Electrochemical device and electronic device

By introducing Mn element into the cathode material of lithium-ion battery and adding boron-containing lithium salt into the electrolyte, combined with appropriate electrolyte components and separator structure, the stability problem of lithium-ion battery under high voltage and high temperature conditions is solved and realized It balances the thermal stability and cycle stability of the battery and improves the overall performance of the battery.

WO2024197646A1PCT designated stage expired Publication Date: 2024-10-03NINGDE AMPEREX TECHNOLOGY LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/084725
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Lithium-ion batteries have poor stability under high voltage and high temperature conditions. In particular, it is difficult to balance the thermal stability and cycle stability of the cathode material, and the increase in doping elements will cause the thermal stability of the negative electrode to deteriorate.

Method used

By introducing Mn element into the cathode material and adding boron-containing lithium salts, especially lithium dioxaloborate, to the electrolyte, the composition of the electrolyte is adjusted to form a stable and effective passivation film, and the thermal stability and conductivity of the electrolyte are improved. , combined with appropriate amounts of carboxylate and nitrile additives, to optimize the membrane structure to enhance interface protection.

Benefits of technology

It achieves both thermal stability and cycle stability of lithium-ion batteries under high voltage and high temperature conditions, extends the service life of the battery, and improves the high-temperature cycle performance and hot box safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023084725-FTAPPB-I100001
    Figure PCTCN2023084725-FTAPPB-I100001
  • Figure PCTCN2023084725-FTAPPB-I100002
    Figure PCTCN2023084725-FTAPPB-I100002
  • Figure PCTCN2023084725-FTAPPB-I100003
    Figure PCTCN2023084725-FTAPPB-I100003
Patent Text Reader

Abstract

The present application provides an electrochemical device and an electronic device. The electrochemical device comprises: a positive electrode, wherein the positive electrode comprises a positive electrode active material, the positive electrode active material comprises metal elements Co and Mn, and the mass percentage of Mn is B% based on the total mass of the positive electrode active material; and an electrolyte, wherein the electrolyte comprises a boron-containing lithium salt, and the mass percentage of the boron-containing lithium salt is C% based on the total mass of the electrolyte, wherein 0.05≤C≤1, and 0.01≤C / 10B≤2. The electrochemical device of the present application has both high-temperature stability and cycle stability under high voltage, and also has excellent hot-box performance.
Need to check novelty before this filing date? Find Prior Art

Description

Electrochemical device and electronic device Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to an electrochemical device and an electronic device. Background Art

[0002] Lithium-ion batteries, with their high specific energy, high operating voltage, low self-discharge rate, compact size, and light weight, are widely used in various fields, including energy storage, portable electronic devices, and electric vehicles. As the use of lithium-ion batteries continues to expand, the market is placing higher demands on them, such as requiring them to have higher energy density and longer service life.

[0003] Increasing the operating cutoff voltage of lithium-ion batteries can significantly increase the battery's energy density. However, as the voltage increases, the battery's stability, especially high-temperature stability, deteriorates sharply. Positive electrode doping can significantly improve the positive electrode's thermal stability. However, as the doping element increases, the positive electrode material gradually dissolves, significantly threatening the negative electrode's thermal stability. This application primarily achieves a balance between positive and negative electrode thermal stability and cycling stability by adjusting the positive electrode material and electrolyte.

[0004] Summary of the Invention

[0005] The purpose of this application is to provide an electrochemical device and an electronic device to improve the high-temperature cycle performance and room-temperature cycle performance of the electrochemical device, as well as the hot box performance. The specific technical solution is as follows:

[0006] In one embodiment, the present application provides an electrochemical device, comprising a positive electrode, the positive electrode comprising a positive electrode active material, the positive electrode active material comprising metal elements Co and Mn, wherein the mass percentage of Mn based on the total mass of the positive electrode active material is B%; and an electrolyte, the electrolyte comprising a boron-containing lithium salt, wherein the mass percentage of the boron-containing lithium salt based on the total mass of the electrolyte is C%; wherein 0.05≤C≤1 and 0.01≤C / 10B≤2.

[0007] The inventors of the present application found that introducing the doping element Mn has an obvious effect on improving the high-temperature stability of the cathode material at high voltages. Without being limited to any theory, this may be because Mn stabilizes O, thereby enhancing the structural stability of the cathode material. However, it was also found that as the content of the Mn element further increases, the thermal stability of the anode deteriorates. However, by introducing a boron-containing lithium salt into the electrolyte, the thermal stability of both the cathode and the anode can be taken into account, and it was found that when C / 10B is within the above range, the effect is the most obvious. Without being limited to any theory, this may be because the introduction of the above boron-containing lithium salt inhibits the dissolution of manganese ions and enhances the thermal stability, hydrolysis stability and oxidation stability of the electrolyte, compensating for the deterioration of the dissolution of the cathode material caused by metal element doping. In addition, the electrolyte containing lithium bis(oxalato)borate (LiBOB) has the following characteristics: it can form a stable and effective passivation film in a propylene carbonate (PC) solution, does not corrode the current collector aluminum foil, and the discharge capacity does not decay under high-temperature conditions, thereby achieving the balance of the thermal stability of the positive and negative electrodes.

[0008] In some embodiments, the electrochemical device satisfies at least one of the following conditions:

[0009] (a) 0.1 ≤ C ≤ 1;

[0010] (b) 0.05 ≤ C / 10B ≤ 1.

[0011] In some embodiments, based on the total mass of the cathode active material, the mass percentage content of Co is A%, and A and B satisfy at least one of the following conditions: 0.05 ≤ B ≤ 0.5; 6 ≤ A / 20B ≤ 60. Without being limited to any theory, within this range of the Mn element, the structural stability of the cathode material can be further enhanced, thereby improving the thermal stability and high-temperature cycle stability of the battery under high voltages.

