Electrochemical device and electronic device comprising electrochemical device
By using aluminum elements and optimized electrolytes in the electrochemical device of lithium-ion batteries, the self-discharge problem of lithium-ion batteries is solved, the cycle and low-temperature performance of the battery is improved, the battery life is extended, and the safety is improved.
Patent Information
- Application Number
- PCT/CN2023/085448
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium-ion batteries are prone to self-discharge after long-term use, especially if they cannot be charged in time, which can lead to severe over-discharge, affect battery performance and may cause safety issues.
By using a cathode active material containing aluminum element and an optimized electrolyte in an electrochemical device, specifically, the weight percentage of aluminum element is 0.01 to 1.00, and the ratio of carboxylate ester to fluoroethylene carbonate is 0.3 to 0.3 to 1.00. 55, combined with trinitrile compounds, a synergistic effect is formed to stabilize the cathode material and improve the side reactions of the electrolyte, reducing self-discharge.
It effectively reduces the self-discharge of lithium-ion batteries, improves the battery's cycle performance, high-temperature storage performance and low-temperature discharge performance, extends the battery life and improves safety.
Smart Images

Figure PCTCN2023085448-FTAPPB-I100001 
Figure PCTCN2023085448-FTAPPB-I100002 
Figure PCTCN2023085448-FTAPPB-I100003
Abstract
Description
Electrochemical device and electronic device including the same Technical Field
[0001] The present application relates to the field of energy storage technology, and in particular to an electrochemical device and an electronic device including the electrochemical device. Background Art
[0002] The concepts of carbon neutrality and carbon peak have accelerated the development of the new energy industry. Lithium batteries, as a key component of this industry, are experiencing rapid growth worldwide. Lithium-ion batteries, due to their high energy density, lack of memory effect, and portability, are used in virtually all consumer electronics applications. However, lithium-ion batteries can self-discharge during long-term storage, especially if they are not recharged after prolonged use. This continuous self-discharge can lead to severe over-discharge in lithium-ion batteries, which in turn can cause gassing, impacting their use and even causing safety issues.
[0003] Therefore, how to effectively improve the self-discharge of lithium-ion batteries and ensure other good performance is the research and development focus in the field of lithium-ion batteries.
[0004] Summary of the Invention
[0005] The present application provides an electrochemical device in an attempt to solve at least one problem existing in the related art to at least some extent.
[0006] The present application provides an electrochemical device comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a positive electrode active material, the positive electrode active material comprises an aluminum element, and the weight percentage of the aluminum element is x% based on the weight of the positive electrode active material; the electrolyte comprises a carboxylate and fluoroethylene carbonate, and the weight percentage of the carboxylate is m% and the weight percentage of the fluoroethylene carbonate is n% based on the weight of the electrolyte; wherein the electrochemical device satisfies: (1) the range of x is 0.01 to 1.00; and (2) 0.3≤m / n≤55, preferably 5≤m / n≤16.
[0007] According to some embodiments of the present application, the electrochemical device further satisfies: (3) m is in the range of 5.0 to 55.0; and (4) n is in the range of 1.0 to 15.0.
[0008] According to some embodiments of the present application, the electrochemical device further satisfies that m+n is in the range of 6.0 to 65.
[0009] According to some embodiments of the present application, the electrochemical device further satisfies a 100x / m range of 0.2 to 20.
[0010] According to some embodiments of the present application, Dn10 of the positive electrode active material is y μm, and satisfies 0.1≤y≤3.5.
[0011] According to some embodiments of the present application, the electrochemical device further satisfies 0.1≤4π×y 3 ×x / 23≤10, preferably 1.0≤4π×y 3 ×x / 23≤10.
[0012] According to some embodiments of the present application, the electrochemical device further satisfies 0.1≤π×y 2 / m≤6.0.
[0013] According to some embodiments of the present application, the electrolyte further includes a trinitrile compound, and the trinitrile compound includes at least one of the following compounds:
[0014] According to some embodiments of the present application, the weight percentage of the trinitrile compound is c%, and c ranges from 0.1 to 5.
[0015] According to some embodiments of the present application, the electrochemical device further satisfies 300×c×x / 27 in a range of 0.01 to 20.
[0016] According to some embodiments of the present application, the carboxylate includes a compound represented by formula (I),
[0017] where R 11 is selected from substituted or unsubstituted C1 to C2 alkyl groups, R 12 The substituent is selected from substituted or unsubstituted C1 to C3 alkyl groups, and when substituted, the substituent is F.
[0018] According to some embodiments of the present application, R 11 is selected from substituted or unsubstituted C1 to C2 alkyl groups, R 12 Selected from C1 to C3 alkyl groups substituted with F atoms.
[0019] According to some embodiments of the present application, the carboxylic acid ester is selected from at least one of the following compounds:
[0020] Ethyl propionate, propyl propionate, ethyl acetate, propyl acetate,
[0021] According to some embodiments of the present application, the carboxylic acid ester comprises at least one of ethyl propionate (EP), propyl propionate (PP), propyl acetate, and ethyl acetate, and
[0022] (2,2,2-trifluoroethyl propionate), (2,2-difluoroethyl acetate), At least one of .
[0023] The present application further provides an electronic device, which includes any one of the above electrochemical devices.
