High-flexibility rubber heat vulcanization adhesive, and fabrication process and use method therefor

By rationally configuring resins and solvents in the production process of rubber thermal vulcanization adhesives, a highly flexible rubber thermal vulcanization adhesive is prepared, which solves the problem of insufficient brittleness of existing rubber vulcanization primers and achieves high efficiency in the automotive industry. , stable bonding effect.

WO2024198111A1PCT designated stage expired Publication Date: 2024-10-03LIYANG BORLIN NEW MATERIALS TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/100989
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2023-06-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing rubber vulcanized primers are highly brittle and cannot meet the automotive industry's needs for high flexibility, temperature and moisture resistance, and anti-corrosion properties. As a result, edge debonding or detachment is prone to occur during the deformation process of metal parts, affecting production efficiency and products. quality.

Method used

Using the production process of high-flexibility rubber hot vulcanization adhesive, by rationally configuring epoxy resin, thermal curing agent, softening resin, resin solvent and acid scavenger, and performing multi-step dissolving and stirring processes, a super-resistant adhesive is prepared. Polar rubber thermally vulcanized adhesive with high flexibility and good adhesion for thermoform bonding on metal parts.

Benefits of technology

It improves the flexibility and adhesion of the adhesive, reduces the rate of defective products, improves production efficiency and customer satisfaction, and meets the needs of high-flexibility application scenarios, especially during the bending and stretching processes of metal parts. Maintain stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023100989_03102024_PF_FP_ABST
    Figure CN2023100989_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a high-flexibility rubber heat vulcanization adhesive, and a fabrication process and a use method therefor. The fabrication process comprises: based on a first dissolution treatment parameter, carrying out a first high-temperature dissolution treatment by using an epoxy resin, a resin solvent and an acid scavenger, so as to obtain a first epoxy resin solution; based on a second dissolution treatment parameter, carrying out a second high-temperature dissolution treatment by using a softened resin, the resin solvent and the acid scavenger, so as to obtain a second softened resin solution; based on a third stirring treatment parameter, carrying out a third mixing and stirring treatment by using a thermal curing agent, an acid scavenger, the first epoxy resin solution and the second softened resin solution, so as to obtain a third mixed and stirred product; and based on a fourth stirring treatment parameter, carrying out a fourth grinding and stirring treatment by using the resin solvent and the third stirred product, so as to obtain a polar rubber heat vulcanization adhesive. In the present invention, a unique rubber resin can be selected and used in the process, and strictly added in an appropriate amount, such that an adhesive having ultrahigh flexibility and adhesive force is produced.
Need to check novelty before this filing date? Find Prior Art

Description

Highly flexible rubber hot-vulcanized adhesive, production process and use method Technical Field

[0001] The present invention relates to the technical field of adhesive materials. Specifically, the present invention is applied to the field of automotive metal parts adhesive materials, and in particular relates to a highly flexible rubber hot-vulcanized adhesive, a production process and a use method. Background Art

[0002] At present, in the automotive sealing strip industry, the international market for automotive exterior sealing strips and automotive sunroof sealing strips mainly uses rubber such as EPDM and thermoplastic vulcanized rubber as the main sound-absorbing and noise-reducing materials. The rubber is bonded to the metal skeleton of the sealing strip during the extrusion process. In order to improve production efficiency and be able to coat the metal skeleton in an environment that meets environmental protection requirements, a coil coating machine is generally used to apply the adhesive to a metal coil of suitable thickness. The metal coil is then cut, rolled, stretched, and deformed to form the skeleton of the sealing strip, which is then hot-extruded and bonded with the corresponding rubber. Therefore, the metal coil coated with the adhesive will deform during the cutting, stretching, and bending processes. If the flexibility and adhesion of the primer directly attached to it do not meet the requirements, results such as edge debonding or even the entire adhesive detachment will occur. Therefore, under the aforementioned development background, the application of the primer in the automotive industry requires it to have excellent flexibility, temperature and moisture resistance, and higher corrosion resistance.

[0003] In the prior art, the common rubber vulcanized primer on the market is mainly used for automobile shock absorbing components and anti-seismic isolation components. It is a general product with good adhesion to metal. In this application direction, it mostly involves hard bonding between two hard parts. The bonding process is carried out after the two bonded parts are produced and processed. The application direction basically does not involve deformation, so there is no requirement for the flexibility of the product. Therefore, the adhesive in the prior art mainly uses phenolic formaldehyde as the main resin. However, due to the high brittleness of phenolic formaldehyde resin, this type of general primer is very brittle and cannot fully meet customer needs. When applied, customers are also required to adjust the process on their own production lines and lower the baking temperature, sacrificing the best performance conditions to barely increase flexibility. The final result is that the T-bend of the product fluctuates unstably between T2 and T4, resulting in defective products often appearing during the deformation and shearing production and processing;

[0004] In summary, the current rubber vulcanization primer is highly brittle and cannot meet customer needs. During secondary processing, it often leads to varying quality problems in the products, affecting the production and processing progress, increasing production and processing costs, and reducing the applicability and performance indicators of the rubber vulcanization primer. Summary of the Invention

[0005] The purpose of the present invention is to provide a highly flexible rubber hot-vulcanized adhesive, a production process and a method of use in response to the above-mentioned problems in the prior art, thereby solving the problem that the rubber vulcanized primer in the prior art is highly brittle and can only meet the needs of hard bonding. Its strong brittleness makes it only applicable to two bonding parts with low flexibility requirements after production processing. The application direction is narrow and cannot meet customer needs. During secondary processing, it often leads to uneven quality problems in the product, affecting the production and processing progress, increasing production and processing costs, and reducing the applicability and performance indicators of the rubber vulcanized primer.

