Negative electrode material and preparation method therefor, electrochemical device, and electronic device

By forming the first Si-C covalently bonded silicon carbide and silicon particle layer on the inner wall surface of the porous carbon matrix, the volume expansion and stability problems of silicon-based anode materials in lithium-ion batteries are solved, and a more stable battery cycle is achieved. performance and safety features.

WO2024197715A1PCT designated stage expired Publication Date: 2024-10-03NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
PCT/CN2023/085140
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Silicon-based anode materials in lithium-ion batteries have poor cycle stability due to their high volume expansion rate and surface activity, which can easily lead to electrolyte consumption and solid electrolyte film formation, leading to rapid battery capacity attenuation.

Method used

It adopts a porous silicon carbon particle structure, in which the first silicon carbide layer and the first silicon particle layer are formed on the inner wall surface of the porous carbon matrix, and are connected through Si-C covalent bonds to limit the expansion of the silicon particles and prevent them from falling off, forming a stable solid electrolyte interface. .

Benefits of technology

Significantly improves the cycle performance and safety performance of lithium-ion batteries, reduces irreversible capacity loss in the first cycle of charge and discharge, and delays capacity fading.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023085140_03102024_PF_FP_ABST
    Figure CN2023085140_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a negative electrode material and a preparation method therefor, an electrochemical device, and an electronic device. The negative electrode material comprises porous silicon carbon particles. Each porous silicon carbon particle comprises a porous carbon matrix, a first silicon carbide layer located on inner wall surfaces of pores of the porous carbon matrix, and a first silicon particle layer located on the side surface of the first silicon carbide layer facing away from the inner wall surfaces. The porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by means of Si-C covalent bonds. The negative electrode material of the present application can enhance the binding force between silicon particles and a porous carbon matrix and avoid falling-off of the silicon particles, so that a stable solid electrolyte interphase (SEI) can be formed between the negative electrode material and an electrolyte, irreversible capacity loss of a first charging and discharging cycle is relatively small, the capacity fading is not obvious, and the cycle performance and safety performance are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode material and preparation method thereof, electrochemical device, and electronic device Technical Field

[0001] The present application relates to the field of batteries, and specifically to a negative electrode material and a preparation method thereof, an electrochemical device, and an electronic device. Background Art

[0002] As the power of electrical devices such as mobile phones, computers, power tools, and electric vehicles continues to increase, people's requirements for the energy density of lithium-ion batteries are also increasing. At present, the energy density of batteries can be increased by adding silicon-based negative electrode materials to the negative electrode active material. However, the high volume expansion rate (about 320%) and high surface activity of silicon-based negative electrode materials after lithium insertion limit the promotion and popularization of such batteries. In addition, the rupture of silicon-based negative electrode materials after expansion will introduce a new electrolyte / active material interface, continuously consume the electrolyte to form a solid electrolyte film (SEI film), which can easily cause rapid decay of battery capacity.

[0003] In order to solve the problem of cyclic stability of silicon-based negative electrode materials, it has been proposed to embed nanosilicon inside porous carbon materials to reduce the expansion of silicon-based negative electrode materials and the accompanying side reactions. In this type of structure, the pores of the carbon material can provide a buffer space for the expansion of nanosilicon, and the skeleton of the carbon material can isolate the nanosilicon from the electrolyte, thereby avoiding the occurrence of side reactions. However, nanosilicon is bound to the carbon surface by van der Waals forces inside the porous carbon, and the interaction between the two is weak. During charging and discharging, the volume of nanosilicon expands and contracts. After multiple cycles, the silicon particles will fall off the carbon surface and deteriorate the cyclic stability performance of the silicon-based negative electrode material.

[0004] Therefore, there is an urgent need to find silicon-based negative electrode materials that can achieve stable cycling.

[0005] Summary of the Invention

[0006] In response to the deficiencies of the prior art, the present application provides a negative electrode material and a preparation method thereof, an electrochemical device, and an electronic device.

[0007] The first aspect of the present application provides a negative electrode material, including porous silicon carbon particles, the porous silicon carbon particles including a porous carbon matrix, a first silicon carbide layer located on the inner wall surface of the pores of the porous carbon matrix, and a first silicon particle layer located on the side surface of the first silicon carbide layer away from the inner wall surface, the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds.

[0008] Optionally, the porous silicon-carbon particles satisfy at least one of the following conditions: (a) the mass fraction of silicon element is 32 wt% to 60 wt% based on the weight of the porous silicon-carbon particles; (b) in the X-ray diffraction pattern of the porous silicon-carbon particles, the peak intensity I1 of the diffraction peak of silicon carbide at 2θ of 35.6°±0.5° and the peak intensity I2 of the diffraction peak of silicon at 2θ of 28.5°±0.5° have a mathematical relationship: 0.025 <I1 / I2<0.47。

[0009] Optionally, the porous silicon carbon particles further satisfy at least one of the following conditions: (c) the pore volume of the porous carbon matrix is ​​0.6 cm 3 / g to 1.1cm 3 / g; (d) the volume proportion of micropores in the pores of the porous carbon matrix is ​​greater than or equal to 70%, and the micropores are pores with a pore diameter of less than 2 nm.

[0010] Optionally, the porous silicon carbon particles further satisfy at least one of the following conditions: (e) the volume distribution of the porous silicon carbon particles satisfies Dv50 of 5 μm to 8 μm and Dv99 of 15 μm to 20 μm; the number distribution of the porous silicon carbon particles satisfies Dn10 of 0.5 μm to 1 μm; (f) the specific surface area of ​​the porous silicon carbon particles is 0.5 m 2 / g to 12m 2 / g.

[0011] Optionally, the porous silicon carbon particles also meet at least one of the following conditions: (g) the porous silicon carbon particles also include a second silicon carbide layer located on the outer surface of the porous silicon carbon, and a second silicon particle layer located on the side surface of the second silicon carbide layer away from the outer surface, and the porous carbon matrix, the second silicon carbide layer and the second silicon particle layer are connected by Si-C covalent bonds; (h) the porous silicon carbon particles also include a carbon particle coating layer, the carbon particle coating layer covers the second silicon carbide layer and the second silicon particle layer located on the side surface of the second silicon carbide layer away from the outer surface; (i) the thickness of the carbon particle coating layer is 2nm to 20nm; (j) based on the weight of the porous silicon carbon particles, the mass fraction of the carbon particle coating layer is 1.3wt% to 3.2wt%.

[0012] A second aspect of the present application provides an electrochemical device, which includes the aforementioned negative electrode material.

[0013] Optionally, the negative electrode material satisfies at least one of the following conditions: (k) the compaction density of the negative electrode material is 0.85 g / cm 3 Up to 1.15g / cm 3 ; (l) The initial porosity of the negative electrode material is 24.7% to 26.1%; (m) The porosity of the negative electrode material after 500 cycles is 26.4% to 34.5%.

[0014] A third aspect of the present application provides an electronic device comprising the aforementioned electrochemical device.

[0015] The fourth aspect of the present application provides a method for preparing a negative electrode material, which is used to form the aforementioned negative electrode material, comprising the following steps: Step 1, providing a porous carbon matrix, and forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix; Step 2, forming a first silicon particle layer on the surface of the first silicon carbide layer facing away from the porous carbon matrix, and the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds.

[0016] Optionally, in step 1, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix includes the following steps: step a, adding the porous carbon matrix into a fluidized bed, introducing a protective gas to make the porous carbon matrix reach a fluidized state, heating the fluidized bed to a pretreatment temperature, and then introducing a first silicon source gas to thermally decompose the first silicon source gas to generate silicon particles that are deposited on the inner wall surface of the pores of the porous carbon matrix to form silicon particles; step b, performing a first heat treatment on the porous carbon matrix and the silicon particles to cause the silicon particles to react with the porous carbon matrix to generate silicon carbide, and forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix.

[0017] Optionally, in step a, the pretreatment temperature is 450°C to 500°C; the protective gas includes nitrogen, and the flow rate of the protective gas is 5L / min to 20L / min; the first silicon source gas includes at least one of monosilane, disilane, and trisilane, and the flow rate of the first silicon source gas is 1L / min to 5L / min.