[0012] In some embodiments, the cathode active material includes Li α Co 1-x-y Mn x M y O β , where M includes one or more of Mg, Al, Ca, Ti, Zr, V, Cr, Fe, Ni, Cu, Zn, Ru or Sn, where 0.95 ≤ α ≤ 1.4, 0 < x ≤ 0.4, 0 ≤ y ≤ 0.3 and 1.90 ≤ β ≤ 2.10.

[0013] In some embodiments, the boron-containing lithium salt includes at least one of lithium bis(1,1-trifluoromethyl oxalato)borate, lithium bis(1-trifluoromethyl oxalato)borate, lithium difluoro(1,1-trifluoromethyl)oxalato borate, lithium difluorooxalato borate, lithium bis(oxalato)borate, lithium bis(1,1-trifluoromethyl malonate)borate, lithium fluoromalonate difluoroborate or lithium bis(fluoromalonate)borate.

[0014] Boron-containing lithium salts will protect the cathode, inhibit the occurrence of related side reactions, and further improve the high-temperature stability of the electrolyte and the cycle stability of the electrochemical device.

[0015] In some embodiments, the electrolyte satisfies at least one of the following:

[0016] (a) the electrolyte further comprises a carboxylate, wherein the mass percentage of the carboxylate is X%, based on the total mass of the electrolyte, and 10≤X≤60;

[0017] (b) the electrolyte further comprises ethylene carbonate and propylene carbonate, wherein, based on the total mass of the electrolyte, the mass percentage of the ethylene carbonate is D%, and the mass percentage of the propylene carbonate is E%, wherein 5≤D+E≤40, and D≥E;

[0018] (c) the electrolyte further comprises at least one of 1,3-propane sultone, vinyl sulfate, vinylene carbonate, a bicyclic carbonate compound, a bicyclic sulfate compound, a trinitrile compound, or a dinitrile compound; or

[0019] (d) The electrolyte further comprises at least one of lithium hexafluorophosphate, lithium bis(trifluoromethane)sulfonyl imide, lithium bis(fluorosulfonyl)imide or lithium difluorophosphate.

[0020] In some embodiments, the electrolyte satisfies at least one of the following conditions:

[0021] a) based on the total mass of the electrolyte, the mass percentage of the 1,3-propane sultone is 0.5% to 5%;

[0022] b) based on the total mass of the electrolyte, the mass percentage of the vinyl sulfate is 0.1% to 1%;

[0023] c) based on the total mass of the electrolyte, the mass percentage of the vinylene carbonate is 0.1% to 1%;

[0024] d) based on the total mass of the electrolyte, the mass percentage of the bicyclic carbonate compound is 0.1% to 30%;

[0025] e) based on the total mass of the electrolyte, the mass percentage of the bicyclic sulfate compound is 0.1% to 5%;

[0026] f) based on the total mass of the electrolyte, the mass percentage of the trinitrile compound is 0.1% to 10%; or

[0027] j) Based on the total mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 10%.

[0028] In some embodiments, the carboxylic acid ester comprises at least one of methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, propyl propionate, butyl propionate, pentyl propionate, methyl haloacetate, ethyl haloacetate, propyl haloacetate, ethyl halopropionate, propyl halopropionate, butyl halopropionate, or pentyl halopropionate.

[0029] Without being limited to any theory, the introduction of carboxylic acid esters can significantly reduce the viscosity of the electrolyte, increase the conductivity of the electrolyte, and thereby increase the transmission rate of lithium ions in the battery, reduce battery polarization, and compensate for the deterioration of the kinetics and room temperature performance caused by the positive electrode doping elements.

[0030] Without being limited by theory, adjusting the amounts of ethylene carbonate and propylene carbonate can enhance interfacial protection of the negative electrode, reduce electrolyte consumption, and further enhance the thermal stability and high-temperature cycling stability of the lithium-ion battery. Without being limited by theory, adjusting the electrolyte additives described above within the scope of this application can further strengthen the interfacial film and further improve the thermal stability of the lithium-ion battery.

[0031] In some embodiments, the electrochemical device further includes a separator, the separator including a porous substrate and a porous coating disposed on at least one surface of the porous substrate, wherein the porous coating includes inorganic particles and a binder.

[0032] In some embodiments, the membrane satisfies at least one of the following:

[0033] (a) the inorganic particles in the porous coating layer include at least one of magnesium hydroxide, boehmite or aluminum oxide;

[0034] (b) the binder in the porous coating layer comprises polyvinylidene fluoride; or

[0035] (c) The thickness of the porous coating layer is T μm, 1≤T≤5.

[0036] In another embodiment, the present application provides an electronic device comprising the electrochemical device according to the embodiment of the present application.

[0037] The electrochemical device provided in the present application has both thermal stability at high voltage and high temperature cycle stability as well as improved hot box performance.

[0038] Additional aspects and advantages of the embodiments of the present application will be described and shown in part in the subsequent description, or explained through the implementation of the embodiments of the present application. DETAILED DESCRIPTION

[0039] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described in detail below with reference to the embodiments. It is apparent that the embodiments described are only a portion of the embodiments of this application, rather than all of them. All other technical solutions derived by those of ordinary skill in the art based on the embodiments in this application fall within the scope of protection of this application.

[0040] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0041] In addition, amounts, ratios, and other numerical values ​​are sometimes presented herein in a range format. It should be understood that such a range format is used for convenience and brevity and should be interpreted flexibly to include not only the values ​​explicitly specified as limits of the range, but also all individual values ​​or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.

[0042] In the detailed description and claims, a list of items linked by the terms "one of," "one of," "a kind of," or other similar terms may mean any of the listed items. For example, if items A and B are listed, the phrase "one of A and B" means only A or only B. In another example, if items A, B, and C are listed, the phrase "one of A, B, and C" means only A; only B; or only C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0043] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.

