High-efficiency and low-cost preparation method for high-graphene-content superfine natural rubber powder masterbatch and use

The high-graphene content ultra-fine natural rubber powder masterbatch is prepared through spray drying and mechanical blending processes, which solves the problems of long production cycle and high cost in the existing technology, and realizes high-efficiency and low-cost graphene-modified natural rubber nanocomposite. The preparation of materials provides green and environmentally friendly solutions for the tire industry.

WO2024197991A1PCT designated stage expired Publication Date: 2024-10-03ZHONGBEI UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/088597
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2023-04-17
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

The existing latex co-precipitation method to prepare graphene-modified natural rubber composites requires a long production cycle and high energy consumption, resulting in high costs and limiting its application in the tire field.

Method used

A spray drying method is used to prepare a high graphene content ultrafine natural rubber powder masterbatch with a particle size below 5 μm, and is mixed with natural rubber rubber and carbon black through a mechanical blending process to prepare graphene-modified natural rubber nanocomposites.

Benefits of technology

It significantly shortens the production cycle and energy consumption, reduces costs, improves the industrialization prospects of the process, and provides high-quality graphene-modified natural rubber nanocomposites for tire preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023088597_03102024_PF_FP_ABST
    Figure CN2023088597_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of functional rubber composite materials, and particularly relates to a high-efficiency and low-cost preparation method for a high-graphene-content superfine natural rubber powder masterbatch and use. Firstly, a high-graphene-content superfine natural rubber powder masterbatch with a particle diameter lower than 5 μm is obtained by adopting a spray drying method easy for industrial production, and then the obtained high-graphene-content superfine natural rubber powder masterbatch is mixed with a natural rubber block, carbon black and the like by adopting a mechanical blending process to prepare a graphene-modified natural rubber nanocomposite material. The present invention utilizes the spray drying process to prepare the graphene-modified natural rubber superfine powder masterbatch, so that the time and energy consumption of dehydration and drying can be greatly reduced, and the production period is greatly shortened, thereby significantly reducing the cost of the graphene-modified natural rubber masterbatch, providing a new thought for the application of the graphene-modified natural rubber nanocomposite material in the tire industry, and also laying a foundation for green and environmentally friendly practices in the tire industry.
Need to check novelty before this filing date? Find Prior Art

Description

A high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content and its application Technical Field

[0001] The present invention belongs to the technical field of functional rubber composite materials, and in particular relates to a high-efficiency and low-cost preparation method of an ultrafine natural rubber powder masterbatch with a high graphene content and its application. Background Art

[0002] Tires are an indispensable component of modern transportation and are mainly made of rubber. Natural rubber is easily available, inexpensive, and has excellent high elasticity and insulation properties. In particular, its typical self-reinforcement properties make natural rubber an indispensable matrix material. It is widely used in the field of engineering tire manufacturing and is the main material for the preparation of load-bearing tires and tank road wheel tires. However, natural rubber is a polymer material. Under the action of long-term dynamic stress, its unique viscoelasticity produces hysteresis, causing the material to convert the mechanical energy it receives into internal heat, resulting in a decrease in the performance of the rubber and ultimately failure. In order to improve the comprehensive performance of natural rubber composites so that they can better meet application requirements, the currently commonly used method is to add nanofillers such as nanocarbon black, carbon nanotubes, nanomontmorillonite, graphene, etc. to enhance the performance of natural rubber composites.

[0003] Graphene is a sp 2 A new material composed of tightly packed, hybrid-connected carbon atoms forming a single-layer, two-dimensional honeycomb lattice structure exhibits excellent optical, electrical, and mechanical properties. It holds significant application prospects in materials, micro-nanofabrication, energy, biomedicine, and drug delivery, and is considered a revolutionary material of the future. Graphene oxide (GO) is a two-dimensional (2D) material with a variety of oxygen-containing functional groups, derived by oxidizing graphite through physical and chemical methods.

[0004] Graphene and its derivatives possess excellent mechanical strength, electrical conductivity, and thermal conductivity, making them widely used in rubber reinforcement and modification, resulting in rubber composites with improved mechanical strength, toughness, and thermal conductivity. However, existing graphene-modified natural rubber composites prepared by latex co-precipitation methods suffer from long production cycles, high energy consumption, and high costs due to the dehydration and drying process, which has become a major obstacle to the application of graphene-modified natural rubber composites in the tire industry.

