modifying component is 500 or less.

[0087] Linker The linker represented by L in the above general formula (1) is a single bond or an (n+1)-valent hydrocarbon group having 1 to 6 carbon atoms. n is 1 or 2, and from the viewpoint of controlling reactivity, n is preferably 1. Examples of the hydrocarbon group include aliphatic hydrocarbon groups such as alkylene groups and alkenylene groups, and aromatic hydrocarbon groups such as phenylene groups. From the viewpoint of completing the reaction of the modifying component, a single bond or an (n+1)-valent aliphatic hydrocarbon group having 1 to 6 carbon atoms is preferred, a single bond or an (n+1)-valent alkylene group having 1 to 6 carbon atoms is more preferred, and a single bond or a divalent alkylene group having 1 to 6 carbon atoms is even more preferred.

[0088] <Other Components> The carbon material according to the present embodiment may contain other components in addition to the carbon raw material and the silicon, aluminum, phosphorus, boron, sulfur atoms, and germanium as constituent elements of the modifying components, as long as the effects of the present invention are not impaired. Examples of other components include metal particles, metal oxide particles, organic compounds, and composites thereof.

[0089] Examples of metals constituting the metal particles or metal oxide particles include metals that can be alloyed with lithium, such as Sn and Bi.

[0090] As the organic compound, a compound having multiple hydroxyl groups or groups capable of self-crosslinking by heat or light in the molecule is preferred from the viewpoint of forming a strong coating. Examples include polyol-based resins such as polyvinyl alcohol-based resins, acrylic polyol resins, polyester polyol resins, and polyether polyol resins, silicone resins, epoxy resins, and acrylic and polyester resins having hydrolyzable silyl groups. Among these, polyvinyl alcohol-based resins, acrylic polyol resins, polyester polyol resins, and acrylic and polyester resins having hydrolyzable silyl groups are more preferred, and polyvinyl alcohol-based resins, acrylic polyol resins, and polyester polyol resins are even more preferred. From the viewpoint of solvent resistance as a negative electrode active material layer, polyvinyl alcohol-based resins are particularly preferred.

[0091] The polyvinyl alcohol resin is not particularly limited in its specific structure as long as it is a resin having a vinyl alcohol structural unit, and is typically obtained by saponifying a polyvinyl carboxylate obtained by polymerizing a vinyl carboxylate monomer such as vinyl acetate, but is not limited thereto.

[0092] The total content of other components in the carbon material according to this embodiment is preferably 0.5 to 15% by mass, more preferably 1 to 10% by mass, and even more preferably 1.5 to 7% by mass. When other components are contained, from the viewpoint of obtaining the effects of the other components, the total content is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more. Furthermore, from the viewpoint of ensuring the capacity of the battery, the total content is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 7% by mass or less.

[0093] <<Method of Manufacturing Carbon Material>> The carbon material according to this embodiment is a carbon material having a total atomic concentration of the constituent elements of the modifying component of x (atomic %) and a specific surface area of ​​y (m 2 / g), x / y (atomic % g / m 2 ) is 0.05 to 1 atom % g / m 2 The method preferably further comprises a step of heating the mixture obtained in the mixing step.

[0094] For example, when silicon atoms are contained as constituent elements of the modifying component, the carbon material according to this embodiment has an atomic concentration of silicon atoms of x (Si) (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g) x (Si) / y(atomic%・g / m 2 ) is 0.05 to 1 atom % g / m 2 The method preferably further comprises a step of heating the mixture obtained in the mixing step.

[0095] Atomic concentration x of silicon atoms in the carbon material (Si)(atomic %) is preferably 0.1 to 15 atomic %, more preferably 0.2 to 10 atomic %, and even more preferably 0.3 to 5 atomic %. 2 / g) is 1 to 15 m 2 / g is preferred, and 1.2 to 10m 2 / g is more preferable, and 1.4 to 5m 2 / g is more preferred.

[0096] When aluminum atoms are contained as constituent elements of the modifying component, the carbon material according to this embodiment has an atomic concentration of aluminum atoms of x (Al) (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g) x (Al) / y(atomic%・g / m 2 ) is 0.05 to 1 atom % g / m 2 The method preferably further comprises a step of heating the mixture obtained in the mixing step.

[0097] In the mixing step, it is preferable to further mix a phosphorus-containing compound, and it is more preferable to mix the carbonaceous raw material and the phosphorus-containing compound and then further mix an aluminum-containing compound, and it is even more preferable to mix the carbonaceous raw material and the phosphorus-containing compound to obtain a phosphate group-containing carbonaceous raw material and then further mix the aluminum-containing compound.

[0098] Atomic concentration x of aluminum atoms in the carbon material (Al) (atomic %) is preferably 0.1 to 15 atomic %, more preferably 0.2 to 10 atomic %, and even more preferably 0.3 to 5 atomic %. 2 / g) is 1 to 15 m 2 / g is preferred, and 1.2 to 10m 2 / g is more preferable, and 1.4 to 5m 2 / g is more preferred.

[0099] When a phosphorus-containing compound is further mixed in the mixing step, the content ratio of phosphorus atoms in the resulting carbon material is preferably 0.1 to 1, more preferably 0.15 to 0.95, and even more preferably 0.2 to 0.9, in terms of atomic concentration ratio when the atomic concentration of aluminum atoms is taken as 1.

[0100] Next, each step will be described.

[0101] <Mixing Step> In the step of mixing the carbonaceous raw material with a compound to be a modifying component, i.e., a silicon-containing compound, an aluminum-containing compound, or the like, the carbonaceous raw material may be the same as that described in <Carbonaceous Raw Material> in the above <Carbonaceous Material>, and the preferred embodiments are also the same.

[0102] For example, the carbonaceous raw material preferably contains at least one selected from the group consisting of artificial graphite and natural graphite, and the Raman R value of the carbonaceous raw material is preferably 0.01 to 0.7, more preferably 0.02 to 0.65, and even more preferably 0.03 to 0.6.

[0103] The carbonaceous raw material may be the above-mentioned carbonaceous raw material that has been further subjected to a spheronization treatment. The spheronization treatment is a treatment in which particles are repeatedly subjected to mechanical actions such as compression, friction, shear force, and particle interactions, mainly by impact force, to form spheroids. A spheronization device, for example, has a rotor with many blades installed inside a casing, and the rotor rotates at high speed to apply mechanical actions such as impact, compression, friction, shear force, and the like to the carbonaceous raw material introduced inside, thereby performing surface treatment.

[0104] Before mixing the carbonaceous raw material with the compound serving as the modifying component, the carbonaceous raw material may be subjected to an isotropic pressure treatment. By isotropically pressing the carbonaceous raw material, the internal voids of the carbonaceous raw material are compressed. As a result, the density of the carbonaceous raw material crushed after the pressure treatment increases, and the high-speed charging characteristics can be improved. In addition, by isotropically pressing the carbonaceous raw material, flattening of the particles is unlikely to occur, allowing the particles to maintain their spherical shape, and preventing a decrease in fluidity when slurried.

[0105] The pressing means may be a roll compactor, a roll press, a briquette machine, a cold isostatic press (CIP), a uniaxial molding machine, a tablet machine, etc. Among these pressing means, a cold isostatic press is preferred from the viewpoint of reducing internal pores while maintaining the particle shape.

[0106] Here, when the compound serving as the modifying component is a silicon-containing compound, the silicon-containing compound is not particularly limited as long as it bonds a silicon atom to the surface of the carbonaceous raw material, and examples thereof include silane coupling agents such as alkoxysilanes, silane compounds having an amino group, an epoxy group, an isocyanate group, a vinyl group, an acetyl group, etc. Among these, silane compounds having a vinyl group or an acetyl group are preferred from the viewpoint of being able to suppress unsaturated bonds with high electron density and radical reactivity.

[0107] As the alkoxysilane, from the viewpoints of easy removal of the substituent after the reaction and suppressing the battery resistance, those having two or less carbon-silicon bonds are more preferable. Specific examples include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, phenyltrimethoxysilane, vinyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, phenyltriethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, acetyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, methylethyldimethoxysilane, methylphenyldimethoxysilane, and methylvinyldimethoxysilane.

[0108] The silane compound having an amino group is not particularly limited as long as it has an amino group, but in order to suppress battery resistance, it is more preferable that the number of carbon-silicon bonds is 2 or less.Specific examples include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, phenylaminopropyltrimethoxysilane, 3-aminoethylaminopropyltrimethoxysilane, and 3-aminoethylaminopropylmethyldimethoxysilane.

[0109] The silane compound having an epoxy group is not particularly limited as long as it has an epoxy group, but in order to suppress battery resistance, it is preferable that the number of carbon-silicon bonds is 2 or less.Specific examples include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0110] The silane compound having an isocyanate group is not particularly limited as long as it has an isocyanate group, but in order to suppress battery resistance, it is preferable that the number of carbon-silicon bonds is 2 or less.Specific examples include tetraisocyanatosilane, triisocyanato(methyl)silane, and 3-isocyanatopropyltriethoxysilane.

[0111] The vinyl or acetyl group-containing silane compound is not particularly limited as long as it contains a vinyl or acetyl group, but in order to suppress battery resistance, it is more preferable for the number of carbon-silicon bonds to be two or less. Specific examples include dimethoxymethylvinylsilane, diethoxymethylvinylsilane, dichloromethylvinylsilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropyloxysilane, aryltrimethoxysilane, aryltriethoxysilane, trichlorovinylsilane, vinyltris(2-methoxyethoxy)silane, acetyltrimethoxysilane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, 5-(triethoxysilyl)-2-norbornene, and octavinyloctasilasesquioxane.

[0112] The mixing ratio of the carbonaceous material raw material and the silicon-containing compound is determined by setting the atomic concentration of silicon atoms in the resulting carbonaceous material at x (Si) (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g) x (Si) / y(atomic%・g / m 2 ) is 0.05 to 1 atom % g / m 2 Here, the specific surface area y (m 2 / g) and the specific surface area (m 2 / g), the mixing ratio may be determined by regarding them as the same value.

[0113] When the compound serving as the modifying component is an aluminum-containing compound, the aluminum-containing compound is not particularly limited as long as it bonds an aluminum atom to the surface of the carbonaceous raw material, and examples thereof include aluminum compounds that react with acid, more specifically, alkoxyaluminum, aluminum halide, aluminum hydroxide, aluminum nitrate, aluminum carbonate, etc. Among these, alkoxyaluminum and aluminum hydroxide are preferred from the viewpoint of the influence of impurities on battery performance.

[0114] The alkoxyaluminum is preferably one whose substituent can be easily removed after the reaction, and specific examples include (ethylacetoacetato)aluminum diisopropoxide, trimethoxyaluminum, triethoxyaluminum, tri(isopropoxy)aluminum, and butoxyaluminum.

[0115] The aluminum halide is preferably one whose substituent can be easily removed after the reaction, and specific examples include aluminum fluoride, aluminum chloride, aluminum bromide, and aluminum iodide.

[0116] The mixing ratio of the carbonaceous material raw material and the aluminum-containing compound is determined by the atomic concentration of aluminum atoms in the resulting carbonaceous material. (Al) (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g) x (Al) / y(atomic%・g / m 2 ) is 0.05 to 1 atom % g / m 2 Here, the specific surface area y (m 2 / g) and the specific surface area (m 2 / g), the mixing ratio may be determined by regarding them as the same value.

[0117] A solvent may be used when mixing the compound serving as the modifying component with the carbonaceous raw material, regardless of whether it is liquid or solid. In particular, when the compound serving as the modifying component is solid, it is preferable to use a solvent from the viewpoint of uniformity during mixing. The solvent is not particularly limited, but examples thereof include water, ethyl methyl ketone, toluene, acetone, methyl isobutyl ketone, ethanol, methanol, tetrahydrofuran, ethylene glycol dimethyl ether, etc. Among these, ethanol, methanol, and acetone are preferred from the viewpoint of ease of removal.

[0118] When mixing the carbonaceous raw material and the compound serving as the modifying component, additives and other components may be further added. Examples of additives include surfactants that contribute to imparting wettability and adhesiveness to the negative electrode active material and binder resin, inorganic oxide particles that contribute to reducing the resistance of the coating, lithium compound particles, conductive polymers such as polyaniline sulfonic acid, and compounds that form complex ions with lithium ions, such as polyethylene oxide and complex hydrides.

[0119] Examples of other components include those described in the section "Other Components" in the "Carbon Material" above.

[0120] In the mixing step in this embodiment, when the compound to be the modifying component is an aluminum-containing compound, as described above, it is preferable to further mix a phosphorus-containing compound with the carbonaceous raw material, more preferably to mix the carbonaceous raw material and the phosphorus-containing compound and then further mix the aluminum-containing compound, and still more preferably to mix the carbonaceous raw material and the phosphorus-containing compound to obtain a phosphate group-containing carbonaceous raw material, and then further mix the aluminum-containing compound.