[0044] 1. Electrochemical Device

[0045] In some embodiments, the present application provides an electrochemical device, comprising: a positive electrode, the positive electrode comprising a positive electrode active material, the positive electrode active material comprising metal elements Co and Mn, wherein the mass percentage of Mn based on the total mass of the positive electrode active material is B%; and an electrolyte, the electrolyte comprising a boron-containing lithium salt, wherein the mass percentage of the boron-containing lithium salt based on the total mass of the electrolyte is C%; wherein 0.05≤C≤1 and 0.01≤C / 10B≤2.

[0046] In some embodiments, the electrochemical device satisfies at least one of the following conditions: (a) 0.1≤C≤1; or (b) 0.05≤C / 10B≤1.

[0047] In some embodiments, C is 0.05, 0.08, 0.1, 0.3, 0.5, 0.8, 1, or a range consisting of any two of these values.

[0048] In some embodiments, C / 10B is 0.01, 0.03, 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.4, 0.5, 0.8, 1, 1.5, 1.8, 2.0, or a range consisting of any two of these values.

[0049] In some embodiments, 0.05≤B≤0.5. In some embodiments, B is 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.5, or a range consisting of any two of these values.

[0050] In some embodiments, the mass percentage of Co based on the total mass of the positive electrode active material is A%, 10≤A≤90. In some embodiments, A is 10, 20, 30, 40, 50, 55, 58, 60, 62, 65, 70, 80, 90, or a range consisting of any two of these values.

[0051] In some embodiments, 6≤A / 20B≤60. In some embodiments, A / 20B is 6, 8, 10, 12, 15, 18, 20, 25, 28, 30, 32, 35, 40, 45, 50, 55, 60, or a range consisting of any two of these values.

[0052] In some embodiments, the positive electrode active material includes Li α Co 1-x-y Mn x M y O β, where M includes one or more of Mg, Al, Ca, Ti, Zr, V, Cr, Fe, Ni, Cu, Zn, Ru, or Sn, where 0.95 ≤ α ≤ 1.4, 0 < x ≤ 0.4, 0 ≤ y ≤ 0.3, and 1.90 ≤ β ≤ 2.10.

[0053] In some embodiments, the positive electrode active material includes lithium cobalt oxide.

[0054] In some embodiments, the boron-containing lithium salt includes at least one of lithium bis(1,1-trifluoromethyl oxalato)borate, lithium bis(1-trifluoromethyl oxalato)borate, lithium difluoro(1,1-trifluoromethyl)oxalato borate, lithium difluorooxalato borate, lithium bisoxalato borate, lithium bis(1,1-trifluoromethyl malonato)borate, lithium fluoromalonate difluoroborate, or lithium bis(fluoromalonate)borate.

[0055] In some embodiments, the boron-containing lithium salt includes at least one of LiDFOB or LiBOB.

[0056] In some embodiments, the electrolyte satisfies at least one of the following:

[0057] (a) The electrolyte further includes a carboxylic acid ester, where, based on the total mass of the electrolyte, the mass percentage of the carboxylic acid ester is X%, and 10 ≤ X ≤ 60;

[0058] (b) The electrolyte further includes ethylene carbonate and propylene carbonate, where, based on the total mass of the electrolyte, the mass percentage of ethylene carbonate is D%, and the mass percentage of propylene carbonate is E%, where 5 ≤ D + E ≤ 40, and D ≥ E;

[0059] (c) The electrolyte further includes at least one of 1,3-propane sultone, vinylene sulfate, vinylene carbonate, bicyclic carbonate compound, bicyclic sulfate compound, trinitrile compound, or dinitrile compound; or

[0060] (d) The electrolyte further includes at least one of lithium hexafluorophosphate, lithium bis(trifluoromethane)sulfonimide, lithium bis(fluorosulfonyl)imide, or lithium difluorophosphate.

[0061] In some embodiments, X is 10, 15, 20, 22, 28, 30, 32, 34, 36, 40, 50, 60, or a range formed by any two of these values.

[0062] In some embodiments, the electrolyte satisfies at least one of the following conditions:

[0063] a) Based on the total mass of the electrolyte, the mass percentage of 1,3-propane sultone is 0.5% to 5%;

[0064] b) based on the total mass of the electrolyte, the mass percentage of the vinyl sulfate is 0.1% to 1%;

[0065] c) based on the total mass of the electrolyte, the mass percentage of the vinylene carbonate is 0.1% to 1%;

[0066] d) based on the total mass of the electrolyte, the mass percentage of the bicyclic carbonate compound is 0.1% to 30%;

[0067] e) based on the total mass of the electrolyte, the mass percentage of the bicyclic sulfate compound is 0.1% to 5%;

[0068] f) based on the total mass of the electrolyte, the mass percentage of the trinitrile compound is 0.1% to 10%; or

[0069] j) Based on the total mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 10%.

[0070] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the 1,3-propane sultone is 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of these values.

[0071] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the vinyl sulfate is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or a range consisting of any two of these values.

[0072] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the vinylene carbonate is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or a range consisting of any two of these values.

[0073] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the bicyclic carbonate compound is 0.1%, 1%, 5%, 10%, 15%, 20%, 25%, 30% or a range consisting of any two of these values.

[0074] In some embodiments, based on the total mass of the electrolyte, the mass percentage of the bicyclic sulfate compound is 0.1%, 0.5%, 1%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or a range consisting of any two of these values. In some embodiments, the carboxylate comprises at least one of the following: methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, propyl propionate, butyl propionate, pentyl propionate, methyl haloacetate, ethyl haloacetate, propyl haloacetate, ethyl halopropionate, propyl halopropionate, butyl halopropionate, or pentyl halopropionate.

[0075] In some embodiments, the carboxylic acid esters include ethyl propionate and propyl propionate.

[0076] In some embodiments, the carboxylic acid esters include ethyl propionate, propyl propionate, and ethyl acetate.