[0005] According to the British BS2955-1993, rubber with a particle size less than 1mm is defined as powdered rubber. Compared to block or sheet rubber, powdered rubber offers numerous advantages in both processing and application. From a rubber processing perspective, powdered rubber offers advantages such as short mixing times, low power consumption, low discharge temperatures, and excellent dispersibility. Furthermore, like fillers such as carbon black, powdered rubber can be piped and automatically weighed, contributing to increased automation in factory mixing operations. From an application perspective, powdered rubber has a wide range of uses, not only in the manufacture of rubber products but also as a modifier in adhesives and polymers. Ultrafine powdered rubber with a particle size less than 0.5mm has become a hot topic.

[0006] Summary of the Invention

[0007] In response to the above background and existing problems, the present invention provides a highly efficient and low-cost method for preparing a high-graphene-content ultrafine natural rubber powder masterbatch and its application. First, a spray drying method, which is easily scalable, is used to obtain a high-graphene-content ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm. The obtained high-graphene-content ultrafine natural rubber powder masterbatch is then mechanically blended with natural rubber block rubber, carbon black, and other materials to produce a graphene-modified natural rubber nanocomposite material suitable for tire production.

[0008] The present invention is achieved through the following technical solution: a high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content, comprising the following steps:

[0009] ① Add an appropriate amount of deionized water to the graphene oxide dispersion, ultrasonically disperse it at a certain power for a certain time, then add an anionic surfactant in a certain proportion to the ultrasonicated graphene oxide dispersion, and mechanically stir it at a certain speed for a certain time to obtain a modified graphene oxide dispersion;

[0010] ② Add an appropriate amount of deionized water to the natural rubber latex, mix well, and then slowly add the prepared latex suspension to the modified graphene oxide dispersion prepared in step ① under mechanical stirring. After stirring for a certain period of time, a uniformly dispersed mixed emulsion is obtained;

[0011] ③ The evenly dispersed mixed emulsion obtained in step ② is pumped into a spray drying device through a feed pump and quickly dried into a powder at a set temperature to obtain an ultrafine natural rubber powder masterbatch with a high graphene content and a particle size of less than 5 μm.

[0012] As a further improvement of the technical solution of the preparation method of the present invention, in step ①, the anionic surfactant is a combination of one or more of anionic polyacrylamide, fatty acid salts, sulfonates, sulfates, and phosphates.

[0013] As a further improvement to the technical solution of the preparation method of the present invention, in step ①, the concentration of the graphene oxide dispersion after adding deionized water is 1 to 5 mg / ml, the ultrasonic power is 100 to 300 W, the ultrasonic time is 10 to 30 min, the mass ratio of graphene oxide to anionic surfactant in the graphene oxide dispersion is 7:1 to 3:1, the speed of mechanical stirring is 300 to 700 r / min, and the mechanical stirring time is 10 to 30 min.

[0014] As a further improvement to the technical solution of the preparation method of the present invention, in step ②, the latex concentration in the prepared latex suspension is 10% to 30%, the speed of mechanical stirring is 300 to 700 r / min, the mass ratio of the latex in the prepared latex suspension to the graphene oxide in the oxidized dispersion in step ① is 100:20 to 50, and the stirring mixing time is 5 to 30 min.

[0015] As a further improvement of the technical solution of the preparation method of the present invention, in step ③, the feed rate of the feed pump is 10-50 ml / min, the inlet air temperature of the spray dryer is 80-120°C, and the outlet air temperature is 50-80°C.

[0016] The present invention further provides an efficient and low-cost preparation method for ultrafine natural rubber powder masterbatch with high graphene content, and the application of the prepared ultrafine natural rubber powder masterbatch with high graphene content in graphene-modified natural rubber nanocomposites.