[0121] The phosphorus-containing compound is not particularly limited as long as it bonds a phosphate group to the surface of the carbonaceous raw material, and examples thereof include vinylphosphonic acid compounds, ethynylphosphonic acid compounds, etc. Among these, aminophosphine compounds, vinylphosphonic acid compounds, and ethynylphosphinic acid compounds are preferred from the viewpoint of being able to form a strong bond with the edge portion of the graphene structure of the carbonaceous material.

[0122] The phosphonic acid is not particularly limited as long as it can form a bond with the edge portion of the graphene structure of the carbon material, but those having an unsaturated carbon bond in part of the phosphonic acid are more preferred in terms of being able to react with the unsaturated bond of the edge.Specific examples include vinylphosphonic acid, dimethyl vinylphosphonate, diethyl vinylphosphonate, dipropyl vinylphosphonate, dibutyl vinylphosphonate, dimethyl allylphosphonate, diethyl allylphosphonate, dipropyl allylphosphonate, dibutyl allylphosphonate, cinamylphosphonic acid, ethynylphosphonic acid, dimethyl ethynylphosphonate, diethyl ethynylphosphonate, dipropyl ethynylphosphonate, dibutyl ethynylphosphonate, propargylphosphonic acid, dimethyl propargylphosphonate, diethyl propargylphosphonate, dipropyl propargylphosphonate, and dibutyl propargylphosphonate.

[0123] The amide phosphoric acid compound is not particularly limited as long as it can form a bond with the edge portion of the graphene structure of the carbon material, but amide phosphoric acid esters are more preferred because they can react efficiently with the acid functional groups at the edge portion of the graphene structure of the carbon material.Specific examples include dimethyl phosphoric acid ester, diethyl phosphoric acid ester, dipropyl phosphoric acid ester, and dibutyl phosphoric acid ester.

[0124] The mixing ratio of the carbonaceous material raw material and the phosphorus-containing compound is preferably adjusted so that the atomic concentration of phosphorus atoms in the resulting carbonaceous material is 0.1 to 1 relative to the atomic concentration of aluminum atoms in the carbonaceous material.

[0125] A solvent may be used when mixing the phosphorus-containing compound with the carbonaceous raw material, regardless of whether the compound is liquid or solid. In particular, when the phosphorus-containing compound is solid, it is preferable to use a solvent from the viewpoint of uniformity during mixing. The solvent is not particularly limited, but examples thereof include water, ethyl methyl ketone, toluene, acetone, methyl isobutyl ketone, ethanol, methanol, tetrahydrofuran, ethylene glycol dimethyl ether, etc. Among these, ethanol, methanol, and acetone are preferred from the viewpoint of ease of removal.

[0126] When a phosphorus-containing compound is mixed with a carbonaceous raw material to obtain a phosphate group-containing carbonaceous raw material first, it is preferable to heat the mixture after mixing the phosphorus-containing compound. The heating temperature is not particularly limited, but is preferably 60 to 200° C., and more preferably 100 to 180° C. The heating time is also not particularly limited, but is preferably 15 minutes to 10 hours, and more preferably 30 minutes to 2 hours.

[0127] The atmosphere during heating is preferably an inert atmosphere from the viewpoint of suppressing oxidation reactions, and examples thereof include a nitrogen atmosphere, an argon atmosphere, and a helium atmosphere.

[0128] After the heating, the phosphate group-containing carbonaceous raw material may be cooled, washed and dried as necessary, and then mixed with the aluminum-containing compound. Washing can remove residues of excess phosphorus-containing compounds that are not bonded to the carbonaceous raw material, and can suppress a decrease in reaction with the aluminum-containing compound, a decrease in battery capacity, an increase in battery resistance, etc. A conventionally known solution can be used for washing, and for example, the same solvent as that used in mixing can be used.

[0129] The method for mixing the carbonaceous material raw material and the compound serving as the modifying component is not particularly limited, and a conventionally known method can be employed. For example, a method of stirring using a stirring blade in a fixed container, a method of mixing by rotating the container itself and rolling the contents, a method of fluidizing and mixing by air current, etc. are mentioned. Among them, from the viewpoint of mixing uniformity, a method of stirring using a stirring blade in a fixed container is preferred.

[0130] When mixing the carbonaceous raw material and the aluminum-containing compound, among methods of stirring using a stirring blade in a fixed container, it is more preferable to stir a dispersion obtained by dispersing the carbonaceous raw material in a solvent and dropwise add a solution containing the aluminum-containing compound thereto.

[0131] The mixing time is not particularly limited as long as the carbonaceous material raw material and the compound serving as the modifying component are mixed uniformly, but is preferably 10 to 90 minutes, more preferably 30 to 60 minutes. Here, the mixing time is preferably 10 minutes or more, more preferably 30 minutes or more, and is preferably 90 minutes or less, more preferably 60 minutes or less.

[0132] The mixing temperature is not particularly limited, but is preferably 10 to 80° C., more preferably 15 to 60° C. Here, the mixing temperature is preferably 10° C. or higher, more preferably 15° C. or higher, and is preferably 80° C. or lower, more preferably 60° C. or lower.

[0133] <Heating Step> In the heating step, the mixture obtained in the mixing step is heated. When the compound to be the modifying component is a silicon-containing compound, the reactive substituent of the silicon-containing compound reacts with the active functional group at the edge of the carbonaceous raw material by heating, thereby bonding the silicon atoms contained in the silicon-containing compound to the surface of the carbonaceous raw material. In addition, when a solvent is used in the mixing step, the solvent can also be removed by heating. Furthermore, the heating step may be performed after solid-liquid separation by filtration or the like before the heating step.

[0134] When the compound to be used as the modifying component is an aluminum-containing compound, if the aluminum-containing compound or phosphorus-containing compound is liquid, heating volatilizes or decomposes the aluminum-containing compound or phosphorus-containing compound, and phosphate groups based on the aluminum atoms or phosphorus atoms contained in the aluminum-containing compound or phosphorus-containing compound react with active functional groups at the edge of the carbonaceous raw material, thereby bonding the aluminum atoms or phosphorus atoms to the surface of the carbonaceous raw material. Furthermore, if a solvent is used in the mixing step, the solvent can also be removed by heating. Furthermore, the heating step may be performed after solid-liquid separation by filtration or the like before the heating step.

[0135] The heating temperature is not particularly limited, but is preferably, for example, 60 to 300°C, more preferably 100 to 250°C, and even more preferably 100 to 180°C. Heating at 120°C or higher is also preferred. Here, the heating temperature is preferably 60°C or higher, more preferably 100°C or higher, and even more preferably 120°C or higher. It is also preferably 300°C or lower, more preferably 250°C or lower, and may be 200°C or lower or 180°C or lower. When the compound to be the modifying component is a silicon-containing compound, the heating temperature is, for example, preferably 60 to 200°C, more preferably 100 to 180°C. Heating at 120°C or higher is also preferred. When the compound to be the modifying component is an aluminum-containing compound, the heating temperature is, for example, preferably 60 to 300°C, more preferably 100 to 250°C. Heating at 120°C or higher is also preferred. In addition, mixing while heating may also serve as the main heating step.

[0136] The heating time is not particularly limited, but is preferably 15 minutes to 10 hours, and more preferably 30 minutes to 2 hours. Here, the heating time is preferably 15 minutes or more, more preferably 30 minutes or more, and is preferably 10 hours or less, and more preferably 2 hours or less.

[0137] The heating temperature in the mixing step is preferably 60 to 300° C., and the heating time is preferably 15 minutes to 10 hours.

[0138] The atmosphere during heating is not particularly limited, and may be air or an inert atmosphere, such as a nitrogen atmosphere, an argon atmosphere, or a helium atmosphere.

[0139] In particular, when the compound serving as the modifying component is a silicon-containing compound, the atmosphere during heating is preferably an inert atmosphere from the viewpoint of suppressing oxidation reactions.

[0140] After the heating step, the carbonaceous material may be cooled, washed again, and dried. Washing can remove residues of compounds that become excess modifying components that are not bonded to the carbonaceous material raw material, and can suppress a decrease in battery capacity and an increase in battery resistance. A conventionally known solution can be used for washing, and for example, the same solvent as that used in the mixing step can be used.

[0141] The heating temperature during drying is usually a temperature equal to or higher than the boiling point of the solvent and equal to or lower than the spontaneous ignition point, for example, preferably 20 to 150° C., more preferably 40 to 100° C. Here, the heating temperature is preferably 20° C. or higher, more preferably 40° C. or higher, and is preferably 150° C. or lower, more preferably 100° C. or lower. By performing sufficient drying, it is possible to suppress deterioration of battery performance due to remaining solvent or residue.

[0142] Drying may be carried out under reduced pressure. In this case, the pressure, expressed as gauge pressure (difference from atmospheric pressure), is usually −0.1 MPa or more, preferably −0.08 MPa or more, and is usually 0 MPa or less, preferably −0.03 MPa or less.

[0143] The obtained carbon material may be subjected to powder processing such as pulverization, crushing, classification, etc., as needed. There are no particular limitations on the equipment used for pulverization or crushing, and examples of coarse crushers include shear mills, jaw crushers, impact crushers, and cone crushers. Examples of intermediate crushers include roll crushers and hammer mills. Examples of fine crushers include ball mills, vibration mills, pin mills, stirring mills, and jet mills.

[0144] The apparatus used for classification is not particularly limited, and in the case of dry sieving, examples include a rotary sieve, a shaking sieve, a gyrating sieve, a vibrating sieve, etc. In the case of dry air classification, examples include a gravity classifier, an inertia classifier, a centrifugal classifier (classifier, cyclone, etc.), etc. In addition, wet sieving, a mechanical wet classifier, a hydraulic classifier, a sedimentation classifier, a centrifugal wet classifier, etc. can also be used.

[0145] <<Composition>> To achieve the second object, the composition according to the present embodiment preferably contains a compound (A) having a polyoxyalkylene structure and a crosslinkable siloxane compound (B) having Q units. It is more preferable that the compound (A) has at least two crosslinkable silicon units per molecule.

[0146] The composition according to the present embodiment contains a compound (A) containing a polyoxyalkylene structure that contributes to flexibility and a crosslinkable siloxane compound (B) containing Q units that contribute to strength, and therefore the cured product obtained from the composition has excellent adhesion and durability. In particular, the three-dimensional siloxane structure containing Q units in the cured product obtained from the composition controls the penetration of water and organic solvents into the cured product, thereby suppressing the elution of components from the cured product and swelling of the cured product. Furthermore, the crosslinkable siloxane compound (B) containing Q units can be cured at low temperatures, so that a cured product can be obtained at temperatures lower than the thermal decomposition temperature of the compound (A) containing the polyoxyalkylene structure, thereby suppressing the elution of components from the cured product due to thermal decomposition. Furthermore, since the polyoxyalkylene structure contributes to lithium ion conductivity, the use of the composition according to the present embodiment allows for the production of a secondary battery with excellent durability without compromising charge / discharge efficiency.

[0147] <Compound (A)> The composition according to the present embodiment includes a compound (A) (hereinafter, sometimes referred to as "compound (A)") having a polyoxyalkylene structure. By including the compound (A), the composition according to the present embodiment provides a cured product obtained from the composition with excellent adhesion, flexibility, and lithium ion conductivity.

[0148] Examples of the compound (A) include polyethylene glycol, polypropylene glycol, polybutylene glycol, polypentylene glycol, polyhexylene glycol, and copolymers thereof. These compounds (A) may be used alone or in combination of two or more. Among these compounds (A), polyethylene glycol and polypropylene glycol are preferred, and polyethylene glycol is more preferred, because they have excellent solubility in various solvents. The compound (A) may be a diol type or a triol type.

[0149] The compound (A) may contain various functional groups other than hydroxyl groups, as long as the effects of the present invention are not impaired. The compound (A) preferably contains a crosslinkable silicon unit, as this increases compatibility and reactivity with the crosslinkable siloxane compound (B) and improves the durability of the cured product obtained from the composition. Specifically, the compound (A) is preferably a compound having at least one crosslinkable silicon unit per molecule, and more preferably a compound having two crosslinkable silicon units per molecule.

[0150] The crosslinkable silicon units are preferably D units or T units, since compound (A) can react with crosslinkable siloxane compound (B) containing Q units and decomposition of the cured product due to leaching can be suppressed. T units are more preferred, since they have many crosslinking points and can suppress swelling as well as leaching.

[0151] In this specification, a silicon unit bonded to one oxygen atom and three organic groups is referred to as an M unit, a silicon unit bonded to two oxygen atoms and two organic groups is referred to as a D unit, a silicon unit bonded to three oxygen atoms and one organic group is referred to as a T unit, and a silicon unit bonded to four oxygen atoms is referred to as a Q unit.