[0077] In some embodiments, 5≤D≤40. In some embodiments, D is 5, 7, 10, 15, 18, 20, 25, 30, 35, 38, 40, or a range consisting of any two of these values.

[0078] In some embodiments, 0≤E≤30. In some embodiments, E is 0, 5, 8, 10, 15, 18, 20, 25, 30, or a range consisting of any two of these values.

[0079] In some embodiments, D>E.

[0080] In some embodiments, D+E is 5, 7, 10, 15, 18, 20, 25, 30, 35, 38, 40, or a range consisting of any two of these values.

[0081] In some embodiments, the trinitrile compound includes at least one of 1,3,5-pentanetricarboxylic acid nitrile, 1,2,3-propanetricarboxylic acid nitrile, 1,3,6-hexanetrinitrile, 1,2,6-hexanetrinitrile, 1,2,3-tris(2-cyanoethoxy)propane, 1,2,4-tris(2-cyanoethoxy)butane, or 1,2,5-tris(cyanoethoxy)pentane.

[0082] In some embodiments, the dinitrile compound includes at least one of succinonitrile, glutaronitrile, adiponitrile, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 1,8-dicyanooctane, 1,9-dicyanononane, 1,10-dicyanodecane, 1,12-dicyanododecane, tetramethylsuccinonitrile, 2-methylglutaronitrile, 2,4-dimethylglutaronitrile, and 2,2,4,4-tetramethylglutaronitrile.

[0083] In some embodiments, the mass percentage of the trinitrile compound is 0-10% based on the total mass of the electrolyte. In some embodiments, the mass percentage of the trinitrile compound is 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of these values.

[0084] In some embodiments, the mass percentage of the dinitrile compound is 0-10% based on the total mass of the electrolyte. In some embodiments, the mass percentage of the dinitrile compound is 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of these values.

[0085] In some embodiments, the weight percentage of the lithium hexafluorophosphate, lithium bis(trifluoromethane)sulfonyl imide, lithium bis(fluorosulfonyl)imide, or lithium difluorophosphate is 0.1-15%. In some embodiments, the weight percentage of the lithium hexafluorophosphate, lithium bis(trifluoromethane)sulfonyl imide, lithium bis(fluorosulfonyl)imide, or lithium difluorophosphate is 0.1%, 0.3%, 0.5%, 1%, 1.5%, 1.8%, 2.0%, 2.5%, 3%, 5%, 8%, 10%, 12%, 15%, or a range consisting of any two of these values.

[0086] In some embodiments, the electrolyte further comprises diethyl carbonate (DEC). In some embodiments, the mass percentage of diethyl carbonate based on the total mass of the electrolyte is 20-70%. In some embodiments, the mass percentage of diethyl carbonate based on the total mass of the electrolyte is 20%, 30%, 40%, 50%, 60%, 70%, or a range consisting of any two of these values.

[0087] In some embodiments, the positive electrode further comprises a conductive agent. In some embodiments, the conductive agent comprises at least one of carbon nanotubes, carbon fibers, acetylene black, graphene, Ketjen black, or carbon black.

[0088] In some embodiments, the positive electrode further includes a binder. In some embodiments, the binder includes at least one of polyvinylidene fluoride, carboxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, acrylated styrene-butadiene rubber, epoxy resin, or nylon.

[0089] In some embodiments, the current collector includes at least one of copper foil or aluminum foil.

[0090] In some embodiments, the positive electrode can be prepared by methods known in the art. For example, the positive electrode can be obtained by mixing a positive electrode active material, a conductive agent, and a binder in a solvent to prepare an active material composition, and then coating the active material composition on a current collector. In some embodiments, the solvent can include, but is not limited to, N-methylpyrrolidone.

[0091] In some embodiments, the electrochemical device includes any device that undergoes an electrochemical reaction.

[0092] In some embodiments, the electrochemical device is a lithium secondary battery.

[0093] In some embodiments, the lithium secondary battery includes, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery or a lithium ion polymer secondary battery, and an all-solid-state secondary lithium battery.

[0094] negative electrode

[0095] In some embodiments, the material, composition and manufacturing method of the negative electrode used in the electrochemical device of the present application may include any technology disclosed in the prior art. In some embodiments, the negative electrode is a negative electrode described in U.S. patent application US9812739B, which is incorporated into the present application by reference in its entirety.

[0096] In some embodiments, the negative electrode includes a current collector and a negative electrode active material layer located on the current collector. In some embodiments, the negative electrode active material layer includes a negative electrode active material. In some embodiments, the negative electrode active material includes, but is not limited to: lithium metal, structured lithium metal, natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, silicon oxide materials (e.g., SiO, SiO2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithiated TiO2-Li4Ti5O 12 , Li-Al alloy or any combination thereof.

[0097] In some embodiments, the negative electrode active material layer includes a binder. In some embodiments, the binder includes, but is not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon.

[0098] In some embodiments, the negative electrode active material layer includes a conductive material. In some embodiments, the conductive material includes, but is not limited to, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, metal powder, metal fiber, copper, nickel, aluminum, silver, or a polyphenylene derivative.

[0099] In some embodiments, the current collector includes, but is not limited to, copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or a polymer substrate coated with a conductive metal.

[0100] In some embodiments, the negative electrode may be obtained by mixing an active material, a conductive material, and a binder in a solvent to prepare an active material composition, and coating the active material composition on a current collector.

[0101] In some embodiments, the solvent may include, but is not limited to, deionized water, N-methylpyrrolidone.

[0102] In some embodiments, the negative electrode in the all-solid-state secondary lithium battery is a metallic lithium foil.

[0103] diaphragm

[0104] In some embodiments, the electrochemical device further comprises a separator located between the positive electrode and the negative electrode, the separator comprising a porous substrate and a porous coating disposed on at least one surface of the porous substrate, wherein the porous coating comprises inorganic particles and a binder.