[0024] Additional aspects and advantages of the present application will be described, shown, or explained in part in the following description through implementation of the embodiments of the present application. DETAILED DESCRIPTION
[0025] The embodiments of the present application will be described in detail below. The embodiments described herein are illustrative and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application.
[0026] As used herein, the terms "substantially," "substantially," and "approximately" are used to describe and illustrate small variations. When used in conjunction with an event or circumstance, the terms may refer to instances where the event or circumstance occurred precisely as well as instances where the event or circumstance occurred very approximately. For example, when used in conjunction with a numerical value, the terms may refer to a range of variation of less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%. For example, two values may be considered “substantially” the same if the difference between them is less than or equal to ±10% of the mean of the values (e.g., less than or equal to ±5%, less than or equal to ±4%, less than or equal to ±3%, less than or equal to ±2%, less than or equal to ±1%, less than or equal to ±0.5%, less than or equal to ±0.1%, or less than or equal to ±0.05%).
[0027] In addition, amounts, ratios, and other numerical values are sometimes presented herein in a range format. It should be understood that such a range format is used for convenience and brevity and should be interpreted flexibly to include not only the values explicitly specified as limits of the range, but also all individual values or sub-ranges encompassed within the range, as if each value and sub-range were explicitly specified.
[0028] In the detailed description and claims, a list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0029] The term "alkyl" is intended to be a straight chain saturated hydrocarbon structure having 1 to 20 carbon atoms. "Alkyl" is also intended to be a branched or cyclic hydrocarbon structure having 3 to 20 carbon atoms. For example, an alkyl group can be an alkyl group having 1 to 2 carbon atoms, an alkyl group having 1 to 3 carbon atoms, an alkyl group having 1 to 5 carbon atoms, an alkyl group having 5 to 20 carbon atoms, an alkyl group having 5 to 15 carbon atoms, or an alkyl group having 5 to 10 carbon atoms. When an alkyl group having a specific carbon number is specified, all geometric isomers having that carbon number are intended to be encompassed; thus, for example, "butyl" is meant to include n-butyl, sec-butyl, isobutyl, tert-butyl, and cyclobutyl; "propyl" includes n-propyl, isopropyl, and cyclopropyl. Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, isopentyl, neopentyl, cyclopentyl, methylcyclopentyl, ethylcyclopentyl, n-hexyl, isohexyl, cyclohexyl, n-heptyl, octyl, cyclopropyl, cyclobutyl, norbornyl, etc. Additionally, the alkyl group may be optionally substituted.
[0030] The present application provides an electrochemical device that can improve self-discharge and has excellent cycle performance, high-temperature storage performance, and low-temperature discharge performance. Specifically, the present application provides a lithium-ion battery that can improve self-discharge and has excellent performance.
[0031] Lithium-ion battery self-discharge can be categorized as physical and chemical. Physical self-discharge is primarily due to foreign matter, metal particles, and other substances introduced during the lithium-ion battery production process, and can be improved through strict process control. Chemical self-discharge is primarily due to the instability of the solid electrolyte interface (SEI) on the negative electrode surface and side reactions of the electrolyte on the positive electrode surface. The inventors have discovered that this can be improved through a combination of positive electrode material modification and electrolyte optimization.
[0032] This application enhances the stability of the positive electrode material, reduces the occurrence of side reactions, and provides a more effective electrolyte additive for SEI stabilization on the negative electrode surface by modifying the positive electrode material and optimizing the electrolyte at the same time. Therefore, the electrochemical device of this application can effectively reduce the occurrence of chemical self-discharge while further improving the overall performance. This application evaluates the self-discharge of the electrochemical device by the open circuit voltage measured by the full-discharge storage voltage drop test. The higher the open circuit voltage, the less self-discharge.
[0033] 1. Electrochemical Device
[0034] The present application discloses an electrochemical device comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a positive electrode active material, the positive electrode active material comprises an aluminum (Al) element, and the weight percentage of the aluminum element is x% based on the weight of the positive electrode active material, wherein the electrolyte comprises a carboxylate and fluoroethylene carbonate (FEC), and the weight percentage of the carboxylate is m%, and the weight percentage of the fluoroethylene carbonate is n% based on the weight of the electrolyte, wherein the electrochemical device satisfies: (1) the range of x is 0.01 to 1.00; and (2) 0.3≤m / n≤55, preferably, 5≤m / n≤16.
[0035] Carboxylic acid esters have low viscosity and good low-temperature discharge performance, but their redox resistance is relatively poor, and they will dissolve or destroy the SEI components of the negative electrode, resulting in a decrease in the open circuit voltage during full discharge storage.
[0036] FEC helps to form a relatively stable SEI on the surface of the negative electrode, which can improve the problem of open circuit voltage drop during full discharge storage. However, at the same time, FEC will undergo electrochemical reaction decomposition on the surface of the positive electrode to produce fluoride ions.
[0037] The Al element in the positive electrode active material can react with the generated fluoride ions to generate AlF3 or LiAlF4. The generated AlF3 or LiAlF4 forms a fast ion conductor layer on the surface of the positive electrode active material, reducing the side reactions of carboxylates on the surface of the positive electrode active material. Therefore, it can effectively stabilize the surface of the positive electrode active material and reduce the impact of the dissolution of metal elements in the positive electrode active material on the stability of the negative electrode SEI, thereby improving the problem of open circuit voltage drop during full storage.