[0017] As a further improvement of the application technical solution of the present invention, the application includes the following steps:

[0018] (1) adding ultrafine natural rubber powder masterbatch with high graphene oxide content and natural rubber raw rubber block into an internal mixer in a certain mass ratio, mixing at a certain temperature for a certain time, adding an antioxidant, an antioxidant, an activator and a reinforcing filler in sequence according to a certain proportion during the mixing, and mixing uniformly to obtain a mixed rubber;

[0019] (2) placing the rubber mix obtained in step (1) in a double roller of an open mill, refining at a certain temperature, then adding an accelerator and a vulcanizing agent, mixing uniformly, and thinning until the rubber material is free of bubbles to obtain a rubber mix;

[0020] (3) The rubber mixture obtained in step (2) is allowed to stand for a certain period of time, and is vulcanized at a certain temperature and a certain pressure for a certain period of time to obtain a graphene-modified natural rubber nanocomposite material.

[0021] As a further improvement of the application technical solution of the present invention, the mass ratio of high graphene content natural rubber powder masterbatch: natural rubber raw rubber block: antioxidant: antioxidant: activator: accelerator: vulcanizer: reinforcing filler is 1.5-3:97.5-99:1:1:5:2:2:50-80; in step (1), the mixing temperature is 100-120°C, and the mixing time is 10-20 min.

[0022] As a further improvement of the application technical solution of the present invention, in step (2), the refining temperature is 50-70°C.

[0023] As a further improvement of the application technical solution of the present invention, in step (3), the storage time of the rubber mix is ​​18 to 36 hours, the vulcanization temperature is 140 to 160° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 10 to 30 minutes.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1) The present invention utilizes a spray drying process to prepare graphene-modified natural rubber masterbatch, which can greatly shorten the time and energy consumed in dehydration and drying, and greatly shorten the production cycle, thereby significantly reducing the cost of graphene-modified natural rubber masterbatch. This provides a new approach for the application of graphene-modified natural rubber nanocomposites in the tire industry and lays a foundation for the green and environmental protection of the tire industry.

[0026] 2) The present invention's process for preparing ultrafine graphene-modified natural rubber powder masterbatch by spray drying helps reduce dust pollution, energy conservation, and emission reduction, further meeting the requirements for green tire production. Furthermore, the process can be operated continuously, with low labor intensity, significantly reducing the cost of the prepared masterbatch. Therefore, the process and the masterbatch produced have great potential for industrialization.

[0027] 3) The high-graphene-content ultrafine natural rubber powder masterbatch provided by the present invention has a simple preparation process, does not require any stringent requirements, involves conventional equipment, is easy to implement, and is also easy to industrialize.

[0028] 4) The high-graphene-content ultrafine natural rubber powder masterbatch prepared by the present invention can be directly added to the natural rubber raw rubber block through conventional processes, thereby conveniently obtaining a graphene-modified natural rubber nanocomposite material for use in the preparation of high-quality tires. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0031] FIG1 is a SEM photograph of the ultrafine natural rubber powder masterbatch with high graphene content prepared in Example 1 of the present invention.

[0032] FIG2 is a SEM photograph of the ultrafine natural rubber powder masterbatch with high graphene content prepared in Example 2 of the present invention.

[0033] FIG3 is a SEM photograph of the ultrafine natural rubber powder masterbatch with high graphene content prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0034] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that, in the absence of conflict, the embodiments of the present invention and the features therein can be combined with each other.

[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all the embodiments.

[0036] The present invention provides a specific embodiment of a method for efficiently and cheaply preparing an ultrafine natural rubber powder masterbatch with a high graphene content, comprising the following steps:

[0037] ① Add an appropriate amount of deionized water to the graphene oxide dispersion, ultrasonically disperse it at a certain power for a certain time, then add an anionic surfactant in a certain proportion to the ultrasonicated graphene oxide dispersion, and mechanically stir it at a certain speed for a certain time to obtain a modified graphene oxide dispersion;

[0038] ② Add an appropriate amount of deionized water to the natural rubber latex, mix well, and then slowly add the prepared latex suspension to the modified graphene oxide dispersion prepared in step ① under mechanical stirring. After stirring for a certain period of time, a uniformly dispersed mixed emulsion is obtained;

[0039] ③ The evenly dispersed mixed emulsion obtained in step ② is pumped into a spray drying device through a feed pump and quickly dried into a powder at a set temperature to obtain an ultrafine natural rubber powder masterbatch with a high graphene content and a particle size of less than 5 μm.