[0105] In some embodiments, the porous substrate has a porous coating disposed on one surface thereof. In some embodiments, the porous substrate has a porous coating disposed on both surfaces thereof.

[0106] In some embodiments, the membrane satisfies at least one of the following conditions:

[0107] (a) the inorganic particles in the porous coating layer include at least one of magnesium hydroxide, boehmite or aluminum oxide;

[0108] (b) the binder in the porous coating layer comprises polyvinylidene fluoride (PVDF); or

[0109] (c) The thickness of the porous coating layer is T μm, 1≤T≤5.

[0110] In some embodiments, T is 1, 2, 3, 4, 5, or a range consisting of any two of these values.

[0111] In some embodiments, the material and shape of the separator used in the electrochemical device of the present application are not particularly limited, and can be any material disclosed in the prior art.

[0112] In some embodiments, the porous substrate can be selected from one or more of a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane.

[0113] In some embodiments, the weight percentage of the fluorine-containing binder is 10-70% based on the total weight of the inorganic particles and the fluorine-containing binder in the porous coating layer. In some embodiments, the weight percentage of the fluorine-containing binder is 10%, 20%, 30%, 40%, 50%, 60%, 70%, or a range consisting of any two of these values, based on the total weight of the inorganic particles and the fluorine-containing binder in the porous coating layer.

[0114] In some embodiments, the mass percentage of the inorganic particles is 30-90% based on the total mass of the inorganic particles and the fluorine-containing binder in the porous coating. In some embodiments, the mass percentage of the inorganic particles is 30%, 40%, 50%, 60%, 70%, 80%, 90%, or a range consisting of any two of these values ​​based on the total mass of the inorganic particles and the fluorine-containing binder in the porous coating. The porous coating can improve the heat resistance, oxidation resistance, and electrolyte wetting properties of the isolation membrane, and enhance the adhesion between the isolation membrane and the electrode.

[0115] In some embodiments, the binder is selected from one or a combination of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polytetrafluoroethylene, and polyhexafluoropropylene.

[0116] electrolytes

[0117] In some embodiments, the electrolyte used in the electrolyte of the embodiment of the present application can be an electrolyte known in the prior art, including but not limited to: inorganic lithium salts, such as LiClO4, LiPF6, LiBF4, LiSbF6, LiSO3F, LiN(FSO2)2, etc.; fluorine-containing organic lithium salts, such as LiCF3SO3, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,3-hexafluoropropane disulfonyl imide lithium, cyclic 1,2-tetrafluoroethane disulfonyl imide lithium, LiN(CF3S O2)(C4F9SO2), LiC(CF3SO2)3, LiPF4(CF3)2, LiPF4(C2F5)2, LiPF4(CF3SO2)2, LiPF4(C2F5SO2)2, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, LiBF2(C2F5SO2)2; lithium salts containing dicarboxylic acid complexes, such as lithium bis(oxalato)borate, lithium difluorooxalatoborate, lithium tris(oxalato)phosphate, lithium difluorobis(oxalato)phosphate, lithium tetrafluoro(oxalato)phosphate, etc. In addition, the above electrolytes can be used alone or in combination of two or more. For example, in some embodiments, the electrolyte includes a combination of LiPF6 and LiBF4. In some embodiments, the electrolyte includes a combination of an inorganic lithium salt such as LiPF6 or LiBF4 and a fluorine-containing organic lithium salt such as LiCF3SO3, LiN(CF3SO2)2, or LiN(C2F5SO2)2. In some embodiments, the concentration of the electrolyte is in a range of 0.8 to 3 mol / L, such as 0.8 to 2.5 mol / L, 0.8 to 2 mol / L, 1 to 2 mol / L, 0.5 to 1.5 mol / L, 0.8 to 1.3 mol / L, 0.5 to 1.2 mol / L, and for example 1 mol / L, 1.15 mol / L, 1.2 mol / L, 1.5 mol / L, 2 mol / L, or 2.5 mol / L.

[0118] The preparation process of an electrochemical device is well known to those skilled in the art and is not particularly limited herein. For example, a lithium-ion battery can be manufactured by overlapping the positive and negative electrodes with a separator, winding and folding the electrodes as needed, and then placing the electrodes within a housing. The electrolyte is then injected into the housing and sealed. Furthermore, overcurrent protection elements, guide plates, and the like may be placed within the housing as needed to prevent internal pressure buildup and overcharging and discharging.

[0119] 2. Electronic Devices

[0120] The electronic device of the present application may be any device using the electrochemical device according to the embodiments of the present application.

[0121] In some embodiments, the electronic device includes, but is not limited to: a laptop computer, a pen-type computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.

[0122] The preparation of lithium-ion batteries is described below using lithium-ion batteries as an example and in combination with specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0123] Example

[0124] The following examples and comparative examples are given to illustrate the embodiments of the present application in more detail. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0125] 1. Test methods and equipment:

[0126] (1) Test of Co and Mn metal element content in positive electrode active materials:

[0127] The active material of the positive electrode sheet after washing with DMC (dimethyl carbonate) was scraped off with a scraper and dissolved in a mixed solvent (for example, 0.4 g of positive electrode active material was dissolved in a mixed solvent of 10 ml (nitric acid and hydrochloric acid mixed in a ratio of 1:1) aqua regia and 2 ml HF), and the volume was fixed to 100 ml. Then, an ICP analyzer was used to test the content of metal elements such as Co and Mn in the solution in %.

[0128] (2) Lithium-ion battery high temperature cycle performance test:

[0129] At 45°C, charge the lithium-ion battery at a constant current of 0.7C (rate) to 4.5V, then charge it at a constant voltage to a current of 0.05C, and then discharge it at a constant current of 1C to 3.0V. This process is one charge-discharge cycle, which is the first cycle. Record the discharge capacity of the lithium-ion battery in the first cycle. Perform charge-discharge cycles on the lithium-ion battery according to the above method, and record the discharge capacity of each cycle until the discharge capacity of the lithium-ion battery decays to 80% of the discharge capacity of the first cycle. Record the number of charge-discharge cycles.