[0018] Optionally, in step a, the time for introducing the first silicon source gas is 1 min to 10 min; in step b, the temperature of the first heat treatment is 550° C. to 1000° C., and the time is 10 min to 2 h.

[0019] Optionally, in step a, the time for introducing the first silicon source gas is 60 min to 300 min; in step b, the temperature of the first heat treatment is 550° C. to 650° C., and the time is 10 min to 2 h.

[0020] Optionally, in step 1, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix includes the following steps: step c, immersing the porous carbon matrix in a silicon-containing solution so that the porous carbon matrix absorbs the silicon-containing solution, and then drying the adsorbed porous carbon matrix to remove the solvent. After the drying treatment, the porous carbon matrix is ​​calcined to form a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix.

[0021] Optionally, the solute of the silicon-containing solution includes silicon-containing molecules soluble in organic solvents such as dimethyldimethoxysilane, methyltrimethoxysilane, tetramethoxysilane, and methyltriethoxysilane. The solvent of the silicon-containing solution includes organic solvents such as ethanol, methanol, isopropanol, acetone, and tetrahydrofuran. The soaking time is 2 hours to 10 hours, the calcination treatment temperature is 700°C to 1200°C, and the calcination time is 1 hour to 3 hours.

[0022] Optionally, step 2 includes the following steps: placing the porous carbon matrix treated in step 1 in a fluidized bed, heating the fluidized bed to a post-processing temperature, introducing a second silicon source gas, and causing the second silicon source gas to thermally decompose to generate silicon particles that are deposited on the surface of the first silicon carbide layer facing away from the porous carbon matrix, thereby forming a first silicon particle layer.

[0023] Optionally, the post-processing temperature is 450°C to 500°C, the flow rate of the second silicon source gas is 1L / min to 5L / min, the time for introducing the second silicon source gas is 20min to 360min, and the second silicon source gas includes at least one of monosilane, disilane, and trisilane.

[0024] Optionally, step 1 further includes forming a second silicon carbide layer on the outer surface of the porous carbon substrate, the second silicon carbide layer being formed simultaneously with the first silicon carbide layer based on the same method; step 2 further includes forming a second silicon particle layer on the surface of the second silicon carbide layer facing away from the porous carbon substrate, the first silicon particle layer and the second silicon particle layer being formed simultaneously based on the same method. The preparation method further includes: step 3, forming a carbon particle coating layer, the carbon particle coating layer covering the second silicon carbide layer and the second silicon particle layer. The step of forming the carbon particle coating layer includes: after step 2, heating the fluidized bed to a temperature of 500°C to 650°C, introducing a carbon source gas, causing the carbon source gas to thermally decompose to generate carbon particles that are deposited on the second silicon carbide layer and the second silicon particle layer facing away from the porous carbon substrate; the flow rate of the carbon source gas is 0.5L / min to 6L / min, and the time for introducing the carbon source gas is 60min to 360min; the carbon source gas includes at least one of acetylene, ethylene, propylene, propane, and methane.

[0025] The technical solution of this application has the following beneficial effects:

[0026] The negative electrode material of the present application forms a first silicon carbide layer and a first silicon particle layer in sequence on the inner wall surface of the pores of the porous carbon matrix, and the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds, so that the porous carbon matrix can provide a space for the expansion of the silicon particles and limit the volume of the silicon particles to avoid excessive expansion of the silicon particles. In addition, since the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds, the first silicon carbide layer and the first silicon particle layer can be prevented from falling off from the pores of the porous carbon matrix, thereby forming a stable structure. Therefore, a relatively stable solid electrolyte interface (SEI) can be formed between the negative electrode material of the present application and the electrolyte, the irreversible capacity loss of the first cycle charge and discharge is small, the capacity decay is not obvious, and the cycle performance and safety performance are significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] FIG1 schematically shows an X-ray diffraction pattern of the negative electrode material of the present application. DETAILED DESCRIPTION

[0028] The present application will be further described below in conjunction with specific embodiments. It should be understood that these specific embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.

[0029] 1. Anode Materials

[0030] One or more embodiments of the present application provide a negative electrode material, including porous silicon carbon particles, the porous silicon carbon particles including a porous carbon matrix, a first silicon carbide layer located on the inner wall surface of the pores of the porous carbon matrix, and a first silicon particle layer located on the side surface of the first silicon carbide layer away from the inner wall surface, the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds.

[0031] The negative electrode material of the present application forms a first silicon carbide layer and a first silicon particle layer in sequence on the inner wall surface of the pores of the porous carbon matrix, and the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds, so that the porous carbon matrix can provide a space for the expansion of the silicon particles and limit the volume of the silicon particles to avoid excessive expansion of the silicon particles. In addition, since the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds, the first silicon carbide layer and the first silicon particle layer can be prevented from falling off from the pores of the porous carbon matrix, thereby forming a stable structure. Therefore, a relatively stable solid electrolyte interface (SEI) can be formed between the negative electrode material of the present application and the electrolyte, the irreversible capacity loss of the first cycle charge and discharge is small, the capacity decay is not obvious, and the cycle performance and safety performance are significantly improved.

[0032] In some embodiments, the silicon particles of the first silicon particle layer are amorphous silicon. It is understood that amorphous silicon has no directional selectivity when inserting lithium, and the amount of lithium inserted at different angles is the same. The stress during expansion is uniform, and the particles will not break.

[0033] In some embodiments, the mass fraction of silicon is 32 wt % to 60 wt % based on the weight of the porous silicon-carbon particles. For example, the mass fraction of silicon is 32 wt %, 34 wt %, 36 wt %, 35 wt %, 38 wt %, 40 wt %, 42 wt %, 45 wt %, 46 wt %, 48 wt %, 50 wt %, 52 wt %, 54 wt %, 55 wt %, 56 wt %, 58 wt %, 60 wt %, or a range consisting of any two of the foregoing values ​​based on the weight of the porous silicon-carbon particles.

[0034] It is understandable that if the silicon content is too low, the improvement of the negative electrode material will not be obvious, while if the silicon content is too high, some silicon elements will easily fail to be fixed and easily fall off from the porous carbon matrix, resulting in structural instability of the negative electrode material. It is also possible to react violently with the electrolyte, causing significant volume expansion, which in turn leads to a large irreversible capacity loss in the first cycle of charge and discharge of the lithium-ion battery, rapid capacity decay, and poor cycle performance. Controlling the silicon content within the above range can not only ensure that the negative electrode material has excellent specific capacity, but also improve the first efficiency, cycle performance and safety performance of the lithium-ion battery.

[0035] 1 , in some embodiments, in the X-ray diffraction pattern of the porous silicon carbon particles, the peak intensity I1 of the diffraction peak of silicon carbide at 2θ of 35.6°±0.5° and the peak intensity I2 of the diffraction peak of silicon at 2θ of 28.5°±0.5° have a mathematical relationship: 0.025 <I1 / I2<0.47。

[0036] It can be understood that in the X-ray diffraction pattern of the porous silicon-carbon particles, there is an obvious characteristic peak of the (111) crystal plane of silicon carbide at 35.6°±0.5°, which proves that silicon carbide is formed in the porous silicon-carbon particles; and there is an obvious characteristic peak of the (111) crystal plane of silicon at 28.5°±0.5°, which proves that silicon element also exists in the porous silicon-carbon particles. In addition, the ratio of the diffraction peak intensity of silicon carbide to the diffraction peak intensity of silicon can reflect the relative content of the two in the porous silicon-carbon particles. When the relative content of silicon carbide is too high, the irreversible lithium insertion behavior of the silicon carbide material will cause the specific capacity and initial efficiency of the lithium-ion battery to decrease. When the relative content of silicon carbide is too low, it is insufficient to fully fix the first silicon particle layer, causing the silicon particles in the first silicon particle layer to easily fall off from the pores of the porous carbon matrix. Due to the high expansion rate and strong surface activity of the silicon particles, the reaction between the negative electrode material and the electrode liquid is intensified, the lithium-ion battery becomes thicker, and the power performance and cycle performance deteriorate, resulting in the risk of expansion and even explosion. The ratio of the diffraction peak intensity of silicon carbide to the diffraction peak intensity of silicon within the above range is conducive to improving the overall performance of the ion battery.

