Property restoration method for flexible microstructure substrate having high aspect ratio
Through the methods of ultrasonic cleaning and supercritical fluid replacement, the problem of aggregation and deformation of flexible microstructure substrates during the demoulding process is solved, and high aspect ratio substrate preparation is achieved, ensuring the accuracy and efficiency of the preparation process.
Patent Information
- Application Number
- PCT/CN2023/084643
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-03
AI Technical Summary
When preparing flexible microstructured substrates with high aspect ratios, structural agglomeration, deformation or collapse is prone to occur during the demolding process, resulting in the inability to obtain high aspect ratio substrates.
Using ultrasonic cleaning and supercritical fluid replacement methods, ultrasonic waves are used to separate the agglomerated flexible microstructure substrates, and the supercritical fluid is used to release the accumulated stress, allowing the substrates to dry and renature, thereby achieving the preparation of high aspect ratio flexible microstructure substrates.
It effectively avoids the agglomeration and deformation of the flexible microstructure substrate during the demoulding process, ensures high aspect ratio substrate preparation, and improves the accuracy and efficiency of the preparation process.
Smart Images

Figure CN2023084643_03102024_PF_FP_ABST
Abstract
Description
Refolding method for flexible microstructure substrates with high aspect ratio Technical Field
[0001] The present invention relates to the field of flexible microstructure substrate processing, in particular to a method for remodeling a flexible microstructure substrate with a high aspect ratio. Background Art
[0002] Flexible microstructured substrates (such as micropillar arrays and microtip arrays) are widely used in biosensors and flexible bio-MEMs due to their lightweight, durable, flexible, low-cost, and easy mass production. Specifically, they can be used to sort different cell types and analyze cell mechanical properties using their structural properties.
[0003] To improve the efficiency of cell sorting and the accuracy of analytical testing, it is necessary to prepare flexible microstructure substrates with a high aspect ratio. Currently, flexible microstructure substrates are usually prepared using a reverse molding method. Specifically, the reverse mold structure is completed on a silicon wafer, and then the reverse mold structure is soaked in liquid prepolymer and thermally cured to form and demold the flexible microstructure substrate.
[0004] When preparing a flexible microstructure substrate with a high aspect ratio, during the demolding process, the flexible microstructure may aggregate, deform, or collapse due to stress, thereby failing to obtain a flexible microstructure substrate with a high aspect ratio.
[0005] Summary of the Invention
[0006] The present invention provides a method for remodeling a flexible microstructure substrate with a high aspect ratio, which improves the problems of microstructure agglomeration, deformation or collapse encountered during substrate preparation, thereby obtaining a flexible microstructure substrate with a high aspect ratio.
[0007] The present invention provides a method for refolding a flexible microstructure substrate, comprising:
[0008] placing the flexible microstructure substrate in a first refolding solvent and performing ultrasound, wherein the first refolding solvent immerses the flexible microstructure substrate;
[0009] Taking the flexible microstructure substrate out of the first refolding solvent and transferring it into a chamber containing a second refolding solvent, wherein the second refolding solvent immerses the flexible microstructure substrate;
[0010] A supercritical fluid is introduced to replace the second refolding solvent in the chamber; after the second refolding solvent is completely replaced, the supercritical fluid is discharged.
[0011] Preferably, the first refolding solvent is an alcohol solution; and the second refolding solvent is an alcohol solution.
[0012] Preferably, the first refolding solvent is the same as the second refolding solvent.
[0013] Preferably, the first refolding solvent includes ethanol or isopropanol; and the second refolding solvent includes ethanol or isopropanol.
[0014] Preferably, the supercritical fluid is carbon dioxide or methane.
[0015] Preferably, the ultrasonication time is 30s-90s, for example, 40s, 50s, 60s, 70s, 80s, etc.
[0016] Preferably, the supercritical fluid replacement time is 10-12 hours.
[0017] Preferably, the flexible microstructure substrate has patterned structural features.
[0018] Preferably, the flexible microstructure substrate is a micro-pillar array or a micro-tip array structure.
[0019] Preferably, the flexible microstructure substrate is made of organic silicon material.
[0020] Preferably, the flexible microstructure substrate is made of PDMS.
[0021] Preferably, the flexible microstructure substrate has an aspect ratio of 3 or more.