[0130] (3) Lithium-ion battery room temperature cycle performance test:

[0131] At 25°C, charge the lithium-ion battery at a constant current of 0.7C (rate) to 4.5V, then charge it at a constant voltage to a current of 0.05C, and then discharge it at a constant current of 1C to 3.0V. This process is one charge-discharge cycle, which is the first cycle. Record the discharge capacity of the lithium-ion battery in the first cycle. Perform charge-discharge cycles on the lithium-ion battery according to the above method, and record the discharge capacity of each cycle until the discharge capacity of the lithium-ion battery decays to 80% of the discharge capacity of the first cycle. Record the number of charge-discharge cycles.

[0132] (4) Lithium-ion battery hot box safety test:

[0133] Before thermal shock testing, fully charge the battery cell. Inspect the appearance and take photos before and after testing. Place a temperature sensor at the center of the battery cell's outer surface. Place the sample vertically in a box and heat it at a rate of 2±2°C to the required test temperature (130 / 135)±2°C, maintaining the temperature for 60 minutes. Measurement frequency: Voltage and internal resistance measurements are performed at 1kHz, after preconditioning and post-test. Test criteria: Pass if no fire or explosion occurs. "5 / 10 Pass" indicates that 5 out of 10 batteries tested in each example passed the test.

[0134] 2. Preparation of lithium-ion batteries

[0135] Examples 1-9 and Comparative Examples 1-3

[0136] (1) Preparation of modified positive electrode active materials:

[0137] Commercially available lithium cobalt oxide (LiCoO2) and manganese dioxide (Mn3O4) were mixed and mixed in a high-speed mixer at 300 r / min for 20 minutes. The mixture was placed in an air kiln and heated to 820°C at 5°C / min, maintained for 24 hours, and then naturally cooled and taken out. The modified positive electrode active material (i.e., modified LiCoO2) was obtained after passing through a 300-mesh sieve. The total content of the metal elements Mn and Co in the modified positive electrode active material is shown in Table 1.

[0138] (2) Preparation of positive electrode sheet

[0139] Modified LiCoO2, conductive carbon nanotubes (CNTs), and binder polyvinylidene fluoride were mixed in a mass ratio of 95:2:3. N-methylpyrrolidone (NMP) was added as a solvent and stirred in a vacuum mixer until a uniform positive electrode slurry with a solids content of 75 wt% was formed. The positive electrode slurry was evenly coated on a 12 μm thick positive electrode current collector aluminum foil, dried at 85°C, and cold pressed to produce a positive electrode sheet with a 100 μm thick positive electrode active material layer. The above steps were repeated on the other surface of the positive electrode sheet to obtain a double-sided positive electrode sheet coated with a positive electrode active material layer. The positive electrode sheet was cut into 74 mm x 867 mm dimensions and welded to the tabs for later use.

[0140] (3) Preparation of negative electrode sheet

[0141] The negative electrode active materials, artificial graphite, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC), were mixed in a mass ratio of 95:2:3. Deionized water was then added as a solvent to form a slurry with a solid content of 70 wt%, which was then stirred evenly. The slurry was evenly coated on one surface of an 8 μm thick copper foil, dried at 110°C, and cold-pressed to produce a negative electrode sheet with a single-sided negative electrode active material layer of 150 μm thickness. The above coating steps were then repeated on the other surface of the negative electrode sheet to produce a negative electrode sheet coated on both sides with a negative electrode active material layer. The negative electrode sheet was cut into a size of (74 mm × 867 mm) and the tabs were welded before use. The defect level of the negative electrode sheet, Id / Ig, was 0.17.

[0142] (4) Preparation of electrolyte

[0143] In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were uniformly mixed in a mass ratio of 20:20:60 to form a base solvent. Lithium hexafluorophosphate (LiPF6) and a boron-containing lithium salt were added to the base solvent and stirred uniformly to form an electrolyte. The mass percentage of LiPF6, calculated based on the total mass of the electrolyte, was 12.5%. The specific types and mass percentages of the boron-containing lithium salts are shown in Table 1. The sum of the contents of each substance in the electrolyte is 100%.

[0144] In Table 1, LiDFOB stands for lithium difluorooxalatoborate, and LiBOB stands for lithium dioxalatoborate.

[0145] (5) Preparation of diaphragm

[0146] A 12μm-thick polyethylene (PE) porous polymer film was used as the separator. A 3μm-thick porous coating composed of Al2O3 and PVDF was applied to both surfaces of the base film. The Al2O3 content of the porous coating was 70% by weight, and the PVDF content was 30% by weight.

[0147] (6) Preparation of lithium-ion batteries

[0148] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to act as an isolate. The electrode assembly is wound to obtain an electrode assembly, which is then placed in an aluminum-plastic film packaging bag and dehydrated at 80°C. The prepared electrolyte is injected and a lithium-ion battery is obtained through processes such as vacuum packaging, standing, formation, and shaping.

[0149] Examples 10-14

[0150] Preparation of electrolyte:

[0151] In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), and a carboxylate were uniformly mixed in a mass ratio of 20:20:(60-X):X) to form a base solvent. LiPF6 and a boron-containing lithium salt were added to the base solvent and stirred uniformly to form an electrolyte. The mass percentage of the boron-containing lithium salt was 0.5%, and the mass percentage of LiPF6 was 12.5%, calculated based on the total mass of the electrolyte. The type and mass percentage of the carboxylate, as well as related preparation parameters and performance changes, are shown in Table 2. The carboxylate content in Table 2 is calculated based on the total mass of the base solvent. The sum of the contents of each substance in the electrolyte is 100%.

[0152] Except that the preparation of the electrolyte is different from that in Example 6, the rest is the same as that in Example 6.

