Series of fluorine-containing rare earth borate compounds and preparation method, and series of fluorine-containing rare earth borate nonlinear optical crystals and preparation method therefor and use thereof
By designing and synthesizing fluorine-containing rare earth borate compounds and using asymmetric [Y-O-F] polyhedron and π-conjugated [B3O6] basic structures, we have solved the problems of ultraviolet cutoff edge and stability of existing deep ultraviolet nonlinear optical crystals. , achieving high transparency and birefringence, suitable for deep ultraviolet nonlinear optical devices.
Patent Information
- Application Number
- PCT/CN2023/089996
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2023-04-23
- Publication Date
- 2024-10-03
AI Technical Summary
There are great challenges in designing and synthesizing deep ultraviolet nonlinear optical crystals. Existing materials have relatively long UV cutoff edges and are unstable, making it difficult to meet the high transparency and birefringence requirements in the deep ultraviolet region.
A2REB3O6F2, a series of fluorine-containing rare earth borate compounds, is prepared through solid-state reaction, hydrothermal or solution methods. It uses asymmetric [Y-O-F] polyhedron and π-conjugated [B3O6] elementary structures to grow asymmetric The orthorhombic nonlinear optical crystal in the center achieves high transparency and birefringence of the crystal.
The obtained crystal has a large second-order nonlinear optical coefficient, a wide light transmission band, high hardness, and good mechanical properties. It is suitable for deep ultraviolet nonlinear optical devices, has low cost, and is easy to process and preserve.
Smart Images

Figure CN2023089996_03102024_PF_FP_ABST
Abstract
Description
Series of fluorine-containing rare earth borate compounds and fluorine-containing rare earth borate nonlinear optical crystals and their preparation methods and uses Technical Field
[0001] The invention relates to a series of fluorine-containing rare earth borate compounds and a preparation method of fluorine-containing rare earth borate nonlinear optical crystals, and a nonlinear optical device manufactured using the series of crystals. Technical Background
[0002] Deep ultraviolet coherent light with a wavelength between 200 and 150 nm is becoming increasingly important due to its potential applications in semiconductor lithography, laser micromachining, and modern scientific instruments. For solid-state lasers, obtaining deep ultraviolet coherent light is achieved through cascade frequency conversion technology of nonlinear optical crystals. However, for a suitable deep ultraviolet nonlinear optical crystal, it must meet the following stringent structural and performance requirements, including i) non-centrosymmetric structure; ii) large second-order nonlinear optical coefficient (d ij ), at least with KDP's d 36 The design and synthesis of deep-ultraviolet nonlinear optical crystals (NLOs) are characterized by: 1) high transparency in the deep ultraviolet region with the shortest possible UV cutoff wavelength; 2) moderate birefringence (Δn = 0.05–0.10) to meet the phase matching conditions for second harmonic generation in the ultraviolet or deep ultraviolet region; and 3) ease of growth, non-toxicity, chemical stability, and good mechanical properties. However, due to the contradiction between some of the above properties, large bandgap materials often exhibit small SHG response and birefringence, and the design and synthesis of deep ultraviolet nonlinear optical crystals remains a huge challenge.
[0003] Fluorinated borates based on asymmetric [YOF] polyhedra and π-conjugated [B3O6] units typically possess large band gaps and are widely considered promising candidates for developing UV or deep UV optical crystals. Notably, BBO exhibits a strong second harmonic response (6×KDP) and a UV cutoff of 189 nm. However, its phase transition at 925°C and relatively long UV cutoff limit preclude its use as a deep UV nonlinear optical crystal. However, the large optical anisotropy of [YOF] polyhedra not only enhances the birefringence of the material but also allows for the formation of 3D frameworks linking other groups within the structure, further shortening the UV cutoff. Therefore, the design and synthesis of fluorinated rare earth borate compounds with asymmetric [YOF] polyhedra and π-conjugated [B3O6] units is an effective approach for designing deep UV nonlinear optical materials.
[0004] Summary of the Invention
[0005] One of the purposes of the present invention is to provide a series of fluorine-containing rare earth borate compounds and a preparation method thereof.
[0006] The second object of the present invention is to provide a series of fluorine-containing rare earth borate nonlinear optical crystals and preparation methods.
[0007] The third object of the present invention is to provide applications of a series of fluorine-containing rare earth borate nonlinear optical crystals.
[0008] One of the purposes of the present invention is achieved in that:
[0009] The present invention aims to provide a series of fluorine-containing rare earth borate compounds, characterized in that the chemical formula of the series of fluorine-containing rare earth borate compounds is A2REB3O6F2, wherein A=Rb, Cs, NH4; RE=Sc, Y, La, and the molecular formulas are Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2, or (NH4)2LaB3O6F2, respectively, and the molecular weight is 247.46-571.14. The series of fluorine-containing rare earth borate compounds are prepared by a solid-phase reaction method, a hydrothermal method, or a solution method according to the following chemical reaction formula:
[0010] 1)4AF(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+6H3BO3→2A2REB3O6F2(A=Rb,Cs,NH4; RE=Sc,Y,La)+9H2O↑
[0011] 2)2AF(A=Rb,Cs,NH4)+3A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+2REF3(RE=Sc,Y,La)+12H3BO3→4A2REB3O6F2(A=Rb,Cs,NH4; RE=Sc,Y,La)+3CO2↑+18H2O↑
[0012] 3)2A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+6H3BO3+4NH4F→2A2REB3O6F2(A=Rb,Cs,NH4; RE=Sc,Y,La)+2CO2↑+4NH3↑+11H2O↑
[0013] 4)4A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+2REF3(RE=Sc,Y,La)+12H3BO3+2NH4F→4A2REB3O6F2(A=Rb,Cs,NH4; RE=Sc,Y,La)+4CO2↑+2NH3↑+19H2O↑
[0014] 5)4AOH(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+6H3BO3+4NH4F→2A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+4NH3↑+13H2O↑
[0015] 6)8AOH(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+2REF3(RE=Sc,Y,La)+12H3BO3+2NH4F→4A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+2NH3↑+23H2O↑
[0016] 7)6A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+4REF3(RE=Sc,Y,La)+18H3BO3→6A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+6CO2↑+27H2O↑
[0017] 8)12AOH(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+4REF3(RE=Sc,Y,La)+18H3BO3→6A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+33H2O↑
[0018] 9)4AF(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+3B2O3→2A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)
[0019] 10)2AF(A=Rb,Cs,NH4)+3A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+2REF3(RE=Sc,Y,La)+6B2O3→4A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+3CO2↑
[0020] 11)2A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+3B2O3+4NH4F→2A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+2CO2↑+4NH3↑+2H2O↑
[0021] 12)4A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+2REF3(RE=Sc,Y,La)+6B2O3+2NH4F→4A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+4CO2↑+2NH3↑+H2O↑
[0022] 13)4AOH(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+3B2O3+4NH4F→2A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+4NH3↑+4H2O↑
[0023] 14)8AOH(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+2REF3(RE=Sc,Y,La)+6B2O3+2NH4F→4A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+2NH3↑+5H2O↑
[0024] 15)6A2CO3(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+4REF3(RE=Sc,Y,La)+9B2O3→6A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+6CO2↑
[0025] 16)12AOH(A=Rb,Cs,NH4)+RE2O3(RE=Sc,Y,La)+4REF3(RE=Sc,Y,La)+9B2O3→6A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+6H2O↑
[0026] 17)2AF(A=Rb,Cs,NH4)+REN3O9·6H2O(RE=Sc,Y,La)+3H3BO3→A2REB3O6F 22 (A=Rb,Cs,NH4;RE=Sc,Y,La)+6H2O↑+3NH3↑+6O2↑
[0027] 18)2AOH(A=Rb,Cs,NH4)+REN3O9·6H2O(RE=Sc,Y,La)+3H3BO3+2AF→A2REB3O6F2(A=Rb,Cs,NH4;RE=Sc,Y,La)+8H2O↑+5NH3↑+6O2↑
[0028] 19)A2CO3(A=Rb,Cs,NH4)+REN3O9·6H2O(RE=Sc,Y,La)+3H3BO3+2AF→A2REB3O6F2(A=Rb,Cs,NH4; RE=Sc,Y,La)+7H2O↑+5NH3↑+6O2↑+CO2↑
[0029] The second object of the present invention is achieved in this way:
[0030] The present invention aims to provide a series of fluorine-containing rare earth borate nonlinear optical crystals, characterized in that the chemical formula of the series of fluorine-containing rare earth borate nonlinear optical crystals is A2REB3O6F2, wherein A=Rb, Cs, NH4, RE=Sc, Y, La, has no symmetry center, belongs to the orthorhombic crystal system, space group Amm2, unit cell parameter Z = 2. A series of fluorine-containing rare earth borate nonlinear optical crystals are grown by high-temperature melt method, hydrothermal method or solution method.