[0038] When the FEC content is low, the reaction film protection is insufficient, resulting in continuous decomposition reaction of the carboxylate; when the FEC content is too high, FEC undergoes thermal decomposition at high temperature to produce HF, which will accelerate the occurrence of electrolyte side reactions.
[0039] The inventors discovered that when the Al element content in the positive electrode active material, the carboxylate content in the electrolyte, and the FEC content in the electrolyte are adjusted to meet a certain relationship, the three can produce a synergistic effect, which can effectively solve the problem of rapid voltage decay after storage due to self-discharge of electrochemical devices, and at the same time achieve better low-temperature discharge performance.
[0040] In some embodiments, the weight percentage of the Al element, x%, based on the weight of the positive electrode active material, may be about 0.01% to about 1.00%. In some embodiments, the weight percentage of the Al element, x%, based on the weight of the positive electrode active material, may be about 0.01%, about 0.05%, about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1.00%, or a range formed by any two of the above values, for example, about 0.01% to about 0.5%, about 0.1% to about 1.00%, about 0.1% to about 0.5%, about 0.01% to about 1.00%, about 0.4% to about 1.00%, etc.
[0041] In some embodiments, the ratio of the weight percent of carboxylic acid ester, m%, to the weight percent of FEC, n%, (ie, m / n) may be greater than or equal to about 0.3 and less than or equal to about 55. In some embodiments, m / n can be about 0.3, about 0.8, about 1, about 2, about 2.3, about 2.8, about 3, about 3.5, about 4, about 4.3, about 5, about 5.5, about 5.7, about 6, about 7, about 8, about 9, about 10, about 11, about 12, about 13, about 14, about 14.3, about 15, about 15.5, about 15.7, about 16, about 157, about 17.5, about 18, about 19, about 20, about 25, about 30, about 35, about 40, about 45, about 50, about 55, or a range consisting of any two of the above values, for example, about 0.3 to about 17.5, about 0.3 to about 20, about 2, about 3.5 to about 17.5, about 3.5 to about 20, about 5 to about 16, about 5 to about 20, or about 10 to about 55, etc.
[0042] In some embodiments, the weight percentage m% of the carboxylate based on the weight of the electrolyte can be about 5.0% to about 55.0% (i.e., m is about 5.0 to about 55.0). In some embodiments, the content m% of the carboxylate based on the weight of the electrolyte is about 5.0%, about 10.0%, about 15.0%, about 20.0%, about 25.0%, about 30.0%, about 35.0%, about 40.0%, about 45.0%, about 50.0%, about 55.0%, or a range consisting of any two of the above values, such as about 5.0% to about 25.0%, about 5.0% to about 35.0%, about 5.0% to about 35.0%, about 15.0% to about 35.0%, about 15.0% to about 55.0%, or about 35.0% to about 55.0%, etc.
[0043] In some embodiments, the weight percentage of FEC, n%, based on the weight of the electrolyte, may be from about 1.0% to about 15.0% (i.e., n is from about 1.0 to about 15.0). In some embodiments, the weight percentage of FEC, n%, based on the weight of the electrolyte, may be from about 1.0%, about 2.0%, about 3.0%, about 3.5%, about 4.0%, about 5.0%, about 6.0%, about 7.0%, 8.0%, about 9.0%, about 10.0%, about 11.0%, about 12.0%, about 13.0%, about 14.0%, about 15.0%, or a range formed by any two of the above values, such as from about 1.0% to about 10.0%, about 2.0% to about 10.0%, about 2.0% to about 15.0%, about 3.5% to about 10.0%, about 3.5% to about 15.0%, or about 5% to about 15.0%, etc.
[0044] In some embodiments, the electrochemical device further satisfies: (3) m is in the range of 5.0 to 55.0; and (4) n is in the range of 1.0 to 15.0.
[0045] In some embodiments, the electrochemical device further satisfies that m+n is in the range of about 6.0 to about 65. In some embodiments, m+n can be in the range of about 6.0, about 7.0, about 8.0, about 9.0, about 10.0, about 15.0, about 18.5, about 20.0, about 23.0, about 23.5, about 25.0, about 30.0, about 35.0, about 37.0, about 38.5, about 40.0, about 45.0, about 50.0, about 55.0, about 58.5, about 60.0, about 65.0, or a range composed of any two of the above values, for example, about 6.0 to about 30, about 18.5 to about 65, about 18.5 to about 58.5, about 38.5 to about 58.5, about 30 to about 65, etc.
[0046] In some embodiments, the electrochemical device further satisfies a 100x / m range of about 0.2 to about 20. In some embodiments, the electrochemical device further satisfies a 100x / m range of about 0.2, about 0.28, about 0.3, about 0.4, about 0.5, about 0.6, about 0.7, about 0.73, about 0.8, about 0.9, about 1.0, about 1.14, about 1.5, about 1.6, about 1.71, about 2.0, about 2.5, about 2.67, about 2.86, about 3, about 3.43, about 3.5, about 4, about 5, about 6, about 7, about 8, about 9, about 10, about 13, about 15, about 18, about 20, or a range consisting of any two of the above values, for example, about 0.2 to about 8, about 0.2 to about 3.43, about 1.14 to about 8, about 1.14 to about 20, or about 8 to about 20, etc.