[0040] In one embodiment provided herein, in step ①, the anionic surfactant is a combination of one or more of anionic polyacrylamide, fatty acid salts, sulfonates, and sulfate esters. The fatty acid salts include potassium, sodium, ammonium, and triethanolammonium salts of higher fatty acids; the sulfonates include alkylbenzene sulfonates, α-olefin sulfonates, alkyl sulfonates, petroleum sulfonates, and alkyl glycerol ether sulfonates; and the sulfate esters include fatty alcohol sulfates and secondary alkyl sulfates.

[0041] In another embodiment provided by the present invention, in step ①, the concentration of the graphene oxide dispersion after adding deionized water is 1 to 5 mg / ml, the ultrasonic power is 100 to 300 W, the ultrasonic time is 10 to 30 min, the mass ratio of graphene oxide to anionic surfactant in the graphene oxide dispersion is 7:1 to 3:1, the speed of mechanical stirring is 300 to 700 r / min, and the mechanical stirring time is 10 to 30 min.

[0042] In one embodiment provided by the present invention, in step ②, the latex concentration in the prepared latex suspension is 10% to 30%, the speed of mechanical stirring is 300 to 700 r / min, the mass ratio of the latex in the prepared latex suspension to the graphene oxide in the oxidized dispersion in step ① is 100:20 to 50, and the stirring mixing time is 5 to 30 min.

[0043] In another embodiment provided by the present invention, in step ③, the feed rate of the feed pump is 10-50 ml / min, the inlet air temperature of the spray dryer is 80-120°C, and the outlet air temperature is 50-80°C.

[0044] The present invention also provides an efficient and low-cost preparation method for ultrafine natural rubber powder masterbatch with high graphene content, and the application of the prepared ultrafine natural rubber powder masterbatch with high graphene content in graphene-modified natural rubber nanocomposites.

[0045] In one embodiment provided by the present invention, the application comprises the following steps:

[0046] (1) adding ultrafine natural rubber powder masterbatch with high graphene oxide content and natural rubber raw rubber block into an internal mixer in a certain mass ratio, mixing at a certain temperature for a certain time, adding an antioxidant, an antioxidant, an activator and a reinforcing filler in sequence according to a certain proportion during the mixing, and mixing uniformly to obtain a mixed rubber;

[0047] (2) placing the rubber mix obtained in step (1) in a double roller of an open mill, refining at a certain temperature, then adding an accelerator and a vulcanizing agent, mixing uniformly, and thinning until the rubber material is free of bubbles to obtain a rubber mix;

[0048] (3) The rubber mixture obtained in step (2) is allowed to stand for a certain period of time, and is vulcanized at a certain temperature and a certain pressure for a certain period of time to obtain a graphene-modified natural rubber nanocomposite material.

[0049] In another embodiment provided by the present invention, the mass ratio of high graphene content natural rubber powder masterbatch: natural rubber raw rubber block: antioxidant: antioxidant: activator: accelerator: vulcanizer: reinforcing filler is 1.5-3:97.5-99:1:1:5:2:2:50-80; in step (1), the mixing temperature is 100-120°C, and the mixing time is 10-20 min.

[0050] In one embodiment provided by the present invention, in step (2), the refining temperature is 50-70°C.

[0051] In another embodiment provided by the present invention, in step (3), the storage time of the rubber mix is ​​18 to 36 hours, the vulcanization temperature is 140 to 160° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 10 to 30 minutes.

[0052] The specific embodiments of the present invention are described in detail below.

[0053] Example 1

[0054] A high-efficiency and low-cost method for preparing ultrafine natural rubber powder masterbatch with high graphene content comprises the following steps:

[0055] ① Add a certain amount of deionized water to 2000 g of graphene oxide (GO) dispersion with a concentration of 10 mg / ml, and ultrasonically disperse it at a power of 100 W for 10 minutes to obtain a GO aqueous dispersion with a concentration of 1 mg / ml. Then, add sodium dodecylbenzenesulfonate (SDBS) according to a mass ratio of GO to sodium dodecylbenzenesulfonate (SDBS) of 7:1, and continuously stir mechanically at a speed of 300 r / min for 10 minutes to obtain a modified GO dispersion.