[0031] The high-temperature melt method for growing a series of fluorine-containing rare earth borate nonlinear optical crystals is specifically performed in the following steps:
[0032] a. Evenly mix a series of fluorine-containing rare earth borate compound single-phase polycrystalline powders with flux, heat it to a temperature of 400-1000°C, keep the temperature constant for a period of time to obtain a mixed melt, and then cool it to a temperature of 300-900°C, wherein the molar ratio of the series of fluorine-containing rare earth borate compound single-phase polycrystalline powders to the flux is 1:0-50; or directly mix a mixture of a compound containing A=Rb, Cs, NH4, a compound containing RE=Sc, Y, La, a boron-containing compound and a fluorine-containing compound, or a compound containing A A mixture of an A-containing compound, an RE-containing compound, a boron-containing compound, a fluorine-containing compound and a flux is prepared, and then heated to a temperature of 400-1000° C., maintained at a constant temperature for a period of time to obtain a mixed melt, and then cooled to a saturation temperature of 300-900° C., wherein the molar ratio of the element A in the A-containing compound, the element RE in the RE-containing compound, the element boron in the boron-containing compound, the element fluorine in the fluorine-containing compound to the flux is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2:0-50;
[0033] The compound containing A=Rb, Cs, NH4 includes at least one of AOH, A2O, and alkali metal salts, and the alkali metal salts include at least one of AF, ACl, ABr, ANO3, A2C2O2, A2CO3, AHCO3, and A2SO4, wherein A=Rb, Cs, and NH4;
[0034] The compounds containing RE=Sc, Y, La include RE2O3, REF3, and RE(NO3)3·6H2O;
[0035] The boron-containing compound includes at least one of B2O3, H3BO3 and borates; borates include at least one of ABO2, ABO3, A3BO3, A2B4O7, wherein A=Rb, Cs, NH4;
[0036] The fluorine-containing compounds include AF and REF3, wherein A=Rb, Cs, NH4; RE=Sc, Y, La, and other fluorine-containing compounds include at least one of KBF4, NaBF4, KPF6, and NH4PF6.
[0037] The flux mainly includes alkali metal salts, namely alkali metal carbonates, alkali metal nitrates, alkali metal sulfates, alkali metal oxalates, alkali metal borates, alkali metal phosphates, alkali metal halides, alkali metal fluoroborates, alkali metal metaborate, and alkali metal oxides, alkali metal hydroxides, and at least one or more of yttrium fluoride, yttrium nitrate, yttrium oxide, lanthanum fluoride, lanthanum nitrate, lanthanum oxide, scandium fluoride, scandium nitrate, scandium oxide, boron oxide, boric acid, phosphoric acid, lead oxide, lead fluoride, molybdenum oxide, and bismuth oxide.
[0038] The series of fluorine-containing rare earth borate compound single-phase polycrystalline powders are prepared by a solid-phase synthesis method, comprising the following steps: mixing a compound containing A = Rb, Cs, NH4, a compound containing RE = Sc, Y, La, a boron-containing compound and a fluorine-containing compound, and adopting a solid-phase reaction method to prepare the series of fluorine-containing rare earth borate compounds, wherein the molar ratio of element A in the A-containing compound, element RE in the RE-containing compound, element boron in the boron-containing compound, and element fluorine in the fluorine-containing compound is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2; the raw materials of the A-containing compound, the RE-containing compound, the boron-containing compound and the fluorine-containing compound are uniformly mixed, ground and placed in a muffle furnace, pre-burned to remove moisture and gas in the raw materials, cooled to room temperature, taken out, ground, placed in a muffle furnace for calcination, heated to 350-1000°C, kept constant at this temperature for a period of time, cooled to room temperature, taken out and ground to obtain the series of fluorine-containing rare earth borate compound single-phase polycrystalline powders.
[0039] b. Preparation of a series of seed crystals of fluorine-containing rare earth borate nonlinear optical crystals: slowly cooling the mixed melt obtained in step a to room temperature, and spontaneously crystallizing to obtain seed crystals;
[0040] c. Place the crucible containing the mixed melt obtained in step a into a crystal growth furnace, fix the seed crystal obtained in step b on the seed crystal rod, lower the seed crystal from the top of the crystal growth furnace, preheat the seed crystal rod, lower the seed crystal until it contacts the surface of the mixed melt or melts back in the mixed melt, maintain the temperature for a period of time, and then slowly reduce the temperature to the saturation temperature;
[0041] d. Continue to slowly cool down and rotate the seed crystal rod to grow the crystal. After the single crystal grows to the required size, lift the crystal from the surface of the mixed melt and slowly cool it to room temperature. Then take the crystal out of the furnace to obtain a series of fluorine-containing rare earth borate nonlinear optical crystals.
[0042] The hydrothermal method for growing a series of fluorine-containing rare earth borate nonlinear optical crystals A2REB3O6F2, wherein A=Rb, Cs, NH4, RE=Sc, Y, La, is specifically performed in the following steps:
[0043] a. Add a compound containing A = Rb, Cs, NH4, a compound containing RE = Sc, Y, La, a boron-containing compound and a fluorine-containing compound into the polytetrafluoroethylene liner of a high-pressure reactor, and then add 0.1-50 mL of deionized water or 0.1-50 g of a mineralizer, and mix them thoroughly to obtain a mixed solution, wherein the molar ratio of the element A in the A-containing compound, the element RE in the RE-containing compound, the element boron in the boron-containing compound and the element fluorine in the fluorine-containing compound to the mineralizer is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2:0-30; the mineralizer includes AO At least one or more of H, A2O, AF, ACl, ABr, ABF4, A3PO4, A3BO3, ANO3, A2C2O4, A2CO3, AHCO3, A2SO4, A2HPO4, AH2PO4, Y2O3, YF3, Y(NO3)3·6H2O, La2O3, LaF3, La(NO3)3·6H2O, Sc2O3, ScF3, Sc(NO3)3·6H2O, B2O3, KBF4, NaBF4, KPF6, NH4PF6, wherein A=Rb, Cs, NH4;
[0044] b. Tighten the polytetrafluoroethylene-lined lid of the mixed solution in step a, then place it into the corresponding high-pressure reactor, and tighten the reactor piston;
[0045] c. Place the autoclave in step b in a thermostat, heat to 120-330°C, keep constant temperature for a period of time, and then cool to room temperature;
[0046] d. Open the high-pressure reactor and filter the solution containing the crystals to obtain a series of transparent fluorine-containing rare earth borate nonlinear optical crystals.