[0047] In some embodiments, the positive electrode active material is selected from Al-doped lithium cobalt oxide, Al-doped lithium nickel cobalt manganese (NCM) ternary material, Al-doped lithium iron phosphate, Al-doped lithium manganese oxide, or any combination thereof. In some embodiments, Al is doped by coating and the doping amount of Al in the positive electrode active material is controlled.
[0048] In some embodiments, the positive electrode active material is a particle, and the D of the positive electrode active material is n 10 is y μm, and 0.1≤y≤3.5 may be satisfied. In some embodiments, y may be about 3.5, about 3, about 2.5, about 2, about 1.5, about 1, about 0.5, about 0.1, or a range consisting of any two of the above values, for example, about 0.1 to about 2, about 0.5 to about 3, about 0.5 to about 2, about 0.5 to about 2.5, about 0.1 to about 3, or about 1 to about 3.5, etc.
[0049] In some embodiments, the electrochemical device may further satisfy 0.1≤4π×y 3 ×x / 23≤10. In some embodiments, 4π×y 3 ×x / 23 can be about 0.1, about 0.5, about 0.8, about 0.9, about 1.0, about 1.5, about 1.7, about 1.75, about 2, about 3, about 3.5, about 4, about 5, about 5.8, about 5.9, about 6, about 7, about 8, about 9, about 9.3, about 9.4, about 10, or a range consisting of any two of the above values, for example, about 0.1 to about 8, about 0.1 to about 9.4, about 0.5 to about 10, about 0.5 to about 5, about 1 to about 9, about 1 to about 10, about 0.9 to about 9.4, or about 5 to about 10, etc.
[0050] In some embodiments, the electrochemical device may further satisfy 0.1≤π×y 2 / m≤6.0. In some embodiments, π×y 2 / m can be about 0.1, about 0.3, about 0.36, about 0.4, about 0.5, about 0.6, about 0.7, about 0.8, about 0.9, about 1.0, about 1.1, about 1.5, about 1.8, about 2.0, about 2.5, about 2.8, about 3.0, about 3.5, about 3.8, about 4.0, about 4.5, about 4.8, about 5.0, about 5.5, about 6.0, or can be a range consisting of any two of the above values, for example, about 0.1 to about 1.1, about 0.2 to about 1.1, about 0.3 to about 1.1, about 0.8 to about 1.1, about 0.8 to about 6, about 0.2 to about 6, or about 1 to about 6, etc.
[0051] In some embodiments, the carboxylate in the electrolyte comprises a compound represented by formula (I),
[0052] where R 11 is selected from substituted or unsubstituted C1 to C2 alkyl groups, R 12 The substituent is selected from substituted or unsubstituted C1 to C3 alkyl groups, and when substituted, the substituent is F.
[0053] In some embodiments, R 11 is selected from substituted or unsubstituted C1 to C2 alkyl groups, R 12 Selected from C1 to C3 alkyl groups substituted by F atoms.
[0054] In some embodiments, when substituted, it is substituted with 1, 2, or 3 substituents.
[0055] In some embodiments, the carboxylic acid ester comprises at least one of the following compounds: ethyl propionate (EP), propyl propionate (PP), propyl acetate, ethyl acetate, (ethyl 3,3,3-trifluoropropionate), (2,2,2-trifluoroethyl propionate), (2,2-difluoroethyl acetate),
[0056] In some embodiments, the carboxylate comprises at least one of ethyl propionate (EP), propyl propionate (PP), propyl acetate, ethyl acetate, and fluorine-containing substituted carboxylate. (2,2,2-trifluoroethyl propionate), (2,2-difluoroethyl acetate), In some embodiments, the (2,2,2-trifluoroethyl propionate), (2,2-difluoroethyl acetate), In some embodiments, the weight percentage of the fluorine-substituted carboxylate is 1% to 30% based on the weight of the electrolyte. In some embodiments, the weight percentage of the fluorine-substituted carboxylate is 1% to 10% based on the weight of the electrolyte.
[0057] The inventors have found that when the carboxylic acid ester includes a fluorine atom-substituted compound, it is beneficial to the low-temperature discharge performance of the electrochemical device. In some embodiments, R 11 is selected from C1 to C2 alkyl, R 12 is selected from substituted or unsubstituted C1 to C3 alkyl groups, and when substituted, the substituent is F. 12 When fluorine atoms are included, the low-temperature discharge performance and storage performance of the electrochemical device in the fully discharged state are significantly improved. This may be because the charge distribution in the carboxylate is affected by the substitution of fluorine atoms. During low-temperature discharge and under low voltage conditions, side reactions are less likely to occur on the positive and negative electrode surfaces, and the stability of the electrolyte is further improved.
[0058] In some embodiments, the electrolyte may further include a trinitrile compound, the trinitrile compound including at least one of the following compounds:
[0059] In some embodiments, the weight percentage of the trinitrile compound is c%, and c ranges from about 0.1 to about 5. In some embodiments, c can be about 0.1, about 0.5, about 1, about 1.5, about 2, about 3, about 3.5, about 4, about 4.5, about 4.95, or a range consisting of any two of the above values, for example, about 0.1 to about 4.95, about 1 to about 4.95, about 1 to about 5, about 1 to about 3, or about 3 to about 5, etc.