[0006] In order to solve the above technical problems, the specific technical solutions of the present invention are as follows:

[0007] In one aspect, the present invention provides a process for preparing a highly flexible rubber heat-vulcanized adhesive, comprising the following steps:

[0008] Raw materials and parameter configuration steps:

[0009] preparing epoxy resin, a thermal curing agent, a softening resin, a resin solvent, and an acid scavenger; and setting a first dissolution processing parameter, a second dissolution processing parameter, a third stirring processing parameter, and a fourth stirring processing parameter;

[0010] Resin solution preparation steps:

[0011] Based on the first dissolution treatment parameters, a first high-temperature dissolution treatment is performed using the epoxy resin, the resin solvent, and the acid scavenger to obtain a first epoxy resin solution;

[0012] Based on the second dissolution treatment parameters, a second high-temperature dissolution treatment is performed using the softening resin, the resin solvent, and the acid scavenger to obtain a second softening resin solution;

[0013] Mixing process steps:

[0014] Based on the third stirring process parameters, a third mixing and stirring process is performed using the thermal curing agent, the acid scavenger, the first epoxy resin solution, and the second softening resin solution to obtain a third mixing and stirring product;

[0015] Based on the fourth stirring process parameters, a fourth grinding and stirring process is performed using the resin solvent and the third stirring product to obtain a polar rubber heat-vulcanized adhesive.

[0016] As an improved solution, the first dissolution processing parameters include: a first initial speed interval, a first intermediate speed interval, a first final speed interval, a first initial time length, and a first final time length;

[0017] The first high-temperature dissolution treatment comprises:

[0018] Setting up a first reactor;

[0019] adding the resin solvent and the acid scavenger into the first reactor, and stirring the resin solvent and the acid scavenger in the first reactor according to the first initial velocity range;

[0020] While stirring the resin solvent and the acid scavenger in the first reaction kettle, adding the epoxy resin into the first reaction kettle;

[0021] After adding the epoxy resin, stirring the resin solvent, the acid scavenger, and the epoxy resin in the first reaction kettle according to the first intermediate speed range and the first primary time to obtain an initial epoxy resin solution;

[0022] After obtaining the initial epoxy resin solution, the resin solvent and the acid scavenger are added to the first reactor, and the initial epoxy resin solution, the resin solvent, and the acid scavenger in the first reactor are stirred according to the first final-stage speed range and the first final-stage time to obtain the first epoxy resin solution.

[0023] As an improved solution, the second dissolution processing parameters include: a second initial speed interval, a second intermediate speed interval, a second final speed interval, a second initial time length, and a second final time length;

[0024] The second high-temperature dissolution treatment includes:

[0025] Setting up a second reactor;

[0026] adding the resin solvent and the acid scavenger into the second reaction kettle, and stirring the resin solvent and the acid scavenger in the second reaction kettle according to the second primary speed range;

[0027] While the resin solvent and the acid scavenger are being stirred in the second reaction kettle, the softening resin is added to the second reaction kettle;

[0028] After adding the softening resin, stirring the resin solvent, the acid scavenger and the softening resin in the second reactor according to the second intermediate speed range and the second primary time to obtain an initial softening resin solution;

[0029] After obtaining the initial softening resin solution, the resin solvent and the acid scavenger are added to the second reactor, and the initial softening resin solution, the resin solvent and the acid scavenger in the second reactor are stirred according to the second final stage speed range and the second final stage time to obtain the second softening resin solution.

[0030] As an improved solution, the third stirring processing parameters include: a third temperature threshold, a third initial speed interval, a third final speed interval, a third initial time length, and a third final time length;

[0031] The third mixing and stirring process comprises:

[0032] Acquiring a room temperature, detecting a first temperature of the first initial epoxy resin solution in the first reactor, and when the first temperature reaches the room temperature, performing a first stirring step based on the second softening resin solution, the third initial speed range, and the third initial time to obtain a first stirring product;

[0033] A second stirring step is performed based on the first stirring product, the thermal curing agent, the acid scavenger, the third temperature threshold, the third final speed range and the third final time to obtain the third mixed stirring product.

[0034] As an improved solution, the first stirring step includes:

[0035] adding the second softening resin solution in the second reactor into the first reactor;

[0036] The first initial epoxy resin solution and the second softening resin solution in the first reactor are stirred according to the third initial speed range and the third initial time to obtain the first stirring product.

[0037] As an improved solution, the second stirring step includes:

[0038] Slowly adding the thermal curing agent and the acid scavenger into the first reaction kettle;

[0039] Detecting the second temperature of the compound in the first reactor, and when the second temperature is not higher than the third mixed stirring product, stirring the first stirring product, the thermal curing agent and the acid scavenger in the first reactor according to the third final speed range and the third final time to obtain the third mixed stirring product.

[0040] As an improved solution, the fourth stirring processing parameters include: a fourth temperature threshold, a fourth grinding time, a fourth grinding fineness and a fourth initial speed range;

[0041] The fourth grinding and stirring process comprises:

[0042] Grinding the third mixed product according to the fourth temperature threshold and the fourth grinding time;

[0043] When grinding the third mixed product, if the first fineness of the third mixed product is lower than the fourth grinding fineness, a first ground product is obtained;

[0044] The first ground product and the resin solvent are stirred in the fourth primary speed range to obtain the polar rubber heat-vulcanized adhesive.

[0045] On the other hand, the present invention also provides a highly flexible rubber hot-vulcanized adhesive, which is made based on a manufacturing process for a highly flexible rubber hot-vulcanized adhesive. The polar rubber hot-vulcanized adhesive is composed of an epoxy resin, a thermal curing agent, a flexibilizing resin, a resin solvent, and an acid scavenger.