[0047] The solution method for growing a series of fluorine-containing rare earth borate nonlinear optical crystals A2REB3O6F2, wherein A=Rb, Cs, NH4, RE=Sc, Y, La, is specifically performed in the following steps:
[0048] Add a compound containing A=Rb, Cs, NH4, a compound containing RE=Sc, Y, La, a boron-containing compound and a fluorine-containing compound into a beaker and then add 0.1-400 mL of deionized water, and stir the solution until it becomes clear. The molar ratio of element A in the A-containing compound, element RE in the RE-containing compound, element boron in the boron-containing compound and element fluorine in the fluorine-containing compound to the co-solvent is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2:0-20; the co-solvent includes at least one or more of AOH, A2O, AF, ACl, ABr, ABF4, A3PO4, A3BO3, ANO3, A2C2O4, A2CO3, AHCO3, A2SO4, Y(NO3)3·6H2O, La(NO3)3·6H2O, Sc(NO3)3·6H2O, B2O3, KBF4, NaBF4, KPF6 and NH4PF6, wherein A=Rb, Cs and NH4; the beaker is placed on a heating table and heated to 25-400°C, and after a period of time, the series of fluorine-containing rare earth borate nonlinear optical crystals are obtained. To further grow the crystals, a seed crystal of this series was suspended in the solution using a thin platinum wire. To reduce water evaporation, the beaker was covered with a polyethylene sheet punctured with dozens of millimeter-sized holes. After a while, a centimeter-sized fluorine-containing rare earth borate nonlinear optical crystal was removed from the solution.
[0049] The third object of the present invention is achieved in this way:
[0050] The aforementioned series of fluorine-containing rare earth borate nonlinear optical crystal products have high purity, the crystals are easy to grow and are transparent and unwrapped, and have the advantages of fast growth rate, low cost, and easy acquisition of larger-sized crystals; the obtained crystals have a relatively wide light transmission band, high hardness, good mechanical properties, are not easy to break and deliquesce, and are easy to process and preserve. A series of fluorine-containing rare earth borate nonlinear optical crystals obtained by the method of the present invention can be used as a nonlinear optical device according to the application requirements of the device. The device comprises a device for generating at least one beam of output radiation with a frequency different from the incident electromagnetic radiation after passing at least one beam of incident electromagnetic radiation through at least one nonlinear optical device. The nonlinear optical crystal is an A2REB3O6F2 (A=Rb, Cs, NH4, RE=Sc, Y, La) crystal, and the molecular formulas are Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] FIG1 is an XRD spectrum of the compound Rb2YB3O6F2 powder in the present invention;
[0052] FIG2 is an XRD spectrum of the compound Cs2YB3O6F2 powder in the present invention;
[0053] FIG3 is a crystal structure diagram of the series of fluorine-containing rare earth borate nonlinear optical crystals A2REB3O6F2 (A=Rb, Cs, NH4; RE=Sc, Y, La) of the present invention;
[0054] FIG4 is a working principle diagram of the nonlinear optical device made by the present invention, wherein 1 is a laser, 2 is an emitted light beam, 3 is a series of fluorine-containing rare earth borate nonlinear optical crystals, 4 is an output light beam, and 5 is a filter. DETAILED DESCRIPTION
[0055] The present invention will be described in detail below with reference to the accompanying drawings and embodiments, but is not limited to the embodiments described. Any improvements and variations made on the basis of the present invention are within the scope of protection of the present invention.
[0056] Example 1
[0057] According to the reaction formula: 4RbF+Y2O3+6H3BO3→2Rb2YB3O6F2+9H2O↑, Rb2YB3O6F2 compound is synthesized:
[0058] RbF, Y2O3, and H3BO3 were weighed in a molar ratio of 2:0.5:3 and placed in a mortar, mixed and carefully ground. The mixture was then placed in a Φ100mm×100mm open corundum crucible, placed in a muffle furnace, slowly heated to 400°C, held at this temperature for 24 hours, cooled to room temperature, and placed in a muffle furnace after grinding. The temperature was then raised to 600°C and held at this temperature for 24 hours. The ground Rb2YB3O6F2 single-phase polycrystalline powder was taken out and subjected to X-ray analysis. The obtained X-ray spectrum was consistent with the X-ray spectrum obtained from the Rb2YB3O6F2 single crystal structure.
[0059] The resulting Rb2YB3O6F2 single-phase polycrystalline powder was placed in an 80mm x 80mm open platinum crucible and heated to 1000°C at a heating rate of 30°C / h. The mixture was held at this temperature for 3 hours to obtain a mixed melt. The mixture was then cooled to 900°C and then slowly cooled to 600°C at a rate of 0.5°C / h. The furnace was then closed. The Rb2YB3O6F2 nonlinear optical crystal seed crystal was obtained by spontaneous crystallization.
[0060] Growing crystals in compound melts: The obtained Rb2YB3O6F2 nonlinear optical crystal seed crystals were fixed on a seed crystal rod and lowered from the top of the crystal growth furnace. The seed crystals were preheated on the surface of the mixed melt for 10 minutes, immersed in the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes, and then the temperature was rapidly lowered to the saturation temperature of 700°C.
[0061] Then cool down at a rate of 0.1℃ / day, rotate the seed crystal rod at a speed of 10rpm, and after the crystal growth is completed, separate the crystal from the liquid surface and cool the temperature to room temperature at a rate of 10℃ / h to obtain Rb2YB3O6F2 crystals with a size of 20mm×18mm×10mm.
[0062] Example 2
[0063] According to the reaction formula: 2RbF+3Rb2CO3+Sc2O3+2ScF3+12H3BO3→4Rb2ScB3O6F2+3CO2↑+18H2O↑, Rb2ScB3O6F2 compound is synthesized:
[0064] RbF, Rb2CO3, Sc2O3, ScF3, and H3BO3 are directly weighed in a molar ratio of 0.5:0.75:0.25:0.5:3, and the weighed raw materials are mixed with flux LiBO2-RbF-H3BO3 in a molar ratio of 1:15, wherein LiBO 2、 The molar ratio of RbF to H3BO3 was 2:5:8, and the mixture was placed in an open platinum crucible of Φ80mm×80mm. The mixture was heated to 900℃ and kept at this temperature for 60 hours to obtain a mixed melt. The mixture was then slowly cooled to obtain a Rb2ScB3O6F2 nonlinear optical crystal seed crystal.