[0152] When the crosslinkable siloxane compound (B) containing Q units contains a reactive organic group derived from a silane coupling agent, the compound (A) may have a reactive organic group that reacts with the reactive organic group of the crosslinkable siloxane compound (B) containing Q units. Examples of the reactive organic group include a vinyl group, an amino group, an epoxy group, a methacryl group, a carboxyl group, an isocyanate group, and a hydrosilyl group.

[0153] The weight-average molecular weight Mw of the compound (A) is preferably 500 to 50,000, and more preferably 1,000 to 2,000. Here, in order to achieve excellent non-volatility and not excessively high solubility in water or organic solvents, the weight-average molecular weight is preferably 500 or more, and more preferably 1,000 or more. Furthermore, in order to achieve resistance to precipitation and crystallization in the composition, and to achieve excellent composition stability and compatibility with the crosslinkable siloxane compound (B) containing Q units, the weight-average molecular weight is preferably 50,000 or less, and more preferably 20,000 or less.

[0154] In this specification, the weight average molecular weight Mw is a value measured by gel filtration chromatography.

[0155] <Compound (B)> The composition according to this embodiment contains a crosslinkable siloxane compound (B) (hereinafter, sometimes referred to as "compound (B)") containing a Q unit. By including compound (B), the composition according to this embodiment can reduce the elution rate and swelling rate in water or organic solvents of a cured product obtained from the composition, and has excellent durability.

[0156] Examples of raw materials for compound (B) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, partially hydrolyzed oligomers of the above-mentioned tetraalkoxysilanes, and modified oligomers having two or more types of alkoxy groups. These raw materials for compound (B) may be used alone or in combination of two or more. Among these raw materials for compound (B), the partially hydrolyzed oligomers of tetraalkoxysilanes are preferred because of their excellent curability, and the partially hydrolyzed oligomers of tetramethoxysilane are more preferred.

[0157] The partially hydrolyzed oligomer of tetraalkoxysilane is preferably a dimer to a dihyadora, more preferably a dimer to a hundred, and even more preferably a dimer to a decamer, because these oligomers have excellent compatibility with compound (A) and provide excellent storage stability to the composition.

[0158] The compound (B) can be obtained by hydrolyzing the above-mentioned raw material of the compound (B).

[0159] The raw material for compound (B) may be used in combination with a silane coupling agent or an alkoxysilane having a non-reactive organic group in order to enhance compatibility with compound (A).

[0160] <Compound (C)> The composition according to the present embodiment may further contain a boron-containing compound (C) (hereinafter, may be referred to as "compound (C)") in addition to the compound (A) and the compound (B). By further containing the compound (C), the composition according to the present embodiment can reduce resistance and is excellent at suppressing side reactions in a battery of a carbonaceous material containing a cured product obtained from the composition (sometimes referred to as a "cured product-containing carbonaceous material").

[0161] Compound (C) alone has high solubility in water and organic solvents, but when used in combination with compound (A) and compound (B), the hydroxyl group bonded to boron reacts with the hydroxyl group or silanol group of compound (A) and the silanol group of compound (B), thereby suppressing leaching from the cured product.

[0162] Examples of the compound (C) include boric acid, boron oxide, metaboric acid, tetraboric acid, borates, alkoxides having 1 to 3 carbon atoms bonded to boron, lithium borates, and organic boronic acids. These compounds (C) may be used alone or in combination of two or more. Among these compounds (C), boric acid, boron oxide, and organic boronic acids are preferred due to their excellent stability, and boric acid and phenylboronic acid are more preferred. As the organic boronic acid, aromatic boronic acids are more preferred.

[0163] <Solvent> The composition according to the present embodiment may further contain a solvent in addition to the compound (A) and the compound (B). Furthermore, the composition according to the present embodiment may further contain the compound (C) and a solvent in addition to the compound (A) and the compound (B). By including a solvent, the composition according to the present embodiment has excellent handleability as a coating material.

[0164] Examples of the solvent include water, methanol, ethanol, propanol, isopropanol, butanol, acetonitrile, acetone, and tetrahydrofuran. These solvents may be used alone or in combination of two or more. Among these solvents, water, methanol, ethanol, and isopropanol are preferred, and methanol and ethanol are more preferred, because they provide excellent productivity when obtaining a cured product from the composition, high solubility of the compound (A) containing a polyoxyalkylene structure, and excellent storage stability of the composition.

[0165] The composition according to this embodiment may further contain other components in addition to the compound (A), the compound (B), the compound (C) and the solvent, as long as the effects of the present invention are not impaired.

[0166] <Composition of the Composition> The content of compound (A) in the composition according to this embodiment is preferably 10 to 90% by mass, more preferably 20 to 80% by mass. Here, since the flexibility and lithium ion conductivity of the cured product obtained from the composition are excellent, the content is preferably 10% by mass or more, more preferably 20% by mass or more. Furthermore, since the durability of the cured product obtained from the composition is excellent, the content is preferably 90% by mass or less, more preferably 80% by mass or less. The content of compound (A) in the composition is the content in a total of 100% by mass of compound (A), compound (B), compound (C), and other components.

[0167] The content of compound (B) in the composition according to this embodiment is preferably 10 to 90% by mass, more preferably 20 to 80% by mass. Here, since the cured product obtained from the composition has excellent durability, the content is preferably 10% by mass or more, more preferably 20% by mass or more. Furthermore, since the cured product obtained from the composition has excellent flexibility, the content is preferably 90% by mass or less, more preferably 80% by mass or less. The content of compound (B) in the composition is the content in a total of 100% by mass of compound (A), compound (B), compound (C), and other components.

[0168] The mass ratio of compound (B) to compound (A) (mass of compound (B) / mass of compound (A)) is preferably 0.2 to 5, and more preferably 0.3 to 3. Here, in order to provide a cured product obtained from the composition with excellent durability, the mass ratio is preferably 0.2 or more, and more preferably 0.3 or more. Furthermore, in order to provide a cured product obtained from the composition with excellent flexibility, the mass ratio is preferably 5 or less, and more preferably 3 or less.

[0169] When compound (C) is used, the content of compound (C) in the composition according to this embodiment is preferably 0.1 to 30% by mass, more preferably 0.3 to 20% by mass. Here, since the cured product obtained from the composition is excellent in suppressing side reactions in the battery, the content is preferably 0.1% by mass or more, more preferably 0.3% by mass or more. Furthermore, since the cured product obtained from the composition is excellent in durability, the content is preferably 30% by mass or less, more preferably 20% by mass or less. Furthermore, the content of compound (C) is preferably less than the content of at least one of compound (A) and compound (B), and more preferably less than the content of both compound (A) and compound (B). The content of compound (C) in the composition is the content in a total of 100% by mass of compound (A), compound (B), compound (C), and other components.

[0170] The total content of other components in the composition according to the present embodiment is preferably 20% by mass or less, more preferably 10% by mass or less, and may be 0% by mass, i.e., may not be contained. The total content of other components in the composition is the content in 100% by mass, which is the total of Compound (A), Compound (B), Compound (C), and other components.

[0171] When a solvent is used, the content of the solvent per 100 parts by mass of the composition according to this embodiment is preferably 5 to 99.9 parts by mass, and more preferably 10 to 99.5 parts by mass. Here, since a uniform cured product can be obtained from the composition, the content is preferably 5 parts by mass or more, and more preferably 10 parts by mass or more. Furthermore, since this provides excellent productivity when obtaining a cured product from the composition, the content is preferably 99.9 parts by mass or less, and more preferably 99.5 parts by mass or less. The solvent content is the content per 100 parts by mass of the total of compound (A), compound (B), compound (C), and other components.

[0172] The content of the polyoxyalkylene structure in the composition according to this embodiment is preferably 10 to 60% by mass, more preferably 15 to 50% by mass. Here, since the flexibility and lithium ion conductivity of the cured product obtained from the composition are excellent, the content is preferably 10% by mass or more, more preferably 15% by mass or more. Furthermore, since the durability of the cured product obtained from the composition is excellent, the content is preferably 60% by mass or less, more preferably 50% by mass or less. The polyoxyalkylene structure refers to the polyoxyalkylene structure constituting the compound (A) containing the polyoxyalkylene structure. The content of the polyoxyalkylene structure in the composition is the content in a total of 100% by mass of the compounds (A), (B), (C), and other components.

[0173] The total content of Q units in the composition according to this embodiment is preferably 10% by mass or more, more preferably 15% by mass or more, because the cured product obtained from the composition has excellent durability. The total content of Q units in the composition according to this embodiment is preferably 50% by mass or less, more preferably 40% by mass or less, because the cured product obtained from the composition has excellent flexibility and does not inhibit lithium ion conductivity. The Q units are Q units constituting the crosslinkable siloxane compound (B) containing Q units. The total content of Q units in the composition is the content in a total of 100% by mass of compound (A), compound (B), and compound (C).

[0174] <Thermosetting Composition> The composition according to the present embodiment is not particularly limited as long as it can be cured. However, a thermosetting composition is preferred because it has excellent productivity for a cured product obtained from the composition and can suppress elution and swelling.

[0175] The heating temperature during curing of the thermosetting composition is preferably 80 to 200°C, more preferably 100 to 180°C. Here, the heating temperature is preferably 80°C or higher, more preferably 100°C or higher, in order to achieve excellent productivity of the cured product obtained from the composition. Furthermore, the heating temperature is preferably 200°C or lower, more preferably 180°C or lower, in order to prevent deterioration of the cured product obtained from the composition.

[0176] <<Cured Product>> The cured product according to this embodiment preferably contains a polyoxyalkylene structure and a three-dimensional siloxane structure containing Q units, and more preferably has a swelling ratio in ethyl methyl carbonate of 70% by mass or less. The cured product according to this embodiment has excellent flexibility and durability because it contains a flexible polyoxyalkylene structure and a three-dimensional siloxane structure containing high-strength Q units. In particular, the three-dimensional siloxane structure containing Q units in the cured product can control the penetration of water or organic solvents into the cured product, thereby suppressing the elution of components from the cured product and the swelling of the cured product.

[0177] Specifically, the cured product according to this embodiment is obtained by curing the composition described above in "Composition," and the preferred embodiments are the same. That is, the method for producing the cured product according to this embodiment includes a step of curing the composition described above in "Composition," and the curing step is preferably a heating step.

[0178] The method for curing the composition to obtain a cured product is not particularly limited, but curing by heating is preferred because it provides excellent productivity.

[0179] The heating temperature is preferably 80 to 200°C, more preferably 100 to 180°C. Here, in order to achieve excellent productivity, the heating temperature is preferably 80°C or higher, more preferably 100°C or higher. In order to prevent deterioration during the production process, the heating temperature is preferably 200°C or lower, more preferably 180°C or lower. The heating atmosphere is preferably an inert gas atmosphere, in order to suppress decomposition of the polyoxyalkylene structure.

[0180] The content of solids derived from compound (A) in the cured product according to this embodiment is preferably 10 to 90% by mass, more preferably 20 to 80% by mass. Here, since the flexibility of the cured product is excellent, the content is preferably 10% by mass or more, more preferably 20% by mass or more. Furthermore, since the durability of the cured product is excellent, the content is preferably 90% by mass or less, more preferably 80% by mass or less. The content of solids derived from compound (A) in the cured product is the content in 100% by mass of the cured product.

[0181] The content of solids derived from compound (B) in the cured product is preferably 10 to 90% by mass, more preferably 20 to 80% by mass. Here, in order to provide excellent durability to the cured product, the content is preferably 10% by mass or more, more preferably 20% by mass or more. In addition, in order to provide excellent flexibility to the cured product, the content is preferably 90% by mass or less, more preferably 80% by mass or less. The content of solids derived from compound (B) in the cured product is the content in 100% by mass of the cured product.

[0182] The mass ratio of the solid content derived from compound (B) in the cured product to the solid content derived from compound (A) in the cured product (mass of compound (B) / mass of compound (A)) is preferably 0.2 to 5, more preferably 0.3 to 3. Here, in order to provide excellent durability to the cured product, the mass ratio is preferably 0.2 or more, more preferably 0.3 or more. Furthermore, in order to provide excellent flexibility to the cured product, the mass ratio is preferably 5 or less, more preferably 3 or less.

[0183] When compound (C) is used, the content of solids derived from compound (C) in the cured product according to this embodiment is preferably 0.1 to 30% by mass, more preferably 0.3 to 20% by mass. Here, the content is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, because this effectively suppresses side reactions in the battery of the carbon material containing the cured product. Furthermore, the content is preferably 30% by mass or less, more preferably 20% by mass or less, because this effectively suppresses side reactions in the battery of the carbon material containing the cured product. The content of solids derived from compound (C) in the cured product is the content in 100% by mass of the cured product.

[0184] The total content of solids derived from other components in the cured product according to this embodiment is preferably 20% by mass or less, more preferably 10% by mass or less, and may be 0% by mass, i.e., not contained. The total content of solids derived from other components in the cured product is the content in 100% by mass of the cured product.