[0060] In some embodiments, the electrochemical device may further satisfy 300×c×x / 27 in the range of about 0.01 to about 20. In some embodiments, 300×c×x / 27 can be about 0.01, about 0.05, about 0.1, about 0.4, about 0.5, about 1, about 1.1, about 2.0, about 3.0, about 4.0, about 4.4, about 5.0, about 6.0, about 7.0, about 8.0, about 9.0, about 10.0, about 11.0, about 12.0, about 13.0, about 13.3, about 14.0, about 15.0, about 16.0, about 17.0, about 18.0, about 19.0, about 20.0, or can be a range consisting of any two of the above values, for example, about 0.01 to about 13.3, about 0.1 to about 15, about 0.4 to about 20, about 4.4 to about 10, about 4.4 to about 20, or about 13.3 to about 20, etc.
[0061] In some embodiments, the positive electrode includes a positive electrode collector and a positive electrode active material layer, the positive electrode active material layer includes the above-mentioned positive electrode active material containing the Al element, the positive electrode collector includes two opposite surfaces in its own thickness direction, and the positive electrode active material layer is arranged on at least one surface of the positive electrode collector.
[0062] In some embodiments, the positive electrode active material layer further includes a binder, which improves the bonding between the positive electrode active material particles and also improves the bonding between the positive electrode active material and the positive electrode current collector.
[0063] In some embodiments, the adhesive includes at least one of styrene-butadiene rubber (SBR), water-based acrylic resin, carboxymethyl cellulose (CMC), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA) or polyvinyl alcohol (PVA), but is not limited thereto. The adhesive can be selected according to actual needs.
[0064] In some embodiments, the weight percentage of the binder is less than or equal to 2.0% based on the weight of the positive electrode active material layer to achieve a lower positive electrode sheet resistance. In some embodiments, the weight percentage of the binder is about 2.0%, about 1.8%, about 1.5%, about 1.2%, about 1.0%, about 0.8%, about 0.5%, about 0.3%, about 0.1%, or a range consisting of any two of the above values, such as about 0.1% to about 2.0%, about 0.5% to about 2.0%, about 0.1% to about 1.0%, or about 1.0% to about 2.0%, based on the weight of the positive electrode active material layer.
[0065] In some embodiments, the positive electrode active material layer also includes a conductive agent, which includes at least one of graphite, conductive carbon black, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers, but is not limited thereto. The conductive agent can be selected according to actual needs.
[0066] In some embodiments, the weight percentage of the conductive agent is greater than or equal to 0.5% based on the weight of the positive electrode active material layer to achieve a lower positive electrode sheet resistance. In some embodiments, the weight percentage of the conductive agent is greater than or equal to 0.5%, greater than or equal to 1.0%, or greater than or equal to 1.5%, etc., based on the weight of the positive electrode active material layer.
[0067] In some embodiments, the positive electrode current collector may be made of a metal foil or a porous metal plate, for example, a foil or a porous plate made of a metal such as aluminum, copper, nickel, titanium, or silver, or an alloy thereof, such as aluminum foil, but not limited thereto.
[0068] In some embodiments, the thickness of the positive electrode collector is about 5 μm to about 20 μm, for example, about 5 μm, about 6 μm, about 7 μm, about 8 μm, about 10 μm, about 12 μm, about 14 μm, about 16 μm, about 18 μm, about 20 μm, or can be a range consisting of any two of the above values, for example, about 6 μm to 18 μm or about 8 μm to about 16 μm.
[0069] In some embodiments, the positive electrode active material layer can be made by the following operations: dry mixing the positive electrode active material and the binder (conductive material and thickener used as needed) to form a sheet, pressing the obtained sheet to the positive electrode collector, or dissolving or dispersing these materials in a liquid medium to form a slurry, coating it on the positive electrode collector and drying it.
[0070] In some embodiments, the positive electrode can be prepared by a preparation method known in the art. For example, the positive electrode can be obtained by mixing a positive electrode active material, a conductive material, and a binder in a solvent to prepare an active material composition, and coating the active material composition on a positive electrode current collector. In some embodiments, the solvent may include N-methylpyrrolidone (NMP) or the like, but is not limited thereto.
[0071] In some embodiments, the negative electrode may be a metal lithium sheet, or may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector.
[0072] In some embodiments, the negative active material layer includes a negative active material and optionally includes a conductive agent, a binder, and a thickener.
[0073] In some embodiments, the negative electrode active material may include natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structured lithium titanate Li4Ti5O 12 , Li-Al alloy and one or more of metallic lithium.
[0074] In some embodiments, the conductive agent may include one or more of graphite, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0075] In some embodiments, the binder may be one or more of styrene-butadiene rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl butyral, a water-based acrylic resin, carboxymethyl cellulose, or polyacrylic acid (PAA).
[0076] In some embodiments, the thickening agent can be carboxymethyl cellulose.
[0077] The negative electrode in the electrochemical device of the present application is not limited to the above materials. The present application may also use other materials that can be used as negative electrode active materials, conductive agents, binders and thickeners for lithium-ion batteries.