[0037] Specifically, referring to Figure 1, in the X-ray diffraction pattern of the porous silicon-carbon particles, obvious diffraction peaks can be observed at 60°±0.5° (corresponding to the characteristic peak of the (220) crystal plane of silicon carbide) and 71.8°±0.5° (corresponding to the characteristic peak of the (311) crystal plane of silicon carbide).

[0038] In some embodiments, the pore volume of the porous carbon matrix is ​​0.6 cm 3 / g to 1.1cm 3 / g. For example, the pore volume of the porous carbon matrix is ​​0.6 cm 3 / g, 0.7cm 3 / g, 0.8cm 3 / g, 0.9cm 3 / g, 1.0cm 3 / g, 1.1cm 3 / g or a range consisting of any two of the above values.

[0039] In some embodiments, the volume proportion of micropores in the pores of the porous carbon matrix is ​​greater than or equal to 70%, and the micropores are pores with a pore diameter less than 2 nm.

[0040] In some embodiments, the volume distribution of the porous silicon-carbon particles satisfies Dv50 of 5 μm to 8 μm and Dv99 of 15 μm to 20 μm; the number distribution of the porous silicon-carbon particles satisfies Dn10 of 0.5 μm to 1 μm. For example, Dv50 is 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, or a range consisting of any two of the above values; Dv99 is 15 μm, 15.5 μm, 16 μm, 16.5 μm, 17 μm, 17.5 μm, 18 μm, 18.5 μm, 19 μm, 19.5 μm, 20 μm, or a range consisting of any two of the above values; and Dn10 is 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, or a range consisting of any two of the above values.

[0041] In some embodiments, the specific surface area of ​​the porous silicon carbon particles is 0.5 m 2 / g to 12m 2 / g. For example, the specific surface area of ​​the porous carbon particles is 0.5m 2 / g、1m 2 / g, 2m 2 / g、3m 2 / g、4m 2 / g、5m 2 / g、6m 2 / g、7m 2 / g、8m 2 / g、9m 2 / g、10m 2 / g、11m 2 / g、12m 2 / g or a range consisting of any two of the above values.

[0042] In some embodiments, the porous silicon carbon particles also include a second silicon carbide layer located on the outer surface of the porous silicon carbon, and a second silicon particle layer located on the side surface of the second silicon carbide layer facing away from the outer surface. The porous carbon matrix, the second silicon carbide layer, and the second silicon particle layer are connected by Si-C covalent bonds.

[0043] It can be understood that the second silicon carbide layer, the second silicon particle layer and the connection relationship between the two and the porous carbon particles can achieve the same effect as the aforementioned first silicon carbide layer, the first silicon particle layer and the connection relationship between the two and the porous carbon particles, and will not be repeated here.

[0044] In some embodiments, the porous silicon carbon particles further include a carbon particle coating layer, which covers the second silicon carbide layer and the second silicon particle layer located on a surface of the second silicon carbide layer facing away from the outer surface.

[0045] It can be understood that the carbon particle layer has a lithium ion conduction function, and the silicon particles in the second silicon particle layer can accept lithium ions that pass through the carbon coating layer to form a lithium-silicon alloy, thereby increasing the specific capacity.

[0046] In some embodiments, the carbon particles in the carbon particle coating layer are amorphous carbon. It is understood that amorphous carbon is conducive to forming a complete coating layer.

[0047] In some embodiments, the carbon particle coating layer has a thickness of 2 nm to 20 nm. Exemplarily, the carbon particle coating layer has a thickness of 2 nm, 4 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, or a range consisting of any two of the foregoing values.

[0048] In some embodiments, the mass fraction of carbon is 40 wt % to 68 wt % based on the weight of the porous silicon-carbon particles. For example, the mass fraction of carbon is 40 wt %, 42 wt %, 44 wt %, 46 wt %, 48 wt %, 50 wt %, 52 wt %, 54 wt %, 56 wt %, 58 wt %, 60 wt %, 62 wt %, 64 wt %, 66 wt %, 68 wt %, or a range consisting of any two of the foregoing values ​​based on the weight of the porous silicon-carbon particles.

[0049] In some embodiments, the mass fraction of the carbon particle coating layer is 1.3 wt % to 3.2 wt % based on the weight of the porous silicon-carbon particles. For example, the mass fraction of the carbon particle coating layer is 1.3 wt %, 1.4 wt %, 1.6 wt %, 1.8 wt %, 2.0 wt %, 2.2 wt %, 2.4 wt %, 2.6 wt %, 2.8 wt %, 3.0 wt %, 3.2 wt %, or a range consisting of any two of the foregoing values, based on the weight of the porous silicon-carbon particles.

[0050] 2. Preparation Method of Anode Materials

[0051] One or more embodiments of the present application provide a method for preparing a negative electrode material, for forming the aforementioned negative electrode material, comprising the following steps:

[0052] Step 1: providing a porous carbon substrate, and forming a first silicon carbide layer on the inner wall surfaces of the pores of the porous carbon substrate;

[0053] In step 2, a first silicon particle layer is formed on the surface of the first silicon carbide layer facing away from the porous carbon substrate. The porous carbon substrate, the first silicon carbide layer and the first silicon particle layer are connected via Si-C covalent bonds.

[0054] In some embodiments, in step 1, forming a first silicon carbide layer on the inner wall surfaces of the pores of the porous carbon matrix comprises the following steps:

[0055] Step a, adding a porous carbon substrate to a fluidized bed, introducing a protective gas to fluidize the porous carbon substrate, heating the fluidized bed to a pretreatment temperature, and then introducing a first silicon source gas to pyrolyze the first silicon source gas to generate silicon particles that are deposited on the inner wall surfaces of the pores of the porous carbon substrate to form silicon particles;

[0056] Step b: performing a first heat treatment on the porous carbon matrix and the silicon particles to react with the porous carbon matrix to generate silicon carbide, and forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix.

[0057] In some embodiments, in step a, the pretreatment temperature is 450°C to 500°C; the protective gas includes nitrogen, and the flow rate of the protective gas is 5L / min to 20L / min; the first silicon source gas includes at least one of monosilane, disilane, and trisilane, and the flow rate of the first silicon source gas is 1L / min to 5L / min.

[0058] In some embodiments, in step a, the first silicon source gas is introduced for 1 to 10 minutes; in step b, the first heat treatment is performed at a temperature of 550° C. to 1000° C. for 10 to 2 hours.

[0059] In some embodiments, in step a, the first silicon source gas is introduced for 60 min to 300 min; in step b, the first heat treatment is performed at a temperature of 550° C. to 650° C. for 10 min to 2 h.

[0060] In some embodiments, in step 1, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix includes the following steps: step c, immersing the porous carbon matrix in a silicon-containing solution so that the porous carbon matrix absorbs the silicon-containing solution, and then drying the adsorbed porous carbon matrix to remove the solvent. After the drying treatment, the porous carbon matrix is ​​calcined to form a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix.

[0061] In some embodiments, the solute of the silicon-containing solution includes but is not limited to silicon-containing molecules soluble in organic solvents such as dimethyldimethoxysilane, methyltrimethoxysilane, tetramethoxysilane, and methyltriethoxysilane. The solvent of the silicon-containing solution includes organic solvents such as ethanol, methanol, isopropanol, acetone, and tetrahydrofuran. The soaking time is 2 hours to 10 hours, the calcination temperature is 700°C to 1200°C, and the calcination time is 1 hour to 3 hours.

[0062] In some embodiments, step 2 includes the following steps: placing the porous carbon matrix treated in step 1 in a fluidized bed, and heating the fluidized bed to a post-processing temperature, introducing a second silicon source gas, and causing the second silicon source gas to pyrolyze to generate silicon particles that are deposited on the surface of the first silicon carbide layer facing away from the porous carbon matrix, thereby forming a first silicon particle layer.