[0185] The content of the polyoxyalkylene structure in the cured product according to this embodiment is preferably 20 to 80% by mass, more preferably 30 to 70% by mass. Here, since the flexibility and lithium ion conductivity of the cured product are excellent, the content is preferably 20% by mass or more, more preferably 30% by mass or more. Furthermore, since the durability of the cured product is excellent, the content is preferably 80% by mass or less, more preferably 70% by mass or less. The content of the polyoxyalkylene structure in the cured product is the content in 100% by mass of the cured product.

[0186] The content of silicon atoms in the cured product according to this embodiment is preferably 10 to 40% by mass, more preferably 15 to 30% by mass. Here, the content is preferably 10% by mass or more, more preferably 15% by mass or more, since the cured product has excellent durability. Furthermore, the content is preferably 40% by mass or less, more preferably 30% by mass or less, since the cured product has excellent flexibility and does not inhibit lithium ion conductivity. The content of silicon atoms in the cured product is the content in 100% by mass of the cured product.

[0187] The total content of Q units in the cured product according to this embodiment is preferably 20 to 60% by mass, more preferably 30 to 50% by mass. Here, since the durability of the cured product is excellent, the total content is preferably 20% by mass or more, more preferably 30% by mass or more. Furthermore, since the flexibility of the cured product is excellent, the total content is preferably 60% by mass or less, more preferably 50% by mass or less. The total content of Q units in the cured product is the content in 100% by mass of the cured product.

[0188] The swelling ratio of the cured product according to this embodiment to ethyl methyl carbonate is preferably less than 70% by mass, more preferably 60% by mass or less, and even more preferably 50% by mass or less. The lower the swelling ratio, the better, but it is, for example, 1% by mass or more. The swelling ratio refers to the swelling ratio measured after immersing the cured product in ethyl methyl carbonate at 23°C for one hour. The swelling ratio can be calculated as the relative value of the mass change after one hour of immersion relative to the mass before immersion.

[0189] The cured product according to this embodiment is preferably hydrolyzable, and more preferably generates a polyoxyalkylene structure and a fragment having at least two silicon atoms per molecule after hydrolysis. From the viewpoint of controlling the three-dimensional structure of the polymer, the ratio of the polyoxyalkylene structure and the fragment having at least two silicon atoms per molecule to 100 mol% of the fragment having an Si atom is preferably 10 mol% or more, more preferably 30 mol% or more, even more preferably 50 mol% or more, even more preferably 50 to 100 mol%, and even more preferably 50 to 70 mol%. The above ratio refers to the ratio when the cured product is hydrolyzed under conditions that allow hydrolysis of the Si—O bond but not the polyoxyalkylene structure. The above ratio can be measured by NMR.

[0190] The cured product-containing carbon material according to this embodiment includes a cured product and a carbon material. The cured product may be any of those described above in the "Cured Product" section, and preferred embodiments are also similar. The carbon material will be described later.

[0191] The cured carbonaceous material according to this embodiment has a low elution rate and swelling rate in water or organic solvents, and therefore protects the carbonaceous material, thereby suppressing side reactions in a battery. Therefore, the cured carbonaceous material according to this embodiment can be suitably used as a negative electrode active material.

[0192] In particular, the cured carbonaceous material of the present invention contains a polyoxyalkylene structure with lithium ion conductivity, and is characterized by low resistance of the cured product. A three-dimensional siloxane structure without Q units cannot suppress swelling of the cured product, and over the long term, components containing the polyoxyalkylene structure leach out of the cured product, resulting in a sparse structure of the cured product, making it unable to maintain its protective performance for the carbonaceous material. On the other hand, the cured carbonaceous material according to this embodiment contains a three-dimensional siloxane structure containing Q units, which controls the compatibility and uniformity of the cured product, suppresses swelling and leach-out, and maintains the structure of the cured product, thereby suppressing side reactions in the battery over a long period of time.

[0193] The carbon material-containing cured product according to this embodiment can be obtained by curing the composition described above in the "Composition" section in the presence of a carbon material.

[0194] The method for curing the composition is not particularly limited, but heating is preferred because it has excellent productivity. That is, one aspect of the method for producing a cured carbonaceous material according to this embodiment includes a step of heating the composition described in the above "Composition" in the presence of a carbonaceous material. The obtained cured carbonaceous material is preferably used as a negative electrode active material.

[0195] The heating temperature in the heating step is preferably 80 to 200° C., more preferably 100 to 180° C. Here, in order to achieve excellent productivity, the heating temperature is preferably 80° C. or higher, more preferably 100° C. or higher. Furthermore, in order to prevent deterioration of the cured product, the heating temperature is preferably 200° C. or lower, more preferably 180° C. or lower.

[0196] The heating atmosphere in the heating step is preferably an inert gas atmosphere, as this inhibits decomposition of the polyoxyalkylene structure.

[0197] <Carbonaceous Material> The carbonaceous material constituting the cured product-containing carbonaceous material according to this embodiment is not particularly limited. For example, the carbonaceous material described above in the <<Carbonaceous Material>> can be used, and the same applies to preferred embodiments. That is, in one embodiment of the carbonaceous material according to this embodiment, a modifying component is bonded to a carbonaceous material raw material, and the modifying component preferably contains at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur, and germanium.

[0198] The d002 value of the carbon material in this embodiment is preferably 3.360 Å or less, more preferably 3.357 Å or less, because the more highly crystalline the graphite is, the better the compressibility during pressing and the more sufficient the charge / discharge capacity.

[0199] The Lc of the carbon material in this embodiment is preferably 900 Å or more, more preferably 1000 Å or more, because the more highly crystalline the graphite is, the better the compressibility during pressing and the more sufficient the charge / discharge capacity.

[0200] In this specification, the d002 value is the value of the interplanar spacing of the lattice plane (002 plane) measured by X-ray diffraction according to the Gakushin method, and Lc is the value of the crystallite size measured by X-ray diffraction according to the Gakushin method. The X-ray diffraction measurement conditions are as follows: Sample: A mixture of the measurement object and X-ray standard high-purity silicon powder, with approximately 15 mass% of the total amount added. X-ray: CuKα ray. Measurement range: 20°≦2θ≦30°. Step angle: 0.013°. Sample preparation: A powder sample was filled into a recess in a sample plate with a depth of 0.2 mm to prepare a flat sample surface.

[0201] The volume-based average particle size (d50) of the carbon material in this embodiment is preferably 1 to 50 μm, more preferably 10 to 30 μm. Here, in order to prevent an increase in irreversible capacity and a loss of initial battery capacity, the volume-based average particle size (d50) is preferably 1 μm or more, more preferably 4 μm or more, and even more preferably 10 μm or more. Furthermore, in order to suppress process defects such as streaking during electrode plate production and to achieve excellent rapid charge / discharge characteristics and low-temperature input / output characteristics, the volume-based average particle size (d50) is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 25 μm or less.

[0202] In this specification, the volume-based average particle size (d50) refers to the volume-based median diameter measured using a laser diffraction / scattering particle size distribution analyzer. Specifically, 0.01 g of a sample is suspended in 10 mL of a 0.2 mass % aqueous solution of a surfactant, polyoxyethylene sorbitan monolaurate, and the suspension is introduced into a laser diffraction / scattering particle size distribution analyzer. After irradiating the suspension with 28 kHz ultrasonic waves at an output of 60 W for 1 minute, the volume-based median diameter is measured using the analyzer.

[0203] The specific surface area (SA) of the carbon material in this embodiment is 3.0 to 11.0 m 2 / g is preferred, and 4.0 to 9.0 m 2 / g is more preferable, and 5.0 to 8.0 m 2 Here, the specific surface area is preferably 3.0 m / g because it ensures a portion through which lithium ions can enter and exit, and provides excellent rapid charge / discharge characteristics and low-temperature input / output characteristics. 2 / g or more is preferable, and 4.0m 2 / g or more is more preferable, and 5.0m 2 Further, the specific surface area is preferably 11.0 m / g or more because side reactions with the electrolyte are suppressed, a decrease in the initial charge / discharge efficiency and an increase in the amount of gas generated are prevented, and the battery capacity is improved. 2 / g or less is preferable, and 9.0m 2 / g or less is more preferable, and 8.0m 2 / g or less is more preferable.

[0204] In this specification, the specific surface area (SA) is a value measured by the BET method. Specifically, using a specific surface area measuring device, a sample is pre-dried under reduced pressure at 350°C for 15 minutes in a nitrogen stream, cooled to the temperature of liquid nitrogen, and measured by the nitrogen adsorption BET single-point method using a gas flow method with a nitrogen-helium mixed gas accurately adjusted so that the relative pressure of nitrogen to atmospheric pressure is 0.3.

[0205] The tap density of the carbon material in this embodiment is 0.70 to 1.30 g / cm 3 is preferably 0.80 to 1.20 g / cm 3 More preferably, 0.90 to 1.10 g / cm 3Here, the tap density is more preferably 0.70 g / cm because process defects such as creases can be suppressed during electrode plate production, the packing property is improved, and therefore a high-density negative electrode sheet with good rollability can be easily formed, the degree of curvature of the lithium ion migration path is reduced when the electrode body is formed, and the shape of the voids between the particles is regular, which allows smooth migration of the electrolyte and improves rapid charge / discharge characteristics. 3 More than 0.80 g / cm 3 More preferably, 0.90 g / cm 3 Furthermore, since the particles have an appropriate amount of space on the surface and inside thereof, the particles do not become too hard and have excellent electrode pressability, rapid charge / discharge characteristics, and low-temperature input / output characteristics, the tap density is preferably 1.30 g / cm. 3 Preferably, 1.20 g / cm or less 3 More preferably, 1.10 g / cm or less 3 The following is even more preferred:

[0206] In the present invention, the tap density is measured using a powder density measuring instrument with a diameter of 1.6 cm and a volume capacity of 20 cm 3 The sample is dropped into a cylindrical tap cell through a sieve with 300 μm openings until the cell is filled to capacity, and then tapped 1000 times with a stroke length of 10 mm, and the density value is calculated from the volume and mass of the sample at that time.

[0207] The circularity of the carbon material in this embodiment is preferably 0.88 to 0.99, more preferably 0.90 to 0.98, and even more preferably 0.92 to 0.97. Here, the degree of tortuosity of lithium ion diffusion is reduced, the movement of the electrolyte into the voids between the particles is smooth, and rapid charge / discharge characteristics are excellent. Therefore, the circularity is preferably 0.88 or more, more preferably 0.90 or more, and even more preferably 0.92 or more. Furthermore, the circularity is preferably 0.99 or less, more preferably 0.98 or less, and even more preferably 0.97 or less, because contact between the carbon materials can be ensured and cycle characteristics are excellent.

[0208] In this specification, the circularity is calculated by the following formula (I) after measuring the particle size distribution of equivalent circle diameters by flow particle image analysis. Specifically, a dispersion is obtained by ultrasonically dispersing particles using ion-exchanged water as a dispersion medium and polyoxyethylene sorbitan monolaurate as a surfactant. Then, the shape of the particles is photographed using a flow image analyzer. From images of at least 1,000 particles, the circularities of particles with equivalent circle diameters in the range of 1.5 μm to 40 μm are averaged to obtain the circularity. [Circularity] = [Peripheral length of an equivalent circle having the same area as the projected shape of a particle] / [Actual periphery of the projected shape of a particle] (I)

[0209] The cumulative pore volume of the carbon material in this embodiment is preferably 0.030 to 0.120 mL / g, more preferably 0.040 to 0.090 mL / g, and even more preferably 0.050 to 0.070 mL / g. Here, since the carbon material is easily deformed to a certain degree during pressing, the cumulative pore volume is preferably 0.030 mL / g or more, more preferably 0.040 mL / g or more, and even more preferably 0.050 mL / g or more, and is preferably 0.120 mL / g or less, more preferably 0.090 mL / g or less, and even more preferably 0.070 mL / g or less.

[0210] In this specification, the cumulative pore volume is measured by mercury intrusion porosimetry. Specifically, a mercury porosimeter is used to measure a sample weighed to a value of approximately 0.2 g, which is then sealed in a powder cell and degassed at 25 °C and 50 μmHg or less for 10 minutes for pretreatment. Next, the pressure is reduced to 4 psia, mercury is introduced into the cell, and the pressure is increased stepwise from 4 psia to 40,000 psia, and then decreased to 25 psia. The number of steps during pressure increase is 80 or more, and after a 10-second equilibration period at each step, the amount of mercury intrusion is measured. The pore distribution is calculated from the mercury intrusion curve obtained in this way using the Washburn equation. The calculation is based on the surface tension (γ) of mercury being 485 dyne / cm and the contact angle (ψ) being 140°. From the obtained results, a graph is prepared with the pore diameter on the horizontal axis and the pore volume on the vertical axis, and the cumulative pore volume (mL / g) is calculated.