[0065] The obtained Rb2ScB3O6F2 nonlinear optical crystal seed crystal is fixed on a seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 10 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 830°C; then the temperature is slowly cooled at a rate of 1°C / day without rotating the seed crystal rod. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 20°C / h. The crystal is then taken out of the furnace to obtain a Rb2ScB3O6F2 crystal with a size of 25mm×22mm×12mm.
[0066] Example 3
[0067] According to the reaction formula: 2Rb2CO3+Y2O3+6H3BO3+4NH4F→2Rb2YB3O6F2+2CO2↑+4NH3↑+11H2O↑, Rb2YB3O6F2 compound is synthesized:
[0068] Rb2CO3, Y2O3, H3BO3, and NH4F are directly weighed in a molar ratio of 1:0.5:3:2, and the weighed raw materials are mixed with a flux K2CO3-RbF-H3BO3 in a molar ratio of 1:50, wherein the molar ratio of K2CO3, RbF, and H3BO3 is 10:15:25, and the mixture is placed in an open platinum crucible of Φ80mm×80mm, and the temperature is raised to 400°C and kept constant for 60 hours to obtain a mixed melt; and the temperature is slowly lowered to obtain an Rb2YB3O6F2 nonlinear optical crystal seed crystal;
[0069] The obtained Rb2YB3O6F2 nonlinear optical crystal seed crystal was fixed on the seed crystal rod and unloaded from the top of the crystal growth furnace. The seed crystal was preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 300°C.
[0070] Then slowly cool down at a rate of 3°C / day, rotate the seed crystal crucible at a speed of 5 rpm, and after the crystal grows to the required size, lift the crystal from the melt surface, cool the temperature to room temperature at a rate of 1°C / h, and then take the crystal out of the furnace to obtain a Rb2YB3O6F2 crystal with a size of 25mm×22mm×20mm.
[0071] Example 4
[0072] According to the reaction formula: 4Cs2CO3+Y2O3+2YF3+12H3BO3+2NH4F→4Cs2YB3O6F2+4CO2↑+2NH3↑+19H2O↑, the Cs2YB3O6F2 compound is synthesized:
[0073] a. Cs2CO3, Y2O3, YF3, H3BO3, and NH4F are directly weighed in a molar ratio of 1:0.25:0.5:3:0.5, and the weighed raw materials are mixed with a flux Cs2CO3-KF-H3BO3 in a molar ratio of 1:40, wherein the molar ratio of Cs2CO3, KF, and H3BO3 is 10:10:20, and the mixture is placed in an open platinum crucible of Φ80mm×80mm, and the temperature is raised to 720°C and kept constant for 60 hours to obtain a mixed melt, which is then lowered to 780°C and spontaneously crystallized to obtain a Cs2YB3O6F2 nonlinear optical crystal seed crystal;
[0074] The obtained Cs2YB3O6F2 nonlinear optical crystal seed crystal is fixed on a seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 760°C; then the temperature is slowly cooled at a rate of 3°C / day, and the seed crystal crucible is rotated at a speed of 5 rpm. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 1°C / h. The crystal is then taken out of the furnace to obtain a Cs2YB3O6F2 crystal with a size of 25 mm×22 mm×20 mm.
[0075] Example 5
[0076] According to the reaction formula: 4RbOH+Y2O3+6H3BO3+4NH4F→2Rb2YB3O6F2+4NH3↑+13H2O↑, Rb2YB3O6F2 compound is synthesized:
[0077] a. RbOH, Y2O3, H3BO3, and NH4F were directly weighed in a molar ratio of 2:0.5:3:2, and the weighed raw materials were mixed with a flux Na2CO3-KF-H3BO3 in a molar ratio of 1:18, wherein the molar ratio of Na2CO3, KF, and H3BO3 was 2:6:10, and the mixture was placed in an open platinum crucible of Φ80mm×80mm, and the temperature was raised to 900°C, maintained at the temperature for 60 hours, and spontaneously crystallized to obtain a Rb2YB3O6F2 nonlinear optical crystal seed crystal;
[0078] The obtained Rb2YB3O6F2 nonlinear optical crystal seed crystal was fixed on a seed crystal rod and removed from the top of the crystal growth furnace. The seed crystal was first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 860°C; then the temperature was slowly cooled at a rate of 3°C / day, and the seed crystal crucible was rotated at a speed of 5 rpm. After the crystal grew to the desired size, the crystal was lifted from the melt surface and the temperature was cooled to room temperature at a rate of 1°C / h. The crystal was then taken out of the furnace to obtain a Rb2YB3O6F2 crystal with a size of 25 mm×22 mm×20 mm.
[0079] Example 6
[0080] According to the reaction formula: 8(NH4)OH+La2O3+2LaF3+12H3BO3+2NH4F→4(NH4)2LaB3O6F2+ 2NH3↑+23H2O↑, (NH4)2LaB3O6F2 compound is synthesized:
[0081] (NH4)OH, La2O3, LaF3, H3BO3, and NH4F were weighed directly and mixed with a cosolvent in a molar ratio of 2:0.25:0.5:3:0.5. The cosolvent, H3BO3, and La(NO3)3·6H2O, were mixed in a molar ratio of 14:6. The mixture was added to a 10mL beaker, followed by 0.1mL of deionized water and stirred until the solution was clear. The beaker was then placed on a heating plate at 25°C. After two days, a (NH4)2LaB3O6F2 nonlinear optical crystal was obtained. To further grow the crystal, a seed crystal of the (NH4)2LaB3O6F2 crystal was suspended in the solution using a fine platinum wire. To minimize water evaporation, the beaker was covered with a polyethylene sheet pierced with several dozen millimeter-sized holes. After three weeks, a centimeter-sized (NH4)2LaB3O6F2 nonlinear optical crystal was removed from the solution.
[0082] Example 7
[0083] According to the reaction formula: 6Cs2CO3+Y2O3+4YF3+18H3BO3→6Cs2YB3O6F2+6CO2↑+27H2O↑, the Cs2YB3O6F2 compound is synthesized:
[0084] Cs2CO3, Y2O3, YF3, and H3BO3 are directly weighed in a molar ratio of 1:0.167:0.667:3, and the weighed raw materials are mixed with a flux KF-Cs2CO3-H3BO3 in a molar ratio of 1:35, wherein the molar ratio of KF, Cs2CO3, and H3BO3 is 8:7:20, and the mixture is placed in an open platinum crucible of Φ80mm×80mm, and the temperature is raised to 880°C and kept constant for 60 hours to obtain a mixed melt, and a Cs2YB3O6F2 nonlinear optical crystal seed crystal is obtained by spontaneous crystallization;
[0085] The obtained Cs2YB3O6F2 nonlinear optical crystal seed crystal is fixed on the seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 860°C; then the temperature is slowly cooled at a rate of 3°C / day, and the seed crystal crucible is rotated at a speed of 5 rpm. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 1°C / h. The crystal is then taken out of the furnace to obtain a Cs2YB3O6F2 crystal with a size of 20 mm×15 mm×6 mm.