[0063] In some embodiments, the post-processing temperature is 450°C to 500°C, the flow rate of the second silicon source gas is 1L / min to 5L / min, the time for introducing the second silicon source gas is 20min to 360min, and the second silicon source gas includes at least one of monosilane, disilane, and trisilane.

[0064] In some embodiments, step 1 further includes forming a second silicon carbide layer on the outer surface of the porous carbon substrate, the second silicon carbide layer being formed simultaneously with the first silicon carbide layer using the same method; step 2 further includes forming a second silicon particle layer on the surface of the second silicon carbide layer facing away from the porous carbon substrate, the first silicon particle layer and the second silicon particle layer being formed simultaneously using the same method. The preparation method further includes step 3, forming a carbon particle coating layer, the carbon particle coating layer covering the second silicon carbide layer and the second silicon particle layer.

[0065] In some embodiments, the step of forming a carbon particle coating layer includes: after step 2, heating the temperature of the fluidized bed to 500°C to 650°C, introducing a carbon source gas, and causing the carbon source gas to thermally decompose to generate carbon particles that are deposited on the second silicon carbide layer and the second silicon particle layer on the side away from the porous carbon matrix; the flow rate of the carbon source gas is 0.5L / min to 6L / min, and the time for introducing the carbon source gas is 60min to 360min; the carbon source gas includes at least one of acetylene, ethylene, propylene, propane, and methane. Specifically, the thermal decomposition reaction equation is C x H y =xC+y / 2H2.

[0066] In a specific example of the present invention, a porous carbon matrix is ​​added to a fluidized bed, and nitrogen gas is introduced at a flow rate of 5 L / min to 20 L / min to allow the porous carbon matrix to reach a fluidized state, and the fluidized bed is heated to 450°C to 500°C. After the temperature stabilizes, a first silicon source gas is introduced for a time period of 1 min to 10 min. The first silicon source gas is pyrolyzed to generate silicon particles, which are deposited on the inner wall surface of the pores of the porous carbon matrix or the outer surface of the porous carbon matrix. The temperature of the fluidized bed is then raised to 550°C to 1000°C for a time period of 10 min to 2 h, so that the silicon particles react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and / or forming a second silicon carbide layer on the outer surface of the porous carbon matrix. The temperature of the fluidized bed is lowered to 450°C to 500°C, and a second silicon source gas is introduced at a flow rate of 1 L / min to 5 L / min. The second silicon source gas is introduced for 20 min to 360 min. The second silicon source gas is pyrolyzed to generate silicon particles, which are deposited on the surface of the second silicon carbide. Subsequently, the temperature of the fluidized bed is heated to 500°C to 650°C, and a carbon source gas is introduced. The carbon source gas is pyrolyzed to generate carbon particles, which are deposited on the second silicon carbide layer and the surface of the second silicon particle layer facing away from the porous carbon matrix. The flow rate of the carbon source gas is 0.5 L / min to 6 L / min. The carbon source gas is introduced for 60 min to 360 min to form a carbon particle coating layer. The carbon particle coating layer covers the second silicon carbide and the silicon particles located on the surface of the second silicon carbide.

[0067] In another specific example of the present invention, a porous carbon matrix is ​​added to a fluidized bed, and nitrogen gas is introduced at a flow rate of 5 L / min to 20 L / min to allow the porous carbon matrix to reach a fluidized state, and the fluidized bed is heated to 450°C to 500°C. After the temperature stabilizes, a first silicon source gas is introduced for a time period of 1 min to 10 min. The first silicon source gas is pyrolyzed to generate silicon particles, which are deposited on the inner wall surface of the pores of the porous carbon matrix or the outer surface of the porous carbon matrix. The temperature of the fluidized bed is then raised to 550°C to 650°C for a time period of 10 min to 2 h, so that the silicon particles react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and / or forming a second silicon carbide layer on the outer surface of the porous carbon matrix. The temperature of the fluidized bed is lowered to 450°C to 500°C, and a second silicon source gas is introduced at a flow rate of 1 L / min to 5 L / min. The second silicon source gas is introduced for 20 min to 360 min. The second silicon source gas is pyrolyzed to generate silicon particles, which are deposited on the surface of the second silicon carbide. Subsequently, the temperature of the fluidized bed is heated to 500°C to 650°C, and a carbon source gas is introduced. The carbon source gas is pyrolyzed to generate carbon particles, which are deposited on the second silicon carbide layer and the surface of the second silicon particle layer facing away from the porous carbon matrix. The flow rate of the carbon source gas is 0.5 L / min to 6 L / min. The carbon source gas is introduced for 60 min to 360 min to form a carbon particle coating layer. The carbon particle coating layer covers the second silicon carbide and the silicon particles located on the surface of the second silicon carbide.

[0068] In another specific example of the present application, the porous carbon matrix is ​​immersed in a silicon-containing solution so that the porous carbon matrix absorbs the silicon-containing solution, and the immersion time is 2 hours to 10 hours. The adsorbed porous carbon matrix is ​​then dried to remove the solvent. After the drying treatment, the porous carbon matrix is ​​calcined to form a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and / or a second silicon carbide layer is formed on the outer surface of the porous carbon matrix. The calcination temperature is 700°C to 1200°C, and the calcination time is 1 hour to 3 hours. Afterwards, it is cooled to room temperature and the treated porous carbon matrix is ​​placed in a fluidized bed, the temperature of the fluidized bed is heated to 500°C to 650°C, and a carbon source gas is introduced to thermally decompose the carbon source gas to generate carbon particles which are deposited on the surface of the second silicon carbide layer and the second silicon particle layer facing away from the porous carbon matrix. The flow rate of the carbon source gas is 0.5L / min to 6L / min, and the time for introducing the carbon source gas is 60min to 360min to form a carbon particle coating layer, which covers the second silicon carbide and the silicon particles located on the surface of the second silicon carbide.

[0069] 3. Electrochemical Device

[0070] One or more embodiments of the present invention further provide an electrochemical device comprising the negative electrode material of the aforementioned embodiment.

[0071] In some embodiments, the compacted density of the negative electrode material is 0.85 g / cm 3 Up to 1.15g / cm 3 For example, the compaction density of the negative electrode material is 0.85 g / cm 3 , 0.9g / cm 3 , 0.95g / cm 3 , 1.0g / cm 3 , 1.05g / cm 3 , 1.1g / cm 3 , 1.15g / cm 3 Or a range consisting of any two of the above values.

[0072] In some embodiments, the initial porosity of the negative electrode material is 24.7% to 26.1%. Exemplarily, the initial porosity of the negative electrode material is 24.7%, 24.8%, 25%, 25.2%, 25.4%, 25.6%, 25.8%, 26%, 26.1%, or a range consisting of any two of the above values.

[0073] In some embodiments, the porosity of the negative electrode material after 500 cycles is 26.4% to 34.5%. For example, the porosity of the negative electrode material after 500 cycles is 26.4%, 26.5%, 26.6%, 26.8%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5%, or a range consisting of any two of the above values.

[0074] It is understandable that the expansion of the battery cell is partly contributed by the porosity of the negative electrode, and the porosity is caused by the repeated expansion and contraction of the negative electrode material in the negative electrode. Due to the differences in the properties of silicon, different silicon-doped negative electrode materials have different porosity characteristics.

[0075] According to some embodiments of the present application, the electrochemical device of the present application includes, but is not limited to, all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In some embodiments, the electrochemical device is a lithium secondary battery. In some embodiments, the lithium secondary battery includes, but is not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.

[0076] In a specific example of the present invention, the electrochemical device is a lithium-ion battery. The present application does not impose any specific restrictions on the type of lithium-ion battery, and it can be any type of lithium-ion battery, such as button-type, cylindrical, soft-pack lithium-ion battery, etc.