[0211] <Method for producing carbon material> In the present embodiment, a commercially available carbon material may be used as is, or a commercially available carbon material raw material may be processed and used, but it is preferable to use spheroidized flake natural graphite because it has high crystallinity and excellent compressibility. When using one of the carbon materials described in the above <<Carbon material>>, the carbon material can be obtained by the method described in the above <<Method for producing carbon material>>

[0212] The raw material of the carbon material in this embodiment is preferably graphite, more preferably natural graphite or artificial graphite because of its high crystallinity and excellent capacity, and even more preferably natural graphite because of its higher crystallinity, higher capacity, and no need for heat treatment during production. Graphite with a low impurity content is preferred, and it is preferable to use it after purification treatment as necessary.

[0213] Examples of natural graphite include amorphous graphite, scaly graphite, flake graphite, etc. Among these natural graphites, scaly graphite and flake graphite are preferred, with flake graphite being more preferred, due to their high degree of graphitization and low impurity content.

[0214] Examples of artificial graphite include those obtained by heating organic substances such as coal tar pitch, coal-based heavy oil, atmospheric residual oil, petroleum-based heavy oil, aromatic hydrocarbons, nitrogen-containing cyclic compounds, sulfur-containing cyclic compounds, polyphenylene, polyvinyl chloride, polyvinyl alcohol, polyacrylonitrile, polyvinyl butyral, natural polymers, polyphenylene sulfide, polyphenylene oxide, furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin to 2500° C. or higher to graphitize them.

[0215] The spheronization method is preferably a method of spheronization by applying mechanical energy, since it is easy to control the particle shape. Examples of mechanical energy include impact, compression, friction, shear force, etc. These mechanical energies may be used alone or in combination of two or more. The method of spheronization by applying mechanical energy may use a device that applies mechanical energy.

[0216] <Physical Properties of the Cured Carbonaceous Material> The carbonaceous material content in the cured carbonaceous material according to this embodiment is preferably 95 to 99.9% by mass, more preferably 98 to 99.7% by mass. Here, in order to provide excellent capacity as a negative electrode material, the content is preferably 95% by mass or more, more preferably 98% by mass or more, based on 100% by mass of the cured carbonaceous material. Furthermore, in order to provide excellent suppression of volume change within a battery, the content is preferably 99.9% by mass or less, more preferably 99.7% by mass or less.

[0217] The content of the cured material in the cured-material-containing carbonaceous material according to this embodiment is preferably 0.3 to 5 mass%, more preferably 0.5 to 3 mass%. Here, the content is preferably 0.3 mass% or more, more preferably 0.5 mass% or more, based on 100 mass% of the cured-material-containing carbonaceous material, because this is effective in suppressing side reactions in the battery. Furthermore, the content is preferably 5 mass% or less, more preferably 3 mass% or less, because this is effective in suppressing battery resistance.

[0218] The content of the polyoxyalkylene structure in the cured carbonaceous material according to this embodiment is preferably 0.05 to 3 mass%, more preferably 0.1 to 1.5 mass%. Here, the content is preferably 0.05 mass% or more, more preferably 0.1 mass% or more, because this provides excellent adhesion between the cured product and the carbonaceous material and excellent lithium ion conductivity. Furthermore, the content is preferably 3 mass% or less, more preferably 1.5 mass% or less, because this provides excellent suppression of side reactions within the battery. The content of the polyoxyalkylene structure in the cured carbonaceous material is the content in 100 mass% of the cured carbonaceous material.

[0219] The silicon element content in the cured product-containing carbon material according to this embodiment is preferably 0.03 to 2 mass%, more preferably 0.05 to 1 mass%. Here, since the durability of the cured product is excellent, the content is preferably 0.03 mass% or more, more preferably 0.05 mass% or more. Furthermore, since the adhesion between the cured product and the carbon material is excellent, the content is preferably 2 mass% or less, more preferably 1 mass% or less. The silicon element content in the cured product-containing carbon material is the content in 100 mass% of the cured product-containing carbon material.

[0220] The total content of Q units in the cured product-containing carbon material according to this embodiment is preferably 0.05 to 2.5% by mass, and more preferably 0.1 to 2% by mass. Here, in order to achieve excellent adhesion between the cured product and the carbon material, the total content is preferably 0.05% by mass or more, and more preferably 0.1% by mass or more. Furthermore, in order to suppress peeling due to shrinkage of the cured product during the production process, the total content is preferably 2.5% by mass or less, and more preferably 2% by mass or less. The total content of Q units in the cured product-containing carbon material is the content in 100% by mass of the cured product-containing carbon material.

[0221] The d002 value of the cured carbonaceous material according to this embodiment is preferably 3.360 Å or less, and more preferably 3.357 Å or less, because the more highly crystalline the graphite, the better the compressibility during pressing and the more sufficient the charge / discharge capacity.

[0222] The Lc of the cured carbonaceous material according to this embodiment is preferably 900 Å or more, more preferably 1000 Å or more, because the more highly crystalline the graphite, the better the compressibility during pressing and the more sufficient the charge / discharge capacity.

[0223] The volume-based average particle size (d50) of the cured product-containing carbon material according to this embodiment is preferably 1 to 50 μm, more preferably 4 to 30 μm, and even more preferably 10 to 25 μm. Here, in order to prevent an increase in irreversible capacity and a loss of initial battery capacity, the volume-based average particle size (d50) is preferably 1 μm or more, more preferably 4 μm or more, and even more preferably 10 μm or more. Furthermore, in order to suppress process defects such as streaking during electrode plate production and to achieve excellent rapid charge / discharge characteristics and low-temperature input / output characteristics, the volume-based average particle size (d50) is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 25 μm or less.

[0224] The specific surface area (SA) of the cured carbonaceous material according to this embodiment is 3.0 to 11.0 m 2 / g is preferred, and 4.0 to 9.0 m 2 / g is more preferable, and 5.0 to 8.0 m 2 Here, the specific surface area is preferably 3.0 m / g because it ensures a portion through which lithium ions can enter and exit, and provides excellent rapid charge / discharge characteristics and low-temperature input / output characteristics. 2 / g or more is preferable, and 4.0m 2 / g or more is more preferable, and 5.0m 2 Further, the specific surface area is preferably 11.0 m / g or more because side reactions with the electrolyte are suppressed, a decrease in the initial charge / discharge efficiency and an increase in the amount of gas generated are prevented, and the battery capacity is improved. 2 / g or less is preferable, and 9.0m 2 / g or less is more preferable, and 8.0m 2 / g or less is more preferable.

[0225] The tap density of the cured carbonaceous material according to this embodiment is 0.70 to 1.30 g / cm 3 is preferably 0.80 to 1.20 g / cm 3 More preferably, 0.90 to 1.10 g / cm 3 Here, the tap density is more preferably 0.70 g / cm because process defects such as creases can be suppressed during electrode plate production, the packing property is improved, and therefore a high-density negative electrode sheet with good rollability can be easily formed, the degree of curvature of the lithium ion migration path is reduced when the electrode body is formed, and the shape of the voids between the particles is regular, which allows smooth migration of the electrolyte and improves rapid charge / discharge characteristics. 3 More than 0.80 g / cm 3 More preferably, 0.90 g / cm 3 Furthermore, since the particles have an appropriate amount of space on the surface and inside thereof, the particles do not become too hard and have excellent electrode pressability, rapid charge / discharge characteristics, and low-temperature input / output characteristics, the tap density is preferably 1.30 g / cm. 3 Preferably, 1.20 g / cm or less 3 More preferably, 1.10 g / cm or less 3 The following is even more preferred:

[0226] The circularity of the cured product-containing carbon material according to this embodiment is preferably 0.88 to 0.99, more preferably 0.90 to 0.98, and even more preferably 0.92 to 0.97. Here, the degree of tortuosity of lithium ion diffusion is reduced, the movement of the electrolyte into the voids between the particles is smooth, and rapid charge / discharge characteristics are excellent. Therefore, the circularity is preferably 0.88 or more, more preferably 0.90 or more, and even more preferably 0.92 or more. Furthermore, the circularity is preferably 0.99 or less, more preferably 0.98 or less, and even more preferably 0.97 or less, because this ensures contact between the carbon materials and results in excellent cycle characteristics.

[0227] The cumulative pore volume of the cured carbonaceous material according to this embodiment is preferably 0.030 to 0.120 mL / g, more preferably 0.040 to 0.090 mL / g, and even more preferably 0.050 to 0.070 mL / g. In order to facilitate moderate deformation during pressing, the cumulative pore volume is preferably 0.030 mL / g or more, more preferably 0.040 mL / g or more, and even more preferably 0.050 mL / g or more, and is preferably 0.120 mL / g or less, more preferably 0.090 mL / g or less, and even more preferably 0.070 mL / g or less.

[0228] The negative electrode according to this embodiment includes a current collector and a negative electrode active material layer formed on the current collector. The negative electrode active material layer includes at least one of the carbon materials described in the above section "Carbon material" and the carbon material described in the above section "Carbon material containing cured product."

[0229] The content of the carbon material in the negative electrode active material layer is preferably 80 to 99.8% by mass, more preferably 90 to 99.8% by mass, and even more preferably 99 to 99.7% by mass. From the viewpoint of suppressing a decrease in battery capacity, the content is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 99% by mass or more, and is preferably 99.8% by mass or less, and more preferably 99.7% by mass or less.

[0230] The negative electrode active material layer may contain, in addition to the carbon material according to this embodiment, a conductive additive, a binder, a thickener, a dispersant, and the like.

[0231] Conventionally known conductive additives can be used, but examples thereof include carbon materials other than the carbon material according to this embodiment. Examples of other carbon materials include graphite and particles of graphite coated with amorphous carbon and / or graphitic material with a low degree of graphitization. The other carbon materials may further contain oxides or other metals. Examples of other metals include metals that can be alloyed with Li, such as Sn, Si, Al, and Bi. In addition to the above, examples of conductive additives include silicone and carbon black. One type of conductive additive may be used alone, or two or more types may be used in combination.

[0232] Any conventionally known binder can be used, and examples of the binder include styrene butadiene rubber (SBR) as an aqueous binder.

[0233] As the thickener or dispersant, a conventionally known thickener or dispersant can be used, for example, carboxymethyl cellulose (CMC).

[0234] The negative electrode can be manufactured by forming a negative electrode active material layer on a current collector using the carbon material according to this embodiment. That is, one aspect of the method for manufacturing a negative electrode according to this embodiment includes a step of forming a negative electrode active material layer using the carbon material described in the above section "Carbon Material" to obtain a negative electrode. Here, preferred aspects of the carbon material are the same as the preferred aspects of the carbon material described in the above section "Carbon Material." Furthermore, one aspect of the method for manufacturing a negative electrode according to this embodiment includes a step of forming a negative electrode active material layer using the cured-material-containing carbon material described in the above section "Cured-Material-Containing Carbon Material" to obtain a negative electrode. Here, preferred aspects of the cured-material-containing carbon material are the same as the preferred aspects of the cured-material-containing carbon material described in the above section "Cured-Material-Containing Carbon Material."

[0235] For example, the carbon material is dispersed in a dispersion medium together with a conductive aid, a binder, a thickener, etc., as desired, to form a slurry, and the resulting slurry is applied onto a current collector to form a negative electrode active material layer.

[0236] Among these, a method of applying a slurry containing the carbon material or the cured carbon material and a binder onto a current collector and drying the slurry is preferred because it is inexpensive and has excellent productivity. The slurry may further contain a thickener.

[0237] It is preferable that a slurry containing the carbon material or the cured product-containing carbon material and a binder is applied to a current collector, dried, and then pressed to increase the density of the active material layer formed on the current collector, thereby increasing the battery capacity per unit volume of the active material layer.

[0238] The density of the active material layer is 1.2 to 2.0 g / cm 3 is preferred, and 1.5 to 1.8 g / cm 3 Here, the density is more preferably 1.2 g / cm because it can suppress a decrease in battery capacity due to an increase in electrode thickness. 3 More preferably, 1.5 g / cm 3 Furthermore, the reduction in voids in the electrode reduces the amount of electrolyte solution held in the voids, reducing the mobility of alkaline ions such as lithium ions, and suppressing the deterioration of rapid charge / discharge characteristics. Therefore, the density is preferably 2.0 g / cm. 3 Preferably, 1.8 g / cm or less 3 The following is more preferred:

[0239] Any conventionally known dispersion medium can be used, and examples thereof include organic solvents such as alcohols and water.

[0240] Any known current collector can be used, including, for example, a thin metal film such as rolled copper foil, electrolytic copper foil, or stainless steel foil.

[0241] <Secondary Battery> The carbon material according to this embodiment can be used in a secondary battery. The basic configuration of a secondary battery, particularly a lithium ion secondary battery, is similar to that of a conventionally known lithium ion secondary battery, and typically preferably includes a positive electrode capable of absorbing and releasing lithium ions, a negative electrode, and an electrolyte. The carbon material according to this embodiment is used in the negative electrode active material layer constituting the negative electrode, and a preferred embodiment thereof is similar to the preferred embodiment described above in <<Negative Electrode>>.