[0086] Example 8
[0087] According to the reaction formula: 12CsOH+Y2O3+4YF3+18H3BO3→6Cs2YB3O6F2+33H2O↑, the Cs2YB3O6F2 compound is synthesized:
[0088] CsOH, Y2O3, ScF3, and H3BO3 are directly weighed as raw materials in a molar ratio of 2:0.167:0.667:3, and the weighed raw materials are mixed with a flux CsF-H3BO3 in a molar ratio of 1:27, wherein the molar ratio of CsF to H3BO3 is 12:15, and the mixture is placed in an open platinum crucible of Φ80mm×80mm, and the temperature is raised to 860°C and kept constant for 60 hours to obtain a mixed melt, and a Cs2YB3O6F2 nonlinear optical crystal seed crystal is obtained by spontaneous crystallization;
[0089] The obtained Cs2YB3O6F2 nonlinear optical crystal seed crystal is fixed on the seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 800°C; then the temperature is slowly cooled at a rate of 3°C / day, and the seed crystal crucible is rotated at a speed of 5 rpm. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 1°C / h. The crystal is then taken out of the furnace to obtain a Cs2YB3O6F2 crystal with a size of 20 mm×15 mm×6 mm.
[0090] Example 9
[0091] According to the reaction formula: 4RbF+La2O3+3B2O3→2Rb2LaB3O6F2, Rb2LaB3O6F2 compound is synthesized:
[0092] RbF, La2O3, and B2O3 were directly weighed in a molar ratio of 2:0.5:1.5, and the weighed raw materials were mixed with a flux RbOH-H3BO3 in a molar ratio of 1:30, wherein the molar ratio of RbOH to H3BO3 was 10:20, and the mixture was placed in an open platinum crucible of Φ80mm×80mm, and the temperature was raised to 800℃ and kept at this temperature for 60 hours to obtain a mixed melt, and a series of Rb2LaB3O6F2-containing nonlinear optical crystal seed crystals were obtained by spontaneous crystallization;
[0093] The obtained series of Rb2LaB3O6F2 nonlinear optical crystal seed crystals were fixed on the seed crystal rod and the seed crystals were removed from the top of the crystal growth furnace. The seed crystals were first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 750°C; then the temperature was slowly cooled at a rate of 3°C / day, and the seed crystal crucible was rotated at a speed of 5 rpm. After the crystal grew to the desired size, the crystal was lifted from the melt surface and the temperature was cooled to room temperature at a rate of 1°C / h. The crystal was then taken out of the furnace to obtain a Rb2LaB3O6F2 crystal with a size of 22mm×20mm×10mm.
[0094] Example 10
[0095] According to the reaction formula: 2CsF+3Cs2CO3+Y2O3+2YF3+6B2O3→4Cs2YB3O6F2+3CO2↑, the Cs2YB3O6F2 compound is synthesized:
[0096] Directly weigh CsF, Cs2CO3, Y2O3, YF3, and B2O3 in a molar ratio of 0.5:0.75:0.25:0.5:1.5, mix the weighed raw materials with a flux CsF-Cs2CO3-H3BO3 in a molar ratio of 1:50, wherein the molar ratio of CsF, Cs2CO3, and B2O3 is 11:7:32, and place the mixture into an open platinum crucible of Φ80mm×80mm, heat to 600°C, maintain the temperature for 10 hours, and spontaneously crystallize to obtain a Cs2YB3O6F2 nonlinear optical crystal seed crystal;
[0097] The obtained Cs2YB3O6F2 nonlinear optical crystal seed crystal was fixed on a seed crystal rod and removed from the top of the crystal growth furnace. The seed crystal was first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 550°C; then the temperature was slowly cooled at a rate of 3°C / day, and the seed crystal crucible was rotated at a speed of 5 rpm. After the crystal grew to the desired size, the crystal was lifted from the melt surface and the temperature was cooled to room temperature at a rate of 1°C / h. The crystal was then taken out of the furnace to obtain a Cs2YB3O6F2 crystal with a size of 13 mm × 10 mm × 7 mm.
[0098] Example 11
[0099] According to the reaction formula: 2Rb2CO3+Y2O3+3B2O3+4NH4F→2Rb2YB3O6F2+2CO2↑+4NH3↑+2H2O↑, Rb2YB3O6F2 compound is synthesized:
[0100] a. Weighing raw materials of Rb2CO3, Y2O3, B2O3, and NH4F in a molar ratio of 1:0.5:1.5:2, mixing the weighed raw materials with a flux RbF-RbOH-B2O3 in a molar ratio of 1:45, wherein the molar ratio of RbF, RbOH, and B2O3 is 15:15:15, placing the mixture into an open platinum crucible of Φ80 mm × 80 mm, heating the mixture to 700° C., maintaining the temperature for 60 hours, and spontaneously crystallizing the mixture to obtain a Rb2YB3O6F2 nonlinear optical crystal seed crystal;
[0101] The obtained Rb2YB3O6F2 nonlinear optical crystal seed crystal was fixed on a seed crystal rod and removed from the top of the crystal growth furnace. The seed crystal was first preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 670°C; then the temperature was slowly cooled at a rate of 3°C / day, and the seed crystal crucible was rotated at a speed of 5 rpm. After the crystal grew to the desired size, the crystal was lifted from the melt surface and the temperature was cooled to room temperature at a rate of 1°C / h. The crystal was then taken out of the furnace to obtain a Rb2YB3O6F2 crystal with a size of 13 mm×10 mm×7 mm.
[0102] Example 12
[0103] According to the reaction formula: 4(NH4)2CO3+Sc2O3+2ScF3+6B2O3+2NH4F→4(NH4)2ScB3O6F2+4CO2↑+2NH3↑+H2O↑, (NH4)2ScB3O6F2 compound is synthesized:
[0104] a. (NH4)2CO3, Sc2O3, ScF3, B2O3, and NH4F were directly weighed and mixed with a mineralizer in a molar ratio of 1:0.25:0.5:1.5:0.5, wherein the molar ratio of the mineralizer H3BO3, (NH4)OH, and (NH4)2C2O4 was 10:10:10, and added to a polytetrafluoroethylene liner of a 21 mL autoclave, and then 0.1 g of phosphoric acid was added and mixed thoroughly to obtain a mixed solution;
[0105] b. Tighten the polytetrafluoroethylene-lined lid of the mixed solution in step a, then place it into a clean and pollution-free high-pressure reactor, and tighten the reactor piston;
[0106] c. Place the autoclave in step b in a thermostat, raise the temperature to 160°C at a heating rate of 10°C / h, maintain the temperature for 11 days, and then cool to room temperature at a cooling rate of 4°C / h;
[0107] d. Open the high-pressure reactor and filter the solution containing the crystal to obtain the (NH4)2ScB3O6F2 nonlinear optical crystal.
[0108] Example 13
[0109] According to the reaction formula: 4(NH4)OH+Y2O3+3B2O3+4NH4F→2(NH4)2YB3O6F2+4NH3↑+4H2O↑, (NH4)2YB3O6F2 compound is synthesized:
[0110] Directly weigh the raw materials (NH4)OH, Y2O3, B2O3 and NH4F in a molar ratio of 2:0.5:1.5:2, and mix the weighed raw materials with the flux (NH4)2C2O4-B2O3-C S F is mixed in a molar ratio of 1:39, wherein (NH4)2C2O4, B2O3 and C S The molar ratio of F is 7:7:25, and the mixture is placed in an open platinum crucible of Φ80mm×80mm, and the temperature is raised to 480℃ and kept constant for 60 hours to obtain a mixed melt, which is spontaneously crystallized to obtain a (NH4)2YB3O6F2 nonlinear optical crystal seed crystal;
[0111] The obtained (NH4)2YB3O6F2 nonlinear optical crystal seed crystal is fixed on a seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 10 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 430°C; then the temperature is slowly cooled at a rate of 1°C / day without rotating the seed crystal rod. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 20°C / h. The crystal is then taken out of the furnace to obtain a (NH4)2YB3O6F2 crystal with a size of 16mm×12mm×10mm.