[0046] The epoxy resin accounts for 5% to 30% of the adhesive by mass;

[0047] The thermal curing agent accounts for 5% to 20% of the mass of the adhesive;

[0048] The softening resin accounts for 0.5% to 15% of the mass of the adhesive;

[0049] The resin solvent accounts for 40% to 80% of the adhesive by mass;

[0050] The acid scavenger accounts for 1% to 20% of the mass of the adhesive.

[0051] As an improved solution, the epoxy resin includes: one or more of bisphenol A resin and bisphenol F resin;

[0052] The thermal curing agent includes: phenolic resin;

[0053] The softening resin includes: rubber resin;

[0054] The resin solvent includes: one or more of xylene and methyl isobutyl ketone;

[0055] The acid scavenger includes one or more of metal stearates and metal oxides, and the metal oxides include one or more of zinc oxide, magnesium oxide and aluminum oxide.

[0056] On the other hand, the present invention also provides a method for using a highly flexible rubber heat-vulcanized adhesive, comprising the following steps:

[0057] applying the polar rubber heat-vulcanized adhesive to a substrate;

[0058] Drying the coated substrate;

[0059] Performing deformation processing on the dried substrate, wherein the deformation processing includes one or more of bending processing, stamping deformation processing and stretching processing;

[0060] The mixture to be bonded is thermoformed on the substrate after the deformation process, and while the mixture to be bonded is thermoformed, a bonding reaction occurs with the polar rubber hot vulcanizing adhesive coated on the surface of the substrate; the thermoforming includes: hot pressing, hot extrusion or injection molding.

[0061] The beneficial effects of the technical solution of the present invention are:

[0062] 1. The manufacturing process of the highly flexible rubber heat-vulcanized adhesive described in the present invention can realize the selection of a unique rubber resin in the process and strictly add it in an appropriate amount, thereby producing an adhesive with ultra-high flexibility and at the same time enabling the adhesive to have good adhesion. The manufacturing process of the highly flexible rubber heat-vulcanized adhesive described in the present invention, through a unique manufacturing method, produces an adhesive with higher quality performance, helps customers improve production yield, enhance customer satisfaction and production efficiency, and helps customers save production costs.

[0063] 2. The high-flexibility rubber hot-vulcanizing adhesive described in the present invention can achieve the performance of the polar rubber hot-vulcanizing adhesive itself without reducing it under the customer's process conditions, ensuring ultra-high flexibility and good adhesion, and thus improving the yield of the customer's products without changing the customer's process, meeting the customer's highest requirements. After experiments, the high-flexibility rubber hot-vulcanizing adhesive described in the present invention has a flexibility improved from T3 to T0 compared with the primer in the prior art, effectively solving the quality problems that customers often encounter during the metal coil forming process, such as primer shedding and rubber bubbles; further, the high-flexibility rubber hot-vulcanizing adhesive described in the present invention can be used in combination with the topcoat currently being used by the customer without changing the customer's existing process and the use of other auxiliary materials. The high-flexibility rubber hot-vulcanizing adhesive described in the present invention has excellent durability and applicability, which is beneficial to improving the customer's production efficiency and reducing the customer's production cost.

[0064] 3. The method for using the highly flexible rubber hot-vulcanized adhesive of the present invention allows the adhesive to be applied to metal parts and to accompany the metal parts in deformation actions such as bending and stretching with high flexibility. Based on the characteristics of this rubber hot-vulcanized adhesive, it can be used in application scenarios requiring high flexibility, especially when facing the bonding needs between hard and soft parts, such as the bonding between metal parts and rubber parts. During the rubber part production, injection molding, hot pressing and other thermal processing production processes, the thermal effect can be used to simultaneously complete the product bonding process, thereby achieving a highly efficient, low-cost and highly stable bonding operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0066] FIG1 is a schematic flow chart of a process for producing a highly flexible rubber heat-vulcanized adhesive according to Example 1 of the present invention;

[0067] FIG2 is a schematic diagram of a detailed process for preparing the highly flexible rubber heat-vulcanized adhesive according to Example 1 of the present invention;

[0068] FIG3 is a flow chart of a method for using the highly flexible rubber heat-vulcanized adhesive according to Example 3 of the present invention. DETAILED DESCRIPTION

[0069] The preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more precise definition of the protection scope of the present invention.

[0070] In the description of the present invention, it should be noted that the embodiments described in the present invention are only part of the embodiments of the present invention, rather than all of the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work are within the scope of protection of the present invention.

[0071] The terms "first," "second," and the like in the specification and claims herein and in the accompanying drawings are used to distinguish similar objects and are not necessarily used to describe a particular order or precedence. It should be understood that the terms used in this manner are interchangeable where appropriate so that the embodiments of the present invention described herein can be implemented in orders other than those illustrated or described herein. In addition, the terms "including" and "having," and any variations thereof, are intended to cover non-exclusive inclusions. For example, a process, method, apparatus, product, or device comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such process, method, product, or device. Example 1

[0072] This embodiment provides a process for producing a highly flexible rubber hot-vulcanized adhesive, as shown in FIG1 and FIG2 , comprising the following steps:

[0073] S100, raw materials and parameter configuration steps, specifically including:

[0074] S110, preparing epoxy resin, thermal curing agent, softening resin, resin solvent and acid scavenger; setting a first dissolution processing parameter, a second dissolution processing parameter, a third stirring processing parameter and a fourth stirring processing parameter;

[0075] S200, resin solution preparation step, specifically comprising:

[0076] S210, performing a first high-temperature dissolution treatment based on the first dissolution treatment parameters and using the epoxy resin, the resin solvent, and the acid scavenger to obtain a first epoxy resin solution;

[0077] S220, performing a second high-temperature dissolution treatment based on the second dissolution treatment parameters and using the softening resin, the resin solvent, and the acid scavenger to obtain a second softening resin solution;

[0078] S300, stirring treatment step, specifically including:

[0079] S310: performing a third mixing and stirring process based on the third stirring process parameters and using the thermal curing agent, the acid scavenger, the first epoxy resin solution, and the second softening resin solution to obtain a third mixing and stirring product;

[0080] S320 , performing a fourth grinding and stirring process based on the fourth stirring process parameters and using the resin solvent and the third stirring product to obtain a polar rubber heat-vulcanized adhesive.