[0242] The positive electrode is formed by forming a positive electrode active material layer containing a positive electrode active material and a binder on a current collector, and any conventionally known positive electrode can be used.

[0243] The electrolyte may be a known one. For example, a non-aqueous electrolyte solution in which a lithium salt is dissolved in a non-aqueous solvent, or a non-aqueous electrolyte solution in the form of a gel, rubber, or solid sheet using an organic polymer compound, etc., may be used. A solid electrolyte may also be used.

[0244] When a non-aqueous electrolyte solution is used as the electrolyte, a porous separator such as a porous membrane or nonwoven fabric may be interposed between the positive electrode and the negative electrode to prevent short-circuiting between the electrodes. A conventionally known separator can be used. In this case, the non-aqueous electrolyte solution is impregnated into the porous separator.

[0245] The method for producing the secondary battery includes a step of forming an anode active material layer on a current collector using the carbon material according to this embodiment to obtain the anode. That is, one aspect of the method for producing the secondary battery according to this embodiment includes a step of forming an anode active material layer on a current collector using the carbon material described in the above section "Carbon Material" to obtain the anode, and the secondary battery includes a positive electrode, a negative electrode, and an electrolyte. Here, preferred aspects of the carbon material are the same as the preferred aspects of the carbon material described in the above section "Carbon Material." Also, one aspect of the method for producing the secondary battery according to this embodiment includes a step of forming an anode active material layer on a current collector using the cured-material-containing carbon material described in the above section "Cured-Material-Containing Carbon Material" to obtain the anode, and the secondary battery includes a positive electrode, a negative electrode, and an electrolyte. Here, preferred aspects of the cured-material-containing carbon material are the same as the preferred aspects of the cured-material-containing carbon material described in the above section "Cured-Material-Containing Carbon Material."

[0246] The negative electrode of a secondary battery using the carbonaceous material according to the present embodiment described in the above section "Carbonaceous Material" can operate stably as a negative electrode, and exhibits good initial efficiency while maintaining a high initial discharge capacity. Therefore, the carbonaceous material according to the present embodiment can be suitably used as a negative electrode active material for secondary batteries, more suitably used as a negative electrode active material for non-aqueous secondary batteries, and particularly suitably used as a negative electrode active material for non-aqueous lithium-ion secondary batteries.

[0247] Furthermore, the cured product according to the present embodiment described above in "Cured Product" can sufficiently reduce the elution rate and swelling rate in water or organic solvents. Therefore, the cured product-containing carbon material described above in "Cured Product-Containing Carbon Material" that includes the cured product is excellent at suppressing side reactions in batteries and can be more suitably used as an active material for the negative electrode of a non-aqueous secondary battery, and can be particularly suitably used as an active material for the negative electrode of a lithium-ion secondary battery.

[0248] The carbon material, composition, cured product, cured product-containing carbon material, anode, secondary battery, and methods for manufacturing them, as well as a method for modifying a carbon material according to the present embodiment have been described above, but one aspect of the present invention also relates to the following. Aspect 1 [1-1] A carbon material comprising a carbon material raw material and silicon atoms as a constituent element, wherein the atomic concentration of the silicon atoms in the carbon material is x (atomic %) and the specific surface area of ​​the carbon material is y (m 2 / g), x / y (atomic % g / m 2 ) is 0.3 to 1 atomic % g / m 2 [1-2] The integrated area of ​​pores with a diameter of 1 nm or less, as determined by pore distribution analysis using the Grand Canonical Monte Carlo (GCMC) method of molecular simulation, is 0.01 m 2 / g or less. [1-3] The carbon material according to [1-1] or [1-2] above, wherein the carbon raw material contains at least one selected from the group consisting of artificial graphite and natural graphite. [1-4] The carbon material according to any one of [1-1] to [1-3] above, wherein x, the atomic concentration of silicon atoms, is 0.1 to 15 atomic %. [1-5] The carbon material according to any one of [1-1] to [1-3] above, wherein y, the specific surface area, is 1 to 15 m 2 [1-6] The carbon material according to any one of the above [1-1] to [1-5], having a Raman R value represented by the following formula of 0.01 to 0.7: Raman R value = (1360 cm in Raman spectroscopy) -1 Nearby Peak P B Intensity I B ) / (1580 cm in Raman spectroscopy -1 Nearby Peak P A Intensity IA [1-7] The carbon material according to any one of [1-1] to [1-6] above, which is used in a secondary battery.

[0249] [1-8] The atomic concentration of silicon atoms in the carbon material is x (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g), x / y (atomic % g / m 2 ) is 0.3 to 1 atomic % g / m 2 [1-9] A method for producing a carbon material according to [1-8] above, wherein the carbon material contains at least one selected from the group consisting of artificial graphite and natural graphite. [1-10] A method for producing a carbon material according to [1-8] or [1-9] above, wherein the carbon material has a Raman R value, represented by the following formula, of 0.01 to 0.7. Raman R value=(1360 cm in Raman spectroscopy) -1 Nearby Peak P B Intensity I B ) / (1580 cm in Raman spectroscopy -1 Nearby Peak P A Intensity I A [1-11] The method for producing a carbon material according to any one of the above [1-8] to [1-10], which comprises a step of heating the mixture obtained after the mixing. [1-12] The method for producing a carbon material according to any one of the above [1-8] to [1-11], wherein x, the atomic concentration of silicon atoms, is 0.1 to 15 atomic %. [1-13] The specific surface area y is 1 to 15 m 2 / g, the method for producing a carbon material according to any one of [1-8] to [1-12].

[0250] [1-14] A method for producing a negative electrode, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [1-1] to [1-7] above to obtain a negative electrode. [1-15] A method for producing a secondary battery including a positive electrode, a negative electrode, and an electrolyte, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [1-1] to [1-7] above to obtain the negative electrode.

[0251] <<Aspect 2>> [2-1] A carbon material comprising a carbonaceous material raw material and aluminum atoms as a constituent element, wherein the atomic concentration of the aluminum atoms in the carbonaceous material is x (atomic %), and the specific surface area of ​​the carbonaceous material is y (m 2 / g), x / y (atomic % g / m 2 ) is 0.05 to 1 atom % g / m 2 [2-2] The carbon material according to [2-1] above, further comprising phosphorus atoms as a constituent element, wherein the atomic concentration of the phosphorus atoms in the carbon material is 0.1 to 1 when the atomic concentration of the aluminum atoms in the carbon material is 1. [2-3] The carbon material according to [2-1] above, wherein the integrated area of ​​pores with a diameter of 1 nm or less, determined by pore distribution analysis using the Grand Canonical Monte Carlo (GCMC) method, which is a molecular simulation method, is 0.01 m 2 / g or less. [2-4] The carbon material according to any one of [2-1] to [2-3] above, wherein the carbon raw material contains at least one selected from the group consisting of artificial graphite and natural graphite. [2-5] The carbon material according to any one of [2-1] to [2-4] above, wherein x, the atomic concentration of aluminum atoms, is 0.1 to 15 atomic %. [2-6] The carbon material according to any one of [2-1] to [2-4] above, wherein y, the specific surface area, is 1 to 15 m 2 [2-7] The carbon material according to any one of the above [2-1] to [2-6], having a Raman R value represented by the following formula of 0.01 to 0.7: Raman R value = (1360 cm in Raman spectroscopy) -1 Nearby Peak P B Intensity I B ) / (1580 cm in Raman spectroscopy -1 Nearby Peak P A Intensity I A [2-8] The carbon material according to any one of [2-1] to [2-7] above, which is used in a secondary battery.

[0252] [2-9] The atomic concentration of aluminum atoms in the carbon material is x (atomic %), and the specific surface area of ​​the carbon material is y (m 2 / g), x / y (atomic % g / m 2) is 0.05 to 1 atom % g / m 2 [2-10] The method for producing a carbon material according to [2-9] above, further comprising mixing a phosphorus-containing compound in the mixing step, so that the atomic concentration of phosphorus atoms in the carbon material is 0.1 to 1 when the atomic concentration of the aluminum atoms in the carbon material is 1. [2-11] The method for producing a carbon material according to [2-9] or [2-10] above, wherein the carbon material raw material contains at least one selected from the group consisting of artificial graphite and natural graphite. [2-12] The method for producing a carbon material according to any one of [2-9] to [2-11] above, wherein the carbon material raw material has a Raman R value, represented by the following formula, of 0.01 to 0.7: Raman R value=(1360 cm in Raman spectroscopy) -1 Nearby Peak P B Intensity I B ) / (1580 cm in Raman spectroscopy -1 Nearby Peak P A Intensity I A [2-13] The method for producing a carbon material according to any one of the above [2-9] to [2-12], which comprises a step of heating the mixture obtained after the mixing. [2-14] The method for producing a carbon material according to any one of the above [2-9] to [2-13], wherein x, the atomic concentration of aluminum atoms, is 0.1 to 15 atomic %. [2-15] The specific surface area y is 1 to 15 m 2 / g, the method for producing a carbon material according to any one of [2-9] to [2-14].

[0253] [2-16] A method for producing a negative electrode, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [2-1] to [2-8] above to obtain a negative electrode. [2-17] A method for producing a secondary battery including a positive electrode, a negative electrode, and an electrolyte, comprising the step of forming a negative electrode active material layer on a current collector using the carbon material according to any one of [2-1] to [2-8] above to obtain the negative electrode.

[0254] <Aspect 3> [3-1] A composition comprising a compound (A) having a polyoxyalkylene structure and a crosslinkable siloxane compound (B) having Q units. [3-2] The composition according to the above [3-1], wherein the content of the polyoxyalkylene structure is 10% by mass to 60% by mass. [3-3] The composition according to the above [3-1] or [3-2], wherein the total content of Q units is 10% by mass to 50% by mass. [3-4] The composition according to any one of the above [3-1] to [3-3], wherein the compound (A) contains a crosslinkable silicon unit. [3-5] The composition according to any one of the above [3-1] to [3-4], wherein the compound (A) includes a compound having two crosslinkable silicon units per molecule. [3-6] The composition according to any one of the above [3-1] to [3-5], further comprising a solvent. [3-7] The composition according to any one of [3-1] to [3-6] above, further comprising a boron-containing compound (C). [3-8] The composition according to any one of [3-1] to [3-7] above, which is a thermosetting composition.

[0255] [3-9] A method for producing a cured product, comprising heating the composition according to any one of [3-1] to [3-8].

[0256] [3-10] A method for producing a cured-material-containing carbon material, comprising heating the composition according to any one of [3-1] to [3-8] above in the presence of a carbon material. [3-11] A method for producing a cured-material-containing carbon material, comprising using the cured-material-containing carbon material obtained by the method according to [3-10] above as a negative electrode active material. [3-12] A method for producing a negative electrode, comprising the step of forming a negative electrode active material layer on a current collector using the cured-material-containing carbon material obtained by the method according to [3-10] above to obtain a negative electrode. [3-13] A method for producing a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, comprising the step of forming a negative electrode active material layer on a current collector using the cured-material-containing carbon material obtained by the method according to [3-10] above to obtain a negative electrode.

[0257] [3-14] A cured product comprising a polyoxyalkylene structure and a three-dimensional siloxane structure containing Q units. [3-15] The cured product according to [3-14] above, wherein the content of the polyoxyalkylene structure is 20% by mass to 80% by mass, based on 100% by mass of the cured product. [3-16] The cured product according to [3-14] or [3-15] above, wherein the content of silicon element is 10% by mass to 40% by mass, based on 100% by mass of the cured product. [3-17] The cured product according to any one of [3-14] to [3-16] above, wherein the total content of Q units is 20% by mass to 60% by mass, based on 100% by mass of the cured product.

[0258] [3-18] A cured-product-containing carbon material comprising the cured product according to any one of [3-14] to [3-17] above and a carbon material. [3-19] The cured-product-containing carbon material according to [3-18] above, which is used as a negative electrode active material.

[0259] [3-20] A method for producing a negative electrode, comprising the step of forming a negative electrode active material layer on a current collector using the cured product-containing carbon material described in [3-18] above to obtain a negative electrode. [3-21] A method for producing a secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, comprising the step of forming a negative electrode active material layer on a current collector using the cured product-containing carbon material described in [3-18] above to obtain a negative electrode.

[0260] The present invention will be explained in more detail below using examples, but the present invention is not limited to the description of the following examples as long as it does not deviate from the gist of the invention.