[0022] Preferably, the aspect ratio of the flexible microstructure substrate is greater than 5.
[0023] In summary, the present invention provides a method for refolding a flexible microstructure substrate with a high aspect ratio. The method comprises placing the flexible microstructure substrate in a first refolding solvent and subjecting it to ultrasonic treatment, wherein the first refolding solvent submerges the flexible microstructure substrate; removing the flexible microstructure substrate from the first refolding solvent and transferring it to a chamber containing a second refolding solvent, wherein the second refolding solvent submerges the flexible microstructure substrate; introducing a supercritical fluid to displace the second refolding solvent in the chamber; and after completely displacing the second refolding solvent, draining the supercritical fluid. The method provided by the present invention utilizes ultrasonic cleaning of the flexible microstructure substrate immersed in the first refolding solvent. Because ultrasonic waves are mechanical waves, they can separate flexible microstructure substrates that have aggregated, deformed, or collapsed. Subsequently, the second refolding solvent in which the flexible microstructure substrate is immersed is replaced with a supercritical fluid. Because the surface tension of the supercritical fluid is zero, the replacement process releases the stress accumulated in the flexible microstructure substrate after ultrasonic cleaning, allowing the flexible microstructure substrate to dry and refold. This makes it possible to prepare flexible microstructure substrates with a high aspect ratio by casting. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0025] FIG1 is a flow chart of a method for refolding a flexible microstructure substrate with a high aspect ratio provided by an embodiment of the present invention;
[0026] FIG2 is a flexible microstructure substrate having a micropillar array provided by an embodiment of the present invention;
[0027] FIG3 is a schematic diagram of supercritical fluid replacement using a supercritical fluid dryer according to an embodiment of the present invention.
[0028] In the above drawings, the components represented by the reference numerals are as follows:
[0029] 1. Micropillar array; 2. Flexible microstructure substrate; 3. Second refolding solvent; 4. Filler; 5. Supercritical fluid dryer; 6. Supercritical fluid. DETAILED DESCRIPTION
[0030] In order to make the above and other features and advantages of the present invention more clear, the present invention is further described below with reference to the accompanying drawings. It should be understood that the specific embodiments given herein are for the purpose of explaining to those skilled in the art and are only exemplary and not restrictive.
[0031] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one such feature. In the description of the present invention, "plurality" means at least two, such as two, three, etc., unless otherwise specifically defined.
[0032] In the description of this specification, the reference terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and features of different embodiments or examples without contradiction.
[0033] In the following description, many specific details are set forth to provide a thorough understanding of the present invention. However, it will be apparent to one of ordinary skill in the art that it is not necessary to employ these specific details to practice the present invention. In other cases, well-known steps or operations are not described in detail to avoid obscuring the present invention.
[0034] The present invention first discloses a method for preparing a flexible microstructure substrate by a reverse molding method, taking the preparation of a microcolumn array from PDMS as an example.
[0035] A counter mold is fabricated, and a microwell array is fabricated on a silicon plate, serving as the counter mold for the micropillar array. The silicon plate is then surface-silanized to render the surface hydrophobic and enhance adhesion to the chemical vapor deposition coating. The silane is preferably trichlorosilane (1H,1H,2H,2H-perfluorooctyl).
[0036] Invert the mold, mix the PDMS matrix and hardener in a ratio of 10:1 and evacuate the mixture to obtain a bubble-free mixture; soak the silicon plate in the mixture and bake it at 70-120℃ for 4.5h-6h, then allow the silicon plate to cool naturally; peel off the silicon plate to obtain a flexible microstructure substrate with a high aspect ratio.
[0037] However, if the aspect ratio of the flexible microstructure is greater than 3, and particularly greater than 5, the flexible microstructure substrate prepared using the above method may exhibit structural agglomeration. Therefore, to address the technical issue of structural agglomeration in flexible microstructure substrates with high aspect ratios similar to those manufactured using the above method, the following solution is proposed.
[0038] Referring to FIG1 , the present invention provides a method for refolding a flexible microstructure substrate with a high aspect ratio, comprising:
[0039] S110 , placing the flexible microstructure substrate in a first refolding solvent and performing ultrasound treatment, wherein the first refolding solvent immerses the flexible microstructure substrate.