[0112] Example 14
[0113] According to the reaction formula: 8CsOH+La2O3+2LaF3+6B2O3+2NH4F→4Cs2LaB3O6F2+2NH3↑+5H2O↑, the Cs2LaB3O6F2 compound is synthesized:
[0114] CsOH, La2O3, LaF3, B2O3, and NH4F are directly weighed in a molar ratio of 2:0.25:0.5:1.5:0.5, and the weighed raw materials are mixed with a flux CsF-LaF3-CsNO3-B2O3 in a molar ratio of 1:36, wherein the molar ratio of CsF, LaF3, CsNO3, and B2O3 is 8:5:8:15, and the mixture is placed in an open platinum crucible of Φ80 mm×80 mm, and the temperature is raised to 780°C, and spontaneously crystallized to obtain a Cs2LaB3O6F2 nonlinear optical crystal seed crystal;
[0115] The obtained Cs2LaB3O6F2 nonlinear optical crystal seed crystal is fixed on a seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 10 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 760°C; then the temperature is slowly cooled at a rate of 1°C / day without rotating the seed crystal rod. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 20°C / h. The crystal is then taken out of the furnace to obtain a Cs2LaB3O6F2 crystal with a size of 16mm×12mm×10mm.
[0116] Example 15
[0117] According to the reaction formula: 6Rb2CO3+La2O3+4LaF3+9B2O3→6Rb2LaB3O6F2+6CO2↑, Rb2LaB3O6F2 compound is synthesized:
[0118] Rb2CO3, La2O3, LaF3, and H3BO3 are directly weighed in a molar ratio of 1:0.167:0.667:1.5, and the weighed raw materials are mixed with a flux CsF-LaF3-KOH-B2O3 in a molar ratio of 1:26, wherein the molar ratio of CsF, LaF3, KOH, and B2O3 is 10:3:5:8, and the mixture is placed in an open platinum crucible of Φ80 mm×80 mm, and the temperature is raised to 950° C. and kept at this temperature for 10 hours for spontaneous crystallization to obtain a Rb2LaB3O6F2 nonlinear optical crystal seed crystal;
[0119] The obtained Rb2LaB3O6F2 nonlinear optical crystal seed crystal is fixed on a seed crystal rod and removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 10 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 930°C; then the temperature is slowly cooled at a rate of 1°C / day without rotating the seed crystal rod. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 20°C / h. The crystal is then taken out of the furnace to obtain a Rb2LaB3O6F2 crystal with a size of 16mm×12mm×10mm.
[0120] Example 16
[0121] According to the reaction formula: 12CsOH+Y2O3+4YF3+9B2O3→6Cs2YB3O6F2+6H2O↑, the Cs2YB3O6F2 compound is synthesized:
[0122] a. CsOH, Y2O3, YF3, and B2O3 are directly weighed in a molar ratio of 2:0.167:0.667:1.5, and the weighed raw materials are mixed with a flux Cs2CO3-YF3-KF-B2O3 in a molar ratio of 1:26, wherein the molar ratio of Cs2CO3, YF3, KF and B2O3 is 10:3:5:8, and the mixture is placed in an open platinum crucible of Φ80mm×80mm, and the temperature is raised to 780°C, maintained at this temperature for 60 hours, and spontaneously crystallized to obtain a Cs2YB3O6F2 nonlinear optical crystal seed crystal;
[0123] The obtained Cs2YB3O6F2 nonlinear optical crystal seed crystal is fixed on a seed crystal rod and the seed crystal is removed from the top of the crystal growth furnace. The seed crystal is first preheated on the surface of the mixed melt for 10 minutes, immersed under the liquid surface, and the seed crystal is melted back in the mixed melt. The temperature is kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 730°C; then the temperature is slowly cooled at a rate of 1°C / day without rotating the seed crystal rod. After the crystal grows to the desired size, the crystal is lifted from the melt surface and the temperature is cooled to room temperature at a rate of 20°C / h. The crystal is then taken out of the furnace to obtain a Cs2YB3O6F2 crystal with a size of 16mm×12mm×10mm.
[0124] Example 17
[0125] According to the reaction formula: 2RbF+La(NO3)3·6H2O+3H3BO3→Rb2LaB3O6F2+6H2O↑+3NH3↑+6O2↑, Rb2LaB3O6F2 compound is synthesized:
[0126] RbF, La(NO3)3·6H2O, and H3BO3 were directly weighed in a molar ratio of 2:1:3, and the weighed raw materials were mixed with a flux RbF-H3BO3 in a molar ratio of 1:35, wherein the molar ratio of RbF to H3BO3 was 13:22. The mixture was placed in an open platinum crucible of Φ80mm×80mm, and the temperature was raised to 710°C and kept constant for 60 hours to obtain a mixed melt, which was spontaneously crystallized to obtain a series of Rb2LaB3O6F2-containing nonlinear optical crystal seed crystals;
[0127] The obtained series of Rb2LaB3O6F2 nonlinear optical crystal seed crystals were fixed on the seed crystal rod and unloaded from the top of the crystal growth furnace. The seed crystals were preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 690℃.
[0128] Then slowly cool down at a rate of 3°C / day, rotate the seed crystal crucible at a speed of 5 rpm, and after the crystal grows to the required size, lift the crystal from the melt surface, cool the temperature to room temperature at a rate of 1°C / h, and then take the crystal out of the furnace to obtain a Rb2LaB3O6F2 crystal with a size of 22mm×18mm×14mm.
[0129] Example 18
[0130] According to the reaction formula: 2(NH4)OH+Y(NO3)3·6H2O+3H3BO3+2NH4F→(NH4)2YB3O6F2+8H2O↑+5NH3↑+6O2↑, (NH4)2YB3O6F2 compound is synthesized:
[0131] a. (NH4)OH, Y(NO3)3·6H2O, H3BO3, and NH4F were directly weighed and mixed with a mineralizer in a molar ratio of 2:1:3:2, wherein the molar ratio of the mineralizer H3BO3, NH4OH, and (NH4)2C2O4 was 10:2:10, and added to a polytetrafluoroethylene liner of a 21 mL autoclave, and then 0.1 g of phosphoric acid was added and mixed thoroughly to obtain a mixed solution;
[0132] b. Tighten the polytetrafluoroethylene-lined lid of the mixed solution in step a, then place it into a clean and pollution-free high-pressure reactor, and tighten the reactor piston;
[0133] c. Place the autoclave in step b in a thermostat, raise the temperature to 160°C at a heating rate of 10°C / h, maintain the temperature for 11 days, and then cool to room temperature at a cooling rate of 4°C / h;
[0134] d. Open the high-pressure reactor and filter the solution containing the crystal to obtain the (NH4)2YB3O6F2 nonlinear optical crystal.