[0081] As an embodiment of the present invention, the first dissolution processing parameters include: a first initial speed range, a first intermediate speed range, a first final speed range, a first initial time, and a first final time. In this embodiment, the first initial speed range is 300-600 rpm, the first intermediate speed range is 1000-1500 rpm, and the first final speed range is 300-600 rpm; the first initial time is 3-4 hours; and the first final time is 15 minutes.

[0082] As an embodiment of the present invention, the first high-temperature dissolution treatment includes: setting up a first reactor; adding the resin solvent and the acid scavenger into the first reactor, and stirring the resin solvent and the acid scavenger in the first reactor according to the first initial speed range; while stirring the resin solvent and the acid scavenger in the first reactor, adding the epoxy resin into the first reactor; after adding the epoxy resin, stirring the resin solvent, the acid scavenger and the epoxy resin in the first reactor according to the first intermediate speed range and the first initial time length to obtain an initial epoxy resin solution; after obtaining the initial epoxy resin solution, adding the resin solvent and the acid scavenger into the first reactor, and stirring the initial epoxy resin solution, the resin solvent and the acid scavenger in the first reactor according to the first final speed range and the first final time length to obtain the final epoxy resin solution. An epoxy resin solution; in this embodiment, the first high-temperature dissolution treatment, when actually applied, includes, as an example, the following steps: adding a certain amount of the resin solvent and the acid scavenger to a first reactor, and slowly stirring the compounds in the first reactor using a high-speed stirrer at a speed of 300-600 rpm; adding the epoxy resin while stirring in the high-speed stirrer, and then increasing the stirring speed to 1000-1500 rpm to dissolve the epoxy resin, at which time the temperature of the first reactor gradually rises to approximately 60 degrees Celsius due to frictional heat; after stirring for approximately 3-4 hours, the epoxy resin is completely dissolved, and an initial epoxy resin solution is obtained; thereafter, the solvent lost during the dissolution process, i.e., the resin solvent and the acid scavenger, is replenished into the first reactor and stirred again at a speed of 300-600 rpm for 15 minutes until the solution is completely uniform, thereby obtaining an epoxy resin solution (i.e., a first epoxy resin solution);

[0083] As an embodiment of the present invention, the second dissolution treatment parameters include: a second initial speed interval, a second intermediate speed interval, a second final speed interval, a second initial time, and a second final time. In this embodiment, the second initial speed interval is 300-600 rpm, the second intermediate speed interval is a second intermediate speed interval, and the second final speed interval is 300-600 rpm; the second initial time is 5-6 hours; and the second final time is 15 minutes.

[0084] As an embodiment of the present invention, the second high-temperature dissolution treatment includes: setting up a second reactor; adding the resin solvent and the acid scavenger into the second reactor, and stirring the resin solvent and the acid scavenger in the second reactor according to the second initial speed range; while stirring the resin solvent and the acid scavenger in the second reactor, adding the softening resin into the second reactor; after adding the softening resin, stirring the resin solvent, the acid scavenger and the softening resin in the second reactor according to the second intermediate speed range and the second initial time length to obtain an initial softening resin solution; after obtaining the initial softening resin solution, adding the resin solvent and the acid scavenger into the second reactor, and stirring the initial softening resin solution, the resin solvent and the acid scavenger in the second reactor according to the second final speed range and the second final time length. The second softening resin solution is obtained; in this embodiment, when the second high-temperature dissolution treatment is actually applied, as an example, it includes the following steps: adding a certain amount of the resin solvent and the acid scavenger to a new second reactor, using a high-speed stirrer to slowly stir, and the speed is maintained at 300-600rpm, adding the softening resin during the stirring process of the high-speed stirrer, and then increasing the stirring speed to 1500-3000rpm to dissolve the softening resin. During this process, the temperature of the second reactor will rise to about 60 degrees due to frictional heat; after stirring for about 5-6 hours, the softening resin is completely dissolved, and the initial softening resin solution is obtained at this time; then the solvent lost in the dissolution process, that is, the resin solvent and the acid scavenger, are added to the second reactor and stirred evenly, the stirring speed is 300-600rpm, and stirred for 15 minutes until the solution is completely uniform, and finally a rubber resin solution (that is, the second softening resin solution) is obtained;

[0085] As an embodiment of the present invention, the third stirring process parameters include: a third temperature threshold, a third initial speed range, a third final speed range, a third initial time, and a third final time. In this embodiment, the third temperature threshold is 55 degrees Celsius, the third initial speed range is 300-600 rpm, the third final speed range is 800-1000 rpm, the third initial time is 30 minutes, and the third final time is 1 hour.