[0153] Examples 15-20

[0154] Preparation of electrolyte:

[0155] In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), and / or propyl propionate (PP) were uniformly mixed to form a base solvent. LiPF6 and a boron-containing lithium salt were added to the base solvent and stirred evenly to form an electrolyte. Based on the total mass of the electrolyte, the mass percentage of the boron-containing lithium salt was 0.5%, and the mass percentage of LiPF6 was 12.5%. The mass percentages of other substances and related preparation parameters and performance changes are shown in Table 3. The contents of EC, PC, and PP in Table 3 are calculated based on the total mass of the base solvent. The sum of the contents of each substance in the electrolyte is 100%.

[0156] Except that the preparation of the electrolyte is different from that in Example 6, the rest is the same as that in Example 6.

[0157] Examples 21-23

[0158] Preparation of electrolyte:

[0159] In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), and / or propyl propionate (PP) were uniformly mixed to form a base solvent. LiPF6, lithium bis(oxalatoborate) (LiBOB), and 1,3,6-hexanetricarbonitrile were added to the base solvent and stirred uniformly to form an electrolyte. Based on the total mass of the electrolyte, the mass percentage of LiPF6 was 12.5%, the mass percentage of the boron-containing lithium salt was 0.5%, and the specific mass percentages of the other substances and changes in performance are shown in Table 4. The contents of EC, PC, and PP in Table 4 are calculated based on the total mass of the base solvent. The mass content of 1,3,6-hexanetricarbonitrile in Table 4 is calculated based on the total mass of the electrolyte. The sum of the contents of each substance in the electrolyte is 100%.

[0160] Except that the preparation of the electrolyte is different from that in Example 6, the rest is the same as that in Example 6.

[0161] Examples 24-27

[0162] In an argon atmosphere glove box with a water content of less than 10 ppm, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), and / or propyl propionate (PP) were uniformly mixed to form a base solvent. LiPF6, lithium bis(oxalatoborate) (LiBOB), and / or 1,3,6-hexanetricarbonitrile were added to the base solvent and stirred uniformly to form an electrolyte. Based on the total mass of the electrolyte, the mass percentage of LiPF6 was 12.5%, the mass percentage of the boron-containing lithium salt was 0.5%, and the specific mass percentages of the other substances and changes in performance are shown in Table 4. The contents of EC, PC, and PP in Table 5 are calculated based on the total mass of the base solvent. The mass content of 1,3,6-hexanetricarbonitrile in Table 5 is calculated based on the total mass of the electrolyte. The sum of the contents of each substance in the electrolyte is 100%.

[0163] Preparation of diaphragm:

[0164] A 12 μm thick polyethylene (PE) porous polymer film was used as the separator. A porous coating composed of Al2O3 and PVDF was coated on both surfaces of the base film. The thickness of the porous coating is shown in Table 5. The mass content of Al2O3 in the porous coating was 70%, and the mass content of PVDF in the porous coating was 30%.

[0165] Except that the preparation of the diaphragm and the electrolyte is different from that in Example 6, the rest is the same as that in Example 6.

[0166] Table 1

[0167] It can be seen from Examples 1 to 9 and Comparative Examples 1 to 3 in Table 1 that by adjusting C / 10B within the scope of this application, the 130°C hot box pass rate and 135°C hot box pass rate of the lithium-ion battery are significantly improved. Without being limited to any theory, this may be due to the stabilization of Mn on O, thereby improving the structural stability of the positive electrode material. However, it was also found that with the further increase of the Mn element content, the thermal stability of the negative electrode deteriorated. However, by introducing boron-containing lithium salts into the electrolyte, the thermal stability of both the positive and negative electrodes can be taken into account, and it was found that when C / 10B is within the above range, the effect is most obvious. Without being limited to any theory, this may be due to the introduction of the above-mentioned boron-containing lithium salts, which inhibits the dissolution of manganese ions and improves the thermal stability, hydrolytic stability and oxidative stability of the electrolyte, compensating for the deterioration of the dissolution of the positive electrode material caused by metal element doping. In addition, the electrolyte containing lithium bis(oxalatoborate) (LiBOB) has the following characteristics: it can form a stable and effective passivation film in propylene carbonate (PC) solution, does not corrode the current collector aluminum foil, and the discharge capacity does not decay under high temperature conditions, thereby achieving a balance between the thermal stability of the positive and negative electrodes.

[0168] Table 2

[0169] As shown in Examples 10 to 14 in Table 2, the introduction of an appropriate amount of carboxylate into the electrolyte improves both the high-temperature and room-temperature cycling stability of lithium-ion batteries. Without being limited by theory, the introduction of carboxylate can significantly reduce electrolyte viscosity and increase electrolyte conductivity, thereby increasing the lithium ion transport rate within the battery, reducing battery polarization, and compensating for the deterioration of kinetic and room-temperature performance caused by positive electrode doping.

[0170] Table 3

[0171] As can be seen from Examples 15 to 20 in Table 3, when D and E are within the scope of this application, the lithium-ion battery can achieve better cycle performance. Without being limited to any theory, adjusting the amount of ethylene carbonate and propylene carbonate can strengthen the interface protection of the negative electrode, reduce the electrolyte consumption rate, and further enhance the thermal stability and high-temperature cycle stability of the lithium-ion battery. Without being limited to any theory, by adjusting the above-mentioned electrolyte additives within the scope of this application, the interface film can be further strengthened, which can further improve the thermal stability of the lithium-ion battery.

[0172] Table 4

[0173] As can be seen from Examples 21 to 23 in Table 4, adding nitrile additives, such as 1,3,6-hexanetricarbonitrile, to the electrolyte can further improve the cycling stability of lithium-ion batteries. Without being limited by any theory, the cyano group in the nitrile additive has strong coordination ability and can bind to active sites on the electrode surface, such as high-valent tetravalent cobalt ions. This acts to mask these active ions on the positive electrode surface, reducing the decomposition of the electrolyte by the electrode, reducing side reactions, and thus improving cycling performance.