[0040] Specifically, the flexible microstructure substrate involved in the present invention does not only refer to the micropillar array prepared by the above method, but is also applicable to structures with patterned structural features and micro-tip array structures. The flexible microstructure substrate is placed in a first refolding solvent and ultrasonicated. The characteristics of ultrasonic waves as mechanical waves can be used to separate the flexible microstructure substrates that have agglomerated by mechanical vibration. The ultrasonication time should not be too short or too long, preferably 30s-90s, for example, 40s, 50s, 60s, 70s, 80s, etc. This is to avoid the purpose of separating the agglomerated flexible microstructure substrates being too short, and the structural performance of the flexible microstructure substrate being easily damaged by too long an ultrasonication time.
[0041] It should be noted that when the flexible microstructure substrate is made of an organosilicon material, particularly polydimethylsiloxane (PDMS), a non-corrosive alcohol, preferably ethanol or isopropanol, should be selected to prevent the first refolding solvent from corroding the flexible microstructure substrate. Furthermore, the first refolding solvent must be able to fully immerse the flexible microstructure substrate so that the mechanical vibrations of the first refolding solvent induced by ultrasound can act on the entire flexible microstructure substrate.
[0042] S120 , taking the flexible microstructure out of the first refolding solvent and transferring it into a chamber containing a second refolding solvent, wherein the second refolding solvent immerses the flexible microstructure substrate.
[0043] After ultrasonicating the flexible microstructure substrate, the flexible microstructure must be immediately removed from the first refolding solvent and transferred to a chamber containing a second refolding solvent to prevent the separated flexible microstructure substrates from reuniting. Furthermore, to prevent reuniting, the second refolding solvent must completely submerge the flexible microstructure substrate. Furthermore, if the flexible microstructure substrate is made of an organosilicon material, particularly polydimethylsiloxane (PDMS), the second refolding solvent should be a non-corrosive alcohol, preferably ethanol or isopropanol, to prevent corrosion of the flexible microstructure substrate.
[0044] S130 , introducing a supercritical fluid to replace the second refolding solvent in the chamber; after the second refolding solvent is completely replaced, the supercritical fluid is discharged.
[0045] The second refolding solvent in the chamber is replaced by a supercritical fluid. The zero surface tension characteristic of the supercritical fluid can be used to release the stress accumulated on the flexible microstructure substrate after ultrasonication, so that the flexible microstructure substrate can be dried and refolded.
[0046] Since the supercritical fluid replaces the second refolding solvent very slowly, excessive use of the second refolding solvent should be avoided while ensuring that the flexible microstructure substrate is completely immersed in the second refolding solvent.
[0047] It should be noted that the choice of refolding solvent requires a critical point significantly lower than that of water (374.15°C, 22.129 MPa) to ensure stress release in flexible microstructures. Therefore, ethanol and isopropanol are preferred. Ethanol has a critical temperature of 243.1°C and a critical pressure of 6.383 MPa, while isopropanol has a critical temperature of 234.9°C and a critical pressure of 4.764 MPa. Acetone can also be used as a refolding solvent for polymers that are not susceptible to acetone corrosion.
[0048] Accordingly, regarding the selection of the refolding solvent, in the method provided by the present invention, the supercritical fluid needs to have a critical point, that is, the fluid is a supercritical fluid when it exceeds the critical temperature and critical pressure, and the fluid is a gas at room temperature and pressure. Therefore, the supercritical fluid used in the present invention is preferably carbon dioxide or methane. Because carbon dioxide or methane is a uniform fluid between a gas and a liquid under a supercritical state, the viscosity of this fluid is close to that of a gas and the diffusion coefficient is about ten times that of a liquid, but the density is close to that of a liquid. This fluid does not have a gas-liquid interface with alcohols during the displacement process, which helps to release the internal stress of the microstructure.
[0049] In addition, during the ultrasonic and supercritical fluid displacement processes, the open side of the micropillar array of the flexible microstructure substrate must face upward. This ensures that the micropillar array of the flexible microstructure substrate has sufficient space to expand, facilitates the separation of aggregated flexible microstructure substrates during the ultrasonic process, and facilitates the release of accumulated stress in the flexible microstructure substrate during the supercritical fluid displacement process.
[0050] In the above discussion, the inventors have used micropillar arrays as an example, but this should not be construed as limiting the present invention. The method provided by the present invention is also applicable to microtip arrays and patterned structures having microstructures.