[0261] Test Example: Carbon Material Example A1-1: A carbon material having a specific surface area of ​​8.2 m 2 10 g of flake natural graphite particles having a rheological index of 0.1 / g and a Raman R value of 0.26 were dispersed in 100 mL of ethanol. 1.5 g of vinyltris(2-methoxyethoxy)silane as a silicon-containing compound was added to the dispersion and stirred for 30 minutes. After stirring, the ethanol was removed, and the mixture was heated at 150°C for 1 hour in a nitrogen atmosphere. After cooling, the mixture was washed with ethanol and vacuum dried in that order to obtain a carbon material.

[0262] Comparative Example A1-1: A carbonaceous material having a specific surface area of ​​8.2 m 210 g of flake natural graphite particles having a Raman R value of 0.26 and a viscosity of 1000 saccharin was heated in a nitrogen atmosphere at 150° C. for 1 hour. After cooling, the particles were washed with ethanol and dried in a vacuum to obtain a carbon material.

[0263] Example A1-2: Carbon material with a specific surface area of ​​1.5 m 2 10 g of artificial graphite particles with a r / g and a Raman R value of 0.05 were dispersed in 100 mL of ethanol. 1.5 g of vinyltris(2-methoxyethoxy)silane as a silicon-containing compound was added to the dispersion and stirred for 30 minutes. After stirring, the ethanol was removed, and the mixture was heated at 150°C for 1 hour under a nitrogen atmosphere. After cooling, the mixture was washed with ethanol and vacuum dried in that order to obtain a carbon material.

[0264] Comparative Example A1-2: A carbonaceous material having a specific surface area of ​​1.5 m 2 10 g of artificial graphite particles having a Raman R value of 0.05 and a viscosity of 100 MPa were heated in a nitrogen atmosphere at 150° C. for 1 hour. After cooling, the particles were washed with ethanol and dried in a vacuum to obtain a carbon material.

[0265] Test Examples: Secondary Battery Examples A2-1, A2-2, and Comparative Examples A2-1, A2-2 The carbon materials obtained in Examples A1-1, A1-2, and Comparative Examples A1-1, A1-2 were used as negative electrode active materials to fabricate negative electrodes having a current collector and a negative electrode active material layer formed on the current collector. Specifically, 98 parts by mass of the carbon material obtained in Example A1-1 was mixed with 1 part by mass of carboxymethyl cellulose (CMC) and 2.1 parts by mass of a 48% by mass aqueous dispersion of styrene butadiene rubber (SBR) using a hybrid mixer to obtain a slurry. The obtained slurry was applied to a 20 μm-thick copper foil current collector at a basis weight of 7 to 8 mg / cm. 2 The coating was applied so that the coating adhered to the surface, and then dried. After that, the density of the negative electrode active material layer was 1.6 to 1.7 g / cm 3 The mixture was roll-pressed using a 250 mmφ roll press equipped with a load cell so that the diameter of the negative electrode was 12.5 mm, and the resultant mixture was punched out into a circular shape having a diameter of 12.5 mm, followed by vacuum drying at 90° C. for 8 hours to obtain a negative electrode.

[0266] <Measurement and Evaluation> <Atomic concentration of silicon atoms x (Si)(atomic %) > atomic concentration x of silicon atoms in the carbon material (Si) The atomic percentages (atomic %) were measured using an X-ray photoelectron spectrometer (KRATOS ULTRA2, manufactured by Shimadzu Corporation). Specifically, the X-ray source was monochromated Al-Kα, output was 15 kV-225 W, charge neutralization filament current, filament bias, charge balance was 0.43 V, 1 V, 4 V, pass energy was 160 eV for wide spectrum, 20 eV for narrow spectrum, measurement area was 700 μm × 300 μm, take-off angle was 90°, and energy correction Si 2p = 103.5 eV (SiO 2 ) and the sample carbon material is embedded in indium metal and sampled, and the atomic concentration of silicon atoms x (Si) The results are shown in Table 1.

[0267] <Specific Surface Area> The specific surface area of ​​the carbonaceous material was measured using a specific surface area measuring device (Macsorb HM Model-1210, manufactured by Mountec Co., Ltd.). Specifically, the carbonaceous material sample was pretreated at 150°C under a nitrogen flow and then cooled to liquid nitrogen temperature. The specific surface area of ​​the carbonaceous material was then measured by the nitrogen adsorption BET single-point method using a gas flow method, using a nitrogen-helium mixed gas precisely adjusted so that the relative pressure of nitrogen to atmospheric pressure was 0.3. The results are shown in Table 1.

[0268] <Raman R value> The carbon material was filled into the measurement cell of a Raman spectrometer (LabRAM-HR Evolutin, manufactured by Horiba, Ltd.) by gravity dropping. Next, an argon ion laser beam (wavelength 514.5 nm) was irradiated into the measurement cell, and the measurement cell was rotated in a plane perpendicular to the laser beam to obtain a Raman spectrum. The measurement conditions were as follows: Wavelength of argon ion laser beam: 514.5 nm Laser power on sample: 25 mW Resolution: 4 cm -1 Measurement range: 1100 cm -1 ~1730cm -1Peak intensity measurement, peak half-width measurement: background processing, smoothing processing (simple average convolution 5 points) From the Raman spectrum obtained above, -1 Nearby Peak P B Intensity I B And 1580 cm -1 Nearby Peak P A Intensity I A respectively, (intensity I B / Intensity I A The Raman R value, represented by

[0269] <Initial Discharge Capacity and Initial Efficiency> The obtained negative electrode and a lithium foil as a counter electrode were stacked with a separator impregnated with an electrolyte solution in between to prepare a battery for charge-discharge tests. The electrolyte solution was a mixture of ethylene carbonate / ethyl methyl carbonate = 30 / 70 (volume ratio) and LiPF 6 was dissolved to a concentration of 1.2 mol / L.

[0270] First, the battery for charge / discharge test was charged at 0.08 mA / cm 2 The battery was charged at a current density of 0.03 mA / cm until the battery voltage reached 5 mV, and then at a constant voltage of 5 mV, the current density was increased to 0.03 mA / cm. 2 This is called the initial charge. 2 The battery was discharged at a current density of 0.05 V until the battery voltage reached 1.5 V. This is called initial discharge. In addition, flowing a current in a direction in which lithium is doped into the negative electrode of the battery for charge / discharge test is called "charging," and flowing a current in a direction in which lithium is de-doped from the negative electrode is called "discharging."

[0271] The initial charge capacity and initial discharge capacity (mAh / g) were calculated by subtracting the mass of the copper foil (current collector) punched to the same area as the negative electrode from the mass of the entire negative electrode to determine the mass of the negative electrode active material. The current capacity during initial charge and discharge was then divided by the mass of the negative electrode active material calculated above to determine the initial charge capacity and initial discharge capacity, and the initial efficiency was calculated using the following formula (II). The results are shown in Table 2. Initial efficiency (%) = initial discharge capacity / initial charge capacity × 100 (II)

[0272] Test Example: Secondary Battery Example A3-1 A methanol solution 1 containing 10% by mass of the same composition as in Example C6 described below was prepared. 10 g of the graphite material obtained in Example A1-2 was dispersed in 100 ml of methanol to prepare a methanol solution 2. 1 g of methanol solution 1 was added to methanol solution 2 and stirred for 1 hour. After stirring, the methanol was removed, and the resulting mixture was heated to 120°C to obtain a cured-material-containing carbon material of Example A3-1. A negative electrode was obtained in the same manner as in Example A2-1 using the cured-material-containing carbon material obtained above.

[0273] Example A3-2 A negative electrode was obtained in the same manner as in Example A3-1, except that 5 g of methanol solution 1 was added to methanol solution 2.

[0274] Example A3-3 A negative electrode was obtained in the same manner as in Example A3-1, except that 10 g of the graphite material obtained in Comparative Example A1-2 was dispersed in 100 ml of methanol to prepare a methanol solution 2.

[0275] The resulting negative electrode and a lithium foil as a counter electrode were stacked with a separator impregnated with an electrolyte solution in between to prepare a battery for charge-discharge tests. The electrolyte solution was a mixture of ethylene carbonate / ethyl methyl carbonate = 30 / 70 (volume ratio) and LiPF 6 The initial charge capacity and the initial discharge capacity were determined by the same evaluation methods as in Examples A2-1 and A2-2, and the results are shown in Table 3.

[0276]

[0277]

[0278]

[0279] From the above results, it was found that the carbon material according to the present embodiment has x / y in a predetermined range, i.e., the atomic concentration of silicon atoms on the surface of the carbon material is in an appropriate range, and therefore, when used in the negative electrode of a secondary battery, the initial efficiency can be improved while maintaining the initial discharge capacity, and stable negative electrode operation is possible.

[0280] Test Example: Carbon Material Example B1-1: A carbon material having a specific surface area of ​​8.2 m was used as a raw material. 2 10 g of flake natural graphite particles having a r / g and a Raman R value of 0.26 were dispersed in 100 mL of ethanol. 1.5 g of vinylphosphonic acid as a phosphorus-containing compound was added to the dispersion and stirred for 30 minutes. After stirring, the ethanol was removed, and the mixture was heated at 150°C for 1 hour under a nitrogen atmosphere. After cooling, the mixture was washed with ethanol and dried in vacuo to obtain a phosphate group-containing carbonaceous raw material. Next, the phosphate group-containing carbonaceous raw material obtained above was dispersed in 80 mL of ethanol. 20 mL of an ethanol solution of 0.3 g of (ethylacetoacetato)aluminum diisopropoxide was added dropwise to this dispersion while stirring the dispersion. After the dropwise addition, the mixture was heated to 40°C and stirred for 1 hour, and then the ethanol was removed. The mixture was then heated at 150°C for 1 hour under air and cooled to obtain a carbonaceous material.

[0281] Example B1-2: Carbon material with a specific surface area of ​​8.2 m 2 10 g of flake natural graphite particles having a r / g and a Raman R value of 0.26 were dispersed in 100 mL of water. 1 g of ammonium persulfate was added to the dispersion, which was then heated to 40°C and stirred for 1 hour. After stirring, the powder was separated by filtration, and the obtained powder was dispersed in 80 mL of ethanol. 20 mL of an ethanol solution of 0.3 g of (ethylacetoacetato)aluminum diisopropoxide was added dropwise to this dispersion while stirring. After the dropwise addition, the dispersion was heated to 40°C and stirred for 1 hour, and then the ethanol was removed. The mixture was then heated in air at 150°C for 1 hour and cooled to obtain a carbon material.

[0282] Comparative Example B1-1: A carbonaceous material having a specific surface area of ​​8.2 m 2 10 g of flake natural graphite particles having a Raman R value of 0.26 and a viscosity of 1000 saccharin was heated in a nitrogen atmosphere at 150° C. for 1 hour. After cooling, the particles were washed with ethanol and dried in a vacuum to obtain a carbon material.

[0283] Comparative Example B1-2: Carbon material with a specific surface area of ​​8.2 m 210 g of flake natural graphite particles having a rheological index of 0.1 / g and a Raman R value of 0.26 were dispersed in 100 mL of ethanol. 1.5 g of vinylphosphonic acid was added to this dispersion and stirred for 30 minutes. After stirring, the ethanol was removed, and the mixture was heated at 150°C under nitrogen for 1 hour. After cooling, the mixture was washed with ethanol and dried in vacuum, to obtain a carbon material.

[0284] Test Example: Secondary Battery Examples B2-1, B2-2, and Comparative Examples B2-1, B2-2 The carbon materials obtained in Examples B1-1, B1-2, and Comparative Examples B1-1, B1-2 were used as negative electrode active materials to fabricate negative electrodes in which a current collector and a negative electrode active material layer were formed on the current collector. Specifically, 98 parts by mass of the carbon material obtained in Example B1-1 were mixed with 1 part by mass of carboxymethyl cellulose (CMC) and 2.1 parts by mass of a 48% by mass aqueous dispersion of styrene butadiene rubber (SBR) using a hybrid mixer to obtain a slurry. The obtained slurry was applied to a 20 μm-thick copper foil current collector at a basis weight of 7 to 8 mg / cm. 2 The coating was applied so that the coating adhered to the surface, and then dried. After that, the density of the negative electrode active material layer was 1.6 to 1.7 g / cm 3 The mixture was roll-pressed using a 250 mmφ roll press equipped with a load cell so that the diameter of the negative electrode was 12.5 mm, and the resultant mixture was punched out into a circular shape having a diameter of 12.5 mm, followed by vacuum drying at 90° C. for 8 hours to obtain a negative electrode.

[0285] <Measurement and Evaluation> <Atomic concentration x of aluminum atoms and phosphorus atoms (Al) (atomic %) > atomic concentration x of aluminum atoms in the carbon material (Al) The atomic concentration (atomic %) of phosphorus atoms and the atomic concentration (atomic %) of phosphorus atoms were measured using an X-ray photoelectron spectrometer (KRATOS ULTRA2, manufactured by Shimadzu Corporation). Specifically, the X-ray source was monochromated Al-Kα, the output was 15 kV-225 W, the filament current for neutralization of electron charge, the filament bias, and the charge balance were set to 0.43 V, 1 V, and 4 V, and the pass energy was set to 160 eV for wide spectrum and 20 eV for narrow spectrum, a measurement area of ​​700 μm×300 μm, a take-off angle of 90°, and an energy correction Si 2p=103.5 eV (SiO 2The carbon material sample was embedded in indium metal and sampled, and the atomic concentrations (atomic %) of aluminum atoms and phosphorus atoms were measured. The results are shown in Table 4.