[0077] The preparation process of an electrochemical device is well known to those skilled in the art and is not particularly limited in this application. For example, it may include, but is not limited to, the following steps: stacking the positive electrode sheet, separator, and negative electrode sheet in sequence, and winding, folding, and other operations as needed to obtain a wound electrode assembly, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag, and sealing the packaging bag to obtain the electrochemical device; or stacking the positive electrode sheet, separator, and negative electrode sheet in sequence, and then securing the four corners of the entire stack with tape to obtain a stacked electrode assembly, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag, and sealing the packaging bag to obtain the electrochemical device. In addition, as needed, overcurrent protection elements, guide plates, etc. may be placed in the packaging bag to prevent pressure buildup and overcharging and discharging within the electrochemical device. This application does not limit the packaging bag, and those skilled in the art may select one based on actual needs, as long as it achieves the objectives of this application. For example, an aluminum-plastic film packaging bag may be used.

[0078] 4. Electronic Devices

[0079] One or more embodiments of the present invention further provide an electronic device. The electronic device of the present application may be any device using the electrochemical device of the aforementioned embodiments.

[0080] In some embodiments, the electronic devices of the present application include but are not limited to: laptop computers, pen-type computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries or lithium-ion capacitors, etc.

[0081] Hereinafter, the present application will be described in more detail with reference to Examples and Comparative Examples. However, the present application is not limited to these Examples unless departing from the gist of the present application.

[0082] Examples and Comparative Examples

[0083] Example 1

[0084] <Preparation of negative electrode sheet>

[0085] 1. Formation of porous silicon carbon particles

[0086] 500g of porous carbon matrix was added to a fluidized bed, and nitrogen was introduced at a rate of 10L / min to fluidize the porous carbon matrix. The fluidized bed was then heated to 500°C. After the temperature stabilized, monosilane was introduced at a rate of 3L / min for 6 minutes. The monosilane pyrolyzed to generate silicon particles, which were deposited on the inner wall surfaces of the pores of the porous carbon matrix or on the outer surface of the porous carbon matrix. The fluidized bed temperature was then raised to 1000°C and maintained for 1 hour to allow the silicon particles to react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surfaces of the pores of the porous carbon matrix and a second silicon carbide layer on the outer surface of the porous carbon matrix. The fluidized bed temperature was lowered to 500°C, and monosilane was continued to be introduced at a rate of 3L / min for 105 minutes. The monosilane pyrolyzed to generate silicon particles, which were deposited on the surface of the second silicon carbide. Subsequently, acetylene gas was introduced at a rate of 5 L / min for 3 hours to form a carbon particle coating layer, which covered the second silicon carbide and the silicon particles located on the surface of the second silicon carbide.

[0087] 2. Forming the negative electrode sheet

[0088] An active material with a gram capacity of 420 mAh / g (porous silicon-carbon particles and graphite mixed in a mass ratio of 5:95) was mixed with carbon nanotubes, lithium carboxymethyl cellulose, and lithium polyacrylate in a mass ratio of 97.4:0.2:0.4:2. An appropriate amount of deionized water was added as a solvent, and a negative electrode slurry with a solid content of 46 wt% was obtained using a vacuum mixer. The negative electrode slurry was evenly coated on one surface of the negative electrode current collector copper foil, and the copper foil was dried at 80°C to obtain a negative electrode sheet with a single-sided negative electrode material layer and a coating thickness of 40 μm. The above steps were repeated on the other surface of the copper foil to obtain a negative electrode sheet coated on both sides with a negative electrode material layer. After cold pressing, cutting, and slitting, a negative electrode sheet with a size of 661 mm x 78 mm was obtained.

[0089] <Preparation of positive electrode sheet>

[0090] The positive electrode active material LiCoO2, conductive carbon black, and binder polyvinylidene fluoride were mixed in a mass ratio of 96.7:1.7:1.6. N-methylpyrrolidone (NMP) was added and a vacuum mixer was used to produce a positive electrode slurry with a solids content of 76 wt%. The positive electrode slurry was evenly coated on one surface of a 9 μm thick positive electrode current collector aluminum foil. The foil was then dried at 120°C to produce a positive electrode sheet with a single-sided positive electrode material layer and a coating thickness of 45 μm. The above steps were repeated on the other surface of the aluminum foil to obtain a positive electrode sheet coated on both sides with a positive electrode material layer. After cold pressing, cutting, and slitting, the resulting positive electrode sheet had a size of 661 mm x 76.5 mm.

[0091] <Preparation of Electrolyte>

[0092] In an argon atmosphere glove box with a water content of less than 10 ppm, FEC, EC, PC, EMC, and DEC were mixed in a mass ratio of 5:10:15:20:50 to obtain an organic solvent. LiPF6, a lithium salt, was then added to the organic solvent to obtain an electrolyte solution. The mass percentage of the lithium salt was 12.5%.

[0093] <Isolation Film>

[0094] A porous polyethylene film with a thickness of 10 μm was used.

[0095] <Preparation of lithium-ion batteries>

[0096] The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator positioned between the positive and negative electrodes to provide isolation, and wound to form an electrode assembly. The electrode assembly is then placed in an aluminum-plastic film packaging bag, dried, and then injected with electrolyte. The lithium-ion battery is then produced through vacuum packaging, resting, formation, degassing, and trimming.

[0097] Example 2

[0098] The only difference between Example 2 and Example 1 is that the fluidized bed is heated to 500° C., and after the temperature stabilizes, monosilane is introduced at 3 L / min for 4 minutes. The remaining steps are the same as in Example 1.

[0099] Example 3

[0100] The only difference between Example 3 and Example 1 is that the fluidized bed is heated to 500° C., and after the temperature stabilizes, monosilane is introduced at 3 L / min for 2 minutes. The remaining steps are the same as in Example 1.

[0101] Example 4

[0102] The difference between Example 4 and Example 1 is that the fluidized bed is heated to 500°C, and after the temperature stabilizes, 3L / min of monosilane is introduced for 160 minutes, and the monosilane is thermally decomposed to generate silicon particles, which are deposited on the inner wall surface of the pores of the porous carbon matrix or the outer surface of the porous carbon matrix; then the fluidized bed temperature is raised to 550°C and kept warm for 1 hour to allow some of the deposited silicon particles to react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and a second silicon carbide layer on the outer surface of the porous carbon matrix.

[0103] The remaining steps are the same as those in Example 1.

[0104] Example 5

[0105] The difference between Example 5 and Example 4 is that the fluidized bed temperature is raised to 575°C and kept warm for 1 hour, so that some of the deposited silicon particles react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and a second silicon carbide layer on the outer surface of the porous carbon matrix.

[0106] The remaining steps are the same as those in Example 4.

[0107] Example 6

[0108] The difference between Example 6 and Example 4 is that the fluidized bed temperature is raised to 600°C and kept warm for 1 hour to allow some of the deposited silicon particles to react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and a second silicon carbide layer on the outer surface of the porous carbon matrix.

[0109] The remaining steps are the same as those in Example 4.

[0110] Example 7

[0111] At room temperature, 1000g of porous carbon matrix was immersed in 5L of 1% dimethyldimethoxysilane ethanol solution for 5h. The porous carbon matrix adsorbed with silicon molecules was filtered and dried in a vacuum oven at 60°C for 24h. The powder was then calcined at 1000°C for 2h in a box furnace filled with argon atmosphere. After cooling, a porous silicon-carbon granular material with silicon carbide modified porous carbon matrix was obtained. 500g of porous silicon-carbon granular material was added to a fluidized bed, and 10L / min of nitrogen was introduced to achieve a fluidized state. The fluidized bed was heated to 500°C. After the temperature stabilized, 3L / min of monosilane was introduced for 130min. The monosilane was pyrolyzed to generate silicon particles, which were deposited on the inner wall surface of the pores of the porous carbon matrix or the outer surface of the porous carbon matrix. Subsequently, acetylene gas was introduced at a rate of 5 L / min for 3 hours to form a carbon particle coating layer, which covered the second silicon carbide and the silicon particles located on the surface of the second silicon carbide.