[0051] 2-3 , in order to make the purpose, technical solutions and beneficial effects of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments, but the specific embodiments described are only used to explain the present invention and are not used to limit the present invention.
[0052] The ultrasonic instrument and supercritical fluid dryer in this application can be selected from commercially available models. In the following examples, the ultrasonic instrument used is a Fisherbrand 11207 advanced ultrasonic cleaner, and the supercritical fluid dryer used is a Leica EM CPD300 fully automatic critical point dryer.
[0053] Example 1
[0054] Fabrication of the reverse mold: After a micropore array is fabricated on a silicon plate using a photolithography-deep silicon etching process as a reverse mold of the micropillar array, the silicon plate is subjected to a surface silanization treatment using trichlorosilane as the silane.
[0055] Molding: PDMS matrix and hardener were mixed in a 10:1 ratio and vacuumed to obtain a bubble-free mixture. This mixture was then immersed in a tin foil box with a micropillar reverse mold placed at the bottom. The mixture was baked on an 80°C hotplate for 6 hours, then the hotplate was turned off and allowed to cool naturally. The tin foil was removed, and the cured PDMS substrate was peeled from the template, resulting in a micropillar array with an aspect ratio of approximately 5. Microscopic observation revealed agglomeration of the micropillar array.
[0056] Ultrasonic cleaning: immerse the agglomerated PDMS substrate in a beaker containing isopropyl alcohol, and place the beaker in an ultrasonic cleaning machine for ultrasonic cleaning at room temperature for 60 seconds.
[0057] Supercritical Fluid Replacement: Immediately transfer the ultrasonically cleaned PDMS substrate with the micropillar array to the replacement chamber of a supercritical fluid dryer. Fill one-third of the chamber with isopropyl alcohol (completely submerging the flexible microstructured substrate) and the remainder with plastic blocks. Start the supercritical fluid dryer and set the replacement time for 11 hours. Use supercritical carbon dioxide fluid to gradually replace the isopropyl alcohol in the replacement chamber.
[0058] Draining: After the supercritical fluid replacement is completed, drain the supercritical fluid in the replacement chamber.
[0059] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. More than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0060] Example 2
[0061] Ultrasonic cleaning: A flexible microstructure substrate having a collapsed patterned structure with an aspect ratio of about 3 was immersed in a beaker containing isopropyl alcohol. The beaker was placed in an ultrasonic cleaning machine and ultrasonically cleaned at room temperature for 30 seconds.
[0062] Supercritical Fluid Replacement: Immediately transfer the ultrasonically cleaned flexible microstructure substrate to the replacement chamber of a supercritical fluid dryer. Fill one-third of the chamber with isopropyl alcohol (completely submerging the flexible microstructure substrate) and the remaining volume with plastic blocks. Start the supercritical fluid dryer, set the replacement time to 10 hours, and gradually replace the isopropyl alcohol in the replacement chamber with supercritical carbon dioxide fluid.
[0063] Draining: After the supercritical fluid replacement is completed, drain the supercritical fluid in the replacement chamber.
[0064] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. More than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0065] Example 3
[0066] Ultrasonic cleaning: A flexible microstructure substrate having agglomeration, a microtip array, and an aspect ratio of about 6 was immersed in a beaker containing ethanol, and the beaker was placed in an ultrasonic cleaning machine for ultrasonic cleaning at room temperature for 90 seconds.
[0067] Supercritical Fluid Replacement: Immediately transfer the ultrasonically cleaned flexible microstructured substrate to the replacement chamber of a supercritical fluid dryer. Fill one-third of the chamber with ethanol (completely submerging the flexible microstructured substrate) and the remaining volume with plastic blocks. Start the supercritical fluid dryer, set the replacement time to 12 hours, and gradually replace the ethanol in the replacement chamber with supercritical methane fluid.
[0068] Draining: After the supercritical fluid replacement is completed, drain the supercritical fluid in the replacement chamber.
[0069] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. More than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0070] Example 4
[0071] The ultrasonic cleaning, supercritical fluid replacement and draining steps of this embodiment are the same as those of Example 2; the difference is that the aspect ratio of the micropillar array of the flexible microstructure with agglomeration phenomenon is about 3.5, the ultrasonic cleaning time is 40 seconds, and the supercritical fluid replacement time is 10 hours.