[0086] As an embodiment of the present invention, the third mixing and stirring process includes: obtaining room temperature, detecting the first temperature of the first initial epoxy resin solution in the first reactor, and when the first temperature reaches the room temperature, performing a first stirring step based on the second softening resin solution, the third initial speed interval and the third initial time to obtain a first stirring product; performing a second stirring step based on the first stirring product, the thermal curing agent, the acid scavenger, the third temperature threshold, the third final speed interval and the third final time to obtain the third mixing and stirring product; specifically, in this embodiment, the room temperature is the current room temperature when the process is applied, and the first temperature is the real-time temperature of the first initial epoxy resin solution in the first reactor. When the first temperature reaches room temperature, it indicates that the first initial epoxy resin solution in the first reactor has cooled to meet the subsequent processing conditions, so the first initial epoxy resin solution and the second softening resin solution can be subjected to preliminary stirring treatment (i.e., the first stirring step); after the preliminary stirring treatment, the stirred product and part of the pre-prepared raw material compound need to be further stirred (i.e., the second stirring step) to obtain the third mixed stirring product before the adhesive product is prepared;

[0087] As an embodiment of the present invention, the first stirring step includes: adding the second softening resin solution in the second reactor to the first reactor; stirring the first initial epoxy resin solution and the second softening resin solution in the first reactor according to the third initial speed range and the third initial time to obtain the first stirring product; in this embodiment, when the first stirring step is actually applied, as an example, it includes the following steps: after the aforementioned first epoxy resin solution is cooled to room temperature, the second softening resin solution prepared in the second reactor is slowly added to the first reactor, the high-speed stirrer is reopened, and the stirring speed is 300-600rpm, and the mixing and stirring are carried out for about 30 minutes until the two are evenly mixed to obtain the first stirring product;

[0088] As an embodiment of the present invention, the second stirring step includes: slowly adding the thermal curing agent and the acid scavenger to the first reactor; detecting a second temperature of the compound in the first reactor, and when the second temperature is not higher than the third mixed stirring product, stirring the first stirred product, the thermal curing agent, and the acid scavenger in the first reactor according to the third final speed range and the third final time to obtain the third mixed stirring product; in this embodiment, when the second stirring step is actually applied, as an example, it includes the following steps: continuing to turn on the high-speed stirrer for the first reactor at a stirring speed of 800-1000 rpm, and then slowly and sequentially adding the thermal curing agent and the acid scavenger in proportion to the first stirred product solution in the first reactor, stirring for 1 hour until the filler in the first reactor is evenly dispersed; during this stirring process, it is necessary to pay attention to the temperature change of the compound in the first reactor to ensure that the temperature of the compound in the first reactor does not exceed 55 degrees Celsius; correspondingly, in this embodiment, in order to prepare a colored adhesive, a pigment set as required is also added when the thermal curing agent and the acid scavenger are added to the first reactor in this step;

[0089] As an embodiment of the present invention, the fourth stirring process parameters include: a fourth temperature threshold, a fourth grinding time, a fourth grinding fineness, and a fourth initial speed range; in this embodiment, the fourth temperature threshold is 55 degrees Celsius, the fourth grinding time is 4-5 hours, the fourth grinding fineness is 25 µm, and the fourth initial speed range is 300-600 rpm;

[0090] As an embodiment of the present invention, the fourth grinding and stirring treatment includes: grinding the third mixed stirring product according to the fourth temperature threshold and the fourth grinding time; when grinding the third mixed stirring product, if the first fineness of the third mixed stirring product is lower than the fourth grinding fineness, a first ground product is obtained; the first ground product and the resin solvent are stirred according to the fourth initial speed range to obtain the polar rubber hot vulcanized adhesive; in this embodiment, when the fourth grinding and stirring treatment is actually applied, as an example, it includes the following steps: using a vertical or horizontal grinder to grind the third mixed stirring product to a fine The particle size is less than 25 μm; the grinding time is usually 4-5 hours, and during the grinding process, attention should also be paid to the temperature change in the grinding cylinder to ensure that the temperature does not exceed 55 degrees Celsius; after grinding to a fineness of less than 25 μm, a first ground product is obtained; the partially ground first ground product is then stirred again using a high-speed stirrer at a stirring speed of 300-600 rpm, and the remaining resin solvent is added during the stirring process to finally complete the flexible primer, that is, the preparation of the polar rubber hot vulcanization adhesive; correspondingly, in actual operation, the polar rubber hot vulcanization adhesive of the present invention needs to be filtered using a nylon filter with a fineness of 25 μm before canning. Example 2

[0091] This embodiment provides a highly flexible rubber hot-vulcanized adhesive prepared by the preparation process of the highly flexible rubber hot-vulcanized adhesive described in Example 1, wherein the polar rubber hot-vulcanized adhesive comprises an epoxy resin, a heat curing agent, a flexibilizing resin, a resin solvent, and an acid scavenger;

[0092] As one embodiment of the present invention, in order to better meet the high-temperature and high-speed production conditions of the pre-coating process, a typical bisphenol A or bisphenol F epoxy resin is selected as the main resin. Because bisphenol A and F epoxy resins have excellent performance after curing, strong adhesion to metal, excellent chemical corrosion resistance and good flexibility, in this embodiment, in order to achieve good flexibility, a unique ratio is adopted, and the total mass ratio of bisphenol A and F epoxy to the polar rubber hot-vulcanized adhesive is set to 5-30%. Therefore, in this embodiment, the epoxy resin includes: one or more of bisphenol A resin and bisphenol F resin, and the epoxy resin accounts for 5% to 30% of the adhesive by mass;

[0093] As an embodiment of the present invention, in order to achieve better corrosion resistance, phenolic resin is used as a thermal curing agent for bisphenol A and F-type epoxy resin in the formulation of the polar rubber heat-vulcanized adhesive of the present invention. After the phenolic resin and the epoxy resin are cured and cross-linked, high flexibility of the paint film and very perfect corrosion resistance can be achieved. Therefore, in this embodiment, a unique ratio is adopted, and the phenolic resin accounts for 5% to 20% of the total mass of the polar rubber heat-vulcanized adhesive. Therefore, in this embodiment, the thermal curing agent includes: phenolic resin; the thermal curing agent accounts for 5% to 20% of the mass of the adhesive;