[0056] ② Add an appropriate amount of deionized water to 166.7 g of a 60% solids natural rubber latex solution to dilute it to a 10% solids natural rubber latex suspension. While mechanically stirring, add the natural rubber latex suspension to the modified GO dispersion obtained in step ①. The GO concentration in the dispersion is 1 mg / ml. Mechanical stirring is continued for 10 minutes at 25°C and 300 rpm. After thorough mixing, a mixture of natural rubber and modified GO containing 20 phr of GO is obtained.

[0057] ③ The natural rubber and modified GO mixture obtained in step ② was pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device was 80°C, the outlet air temperature was 50°C, and the flow rate of the flow pump was 10 ml / min. An ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm and a GO content of 20 phr was obtained. The SEM photo of the masterbatch is shown in Figure 1.

[0058] Example 2

[0059] A high-efficiency and low-cost method for preparing ultrafine natural rubber powder masterbatch with high graphene content comprises the following steps:

[0060] ① Add a certain amount of deionized water to 3000g of GO dispersion with a concentration of 10mg / ml. Ultrasonic dispersion is performed at 300W power for 30 minutes to obtain a GO aqueous dispersion with a concentration of 5mg / ml. SDBS is added according to a mass ratio of GO to SDBS of 5:1. The mixture is continuously mechanically stirred at a speed of 300r / min for 10 minutes to obtain a modified GO dispersion.

[0061] ② Add an appropriate amount of deionized water to 166.7 g of a 60% solids natural rubber latex solution to dilute it to a 30% solids natural rubber latex suspension. While mechanically stirring, add the natural rubber latex suspension to the modified GO dispersion obtained in step ①. The GO concentration in the dispersion is 5 mg / ml. Mechanical stirring is continued for 30 minutes at 25°C and 700 rpm. After mixing, a mixture of natural rubber and modified GO containing 30 phr of GO is obtained.

[0062] ③ The natural rubber and modified GO mixture obtained in step ② was pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device was 110°C, the outlet air temperature was 70°C, and the flow rate of the flow pump was 30 ml / min. An ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm and a GO content of 30 phr was obtained. The SEM photo of the masterbatch is shown in Figure 2.

[0063] Example 3

[0064] A high-efficiency and low-cost method for preparing ultrafine natural rubber powder masterbatch with high graphene content comprises the following steps:

[0065] ① Add a certain amount of deionized water to 5000g of GO dispersion with a concentration of 10mg / ml, and ultrasonically disperse it at a power of 300W for 30 minutes to obtain a GO aqueous dispersion with a concentration of 5mg / ml. Add SDBS according to the mass ratio of GO to SDBS 3:1, and continuously stir it mechanically at a speed of 700r / min for 30 minutes to obtain a modified GO dispersion.

[0066] ② Add an appropriate amount of deionized water to 166.7 g of a 60% solids natural rubber latex solution to dilute it to a 30% solids natural rubber latex suspension. While mechanically stirring, add the natural rubber latex suspension to the modified GO dispersion obtained in step ①. The GO concentration in the dispersion is 5 mg / ml. Mechanical stirring is continued at 25°C and 700 rpm for 30 minutes. After mixing, a mixture of natural rubber and modified GO containing 50 phr of GO is obtained.

[0067] ③ The natural rubber and modified GO mixture obtained in step ② was pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device was 120°C, the outlet air temperature was 80°C, and the flow rate of the flow pump was 50 ml / min. An ultrafine natural rubber powder masterbatch with a particle size of less than 5 μm and a GO content of 50 phr was obtained. The SEM photo of the masterbatch is shown in Figure 3.

[0068] Example 4

[0069] A process for preparing a graphene-modified natural rubber nanocomposite material using ultrafine natural rubber powder masterbatch with a high graphene content comprises the following steps:

[0070] (1) 3 g of the ultrafine natural rubber masterbatch with high graphene oxide content prepared in Example 1 and 97.5 g of natural rubber raw rubber block were added to an internal mixer and kneaded at 100° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and kneaded for 5 min. Then, 5 g of ZnO, 2 g of stearic acid, and 25 g of carbon black were added in sequence and kneaded for 2.5 min. Then, 25 g of carbon black was added and kneaded for another 2.5 min to obtain a kneaded rubber.