[0078] The negative electrode current collector may be made of a metal foil or a porous metal plate, for example, a foil or a porous plate made of a metal such as copper, nickel, titanium, or iron, or an alloy thereof, such as copper foil.
[0079] The negative electrode can be prepared according to conventional methods in the art. Typically, the negative electrode active material and optional conductive agent, binder, and thickener are dispersed in a solvent, such as N-methylpyrrolidone or deionized water, to form a uniform negative electrode slurry. This slurry is then coated onto the negative electrode current collector. The negative electrode sheet is then produced through drying and cold pressing.
[0080] There are no special restrictions on the isolation membrane in the electrochemical device of the present application. Any well-known porous structure isolation membrane with electrochemical stability and chemical stability can be selected, such as a single-layer or multi-layer film of one or more of glass fiber, non-woven fabric, polyethylene (PE), polypropylene (PP) and polyvinylidene fluoride.
[0081] The electrolyte in the electrochemical device of the present application may include, in addition to carboxylic acid ester and FEC, an organic solvent, an electrolyte lithium salt, and additives. The present application does not impose any specific restrictions on the types of organic solvent and electrolyte lithium salt, and they can be selected according to actual needs.
[0082] In some embodiments, the organic solvent may be at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), vinylene carbonate (VC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE). In some embodiments, the organic solvent includes at least two of the above compounds.
[0083] In some embodiments, the electrolyte lithium salt can be one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0084] In some embodiments, the electrolyte may optionally include other additives. These additives may be any additives that can be used in lithium-ion batteries, and are not specifically limited herein and may be selected based on actual needs. In some embodiments, the additives may be one or more of vinyl ethylene carbonate (VEC), succinonitrile (SN), adiponitrile (AND), 1,3-propylene sultone (PST), cyclic quaternary ammonium salts of sulfonates, tris(trimethylsilyl)phosphate (TMSP), and tris(trimethylsilyl)borate (TMSB).
[0085] The electrolyte in the electrochemical device of the present application can be prepared according to the method routine in this area. For example, an organic solvent, an electrolyte lithium salt, fluoroethylene carbonate and other optional additives are mixed to obtain an electrolyte, wherein the order of addition of each material is not particularly limited. For example, an electrolyte lithium salt, fluoroethylene carbonate and other optional additives are added to an organic solvent and mixed to obtain an electrolyte. Wherein, the electrolyte lithium salt can be first added to the organic solvent, and then fluoroethylene carbonate and other optional additives are added to the organic solvent respectively or simultaneously.
[0086] The electrochemical device of the present application can be prepared according to conventional methods in the art. For example, the positive electrode, separator, and negative electrode are stacked in order, with the separator positioned between the positive and negative electrodes to provide isolation, to obtain a battery cell. Alternatively, the battery cell can be wound to obtain a battery cell. The battery cell is then placed in a packaging casing, injected with electrolyte, and sealed to obtain the electrochemical device.
[0087] 2. Electronic Devices
[0088] The electrochemical device described in this application is applicable to electronic devices in various fields.
[0089] The use of the electrochemical device of the present application is not particularly limited, and it can be used for any use known in the prior art. In one embodiment, the electrochemical device of the present application can be used for, but is not limited to, laptop computers, pen-type computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, and lithium-ion capacitors.
[0090] 3. Examples
[0091] Hereinafter, the present application will be described in more detail with reference to Examples and Comparative Examples. However, the present application is not limited to these Examples unless departing from the gist of the present application.
[0092] Preparation of positive electrode active materials
[0093] The positive electrode active material used in the examples and comparative examples is LiCoAl x O2, the doping content of Al element is controlled by coating, and the D of the positive electrode active material is controlled by a certain sintering temperature and sintering time. n10 , thereby obtaining different positive electrode active materials.
[0094] Preparation of lithium-ion batteries
[0095] (1) Preparation of positive electrode sheet
[0096] The positive electrode active material, conductive carbon black, and polyvinylidene fluoride are mixed in a weight ratio of 97:1.4:1.6, N-methylpyrrolidone is added, and the mixture is stirred evenly under the action of a vacuum mixer to obtain a positive electrode slurry, wherein the solid content of the positive electrode slurry is 72wt%; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil; the coated aluminum foil is dried at 85°C, and then cold pressed, cut into pieces, and slit, and then dried under vacuum conditions at 85°C for 4h to obtain a positive electrode sheet.
[0097] (2) Preparation of negative electrode sheet
[0098] Artificial graphite, conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber were mixed in a weight ratio of 96:2:0.8:1.2, and deionized water was added to obtain a negative electrode slurry under the action of a vacuum mixer, wherein the solid content of the negative electrode slurry was 54 wt%; the negative electrode slurry was prepared at a surface density of 7.8 mg / cm 2The negative electrode sheet was obtained by uniformly coating the negative electrode current collector copper foil; drying the coated copper foil at 85°C, cold pressing, cutting, and slitting the copper foil, and drying the negative electrode sheet at 120°C under vacuum for 12 hours.