[0094] As an embodiment of the present invention, in order to further improve the flexibility of the product, a rubber resin is used as a softening resin in the formula of the polar rubber hot-vulcanized adhesive of the present invention. The rubber resin can play a role in perfect adhesion of the topcoat, and the rubber resin can greatly improve the flexibility of the epoxy resin system due to its good ductility. As an example, the rubber resin in this embodiment includes but is not limited to chlorinated rubber, nitrile rubber, chlorinated polyethylene, and chlorosulfonated polyethylene, and in this embodiment, a unique ratio is adopted to set the rubber resin to a total mass ratio of 0.5% to 15% of the polar rubber hot-vulcanized adhesive. Therefore, in this embodiment, the softening resin includes: rubber resin; the softening resin accounts for 0.5% to 15% of the mass of the adhesive;

[0095] As one embodiment of the present invention, a resin solvent is provided in the formulation of the polar rubber hot-vulcanized adhesive of the present invention in combination with the epoxy resin. The resin solvent includes, but is not limited to, xylene and methyl isobutyl ketone, which are solvents that can well dissolve bisphenol A and F-type epoxy resin. In this embodiment, a unique ratio is adopted to set the resin solvent to account for 40% to 80% of the mass of the adhesive. Therefore, in this embodiment, the resin solvent includes: one or more of xylene and methyl isobutyl ketone; the resin solvent accounts for 40% to 80% of the mass of the adhesive.

[0096] As an embodiment of the present invention, the formula of the polar rubber hot vulcanization adhesive of the present invention is further provided with an acid scavenger. The acid scavenger is a chemical substance added to the mixture to remove or passivate impurities and unwanted reaction products to ensure that no reaction that is detrimental to the preparation of the target compound is caused. As an example, the acid scavenger includes but is not limited to metal stearates and metal oxides; and the acid scavenger is preferably zinc, magnesium, aluminum oxide or stearate in this embodiment; in this embodiment, a unique ratio is adopted, and the acid scavenger is set to account for 1% to 20% of the mass of the adhesive. Therefore, in this embodiment, the acid scavenger includes: one or more of metal stearates and metal oxides, and the metal oxides include one or more of zinc oxide, magnesium oxide and aluminum oxide; the acid scavenger accounts for 1% to 20% of the mass of the adhesive;

[0097] As an embodiment of the present invention, since the production process in Example 1 may involve the color production of the adhesive, the polar rubber hot vulcanization adhesive in this embodiment is optionally further provided with a pigment. That is, in order to comply with the usage habits of customers and the industry, carbon black and titanium dioxide are added as pigments during the preparation of the polar rubber hot vulcanization adhesive, and the finished product is made gray. The ratio of titanium dioxide to carbon black is approximately 5:1 to 10:1, and the total amount of pigment added accounts for 3 to 8% of the mass of the adhesive. Correspondingly, the specific color of the finished product and the color ratio requirements of the pigment are set according to the specific color requirements.

[0098] In the present invention, the performance of the polar rubber hot-vulcanized adhesive is tested to show its performance superior to that of the prior art: accordingly, the following experiments focus on studying the effect of the addition amount of rubber resin on the quality. In order to reflect the effect of rubber resin and reduce uncertainty, this application shows the experimental process and results of keeping the addition amount of other materials except solvent unchanged; in the experimental process, the topcoat adhesive BDL-017 commonly used in the prior art is used to verify the adhesion of the primer and topcoat and the flexibility of the entire system of primer and topcoat; accordingly, the ratio is mass percentage, and the sum of the formulas of each test experiment is 100%; the following are the test benchmark auxiliary raw materials and test identification methods used: the metal material used is aluminum sheet, and the metal pretreatment process is hot alkaline water degreasing, passivation liquid treatment and cleaning; the primer dry film thickness is 3µm; the primer baking condition is metal peak temperature PMT199~204 degrees Celsius; the topcoat dry film thickness is 10µm; the topcoat baking condition is metal peak temperature PMT149 degrees Celsius; the adhesion identification method used is ASTM D3359-87 "Determination of Adhesion by Tape Test"; the flexibility evaluation method used is GB_T 30791-2014 "Paints and Varnishes T-Bend Test"; ultimately, the following performance statistics are obtained, Table 1:

[0099] Table 1

[0100] Experimental No. ABCDEFG Epoxy resin 15151515151515 Phenolic resin 8888888 Rubber 1585881014 Rubber 25582100 Solvent 59.556.556.558.559.562.566.5 Acid scavenger 3333333 Carbon black 0.50.50.50.50.50.50.5 Titanium dioxide 4444444 Adhesion 5351000 Flexibility of primer T5T4T5T0-0.5T0-0.5T4T4 Flexibility after topcoat T4T4T4T1-T2T0-0.5T3T3

[0101] The data in Table 1 clearly demonstrate that the polar rubber hot-vulcanizing adhesive prepared by the formulation and manufacturing process of the polar rubber hot-vulcanizing adhesive employed in the present invention improves the primer flexibility of the prior art from T3 to T0, effectively resolving quality issues commonly encountered by customers during the metal coil forming process, such as primer detachment and rubber bubbles. Example 3

[0102] This embodiment provides a method for using a highly flexible rubber heat-vulcanized adhesive, as shown in FIG3 , comprising the following steps:

[0103] In this embodiment, the method of use is the usage requirement for the polar rubber heat-vulcanized adhesive described in Example 2, and is specifically as follows:

[0104] A. Applying the polar rubber hot-vulcanized adhesive to a substrate. In practice, the polar rubber hot-vulcanized adhesive of the present invention can be applied to a metal substrate using various common sizing processes, and a recommended dry film thickness during application is 5 to 15 µm.