[0071] (2) The rubber mix obtained in step (1) was placed in a double roller of an open mill and mixed at 50° C., and then 2 g of accelerator 2-(4-morpholinothio)benzothiazole and 2 g of sulfur were added. After mixing evenly, the mixture was thinly passed until there were no bubbles in the rubber to obtain a rubber mix.

[0072] (3) The rubber mixture obtained in step (2) was allowed to stand for 18 hours and vulcanized on a flat vulcanizer at 140° C. and 10 MPa for 30 minutes to obtain a graphene-modified natural rubber nanocomposite material.

[0073] Example 5

[0074] A process for preparing a graphene-modified natural rubber nanocomposite material using ultrafine natural rubber powder masterbatch with a high graphene content comprises the following steps:

[0075] (1) 2.17 g of the ultrafine natural rubber masterbatch with high graphene oxide content prepared in Example 2 and 98.33 g of natural rubber raw rubber block were added to an internal mixer and mixed at 110° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and mixed for 5 min. Then, 5 g of ZnO, 2 g of stearic acid, and 25 g of carbon black were added in sequence and mixed for 5 min. Then, 25 g of carbon black was added and mixed for 5 min to obtain a mixed rubber.

[0076] (2) The rubber mix obtained in step (1) was placed in a double roller of an open mill and mixed at 70° C., and then 2 g of accelerator 2-(4-morpholinothio)benzothiazole and 2 g of sulfur were added. After mixing evenly, the mixture was thinly passed until there were no bubbles in the rubber to obtain a rubber mix.

[0077] (3) The rubber mixture obtained in step (2) was allowed to stand for 36 hours and vulcanized on a flat vulcanizer at 160° C. and 30 MPa for 10 minutes to obtain a graphene-modified natural rubber nanocomposite material.

[0078] Example 6

[0079] A process for preparing a graphene-modified natural rubber nanocomposite material using ultrafine natural rubber powder masterbatch with a high graphene content comprises the following steps:

[0080] (1) 1.5 g of the ultrafine natural rubber masterbatch with high graphene oxide content prepared in Example 3 and 99 g of natural rubber raw rubber block were added to an internal mixer and kneaded at 120° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and kneaded for 5 min. Then, 5 g of ZnO, 2 g of stearic acid, and 25 g of carbon black were added in sequence and kneaded for 5 min. Then, 25 g of carbon black was added and kneaded for 5 min to obtain a kneaded rubber.

[0081] (2) The rubber mix obtained in step (1) is placed in a double roller of an open mill and mixed at 70° C., and then 2 g of accelerator 2-(4-morpholinothio)benzothiazole and 2 g of sulfur are added. After mixing evenly, the mixture is thinly passed until there are no bubbles in the rubber to obtain a rubber mix.

[0082] (3) The rubber mixture obtained in step (2) was allowed to stand for 36 hours and vulcanized on a flat vulcanizer at 160° C. and 30 MPa for 20 minutes to obtain a graphene-modified natural rubber nanocomposite material.

[0083] Comparative Example 1:

[0084] A method for preparing a natural rubber powder masterbatch with a high graphene content and without graphene oxide modification, comprising the following steps:

[0085] ① Add a certain amount of deionized water to 2000 g of GO dispersion with a concentration of 10 mg / ml, ultrasonically disperse at a power of 100 W for 10 minutes to obtain a GO aqueous dispersion with a concentration of 1 mg / ml, and continuously mechanically stir at a speed of 300 r / min for 10 minutes to obtain a GO dispersion.

[0086] ② Add an appropriate amount of deionized water to 166.7 g of a 60% solids natural rubber latex solution to dilute it to a 10% solids natural rubber latex suspension. While mechanically stirring, add the natural rubber latex suspension to the GO dispersion obtained in step ①. The GO concentration in the dispersion is 1 mg / ml. Mechanical stirring is continued for 10 minutes at 25°C and 300 rpm. After mixing, a natural rubber and GO mixture containing 20 phr of GO is obtained.

[0087] ③ The mixture of natural rubber and GO obtained in step ② was pumped into a spray drying device through a flow pump. The inlet air temperature of the spray drying device was 80°C, the outlet air temperature was 50°C, and the flow rate of the flow pump was 10 ml / min to obtain a natural rubber powder masterbatch with a GO content of 20 phr.