[0099] (3) Preparation of electrolyte
[0100] In a dry argon atmosphere glove box, 30% EC, (1-42.5%-m%-n%-c%) DEC, and m% carboxylate were mixed, based on the total weight of the electrolyte. LiPF6 was then added, dissolved, and thoroughly stirred. Then, n% FEC and c% trinitrile compound were added to the electrolyte according to the tables, and mixed thoroughly to obtain an electrolyte. The contents and types of the carboxylate, FEC, and trinitrile compound in the electrolyte are shown in the tables. The content of LiPF6 in the electrolyte was 12.5%.
[0101] (4) Preparation of isolation membrane
[0102] A 9μm thick polyethylene (PE) separator was selected, and the final separator was obtained after coating and drying with a PVDF slurry and inorganic particles (flaky boehmite and Al2O3 in a ratio of 70:30). The coating thickness was 3um and the membrane porosity was 55%.
[0103] (5) Preparation of lithium-ion batteries
[0104] The positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation, and then wound to obtain a bare cell. After welding the tabs, the bare cell is placed in an outer packaging foil aluminum-plastic film, and the prepared electrolyte is injected into the dried bare cell. After vacuum packaging, standing, formation (0.02C constant current charging to 3.3V, then 0.1C constant current charging to 3.6V), shaping, capacity testing and other processes, a soft-pack lithium-ion battery is obtained.
[0105] Test Method
[0106] (1) Full storage voltage drop test:
[0107] In a 25°C environment, the lithium-ion battery is first discharged to 3.0V at a 0.2C rate, and then the lithium-ion battery is kept in a 25°C environment for 365 days. The open circuit voltage of the lithium-ion battery at this time is monitored and recorded as OCV.
[0108] (2) Low temperature discharge test:
[0109] Place the lithium-ion battery in a high and low temperature box, adjust the temperature to 25°C, then charge it at a constant current and constant voltage of 0.2C to 4.35V, and then discharge it at 0.2C to 3.0V. Record the discharge capacity at this time as C 25(mAh); then charge to 4.35V at 0.2C constant current and constant voltage, then adjust the temperature of the high and low temperature box to -20℃, and then discharge to 3.0V at 0.2C cross current, record the discharge capacity at this time as C -20 (mAh), low temperature discharge capacity retention rate C -20 / C 25 .
[0110] (3) First efficiency test:
[0111] The total capacity of the lithium-ion battery when it is first charged to 4.35V is C0, the capacity when it is first discharged to 3.0V is D0, and the first efficiency is D0 / C0.
[0112] (4) High temperature cycle test:
[0113] Place the lithium-ion battery in a 45°C high temperature box, charge it to 4.35V at 1C constant current and constant voltage, let it stand for 15 minutes, then discharge it to 3.0V at 1C constant current and let it stand for 15 minutes as one cycle. The capacity of the first cycle is recorded as C1, and the capacity of the 800th cycle is recorded as C 800 , then the high temperature cycle capacity retention rate is C 800 / C1.
[0114] (5) High temperature full charge storage test:
[0115] First, the lithium-ion battery was charged to 4.35V at a constant current and constant voltage of 0.2C, and the initial thickness d1 was tested. Then the lithium-ion battery was placed in a high-temperature furnace at 60°C and stored for 30 days, and the thickness d2 was tested. The thickness change rate of high-temperature fully charged storage was d2 / d1-1.
[0116] Test results
[0117] The lithium ion batteries of the examples and comparative examples were prepared according to the above preparation method. The Al content in the positive electrode active material, the carboxylate ester and FEC content in the electrolyte of each example and comparative example are shown in Table 1 below. The prepared lithium ion batteries were subjected to full discharge storage voltage drop test and low temperature discharge test. The test results are shown in Table 1. n 10 are all 2μm.
[0118] Table 1
[0119] As shown in Table 1, the Al content, carboxylate, and FEC in the positive electrode materials of Examples 1-1 to 1-25 satisfy (1) x is in the range of 0.01 to 1.00 and (2) 0.3 ≤ m / n ≤ 55. Compared with Comparative Examples 1-1 to 1-11, the open circuit voltage and low-temperature discharge capacity retention rate of Examples 1-1 to 1-25 are significantly improved. This is because the presence of a certain amount of carboxylate in the electrolyte can improve low-temperature discharge performance. The Al doped in the positive electrode active material and the FEC in the electrolyte can effectively reduce the voltage drop after storage, while maintaining the low-temperature discharge advantage brought by the carboxylate.
[0120] While Al-doping the positive electrode active material has limited effect on improving low-temperature discharge, the Al in the positive electrode active material can react with the easily decomposed FEC in the electrolyte to form a fast ion conductor layer on the surface of the positive electrode active material, similar to AlF3 or LiAlF4. This fast ion conductor layer can, on the one hand, reduce side reactions of the carboxylate on the positive electrode surface; on the other hand, it can maintain a low interfacial impedance while fully utilizing the low viscosity of the carboxylate, thereby improving the low-temperature discharge performance of the electrochemical device.
[0121] Control the D of the positive electrode active material according to Table 2 n 10. The prepared lithium-ion battery was subjected to a full-discharge storage voltage drop test, an initial efficiency test, and a high-temperature cycle test. The test results are shown in Tables 2 and 3.