[0105] B. Dry the coated substrate. In actual operation, the metal substrate to be applied needs to be placed in an oven for drying. The recommended curing temperature in this application is a maximum metal plate temperature of 215-249 degrees Celsius, and the corresponding drying time is 30 seconds to 2 minutes.

[0106] C. Deforming the dried substrate, wherein the deformation processing includes one or more of bending, stamping, and stretching. In actual operation, the cured metal substrate can be subjected to bending, stamping, and other processes. Due to the high flexibility of the polar rubber hot-vulcanized adhesive of the present invention, it is suitable for application scenarios with high flexibility requirements;

[0107] D. The mixture to be bonded is thermoformed on the substrate after the deformation process, and while the mixture to be bonded is thermoformed, a bonding reaction occurs with the polar rubber hot vulcanized adhesive coated on the surface of the substrate; the thermoforming includes: hot pressing, hot extrusion or injection molding; in actual operation, the formed metal substrate can be bonded to polypropylene and its blends by hot pressing / hot extrusion / injection molding, and the strength can reach that of polypropylene and its blends.

[0108] Different from the existing technology, the present application uses a highly flexible rubber hot-vulcanized adhesive, manufacturing process and equipment. A unique rubber resin can be selected in the process and strictly added in an appropriate amount to produce an adhesive with ultra-high flexibility. At the same time, the adhesive can also have good adhesion. The manufacturing process of the highly flexible rubber hot-vulcanized adhesive described in the present invention produces an adhesive with higher quality performance through a unique manufacturing method, helping customers improve production yield, improve customer satisfaction and production efficiency, and help customers save production costs.

[0109] It should be understood that in the various embodiments of this document, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this document.

[0110] It should also be understood that in the embodiments herein, the term "and / or" merely describes an association between associated objects, indicating that three possible relationships exist. For example, "A and / or B" could represent: A alone, A and B simultaneously, or B alone. Furthermore, the character " / " in this document generally indicates an "or" relationship between the associated objects.

[0111] Those skilled in the art will appreciate that the units and algorithm steps of each example described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, computer software, or a combination of the two. In order to clearly illustrate the interchangeability of hardware and software, the above description has generally described the composition and steps of each example according to function. Whether these functions are performed in hardware or software depends on the specific application and design constraints of the technical solution. Professional and technical personnel can use different methods to implement the described functions for each specific application, but such implementation should not be considered beyond the scope of this document.

[0112] Those skilled in the art will clearly understand that, for the convenience and brevity of description, the specific working processes of the systems, devices and units described above can refer to the corresponding processes in the aforementioned method embodiments and will not be repeated here.

[0113] In the several embodiments provided herein, it should be understood that the disclosed systems, devices, and methods can be implemented in other ways. For example, the device embodiments described above are merely illustrative. For example, the division of the units is merely a logical function division. In actual implementation, there may be other division methods, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. In addition, the mutual coupling or direct coupling or communication connection shown or discussed can be an indirect coupling or communication connection through some interfaces, devices, or units, or can be an electrical, mechanical, or other form of connection.

[0114] The units described as separate components may or may not be physically separate, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed across multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the embodiments herein.

[0115] In addition, the functional units in the various embodiments herein may be integrated into a single processing unit, each unit may exist physically separately, or two or more units may be integrated into a single unit. The aforementioned integrated units may be implemented in the form of hardware or software functional units.

[0116] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention's description and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A process for producing a highly flexible rubber hot-vulcanized adhesive, characterized in that: The following steps are involved: Raw materials and parameter configuration steps: preparing epoxy resin, thermal curing agent, softening resin, resin solvent and acid scavenger; setting a first dissolution processing parameter, a second dissolution processing parameter, a third stirring processing parameter and a fourth stirring processing parameter; Resin solution preparation steps: Based on the first dissolution treatment parameters, a first high-temperature dissolution treatment is performed using the epoxy resin, the resin solvent and the acid scavenger to obtain a first epoxy resin solution; Based on the second dissolution treatment parameters, a second high-temperature dissolution treatment is performed using the softening resin, the resin solvent and the acid scavenger to obtain a second softening resin solution; Mixing process steps: Based on the third stirring process parameters, a third mixing and stirring process is performed using the thermal curing agent, the acid scavenger, the first epoxy resin solution and the second softening resin solution to obtain a third mixing and stirring product; Based on the fourth stirring treatment parameters, the resin solvent and the third stirring product are used to perform a fourth grinding and stirring treatment to obtain a polar rubber heat-vulcanized adhesive.

2. The process for producing a highly flexible rubber hot-vulcanized adhesive according to claim 1, characterized in that: The first dissolution processing parameters include: a first initial speed interval, a first middle speed interval, a first final speed interval, a first initial duration, and a first final duration; The first high temperature dissolution treatment comprises: Setting up a first reaction kettle; Adding the resin solvent and the acid scavenger into the first reaction kettle, and stirring the resin solvent and the acid scavenger in the first reaction kettle according to the first initial speed range; While the resin solvent and the acid scavenger in the first reaction kettle are being stirred, the epoxy resin is added into the first reaction kettle; After adding the epoxy resin, stirring the resin solvent, the acid scavenger and the epoxy resin in the first reaction kettle according to the first intermediate speed range and the first primary time to obtain an initial epoxy resin solution; After obtaining the initial epoxy resin solution, the resin solvent and the acid scavenger are added to the first reactor, and the initial epoxy resin solution, the resin solvent and the acid scavenger in the first reactor are stirred according to the first final-stage speed interval and the first final-stage time to obtain the first epoxy resin solution.