[0072] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. More than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0073] Example 5
[0074] The ultrasonic cleaning, supercritical fluid replacement and draining steps of this embodiment are the same as those of Example 2; the difference is that the aspect ratio of the micropillar array of the flexible microstructure with agglomeration phenomenon is about 4, the ultrasonic cleaning time is 50 seconds, and the supercritical fluid replacement time is 11 hours.
[0075] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. More than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0076] Example 6
[0077] The ultrasonic cleaning, supercritical fluid replacement and draining steps of this embodiment are the same as those of Example 2; the difference is that the aspect ratio of the micropillar array of the flexible microstructure with agglomeration is about 4.5, the ultrasonic cleaning time is 70 seconds, and the supercritical fluid replacement time is 11 hours.
[0078] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. It was found that more than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0079] Example 7
[0080] The ultrasonic cleaning, supercritical fluid replacement and draining steps of this embodiment are the same as those of Example 2; the difference is that the aspect ratio of the micropillar array of the flexible microstructure with agglomeration phenomenon is about 5.5, the ultrasonic cleaning time is 80 seconds, and the supercritical fluid replacement time is 12 hours.
[0081] Result analysis: The PDMS micropillar array was taken out from the replacement chamber and observed under a microscope. More than 95% of the micropillars in the PDMS micropillar array had been deagglomerated.
[0082] In summary, by comparing Examples 1 to 7, it can be seen that the method provided by the present invention is suitable for flexible microstructure substrates with an aspect ratio of more than 3 that have problems of agglomeration, deformation or collapse. Furthermore, in Examples 1, 3 and 7, when the aspect ratio is more than 5, this method is also applicable.
[0083] Although the embodiments of the present invention have been shown and described above, it will be understood that the above embodiments are illustrative and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention.
Claims
1. A method for renaturing a flexible microstructure substrate, characterized in that: include: Placing the flexible microstructure substrate in a first remodeling solvent and performing ultrasound, wherein the first remodeling solvent immerses the flexible microstructure substrate; Taking the flexible microstructure substrate out of the first remodeling solvent and transferring it into a chamber containing a second remodeling solvent, wherein the second remodeling solvent immerses the flexible microstructure substrate; A supercritical fluid is introduced to replace the second refolding solvent in the chamber; after the second refolding solvent is completely replaced, the supercritical fluid is discharged.
2. The renaturation method according to claim 1, characterized in that: The first refolding solvent is an alcohol solution; the second refolding solvent is an alcohol solution.
3. The renaturation method according to claim 1 or 2, characterized in that: The first refolding solvent is the same as the second refolding solvent.
4. The renaturation method according to any one of claims 1 to 3, characterized in that: The first refolding solvent includes ethanol or isopropanol; the second refolding solvent includes ethanol or isopropanol.
5. The renaturation method according to any one of claims 1 to 4, characterized in that: The supercritical fluid is carbon dioxide or methane.
6. The renaturation method according to any one of claims 1 to 5, characterized in that: The ultrasound time is 30s-90s.
7. The renaturation method according to any one of claims 1 to 6, characterized in that: The supercritical fluid replacement time is 10-12h.
8. The renaturation method according to any one of claims 1 to 7, characterized in that: The flexible microstructure substrate has patterned structural features.
9. The renaturation method according to any one of claims 1 to 8, characterized in that: The flexible microstructure substrate is a micro-column array or a micro-tip array structure.
10. The renaturation method according to any one of claims 1 to 9, characterized in that: The flexible microstructure substrate is made of organic silicon material.
11. The renaturation method according to any one of claims 1 to 10, characterized in that: The flexible microstructure substrate is made of PDMS.
12. The renaturation method according to any one of claims 1 to 11, characterized in that: The aspect ratio of the flexible microstructure substrate is greater than 3.
13. The renaturation method according to any one of claims 1 to 11, characterized in that: The flexible microstructure substrate has a depth-to-width ratio of greater than 5.
Citation Information
Patent Citations
Flexible pressure sensor manufacturing method based on V-shaped groove array electrode
CN106946221A
Preparation method of flexible thin film based on graphene micro column array
CN107556508A
Ultrasonic transducer using aerogel as filler material
CN109569999A
Preparation method of secondary microstructure realizing super-hydrophobicity of material surface
CN109679128A
Flexible pressure sensor and preparation method thereof
CN115307793A