[0135] Example 19
[0136] According to the reaction formula: Cs2CO3+Sc(NO3)3·6H2O+3H3BO3+2NH4F→Cs2ScB3O6F2+7H2O↑+5NH3↑+6O2↑+CO2↑, the Cs2ScB3O6F2 compound is synthesized:
[0137] The raw materials of Cs2CO3, Sc(NO3)3·6H2O, H3BO3 and NH4F were directly weighed in a molar ratio of 1:1:3:2, and the weighed raw materials were mixed with a flux LiF-Cs2CO3-H3BO3 in a molar ratio of 1:33, wherein the molar ratio of LiF, Cs2CO3 and H3BO3 was 7:8:18, and the mixture was placed in an open platinum crucible of Φ80mm×80mm, and the temperature was raised to 750℃ and kept at this temperature for 60 hours, and a series of nonlinear optical crystal seed crystals containing Cs2ScB3O6F2 were obtained by spontaneous crystallization;
[0138] The obtained series of Cs2ScB3O6F2 nonlinear optical crystal seed crystals were fixed on the seed crystal rod and unloaded from the top of the crystal growth furnace. The seed crystals were preheated on the surface of the mixed melt for 15 minutes, immersed under the liquid surface, and melted back in the mixed melt. The temperature was kept constant for 30 minutes and then rapidly cooled to the saturation temperature of 720℃.
[0139] Then slowly cool down at a rate of 3°C / day, rotate the seed crystal crucible at a speed of 5 rpm, and after the crystal grows to the desired size, lift the crystal from the melt surface, cool the temperature to room temperature at a rate of 1°C / h, and then take the crystal out of the furnace to obtain a Cs2ScB3O6F2 crystal with a size of 22mm×18mm×14mm.
[0140] Example 20
[0141] A single crystal device is processed into a device in a matching direction from any of the Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2 crystals obtained in Examples 1-19, and is placed at position 3 as shown in FIG4 . At room temperature, a Nd:YAG Q-switched laser light source with a wavelength of 1064 nm is used as a pump source. When Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2 nonlinear optical crystal 3 is injected, frequency-doubled light with a wavelength of 532nm is generated, and the output light beam 4 contains infrared light with a wavelength of 1064nm and frequency-doubled light of 532nm, which is filtered out by filter 5 to obtain laser with a wavelength of 532nm.
[0142] Example 21
[0143] A single crystal device is processed into any Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2 crystal obtained in Examples 1-19 in a matching direction and placed at position 3 as shown in FIG4. At room temperature, a Nd:YAG Q-switched laser light source with a wavelength of 532 nm is used as a pump. A source is injected into a nonlinear optical crystal 3 of Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2 to generate a frequency-doubled light with a wavelength of 266 nm. The output beam 4 contains the frequency-doubled light with wavelengths of 532 nm and 266 nm, which is filtered out by a filter 5 to obtain a laser with a wavelength of 266 nm.
[0144] Example 22
[0145] Any Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2 nonlinear optical crystal obtained in Examples 1-19 is processed into a single crystal device after directional cutting and polishing. A 1064nm Nd:YAG Q-switched laser light source is used as a pump source to generate a laser output with a wavelength shorter than 266nm.
Claims
1. A series of fluorine-containing rare earth borate compounds, characterized in that: The molecular formula of this series of fluorine-containing rare earth borate compounds is A2REB3O6F2, wherein A=Rb, Cs, NH4; RE=Sc, Y, La, and their molecular formulas are Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2, with molecular weights of 247.46-571.
14.
2. The method for preparing a series of fluorine-containing rare earth borate compounds according to claim 1, characterized in that: The product was prepared by solid phase reaction method and hydrothermal method.
3. The series of fluorine-containing rare earth borate compounds according to claim 2 are prepared by a solid phase reaction method, characterized in that: The following steps are involved: A compound containing A = Rb, Cs, NH4, a compound containing RE = Sc, Y, La, a boron-containing compound, and a fluorine-containing compound are mixed, wherein the molar ratio of the element A in the A-containing compound, the element RE in the RE-containing compound, the element boron in the boron-containing compound, and the element fluorine in the fluorine-containing compound is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2; then the raw materials of the A-containing compound, the RE-containing compound, the boron-containing compound, and the fluorine-containing compound are uniformly mixed, ground, and put into a muffle furnace, pre-burned to remove moisture and gas in the raw materials, cooled to room temperature, taken out, ground, and put into a muffle furnace for calcination to obtain a series of single-phase polycrystalline powders of fluorine-containing rare earth borate compounds. The hydrothermal method for preparing a series of fluorine-containing rare earth borate compounds is characterized by comprising the following steps: A compound containing A = Rb, Cs, NH4, a compound containing RE = Sc, Y, La, a boron-containing compound and a fluorine-containing compound are added to the polytetrafluoroethylene lining of a high-pressure reactor, and then deionized water and a mineralizer are added to mix them thoroughly and evenly to obtain a mixed solution, and the high-pressure reactor is placed in a constant temperature box for heating, and then cooled to room temperature, and the solution containing powder is filtered to obtain a series of single-phase polycrystalline powders of fluorine-containing rare earth borate compounds; wherein the molar ratio of element A in the A-containing compound, element RE in the RE-containing compound, element boron in the boron-containing compound, and element fluorine in the fluorine-containing compound is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.
2. The compound containing A=Rb, Cs, NH4 includes at least one of AOH, A2O, and alkali metal salts, and the alkali metal salts include at least one of AF, ACl, ABr, ANO3, A2C2O2, A2CO3, AHCO3, and A2SO4, wherein A=Rb, Cs, NH4; The compounds containing RE=Sc, Y, La include RE2O3, REF3, and RE(NO3)3·6H2O; The boron-containing compound includes at least one of B2O3, H3BO3 and borates; borates include at least one of ABO2, ABO3, A3BO3, A2B4O7, wherein A=Rb, Cs, NH4; The fluorine-containing compounds include AF, REF3, wherein A=Rb, Cs, NH4; RE=Sc, Y, La, and others The fluorine-containing compound includes at least one of KBF4, NaBF4, KPF6, and NH4PF6.
4. A series of fluorine-containing rare earth borate nonlinear optical crystals, characterized by The chemical formula of this series of crystals is A2REB3O6F2, where A=Rb, Cs, NH4, RE=Sc, Y, La, and the molecular formulas are Rb2ScB3O6F2, Cs2ScB3O6F2, (NH4)2ScB3O6F2, Rb2YB3O6F2, Cs2YB3O6F2, (NH4)2YB3O6F2, Rb2LaB3O6F2, Cs2LaB3O6F2 or (NH4)2LaB3O6F2, all of which crystallize in the orthorhombic system, with space group Amm2 and unit cell parameters. Z=2.
5. The method for preparing the fluorine-containing rare earth borate nonlinear optical crystal according to claim 4, characterized in that: High temperature melt method, hydrothermal method and solution method were used to grow fluorine-containing rare earth borate nonlinear optical crystals.