3. The process for producing a highly flexible rubber hot-vulcanized adhesive according to claim 1, characterized in that: The second dissolution processing parameters include: a second initial speed interval, a second middle speed interval, a second final speed interval, a second initial time length, and a second final time length; The second high temperature dissolution treatment comprises: Setting up a second reactor; Adding the resin solvent and the acid scavenger into the second reaction kettle, and stirring the resin solvent and the acid scavenger in the second reaction kettle according to the second primary speed range; While the resin solvent and the acid scavenger are being stirred in the second reaction kettle, the softening resin is added into the second reaction kettle; After adding the softening resin, stirring the resin solvent, the acid scavenger and the softening resin in the second reaction kettle according to the second intermediate speed range and the second primary time length to obtain an initial softening resin solution; After obtaining the initial softening resin solution, the resin solvent and the acid scavenger are added to the second reactor, and the initial softening resin solution, the resin solvent and the acid scavenger in the second reactor are stirred according to the second final-stage speed range and the second final-stage time length to obtain the second softening resin solution.

4. The process for producing a highly flexible rubber hot-vulcanized adhesive according to claim 1, characterized in that: The third stirring processing parameters include: a third temperature threshold, a third initial speed interval, a third final speed interval, a third initial time length and a third final time length; The third mixing and stirring process comprises: Acquiring room temperature, detecting a first temperature of the first initial epoxy resin solution in the first reaction kettle, and when the first temperature reaches the room temperature, performing a first stirring step based on the second softening resin solution, the third initial speed interval, and the third initial time to obtain a first stirring product; A second stirring step is performed based on the first stirring product, the thermal curing agent, the acid scavenger, the third temperature threshold, the third final speed interval and the third final time to obtain the third mixed stirring product.

5. The process for producing a highly flexible rubber hot-vulcanized adhesive according to claim 4, characterized in that: The first stirring step comprises: Adding the second softening resin solution in the second reactor into the first reactor; The first initial epoxy resin solution and the second softening resin solution in the first reaction kettle are stirred according to the third initial speed range and the third initial time length to obtain the first stirring product.

6. The process for producing a highly flexible rubber hot-vulcanized adhesive according to claim 4, characterized in that: The second stirring step comprises: Slowly adding the thermal curing agent and the acid scavenger into the first reaction kettle; The second temperature of the compound in the first reactor is detected. When the second temperature is not higher than the third mixed stirring product, the first stirring product, the thermal curing agent and the acid scavenger in the first reactor are stirred according to the third final speed range and the third final time to obtain the third mixed stirring product.

7. The process for producing a highly flexible rubber hot-vulcanized adhesive according to claim 1, characterized in that: The fourth stirring processing parameters include: a fourth temperature threshold, a fourth grinding time, a fourth grinding fineness and a fourth initial speed range; The fourth grinding and stirring process comprises: Grinding the third mixed stirring product according to the fourth temperature threshold and the fourth grinding time; When grinding the third mixed product, if the first fineness of the third mixed product is lower than the fourth grinding fineness, a first ground product is obtained; The first grinding product and the resin solvent are stirred in the fourth primary speed range to obtain the polar rubber heat-vulcanized adhesive.

8. A highly flexible rubber hot-vulcanized adhesive, made based on the manufacturing process of a highly flexible rubber hot-vulcanized adhesive according to any one of claims 1 to 7, characterized in that: The polar rubber heat-vulcanized adhesive is composed of epoxy resin, heat curing agent, softening resin, resin solvent and acid scavenger; The epoxy resin accounts for 5% to 30% of the mass of the adhesive; The mass proportion of the thermal curing agent to the adhesive is 5% to 20%; The softening resin accounts for 0.5% to 15% of the mass of the adhesive; The resin solvent accounts for 40% to 80% of the mass of the adhesive; The acid scavenger accounts for 1% to 20% of the mass of the adhesive.

9. The highly flexible rubber heat-vulcanized adhesive according to claim 8, characterized in that: The epoxy resin includes: one or more of bisphenol A type resin and bisphenol F type resin; The thermal curing agent includes: phenolic resin; The softening resin includes: rubber resin; The resin solvent includes: one or more of xylene and methyl isobutyl ketone; The acid scavenger includes: one or more of metal stearates and metal oxides, and the metal oxides include one or more of zinc oxide, magnesium oxide and aluminum oxide.

10. The method for using a highly flexible rubber heat-vulcanized adhesive according to claim 9, characterized in that: The method of use comprises the following steps: Applying the polar rubber heat-vulcanized adhesive to a substrate; Drying the coated substrate; Performing deformation processing on the dried substrate, wherein the deformation processing includes: one or more of bending processing, stamping deformation processing and stretching processing; The mixture to be bonded is thermoformed on the substrate after the deformation process, and while the mixture to be bonded is thermoformed, a bonding reaction occurs with the polar rubber hot vulcanizing adhesive coated on the surface of the substrate; the thermoforming includes: hot pressing, hot extrusion or injection molding.

Citation Information

Patent Citations

  • Halogen-free high heat-resistant and heat-conducting resin film and manufacturing method thereof

    CN102660210A

  • Heat vulcanization adhesive and preparation method thereof

    CN103525349A

  • Adhesive, preparation method for same and adhesive copper foil produced by applying same

    CN107760241A

  • Thermal bonding adhesive suitable for polypropylene and blend thereof

    CN113913143A

  • Special high-flexibility heat-vulcanized adhesive for bonding easily-deformed base material

    CN115058221A