[0286] <Specific Surface Area> The specific surface area of ​​the carbonaceous material was measured using a specific surface area measuring device (Macsorb HM Model-1210, manufactured by Mountec Co., Ltd.). Specifically, the carbonaceous material sample was pretreated at 150°C under a nitrogen flow and then cooled to liquid nitrogen temperature. The specific surface area of ​​the carbonaceous material was then measured by the nitrogen adsorption BET single-point method using a gas flow method, using a nitrogen-helium mixed gas precisely adjusted so that the relative pressure of nitrogen to atmospheric pressure was 0.3. The results are shown in Table 4.

[0287] <Raman R value> The carbon material was filled into the measurement cell of a Raman spectrometer (LabRAM-HR Evolutin, manufactured by Horiba, Ltd.) by gravity dropping. Next, an argon ion laser beam (wavelength 514.5 nm) was irradiated into the measurement cell, and the measurement cell was rotated in a plane perpendicular to the laser beam to obtain a Raman spectrum. The measurement conditions were as follows: Wavelength of argon ion laser beam: 514.5 nm Laser power on sample: 25 mW Resolution: 4 cm -1 Measurement range: 1100 cm -1 ~1730cm -1 Peak intensity measurement, peak half-width measurement: background processing, smoothing processing (simple average convolution 5 points) From the Raman spectrum obtained above, -1 Nearby Peak P B Intensity I B And 1580 cm -1 Nearby Peak P A Intensity I A respectively, (intensity I B / Intensity I A The Raman R value, represented by

[0288] <Initial Discharge Capacity and Initial Efficiency> The obtained negative electrode and a lithium foil as a counter electrode were stacked with a separator impregnated with an electrolyte solution in between to prepare a battery for charge-discharge tests. The electrolyte solution was a mixture of ethylene carbonate / ethyl methyl carbonate = 30 / 70 (volume ratio) and LiPF 6 was dissolved to a concentration of 1.2 mol / L.

[0289] First, the battery for charge / discharge test was charged at 0.08 mA / cm 2 The battery was charged at a current density of 0.03 mA / cm until the battery voltage reached 5 mV, and then at a constant voltage of 5 mV, the current density was increased to 0.03 mA / cm. 2 This is called the initial charge. 2 The battery was discharged at a current density of 0.05 V until the battery voltage reached 1.5 V. This is called initial discharge. In addition, flowing a current in a direction in which lithium is doped into the negative electrode of the battery for charge / discharge test is called "charging," and flowing a current in a direction in which lithium is de-doped from the negative electrode is called "discharging."

[0290] The initial charge capacity and initial discharge capacity (mAh / g) were calculated by subtracting the mass of the copper foil (current collector) punched to the same area as the negative electrode from the mass of the entire negative electrode to determine the mass of the negative electrode active material. The current capacity during initial charge and discharge was then divided by the mass of the negative electrode active material calculated above to determine the initial charge capacity and initial discharge capacity, and the initial efficiency was calculated using the following formula (II). The results are shown in Table 5. Initial efficiency (%) = initial discharge capacity / initial charge capacity × 100 (II)

[0291]

[0292]

[0293] From the above results, it was found that the carbon material according to the present embodiment has x / y in a predetermined range, i.e., the atomic concentration of aluminum atoms on the surface of the carbon material is in an appropriate range, and therefore, when used in the negative electrode of a secondary battery, the initial efficiency can be improved while maintaining the initial discharge capacity, and stable negative electrode operation is possible.

[0294] Test Examples: Compositions and Cured Products Measurement Methods for Dissolution Rate and Swelling Rate 0.15 g of the cured product obtained in the Examples and Comparative Examples was precisely weighed into a 20 mL glass bottle, and the mass (W S ) was recorded. Next, 15 mL of demineralized water at 23°C was added using a measuring cylinder, the glass bottle was sealed, and the bottle was immersed for 1 hour while being shaken every 10 minutes. After 1 hour, the cured product was removed with tweezers, excess water was absorbed with a paper towel, and the product was placed in an aluminum cup on a balance and accurately weighed. The wet weight (W W The cured product was then placed in the aluminum cup in a dryer at 110°C and dried for 2 to 3 hours until it reached a constant weight. The temperature was then returned to 23°C in a desiccator and the dry weight (W D The water elution rate was calculated by the following formula (III), and the water swelling rate was calculated by the following formula (VI). The same procedures as above were carried out to determine the organic solvent elution rate and the organic solvent swelling rate, except that demineralized water was replaced with ethyl methyl carbonate. Elution rate [mass %] = (W S -W D ) ÷ W S × 100 (III) Swelling ratio [mass%] = (W W -W S ) ÷ W S × 100 (VI)

[0295] <Raw Materials> Compound (A-1) Bis(3-triethoxysilylpropyl)polyethylene oxide (25-30 EO) (product name "SIB1824.84", manufactured by Gelest) was used as compound (A-1). Compound (A-1) is a compound having alkoxysilyl groups of T units attached to both ends of a polyoxyalkylene structure via organic linking chains, and has an oxide-equivalent solid content of 86 mass%. The oxide-equivalent solid content is a calculated value obtained by expressing the molecular weight, as a percentage of the molecular weight of the original compound, when all of the alkoxy groups of the compound have been hydrolyzed and completely converted to siloxane bonds.

[0296] Compound (A-2) N,N'-bis-[(3-triethoxysilylpropyl)aminocarbonyl]polyethylene oxide (10-15 EO) (product name "SIB1824.82", manufactured by Gelest Co., Ltd.) was used as compound (A-2). Compound (A-2) is a compound having alkoxysilyl groups of T units at both ends of a polyoxyalkylene structure via organic linking chains, and has a solid content of 79 mass% calculated as oxide.

[0297] Compound (A-3) N,N'-bis-[(3-triethoxysilylpropyl)aminocarbonyl]polyethylene oxide (7-10 EO) (product name "SIB1824.81", manufactured by Gelest Co., Ltd.) was used as compound (A-3). Compound (A-3) is a compound having alkoxysilyl groups of T units at both ends of a polyoxyalkylene structure via organic linking chains, and has a solid content of 75 mass% calculated as oxide.

[0298] Compound (B-1) 30.8 parts by mass of a partially hydrolyzed oligomer of tetramethoxysilane consisting of silicon of Q units (product name "MKC Silicate MS51"), 62.4 parts by mass of methanol, 0.3 parts by mass of maleic acid as a catalyst, and 6.5 parts by mass of demineralized water for hydrolysis were stirred in a sealed container at 23°C for 1 hour to cause hydrolytic polycondensation, and then allowed to stand at 23°C for 24 hours to obtain compound (B-1). The solid content of compound (B-1) was SiO 2 This corresponds to 16% by mass.

[0299] Production Example 1: Production of Compound (C-1) Solution Phenylboronic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as compound (C-1). When compound (C-1) was used, it was diluted with methanol and used as a 20 mass % methanol solution.

[0300] Example C1 77 parts by mass of compound (A-1), 207 parts by mass of compound (B-1), and 4 parts by mass of 0.01N aqueous acetic acid for hydrolysis of compound (A-1) were blended so that the solid content derived from compound (A-1) in the cured product was 70% by mass and the solid content derived from compound (B-1) was 30% by mass, and the mixture was stirred at 23°C for 3 hours to obtain a composition containing methanol as a solvent. The obtained composition was air-dried overnight in an aluminum cup and then dried to a constant weight in a dryer at 120°C to obtain a cured product. The evaluation results of the obtained cured product are shown in Table 6.

[0301] Examples C2 to C6, Comparative Examples C1 to C3 Cured products were obtained in the same manner as in Example C1, except that the type of compound (A), the content of solids derived from compound (A) in the cured product, the type of compound (B), the content of solids derived from compound (B) in the cured product, the type of compound (C), and the content of solids derived from compound (C) in the cured product were changed as shown in Table 6. The evaluation results of the obtained cured products are shown in Table 7.

[0302]

[0303]

[0304] As can be seen from Table 7, the cured products obtained in Examples C1 to C6, which contained a polyoxyalkylene structure and a three-dimensional siloxane structure, were able to reduce the water elution rate, organic solvent elution rate, water swelling rate, and organic solvent swelling rate. On the other hand, the cured products obtained in Comparative Examples C1 and C2, which did not contain Q units, were unable to reduce the water elution rate, organic solvent elution rate, water swelling rate, or organic solvent swelling rate. Furthermore, the cured product obtained in Comparative Example C3, which did not contain Q units, was able to reduce the water elution rate and organic solvent elution rate, but was unable to reduce the water swelling rate or organic solvent swelling rate.

[0305] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent applications filed on March 13, 2023 (Patent Application No. 2023-038966), March 13, 2023 (Patent Application No. 2023-038967), and March 14, 2023 (Patent Application No. 2023-040025), the contents of which are incorporated herein by reference.

[0306] The carbon material according to the present embodiment can be used as a negative electrode active material for a secondary battery to improve initial efficiency while maintaining initial discharge capacity, thereby enabling stable negative electrode operation. Therefore, the carbon material can be suitably used as a negative electrode active material for a secondary battery, more suitably used as a negative electrode active material for a non-aqueous secondary battery, and particularly suitably used as a negative electrode active material for a non-aqueous lithium-ion secondary battery.

[0307] The cured product according to the present embodiment has a sufficiently reduced elution rate and swelling rate in water or organic solvents, and therefore a cured-product-containing carbon material containing the cured product is excellent in suppressing side reactions in batteries and can be used more preferably as an active material for the negative electrode of a nonaqueous secondary battery, and particularly preferably as an active material for the negative electrode of a lithium-ion secondary battery.

Claims

1. A cured product comprising a polyoxyalkylene structure and a three-dimensional siloxane structure having a Q unit, and having a swelling rate with ethyl methyl carbonate of 70 mass% or less.

2. The cured product according to claim 1, wherein the content of the polyoxyalkylene structure in the cured product is 20% by mass to 80% by mass.

3. The cured product according to claim 1, wherein the content of silicon atoms in the cured product is 10% by mass to 40% by mass.

4. The cured product according to claim 1, wherein the total content of the Q units in the cured product is 20% by mass to 60% by mass.

5. The cured product according to claim 1, which contains a polyoxyalkylene structure and a fragment having at least two silicon atoms in one molecule after the cured product is hydrolyzed.

6. A cured product-containing carbon material comprising the cured product according to claim 1 and a carbon material.

7. The carbon material containing a cured product according to claim 6, wherein the carbon material has a modifying component bonded to a raw carbon material, and the modifying component contains at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur and germanium.

8. The cured carbonaceous material according to claim 7, wherein the modifying component has a binding site capable of binding to the carbonaceous material.

9. The cured carbon material according to claim 7, wherein the modifying component has a molecular weight of 500 or less.

10. The cured carbon material according to claim 7, wherein the modifying component is represented by the following general formula (1): (Z) n -L-W (1) (In the general formula (1), Z is a group capable of chemically bonding to a carbon material, W is a group containing at least one element selected from the group consisting of boron, aluminum, silicon, phosphorus, sulfur and germanium, L is a linker, and n is 1 or 2.) 11. The carbon-containing cured material according to claim 10, wherein in said general formula (1), W is a group containing silicon.

12. The carbon-containing cured material according to claim 10, wherein Z in the general formula (1) contains a structure capable of addition by a Diels-Alder reaction.

13. The carbon-containing cured material according to claim 10, wherein Z in the general formula (1) is a group containing an unsaturated bond at the end.

14. The carbon-containing cured material according to claim 10, wherein Z in the general formula (1) is a vinyl group.

15. The carbon material containing a cured product according to claim 7, wherein the surface of the carbon material contains carbon-carbon unsaturated bonds and carbon radical structures.

16. A negative electrode comprising the cured carbon material according to any one of claims 6 to 15.

17. A non-aqueous secondary battery comprising a positive electrode and a negative electrode capable of absorbing and releasing lithium ions, and an electrolyte, wherein the negative electrode comprises the cured product-containing carbon material according to any one of claims 6 to 15.

Citation Information

Patent Citations

  • Carbon electrode material for lithium secondary battery, manufacture of it, and lithium secondary battery using it

    JP1997161848A

  • Anode material for lithium secondary battery, manufacturing method of the same, lithium secondary battery anode using the same, and lithium secondary battery

    JP2007042285A

  • Topical skin preparation

    JP2023038966A

  • Topical skin preparation

    JP2023038967A

  • Composite substrate for electro-optical devices

    JP2023040025A