6. The method for preparing a series of fluorine-containing rare earth borate nonlinear optical crystals according to claim 5, characterized in that: The high-temperature melt method is used to grow a series of fluorine-containing rare earth borate nonlinear optical crystals A2REB3O6F2, wherein A=Rb, Cs, NH4, RE=Sc, Y, La, and the specific operation is as follows: a single-phase polycrystalline powder of a series of fluorine-containing rare earth borate compounds or a mixture of a single-phase polycrystalline powder of a series of fluorine-containing rare earth borate compounds and a flux, or a mixture of an A-containing compound, an RE-containing compound, a boron-containing compound and a fluorine-containing compound or a mixture of an A-containing compound, an RE-containing compound, a boron-containing compound and a fluorine-containing compound and a flux, is heated to melt to obtain a mixed melt; then a crucible containing the mixed melt is placed in a crystal growth furnace for heating, and the temperature is lowered to a saturation temperature point, at which time a seed crystal rod is extended below the liquid surface, and then the seed crystal rod is lifted out of the liquid surface before the melt solidifies, to prepare a series of fluorine-containing rare earth borate nonlinear optical crystals; The hydrothermal method for growing a series of fluorine-containing rare earth borate nonlinear optical crystals A2REB3O6F2, wherein A=Rb, Cs, NH4, RE=Sc, Y, La, is specifically performed as follows: adding a single-phase polycrystalline powder of a series of fluorine-containing rare earth borate compounds or a mixture of a single-phase polycrystalline powder of a series of fluorine-containing rare earth borate compounds and a mineralizer, or directly adding a mixture of an A-containing compound, an RE-containing compound, a boron-containing compound and a fluorine-containing compound or a mixture of an A-containing compound, an RE-containing compound, a boron-containing compound and a fluorine-containing compound and a mineralizer to the polytetrafluoroethylene lining of an autoclave, and then adding deionized water to mix them thoroughly to obtain a mixed solution. The polytetrafluoroethylene lining is placed in an autoclave, and the autoclave is placed in a thermostat for heating, and then cooled to room temperature, and the solution containing the crystal is filtered to obtain a transparent series of fluorine-containing rare earth borate nonlinear optical crystals; The solution method grows a series of fluorine-containing rare earth borate nonlinear optical crystals A2REB3O6F2, wherein A=Rb, Cs, NH4, RE = Sc, Y, La, the specific operation is as follows: add a series of single-phase polycrystalline powders of fluorine-containing rare earth borate compounds or a mixture of a series of single-phase polycrystalline powders of fluorine-containing rare earth borate compounds and a solvent, or directly add a mixture of A-containing compounds, RE-containing compounds, boron-containing compounds and fluorine-containing compounds or a mixture of A-containing compounds, RE-containing compounds, boron-containing compounds and fluorine-containing compounds and a solvent into a beaker; then add deionized water to dissolve, and stir the solution until it is clear. Then place the beaker in the air, evaporate the solution, and grow a series of fluorine-containing rare earth borate nonlinear optical crystals.
7. The method for preparing a series of fluorine-containing rare earth borate nonlinear optical crystals according to claim 6, characterized in that: The high-temperature melt method is used to grow a series of fluorine-containing rare earth borate nonlinear optical crystals, wherein the molar ratio of the single-phase polycrystalline powder of the series of fluorine-containing rare earth borate compounds to the flux is 1:0-50; or the molar ratio of the element A in the compound containing A=Rb, Cs, NH4, the element RE in the compound containing RE=Sc, Y, La, the element boron in the boron-containing compound, and the element fluorine in the fluorine-containing compound to the flux is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2:0- 50; wherein the flux comprises alkali metal salts, namely alkali metal carbonates, alkali metal nitrates, alkali metal sulfates, alkali metal oxalates, alkali metal borates, alkali metal phosphates, alkali metal halides, alkali metal fluoroborates, alkali metal metaborate, and alkali metal oxides, alkali metal hydroxides, and one or more of yttrium fluoride, yttrium nitrate, yttrium oxide, lanthanum fluoride, lanthanum nitrate, lanthanum oxide, scandium fluoride, scandium nitrate, scandium oxide, boron oxide, boric acid, phosphoric acid, lead oxide, lead fluoride, molybdenum oxide, and bismuth oxide; The hydrothermal method is used to grow a series of fluorine-containing rare earth borate nonlinear optical crystals, wherein the molar ratio of the single-phase polycrystalline powder of the series of fluorine-containing rare earth borate compounds to the mineralizer is 1:0-30; or the molar ratio of the element A in the compound containing A=Rb, Cs, NH4, the element RE in the compound containing RE=Sc, Y, La, the element boron in the boron-containing compound, and the element fluorine in the fluorine-containing compound to the mineralizer is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2:0- 30; the mineralizer includes at least one or more of AOH, A2O, AF, ACl, ABr, ABF4, A3PO4, A3BO3, ANO3, A2C2O4, A2CO3, AHCO3, A2SO4, Y(NO3)3·6H2O, La(NO3)3·6H2O, Sc(NO3)3·6H2O, B2O3, KBF4, NaBF4, KPF6, NH4PF6, wherein A=Rb, Cs, NH4; The aqueous solution method grows a series of fluorine-containing rare earth borate nonlinear optical crystals, wherein the molar ratio of the single-phase polycrystalline powder of the series of fluorine-containing rare earth borate compounds to the auxiliary solvent is 1:0-20; or the molar ratio of the element A in the A-containing compound, the element RE in the RE-containing compound, the element boron in the boron-containing compound and the element fluorine in the fluorine-containing compound to the auxiliary solvent is 1.5-2.2:0.8-1.5:2.5-3.5:1.5-2.2:0-20; the auxiliary solvent includes AOH, A2O, AF, ACl, ABr, At least one or more of ABF4, A3PO4, A3BO3, ANO3, A2C2O4, A2CO3, AHCO3, A2SO4, A2HPO4, AH2PO4, Y(NO3)3·6H2O, La(NO3)3·6H2O, Sc(NO3)3·6H2O, B2O3, KBF4, NaBF4, KPF6, NH4PF6, wherein A=Rb, Cs, NH4; 8. A nonlinear optical device comprising means for generating at least one output radiation having a frequency different from that of the incident electromagnetic radiation after passing at least one incident electromagnetic radiation through at least one nonlinear optical crystal, characterized in that: The nonlinear optical crystal is the series of fluorine-containing rare earth borate nonlinear optical crystal A2REB3O6F2, where A=Rb, Cs, NH4, RE=Sc, Y, La.
9. The series of fluorine-containing rare earth borate nonlinear optical crystals according to claim 4 are used to prepare multi-band frequency doubling devices or optical elements.
10. The use of a series of fluorine-containing rare earth borate nonlinear optical crystals according to claim 4, characterized in that: This series of fluorine-containing rare earth borate nonlinear optical crystals are used in nonlinear optical devices such as second harmonic generators, up and down frequency converters, optical parametric oscillators, laser frequency conversion devices, laser communications, etc.
Citation Information
Patent Citations
Fluoborate and crystal containing rare earth ions, growing method and application of crystal
CN101514489A
Compound ammonium borofluoride, ammonium borofluoride non-linear optic crystal and preparation methods and application thereof
CN106745022A
Compound rubidium borofluoride and rubidium borofluoride non-linear optical crystal and preparation method and use of rubidium borofluoride non-linear optical crystal
CN107265473A
Rare earth doped barium calcium fluoborate laser crystal, preparation method thereof and method for realizing laser
CN112144119A
Scandium rubidium lithium fluosilicate nonlinear optical crystal and preparation method and application thereof
CN115198343A
Cited By
Compound guanidine fluoroborate, guanidine fluoroborate nonlinear optical crystal, and preparation method and application of compound guanidine fluoroborate nonlinear optical crystal
CN119824547A