[0174] Table 5

[0175] It can be seen from Examples 24-27 in Table 5 that the high-temperature and room-temperature cycling performance of lithium-ion batteries can be further improved when the thickness of the porous coating of the separator is 1-5 μm.

[0176] References throughout this specification to "some embodiments," "some embodiments," "one embodiment," "another example," "an example," "a specific example," or "a portion of an example" mean that at least one embodiment or example in this application includes the particular features, structures, materials, or characteristics described in that embodiment or example. Therefore, descriptions appearing throughout this specification, such as "in some embodiments," "in an embodiment," "in one embodiment," "in another example," "in an example," "in a specific example," or "an example," are not necessarily references to the same embodiment or example in this application. In addition, the particular features, structures, materials, or characteristics described herein may be combined in any suitable manner in one or more embodiments or examples.

[0177] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.

Claims

1. An electrochemical device comprising: A positive electrode, the positive electrode comprising a positive electrode active material, the positive electrode active material comprising metal elements Co and Mn, wherein the mass percentage of Mn is B% based on the total mass of the positive electrode active material; and An electrolyte, wherein the electrolyte comprises a boron-containing lithium salt, wherein the mass percentage of the boron-containing lithium salt is C% based on the total mass of the electrolyte; Among them, 0.05≤C≤1, and 0.01≤C / 10B≤2.

2. The electrochemical device according to claim 1, wherein: The electrochemical device satisfies at least one of the following conditions: (a) 0.1≤C≤1; (b)0.05≤C / 10B≤1.

3. The electrochemical device according to claim 1, wherein Based on the total mass of the positive electrode active material, the mass percentage content of Co is A%, and A and B satisfy at least one of the following conditions: 0.05≤B≤0.5; 6≤A / 20B≤60.

4. The electrochemical device according to claim 1, wherein The positive electrode active material includes Li α Co 1-x-y Mn x M y O β , wherein M includes one or more of Mg, Al, Ca, Ti, Zr, V, Cr, Fe, Ni, Cu, Zn, Ru or Sn, wherein 0.95 ≤ α ≤ 1.4, 0 < x ≤ 0.4, 0 ≤ y ≤ 0.3 and 1.90 ≤ β ≤ 2.

10.

5. The electrochemical device according to claim 1, wherein The boron-containing lithium salt includes at least one of lithium bis(1,1-trifluoromethyloxalato)borate, lithium bis(1-trifluoromethyloxalato)borate, lithium difluoro(1,1-trifluoromethyl)oxalatoborate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium bis(1,1-trifluoromethylmalonate)borate, lithium fluoromalonate difluoroborate or lithium bis(fluoromalonate)borate.

6. The electrochemical device according to claim 1, wherein The electrolyte satisfies at least one of the following: (a) The electrolyte further comprises a carboxylate, wherein the mass of the carboxylate is The percentage content is X%, 10≤X≤60; (b) the electrolyte further comprises ethylene carbonate and propylene carbonate, wherein, based on the total mass of the electrolyte, the mass percentage of the ethylene carbonate is D%, and the mass percentage of the propylene carbonate is E%, wherein 5≤D+E≤40, and D≥E; (c) the electrolyte further comprises at least one of 1,3-propane sultone, vinyl sulfate, vinylene carbonate, a bicyclic carbonate compound, a bicyclic sulfate compound, a trinitrile compound or a dinitrile compound; or (d) The electrolyte further comprises at least one of lithium hexafluorophosphate, lithium bis(trifluoromethane)sulfonyl imide, lithium bis(fluorosulfonyl)imide or lithium difluorophosphate.

7. The electrochemical device of claim 6, wherein the carboxylic acid ester comprises at least one of methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, propyl propionate, butyl propionate, pentyl propionate, methyl haloacetate, ethyl haloacetate, propyl haloacetate, ethyl halopropionate, propyl halopropionate, butyl halopropionate, or pentyl halopropionate.

8. The electrochemical device according to claim 5, wherein the electrolyte satisfies at least one of the following conditions: a) based on the total mass of the electrolyte, the mass percentage of the 1,3-propane sultone is 0.5% to 5%; b) based on the total mass of the electrolyte, the mass percentage of the vinyl sulfate is 0.1% to 1%; c) based on the total mass of the electrolyte, the mass percentage of the vinylene carbonate is 0.1% to 1%; d) based on the total mass of the electrolyte, the mass percentage of the bicyclic carbonate compound is 0.1% to 30%; e) based on the total mass of the electrolyte, the mass percentage of the bicyclic sulfate compound is 0.1% to 5%; f) based on the total mass of the electrolyte, the mass percentage of the trinitrile compound is 0.1% to 10%; or j) Based on the total mass of the electrolyte, the mass percentage of the dinitrile compound is 0.1% to 10%.

9. The electrochemical device according to claim 1, further comprising a separator, the separator comprising a porous substrate and a porous coating disposed on at least one surface of the porous substrate, wherein The porous coating layer includes inorganic particles and a binder.

10. The electrochemical device according to claim 9, wherein: The diaphragm satisfies at least one of the following: (a) the inorganic particles in the porous coating layer include at least one of magnesium hydroxide, boehmite or aluminum oxide; (b) the binder in the porous coating layer includes polyvinylidene fluoride; or (c) The thickness of the porous coating layer is T μm, 1≤T≤5.

11. An electronic device comprising the electrochemical device according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Electrolyte additive and use thereof in lithium-ion battery

    US9812739B2

  • Lithium titanate battery electrolyte film-forming additive doped with zirconium by gradients

    CN103840191A

  • High-rate high-energy density lithium ion battery

    CN110350239A

  • High-nickel lithium ion battery non-aqueous electrolyte and lithium ion battery

    CN112349959A

  • Electrochemical device and electronic device including same

    CN114051662A