[0112] The remaining steps are the same as those in Example 1.

[0113] Example 8

[0114] The only difference between Example 8 and Example 7 is that, when forming the porous silicon-carbon particle material, the volume concentration of the dimethyldimethoxysilane ethanol solution is 2%.

[0115] The remaining steps are the same as those in Example 7.

[0116] Example 9

[0117] The only difference between Example 9 and Example 7 is that, when forming the porous silicon-carbon particle material, the volume concentration of the dimethyldimethoxysilane ethanol solution is 3%.

[0118] The remaining steps are the same as those in Example 7.

[0119] Comparative Example 1

[0120] 500g of porous carbon substrate was added to a fluidized bed. Nitrogen was introduced at a rate of 10 L / min to achieve a fluidized state, and the bed was heated to 500°C. Once the temperature stabilized, monosilane was introduced at a rate of 3 L / min for 130 minutes. The monosilane pyrolyzed to form silicon particles, which deposited on the inner walls of the pores or on the outer surface of the porous carbon substrate. Subsequently, acetylene gas was introduced at a rate of 5 L / min for 3 hours.

[0121] The remaining steps are the same as those in Example 1.

[0122] Comparative Example 2

[0123] Comparative Example 2 differs from Comparative Example 1 in that, after preparing the porous silicon-carbon granules, the resulting porous silicon-carbon granules were immersed in a 2% by mass dispersion of nano-silicon carbide (100 nm in size) in a 0.5% by mass polyacrylic acid. After a period of time, the silicon-carbon powder was filtered and dried to obtain a silicon-carbon powder material with silicon carbide attached to its surface.

[0124] The remaining steps are the same as those in Comparative Example 1.

[0125] Comparative Example 3

[0126] The difference between Comparative Example 3 and Example 1 is that the fluidized bed is heated to 500°C, and after the temperature stabilizes, 3L / min of monosilane is introduced for 20 minutes. The monosilane is pyrolyzed to generate silicon particles, which are deposited on the inner wall surface of the pores of the porous carbon matrix or the outer surface of the porous carbon matrix. The fluidized bed temperature is then raised to 1000°C and maintained for 1 hour to allow the deposited silicon particles to react with the porous carbon matrix to generate silicon carbide, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix, and a second silicon carbide layer on the outer surface of the porous carbon matrix. The fluidized bed temperature is lowered to 500°C, and 3L / min of monosilane is continued to be introduced for 140 minutes. The monosilane is pyrolyzed to generate silicon particles, which are deposited on the surface of the second silicon carbide.

[0127] The remaining steps are the same as those in Example 1.

[0128] Test method:

[0129] Battery cycle test:

[0130] The test temperature was 25°C. The battery was charged at a constant current of 0.7C to 4.50V, then charged at a constant voltage of 0.025C. After standing for 5 minutes, the battery was discharged at 0.5C to 3.0V. The capacity obtained in this step was used as the initial capacity. Cycling tests were performed at 0.7C charge / 0.5C discharge. The capacity at each step was compared to the initial capacity to obtain the capacity decay curve.

[0131] Battery cell full charge expansion rate test:

[0132] Repeat three measurements with a micrometer at the location where the aluminum tab is embedded in the battery cell, and take the average value to determine the cell thickness. Measure the thickness of a fresh cell when it is charged to 3.85V, and use this as the initial thickness. After a specific number of charge and discharge cycles, fully charge the cell to 4.5V and measure its thickness again with a micrometer. Compare this to the initial thickness to determine the cell expansion rate at this point.

[0133] Powder particle size test:

[0134] The particle size distribution of the powder was tested by laser diffraction. A 50ml beaker was taken, 0.2g of sample was added, 2 drops of 1wt% P-40 surfactant were dripped into it, and 20ml of water was added after gentle shaking. The sample dispersion was obtained by ultrasonic dispersion for 5 minutes using an ultrasonic cleaner with a power of 120W. The sample dispersion was tested using MasterSizer 2000 to obtain the Dv50 and Dv99 of the sample. Among them, Dv50 means that the diameter of particles accounting for 50% of the total volume of the sample is greater than this value, and the diameter of particles accounting for another 50% of the total volume is less than this value. Dv99 means that the diameter of particles accounting for 90% of the total sample volume is less than this value. Dn10 means that the diameter of particles accounting for 10% of the total number of sample particles is less than this value.

[0135] Powder silicon content test:

[0136] Weigh 0.1g of sample into a PTFE beaker, add 10mL of nitric acid, and heat to digest. Add another 10mL of nitric acid and repeat the digestion process. After cooling, filter the digestion solution to remove the residue and dilute to 100mL in a volumetric flask. Add the prepared solution to a spray chamber and perform analysis using inductively coupled plasma optical emission spectrometry.

[0137] Powder XRD test:

[0138] Remove the sample holder, glass slide, and angle key used for sample preparation. Place an appropriate amount of powder into the groove of the sample holder. Use the angle key to flatten the sample, then gently press the sample surface with the glass slide to align the powder surface with the sample holder surface. The test radiation source is a Cu target, with a tube voltage of 40 kV, a tube current of 30 mA, a scan speed of 8 degrees / min, and a 2θ range of 10 to 80 degrees.

[0139] Powder Gram Capacity Test:

[0140] The silicon-carbon anode is prepared by mixing silicon-carbon powder, a conductive agent (SP), a binder (SBR), carbon nanotubes (CNTs), and a dispersant (CMC) in a mass ratio of 84:10%:5%:0.4%:0.6%. Deionized water is added to adjust the solids content to 48%. The slurry is mixed evenly and then coated onto copper foil. After drying, cold pressing, and punching, the silicon-carbon anode electrode is obtained. In a glove box with a water and oxygen content of less than 10 ppm, ethyl methyl carbonate (EMC), ethylene carbonate (EC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1. Fluoroethylene carbonate (FEC) is then added at a 10% volume fraction of the mixed solvent. Finally, LiPF6 is added to obtain an electrolyte with a lithium salt concentration of 1 mol / L. In a glove box with a water and oxygen content of less than 10 ppm, the silicon-carbon anode electrode, a metal lithium counter electrode, a PP separator, and the above electrolyte are assembled into a CR2430 button cell. The gram capacity test was conducted at 25°C. After standing for 6 hours, the coin cell was discharged at 0.05C to 5mV. It was then discharged at 50A to 5mV. After standing for 5 minutes, it was again discharged at 10A to 5mV. The cell was then allowed to stand for 5 minutes and then charged to 2.0V at a rate of 0.05C. The initial coulombic efficiency of the silicon-carbon anode material is calculated as: initial charge capacity / initial discharge capacity.

[0141] Negative electrode porosity test:

[0142] The sample used for sample preparation was removed and the negative electrode was punched into 10mm diameter discs. The cycled negative electrode was cleaned with dimethyl carbonate (DMC) and vacuum-dried before punching. The apparent volume V1 of the disc was calculated based on the thickness and diameter. Forty punched discs were taken and the true volume V2 was accurately measured using the Archimedean principle of gas displacement (density = mass / volume) and Bohr's law for small molecular diameter helium under certain conditions (PV = nRT). The porosity of the electrode was calculated using the formula Porosity = (V2 - V1) × V1 × 100%.

[0143] Test of specific surface area of ​​porous silicon carbon particles:

[0144] A 2.0g sample was weighed and placed in a sample tube. The sample tube was then installed in a degassing station and heated to 200°C for 120 minutes. A certain amount of nitrogen was introduced into the sample tube. The equilibrium pressure in the sample tube was controlled to directly measure the adsorption partial pressure, and the adsorption capacity at that partial pressure point was determined from the gas equation of state. During the measurement, the adsorbate gas was gradually added to increase the adsorption equilibrium pressure, ultimately generating an adsorption isotherm. The adsorption equilibrium pressure was then gradually reduced by removing the adsorbate gas, resulting in a desorption isotherm. Barrett-Joyner-Halenda (BJH) theory was used to calculate parameters such as pore size, specific surface area, and pore volume.