[0122] Table 2
[0123] Table 3
[0124] As shown in Table 2, the doping amount of Al element in the positive electrode active material is related to the D n 10 needs to be controlled within a reasonable range (for example, x is between 0.01 and 1.0 and y is between 0.1 and 3.5) to obtain a higher full-discharge storage open circuit voltage and first efficiency. This is because Al doping determines the structural stability of the positive electrode active material to a certain extent. The better the structural stability of the positive electrode active material, the less active lithium loss and the better the capacity. n The smaller 10 is, the smaller the particles of the positive electrode active material are. Small particles of positive electrode active material can provide more specific surface area, which will increase the occurrence of side reactions and in turn affect the structural stability of the positive electrode active material.
[0125] As shown in Table 3, when D n 10 and the carboxylate solvent content satisfy π×y 2When the ratio of m / s to m is less than 6.0, lithium-ion batteries can maintain good full-discharge storage performance and maintain good cycling performance. This is mainly because carboxylic acid esters are prone to side reactions, which are accelerated by small particles of positive electrode active materials. Only by controlling the relationship between these two can optimal lithium-ion battery performance be achieved.
[0126] A trinitrile compound was added to the electrolyte of the lithium-ion battery. The specific type and content of the trinitrile compound are shown in Table 4. The lithium-ion battery was subjected to a full-discharge storage voltage drop test and a high-temperature full-charge storage test. The test results are shown in Table 4. Except for the type and content of the trinitrile compound and the Al content, the examples in Table 4 are the same as Examples 1-3.
[0127] Table 4
[0128] According to Table 4, the addition of trinitrile compounds to the electrolyte can further increase the open circuit voltage of full discharge storage and further reduce the thickness change rate of high-temperature full charge storage. This is because the trinitrile compounds can undergo a complex reaction on the surface of the positive electrode to form an effective protective layer on the surface of the positive electrode, thereby reducing the side reaction at the interface between the positive electrode and the electrolyte in the fully charged state and reducing gas production.
[0129] References throughout this specification to "some embodiments," "some embodiments," "one embodiment," "another example," "an example," "a specific example," or "a portion of an example" mean that at least one embodiment or example in this application includes the particular features, structures, materials, or characteristics described in that embodiment or example. Therefore, descriptions appearing throughout this specification, such as "in some embodiments," "in an embodiment," "in one embodiment," "in another example," "in an example," "in a specific example," or "an example," are not necessarily references to the same embodiment or example in this application. In addition, the particular features, structures, materials, or characteristics described herein may be combined in any suitable manner in one or more embodiments or examples.
[0130] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions, and modifications may be made to the embodiments without departing from the spirit, principles, and scope of the present application.
Claims
1. An electrochemical device comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises a positive electrode active material, the positive electrode active material comprises an aluminum element, and the weight percentage of the aluminum element is x% based on the weight of the positive electrode active material. The electrolyte comprises carboxylic acid ester and fluoroethylene carbonate. Based on the weight of the electrolyte, the weight percentage of the carboxylic acid ester is m%, and the weight percentage of the fluoroethylene carbonate is n%. The electrochemical device satisfies: (1) x is in the range of 0.01 to 1.00; and (2) 0.3≤m / n≤55, preferably, 5≤m / n≤16.
2. The electrochemical device according to claim 1, wherein the electrochemical device further satisfies: (3) m is in the range of 5.0 to 55.0; and (4) n is in the range of 1.0 to 15.
0.
3. The electrochemical device according to claim 1, wherein The electrochemical device further satisfies that m+n is in the range of 6.0 to 65. The electrochemical device according to claim 1 , wherein the electrochemical device further satisfies that 100x / m is in the range of 0.2 to 20.
5. The electrochemical device according to claim 1, wherein the D of the positive electrode active material n 10 is y μm, and 0.1≤y≤3.5 is satisfied.
6. The electrochemical device according to claim 5, wherein the electrochemical device further satisfies 0.1≤4π×y 3 ×x / 23≤10, preferably 1.0≤4π×y 3 ×x / 23≤10.
7. The electrochemical device according to claim 5, wherein the electrochemical device further satisfies 0.1≤π×y 2 / m≤6.
0.
8. The electrochemical device according to claim 1, wherein the electrolyte further comprises a trinitrile compound, the trinitrile compound comprising at least one of the following compounds: 9 . The electrochemical device according to claim 8 , wherein the weight percentage of the trinitrile compound is c %, and c ranges from 0.1 to 5. 10 . The electrochemical device according to claim 9 , wherein the electrochemical device further satisfies that 300×c×x / 27 is in the range of 0.01 to 20.
11. The electrochemical device according to claim 1, wherein the carboxylic acid ester comprises a compound represented by formula (I), Where R 11 is selected from substituted or unsubstituted C1 to C2 alkyl groups, R 12 The substituent is selected from substituted or unsubstituted C1 to C3 alkyl groups, and when substituted, the substituent is F.
12. The electrochemical device according to claim 11, wherein the carboxylic acid ester comprises at least one of the following compounds: ethyl propionate, propyl propionate, ethyl acetate, propyl acetate, 13. An electronic device comprising the electrochemical device according to claims 1 to 12.
Citation Information
Patent Citations
Cathode active material for lithium secondary battery, lithium secondary battery and method of manufacturing same
CN113823778A
Electrochemical device and electronic device
CN113921909A
Electrolyte, and electrochemical device and electronic device including same
CN114287078A
Lithium secondary battery
JP2016167446A