[0088] Comparative Example 2

[0089] A process for preparing a graphene-modified natural rubber composite material using a high-graphene-content natural rubber powder masterbatch without graphene oxide modification comprises the following steps:

[0090] (1) 3 g of the high graphene oxide content natural rubber powder masterbatch prepared in Comparative Example 1 and 97.5 g of natural rubber raw rubber block were added to an internal mixer and mixed at 100° C. for 5 min. Then, 1 g of N-isopropyl-N′-phenyl-p-phenylenediamine and 1 g of 2,2,4-trimethyl-1,2-dihydroquinoline were added in sequence and mixed for 5 min. Then, 5 g of ZnO, 2 g of stearic acid and 25 g of carbon black were added in sequence and mixed for 5 min. Then, 25 g of carbon black was added and mixed for 5 min to obtain a mixed rubber.

[0091] (2) The internal rubber obtained in step (1) is placed in a double roller of an open mill and mixed at 50° C., and then 2 g of accelerator 2-(4-morpholinothio)benzothiazole and 2 g of sulfur are added. After mixing evenly, the mixture is thinly passed until there are no bubbles in the rubber to obtain a mixed rubber.

[0092] (3) The rubber mixture obtained in step (2) was allowed to stand for 18 hours and vulcanized on a flat vulcanizer at 140° C. and 10 MPa for 30 minutes to obtain a graphene-modified natural rubber nanocomposite material.

[0093] The formulations of Examples 1 to 3 and Comparative Example 1 are shown in Table 1, the formulations of Examples 4 to 6 and Comparative Example 2 are shown in Table 2, and the performance test results of Examples 4 to 6 and Comparative Example 2 are shown in Table 3.

[0094] Table 1 Formula table of Examples 1 to 3 of the present invention and Comparative Example 1

[0095] Table 2 Formula table of Examples 4 to 6 of the present invention and Comparative Example 2

[0096] The mechanical, thermal conductivity, heat buildup, abrasion, and compression set properties of Examples 4-6 and Comparative Example 2 were tested. Mechanical properties were tested according to ISO 37-2005, with a tensile rate of 500 mm / min and a tear rate of 500 mm / min. Thermal conductivity was tested according to GB / T 3399. Heat buildup and compression set were tested according to ISO 4666. Abrasion properties were tested according to GB / T 9867-2008.

[0097] Table 3 Properties of graphene-modified natural rubber nanocomposites prepared by the present invention

[0098] As shown in Table 3, the graphene-modified natural rubber nanocomposite prepared using the high-graphene-content ultrafine natural rubber powder masterbatch of the present invention exhibits excellent mechanical, thermal conductivity, heat generation, wear resistance, and permanent deformation properties. Compared to Comparative Example 2, which uses the same processes as those in Comparative Example 2 except for the graphene oxide, the graphene-modified natural rubber nanocomposite prepared using the high-graphene-content ultrafine natural rubber powder masterbatch of Example 4 exhibits even better mechanical, thermal conductivity, heat generation, wear resistance, and permanent deformation properties.

[0099] As can be seen from Figures 1-3, the particle size of the high graphene content natural rubber powder masterbatch prepared by the present invention is less than 5 μm, and it is an ultrafine powder masterbatch.

[0100] The above description is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Although detailed descriptions have been made with reference to the aforementioned embodiments, those skilled in the art should understand that they may still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents; and such modifications or replacements do not deviate from the essence of the corresponding technical solutions within the scope of the technical solutions of the embodiments, and they should all be included in the scope of protection of the claims.

Claims

1. A high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content, characterized in that: The following steps are involved: ① Adding an appropriate amount of deionized water to the graphene oxide dispersion, after ultrasonic dispersion at a certain power for a certain time, adding an anionic surfactant in a certain proportion to the ultrasonic graphene oxide dispersion, and mechanically stirring at a certain speed for a certain time to obtain a modified graphene oxide dispersion; ② Add an appropriate amount of deionized water to the natural latex, mix well, and then slowly add the prepared latex suspension to the modified graphene oxide dispersion prepared in step ① under mechanical stirring, and stir and mix for a certain period of time to obtain a uniformly dispersed mixed emulsion; ③ The uniformly dispersed mixed emulsion obtained in step ② is pumped into a spray drying device through a feed pump, and quickly dried into a powder at a set temperature to obtain an ultrafine natural rubber powder masterbatch with a high graphene content and a particle size of less than 5 μm.