[0145] Test of the micropore ratio of porous carbon matrix:

[0146] The adsorption-desorption isotherm test method of the porous carbon matrix is ​​the same as that of the porous silicon-carbon particles. The density functional theory (DFT) method is then used to analyze the total pore volume V1 of the porous carbon matrix and the pore volume V2 of micropores with a pore diameter less than 2 nm. The ratio of V2 / V1 can be used to obtain the micropore ratio of the porous carbon matrix.

[0147] Test of the thickness of the carbon particle coating:

[0148] The thickness of the carbon coating layer on the surface of the material particles was determined by combining high-resolution TEM and corresponding EDS images. Since the carbon particle coating layer does not contain silicon, the carbon layer on the particle surface that does not contain silicon can be considered as the carbon particle coating layer. Five test points were selected and the average value was taken to obtain the thickness of the carbon particle coating layer.

[0149] Test of compaction density of negative electrode materials:

[0150] A 1.0g sample of powdered material was placed in an extrusion die with a diameter of 13mm. The sample was then pressurized using an electronic pressure testing machine. The pressure was controlled at 5t, the displacement rate was 10mm / min, and the hold time was 30s. After the hold, the pressure was released at a displacement rate of 30mm / min. The compacted density of the material was calculated based on the volume of the material after release using the equation ρ = m / V.

[0151] Table 1

[0152] In Examples 1, 2, and 3, different amounts of silicon particles were first introduced into the porous carbon matrix by pyrolysis of silane, and then high-temperature treatment was performed to react the silicon particles with the porous carbon matrix to form silicon carbide. Since the content of silicon particles used to generate silicon carbide in the three examples decreased successively, the content of silicon carbide in the three examples also decreased successively. Compared with Comparative Example 1, in Examples 1 to 3, due to the formation of silicon carbide, silicon carbide was formed in situ at the silicon particle / porous carbon matrix interface, which played a role in connecting the porous carbon matrix and the silicon particles, resulting in a significant improvement in the cycle capacity retention rate of the lithium battery and a significant decrease in the cycle expansion rate.

[0153] In Examples 4, 5, and 6, a large number of silicon particles are first introduced into the porous carbon matrix by pyrolysis of silane, and then silicon carbide is generated under relatively low temperature conditions. Silicon carbide can still be formed in situ at the silicon particle / porous carbon matrix interface, serving to connect the porous carbon matrix and the silicon particles. In addition, as the heat treatment temperature changes, the thickness of the silicon carbide interface layer can be controlled, thereby achieving the purpose of regulating the material properties. Compared with Comparative Example 1, the cycle capacity retention rate of the lithium batteries of Examples 4 to 6 is significantly improved, and the cycle expansion rate is significantly reduced.

[0154] In Examples 7, 8, and 9, organosilane molecules were first adsorbed into a porous carbon matrix, and then high-temperature treatment was performed to convert the organosilane molecules into silicon carbide. The silicon carbide content was adjusted by controlling the concentration of the organosilane molecules. During subsequent silane deposition, the silicon particles formed by pyrolysis were directly adsorbed onto the surface of the silicon carbide rather than the carbon material. Compared to Comparative Example 1, the lithium batteries of Examples 7 to 9 exhibited significantly improved cycle capacity retention and significantly reduced cycle expansion.

[0155] This shows that a silicon carbide layer forms at the interface between the silicon particles and the porous carbon matrix. Silicon carbide can connect the porous carbon matrix and the silicon particles, reducing or even preventing silicon particles from falling off, thereby improving the cycle performance of lithium batteries. In addition, different preparation methods can achieve this effect when forming the silicon carbide layer.

[0156] It can be seen from Table 1 that the value of I1 / I2 decreases as the silicon carbide content decreases. This is because I1 corresponds to the characteristic diffraction peak of silicon carbide, and the intensity of this peak weakens as the silicon carbide content decreases.

[0157] As the silicon carbide content increases, the compaction density of the silicon-carbon material increases. This is because the increase in the amount of silicon carbide in the porous carbon matrix will increase the mass of the same volume of material.

[0158] As the silicon carbide content increases, the material's initial efficiency and gram capacity decrease slightly. This is because silicon carbide has poor ion conductivity and some embedded lithium ions fail to be released in time.

[0159] With the increase of silicon carbide content, the capacity retention rate and expansion rate of the battery cell after 500 cycles tend to improve. This is because the silicon carbide interface layer can prevent the silicon embedded lithium from falling off from the surface of the porous carbon matrix when it is deformed, and silicon carbide has a certain restraining effect on the volume change of silicon particles.

[0160] Comparative Example 1 contains no silicon carbide, and there is no silicon carbide peak at the I1 position, resulting in no I1 / I2 value. Due to the absence of silicon carbide, which has poor ion conductivity, its specific capacity and initial efficiency are slightly higher than those of Examples 7 to 9. However, due to the lack of silicon carbide's bridging and buffering effects, the capacity retention and expansion rate of the battery cell deteriorate to a certain extent.

[0161] The silicon carbide particles introduced in Comparative Example 2 are too large, resulting in an increase in the amount of irreversible lithium ions. In addition, silicon carbide cannot serve as the interface layer between silicon and the porous carbon matrix, which deteriorates the performance of the material and the battery cell to a certain extent.

[0162] Comparative Example 3 introduces 10% silicon carbide. The large amount of silicon carbide deteriorates the ion and electron transport properties of the material, resulting in a significant deterioration in the performance of the material and the battery cell. However, due to the stronger binding effect, the expansion rate of the battery cell is effectively improved.

[0163] Table 2

[0164] Referring to Table 1 and Table 2, since the negative electrode mixed gram capacity is fixed at 420mAh / g, the irreversible lithium insertion behavior of silicon carbide will reduce the gram capacity of the silicon-carbon negative electrode to a certain extent. Therefore, the higher the gram capacity of the material in the embodiment and the comparative example, the lower the mixing ratio of the porous silicon-carbon particles in the negative electrode. Since the density of the porous silicon-carbon particles is lower than that of graphite, the higher the silicon content, the larger the volume of the electrode, which ultimately leads to the phenomenon of higher gram capacity of silicon-carbon and greater porosity of the negative electrode before cycling. By controlling the relative content of silicon carbide and silicon, the relationship between gram capacity and porosity can be achieved, thereby improving the overall performance of lithium-ion batteries.

[0165] Referring to Table 2, the porosity of the negative electrode sheet after cycling increases with the increase in the thickness expansion rate of the battery cell. This is because the expansion of the battery cell thickness is mainly caused by the negative electrode sheet. The increase in the expansion rate will cause the gaps between the particles in the negative electrode coating to become larger. The greater the battery cell expansion rate, the greater the porosity of the negative electrode sheet. The porous silicon-carbon particles of the present application can use the pores of the porous carbon matrix to limit the expansion of silicon particles, thereby alleviating the increase in the porosity of the negative electrode sheet caused by repeated expansion and contraction of the negative electrode material.

[0166] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application, and that these changes, substitutions and modifications also fall within the scope of protection of the present application.

Claims

1. A negative electrode material, characterized in that: The porous silicon-carbon particles include a porous carbon matrix, a first silicon carbide layer located on the inner wall surface of the pores of the porous carbon matrix, and a first silicon particle layer located on the side surface of the first silicon carbide layer away from the inner wall surface, wherein the porous carbon matrix, the first silicon carbide layer and the first silicon particle layer are connected by Si-C covalent bonds.

2. The negative electrode material according to claim 1, characterized in that The porous silicon carbon particles satisfy at least one of the following conditions: (a) based on the weight of the porous silicon-carbon particles, the mass fraction of the silicon element is 32 wt % to 60 wt %; (b) In the X-ray diffraction pattern of the porous silicon-carbon particles, the peak intensity I1 of the diffraction peak of silicon carbide at 2θ of 35.6°±0.5° and the peak intensity I2 of the diffraction peak of silicon at 2θ of 28.5°±0.5° have a mathematical relationship: 0.025 <I1 / I2<0.47。 3. The negative electrode material according to claim 1, characterized in that The porous silicon carbon particles satisfy at least one of the following conditions: (c) The pore volume of the porous carbon matrix is ​​0.6 cm 3 / g to 1.1cm 3 / g; (d) The volume proportion of micropores in the pores of the porous carbon matrix is ​​greater than or equal to 70%, and the micropores are pores with a pore diameter less than 2 nm.

4. The negative electrode material according to claim 1, characterized in that The porous silicon carbon particles also meet at least one of the following conditions: (e) the volume distribution of the porous silicon-carbon particles satisfies Dv50 of 5 μm to 8 μm and Dv99 of 15 μm to 20 μm; the number distribution of the porous silicon-carbon particles satisfies Dn10 of 0.5 μm to 1 μm; (f) The specific surface area of ​​the porous silicon carbon particles is 0.5 m 2 / g to 12m 2 / g.

5. The negative electrode material according to any one of claims 1 to 3, characterized in that The porous silicon carbon particles also meet at least one of the following conditions: (g) the porous silicon carbon particles further include a second silicon carbide layer located on the outer surface of the porous silicon carbon, and a second silicon particle layer located on a surface of the second silicon carbide layer away from the outer surface, and the porous carbon matrix, the second silicon carbide layer and the second silicon particle layer are connected by Si-C covalent bonds; (h) The porous silicon carbon particles further include a carbon particle coating layer, wherein the carbon particle coating layer covers the second carbonized a silicon layer and a second silicon particle layer located on a surface of the second silicon carbide layer facing away from the outer surface; (i) the thickness of the carbon particle coating layer is 2 nm to 20 nm; (j) Based on the weight of the porous silicon carbon particles, the mass fraction of the carbon particle coating layer is 1.3 wt % to 3.2 wt %.

6. An electrochemical device, characterized in that: The electrochemical device comprises the negative electrode material according to any one of claims 1 to 5.

7. The electrochemical device according to claim 6, characterized in that The negative electrode material satisfies at least one of the following conditions: (k) The compaction density of the negative electrode material is 0.85 g / cm 3 Up to 1.15g / cm 3 ; (l) the initial porosity of the negative electrode material is 24.7% to 26.1%; (m) The porosity of the negative electrode material after 500 cycles is 26.4% to 34.5%.

8. An electronic device, characterized in that: An electrochemical device comprising any one of claims 6 or 7.

9. A method for preparing a negative electrode material, characterized in that: The method for forming the negative electrode material according to any one of claims 1 to 5 comprises the following steps: Step 1, providing a porous carbon substrate, and forming a first silicon carbide layer on the inner wall surfaces of the pores of the porous carbon substrate; Step 2: forming a first silicon particle layer on a surface of the first silicon carbide layer facing away from the porous carbon substrate, wherein the porous carbon substrate, the first silicon carbide layer and the first silicon particle layer are connected via Si—C covalent bonds.

10. The method for preparing the negative electrode material according to claim 9, characterized in that: In step 1, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix comprises the following steps: Step a, adding a porous carbon matrix into a fluidized bed, introducing a protective gas to make the porous carbon matrix reach a fluidized state, heating the fluidized bed to a pretreatment temperature, and then introducing a first silicon source gas to thermally decompose the first silicon source gas to generate silicon particles that are deposited on the inner wall surface of the pores of the porous carbon matrix to form silicon particles; Step b: performing a first heat treatment on the porous carbon matrix and the silicon particles, so that the silicon particles react with the porous carbon matrix to generate silicon carbide, and forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix.

11. The method for preparing the negative electrode material according to claim 10, characterized in that: In step a, the pretreatment temperature is 450°C to 500°C; the protective gas includes nitrogen, and the flow rate of the protective gas is 5L / min to 20L / min; the first silicon source gas includes at least one of monosilane, disilane, and trisilane, and the flow rate of the first silicon source gas is 1L / min to 5L / min.

12. The method for preparing the negative electrode material according to claim 10, characterized in that: In step a, the time for introducing the first silicon source gas is 1 min to 10 min; In step b, the temperature of the first heat treatment is 550° C. to 1000° C., and the time is 10 min to 2 h.

13. The method for preparing the negative electrode material according to claim 10, characterized in that: In step a, the time for introducing the first silicon source gas is 60 min to 300 min; In step b, the temperature of the first heat treatment is 550° C. to 650° C., and the time is 10 min to 2 h.

14. The method for preparing the negative electrode material according to claim 9, characterized in that: In step 1, forming a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix comprises the following steps: Step c, immersing the porous carbon matrix in a silicon-containing solution so that the porous carbon matrix absorbs the silicon-containing solution, and then drying the porous carbon matrix after adsorption to remove the solvent. After drying, calcining the porous carbon matrix to form a first silicon carbide layer on the inner wall surface of the pores of the porous carbon matrix.

15. The method for preparing the negative electrode material according to claim 14, characterized in that: The solute of the silicon-containing solution includes silicon-containing molecules soluble in organic solvents such as dimethyldimethoxysilane, methyltrimethoxysilane, tetramethoxysilane, and methyltriethoxysilane. The solvent of the silicon-containing solution includes organic solvents such as ethanol, methanol, isopropanol, acetone, and tetrahydrofuran. The immersion time is 2 hours to 10 hours, the calcination treatment temperature is 700°C to 1200°C, and the calcination time is 1 hour to 3 hours.

16. The method for preparing a negative electrode material according to any one of claims 9 to 15, characterized in that: Step 2 includes the following steps: placing the porous carbon matrix treated in step 1 in a fluidized bed, and heating the fluidized bed to a post-processing temperature, introducing a second silicon source gas, and causing the second silicon source gas to thermally decompose to generate silicon particles which are deposited on the surface of the first silicon carbide layer facing away from the porous carbon matrix, thereby forming a first silicon particle layer.

17. The method for preparing the negative electrode material according to claim 16, characterized in that: The post-processing temperature is 450°C to 500°C, the flow rate of the second silicon source gas is 1L / min to 5L / min, the time for introducing the second silicon source gas is 20min to 360min, and the second silicon source gas includes at least one of monosilane, disilane, and trisilane.

18. The preparation method according to claims 9 to 15, characterized in that: The step 1 also includes forming a second silicon carbide layer on the outer surface of the porous carbon substrate, and the second silicon carbide layer and the first silicon carbide layer are formed simultaneously based on the same method; the step 2 also includes forming a second silicon particle layer on the surface of the second silicon carbide layer on the side away from the porous carbon substrate, and the first silicon particle layer and the second silicon particle layer are formed simultaneously based on the same method; The preparation method further comprises: step 3, forming a carbon particle coating layer, wherein the carbon particle coating layer covers the second silicon carbide layer and the second silicon particle layer; The step of forming a carbon particle coating layer includes: after step 2, heating the temperature of the fluidized bed to 500°C to 650°C, introducing a carbon source gas, and causing the carbon source gas to thermally decompose to generate carbon particles that are deposited on the surface of the second silicon carbide layer and the second silicon particle layer facing away from the porous carbon matrix; the flow rate of the carbon source gas is 0.5L / min to 6L / min, and the time for introducing the carbon source gas is 60min to 360min; the carbon source gas includes at least one of acetylene, ethylene, propylene, propane and methane.

Citation Information

Patent Citations

  • Porous carbon, nano silicon and carbon core shell structure material and preparation method thereof

    CN110224125A

  • Negative pole piece, electrochemical device comprising negative pole piece and electronic device

    CN114127985A

  • Silicon-based negative electrode material and preparation method and application thereof

    CN114976026A

  • Nano silicon-carbon composite material for secondary lithium battery as well as preparation method and application of nano silicon-carbon composite material

    CN115020689A

  • Silicon carbon material, secondary battery, and electronic device

    CN115763769A

Cited By

  • Metal coating coated silicon-based material and secondary battery

    CN119419233A

  • Silicon-carbon-based composite material, preparation method thereof and application of silicon-carbon-based composite material in lithium ion battery

    CN120518058A

  • Silicon-carbon composite for anode active material and preparing method thereof

    KR102991710B1