2. The high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content according to claim 1 is characterized in that: In step ①, the anionic surfactant is a combination of one or more of anionic polyacrylamide, fatty acid salts, sulfonates, sulfate esters, and phosphate esters.

3. The high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content according to claim 1 is characterized in that: In step ①, the concentration of the graphene oxide dispersion after adding deionized water is 1 to 5 mg / ml, the ultrasonic power is 100 to 300 W, the ultrasonic time is 10 to 30 min, the mass ratio of graphene oxide to anionic surfactant in the graphene oxide dispersion is 7:1 to 3:1, the speed of mechanical stirring is 300 to 700 r / min, and the mechanical stirring time is 10 to 30 min.

4. The high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content according to claim 1 is characterized in that: In step ②, the latex concentration in the prepared latex suspension is 10% to 30%, the speed of mechanical stirring is 300 to 700 r / min, the mass ratio of the latex in the prepared latex suspension to the graphene oxide in the oxidized dispersion in step ① is 100:20 to 50, and the stirring and mixing time is 5 to 30 min.

5. The high-efficiency and low-cost preparation method of ultrafine natural rubber powder masterbatch with high graphene content according to claim 1, characterized in that: In step ③, the feed speed of the feed pump is 10-50 ml / min, the air inlet temperature of the spray dryer is 80-120°C, and the air outlet temperature is 50-80°C.

6. Application of the ultrafine natural rubber powder masterbatch with high graphene content prepared by the efficient and low-cost preparation method of the ultrafine natural rubber powder masterbatch with high graphene content as claimed in any one of claims 1 to 5 in graphene-modified natural rubber nanocomposites.

7. The use according to claim 6, characterized in that The following steps are involved: (1) adding ultrafine natural rubber powder masterbatch with high graphene oxide content and natural rubber raw rubber block into an internal mixer in a certain mass ratio, mixing at a certain temperature for a certain time, adding an antioxidant, an antioxidant, an activator and a reinforcing filler in sequence according to a certain proportion, and mixing evenly to obtain a mixed rubber; (2) placing the rubber mixture obtained in step (1) in a double roll of an open mixing mill, mixing at a certain temperature, then adding an accelerator and a vulcanizing agent, mixing evenly, and thinning until there are no bubbles in the rubber material to obtain a rubber mixture; (3) The mixed rubber obtained in step (2) is allowed to stand for a certain period of time, and vulcanized at a certain temperature and a certain pressure for a certain period of time to obtain a graphene-modified natural rubber nanocomposite material.

8. The use according to claim 7, characterized in that The mass ratio of high-graphene-content natural rubber powder masterbatch: natural rubber raw rubber block: antioxidant: antioxidant: activator: accelerator: vulcanizer: reinforcing filler is 1.5-3: 97.5-99: 1: 1: 5: 2: 2: 50-80; in step (1), the mixing temperature is 100-120° C., and the mixing time is 10-20 min.

9. The use according to claim 7, characterized in that: In step (2), the refining temperature is 50-70°C.

10. The use according to claim 7, characterized in that: In step (3), the storage time of the rubber mix is ​​18 to 36 hours, the vulcanization temperature is 140 to 160° C., the vulcanization pressure is 10 to 30 MPa, and the vulcanization time is 10 to 30 minutes.

Citation Information

Patent Citations

  • Preparation method of completely peeled oxidation graphene / rubber nanometer composite material

    CN102532629A

  • Preparation method of high-dispersibility graphene oxide based rubber composite material

    CN109942913A

  • Preparation method of graphene composite aerogel and application of graphene composite aerogel in oxidative removal of organic matters in wastewater

    CN112791745A

  • Method for preparing graphene masterbatch by water-phase synergistic coagulation process and forming long-service-life loading wheel tire of heavy vehicle

    CN114591545A

  • High-efficiency low-cost preparation method and application of superfine natural rubber powder masterbatch with high graphene content